Resin composition, cured body and method for producing the same, sealant, adhesive, and disassemblable adhesive
A solvent-free resin composition using polyphenylene ether and epoxy resin with specific hydrocarbon groups addresses viscosity and dielectric challenges, ensuring low water absorption and improved processing fluidity for electronic applications.
Patent Information
- Application Number
- JP2023044643
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing epoxy resin compositions require high-temperature melting and large amounts of solvent to reduce viscosity, leading to challenges in processing and solvent resistance, while also needing improved dielectric properties for electronic applications.
A resin composition comprising polyphenylene ether with a glass transition temperature of -100°C to 50°C, mixed with an epoxy resin, allowing solvent-free processing and maintaining low dielectricity and water absorption, achieved by adjusting the content ratio and incorporating specific hydrocarbon groups.
The composition achieves adjustable viscosity, solvent resistance, low water absorption, and improved fluidity during processing without solvents, enhancing dielectric properties for electronic applications.
Smart Images

Figure 2024134377000001 
Figure 2024134377000002 
Figure 2024134377000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a cured product and a method for producing the same, a sealant, an adhesive, and a dismantlable adhesive. [Background technology]
[0002] Conventionally, prepregs made of glass cloth impregnated with epoxy resin etc. have been mainly used as insulating materials for electronic components. In the next generation of high speed communications, transmission loss is on the rise due to the use of high frequencies, so low dielectric epoxy resin compositions are being studied to reduce transmission loss. In addition, in recent years, with the expansion of the market for liquid epoxy resin compositions such as liquid sealing materials, underfill materials, adhesives, etc., there is a growing need for solvent-free liquid curing agents and modifiers that have excellent low flow, low water absorption, and low dielectric properties while maintaining the solvent resistance of the cured product. Polyphenylene ether (hereinafter, also referred to as "PPE") is known as a modifier for improving low dielectric tangent, low water absorption, heat resistance, etc., and is widely used as a material for products and parts in the electrical and electronic fields, automotive fields, and food and packaging fields, as well as in various other industrial materials. In particular, taking advantage of its low dielectric properties, it is being applied as a modifier in various applications, such as electrical and electronic applications such as substrate materials.
[0003] Epoxy resins come in a wide range of specifications, from low-viscosity liquids to solids with high viscosity when molten, and it is necessary to increase or decrease the viscosity according to the manufacturing conditions for impregnating the base material and the curing conditions, etc. Viscosity adjusters are required to have a low dielectric tangent, be capable of reacting with epoxy resins, and not be extracted from the cured product, and it is known to add mixtures of two or more epoxy resins with different viscosities, high molecular weight bisphenol A epoxy resins (phenoxy resins), etc. However, in recent years, the demand for electrical insulation properties has become increasingly severe, and there is a demand for viscosity modifiers for epoxy resins with low water absorption and low dielectric constant. For example, Patent Documents 1 and 2 disclose epoxy resin compositions containing phenoxy resins with lower dielectric constant and lower dielectric loss tangent.
[0004] Furthermore, when polyphenylene ether is used for printed wiring boards, etc., it is used after being dissolved in an organic solvent. However, it is known that high molecular weight polyphenylene ether having a repeating unit derived from a monohydric phenol, such as 2,6-dimethylphenol, is difficult to dissolve at high concentrations at room temperature even in aromatic solvents such as toluene, which are known to be good solvents, although it is soluble in highly toxic solvents such as chloroform. Therefore, Patent Document 3 discloses an epoxy resin composition in which a low molecular weight polyphenylene ether is mixed with an epoxy resin at a high temperature of 220 to 260° C. without using a solvent. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-101449 A [Patent Document 2] JP 2007-277333 A [Patent Document 3] Special Publication No. 2003-527462 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the phenoxy resins and polyphenylene ethers used as modifiers for epoxy resins as disclosed in Patent Documents 1 to 3 are solid, and thus have the problem that a preparation method is required in which a solution is prepared using a large amount of solvent to reduce the viscosity, or the epoxy resin itself is melted at high temperature.
[0007] The present invention has been made in consideration of the above problems, and has an object to provide a resin composition containing polyphenylene ether and an epoxy resin, which is viscosity adjustable, has low water absorption and low dielectric properties while maintaining the solvent resistance of the cured product, and further has improved fluidity during processing without the use of a solvent, a cured product and a method for producing the same, a sealant, an adhesive, and a dismantlable adhesive. [Means for solving the problem]
[0008] That is, the present invention is as follows. [1] A resin composition comprising: a polyphenylene ether having a glass transition temperature of −100° C. to 50° C. as measured by differential scanning calorimetry (DSC); and an epoxy resin. [2] The resin composition according to the above [1], wherein the polyphenylene ether has a saturated or unsaturated hydrocarbon group having 7 to 25 carbon atoms which may be substituted. [3] The resin composition according to [2] above, wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (1): [ka] (In formula (1), R 13 represents an optionally substituted saturated or unsaturated hydrocarbon group having 15 carbon atoms; R 11 and R 12 are each independently a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, or a substituent represented by the following formula (3), 11 and R 12 None of the are hydrogen atoms.) [ka] (In formula (3), R 31 each independently forms a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or two R 31 The atoms in R are bonded to each other to form a cyclic alkyl group having 1 to 8 carbon atoms. 32each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group. [4] R in the above formula (1) 11 is a substituent represented by formula (3). [5] The resin composition according to the above [4], wherein the substituent represented by the formula (3) is a t-butyl group. [6] The resin composition according to the above [3], characterized in that the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (2) in addition to the repeating unit derived from the phenol represented by the formula (1): [ka] (In formula (2), R 21 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 22 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. [7] The polyphenylene ether contains, relative to a total of 100 mol % of the repeating units derived from the phenol represented by the formula (1) and the repeating units derived from the phenol represented by the formula (2), The content of the repeating unit derived from the phenol of the formula (1) is 51 mol % or more and less than 100 mol %, The content of the repeating unit of the formula (2) derived from phenol is more than 0 mol% and not more than 49 mol%. The resin composition according to the above item [6]. [8] The resin composition according to the above [2], wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (4): [ka] ...Equation (4) (In formula (4), R 41 , R 42 , R 43 are each independently a linear saturated hydrocarbon group having 1 to 12 carbon atoms, or an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of an optionally substituted nitrogen atom, an oxygen atom, and a sulfur atom, and R 41 , R 42 , R 43 At least one of the above is an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of optionally substituted nitrogen atoms, oxygen atoms, and sulfur atoms.) [9] The resin composition according to the above [8], characterized in that the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (2) in addition to the repeating unit derived from the phenol represented by the above formula (4): [ka] (In formula (2), R 21 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 22 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
[10] The polyphenylene ether comprises a repeating unit derived from a phenol represented by the formula (4) and a repeating unit derived from a phenol represented by the formula (2), each of which is represented by the formula (4) in a total of 100 mol %. The content of the repeating unit derived from the phenol of the formula (4) is 7 to 50 mol %, The content of the repeating unit derived from the phenol of the formula (2) is 50 to 93 mol %. The resin composition according to the above item [9].
[11] based on the total amount of the polyphenylene ether and the epoxy resin, The content of the polyphenylene ether is 0.5 to 59.0 mass %, The content of the epoxy resin is 41.0 to 99.5% by mass. The resin composition according to any one of the above items [1] to
[10] .
[12] The resin composition according to any one of the above [1] to
[11] , wherein the polyphenylene ether has a weight average molecular weight of less than 60,000.
[13] A cured product comprising the resin composition according to any one of [1] to
[12] above.
[14] A method for producing a cured product, comprising mixing the resin composition according to any one of [1] to
[12] above at 0 to 70°C without using a solvent, and then thermally curing the mixture at 100 to 300°C.
[15] The method for producing a cured product according to the above
[14] , characterized in that in the thermal curing step, a curing accelerator that is liquid at 25°C is used.
[16] A sealant comprising the cured product according to
[13] above.
[17] An adhesive comprising the cured product described in
[13] above.
[18] A dismantlable adhesive comprising the cured product described in
[13] above. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition containing polyphenylene ether and an epoxy resin, which is capable of adjusting the viscosity, has low water absorption and low dielectric properties while maintaining the solvent resistance of the cured product, and further has improved fluidity during processing without the use of a solvent, a cured product and a method for producing the same, a sealant, an adhesive, and a dismantlable adhesive. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The following embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment. The present invention can be practiced by appropriately modifying it within the scope of its gist.
[0011] In this specification, A (numeric value) to B (numeric value) mean greater than or equal to A and less than or equal to B. In addition, in this specification, the term "substituent" refers to, for example, a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a halogen atom, etc.
[0012] In the present embodiment, polyphenylene ether in which some or all of the hydroxyl groups contained in the polyphenylene ether have been modified may be simply referred to as "polyphenylene ether". Therefore, when the term "polyphenylene ether" is used, it includes both unmodified polyphenylene ether and modified polyphenylene ether, unless there is a particular contradiction.
[0013] <Resin composition> The resin composition of the present embodiment contains polyphenylene ether having a glass transition temperature of −100° C. to 50° C. as measured by differential scanning calorimetry (DSC), and an epoxy resin. By using polyphenylene ether having a glass transition temperature of -100°C to 50°C as a modifier, it is possible to more highly balance the fluidity of the resin composition during the curing process and the heat resistance of the cured product. As a result, it becomes possible to adjust the viscosity of the resin composition, and the solvent resistance, low water absorption, and low dielectric properties of the cured product can be well maintained. Furthermore, fluidity during processing can be ensured without the use of a solvent.
[0014] In addition, in the resin composition of the present embodiment, it is preferable that the content of the polyphenylene ether is 0.5 to 59.0 mass% and the content of the epoxy resin is 41.0 to 99.5 mass% relative to the total amount of the polyphenylene ether and the epoxy resin. When the content of the polyphenylene ether is 0.5 mass% or more and the content of the epoxy resin is 99.5 mass% or less, the cured product of the resin composition tends to have lower dielectric properties. Also, when the content of the polyphenylene ether is 59.0 mass% or less and the content of the epoxy resin is 41.0 mass% or more, the curing tends to be better. The viscosity of the resin composition of the present embodiment can be appropriately adjusted according to the processing method and curing conditions by selecting the polyphenylene ether and the epoxy resin.
[0015] (Polyphenylene ether)
[0016] The resin composition of the present embodiment contains polyphenylene ether, and the polyphenylene ether has a glass transition temperature of -100°C to 50°C as measured by DSC. The polyphenylene ether must have a glass transition temperature of −100° C. or higher by DSC, preferably −80° C. or higher, and more preferably −50° C. or higher. When the polyphenylene ether has a glass transition temperature of −100° C. or higher by DSC, the cured product obtained by curing the resin composition can exhibit heat resistance. The polyphenylene ether must have a glass transition temperature of 50° C. or lower by DSC, preferably 25° C. or lower, and more preferably −5° C. or lower. If the polyphenylene ether has a glass transition temperature of 50° C. or lower, the resin composition can maintain sufficient fluidity at a curing temperature of 80 to 300° C.
[0017] As a method for adjusting the glass transition temperature by DSC, for example, the glass transition temperature can be lowered by performing molecular design that weakens the interaction between polymer chains and makes the polymer chains easier to move. Although not particularly limited, for example, the glass transition temperature can be lowered by introducing a repeating unit having a long-chain alkyl group into polyphenylene ether. In addition, the glass transition temperature by DSC can be adjusted by appropriately adjusting the introduction ratio of the repeating unit having a long-chain alkyl group or the chain length of the long-chain alkyl group. The measuring device for measuring the differential scanning calorimetry is not particularly limited, and a commercially available device can be used. For example, the differential scanning calorimetry device can be "DSC250" manufactured by TA Instruments.
[0018] From the viewpoint of achieving a higher compatibility between the fluidity during the curing treatment of the resin composition and the heat resistance of the cured product, the polyphenylene ether preferably has an optionally substituted saturated or unsaturated hydrocarbon group having 7 to 25 carbon atoms. From the viewpoint of improving the heat resistance of the cured product obtained by curing the resin composition of the present embodiment, the polyphenylene ether preferably has a saturated or unsaturated hydrocarbon group having 20 or less carbon atoms, more preferably having 15 carbon atoms. Furthermore, from the viewpoint of maintaining sufficient fluidity at the curing temperature (about 80 to 300°C) of the resin composition, the polyphenylene ether more preferably has a saturated or unsaturated hydrocarbon group having 8 or more carbon atoms, and further preferably has 9 or more carbon atoms.
[0019] The polyphenylene ether may contain a repeating unit derived from phenol represented by the following formula (1). [ka] In the above formula (1), R 11 and R 12 are each independently at least one selected from the group consisting of a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, and a substituent represented by formula (3). However, R11 and R 12 None of the groups can be hydrogen atoms. Preferred R 11 and R 12 are each independently at least one selected from a hydrogen atom, a methyl group, an ethyl group, and a substituent represented by formula (3). 11 is a substituent represented by formula (3). Particularly preferably, R 11 is a substituent represented by formula (3), and R 12 is a hydrogen atom.
[0020] [ka] (In formula (3), R 31 are each independently a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or two R 31 The atoms contained therein are bonded to each other to form a cyclic alkyl group having 1 to 8 carbon atoms, and R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group. The substituent represented by the above formula (3) is preferably a group containing secondary and / or tertiary carbon, such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a tert-amyl group, a 2,2-dimethylpropyl group, a cyclohexyl group, and a group in which the hydrogen of the terminal hydrocarbon group in these groups is replaced with a phenyl group. More preferably, the substituent represented by the above formula (3) is a tert-butyl group or a cyclohexyl group, and even more preferably a tert-butyl group. Furthermore, the atoms contained in these groups may be bonded to each other to form a ring structure.
[0021] In the resin composition of the present embodiment, R 11 is a t-butyl group, and R 12is preferably a hydrogen atom.
[0022] In the above formula (1), R 13 is an optionally substituted saturated or unsaturated hydrocarbon group having 15 carbon atoms, preferably R 13 C 15 H 31-2n (each n is independently an integer of 0 to 3).
[0023] The polyphenylene ether may contain a repeating unit derived from a phenol of formula (2) in addition to the repeating unit derived from a phenol of formula (1). [ka] (In formula (2), R 21 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 22 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
[0024] In addition, in the above formula (2), R 21 are each independently preferably a saturated hydrocarbon group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, more preferably a methyl group or a phenyl group, and further preferably a methyl group. 21 Preferably, both have the same structure.
[0025] Furthermore, in the above formula (2), R 22 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, more preferably a hydrogen atom or a methyl group. 22 may be the same or different. In a preferred embodiment, two R 22and one of them is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (more preferably a methyl group).
[0026] In this embodiment, the structure of the polyphenylene ether can be identified by analyzing the polyphenylene ether by techniques such as NMR and mass spectrometry. As a specific method for identifying the structure of the polyphenylene ether, it is possible to carry out field desorption mass spectrometry (FD-MS), which is known to be less prone to fragmentation, and estimate the repeating units based on the intervals between the detected ions. In addition, there is a method for estimating the structure of the polyphenylene ether by combining peak analysis of fragment ions by electron ionization (EI) and structural analysis by NMR. 1 It can be determined using analytical techniques such as H NMR. More specifically, the structure of the polyphenylene ether can be identified by the method described in the Examples below.
[0027] In addition, in the polyphenylene ether, the content of the repeating unit derived from phenol of the above formula (1) is preferably 51 mol% or more and less than 100 mol%, and the content of the repeating unit derived from phenol of the above formula (2) is preferably more than 0 mol% and 49 mol% or less, relative to 100 mol% in total of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2).
[0028] Furthermore, from the viewpoint of making the composition liquid at room temperature, the content ratio of the repeating unit derived from phenol of the above formula (1) relative to the total 100 mol % of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2) is preferably 51 mol % or more, more preferably 55 mol % or more, and even more preferably 60 mol % or more. Furthermore, from the viewpoint of further exhibiting the heat resistance of the cured product of the resin composition of this embodiment, the content ratio of the repeating unit derived from phenol of the above formula (1) to the total of 100 mol % of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2) is more preferably 95 mol % or less, and even more preferably 90 mol % or less.
[0029] The content of the repeating unit derived from the phenol of the above formula (2) can be appropriately selected depending on the application. For example, when it is desired to adjust the viscosity to a higher level, it is preferable that the repeating unit derived from the phenol of the above formula (2) is more.
[0030] In this embodiment, the total molar ratio of the repeating units derived from phenol of the above formula (1) and the repeating units derived from phenol of the above formula (2) relative to 100 mol% of the polyphenylene ether is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more, and may be 100 mol%.
[0031] The molar ratio of the repeating unit derived from phenol of the above formula (1) and the molar ratio of the repeating unit derived from phenol of the above formula (2) relative to the total of 100 mol % of the repeating unit derived from phenol of the above formula (1) and the repeating unit derived from phenol of the above formula (2) are, for example, 1 H-NMR, 13 It can be determined using an analytical technique such as C-NMR, and more specifically, it can be measured by the method described in the Examples below.
[0032] In addition, since the phenol of the above formula (2) does not have an unsubstituted ortho position (i.e., since no hydrogen atoms are bonded to the two carbon atoms at the ortho positions relative to the carbon atom to which the hydroxyl group is bonded), it can react with another phenolic monomer predominantly at the carbon atoms at the para positions to the phenolic hydroxyl group. Therefore, the repeating unit derived from the phenol of the above formula (2) includes a repeating unit having the structure of the following formula (5). [ka] (In formula (5), R 21 and R 22 is R in Eq. (2) 21 and R 22 is the same as
[0033] The content of the repeating unit having the structure of formula (5) in the repeating unit derived from the phenol of formula (2) above on a molar basis is preferably 90% or more, more preferably 95% or more, even more preferably 99%, and may be 100%.
[0034] On the other hand, R of phenol in the above formula (1) 11 and R 12 are each independently a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, or a substituent represented by the above formula (3) (wherein R 11 and R 12 None of the groups can be hydrogen atoms), R 11 and R 12 When either of is a hydrogen atom, in addition to the phenolic hydroxyl group, it can react with another phenolic monomer at either the ortho or para position of the phenol. Therefore, the repeating unit derived from the phenol of the above formula (1) can contain at least one selected from the group consisting of a structural unit of the following formula (6), a structural unit of the following formula (7), and a structural unit of the following formula (8). [ka] [ka] [ka] (R in Equation (6), Equation (7), and Equation (8) 11 , R 12 , R 13 is R in the above formula (1). 11 , R 12 , R 13 is equivalent to.)
[0035] In the repeating units derived from the phenol of the formula (1), the total content on a molar basis of the structural units of the formula (6), the structural units of the formula (7) and the structural units of the formula (8) is preferably 90% or more, more preferably 95% or more, even more preferably 99%, and may be 100%.
[0036] The polyphenylene ether of the present embodiment may contain a repeating unit derived from phenol, as represented by the following formula (4). [ka] In the above formula (4), R 41 , R 42 , R 43 are each independently a linear saturated hydrocarbon group having 1 to 12 carbon atoms, and an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of an optionally substituted nitrogen atom, an oxygen atom, and a sulfur atom; R 41 , R 42 , R 43 At least one of these is an organic group having 7 to 25 carbon atoms and having at least one atom selected from the group consisting of a nitrogen atom, an oxygen atom, and a sulfur atom.
[0037] In the above formula (4), R 41 , R 42 , R 43 At least one of the above is preferably an organic group having 8 to 20 carbon atoms and a sulfur atom, and more preferably an organic group having 9 to 15 carbon atoms and a sulfur atom.
[0038] Specifically, the phenol of the above formula (4) is preferably 4,6-bis(octylthiomethyl)-o-cresol or 4,6-bis(dodecylthiomethyl)-o-cresol.
[0039] Furthermore, the polyphenylene ether of the present embodiment may contain a repeating unit derived from a phenol of the above formula (2), in addition to the repeating unit derived from a phenol of the formula (4).
[0040] In the polyphenylene ether of the present embodiment, the content of the repeating unit derived from phenol of the above formula (4) is preferably 7 to 50 mol % and the content of the repeating unit derived from phenol of the above formula (2) is preferably 50 to 93 mol % relative to 100 mol % in total of the repeating unit derived from phenol of the above formula (4) and the repeating unit derived from phenol of the above formula (2).
[0041] From the viewpoint of making the composition liquid at room temperature, the content ratio of the repeating unit derived from phenol of the above formula (4) relative to the total 100 mol % of the repeating unit derived from phenol of the above formula (4) and the repeating unit derived from phenol of the above formula (2) is preferably 7 mol % or more, more preferably 10 mol % or more, and even more preferably 15 mol % or more. From the viewpoint of further improving the heat resistance of the cured product of the resin composition, the content ratio of the repeating unit derived from phenol of the above formula (4) relative to the total 100 mol % of the repeating unit derived from phenol of the above formula (4) and the repeating unit derived from phenol of the above formula (2) is preferably 50 mol % or less, more preferably 30 mol % or less, and even more preferably 20 mol % or less.
[0042] The content of the repeating unit derived from the phenol of the above formula (2) can be appropriately selected depending on the application. For example, when it is desired to adjust the viscosity to a higher level, it is preferable that the repeating unit derived from the phenol of the above formula (2) is more.
[0043] In this embodiment, the total molar ratio of the repeating units derived from phenol of the above formula (4) and the repeating units derived from phenol of the above formula (2) is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 95 mol% or more, and may be 100 mol% based on 100 mol% of the polyphenylene ether.
[0044] The molar ratio of the repeating unit derived from the phenol of the above formula (4) and the repeating unit derived from the phenol of the above formula (2) relative to the total of 100 mol % of the repeating unit derived from the phenol of the above formula (4) and the repeating unit derived from the phenol of the above formula (2) is, for example, 1 H-NMR, 13 It can be determined using analytical techniques such as C-NMR.
[0045] The repeating unit derived from phenol of the above formula (4) has a structural unit of the following formula (9) and can be added to the end of a polyphenylene ether. [ka] (R in Equation (9) 41 , R 42 , R 43 is R in the above formula (4). 41 , R 42 , R 43 is equivalent to.)
[0046] The polyphenylene ether in the present embodiment preferably has a weight average molecular weight of less than 60,000, more preferably less than 40,000, and even more preferably less than 20,000, from the viewpoint of fluidization.
[0047] The polyphenylene ether in the present embodiment may have at least one partial structure selected from the group consisting of a partial structure of the following formula (10), a partial structure of the following formula (11), a partial structure of the following formula (12), and a partial structure of the following formula (13). [ka] [ka] [ka] (In formula (12), R 4 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 4 may have a substituent within the range of a total carbon number of 1 to 10.) [ka] (In formula (13), R 5 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon is R 5 may have a substituent within a range in which the total carbon number of R is 1 to 10; 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 6 may have a substituent within the range of a total carbon number of 1 to 10.)
[0048] At least one partial structure selected from the group consisting of the partial structure of formula (10), the partial structure of formula (11), the partial structure of formula (12), and the partial structure of formula (13) may be introduced by a modification step described later, and may be directly bonded to an oxygen atom of a hydroxyl group contained in the polyphenylene ether.
[0049] (Production method of polyphenylene ether) The polyphenylene ether of the present embodiment can be obtained, for example, by a method including at least a step of oxidatively polymerizing a monovalent raw material phenol containing the phenol of the above formula (1). The step of oxidatively polymerizing is preferably a step of oxidatively polymerizing raw material phenols containing the phenol of the above formula (1) and the phenol of the above formula (2).
[0050] Examples of the phenol of the above formula (1) include 3-pentadecylphenol, commercially available cardanol, modified 3-pentadecylphenol obtained by introducing a linear saturated hydrocarbon group having 1 to 12 carbon atoms or a substituent represented by the above formula (3) into 3-pentadecylphenol, and modified cardanol obtained by introducing a linear saturated hydrocarbon group having 1 to 12 carbon atoms or a substituent represented by the above formula (3) into commercially available cardanol. The substituent to be introduced into the 3-pentadecylphenol or commercially available cardanol is preferably R 11 By introducing a bulky substituent such as a tert-butyl group or a cyclohexyl group into R 11 and R 12 It is preferable to introduce a methyl group into both R 11 and R 12 Examples of a method for introducing a substituent into include A) a method of reacting with an alkyl halide in the presence of a Lewis acid, and B) a method of reacting with isobutene or the like in the presence of a Bronsted acid. The phenol of the formula (1) may be used alone or in combination of two or more kinds.
[0051] Examples of the phenol of the above formula (2) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, 2,3,6-trimethylphenol, 2,3-diethyl-6-n-propylphenol, 2,3,6-tributylphenol, 2,6-di-n-butyl-3-methylphenol, 2,6-dimethyl-3-n-butylphenol, and 2,6-dimethyl-3-t-butylphenol. Among these, 2,6-dimethylphenol, 2,3,6-trimethylphenol, and 2,6-diphenylphenol are particularly preferable since they are inexpensive and easily available. The phenol of the above formula (2) may be used alone or in combination of two or more kinds.
[0052] The polyphenylene ether can be obtained by a method including at least a step of oxidatively polymerizing a monovalent raw material phenol including the phenol of the formula (4) above. The step of oxidatively polymerizing is preferably a step of oxidatively polymerizing raw material phenol including the phenol of the formula (4) above and the phenol of the formula (2) above.
[0053] As the phenol of the above formula (4), commercially available products such as 4,6-bis(octylthiomethyl)-o-cresol and 4,6-bis(dodecylthiomethyl)-o-cresol are preferred.
[0054] Here, in the method for producing polyphenylene ether, an aromatic solvent that is a good solvent for polyphenylene ether can be used as the polymerization solvent in the oxidative polymerization step. Here, a good solvent for polyphenylene ether is a solvent capable of dissolving polyphenylene ether. Examples of such solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p-isomers) and ethylbenzene; halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; and nitro compounds such as nitrobenzene.
[0055] As the polymerization catalyst used in this embodiment, a known catalyst system that can be generally used for the production of polyphenylene ether can be used. A generally known catalyst system is one that is composed of a transition metal ion having redox ability and an amine compound that can form a complex with the transition metal ion, such as a catalyst system composed of a copper compound and an amine compound, a catalyst system composed of a manganese compound and an amine compound, a catalyst system composed of a cobalt compound and an amine compound, etc. Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or an additional amine compound may be added thereto.
[0056] The polymerization catalyst preferably used in the present embodiment is a catalyst containing a copper compound, a halogen compound, and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (14) as the amine compound. [ka] (In formula (14), R 14 , R 15 , R 16 , R 17 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, but are not all hydrogen atoms at the same time. 18 is a linear or methyl-branched alkylene group having 2 to 5 carbon atoms.
[0057] Examples of the copper compound of the catalyst component described herein are listed below. Suitable copper compounds include cuprous compounds, cupric compounds, and mixtures thereof. Examples of cupric compounds include, for example, cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate. Examples of cuprous compounds include, for example, cuprous chloride, cuprous bromide, cuprous sulfate, and cuprous nitrate. Particularly preferred metal compounds among these are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide. These copper salts may be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and the like and corresponding halogens or acids. A method that is often used is to mix the cuprous oxide exemplified above with hydrogen halide (or a solution of hydrogen halide) to prepare the copper salt.
[0058] Examples of the halogen compounds include hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, and tetraethylammonium iodide. These compounds can be used as an aqueous solution or a solution using a suitable solvent. These halogen compounds can be used alone as a component, or in combination of two or more kinds. Preferred halogen compounds are an aqueous solution of hydrogen chloride and an aqueous solution of hydrogen bromide.
[0059] The amount of these compounds used is not particularly limited, but is preferably 2 to 20 times the number of moles of halogen atoms relative to the number of moles of copper atoms, and the amount of copper atoms used is preferably in the range of 0.02 to 0.6 moles per 100 moles of the phenol compound added to the polymerization reaction.
[0060] Next, examples of the diamine compound of the catalyst component are listed below. For example, N,N,N',N'-tetramethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, Nn-propylethylenediamine, N,N'-n-propylethylenediamine, Ni-propylethylenediamine, N,N'-i-propylethylenediamine, Nn-butylethylenediamine, amine, N,N'-n-butylethylenediamine, Ni-butylethylenediamine, N,N'-i-butylethylenediamine, Nt-butylethylenediamine, N,N'-t-butylethylenediamine, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N'-trimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diamino-1-methylpropane, N,N,N',N'-tetramethyl-1,3-diamino-2-methylpropane, N,N,N',N'-tetramethyl-1,4-diaminobutane, and N,N,N',N'-tetramethyl-1,5-diaminopentane. A preferred diamine compound for this embodiment is one in which the number of carbon atoms in the alkylene group connecting the two nitrogen atoms is 2 or 3. The amount of these diamine compounds used is not particularly limited, but is preferably in the range of 0.01 mol to 10 mol per 100 mol of the phenol compound added to the polymerization reaction.
[0061] In this embodiment, the polymerization catalyst may contain a primary amine and a secondary monoamine as a component thereof. Examples of the secondary monoamine include, but are not limited to, dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-t-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-ethylaniline, N-butylaniline, N-methyl-2-methylaniline, N-methyl-2,6-dimethylaniline, and diphenylamine.
[0062] The polymerization catalyst may also contain a tertiary monoamine compound as a component thereof. The tertiary monoamine compound is an aliphatic tertiary amine including an alicyclic tertiary amine. Examples of the tertiary monoamine compound include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used alone or in combination of two or more. The amount of these compounds used is not particularly limited, but is preferably in the range of 15 moles or less relative to 100 moles of the phenol compound added to the polymerization reaction.
[0063] In this embodiment, there is no limitation on adding a surfactant that has been known to have an effect of improving polymerization activity. Examples of such surfactants include trioctylmethylammonium chloride, known under the trade names Aliquat 336 and Capriquat. The amount of the surfactant used is preferably within a range not exceeding 0.1% by mass relative to the total amount (100% by mass) of the polymerization reaction mixture.
[0064] As the oxygen-containing gas in the polymerization of this embodiment, in addition to pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any ratio, air, or a mixture of air and an inert gas such as nitrogen in any ratio can be used. Normal pressure is sufficient for the pressure in the system during the polymerization reaction, but reduced or increased pressure can be used as necessary.
[0065] The polymerization temperature is not particularly limited, but if it is too low, the reaction does not proceed easily, and if it is too high, the reaction selectivity may decrease or gel may be formed, so it is in the range of 0 to 60°C, preferably 10 to 40°C.
[0066] In the process for producing polyphenylene ether, the polymerization can also be carried out in a poor solvent such as an alcohol.
[0067] In this embodiment, there is no particular restriction on the post-treatment method after the polymerization reaction is completed. Usually, an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc. are added to the reaction liquid to deactivate the catalyst. In addition, a method for removing and treating the dihydric phenol by-product generated by the polymerization of polyphenylene ether can be performed using a conventionally known method. If the metal ions, which are the catalyst, are substantially deactivated as described above, the mixture can be decolorized simply by heating it. Alternatively, a method of adding a required amount of a known reducing agent is also possible. Examples of known reducing agents include hydroquinone and sodium dithionite.
[0068] In the method for producing polyphenylene ether, water may be added to extract the compound that has deactivated the copper catalyst, and then the organic phase and the aqueous phase are separated into liquid-liquid separation, and the aqueous phase is removed to remove the copper catalyst from the organic phase. This liquid-liquid separation step is not particularly limited, and may include methods such as static separation and separation by a centrifuge. In order to promote the liquid-liquid separation, a known surfactant or the like may be used.
[0069] Next, in the method for producing polyphenylene ether, the organic phase containing the polyphenylene ether after liquid-liquid separation may be concentrated and dried by volatilizing the solvent.
[0070] The method for volatilizing the solvent contained in the organic phase is not particularly limited, but examples thereof include a method of transferring the organic phase to a high-temperature concentration tank and distilling off the solvent to concentrate it, a method of distilling off toluene using an apparatus such as a rotary evaporator, etc. From the viewpoint of suppressing thermal deterioration due to heating, low-temperature concentration under reduced pressure is more preferable.
[0071] The temperature of the drying treatment in the drying step is preferably at least 60° C. or higher, more preferably 80° C. or higher, and even more preferably 110° C. or higher. When the polyphenylene ether is dried at a temperature of 60° C. or higher, the content of high-boiling-point volatile components in the polyphenylene ether powder can be efficiently reduced.
[0072] In order to obtain the polyphenylene ether with high efficiency, a method of increasing the drying temperature, a method of increasing the degree of vacuum in the drying atmosphere, a method of stirring during drying, and the like are effective, but in particular, a method of increasing the drying temperature is preferable from the viewpoint of production efficiency. In the drying step, it is preferable to use a dryer equipped with a mixing function. Examples of the mixing function include a stirring type dryer and a rolling type dryer. This allows the processing amount to be increased, and the productivity to be maintained at a high level.
[0073] The polyphenylene ether of this embodiment can also be produced by a redistribution reaction in which a polyphenylene ether derived from a phenol of the above formula (2) is equilibrated with a phenolic compound of the above formula (1) or the above formula (4) in the presence of an oxidizing agent. Redistribution reactions are known in the art and are described, for example, in U.S. Patent No. 3,496,236 to Cooper et al. and U.S. Patent No. 5,880,221 to Liska et al.
[0074] There is no limitation on the method for introducing a functional group into a hydroxyl group of an unmodified polyphenylene ether. For example, the functional group can be obtained by a reaction of a hydroxyl group of an unmodified polyphenylene ether with a carboxylic acid having a carbon-carbon double bond (hereinafter, carboxylic acid) to form an ester bond. The ester bond can be formed by various known methods, such as a) a reaction between a carboxylic acid halide and a hydroxyl group at the polymer terminal, b) a reaction with a carboxylic acid anhydride to form an ester bond, c) a direct reaction with a carboxylic acid, and d) a method using an ester exchange reaction. The reaction of a with an carboxylic acid halide is one of the most common methods. Although chlorides and bromides are generally used as carboxylic acid halides, other halogens may also be used. The reaction may be either a direct reaction with a hydroxyl group or a reaction with an alkali metal salt of a hydroxyl group. In the direct reaction of a carboxylic acid halide with a hydroxyl group, an acid such as hydrogen halide is generated, so a weak base such as an amine may be used in order to trap the acid. In the reaction of b with a carboxylic acid anhydride or the direct reaction of c with a carboxylic acid, a compound such as a carbodiimide or dimethylaminopyridine may be coexisted in order to activate the reaction site and promote the reaction. In the case of the transesterification reaction of d, it is desirable to remove the generated alcohols as necessary. In addition, known metal catalysts may be used to promote the reaction. After the reaction, the reaction mixture may be washed with water, an acidic or alkaline aqueous solution to remove by-products such as amine salts, or the polymer solution may be dropped into a poor solvent such as alcohols to recover the target product by reprecipitation. After washing the polymer solution, the solvent may be distilled off under reduced pressure to recover the polymer.
[0075] The method for producing the modified polyphenylene ether is not limited to the method for producing the polyfunctional modified polyphenylene ether of the present embodiment described above, and the order and number of the above-mentioned oxidative polymerization step, copper extraction and by-product removal step, liquid-liquid separation step, and concentration / drying step may be appropriately adjusted.
[0076] The polyphenylene ether of the present embodiment may be obtained by oxidatively polymerizing 3-pentadecylphenol or commercially available cardanol, and optionally 2,6-dimethylphenol as the phenol of formula (2), and then introducing at least one partial structure selected from the group consisting of formulas (10), (11), (12), and (13) into the obtained polyphenylene ether. The polyphenylene ether of the present embodiment may be obtained by oxidatively polymerizing 3-pentadecylphenol or commercially available cardanol as the phenol of formula (1), and optionally 2,6-dimethylphenol as the phenol of formula (2). The polyphenylene ether of the present embodiment may be obtained by oxidative polymerization of modified 3-pentadecylphenol or modified cardanol as the phenol of formula (1) and, optionally, 2,6-dimethylphenol as the phenol of formula (2), and then introducing at least one partial structure selected from the group consisting of formulas (10), (11), (12), and (13) into the obtained polyphenylene ether.
[0077] Further, for example, the polyphenylene ether of the present embodiment may be obtained by oxidative polymerization of 4,6-bis(octylthiomethyl)-o-cresol or 4,6-bis(dodecylthiomethyl)-o-cresol as the phenol of formula (4), and optionally 2,6-dimethylphenol as the phenol of formula (2), and then introducing at least one partial structure selected from the group consisting of formulas (10), (11), (12), and (13) into the obtained polyphenylene ether.
[0078] (Epoxy resin) The resin composition according to the present embodiment contains an epoxy resin in addition to the polyphenylene ether described above. The epoxy resin is not particularly limited as long as it is an epoxy resin having one or more epoxy groups in one molecule. From the viewpoint of expressing the heat resistance of the cured product, an epoxy resin containing two or more epoxy groups is preferable. Examples of epoxy resins having one epoxy group in one molecule include phenyl glycidyl ether, phenol poly(n=2-8) ethylene oxide glycidyl ether, para-t-butylphenyl glycidyl ether, N-glycidyl phthalimide, and dibromophenyl glycidyl ether. Examples of epoxy resins having two or more epoxy groups in one molecule include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, etc. The epoxy resin composition may contain one or more types of epoxy resins. Among them, bisphenol A type epoxy resins and bisphenol F type epoxy resins, especially bisphenol A type epoxy resins, are preferably used. Such epoxy resins are commercially available.
[0079] The epoxy resin may be either solid or liquid depending on the intended use. As the liquid epoxy resin, an epoxy resin having a small number of repeating units in the main chain may be selected, and examples of the liquid epoxy resin include liquid bisphenol A type epoxy resin and liquid bisphenol F type epoxy resin.
[0080] The epoxy resin has a viscosity at 25° C. of preferably 5 to 30 Pa·s, more preferably 5 to 25 Pa·s, and even more preferably 5 to 20 Pa·s. The epoxy resin composition may contain one type of epoxy resin or two or more types of epoxy resins.
[0081] The resin composition according to the present embodiment contains a curing agent in addition to the polyphenylene ether and the epoxy resin, and may further contain a peroxide, a thermoplastic resin, a flame retardant, and other additives as desired. The components of the resin composition containing a solvent according to the present embodiment are described below.
[0082] (Cure accelerator) In the resin composition of the present embodiment, in addition to the polyphenylene ether and epoxy resin described above, a curing accelerator can be used. For example, it can be selected from imidazoles, amines, organic phosphines, phenolic resins, etc. Specific examples include 1-methylimidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-dimethylaminopyridine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, triphenylphosphine, tributylphosphine, tris-2,6-dimethoxyphenylphosphine, tri-p-tolylphosphine, o-cresol novolac, phenol novolac, allylated phenol novolac, and bisphenol A novolac. The curing accelerator may be used alone or in combination of two or more kinds. As the curing agent, a curing accelerator that is liquid at 25° C. is preferable because it can improve the workability at room temperature and the dispersibility in the resin composition. Specific examples include 1-methylimidazole, allylated phenol novolak, etc.
[0083] (Crosslinking agent) In the resin composition of the present embodiment, any crosslinking agent capable of initiating or accelerating a crosslinking reaction can be used. The crosslinking agent preferably has a number average molecular weight of 4,000 or less. When the number average molecular weight of the crosslinking agent is 4,000 or less, the increase in viscosity of the resin composition containing the solvent can be suppressed, and good resin fluidity can be obtained during heat molding. The number average molecular weight may be a value measured by a general molecular weight measurement method, and specifically, a value measured using GPC can be mentioned.
[0084] From the viewpoint of crosslinking reaction, the crosslinking agent preferably has an average of two or more carbon-carbon unsaturated double bonds in one molecule. The crosslinking agent may be composed of one type of compound, or may be composed of two or more types of compounds. In this specification, the term "carbon-carbon unsaturated double bond" refers to a double bond located at an end branched from the main chain when the crosslinking agent is a polymer or oligomer. An example of the carbon-carbon unsaturated double bond is a 1,2-vinyl bond in polybutadiene.
[0085] When the number average molecular weight of the crosslinking agent is less than 600, the number (average) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 2 to 4. When the number average molecular weight of the crosslinking agent is 600 or more and less than 1,500, the number (average) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 4 to 26. When the number average molecular weight of the crosslinking agent is 1,500 or more and less than 4,000, the number (average) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 26 to 60. When the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or more than the specific value, so that the resin composition containing the solvent of this embodiment has higher reactivity of the crosslinking agent and higher crosslink density of the cured product of the resin composition, and as a result, can be imparted with better heat resistance. On the other hand, when the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or less than the specific value, so that better resin fluidity can be imparted during hot molding.
[0086] Examples of the crosslinking agent include trialkenyl isocyanurate compounds such as triallyl isocyanurate (TAIC), trialkenyl cyanurate compounds such as triallyl cyanurate (TAC), polyfunctional methacrylate compounds having two or more methacrylic groups in the molecule, polyfunctional acrylate compounds having two or more acrylic groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule such as polybutadiene, vinylbenzyl compounds such as divinylbenzene having a vinylbenzyl group in the molecule, polyfunctional maleimide compounds having two or more maleimide groups in the molecule such as 4,4'-bismaleimide diphenylmethane, polyfunctional acrylates having two or more acrylic groups in the molecule such as tricyclodecane dimethanol diacrylate, polyfunctional methacrylates having two or more acrylic or methacrylic groups in the molecule such as tricyclodecane dimethanol dimethacrylate, etc. These crosslinking agents can be used alone or in combination of two or more. Among these, the crosslinking agent preferably contains at least one compound selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, tricyclodecane dimethanol dimethacrylate, and polybutadiene.
[0087] (organic peroxide) In this embodiment, any organic peroxide capable of promoting the polymerization reaction of the polyphenylene ether and the crosslinking agent may be used. Examples of the organic peroxides include benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. In addition, radical generators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for the resin composition. Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di(2-t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are preferred from the viewpoint of providing a cured product having excellent heat resistance and mechanical properties and a low dielectric tangent (preferably also a low dielectric constant).
[0088] The one-minute half-life temperature of the organic peroxide is preferably 155 to 185° C., more preferably 160 to 180° C., and further preferably 165 to 175° C. In this specification, the one-minute half-life temperature is the temperature at which the organic peroxide decomposes and the amount of active oxygen is reduced to half in one minute. The one-minute half-life temperature is a value confirmed by a method in which an organic peroxide is dissolved in a solvent inactive against radicals, such as benzene, to a concentration of 0.05 to 0.1 mol / L, and the organic peroxide solution is thermally decomposed in a nitrogen atmosphere.
[0089] When the polyphenylene ether-containing resin composition is subjected to heat and pressure molding, the polyphenylene ether is sufficiently melted before reaction with the crosslinking agent is started, and thus the moldability tends to be excellent. On the other hand, when the organic peroxide has a one-minute half-life temperature of 185°C or less, the decomposition speed of the organic peroxide is sufficient under normal heat and pressure molding conditions (e.g., maximum temperature of 200°C), and therefore the crosslinking reaction with the crosslinking agent can be efficiently and slowly progressed, and thus a cured product having good electrical properties (especially dielectric tangent) can be formed.
[0090] Here, examples of organic peroxides having a one-minute half-life temperature in the range of 155 to 185°C include t-hexylperoxyisopropyl monocarbonate (155.0°C), t-butylperoxy-3,5,5-trimethylhexanoate (166.0°C), t-butylperoxylaurate (159.4°C), t-butylperoxyisopropyl monocarbonate (158.8°C), t-butylperoxy 2-ethylhexyl monocarbonate (161.4°C), t-hexylperoxybenzoate (160.3°C), 2,5-dimethyl-2,5-di(benzoylperoxy)hexane (158. 2°C), t-butyl peroxyacetate (159.9°C), 2,2-di-(t-butylperoxy)butane (159.9°C), t-butyl peroxybenzoate (166.8°C), n-butyl 4,4-di-(t-butylperoxy)valerate (172.5°C), di(2-t-butylperoxyisopropyl)benzene (175.4°C), dicumyl peroxide (175.2°C), di-t-hexyl peroxide (176.7°C), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (179.8°C), and t-butylcumyl peroxide (173.3°C).
[0091] (thermoplastic resin) The resin composition of the present embodiment preferably contains a thermoplastic resin. The thermoplastic resin is preferably at least one selected from the group consisting of a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound and a hydrogenated product thereof (a hydrogenated block copolymer obtained by hydrogenating a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound), and a homopolymer of a vinyl aromatic compound.
[0092] The content of the vinyl aromatic compound-derived units in the block copolymer or its hydrogenated product is preferably 20% by mass or more, more preferably 22% by mass or more, and can be 99% by mass or less. When the content of the vinyl aromatic compound-derived units in the block copolymer or its hydrogenated product is 20% by mass or more, the compatibility with polyphenylene ether is further improved, and the adhesive strength with the metal foil tends to be further improved.
[0093] The vinyl aromatic compound may have an aromatic ring and a vinyl group in the molecule, and may be, for example, styrene, etc. The olefin-based alkene compound may have a linear or branched structure in the molecule, and may be, for example, ethylene, propylene, butylene, isobutylene, butadiene, isoprene, etc. Among these, from the viewpoint of even better compatibility with polyphenylene ether, the thermoplastic resin is preferably at least one selected from the group consisting of styrene-butadiene block copolymers, styrene-ethylene-butadiene block copolymers, styrene-ethylene-butylene block copolymers, styrene-butadiene-butylene block copolymers, styrene-isoprene block copolymers, styrene-ethylene-propylene block copolymers, styrene-isobutylene block copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-ethylene-butadiene block copolymers, hydrogenated styrene-butadiene-butylene block copolymers, hydrogenated styrene-isoprene block copolymers, and homopolymers of styrene (polystyrene), and more preferably at least one selected from the group consisting of styrene-butadiene block copolymers, hydrogenated styrene-butadiene block copolymers, and polystyrene.
[0094] The hydrogenation rate in the hydrogenated product is not particularly limited, and some of the carbon-carbon unsaturated double bonds derived from the olefin-based alkene compound may remain.
[0095] The weight average molecular weight of the thermoplastic resin is preferably 10,000 to 300,000, more preferably 20,000 to 290,000, and further preferably 30,000 to 280,000. By having a weight average molecular weight of 10,000 or more, the resin composition of the present embodiment tends to have better heat resistance when cured. By having a weight average molecular weight of 300,000 or less, the resin composition of the present embodiment tends to have better resin fluidity during heat molding. The weight average molecular weight may be a value measured by a general molecular weight measurement method, and specifically, a value measured using GPC or the like may be mentioned.
[0096] The resin composition of the present embodiment may also contain a thermoplastic resin other than the thermoplastic resin having the type and weight average molecular weight described above.
[0097] (Flame retardant) The resin composition of the present embodiment preferably further contains a flame retardant. The flame retardant is not particularly limited as long as it is incompatible with other components contained in the resin composition after the resin composition is cured, from the viewpoint of improving heat resistance. Preferably, the flame retardant is incompatible with polyphenylene ether and / or crosslinking agent in the resin composition after the resin composition is cured. Examples of the flame retardant include inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylene bistetrabromophthalimide; and phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis-dixylenyl phosphate. These flame retardants may be used alone or in combination of two or more. Among these, the flame retardant is preferably decabromodiphenylethane from the viewpoints of compatibility between the flame retardant and the modified polyphenylene ether, coatability of the resin composition, and superior properties of the mounted electronic circuit board.
[0098] The content of the flame retardant is not particularly limited, but from the viewpoint of maintaining flame retardancy at V-0 level of UL Standard 94, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the total of the polyphenylene ether resin and the crosslinking agent. Moreover, from the viewpoint of maintaining a low dielectric tangent of the obtained cured product (preferably also maintaining a low dielectric constant), the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.
[0099] (Silica filler) The resin composition of the present embodiment may further contain a silica filler. Examples of the silica filler include natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica. The content of the silica filler may be 10 to 100 parts by mass per 100 parts by mass of the total of the polyphenylene ether and the crosslinking agent. The silica filler may be surface-treated with a silane coupling agent or the like.
[0100] In addition to the above-mentioned components, the resin composition of the present embodiment may further contain additives such as a heat stabilizer, an antioxidant, a UV absorber, a surfactant, and a lubricant.
[0101] <Cured body> The cured product of the present embodiment can be obtained by curing the resin composition of the present embodiment. For example, the resin composition of the present embodiment can be mixed without substantially using a solvent, and then thermally cured at 100 to 300° C. to obtain a cured product of the resin composition of the present embodiment. The mixing conditions for the resin composition when obtaining a cured product are not particularly limited, but are preferably 0 to 70° C., more preferably 0 to 50° C., and even more preferably 0 to 30° C. Mixing the resin composition at around room temperature improves handleability. Furthermore, when curing the resin composition of the present embodiment, a curing accelerator that is liquid at 25° C. can be used. If the curing accelerator is liquid, it can be uniformly dispersed in the resin composition when the resin composition is mixed at around room temperature.
[0102] <Sealant> The sealant of the present embodiment includes the cured product of the resin composition of the present embodiment described above, and can be used for various applications. For example, it can be used as a resin composition for semiconductor encapsulation for semiconductor packages. Examples of methods for encapsulating semiconductor packages include transfer molding and underfill methods. The epoxy resin composition for encapsulation is preferably in the form of a liquid, powder, granule, tablet, or sheet. In the case of the transfer molding method, the sealant is charged in tablet form, so it must basically be solid. From the viewpoints of heat resistance, moisture resistance, and flame retardancy, brominated epoxy, cresol novolac epoxy, biphenyl epoxy, and naphthol novolac epoxy are preferred. From the same viewpoint, phenol novolac, aralkyl novolac, dicyclopentadiene phenol, and trisphenol methane are preferred as hardeners. In the case of the die and fill method and underfill method, the epoxy resin must be basically liquid. From the viewpoint of heat resistance and moisture resistance, bisphenol A type epoxy and naphthalene epoxy are preferred, and naphthalene epoxy is more preferred. As the curing agent, acid anhydrides such as 4-methylcyclohexane-1,2-dicarboxylic anhydride and methylnadic acid, and aromatic amines such as Kayahard AA manufactured by Nippon Kayaku and JER-W manufactured by Mitsubishi Chemical are preferred.
[0103] <Adhesives, dismantlable adhesives> The adhesive of this embodiment includes the cured product of the resin composition of this embodiment and can be used for various applications. For example, it can be used as a resin composition for adhesives for building materials, vehicles (automotive industry, etc.), and the electrical and electronics industry. It can also be used as a dismantlable adhesive that can be applied to the recycling of the target components that are bonded and that enables advanced resource recycling in various industries. A dismantlable adhesive is an epoxy resin adhesive that has excellent adhesive strength properties and heat resistance, while allowing the bonded body to be easily dismantled after the use of the adhesive / bonding components.
[0104] The dismantlable adhesive of this embodiment includes a cured product of the resin composition of this embodiment described above, and as a characteristic thereof, the glass transition temperature is preferably 80°C or higher, more preferably 100°C or higher, in order to improve heat resistance. In addition, considering that the adhesive cured product is thermally softened and dismantled at 120 to 250°C, which is higher than the use environment temperature and the glass transition temperature of the resin composition, the storage modulus at 250°C is preferably 80 MPa or lower, more preferably 50 MPa or lower, and even more preferably 20 MPa or lower. The storage modulus can be adjusted by lowering the filling rate of inorganic fillers such as silica. When used as a resin composition for dismantlable adhesives, it may contain thermally expandable microcapsules and expandable graphite to improve dismantling properties. Thermally expandable graphite generally refers to graphite that has the property of expanding by several times to several hundred times its original volume when heated. Thermally expandable microcapsules are fine particles in which liquid gas is enclosed in a polymer membrane, and are particles that dramatically expand in volume when heated by increasing the gas pressure inside the shell and softening the polymer membrane.
[0105] The reason why the resin composition of this embodiment maintains a high glass transition temperature while the storage modulus drops significantly above the glass transition temperature is considered to be as follows. By adding monofunctional polyphenylene ether to a bifunctional or higher epoxy resin, the crosslink density is reduced, and the storage modulus at high temperatures can be reduced. On the other hand, by finely dispersing polyphenylene ether with a rigid main chain in the epoxy resin matrix, a significant drop in the glass transition temperature of the epoxy resin matrix can be suppressed. EXAMPLES
[0106] Hereinafter, the present embodiment will be described in more detail based on examples, but the present embodiment is not limited to the following examples.
[0107] First, the measurement methods and evaluation criteria for each physical property will be described below. <Analysis of polyphenylene ether> (1) Weight average molecular weight of polyphenylene ether A gel permeation chromatograph (Shimadzu Corporation, LC-2030C Plus) was used as a measuring device, and a calibration curve was prepared using standard polystyrene and ethylbenzene. The weight average molecular weight (Mw) of the modified polyphenylene ether obtained was measured using this calibration curve. Standard polystyrenes with molecular weights of 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550 were used.
[0108] The column used was two Showa Denko K-805L columns connected in series. The solvent used was chloroform, the solvent flow rate was 1.0 mL / min, and the column temperature was 40°C. A 1 g / L chloroform solution of polyphenylene ether was prepared and used as the measurement sample. The UV wavelength of the detection unit was 254 nm for standard polystyrene and 283 nm for polyphenylene ether. The weight average molecular weight was calculated from the peak area ratio based on the curve showing the molecular weight distribution obtained by GPC based on the above measurement data.
[0109] (2) Measurement of glass transition temperature The glass transition temperature of polyphenylene ether was measured using a differential scanning calorimeter DSC250 (TA Instruments). In a nitrogen atmosphere, the sample was heated from -90 to 30°C at a heating rate of 10°C per minute, then cooled to -90°C at a heating rate of 20°C per minute, and the glass transition temperature was then measured at a heating rate of 10°C per minute.
[0110] <Evaluation> (1) Viscosity of resin composition (40°C) The liquid viscosity of the prepared resin composition sample at 40° C. was measured using a viscometer (Kyoto Electronics Manufacturing: EMS-1000S, motor rotation speed 1000 rpm). (2) Liquidity The plates of the cured resin compositions produced in the Examples and Comparative Examples were observed, and the fluidity of the resin compositions was evaluated according to the following criteria. ○: No bubbles were observed in the cured product. ×: Air bubbles were observed in the cured product.
[0111] (3) Toluene immersion test Samples of the cured resin compositions produced in the Examples and Comparative Examples were cut to a width of 5 mm and a length of 50 mm, and then immersed in a sufficient amount of toluene for 24 hours. The weight loss was then evaluated according to the following criteria. ○ (Good): Weight loss before and after immersion is less than 1% by mass × (bad): Weight loss before and after immersion is 1% by mass or more
[0112] (4) Dielectric constant, dielectric tangent, and change in dielectric tangent due to water absorption The dielectric constant and dielectric loss tangent at 10 GHz of the cured samples of the resin compositions produced in the Examples and Comparative Examples were measured by the split cylinder method using a network analyzer (N5227B, manufactured by KEYSIGHT TECHNOLOGIES) and a split cylinder resonator (CR-710, manufactured by EM Lab Co., Ltd.) as measuring devices. A sample of the cured resin composition prepared by the method described below was cut into a plate of 40 mm width, 40 mm length, and approximately 0.5 mm thickness. It was then placed in an oven at 200°C to dry for 1 hour, and immediately after that, the dielectric constant and dielectric loss tangent were measured. The sample was then left to stand for 24±2 hours in an environment at 23°C and a relative humidity of 50±2%.The dielectric constant and dielectric loss tangent were then measured using the above-mentioned measuring device in an environment at 23°C and a relative humidity of 50±2%. The change in dielectric tangent due to water absorption was confirmed by examining the change in dielectric tangent before and after leaving the material to stand for 24±2 hours in an environment of 23°C and 50±2% relative humidity. In other words, the increase in dielectric tangent due to water absorption is suppressed for cured materials with lower water absorption.
[0113] (5) Glass transition temperature, storage modulus at 250°C The glass transition temperature and storage modulus of the cured samples of the resin compositions produced in the Examples and Comparative Examples were analyzed. The measurement was performed using an RSA-G2 (manufactured by TA Instruments) under the following measurement conditions. Sample shape: Length 25mm, width 5mm, thickness 0.5mm Measurement frequency: 1Hz Measurement strain: 0.1% (initial value) Measurement temperature: -80℃~300℃ Heating rate: 10℃ / min Carrier gas: N2
[0114] <Materials used to form the resin composition and its cured product> In the examples and comparative examples described below, the materials shown below were used. (Polyphenylene ether) The polyphenylene ethers obtained in the following Production Examples 2 to 5 were used.
[0115] (Production Example 1) Cardanol (product name NX-2026, manufactured by Cardolite, 345 g) and p-toluenesulfonic acid monohydrate (5.9 g) were added in sequence to a 1 L flask connected to a Dewar condenser at -10°C, and stirred with a stirring blade. Then, the external temperature was set to 80°C using an aluminum block heating device and heated. Isobutene (100 g) was gradually introduced over 10 hours. The supply of isobutene was stopped, and then stirring was continued at 80°C for 15 hours. The temperature of the reaction solution was lowered to 40°C, and toluene (300 g) was added to the reaction solution. Furthermore, a 5% aqueous sodium hydroxide solution (27 g) was dropped. Ion-exchanged water (320 g) was added, the temperature of the reaction solution was raised to 70°C, and after stirring for 30 minutes, the organic layer was collected using a separatory funnel. Ion-exchanged water (760 g) was added to the collected organic layer, the temperature of the reaction solution was raised to 70° C., and the mixture was stirred for 30 minutes and then allowed to stand. The organic layer was collected using a separatory funnel. The washed organic layer was concentrated using a rotary evaporator to obtain a pale yellow oily modified cardanol (370 g). The structure of the obtained compound was identified as follows: 1 The results were analyzed using H-NMR, and it was found that the main component was cardanol with a tert-butyl group introduced at the 2-position of the raw cardanol before the reaction.
[0116] Cardanol Source: 1 H-NMR(CDCl3) δ 7.15-7.10(m,1H),6.78-6.73(m,1H),6.68-6.62(m,2H),5.88-5.77(m,0.37H),5.50-5.29(m,3.44H),5.10-4.95(m,0.80H),4.81-4.64( m,1H),2.88-2.75(m,2.14H),2.55(t,2.13H),2.08-1.98(m,3.31H),1.69-1.53(m,3.15H),1.51-1.12(m,14.10H),0.94-0.85(m,1.95H) Modified Cardanol (Product): 1H-NMR(CDCl3) δ 7.16(d,1H), 6.69(dd,1H),6.49(d,1H),5.88-5.77(m,0.39H),5.50-5.29(m,3.56H),5.10-4.95(m,0.80H),4.64(s,1H),2.87-2.75(m ,2.12H),2.56-2.46(m,2.22H),2.12-1.95(m,3.60),1.65-1.53(m,2.62H),1.43-1.24(m,23.42H),0.96-0.80(m,2.20H)
[0117] (Production Example 2) Synthesis of polyphenylene ether 1 (PPE1) A 1.0-liter jacketed reactor equipped with a line for introducing nitrogen gas at the top of the reactor, a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.033 g of cuprous oxide and 0.248 g of 47% hydrogen bromide, which had been previously prepared, 0.079 g of N,N'-di-t-butylethylenediamine, 1.17 g of dimethyl-n-butylamine, 0.38 g of di-n-butylamine, 6.40 g of 2,6-dimethylphenol, 43.6 g of modified cardanol, 0.05 g of methyltri-n-octylammonium chloride, and 448 g of toluene, while flowing nitrogen gas at a rate of 0.77 L / min. Then, air was introduced into the reactor from the sparger at a rate of 0.53 L / min while vigorously stirring. The polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 40°C. 120 minutes after the start of air introduction, the air flow was stopped, the inside of the reactor was replaced with nitrogen gas, and then 0.35 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added as an aqueous solution of 50 g of water. The mixture was heated to 70°C, and copper extraction was carried out at 70°C for 3 hours. Thereafter, the mixture was separated by standing to separate into a polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The solvent of the organic phase was removed by a rotary evaporator. The liquid polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of each analysis are shown in Table 1.
[0118] (Production Example 3) Synthesis of polyphenylene ether 2 (PPE2) A 1.0 liter jacketed reactor equipped with a line for introducing nitrogen gas at the top of the reactor, a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.11 g of cuprous oxide and 0.83 g of 47% hydrogen bromide, 0.27 g of N,N'-di-t-butylethylenediamine, 3.90 g of dimethyl-n-butylamine, 1.28 g of di-n-butylamine, 12.8 g of 2,6-dimethylphenol, 87.2 g of modified cardanol, 0.05 g of methyltri-n-octylammonium chloride, and 394 g of toluene, while flowing nitrogen gas at a rate of 1.54 L / min. Then, air was introduced into the reactor from the sparger at a rate of 1.05 L / min while vigorously stirring. The polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 40°C. 140 minutes after the start of air introduction, the air flow was stopped, the inside of the reactor was replaced with nitrogen gas, and then 1.18 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added as an aqueous solution of 50 g of water. The mixture was heated to 70°C, and copper extraction was carried out at 70°C for 3 hours. Thereafter, the mixture was separated by standing to separate into a polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The solvent of the organic phase was removed by a rotary evaporator. The liquid polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of each analysis are shown in Table 1.
[0119] (Production Example 4) Synthesis of polyphenylene ether 3 (PPE3) A 1.0-liter jacketed reactor equipped with a line for introducing nitrogen gas at the top of the reactor, a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.068 g of cuprous oxide and 0.511 g of 47% hydrogen bromide, which had been previously prepared, 0.164 g of N,N'-di-t-butylethylenediamine, 2.41 g of dimethyl-n-butylamine, 0.793 g of di-n-butylamine, 43.8 g of 2,6-dimethylphenol, 31.2 g of 4,6-bis(octylthiomethyl)-o-cresol, 0.05 g of methyltri-n-octylammonium chloride, and 421 g of toluene while flowing nitrogen gas at a rate of 1.16 L / min. Then, air was introduced into the reactor from the sparger at a rate of 0.79 L / min while vigorously stirring. The polymerization temperature was adjusted to maintain 40°C by passing a heat medium through the jacket. 120 minutes after the start of air introduction, the air flow was stopped, and the inside of the reactor was replaced with nitrogen gas, after which 0.73 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added as an aqueous solution of 50 g of water. The mixture was heated to 70°C, and copper extraction was carried out at 70°C for 3 hours. Thereafter, the mixture was separated by standing to separate into a polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The solvent of the organic phase was removed by a rotary evaporator. The liquid polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of each analysis are shown in Table 1.
[0120] (Production Example 5) Synthesis of polyphenylene ether 4 (PPE4) A liquid polyphenylene ether was obtained in the same manner as in Production Example 2, except that 3.9 g of 2,6-dimethylphenol and 46.1 g of modified cardanol were used. The liquid polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of each analysis are shown in Table 1.
[0121] (Production Example 6) Synthesis of polyphenylene ether 5 (PPE5) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.092 g of cuprous oxide and 0.69 g of 47% hydrogen bromide, which had been previously prepared, 0.22 g of N,N'-di-t-butylethylenediamine, 3.27 g of dimethyl-n-butylamine, 1.07 g of di-n-butylamine, 714.65 g of toluene, 65.03 g of 2,6-dimethylphenol, and 14.97 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane. Then, air was introduced into the reactor from the sparger at a rate of 0.84 L / min while vigorously stirring, and the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 20°C. 150 minutes after the start of air introduction, the air flow was stopped, and the inside of the reactor was replaced with nitrogen gas. Then, 0.99 g of tetrasodium ethylenediaminetetraacetate tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution of 160 g of water. The mixture was then heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. After that, the mixture was separated by standing separation into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The organic phase was concentrated by a rotary evaporator until the polymer concentration reached 25% by mass. The above solution was mixed with methanol such that the ratio of methanol to polymer solution was 6, and polymer precipitation was performed. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to wet polyphenylene ether was 3. The above washing operation was performed three times. Next, the wet polyphenylene ether was kept at 140°C and 1 mmHg for 120 minutes, and dry polyphenylene ether was obtained. The analytical results are shown in Table 1.
[0122] (Production Example 7) Synthesis of polyphenylene ether 6 (PPE6) In a 40-liter jacketed polymerization tank equipped with a sparger, stirring turbine blades and baffles for introducing oxygen-containing gas at the bottom of the polymerization tank and a reflux condenser on the vent gas line at the top of the polymerization tank, 4.02 g of cupric oxide, 29.876 g of 47 mass% aqueous hydrogen bromide solution, 9.684 g of di-t-butylethylenediamine, 46.88 g of di-n-butylamine, 122.28 g of butyldimethylamine, 17.53 kg of toluene, and 1.5 kg of 2,6-dimethylphenol were added while blowing nitrogen gas at a flow rate of 0.5 L / min, and the mixture was stirred until a homogeneous solution was obtained and the internal temperature of the polymerization tank reached 25° C. Next, dry air was introduced into the polymerization tank from the sparger at a rate of 32.8 NL / min, and at the same time, a solution consisting of 1.62 kg of 2,6-dimethylphenol and 3.12 kg of toluene was added to the polymerization tank over 30 minutes from the plunger pump. Dry air was passed through the reactor for 86 minutes, the air was stopped, and the inside of the reactor was replaced with nitrogen gas. Then, a 20% methanol solution in which 1.03 g of hydroquinone (a reagent manufactured by Wako Pure Chemical Industries, Ltd.) was dissolved was added little by little. Thirty minutes after the addition of the methanol solution of hydroquinone, 1.61 g of tetrasodium ethylenediaminetetraacetate tetrahydrate (a reagent manufactured by Dojindo Laboratories, Ltd.) was added as an aqueous solution of 200 g of water. The mixture was heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. Then, the mixture was separated into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred by static separation. The above solution was mixed with methanol in a ratio of 10 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol in a ratio of 2.5 to the wet polyphenylene ether. The above washing operation was carried out three times. The wet polyphenylene ether was then kept at 140° C. and 1 mmHg for 120 minutes to obtain dry polyphenylene ether. The analytical results are shown in Table 1.
[0123] [Table 1]
[0124] (Epoxy resin) Bisphenol A type epoxy resin (product name: jER828, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of approximately 190 g / eq, liquid at 25°C) was used.
[0125] (Cure accelerator) 1-Methylimidazole (Tokyo Chemical Industry Co., Ltd., liquid at 25°C)
[0126] (Filler) Silica filler (product name SO-C2, manufactured by ADMAFINE) was used.
[0127] The methods for producing polyphenylene ether in each of the Examples and Comparative Examples will be described below. [Example 1] According to the composition shown in Table 2, the epoxy resin, the polyphenylene ether synthesized in Production Example 2, the silica filler, and the curing accelerator were mixed together. Then, the mixture was dispersed using a mixer (THINKY, Model AR-100) to obtain a resin composition. The resin composition was poured into a 5.0 cm × 5.0 cm × 0.5 mm mold and temporarily cured at 130° C. for 2 hours, after which the molded product was removed from the mold and cured at 200° C. for 3 hours to obtain a cured product of the resin composition. The analytical results are shown in Table 2.
[0128] [Example 2] A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except for using 30 parts by mass of the polyphenylene ether synthesized in Production Example 2. The analysis results are shown in Table 2.
[0129] [Example 3] A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except for using the polyphenylene ether synthesized in Production Example 3. The analysis results are shown in Table 2.
[0130] Example 4 A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except for using the polyphenylene ether synthesized in Production Example 5. The analysis results are shown in Table 2.
[0131] [Example 5] A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except that the polyphenylene ether synthesized in Production Example 6 was used and silica was not added as a filler. The analysis results are shown in Table 2.
[0132] [Comparative Example 1] Except for blending the resin composition without adding polyphenylene ether, a resin composition and a cured product thereof were obtained in the same manner as in Example 1. The analytical results are shown in Table 2.
[0133] [Comparative Example 2] A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except for using the polyphenylene ether synthesized in Production Example 6. The analysis results are shown in Table 2.
[0134] [Comparative Example 3] A resin composition and a cured product thereof were obtained in the same manner as in Example 1, except for using the polyphenylene ether synthesized in Production Example 7. The analysis results are shown in Table 2.
[0135] [Table 2]
[0136] As shown in Table 2, the cured products of the resin compositions shown in the Examples have excellent low water absorption and low dielectric properties compared to Comparative Example 1. Furthermore, compared to Comparative Examples 2 and 3, no air bubbles were observed in the cured plate, so the fluidity at 130°C during processing is also excellent. Compared to Comparative Examples 2 and 3, the cured products of the resin compositions shown in each Example were not extracted in a toluene immersion test, and it was confirmed that the cured products maintain their solvent resistance. Furthermore, compared to the resin composition of Comparative Example 1, the resin compositions shown in the Examples can increase the viscosity, and in addition to lowering the dielectric tangent, it is possible to adjust the viscosity of the epoxy resin within a range that does not affect processability, and it has been confirmed that they are useful as viscosity adjusters for epoxy resins. Furthermore, compared to the cured products of the resin compositions of Comparative Examples 1, 2, and 3, the cured products of the resin compositions shown in Examples 1 and 2 are characterized by a low storage modulus at 250°C while maintaining a glass transition temperature of 150°C or higher. For this reason, it was confirmed that they are useful as dismantling adhesives that take advantage of the extreme softening that occurs when heated at high temperatures. [Industrial Applicability]
[0137] The resin composition containing the polyphenylene ether and epoxy resin of the present invention is capable of adjusting its viscosity, and while maintaining the solvent resistance of the cured product, it also has excellent fluidity, low water absorption and low dielectric properties, and has improved handleability and processability, and therefore has industrial utility as an insulating material, sealant, adhesive and dismantlable adhesive used in the electronic and electrical fields.
Claims
1. A resin composition comprising: a polyphenylene ether having a glass transition temperature of −100° C. to 50° C. as measured by differential scanning calorimetry (DSC); and an epoxy resin.
2. 2. The resin composition according to claim 1, wherein the polyphenylene ether has a saturated or unsaturated hydrocarbon group having 7 to 25 carbon atoms which may be substituted.
3. 3. The resin composition according to claim 2, wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (1): 【Chemistry 1】 (In formula (1), R 13 represents an optionally substituted saturated or unsaturated hydrocarbon group having 15 carbon atoms; R 11 and R 12 are each independently a hydrogen atom, a linear saturated hydrocarbon group having 1 to 12 carbon atoms, or a substituent represented by the following formula (3), 11 and R 12 None of the atoms can be hydrogen atoms.) 【Chemistry 2】 (In formula (3), R 31 each independently forms a linear alkyl group having 1 to 8 carbon atoms which may be substituted, or two R 31 The atoms in R are bonded to each other to form a cyclic alkyl group having 1 to 8 carbon atoms. 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.
4. R in the above formula (1) 11 The resin composition according to claim 3 , wherein the substituent is represented by formula (3).
5. The resin composition according to claim 4, wherein the substituent represented by the formula (3) is a t-butyl group.
6. The resin composition according to claim 3, wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (2) in addition to the repeating unit derived from the phenol represented by the formula (1): 【Chemistry 3】 (In formula (2), R 21 are each independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 22 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
7. The polyphenylene ether contains, relative to a total of 100 mol % of the repeating units derived from the phenol of the formula (1) and the repeating units derived from the phenol of the formula (2), The content ratio of the repeating unit derived from the phenol of the formula (1) is 51 mol % or more and less than 100 mol %, The content of the repeating unit of the formula (2) derived from phenol is more than 0 mol % and not more than 49 mol %. The resin composition according to claim 6 .
8. 3. The resin composition according to claim 2, wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (4): 【Chemistry 4】 ...Formula (4) (In formula (4), R 41 , R 42 , R 43 are each independently a linear saturated hydrocarbon group having 1 to 12 carbon atoms, or an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of an optionally substituted nitrogen atom, an oxygen atom, and a sulfur atom; R 41 , R 42 , R 43 At least one of the above is an organic group having 7 to 25 carbon atoms and having one or more atoms selected from the group consisting of optionally substituted nitrogen atoms, oxygen atoms, and sulfur atoms.
9. The resin composition according to claim 8, wherein the polyphenylene ether contains a repeating unit derived from a phenol represented by the following formula (2) in addition to the repeating unit derived from the phenol represented by the formula (4): 【Chemistry 5】 (In formula (2), R 21 are each independently an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 22 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom.
10. The polyphenylene ether has a repeating unit derived from a phenol represented by the formula (4) and a repeating unit derived from a phenol represented by the formula (2) of 100 mol % in total. The content of the repeating unit derived from the phenol of the formula (4) is 7 to 50 mol %, The content of the repeating unit of the formula (2) derived from phenol is 50 to 93 mol %. The resin composition according to claim 9 .
11. relative to the total amount of the polyphenylene ether and the epoxy resin, The content ratio of the polyphenylene ether is 0.5 to 59.0 mass %, The content of the epoxy resin is 41.0 to 99.5% by mass. The resin composition according to claim 2 .
12. The resin composition according to claim 2 , wherein the polyphenylene ether has a weight average molecular weight of less than 60,000.
13. A cured product comprising the resin composition according to any one of claims 1 to 12.
14. A method for producing a cured product, comprising mixing the resin composition according to any one of claims 1 to 12 at 0 to 70°C without using a solvent, and then thermally curing the mixture at 100 to 300°C.
15. The method for producing a cured product according to claim 14, wherein a curing accelerator that is liquid at 25°C is used in the thermal curing step.
16. A sealant comprising the cured product according to claim 13.
17. An adhesive comprising the cured product according to claim 13.
18. A dismantlable adhesive comprising the cured product according to claim 13.
Citation Information
Patent Citations
powder coating composition
JP2003527462A
Resin composition, phenoxy resin, coating material composition, adhesive agent composition, adhesive film, prepreg, multilayer printed wiring board and resin-clad copper foil
JP2007277333A
Phenoxy resin, curable resin composition, cured product thereof, prepreg, circuit board and buildup film
JP2014101449A
Cited By
Rubber composition and method for using polyphenylene ether
WO2025127084A1