Coating composition for electroless plating and method for forming electroless plating

The coating composition for electroless plating, comprising a palladium-dispersant complex, a specific resin ratio, and nanoparticles, addresses long drying times by enhancing pot life and efficiency, enabling faster and more effective electroless plating.

JP2024134204AActive Publication Date: 2024-10-03宫城県 +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044395
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Conventional coating compositions for electroless plating have long drying times, which affect the efficiency and productivity of the plating process.

Method used

A coating composition for electroless plating containing a complex of palladium particles and a dispersant, a solvent, and a binder resin with a specific ratio of polyamide and epoxy resin, along with nanoparticles, which improves pot life and shortens drying time.

Benefits of technology

The composition enhances pot life and reduces drying time, allowing for more efficient electroless plating with improved adhesion and reactivity, eliminating the need for additional processes like etching or increasing reducing agent concentration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134204000001
    Figure 2024134204000001
  • Figure 2024134204000002
    Figure 2024134204000002
  • Figure 2024134204000003
    Figure 2024134204000003
Patent Text Reader

Abstract

To provide a novel coating composition for electroless plating.SOLUTION: A coating composition for electroless plating comprises (1) a complex of palladium particles and a dispersant, (2) a solvent, and (3) a binder resin. The (3) binder resin comprises a polyamide resin and an epoxy resin. For 100 pts.mass of the binder resin, the amount of the added epoxy resin is more than 0 and 20 pts.wt. or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating composition for electroless plating and a method for forming an electroless plating. [Background technology]

[0002] Patent Document 1 discloses a coating composition for electroless plating that contains (1) a complex of palladium particles and a dispersant, (2) a solvent, and (3) a binder. When this coating composition for electroless plating is used to carry out a coating process, a curing process, and then an electroless plating process, it is possible to form a film that has high reactivity for electroless plating and exhibits excellent adhesion. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5422812 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a novel coating composition for electroless plating. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have developed a technology in which a coating composition for electroless plating contains (1) a complex of palladium particles and a dispersant, (2) a solvent, and (3) a binder resin, and by adjusting the binder resin (3) to a specific content, the pot life after formulation can be improved, and when electroless plating is performed using this coating composition for electroless plating, the drying time of the plating can be shortened.

[0006] That is, the present invention includes the following coating composition for electroless plating and a method for forming an electroless plating.

[0007] Section 1. A coating composition for electroless plating, comprising: (1) A composite of palladium particles and a dispersant, (2) a solvent, and (3) Binder resin Contains The coating composition for electroless plating (3), wherein the binder resin comprises a polyamide resin and an epoxy resin, and the amount of the epoxy resin added in 100 parts by mass (total amount) of the binder resin is more than 0 and not more than 20 parts by mass (20% by weight).

[0008] Section 2. Further, (4) nanoparticles are contained, The (4) nanoparticles are surface-treated, 2. The coating composition for electroless plating according to item 1, wherein the amount of the (4) nanoparticles added is 0.01 to 100 parts by mass per 1 part by weight of the (3) binder resin.

[0009] Section 3. 3. The coating composition for electroless plating according to claim 2, wherein the nanoparticles (4) are inorganic oxides.

[0010] Section 4. 4. The coating composition for electroless plating according to item 2 or 3, wherein the nanoparticles (4) have an average particle size of 10 nm to 1,000 nm.

[0011] Section 5. Item 4. The coating composition for electroless plating according to item 2 or 3, wherein the nanoparticles (4) are silicon dioxide.

[0012] Section 6. 3. A method for forming an electroless plating on a substrate by using the coating composition for electroless plating according to item 1 or 2 and carrying out a coating treatment, a curing treatment, an alkali treatment, and an electroless plating treatment. Effect of the Invention

[0013] The present invention can provide a novel coating composition for electroless plating.

[0014] The coating composition for electroless plating of the present invention can improve the pot life after formulation, and when this coating composition for electroless plating is used for electroless plating, the drying time of the plating can be shortened. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below.

[0016] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.

[0017] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist of."

[0018] In this specification, when a numerical range is indicated as "A to B," it means A or more and B or less.

[0019] [1] Coating composition for electroless plating Conventionally, electroless plating coating compositions contain polyamide resin and an epoxy curing agent as basic components, and have had the problem that the pot life after blending is short, or that when electroless plating is performed using this electroless plating coating composition, the drying time of the plating is long.

[0020] The electroless plating coating composition of the present invention comprises: (1) A composite of palladium particles (Pd particles) and a dispersant (Pd composite), (2) a solvent, and (3) Binder resin Contains The (3) binder resin contains a polyamide resin and an epoxy resin, and the amount of the epoxy resin added in 100 parts by weight (total amount) of the binder resin is more than 0 and 20 parts by weight (20% by weight) or less.

[0021] The coating composition for electroless plating of the present invention preferably further contains (4) nanoparticles, which are surface-treated, and the amount of the nanoparticles added is 0.01 to 100 parts by weight per part by weight of the (3) binder resin.

[0022] In the coating composition for electroless plating of the present invention, (4) the nanoparticles are preferably an inorganic oxide, have an average particle size of 10 nm to 1,000 nm, and are silicon dioxide.

[0023] The present invention further includes a method for forming an electroless plating on a substrate by carrying out a coating treatment, a curing treatment, an alkali treatment, and an electroless plating treatment using the coating composition for electroless plating of the present invention.

[0024] The electroless plating coating composition of the present invention can improve the pot life after formulation as compared with conventional electroless plating coating compositions.

[0025] When electroless plating is carried out using the coating composition for electroless plating of the present invention, the drying time of the plating can be shortened as compared with the case of using conventional coating compositions for electroless plating.

[0026] (1) Composite of palladium particles and dispersant (Pd composite) The coating composition for electroless plating of the present invention contains a complex of palladium particles (hereinafter also referred to as "Pd particles") and a dispersant (hereinafter also referred to as "palladium complex" or "Pd complex").

[0027] The Pd complex can be prepared in the following manner.

[0028] It can be prepared by reducing palladium ions (hereinafter also referred to as "Pd ions") supplied from a palladium compound (hereinafter also referred to as "Pd compound") such as palladium chloride with a secondary or tertiary amine such as hydrazine hydrate in the presence of a dispersant such as a polycarboxylic acid polymer.

[0029] Dispersants The dispersant used is preferably a polycarboxylic acid dispersant, a block copolymer type polymer dispersant having a hydroxyl group, and / or a block copolymer type polymer dispersant having a carboxyl group, etc. Commercially available dispersants may be used.

[0030] The polycarboxylic acid-based polymer dispersant is preferably a polycarboxylic acid ammonium salt, a polycarboxylic acid sodium salt, a polycarboxylic acid triethylamine salt, a polycarboxylic acid triethanolamine salt, etc. Examples of the polycarboxylic acid-based polymer dispersant that may be used include Nopcosant K, R, RFA, Nopcosperse 44-C, SN Dispersant 5020, 5027, 5029, 5034, 5045, and 5468 manufactured by San Nopco Ltd., and Demol P, EP, Poise 520, 521, 530, and 532A manufactured by Kao Corporation.

[0031] The block copolymer type polymer dispersant having a hydroxyl group is preferably a polyoxyethylene alkyl ether carboxylate, an alkyl hydroxy ether carboxylate, etc. The block copolymer type polymer dispersant having a hydroxyl group may be, for example, DISPERBYK190, 2010, etc. manufactured by BYK Japan Co., Ltd.

[0032] The block copolymer type polymer dispersant having a carboxyl group is preferably an acrylic acid-maleic acid copolymer, a styrene-maleic acid copolymer, an acrylic acid-sulfonic acid copolymer, etc. The block copolymer type polymer dispersant having a carboxyl group may be, for example, DISPERBYK180, 187, 191, 194 manufactured by BYK Japan Co., Ltd., or AQUALIC TL, GL, LS manufactured by Nippon Shokubai Co., Ltd.

[0033] The dispersant may be used alone or in combination of two or more kinds (blend).

[0034] Among the dispersants, it is more preferable to use a block copolymer type polymer dispersant having a carboxyl group.

[0035] Palladium particles (Pd particles) The Pd particles can be prepared by reducing Pd ions supplied from a Pd compound with a reducing agent in the presence of a dispersing agent.

[0036] The Pd compound that supplies Pd ions is preferably palladium chloride, palladium sulfate, palladium nitrate, palladium acetate, palladium benzoate, palladium salicylate, palladium toluenesulfonate, palladium perchlorate, palladium benzenesulfonate, or the like.

[0037] The Pd compound may be used alone or in combination of two or more kinds (blend).

[0038] The reducing agent used is preferably a secondary or tertiary amine such as hydrazine hydrate (hydrazine monohydrate), sodium borohydride, N,N dimethylethanolamine, or diethanolamine.

[0039] The solvent used in the reduction (solvent for making the dispersant and Pd ions present) is preferably the following (2) solvent.

[0040] The solvent may be one of these solvents alone, or two or more of them may be mixed (blended) and used.

[0041] The method for reducing Pd ions is preferably a method in which a dispersant and Pd ions are placed in a solvent, and then a reducing agent is added to the solvent, whereby the Pd ions come into contact with the reducing agent, thereby enabling the Pd ions to be reduced.

[0042] It is believed that most of the Pd particles are attached to the outside of the dispersant. For example, if the shape of the Pd complex (the overall shape of the dispersant) is a dense sphere, it is believed that most of the Pd particles are attached to the surface side (outside) of the sphere.

[0043] The weight ratio of Pd particles to dispersant in the Pd composite is preferably Pd particles:dispersant=about 35:65 to 85:15, and more preferably Pd particles:dispersant=about 50:50 to 75:25.

[0044] The average particle size of the Pd particles alone is preferably about 2 nm to 10 nm.

[0045] The particle size of the Pd particles is measured, for example, using a transmission electron microscope. The average particle size of the Pd particles alone is calculated by randomly selecting 10 Pd particles, measuring the particle sizes of the Pd particles using a transmission electron microscope, and averaging the numbers (number-based average size).

[0046] The structure of the Pd complex is preferably a spherical structure.

[0047] The average particle size of the Pd composite is preferably about 10 nm to 300 nm, and more preferably about 10 nm to 100 nm.

[0048] The average particle size of the Pd complex is measured, for example, by a particle size analyzer (Otsuka Electronics Co., Ltd., FPAR-1000) (weight-based average size).

[0049] (2) Solvent The coating composition for electroless plating of the present invention contains a solvent.

[0050] The solvent (dispersion solvent) is capable of dispersing the Pd complex.

[0051] The solvent has excellent affinity with the following (3) binder resin.

[0052] From the viewpoint of being able to impart dispersibility of the Pd complex in the electroless plating coating composition, it is preferable to use at least one solvent selected from the group consisting of water and aprotic polar solvents such as N-methylpyrrolidone.

[0053] The aprotic polar solvent preferably used is an aprotic polar solvent such as N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), γ-butyrolactone (GBL), or the like.

[0054] The aprotic polar solvent is preferably at least one aprotic polar solvent selected from the group consisting of NMP, DMF and DMAc.

[0055] The solvent can be converted after the reduction reaction of Pd ions. For example, the solvent can be converted from water to NMP.

[0056] The amount of the solvent (dispersion solvent) used is preferably 1×10 2 Mass part~1×10 6 Adjust so that it is about parts by mass.

[0057] When water is used as a solvent, the amount of the solvent is preferably 5×10 3 Part of mass ~3×10 5 parts by mass, more preferably 1×10 4 Part of mass ~2×10 5 Adjust so that it is about parts by mass.

[0058] When an aprotic polar solvent is used as the solvent, the amount of the solvent is preferably 5×10 2 Mass part~5×10 3 parts by mass, more preferably 1×10 3 Part of mass ~3×10 3 Adjust so that it is about parts by mass.

[0059] The solvent may be one of these solvents alone, or two or more of them may be mixed (blended) and used.

[0060] The solvent is preferably selected from the viewpoints of (1) the dispersibility of the Pd complex contained in the electroless plating coating composition, the solubility of the binder resin below, and (4) the dispersibility of the nanoparticles, as well as the viscosity, evaporation rate, and other aspects of the electroless plating coating composition, and the adhesion between the electroless plating coating composition and the substrate (ABS resin, glass plate, etc.).

[0061] In addition to the solvent used for dispersing the Pd complex, another type of solvent (additional solvent) may be used.

[0062] The additional solvent is preferably an alcohol such as methanol, ethanol, isopropyl alcohol (IPA), 1-butyl alcohol, isobutyl alcohol, etc.; a ketone such as acetone, methyl ethyl ketone (MEK), methyl isobutyl ketone, diacetone alcohol (4-hydroxy-4-methyl-2-pentanone), cyclohexanone, etc.; a glycol ether such as ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, etc.; an aromatic carboxylic acid ester such as methyl benzoate, ethyl benzoate, methyl salicylate, etc.; an aromatic hydrocarbon such as toluene, xylene, etc.; an aliphatic hydrocarbon such as n-hexane, n-heptane, mineral spirit, etc.; a glycol ether ester such as methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, methyl carbitol acetate, butyl carbitol acetate, etc.; an alkanol ester such as ethyl acetate, butyl acetate, etc.; 2-phenoxyethanol (ethylene glycol phenyl ether), etc. are used.

[0063] The additional solvent is preferably a solvent having a slow evaporation rate from the viewpoints of printability, paintability, and the leveling process after printing and painting. The solvent having a slow evaporation rate is preferably diacetone alcohol, cyclohexanone, methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, methyl carbitol acetate, butyl carbitol acetate, 2-phenoxyethanol, etc. The additional solvent may be used as a dilution solvent.

[0064] The additional solvent may be used alone or in combination of two or more kinds (blend).

[0065] (3) Binder resin The coating composition for electroless plating of the present invention contains a binder resin.

[0066] The electroless plating coating composition of the present invention contains a binder resin, which contains a polyamide resin and an epoxy resin. The amount of the epoxy resin added in 100 parts by mass (total amount) of the binder resin is preferably more than 0 parts by mass and not more than 25 parts by mass (25% by mass), more preferably 1 part by mass to 20 parts by mass, and even more preferably 5 parts by mass to 15 parts by mass.

[0067] The binder resin is selected from the viewpoints of the viscosity of the electroless plating coating composition, the adhesion between the electroless plating coating composition and the substrate (ABS resin, glass plate, etc.), and the curing conditions, so that the binder resin can be used to perform electroless plating satisfactorily.

[0068] In the coating composition for electroless plating of the present invention, by adjusting the binder resin to a specific content as described above, the pot life after formulation can be improved compared to conventional coating compositions for electroless plating.

[0069] In the electroless plating coating composition of the present invention, by adjusting the binder resin to a specific resin content as described above, when electroless plating is performed using this electroless plating coating composition, the drying time of the plating can be shortened compared to conventional electroless plating coating compositions.

[0070] The binder resin is dispersible or soluble in the above-mentioned (2) solvent.

[0071] The binder resin used is polyamide (resin).

[0072] polyamide The polyamide is preferably a polyetherester polyamide.

[0073] Polyetherester polyamide is obtained by reacting a polyamide component with a polyetherester component consisting of polyoxyalkylene glycol and dicarboxylic acid, and is a block copolymer having amide bonds, ether bonds, and ester bonds in the molecular chain.

[0074] The polyamide component is preferably a polyamide made from hexamethylenediamine and adipic acid, a polyamide made from hexamethylenediamine, polymerized fatty acid and azelaic acid, or sebacic acid, or a polyamide made from 12-aminododecanoic acid, caprolactam.

[0075] The polymerized fatty acids of the polyamides are preferably dimers of oleic acid, linoleic acid, erucic acid, and the like.

[0076] When using commercially available polymerized fatty acids, the main component is dimerized fatty acid, and other components include raw material fatty acid and trimerized fatty acid. Preferably, the dimerized fatty acid content is 70% by weight or more, and more preferably 95% by weight or more.

[0077] In the polyether ester component of the polyether ester amide, the polyoxyalkylene glycol is preferably polyoxyethylene glycol, polyoxypropylene glycol, polyoxytetramethylene glycol, a block or random copolymer of ethylene oxide and propylene oxide, a block or random copolymer of ethylene oxide and tetrahydrofuran, a copolymer of a dihydric phenol compound and a polyoxyalkylene glycol, or the like.

[0078] The dicarboxylic acid of the polyetheresteramide is preferably a dicarboxylic acid having a carbon number of 6 to 20. The dicarboxylic acid having a carbon number of 6 to 20 is preferably adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, or the like.

[0079] The weight ratio of the polyether ester amide (polyamide block / polyether ester block) is preferably 95 / 5 to 20 / 80.

[0080] The terminal end of the polyetheresteramide is preferably an amino group or a hydroxyl group.

[0081] The binder resin is an epoxy resin.

[0082] The epoxy resin to be used is preferably a solid type bisphenol A type epoxy resin having an epoxy equivalent of 440 to 4,100.

[0083] The epoxy resin curing agent is preferably a phenol-based curing agent or an amine-based curing agent. When a phenol-based curing agent is used, a liquid amine is preferably used as a catalyst.

[0084] The amount of epoxy resin added in 100 parts by mass (total amount) of binder resin is more than 0 and not more than 20 parts by mass (20 mass%), preferably 1 part by mass to 15 parts by mass (1% by mass to 15% by mass), and more preferably 5 parts by mass to 10 parts by mass (5% by mass to 10% by mass).

[0085] The binder resin may additionally be polyester resin, acrylic resin, polyurethane resin, polyimide resin, polyamide-imide resin (PAI), shellac resin, melamine resin, urea resin, polyolefin resin, vinyl acetate-vinyl chloride copolymer resin, butyral resin, or the like.

[0086] The acrylic resin is a polymer of an acrylic acid ester or a polymer of a methacrylic acid ester, or a copolymer having these as a comonomer. The acrylic resin is preferably a polymethyl methacrylate resin, a polymethyl acrylate resin, an ethylene-methyl acrylate copolymer, an ethylene-methyl methacrylate copolymer, or the like.

[0087] The polyamide-imide resin is a resin having an amide bond introduced into a polyimide main chain, and is preferably a resin obtained by a reaction between trimellitic anhydride and a diisocyanate, or between trimellitic anhydride chloride and a diamine, or the like.

[0088] As the additional binder resin, preferably, a polyester resin, a polyimide resin, a polyolefin resin, or the like is used, and more preferably, a polyolefin resin, or the like is used.

[0089] The additional binder resin may be used alone or in combination of two or more kinds (blend).

[0090] The amount of binder resin used (total amount used) is preferably 1 part by mass to 1 × 10 5 parts by mass, more preferably 50 parts by mass to 5×10 4 Adjust so that it is about parts by mass.

[0091] In the coating composition for electroless plating of the present invention, by adjusting the binder resin to a specific content as described above, the pot life after blending can be improved, and in addition, when electroless plating is performed using this coating composition for electroless plating, the drying time of the plating can be shortened.

[0092] (4) Nanoparticles The coating composition for electroless plating of the present invention preferably further contains nanoparticles, the nanoparticles being surface-treated, and the amount of the nanoparticles added is 0.01 to 100 parts by weight per 1 part by weight of the binder resin.

[0093] The nanoparticles are preferably made of an inorganic oxide, more preferably made of silicon dioxide, and preferably have an average particle size of 10 nm to 1,000 nm.

[0094] The nanoparticles preferably use inorganic oxides, such as silicon dioxide, aluminum oxide, titanium oxide, zirconium oxide, and the like.

[0095] The nanoparticles may be used alone or in combination of two or more kinds (blend).

[0096] As the inorganic oxide, more preferably, nanoparticles mainly composed of silicon dioxide are used. Silicon dioxide (SiO 2 Silica is a type of nanoparticle that is mainly composed of silicon dioxide. In addition to silicon dioxide, silica is also called silicic anhydride, silicic acid, and silicon oxide. Nanoparticles that are mainly composed of silicon dioxide have high reactivity and adhesion for electroless plating because the nanoparticles themselves dissolve when treated with alkali.

[0097] Even if the nanoparticles are not dissolved by alkaline treatment, by using a binder resin, the binder resin swells and dissolves by alkaline treatment, resulting in gaps between the nanoparticles and the binder and causing the nanoparticles to fall off, and therefore it is possible to obtain the same effect as with nanoparticles that are dissolved by alkaline treatment.

[0098] The shape of the nanoparticles is preferably spherical, polygonal, or the like.

[0099] The amount of nanoparticles used is adjusted to be preferably about 0.01 to 100 parts by weight, more preferably about 0.05 to 20 parts by weight, and even more preferably about 0.1 to 3 parts by weight, relative to 1 part by weight of binder resin.

[0100] In the electroless plating coating composition, by adjusting the amount of nanoparticles used, the viscosity of the electroless plating coating composition is well maintained, and the electroless plating coating composition is easy to apply. In the electroless plating coating composition, by adjusting the amount of nanoparticles used, the adhesion between the electroless plating coating composition and the substrate is good, and the electroless plating film is not easily peeled off.

[0101] The average particle size of the nanoparticles is preferably about 10 nm to 1,000 nm, more preferably about 10 nm to 500 nm, and even more preferably about 10 nm to 250 nm. The nanoparticles may contain nanoparticles that do not satisfy the above average particle size range, as long as the effects of the present invention are not impaired.

[0102] In the present invention, the average particle size of nanoparticles means the particle size of the primary particles of the nanoparticles.

[0103] The particle size of nanoparticles depends on the particle size range, but if it is about 0.1 μm or less, it is measured, for example, by dynamic light scattering or electron microscope observation. The average particle size of nanoparticles measured by dynamic light scattering is the harmonic mean particle size (diameter) based on the scattered light intensity.

[0104] The particle size of nanoparticles depends on the particle size range, but if it is about 0.1 μm or more, it is measured by, for example, a laser diffraction / scattering method.

[0105] The average particle size of nanoparticles is a value measured according to weight conversion distribution using a particle size analyzer (for example, FPAR-1000 manufactured by Otsuka Electronics Co., Ltd.).

[0106] Since the average particle diameter of the nanoparticles is in the range of about 10 nm to 1,000 nm, the particles are less likely to aggregate, have good dispersibility, and the electroless plating coating composition is easy to handle. When the electroless plating coating composition containing the nanoparticles is used, the appearance after plating is good.

[0107] Surface treatment of nanoparticles The nanoparticles are surface-treated (surface-treated nanoparticles).

[0108] Since the nanoparticles are surface-treated, the nanoparticles are well dispersed and do not re-aggregate, so that uniform plating can be obtained by using the coating composition for electroless plating.

[0109] The surface treatment of the nanoparticles is preferably a hydrophilic treatment and / or a hydrophobic treatment, and is appropriately selected depending on the types of the solvent and binder contained in the ink composition.

[0110] The surface treatment of the nanoparticles is preferably a hydrophobic treatment, since many binder resins and solvents have hydrophobic properties. The hydrophobic treatment is preferably a surface treatment using a silane coupling agent.

[0111] The silane coupling agent used for the surface treatment is preferably phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, or the like.

[0112] From the viewpoint of dispersion stability, it is more preferable to use phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, or the like for the surface treatment.

[0113] The silane coupling agent may be used alone or in combination of two or more kinds (blend).

[0114] The surface treatment of nanoparticles (inorganic oxides) is carried out, for example, by adding and spraying a silane coupling agent to untreated inorganic filler while stirring and dispersing it in a mixer at room temperature, and stirring for 5 to 15 minutes.

[0115] The mixer may be a known mixer, preferably a blender such as a V blender, a ribbon blender or a bubble cone blender, a mixer such as a Henschel mixer or a concrete mixer, or a ball mill, more preferably a mixer.

[0116] Examples of silane coupling agents include phenyltrimethoxysilane ((CH 3 O) 3 Silicon Carbide 6 H 5 ), phenyltriethoxysilane ((C 2 H 5 O) 3 Silicon Carbide 6 H 5 ) or the like, it is possible to treat the surface of nanoparticles with phenylsilane.

[0117] The coating composition for electroless plating of the present invention preferably contains nanoparticles whose surfaces have been treated with phenylsilane, in other words, nanoparticles whose surfaces have been modified with phenylsilane groups (phenylsilane surface-treated nanoparticles).

[0118] The amount of the silane coupling agent used (amount used) is preferably adjusted to about 0.5 to 2 parts by weight per 100 parts by weight of the nanoparticles.

[0119] The nanoparticles are preferably spherical silica having an average particle size of about 10 nm to 1,000 nm, and the silica is preferably surface-treated (hydrophobized) with a silane coupling agent.

[0120] The coating composition for electroless plating of the present invention preferably contains nanoparticles (such as silicon dioxide) and / or surface-treated nanoparticles (such as phenylsilane-treated silica).

[0121] By carrying out coating treatment, curing treatment, alkali treatment, and then electroless plating treatment in a predetermined manner using the coating composition for electroless plating of the present invention, it is possible to form a film that has high reactivity for electroless plating, excellent adhesion to withstand chrome plating, and excellent smoothness to withstand decorative plating. By using the ink composition, it is further possible to form partial plating on a substrate while suppressing the spread of the pattern.

[0122] Since the coating composition for electroless plating of the present invention contains nanoparticles and / or surface-treated nanoparticles, a film formed using this coating composition for electroless plating has an excellent effect of relieving stress that occurs between the substrate and the plating film due to temperature differences. The film, which exists between the substrate and the plating film, can relieve the stress and prevent a decrease in adhesion.

[0123] A plating film formed using the coating composition for electroless plating of the present invention can maintain high adhesion even when exposed to an environment with a large temperature difference for a long period of time.

[0124] [2] Method for producing coating composition for electroless plating The coating composition for electroless plating of the present invention can be produced by the following method.

[0125] As described above, the Pd particles can be prepared by reducing Pd ions supplied from a Pd compound with a reducing agent in the presence of a dispersing agent.

[0126] The coating composition for electroless plating of the present invention is preferably (i)(2) a step of causing Pd ions and a dispersant to be present in a solvent and reducing the Pd ions with a reducing agent to prepare a composite of Pd particles and the dispersant (1); (ii) (2) additionally dispersing (4) nanoparticles in a solvent, and then mixing (3) a binder resin to form a mixture; and (iii) mixing the mixture of (2) the solvent obtained in the step (i) and the complex of (1) the Pd particles and the dispersant with the mixture of (2) the solvent obtained in the step (ii), additionally (4) the nanoparticles, and (3) the binder resin; The method includes the steps of:

[0127] Either step (i) or step (ii) may be carried out first.

[0128] Depending on the production method, it is possible to produce a coating composition for electroless plating to be used in a pretreatment for electroless plating.

[0129] By using the coating composition for electroless plating of the present invention, it is possible to form a film that has high reactivity in electroless plating, excellent adhesion to withstand chrome plating, and excellent smoothness to withstand decorative plating. By using the coating composition for electroless plating of the present invention, it is possible to form partial plating on a substrate while suppressing the spread of a pattern. By using the coating composition for electroless plating of the present invention, it is not necessary to increase the concentration of a reducing agent in electroless plating or to increase the reaction temperature in order to improve the reactivity of electroless plating. By using the coating composition for electroless plating of the present invention, it is also not necessary to perform an etching process using harmful substances, a complicated catalyst application process, etc.

[0130] The coating composition for electroless plating of the present invention has an improved pot life after formulation, and when this coating composition for electroless plating is used for electroless plating, the drying time of the plating can be shortened.

[0131] Process (i) (2) Pd ions and a dispersant are placed in a solvent, and the Pd ions are reduced using a reducing agent to produce (1) a composite of Pd particles and the dispersant (Pd composite).

[0132] First, Pd ions and a dispersant are placed in a solvent (dispersion medium). A Pd compound that supplies the Pd ions is used as a supply source of the Pd ions.

[0133] The amount of each component used (parts by weight) is based on "Pd compound."

[0134] The dispersant is the above-mentioned dispersant. The ratio (weight ratio) of Pd ions to the dispersant is preferably about 10 parts by weight to 200 parts by weight, and more preferably about 30 parts by weight to 150 parts by weight, per 100 parts by weight of the Pd compound.

[0135] As the solvent, the above-mentioned (2) solvent such as water is used. The amount of the solvent used is adjusted to a range in which the Pd ions and the dispersant are uniformly present, and is preferably 1×10 4 Weight part~3×10 5 parts by weight, more preferably 1×10 4 ~1×10 5 Use about parts by weight.

[0136] Next, the Pd ions are reacted with the reducing agent, and the Pd ions are reduced by the reducing agent. That is, a reduction reaction of the Pd ions occurs, and as a result, the above-mentioned (1) composite of the Pd particles and the dispersant (Pd composite) can be obtained. The reducing agent used is the same as that used to prepare the Pd composite. The amount of the reducing agent used is preferably about 100 to 800 parts by weight, and more preferably about 200 to 600 parts by weight, relative to 100 parts by weight of the Pd compound.

[0137] The reaction temperature for the reaction using a reducing agent is preferably about 35°C to 45°C, and the temperature is then raised to about 50°C to 60°C.

[0138] The reaction time for the reaction using a reducing agent is preferably about 1 hour to 5 hours.

[0139] The pressure and atmosphere during the reaction using a reducing agent are preferably atmospheric pressure or air (air) atmosphere. The reaction is preferably carried out in an open system such as a beaker. The reaction is preferably carried out by stirring a solution containing Pd ions (Pd compound), a dispersant and a reducing agent with a bladed stirring rod.

[0140] Next, the mixture containing the solvent and the Pd complex (Pd complex-containing liquid) is ultrafiltered to separate the complex of the Pd particles and the dispersant. This operation makes it possible to remove inorganic salts and excess dispersant contained in the Pd complex-containing liquid. For example, it is possible to filter the Pd complex-containing liquid and replenish it with a solvent such as water or NMP. This process can be repeated.

[0141] After the reduction reaction of Pd ions, the solvent can be changed. For example, the solvent is preferably water, and then the water is changed to NMP or the like (solvent, dispersion medium), thereby making it possible to prepare a mixture of NMP ((2) solvent) and (1) Pd complex.

[0142] Process (ii) (4) Nanoparticles are additionally dispersed in the (2) solvent, and then (3) Binder resin is mixed to prepare a mixture.

[0143] The nanoparticles are dispersed in a solvent (dispersion medium). The nanoparticles used are the above-mentioned nanoparticles, and preferably surface-treated nanoparticles. The nanoparticles used are preferably spherical silica having an average particle size of about 10 nm to 1,000 nm, and more preferably silica that has been surface-treated (hydrophobized) with a silane coupling agent.

[0144] As the solvent, the above-mentioned (2) solvent such as 2-phenoxyethanol, diacetone alcohol, cyclohexanone, etc. The amount of the solvent used is adjusted within a range in which the nanoparticles are uniformly present, and is preferably about 100 parts by weight to 10,000 parts by weight, more preferably about 200 parts by weight to 5,000 parts by weight, per 100 parts by weight of the nanoparticles.

[0145] The binder is the binder resin (3) described above. The amount of the binder used is preferably about 1 to 10,000 parts by weight, more preferably about 5 to 2,000 parts by weight, and even more preferably about 33 to 1,000 parts by weight, based on 100 parts by weight of the nanoparticles, from the viewpoints of the viscosity of the coating composition for electroless plating, the adhesion between the coating composition for electroless plating and the substrate (ABS resin, glass plate, etc.), and the curing conditions.

[0146] The mixing is not particularly limited, and is preferably performed under atmospheric pressure or in an atmospheric (air) atmosphere. The mixing is preferably performed in an open system such as a beaker. The mixing is preferably performed by stirring the mixture containing the solvent, nanoparticles, and binder with a bladed stirring rod.

[0147] Process (iii) The mixture of (2) solvent and (1) Pd complex obtained in the step (i) is mixed with the mixture of (2) solvent obtained in the step (ii) and, additionally, the mixture of (4) nanoparticles and (3) binder resin.

[0148] [3] Plating method By carrying out coating treatment, curing treatment, alkali treatment, and electroless plating treatment using the coating composition for electroless plating of the present invention, plating can be formed on a substrate. Using the coating composition for electroless plating of the present invention, (i) the coating composition for electroless plating is applied to a substrate, (ii) the (2) solvent contained in the coating composition for electroless plating is volatilized and / or dried, (iii) the (3) binder resin contained in the coating composition for electroless plating is cured, (iv) the substrate to which the coating composition for electroless plating has been applied is subjected to an alkali treatment, and (v) the substrate is electrolessly plated.

[0149] Base material The substrate is preferably made of plastic (resin), glass, metal, ceramics, or the like.

[0150] The plastic (resin) is preferably a polyolefin such as polyethylene (PE), polypropylene (PP), polystyrene (PS), polybutadiene, polybutene, polyisoprene, polychloroprene, polyisobutylene, polyisoprene, or polymethylpentene (TPX).

[0151] The plastic (resin) preferably used is ABS resin (a copolymer synthetic resin of acrylonitrile, butadiene, and styrene), AES resin (a copolymer synthetic resin of acrylonitrile, ethylene, and styrene), ASA resin (a copolymer synthetic resin of acrylonitrile, acrylate, and styrene), or the like.

[0152] The plastic (resin) to be used preferably includes polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polylactic acid ester; acrylic resins such as polymethyl methacrylate (PMMA); polycarbonate (PC); PC / ABS; polyvinyl chloride; polyamide; polyimide; polyamideimide; polyetherimide; polyacetal; polyether ether ketone; cyclic polyolefins having a norbornene skeleton; polyphenylene sulfide (PPS); liquid crystal polymer (LCP); modified polyphenyl ether; polysulfone; polyether sulfone (PES); phenol; polyphthalamide (PPA); polyarylate, etc.

[0153] For the plastic (resin), the above may be combined with inorganic compounds such as glass fiber or talc, or rubber, as necessary. The ceramics used are preferably glass, alumina, or the like.

[0154] When a nonwoven fabric is used as the substrate, it is preferable to use a nonwoven fabric made of wood fiber, glass fiber, asbestos, polyester fiber, vinylon fiber, rayon fiber, polyolefin fiber, or the like.

[0155] The shape of the substrate is preferably a plate (or film), a nonwoven fabric (or woven fabric), a thread, or any of various shapes formed by a mold.

[0156] The solvent, binder, etc. contained in the coating composition for electroless plating are appropriately selected according to the substrate.

[0157] Coating Treatment The method for applying the coating composition for electroless plating of the present invention to a substrate is preferably a coating method using a bar coater, a gravure printer (gravure offset), a flexographic printer, an inkjet printer, a dispenser, dipping, spraying, a spin coater, a roll coater, a reverse coater, a screen printer, or the like.

[0158] As the application method, gravure offset printing, pad printing, and a dispenser are preferably adopted from the viewpoints of masking-less, production efficiency, etc. Spray coating is preferably adopted according to the plating pattern.

[0159] The viscosity of the coating composition for electroless plating is adjusted according to the application method.

[0160] When the electroless plating coating composition is applied by gravure offset printing or pad printing, the viscosity of the electroless plating coating composition is preferably about 50 mPa·s to 1,000 mPa·s.

[0161] When the coating composition for electroless plating is applied with a dispenser, or when it is spray-applied after masking, the viscosity of the coating composition for electroless plating is preferably about 100 mPa·s or less.

[0162] The thickness of the coating composition for electroless plating before drying and curing is appropriately selected depending on the intended use and depends on the viscosity of the coating composition for electroless plating. The thickness of the coating composition for electroless plating before drying and curing is preferably about 1 μm to 120 μm, more preferably about 10 μm to 100 μm, from the viewpoint of being able to apply the coating composition for electroless plating well and preventing dripping of the coating composition for electroless plating.

[0163] Hardening Treatment After the coating composition for electroless plating is applied to the substrate, the solvent contained in the coating composition for electroless plating is evaporated and / or dried, and then a curing treatment is performed. The binder is cured by the curing treatment.

[0164] After the coating composition for electroless plating is applied to the substrate, a drying treatment is preferably performed. The drying treatment efficiently removes unnecessary solvent when performing electroless plating, and improves the adhesion between the coating film and the substrate and the surface strength of the coating film. The temperature of the drying treatment is preferably about 60°C to 400°C, and more preferably about 80°C to 150°C. The time of the drying treatment is preferably about 6 seconds to 60 minutes, and more preferably about 10 minutes to 30 minutes, depending on the drying temperature.

[0165] The temperature of the curing treatment is appropriately adjusted according to the type of the (3) binder resin contained in the coating composition for electroless plating. The temperature of the curing treatment is preferably about 40° C. to 400° C. When a plastic is used as the substrate, the temperature of the curing treatment is preferably set to about 40° C. to 200° C., taking into consideration the softening temperature of the plastic material.

[0166] The film thickness of the coating composition for electroless plating after drying and curing depends on the solid content concentration of the coating composition for electroless plating. From the viewpoint of efficient electroless plating (good reaction rate of electroless plating) and good plating adhesion, the film thickness of the coating composition for electroless plating after drying and curing is preferably about 0.05 μm to 20 μm, more preferably 1 μm to 5 μm.

[0167] Alkaline Treatment The solvent contained in the coating composition for electroless plating is evaporated and / or dried, and the binder contained in the coating composition for electroless plating is cured, and then the substrate to which the coating composition for electroless plating has been applied is subjected to an alkali treatment.

[0168] The alkali treatment can dissolve and / or remove the nanoparticles in the outermost layer that are not coated with the binder resin, thereby exposing the nanoparticle layer coated with the binder component of a thin film in the next layer (the layer below the outermost layer).

[0169] By carrying out a series of these treatments using the coating composition for electroless plating of the present invention, a coating film (ink film) of the coating composition for electroless plating can be formed on a substrate. The ink film contains a Pd complex. The Pd complex is present in a state of being uniformly dispersed in the coating film. By using the coating composition for electroless plating of the present invention, electroless plating can be carried out on the ink film more efficiently.

[0170] Electroless plating After the alkali treatment, the ink film is washed with water and then electroless plating is performed, allowing plating (pattern plating) to be formed on the substrate. The substrate with the ink film formed is then contacted with a plating solution to deposit metal, forming an electroless plating film. The ink film has good reactivity to electroless plating, is uniform, and has excellent adhesion and appearance.

[0171] The plating solution used is generally a plating solution used in electroless plating. The plating solution used is preferably copper, gold, silver, nickel, chromium, etc. More preferably, the plating solution used is a plating solution containing copper or nickel.

[0172] The plating conditions are the same as in the conventional method. The ink film of the present invention has very good electroless plating reactivity, so there is no need to increase the reducing agent concentration or alkaline component concentration of the plating solution. Therefore, not only does the plating solution last a long time, but the plating is selectively deposited according to the ink pattern. The ink film (a coating film formed using the electroless plating coating composition of the present invention) has excellent pattern forming ability.

[0173] When an electroless copper plating bath is used in the electroless plating process, the treatment temperature is preferably about 25° C. to 65° C., and the treatment time is preferably about 10 minutes to 20 minutes. This electroless plating process forms a deposit film with a thickness of about 0.3 μm to 1.0 μm.

[0174] When an electroless nickel boron bath is used in the electroless plating process, the treatment temperature is preferably about 55 to 70° C., and the deposition rate is preferably about 5 μm / hr (60° C.).

[0175] When an electroless nickel-phosphorus bath is used in the electroless plating process, the treatment temperature is preferably about 30°C to 95°C, and the deposition rate is preferably about 3 μm / hr at a bath temperature of 30°C and about 20 μm / hr at 90°C.

[0176] The technique of forming a plating on a substrate using the coating composition for electroless plating of the present invention is preferably used for full surface plating or pattern plating.

[0177] For decorative purposes, after electroless plating, a common process such as electrolytic copper plating, semi-bright nickel plating, bright nickel plating, or chrome plating is preferably used.

[0178] When an electrolytic copper plating bath is used in the decorative treatment, the treatment temperature is preferably about 20°C to 60°C, and the current density is preferably 1 A / m 2 ~10A / m 2 The treatment time is preferably about 10 to 60 minutes. This decoration treatment forms a deposition film having a thickness of about 5 μm to 40 μm.

[0179] When a semi-bright nickel plating bath is used in the decorative treatment, the treatment temperature is preferably about 45°C to 55°C, and the current density is preferably 1 A / m 2 ~10A / m 2 The treatment time is preferably about 10 to 60 minutes. This decorative treatment results in a deposited film thickness of about 5 μm to 20 μm.

[0180] When a bright nickel plating bath is used in the decorative treatment, the treatment temperature is preferably about 45°C to 55°C, and the current density is preferably 1 A / dm 2 ~10A / dm 2The treatment time is preferably about 10 to 60 minutes. This decorative treatment results in a deposited film thickness of about 5 μm to 20 μm.

[0181] When a chrome plating bath is used in the decorative treatment, the treatment temperature is preferably about 40°C to 60°C, and the current density is preferably 10 A / m 2 ~60A / m 2 The treatment time is preferably about 1 to 5 minutes. This decoration treatment results in a deposition film thickness of about 0.1 μm to 0.3 μm.

[0182] [3] Electroless plating film and molded products with the film The electroless plating coating composition of the present invention can improve the pot life after blending by adjusting the binder resin to a specific content.

[0183] The electroless plating coating composition of the present invention has a binder resin that is adjusted to a specific resin content, and when electroless plating is performed using this electroless plating coating composition, the drying time of the plating can be shortened.

[0184] The coating composition for electroless plating of the present invention is applied to a substrate to form an ink film, and electroless plating is then performed. The molded article (subject to be plated) on which the electroless plating film is formed has excellent adhesion of the plating film.

[0185] Molded articles having electroless plating films thereon are used, for example, in the housings of electrical appliances such as mobile phones, personal computers, and refrigerators; and in automotive parts such as emblems, switch bases, radiator grilles, door handles, and wheel covers.

[0186] By using the coating composition for electroless plating of the present invention, in electroless plating on a substrate (plastic (resin) etc.), the reactivity of the electroless plating is high, and excellent adhesion that can withstand multi-layer plating up to chrome plating and excellent smoothness that can withstand decorative plating can be achieved. In electroless plating, the spread of the pattern is suppressed, and good partial plating can be achieved.

[0187] When the coating composition for electroless plating of the present invention is used, it is not necessary to increase the concentration of the reducing agent in electroless plating in order to improve the reactivity of electroless plating, nor is it necessary to increase the reaction temperature of electroless plating.Furthermore, there is no need for an etching process using harmful substances, a complicated catalyst application process, etc.

[0188] The reason why the coating composition for electroless plating of the present invention has high reactivity to electroless plating and can realize good adhesion capable of withstanding multi-layer plating up to chrome plating is believed to be due to the following principle. First, the adhesion mechanism between the substrate (plastic, etc.) and the ink composition is as follows. The substrate surface is eroded by the solvent component contained in the coating composition for electroless plating of the present invention, and the binder resin of the coating composition for electroless plating penetrates into the substrate and becomes compatible with the substrate to form a hybrid layer. For example, in the case of ABS resin, the butadiene rubber contained in the ABS resin dissolves and swells, so that the binder resin of the coating composition for electroless plating penetrates into the substrate.

[0189] The mechanism of the improvement in reactivity and adhesion of electroless plating is as follows. By treating a substrate coated with the coating composition for electroless plating of the present invention with alkali, the nanoparticles in the outermost layer that are not coated with a binder resin are dissolved and / or dropped off. This causes the nanoparticle layer thinly coated with the binder component of the next layer (the layer below the outermost layer) below the outermost layer to be exposed. As a result, the frequency of contact between the Pd particles, which have catalytic activity for electroless plating and are contained in the thin binder coating that covers this nanoparticle layer, and the electroless plating solution increases.

[0190] In addition, the alkali treatment creates gaps between the nanoparticles and the binder components, which causes capillary action in the gaps, improving the permeability of the plating solution into the ink film and increasing the frequency of contact between the Pd particles and the electroless plating solution. Due to this phenomenon, the metal ions in the electroless plating solution are reduced by the Pd particles that exist deep inside the ink film from the surface, and the reduced metal precipitates from inside the film like roots, resulting in high adhesion between the ink film and the plating film. EXAMPLES

[0191] The present invention will be specifically described below with reference to examples and comparative examples.

[0192] The present invention is not limited to the following specific examples.

[0193] [1] Preparation of a composite of palladium particles (Pd particles) and a dispersant (Pd composite) In a 3L flask, 944.5g of ion-exchanged water and 5.0g of palladium nitrate were added and stirred to prepare an aqueous solution of palladium nitrate. 3.8g of a block copolymer-type polymer dispersant having a carboxyl group (DISPERBYK194, manufactured by BYK Japan, non-volatile content 53wt%) was further added to the aqueous solution of palladium nitrate to dissolve the palladium nitrate.

[0194] The solution was heated to 42°C, and 10.0 g of hydrazine monohydrate was added while stirring. The solution was then stirred at room temperature (23°C) for 1 hour. The temperature of the solution rose to 53°C after the addition of hydrazine monohydrate, but after stirring for 1 hour, the temperature of the solution was 40°C.

[0195] This operation reduced the palladium ions (Pd ions) in the aqueous solution. This solution was separated into a reduced Pd complex-containing solution and an inorganic salt-containing solution using an ultrafiltration filter AHP-1010 (manufactured by Asahi Kasei Corporation) to obtain a Pd complex-containing solution (a complex of Pd particles and a dispersant).

[0196] The Pd complex-containing liquid was rotated for 16 hours at a rotation speed of 13,000 G load using a centrifuge to settle the solids. The resulting supernatant was removed by decantation, and then N-methylpyrrolidone (NMP) was added in an amount equal to the weight of the removed supernatant. This operation was repeated several times to obtain a complex of Pd particles and a dispersant (Pd complex) with NMP as the dispersion medium.

[0197] [2] Preparation of electroless plating coating composition of the embodiment In the examples, the binder resin contained a polyamide resin and an epoxy resin, and the amount of the epoxy resin added in 100 parts by mass (total amount) of the binder resin was prepared to be more than 0 and 20 parts by weight (20% by weight) or less.

[0198] Example 1 (10% by mass of epoxy resin in binder resin) To 14 parts by weight of 2-phenoxyethanol, 1.9 parts by weight of phenylsilane-treated silica nanoparticles having an average particle size of 50 nm (Admatechs' Admanano YA050C-SP3) were added, and the mixture was stirred with a medicine spoon (small) to disperse.

[0199] To this nanoparticle dispersion solution, 5 parts by mass of binder resin (a binder resin containing 90 parts by mass of polyamide resin and 10 parts by mass of epoxy resin in 100 parts by mass (total amount) of binder resin) and 1 part by mass of the Pd complex were added, and the mixture was shaken and stirred to prepare a coating composition for electroless plating.

[0200] Example 2 (20% by mass of epoxy resin in binder resin) To this nanoparticle dispersion solution, 5 parts by mass of binder resin (a binder resin containing 80 parts by mass of polyamide resin and 20 parts by mass of epoxy resin in 100 parts by mass (total amount) of binder resin) and 1 part by mass of the Pd complex were added, and the mixture was shaken and stirred to prepare a coating composition for electroless plating.

[0201] Example 3 (5% by mass of epoxy resin in binder resin) To this nanoparticle dispersion solution, 5 parts by mass of binder resin (a binder resin containing 95 parts by mass of polyamide resin and 5 parts by mass of epoxy resin in 100 parts by mass (total amount) of binder resin) and 1 part by mass of the Pd complex were added, and the mixture was shaken and stirred to prepare a coating composition for electroless plating.

[0202] As a result, a coating sample of the electroless plating coating composition of the embodiment was obtained.

[0203] [3] Preparation of electroless plating coating composition of comparative example In the comparative examples, the binder resin contained a polyamide resin and an epoxy resin, and the amount of the epoxy resin added in 100 parts by mass (total amount) of the binder resin was prepared to be 0 (no addition) or more than 20 parts by weight (20% by weight).

[0204] Comparative Example 1 (epoxy resin: 0% by mass in binder resin) An electroless plating coating composition was prepared in the same manner as in Example 1, except that in the electroless plating coating composition of Example 1, 5 parts by mass of a binder resin (a binder resin containing 100 parts by mass of polyamide resin and 0 parts by mass of epoxy resin in 100 parts by mass (total amount) of binder resin) was used.

[0205] Comparative Example 2 (Epoxy resin: 30% by mass in binder resin) An electroless plating coating composition was prepared in the same manner as in Example 1, except that in the electroless plating coating composition of Example 1, 5 parts by mass of a binder resin (a binder resin containing 70 parts by mass of a polyamide resin and 30 parts by mass of an epoxy resin in 100 parts by mass (total amount) of the binder resin) was used.

[0206] Comparative Example 3 (Epoxy resin: 40% by mass in binder resin) An electroless plating coating composition was prepared in the same manner as in Example 1, except that in the electroless plating coating composition of Example 1, 5 parts by mass of a binder resin (a binder resin containing 60 parts by mass of a polyamide resin and 40 parts by mass of an epoxy resin in 100 parts by mass (total amount) of the binder resin) was used.

[0207] Comparative Example 4 (100% modified epoxy resin in binder resin) An electroless plating coating composition was prepared in the same manner as in Example 1, except that in the electroless plating coating composition of Example 1, 5 parts by mass of a commercially available modified epoxy resin (Alonmighty BX-60) was used as the binder resin.

[0208] [4] Coating conditions The obtained coating composition for electroless plating was applied using a bar coater to obtain a coated sample.

[0209] Coating conditions (1) The electroless plating coating composition was applied to a flat plate made by injection molding of polycarbonate resin (Teijin Panlite 2151) as a raw material using a bar coater (OSG System Products Co., Ltd., A-bar #6) and dried at 120°C for 10 minutes.

[0210] Coating conditions (2) The electroless plating coating composition was applied to a flat plate made by injection molding of polycarbonate resin (Teijin Panlite 2151) as a raw material using a bar coater (OSG System Products Co., Ltd., A-bar #6) and dried at 120°C for 2 minutes.

[0211] Coating conditions (3) The coating composition for electroless plating was applied to a flat plate made by injection molding using polycarbonate resin (Teijin Panlite 2151) as the raw material, 20 days after mixing, using a bar coater (OSG System Products Co., Ltd., A-bar #6) and dried at 120°C for 10 minutes.

[0212] Coating conditions (4) The electroless plating coating composition was applied to a flat plate made by injection molding acrylic resin (Acrylite L manufactured by Mitsubishi Chemical) as a raw material using a bar coater (A-bar #6 manufactured by OSG System Products Co., Ltd.), and dried at 80°C for 30 minutes.

[0213] [5] Plating conditions Plating Conditions (1) The samples coated with the coating compositions for electroless plating obtained under the coating conditions (1), (2), and (3) were immersed for 3 minutes in an alkaline treatment solution adjusted to pH 11 to pH 14 and heated to 45° C. Thereafter, the samples were washed with city water and replaced with ion-exchanged water.

[0214] Next, the sample coated with the coating composition for electroless plating was immersed in an electroless copper plating bath to evaluate the appearance after plating.

[0215] Furthermore, the obtained electroless copper plated sample was subjected to electrolytic copper plating and dried at 120° C. for 30 minutes.

[0216] The electrolytic copper plating bath was 80g / L copper sulfate, 150g / L sulfuric acid, and 5mL / L Cu-brite manufactured by JCU Corporation. The plating conditions were 25°C, 1A / dm 2 ×3 minutes, 4A / dm 2 × 27 minutes, a 25 μm copper plating film was formed.

[0217] A cutter knife was used to make a 10 mm wide cut in this electrolytic copper plating film, and the peel strength (N / cm) was measured using a peel strength tester (digital force gauge ZTA-DPU, manufactured by IMADA Co., Ltd.).

[0218] Plating Conditions (2) The coated sample of the coating composition for electroless plating obtained under coating condition (4) was immersed for 3 minutes in an alkaline treatment liquid adjusted to pH 11 to pH 14 and heated to 45° C. Thereafter, it was washed with city water and replaced with ion-exchanged water.

[0219] Next, the sample coated with the coating composition for electroless plating was immersed in an electroless nickel plating bath, washed with water, and dried for 30 minutes at 80° C. The appearance of the obtained sample after plating and the adhesion were evaluated by a cross-cut test.

[0220] [6] Evaluation test Appearance after plating ◯: Appearance after plating is metallic (copper, nickel) color. ×: The appearance after plating is black due to insufficient deposition.

[0221] Back blackening after plating When forming wiring for display applications on transparent substrates such as polycarbonate and acrylic, the wiring on the back surface (the surface seen from the substrate side) needs to be blackened to suppress glossy reflection.

[0222] ◯: The rear surface of the plated product was blackened and the product was black in appearance. ×: The appearance after plating is not blackened on the back side and has a copper luster.

[0223] Peel strength of plating The peel strength of the electroless plating coating composition coated sample was evaluated by a 90° peel test method. A 10 mm wide plated film was peeled off, and one end of the film was held by a tensile jig of a tensile tester (IMADA digital force gauge ZTS-50N). The other end of the plated film that had not been peeled off was held by another tensile jig, and a tensile test was performed at a test speed of 25 mm / min.

[0224] The maximum load was taken as the peel strength and the adhesion was evaluated.

[0225] ⊚: Average peel strength is 5 N / cm or more. ◯: Average peel strength is 3N / cm to 5N / cm. ×: The average peel strength is 3 N / cm or less.

[0226] Cross-cut test On the obtained nickel plating film, 25 squares were cut at 1 mm intervals based on JIS K 5600 (cross-cut method). Cellophane tape (Cellotape (registered trademark), manufactured by Nichiban Co., Ltd.) was applied on the cuts, and the number of squares that remained when the tape was peeled off was counted.

[0227] As an example, in the table, "25 / 25" indicates that all 25 squares have not peeled off, and "2 / 25" indicates that 23 squares have peeled off and the remaining 2 squares have not peeled off.

[0228] Cross-cut test comprehensive evaluation : Appearance after plating is "good", back surface blackening after plating is "good", average peel strength is 5N / cm or more. Good: Appearance after plating is "good", back surface blackening after plating is "good", average peel strength is 3N / cm or more.

[0229] [Table 1]

[0230] [Table 2]

[0231] From the results in Table 2, in Comparative Example 4 (modified epoxy resin), when the drying time after preparation was shortened (from 10 minutes to 2 minutes), the peel strength was low.

[0232] From the results in Table 2, when electroless plating is performed using the coating composition for electroless plating of the embodiment (present invention), good plating adhesion is obtained even when the drying time is shortened to 2 minutes (from 10 minutes to 2 minutes), so the drying time of the plating can be shortened.

[0233] [Table 3]

[0234] From the results in Table 3, in Comparative Example 4 (modified epoxy resin), as time passed after preparation (ink immediately after preparation → ink after 20 days), the peel strength was low, and the appearance after plating was black due to insufficient precipitation, and the back surface did not blacken.

[0235] From the results in Table 3, it can be seen that the electroless plating coating composition of the embodiment (present invention) has a longer pot life after formulation (ink immediately after preparation → ink after 20 days), which indicates that the pot life after formulation can be improved.

[0236] [Table 4]

[0237] From the results in Table 4, when electroless plating is performed using the coating composition for electroless plating of the embodiment (present invention), good plating adhesion is obtained even when the drying time is lowered to 80°C (120°C → 80°C), so that a good plating film can be formed even on substrates with low heat resistance.

[0238] [7] Industrial Applicability The electroless plating coating composition of the present invention can improve the pot life after blending by adjusting the binder resin to a specific content.

[0239] The electroless plating coating composition of the present invention has a binder resin that is adjusted to a specific resin content, and when electroless plating is performed using this electroless plating coating composition, the drying time of the plating can be shortened.

Claims

1. A coating composition for electroless plating, comprising: (1) A composite of palladium particles and a dispersant, (2) Solvent, and (3) Binder resin Contains The coating composition for electroless plating (3), wherein the binder resin comprises a polyamide resin and an epoxy resin, and the amount of the epoxy resin added per 100 parts by weight of the binder resin is more than 0 and not more than 20 parts by weight.

2. (4) further comprising nanoparticles; The (4) nanoparticles are surface-treated, 2. The coating composition for electroless plating according to claim 1, wherein the amount of the nanoparticles (4) added is 0.01 to 100 parts by weight per 1 part by weight of the binder resin (3).

3. 3. The coating composition for electroless plating according to claim 2, wherein the nanoparticles (4) are inorganic oxides.

4. 4. The coating composition for electroless plating according to claim 2 or 3, wherein the nanoparticles (4) have an average particle size of 10 nm to 1,000 nm.

5. 4. The coating composition for electroless plating according to claim 2 or 3, wherein the nanoparticles (4) are silicon dioxide.

6. 3. A method for forming an electroless plating on a substrate by using the coating composition for electroless plating according to claim 1 or 2 and carrying out a coating treatment, a curing treatment, an alkali treatment and an electroless plating treatment.

Citation Information

Patent Citations

  • Film for electroless plating

    JP2019116673A

  • Electroless plating primer composition, laminate using the same and method for manufacturing the same

    JP2022154466A

  • Feedback amplifying circuit with FET switch circuit

    JP1979022812A