Method for manufacturing hollow silica particle

By using sodium silicate and an organic solvent with a lower dielectric constant to form silica shells on calcium carbonate, the method addresses the high cost and toxicity issues of conventional methods, achieving efficient and cost-effective production of hollow silica particles.

JP2024134438APending Publication Date: 2024-10-03NAGOYA INSTITUTE OF TECHNOLOGY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023044744
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for producing hollow silica particles using calcium carbonate as a template involve the use of expensive and toxic silicon alkoxide, leading to high production costs and environmental concerns.

Method used

A method utilizing sodium silicate instead of silicon alkoxide, where the dehydration condensation reaction is facilitated by mixing with an organic solvent having a lower dielectric constant than water, forming a silica shell on calcium carbonate, followed by acid treatment to obtain hollow silica particles.

Benefits of technology

This approach reduces production costs and environmental hazards while effectively forming hollow silica particles with controlled silica shells, enhancing yield and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134438000001_ABST
    Figure 2024134438000001_ABST
Patent Text Reader

Abstract

To provide a silica particle manufacturing method capable of manufacturing hollow silica particles by using calcium carbonate as a template and sodium silicate as a silica source.SOLUTION: The hollow silica particle manufacturing method of the present invention includes: a mixing step S1 of mixing water, an organic solvent soluble in water and having a dielectric constant smaller than that of water, calcium carbonate, and an aqueous solution of sodium silicate in a predetermined ratio; a separation step S2 of separating a solid phase from the mixed solution; and a dissolution step S3 of treating the separated solid phase with acid to dissolve calcium carbonate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing hollow silica particles. [Background technology]

[0002] Hollow inorganic particles have properties such as a high specific surface area, low density, and low thermal conductivity compared to solid inorganic particles, and are therefore used as functional materials such as insulation materials taking advantage of these properties.

[0003] A known method for producing hollow silica particles is the template method, in which a silica film is formed on the surface of calcium carbonate by hydrolyzing silicon alkoxide in a dispersion of calcium carbonate, and then the calcium carbonate is dissolved with an acid to form hollow silica particles (Patent Documents 1 and 2).

[0004] For example, in Patent Document 1, a hydrolysis reaction of silicon alkoxide in a dispersion of calcium carbonate is accelerated by an ammonia catalyst to obtain nano-sized hollow silica particles having a dense silica shell.

[0005] Furthermore, Patent Document 2 discloses a method for producing hollow nano-silica particles that uses sodium carbonate instead of the ammonia catalyst in the method of Patent Document 1, and that has less odor and toxicity. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-263550 A [Patent Document 2] JP 2008-222459 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the conventional method for producing hollow silica particles using calcium carbonate as a template, silicon alkoxide, which is an expensive material, is used as a silica source, which leads to high production costs. In addition, silicon alkoxide is highly toxic, so sufficient care must be taken with regard to the working environment during the production process.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for producing hollow silica particles using calcium carbonate as a template, which is capable of producing hollow silica particles using inexpensive and less toxic sodium silicate without using silicon alkoxide. [Means for solving the problem]

[0009] The present inventors have investigated the use of inexpensive sodium silicate instead of silicon alkoxide, which has been conventionally used as a silica raw material, in a method for producing hollow silica particles using calcium carbonate as a template. However, they found that the silicate ions in the sodium silicate aqueous solution are stabilized by hydration, making it difficult for the dehydration condensation reaction to proceed, and it is therefore difficult to form silica shells with calcium carbonate as the core.

[0010] As a result of further intensive research, the inventors discovered that by mixing an organic solvent with a smaller dielectric constant than water, the dehydration condensation reaction of silicate ions proceeds rapidly, making it possible to form a silica shell on the surface of calcium carbonate, and thus completed the present invention.

[0011] That is, the method for producing hollow silica particles of the present invention is a mixing step of mixing water, an organic solvent that is soluble in water and has a dielectric constant smaller than that of water, calcium carbonate, and an aqueous solution of sodium silicate in a predetermined ratio; A separation step of separating a solid phase from the mixed solution; a dissolving step of treating the separated solid phase with an acid to dissolve calcium carbonate; The present invention is characterized by comprising:

[0012] In the method for producing hollow silica particles of the present invention, the relative dielectric constant of the mixed liquid in the mixing step is smaller than that of water, so that dehydration condensation of sodium silicate is rapidly carried out. That is, silicate ions are rapidly generated by hydration to sodium silicate, and the silicate ions are adsorbed on the surface of calcium carbonate, and dehydration condensation forms a silica shell. Then, in the separation step, the calcium carbonate with the silica shell formed on its surface is separated. Finally, the calcium carbonate is dissolved by acid treatment to obtain hollow silica particles.

[0013] The mixing ratio of water, organic solvent, calcium carbonate, and sodium silicate aqueous solution is preferably set to a condition suitable for forming calcium carbonate covered with a silica shell in the mixing step S1, and difficult for solid silica particles to be formed. Such a suitable mixing ratio is preferably determined in advance by a test.

[0014] The dielectric constant of the mixed solution is preferably 50 to 75. If the dielectric constant of the mixed solution is in the range of 50 to 75, the dehydration and condensation of sodium silicate can be rapidly carried out, and a silica shell can be formed on the surface of calcium carbonate. If the dielectric constant of the mixed solution exceeds 75, the dehydration and condensation reactions of sodium silicate slow down, making it difficult to form silica. If the dielectric constant of the mixed solution is less than 50, the dehydration and condensation reactions of sodium silicate are too fast, resulting in the formation of solid silica particles in the mixed solution, making it difficult to form a silica shell on the surface of calcium carbonate. More preferably, the dielectric constant of the mixed solution is in the range of 57 to 64.

[0015] In addition, it is preferable that ammonia is adsorbed to the calcium carbonate, because the use of calcium carbonate with ammonia adsorbed thereto makes it easier for the silica precursor (see FIG. 2) to be adsorbed to the calcium carbonate, and therefore a silica shell is rapidly formed on the surface of the calcium carbonate, suppressing the generation of unintended solid silica particles.

[0016] The organic solvent may be an alkyl alcohol having up to 3 carbon atoms. Particularly preferred are ethanol and methanol, which are alkyl alcohols having up to 2 carbon atoms. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a process diagram of a method for producing hollow silica particles. [Diagram 2] FIG. 1 is a schematic diagram showing a process in which sodium silicate becomes silica via a silica precursor. [Diagram 3] FIG. 2 is a schematic diagram showing the adsorption process of a silica precursor onto calcium carbonate. [Figure 4] This is a schematic diagram showing that silica precursors rapidly undergo dehydration and condensation reactions to form silica particles, and are not adsorbed onto the calcium carbonate surface. [Diagram 5] FIG. 1 is a process diagram for Test Example 1. [Figure 6] 1 is a scanning electron microscope photograph of calcium carbonate particles. [Figure 7] This is a graph plotting the evaluation of the product when the amount of ethanol added (X) and the amount of water added (Y) are changed. [Figure 8] This is a scanning electron microscope photograph of particles synthesized under the conditions on Line A. [Figure 9] This is a scanning electron microscope photograph of particles synthesized under the conditions on Line B. [Figure 10] FIG. 2 is a schematic diagram showing the process in which multiple calcium carbonates become aggregates connected by silica shells as the silica shell grows. [Figure 11] Scanning electron microscope images of particles synthesized under the conditions of Regions C, D, E, and F. [Figure 12] FIG. 2 is a schematic diagram showing the formation of the first layer of a silica shell by a solid-state acid-base reaction between the Ca site of calcium carbonate and the silanol group of a silica precursor. [Figure 13]1 is a graph showing the region in which hollow silica particles can be synthesized and the center of gravity of that region in a plot of product evaluation when the amount of ethanol added (X) and the amount of water added (Y) are changed. [Figure 14] 1 is a scanning electron microscope photograph of hollow silica particles synthesized at a composition at the center of gravity of the region in which hollow silica particles can be synthesized in a two-dimensional diagram. [Figure 15] FIG. 2 is a diagram showing a possible synthesis area of ​​hollow silica particles in a three-dimensional diagram. [Figure 16] 16 is a scanning electron microscope photograph of hollow silica particles synthesized with a composition at the center of gravity of the synthesis possible region in the three-dimensional diagram of FIG. 15. [Figure 17] FIG. 1 is a process diagram of Example 2. [Figure 18] 1 is a scanning electron microscope photograph of the hollow silica particles obtained in Example 1 and Example 2. [Figure 19] FIG. 2 is a process diagram for measuring the amount of ammonia adsorption. [Figure 20] 1 is an adsorption isotherm of ammonia onto calcium carbonate. [Figure 21] FIG. 1 is a process diagram showing a method for synthesizing hollow silica particles using calcium carbonate having ammonia adsorbed thereon. [Figure 22] 1 is a scanning electron microscope photograph of hollow silica particles of Examples 3-1, 3-2, and 3-3. [Diagram 23] FIG. 2 is a schematic diagram showing the process of forming a silica shell on a calcium carbonate particle. [Figure 24] t-plots for Examples 3-1, 3-2, and 3-3. [Diagram 25] FIG. 2 is a schematic diagram showing the change in the structure of synthetic hollow silica particles by controlling the amount of ethanol added. [Figure 26] 1 is a scanning electron microscope photograph of hollow silica particles obtained in Example 12 (water-NMP mixed solvent system). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, specific embodiments of the present invention will be described. <Method of manufacturing hollow silica particles> ·Mixing process S1 A process diagram of the method for producing hollow silica particles is shown in Fig. 1. First, in the mixing step S1, water, an organic solvent, calcium carbonate powder, and an aqueous sodium silicate solution are mixed in a predetermined ratio. The order of mixing is not particularly limited, but it can be performed, for example, by a method of 1) adding a water-organic solvent mixed solution to calcium carbonate and preparing a dispersion using a homogenizer, then adding an aqueous sodium silicate solution and stirring, or 2) adding calcium carbonate to water and preparing a dispersion using a homogenizer, then adding an aqueous sodium silicate solution and adding an organic solvent while stirring, etc.

[0019] The organic solvent must be soluble in water. Here, soluble in water means an organic solvent that can dissolve 10 g or more in 100 g of water. For example, alcohols such as methanol, ethanol, and various propanols, ketones such as acetone, nitriles such as acetonitrile, ethers such as THF and dioxane, formamides such as DMF, and lactams such as NMP can be used. In the mixing step S1, sodium silicate is dissolved in the aqueous-organic mixture to form a mixed solution. On the other hand, calcium carbonate powder is poorly soluble in the mixed solution, so the powder is dispersed in the mixed solution.

[0020] The sodium silicate in the added sodium silicate aqueous solution becomes a silica precursor as sodium ions are replaced by hydrogen ions (see Figure 2), and is adsorbed onto the surface of the calcium carbonate powder. The adsorbed silica precursor is then further dehydrated and condensed to become poorly soluble silica. It is believed that the adsorption of the silica precursor onto calcium carbonate begins at the corners of the calcium carbonate crystals with the highest surface energy, and then the formation progresses in the order of sides and faces (see Figure 3).

[0021] The reason why a mixed solvent of water and an organic solvent is used in the method for producing hollow silica particles of the present invention is as follows (the case where the organic solvent is ethanol will be described as an example). When the solvent consists of ethanol alone, sodium silicate is insoluble in ethanol, and ethanol acts as a dehydrating agent, rapidly dehydrating and condensing it to form silica. Therefore, the silica precursor precipitates as silica offshore before it can be adsorbed on the calcium carbonate surface, and no silica shell is formed on the calcium carbonate surface (see Figure 4). On the other hand, when the solvent consists only of water and does not contain ethanol, sodium silicate dissolves in water, but due to its large relative dielectric constant, it is stabilized by hydration energy, the dehydration condensation reaction is slowed down, and silica is not formed.

[0022] For the above reasons, controlling the polarity of the solvent is essential to adsorb the silica precursor onto the surface of calcium carbonate particles and form a silica shell. Polarity is a value determined by the charge imbalance caused by the difference in electronegativity, and a substance with a dipole moment can be said to be a polar substance. The dielectric constant is also a value whose magnitude is determined by the charge imbalance, so the polarity is determined by the dielectric constant. For this reason, by using a solvent in which water and an organic solvent with a smaller dielectric constant than water (e.g., ethanol) are mixed in various ratios, it is possible to control the dielectric constant (polarity) of the mixed solution, and thus to control the formation of a silica shell on the calcium carbonate surface. For example, the dielectric constants of water and ethanol (the dielectric constant of a substance relative to the dielectric constant of a vacuum) are 80.4 and 24, respectively. The dielectric constant δ of this two-component mixed solvent is Mix If the ratio of ethanol present is α, it can be expressed by the following formula: This formula shows that by changing the mixture ratio of ethanol and water, the relative dielectric constant of the mixed solvent can be controlled, and therefore the polarity can be controlled.

[0023]

number

[0024] According to the results of tests conducted by the inventors, by controlling the relative dielectric constant of the mixed solution to be within a predetermined range, the formation of solid silica particles was suppressed and the yield of hollow silica particles was increased.

[0025] ·Separation process S2 In the separation step S2, the calcium carbonate on which the silica shell has been formed is separated from the mixed solution by filtration, centrifugation, etc. The separated precipitate is then washed with water, an organic solvent, or a mixed solvent of water and an organic solvent, and the separation step is carried out again.

[0026] ·Dissolution process S3 An acid is added to the calcium carbonate thus separated and purified on which the silica shell is formed, to dissolve the calcium carbonate. As the acid, hydrochloric acid, nitric acid, or the like capable of dissolving calcium carbonate can be used. The calcium carbonate is then washed with water, an organic solvent, or a mixed solvent of water and an organic solvent, and separated by filtration, centrifugation, or the like, and dried to obtain hollow silica particles. The hollow silica particles thus obtained are formed using the shape of the calcium carbonate powder as a matrix, and therefore have the same shape as the calcium carbonate powder. EXAMPLES

[0027] (Test Example 1) In Test Example 1, ethanol was used as the organic solvent in the mixing step S1, and the ratio of water to ethanol was changed to determine the extent to which a silica shell was formed on the calcium carbonate surface. The process diagram is shown in Figure 5.

[0028] ·Mixing process S1 Colloidal calcium carbonate (FB80, manufactured by F-Paln LLC) was used as calcium carbonate particles. An SEM image of the calcium carbonate particles is shown in Figure 6. From this image, it was found that the average silica particle diameter was 130 nm and the particles were cubic in shape. X ml of ethanol (99.5%, manufactured by Wako Pure Chemical Industries) and Y ml of distilled water were added to 1.5 g of calcium carbonate powder, and the calcium carbonate particles were dispersed at 8000 rpm for 10 minutes using a homogenizer (Hiscotron NS-52K, manufactured by Microtech Nithion) to prepare a uniform suspension. The suspension was stirred with a magnetic stirrer, and a solution of 1 ml of water glass No. 3 (SiO2 28-30 wt%, Na2O 9-10 wt%, Kishida Chemical Co., Ltd.) diluted with 10 ml of distilled water as a sodium silicate aqueous solution and stirred with a magnetic stirrer for 10 minutes was added thereto and stirred for 180 minutes.

[0029] ·Separation process S2 The solid phase was then separated by ultracentrifugation at 15,000 rpm for 10 minutes. To remove unreacted water glass, the separated particles were dispersed in distilled water, and the solid phase was separated again by centrifugation. The washing procedure with distilled water was performed twice.

[0030] ·Dissolution process S3 The obtained solid phase was redispersed in water, and 3 mol / L hydrochloric acid (Wako Pure Chemical Industries, Ltd.) was added to lower the pH to about 3, dissolving the calcium carbonate core particles. The particles were again subjected to ultracentrifugation at 15,000 rpm for 10 minutes for solid-liquid separation. The separated solid phase was dispersed twice in water and once in ethanol, and solid-phase separation by dispersion and centrifugation was repeated to remove impurities, and then dried in a dryer at 80°C to obtain particles.

[0031] <Evaluation> The particles obtained as described above were observed in secondary electron mode (SEI) and transmission electron mode (TED) using a field emission scanning electron microscope (FE-SEM: JSM-7600F, manufactured by JEOL Ltd.). The sample for observation was prepared by dropping a suspension of the sample ultrasonically dispersed in ethanol onto a microgrid (carbon support film Cu grid, grid pitch: 200 μm, manufactured by EM Japan Co., Ltd.) and drying the grid in a vacuum dryer at 180 °C for 12 hours. The accelerating voltage and the irradiation current during observation were 15 kV and 0.2 nA, respectively. To prevent the sample from being charged, the sample was coated with osmium tetroxide (OsO4) using an osmium coater (OSMIUM PLASMA COATER OPC60A, manufactured by Filgen).

[0032] In the scanning electron microscope observation, the evaluation was carried out according to the following three categories. ◯: Only hollow particles, or mostly hollow particles with a small amount of solid particles observed. Δ: A small number of hollow particles were observed, and the majority were observed as solid particles. ×: A large number of solid particles or shell fragments were observed. The particles synthesized at each mixed amount (X, Y) of the ethanol / water mixed solvent were observed using a scanning electron microscope, and the results were plotted as ○, △, or × on a graph with the horizontal axis representing the amount of ethanol added (X) and the vertical axis representing the amount of water added (Y). The results are shown in Figure 7.

[0033] As a result, the particles could be classified into the following regions: 1) the region between Line. A (α = 0.25) and Line. B (α = 0.4), which is the region marked with an O where only hollow particles or mostly hollow particles with a small amount of solid particles were observed; 2) Region C and Region F, which are marked with a △ where a small amount of hollow particles and the majority were observed as solid particles; and 3) Region D and Region E, which are mainly marked with an X where a large number of solid particles or broken shells were observed. Below we will describe the characteristics of each area and the reasons why they were formed.

[0034] The area between Line.A and Line.B This region is sandwiched between Line. A, where the volume ratio α of ethanol in the mixed solvent is 0.25, and Line. B, where α is 0.4. When the particles synthesized under the conditions on Line.A were observed by SEM, the particles had a thin silica shell, and no solid particles were observed, only hollow particles, as shown in Figure 8. Broken silica shells were also confirmed. On the other hand, it was found that the particles synthesized under the conditions on Line. B had thicker silica shells than the particles synthesized under the conditions on Line. A, as shown in Figure 9. In addition, no broken silica shells were observed, and a small amount of solid particles were also generated.

[0035] The ethanol abundance ratios α in Line A and Line B are 0.25 and 0.4, respectively. In addition, from formula (1), the relative dielectric constant ΔA of the mixed solvent on Line A is calculated to be 66.3, and the relative dielectric constant ΔB of the mixed solvent on Line B is calculated to be 57.8. Therefore, it was found that the range of the relative dielectric constant of the mixed solvent from 57.8 to 66.3 is the region in which hollow particles can be synthesized. When the relative permittivity δMix of the mixed solvent approaches 57.8, the silica shell of the hollow particles becomes thicker, creating conditions that favor the formation of solid particles. The reason is that the formation of the silica shell on the calcium carbonate particle surface becomes faster as the polarity of the solvent decreases. In other words, the decrease in polarity causes the dehydration and condensation reaction to the silica precursor to proceed quickly, and more silica is adsorbed on the calcium carbonate surface, resulting in a thicker silica shell. However, not only the adsorption on the calcium carbonate surface but also the growth of silica particles offshore becomes faster, making it easier to form solid particles. For the above reasons, the rate of silica shell formation on the calcium carbonate surface slows down on the line A, where the ratio of water is high and the relative dielectric constant is large. This results in a thin silica shell that is easily broken. Furthermore, when the relative dielectric constant is smaller than that on line A, the polarity of the mixed solvent decreases, the rate of silica shell formation increases, and a thick silica shell is formed. On the other hand, in Line B, in addition to the adsorption of silica onto the calcium carbonate surface, silica particles are also generated and grow offshore, and solid particles are generated offshore before being adsorbed onto the calcium carbonate surface. Therefore, in order to produce hollow silica particles, the condition for forming hollow silica particles is the region between Line. A and Line. B (i.e., the volume ratio α of ethanol in the mixed solvent is 0.25 or more and 0.40 or less).

[0036] Region C In Region C, both ethanol and water are low in both solvents, and the total amount of solvent is low (in other words, the concentrations of calcium carbonate and sodium silicate are high). For this reason, the distance between the silica precursors is close, and it is easy for dehydration and condensation to occur. In addition, the distance between the silica precursors formed in the dispersion and the calcium carbonate particles is also close, so the condition is such that the silica precursors are easy to adsorb to the calcium carbonate surface. However, since the distance between the calcium carbonates is also close, when the silica shells grow, they form a mass in which multiple calcium carbonates are connected by silica shells. In addition, since the dehydration and condensation of the silica precursors proceeds quickly offshore of the calcium carbonate particles, solid particles made of silica are likely to form offshore, but the silica precursors formed near the calcium carbonate are adsorbed by the calcium carbonate to form a silica shell (see Figure 10). For the above reasons, the particles formed in Region C are a mixture of a small amount of hollow silica particles, solid silica particles, and even a mass in which multiple calcium carbonates are connected by silica shells (see Figure 11).

[0037] Region D In Region D, the ratio of water in the mixed solvent is much greater than the ratio of ethanol. This makes it difficult for the dehydration and condensation reaction of the silica precursor to proceed. As shown in the photograph of Region D in Figure 11, the particles synthesized under these conditions are aggregates of a small amount of hollow particles and tiny non-spherical solid silica particles, and the formation of hollow silica particles could not be confirmed.

[0038] Region E In contrast to Region C, Region E has a high concentration of both ethanol and water, and the total amount of solvent is high. In other words, the concentrations of calcium carbonate and sodium silicate are low, and the distance between the calcium carbonate particles and the silica precursor is long. For this reason, it is presumed that the silica particles generated by dehydration and condensation of the silica precursor are more likely to aggregate with other silica particles before being adsorbed onto the calcium carbonate particles. On the other hand, when the silica particles reach the vicinity of the calcium carbonate particle surface, the free energy decreases due to the increase in particle size, and the particle becomes stable, making it difficult for them to be adsorbed onto the calcium carbonate surface (see Figure 4). As shown in Region E in Figure 11, it can be seen that the particles synthesized in this region are mostly solid particles.

[0039] Region F In Region F, the conditions are the opposite of those in Region D, where the ratio of ethanol in the mixed solvent is much higher than the ratio of water. Therefore, the polarity of the mixed solvent is dominated by ethanol, and the polymerization reaction proceeds rapidly. As a result, the generated silica particles are hollow particles with broken silica shells, as shown in Region F of Figure 11. From the above results, it was found that hollow silica particles are difficult to form under conditions where the polarity is extremely low or the ratio of water in the mixed solvent is extremely low.

[0040] The reason why hollow silica particles are not formed in Region D, Region E, and Region F is presumed to be because the first layer of silica is not formed on the calcium carbonate surface. The first layer of the silica shell is thought to form a strong bond by a solid acid-base reaction between the Ca site of calcium carbonate and the silanol group of the silica precursor (see Figure 12). This first layer becomes a site for the growth and precipitation of silica, and the silica particles grow. Under conditions of low polarity of the mixed solvent or conditions of a large amount of solvent, it is difficult to form the first layer, so selective grain growth is difficult to occur, or grain formation and grain growth occur regardless of the calcium carbonate surface before the first layer is formed, so it is presumed that hollow silica particles are not formed and solid silica particles are formed.

[0041] ·Optimal conditions for hollow silica particle synthesis in Test 1 In Test 1, a region where hollow particles can be synthesized was created using a graph of the volume of ethanol:volume of water, and the center of gravity of that region was determined to estimate the optimal mixing ratio of ethanol / water mixed solvents for hollow particle synthesis.

[0042] As shown in Figure 7, the region where hollow silica particles can be synthesized in Test 1 is established under the conditions that the amount of the ethanol / water mixed solvent is 60-150 ml and the ethanol content is 0.25-0.40. Using these results, the region where hollow particles can be synthesized is shown on a graph of the volume of ethanol:volume of water, and the center of gravity of the region is obtained to determine the optimal solvent mixing ratio. Figure 13 shows the region and the center of gravity of the region. The region surrounded by the dotted line is the region where synthesis is possible. The coordinates of the center of gravity of this region where synthesis is possible are (34, 71). From this value, the optimal synthesis conditions for hollow silica particles using sodium silicate as the starting material in this study were the conditions of adding a precursor solution of 1 ml of water glass diluted with 10 ml of distilled water to a mixed solvent of 1.5 g of calcium carbonate, 34 ml of ethanol, and 61 ml of distilled water. Furthermore, hollow silica particles were synthesized under these conditions and observed by scanning electron microscope. As a result, as shown in Figure 14, no solid silica particles were observed, and no significant breakage of the silica shell was observed. Instead, hollow silica particles with thin silica shells were formed, indicating that these were the most suitable conditions for synthesizing hollow silica particles.

[0043] <3D graph with water-ethanol-sodium silicate concentration as parameters> Figure 7 is a graph showing the results when the amount of sodium silicate added is constant. Based on this graph, a three-dimensional graph was derived using the following method, with the three variables of water, ethanol, and sodium silicate concentration as parameters. The conditions used to calculate the synthesisable region in Test 1 were as follows: 1) and 2). 1) Total volume of solvent: Ethanol + Water: 60-150ml 2) Ethanol ratio α: Ethanol / (Ethanol + Water) is 0.25 to 0.40 The above 1) is a condition related to the amount of mixed solvent, in other words, a condition related to the concentration of sodium silicate in the mixed solvent. In addition, since the amount of sodium silicate aqueous solution added in Test 1 was 1 ml, the concentration of sodium silicate can be expressed as 1 / (volume of ethanol + volume of water). Therefore, when the condition 1) is converted into the concentration of sodium silicate, the concentration of sodium silicate is 0.67 vol.% to 1.67 vol.% (1´). On the other hand, since 2) is a condition related to the ethanol abundance ratio α, by substituting this condition into the above-mentioned equation (1), it can be replaced with the condition that the relative dielectric constant is a value between 57.8 and 66.3 (2´). 1´) Sodium silicate concentration: Waterglass / (Ethanol + Water) is 0.67~1.67vol.% 2´) Dielectric constant of mixed solvent (δ Mix ) is 57.8~66.3

[0044] Under the conditions of 1´), the concentration of sodium silicate in the synthesis range is 0.67 to 1.67 vol.%. Next, δ Mix Determine the upper and lower limits of the sodium silicate concentration when is 57.8.

[0045] A) Upper and lower limits of (15, 45) Under the condition of 15 ml of ethanol and 45 ml of water, this is the lower limit (60 ml) of the solvent amount in the synthesis region, so the amount of sodium silicate added is 1 ml and the sodium silicate concentration is the upper limit (1.67%). Furthermore, calculations show that the lower limit of the sodium silicate concentration, 0.67%, is the amount of sodium silicate added of 0.4 ml. Therefore, under the condition of (15, 45), the upper limit of the amount of sodium silicate added is 1 ml and the lower limit is 0.4 ml.

[0046] B) The upper and lower limits of (37.5, 112.5) Under the condition of 37.5 ml of ethanol and 112.5 ml of water, this is the upper limit (150 ml) of the amount of solvent in the region where synthesis is possible, so it can be said that the amount of sodium silicate added is 1 ml and the sodium silicate concentration is the lower limit (0.67%). Furthermore, calculations show that the upper limit of the sodium silicate concentration, 1.67%, is the amount of sodium silicate added of 2.5 ml. Therefore, under the condition of (37.5,112.5), the upper limit of the amount of sodium silicate added is 2.5 ml and the lower limit is 1 ml.

[0047] Next, δ Mix Determine the upper and lower limits of the amount of sodium silicate to be added under the condition that the pH is 66.3.

[0048] C) Upper and lower limits of (24, 36) Under the condition of 24 ml of ethanol and 36 ml of water, this is the lower limit (60 ml) of the solvent amount in the synthetic range, so the upper limit of the amount of sodium silicate to be added is 1 ml and the lower limit is 0.4 ml.

[0049] D) Upper and lower limits of (60, 90) Under the condition of 60 ml of ethanol and 90 ml of water, this is the upper limit (150 ml) of the solvent amount in the synthetic range, so the upper limit of the amount of sodium silicate to be added is 2.5 ml and the lower limit is 1 ml. Using these results, the three-dimensional synthesis region was determined when the mixture of ethanol, water, and sodium silicate was changed in amount. Table 1 shows the upper and lower limits of the amount of sodium silicate added determined under conditions A) to D).

[0050] [Table 1]

[0051] A three-dimensional diagram of the synthesis region constructed by these coordinates is shown in Figure 15. From this three-dimensional diagram, a synthesis region consisting of an octahedron was obtained. The center of gravity of the octahedron was (34, 71, 1.225), and the coordinates of this center of gravity were estimated to be the optimal conditions for synthesizing hollow silica particles.

[0052] For this reason, hollow silica particles were synthesized under the conditions of this center of gravity coordinate and observed with a scanning electron microscope. As a result, as shown in Figure 16, it was found that only hollow silica particles were generated, and no solid silica particles were generated. In addition, compared to Figure 14, which is an SEM image of hollow particles synthesized under the optimal conditions calculated from the 2D diagram, hollow silica particles with thicker and stronger silica shells were formed. The above results indicate that the optimal conditions for the three variables of changing the amounts of ethanol, water, and sodium silicate added are the optimal conditions for obtaining hollow silica particles with stronger silica shells than the optimal conditions for the two variables.

[0053] (Examples 1 and 2) In Example 1 and Example 2, the mixing order of the drugs in the mixing step S1 was changed. Example 1 In Example 1, the mixing order of each agent in the mixing step S1 was the same as in Test Example 1. That is, a mixture of 40 ml of ethanol and 60 ml of water was added to 1.5 g of calcium carbonate and made into a dispersion using a homogenizer, and then 1 ml of a sodium silicate aqueous solution (water glass No. 3 (SiO2 28-30 wt%, Na2O 9-10 wt%, Kishida Chemical Co., Ltd.) was added and stirred (see FIG. 5). Example 2 In Example 2, the mixing order of each agent in the mixing step S1 was performed as shown in Figure 17. That is, 1.5 g of colloidal calcium carbonate was weighed out, added to 60 ml of distilled water, and dispersed for 10 minutes at 8000 rpm using a homogenizer. 1 ml of sodium silicate aqueous solution (water glass No. 3 (SiO2 28-30 wt%, Na2O 9-10 wt%, Kishida Chemical Co., Ltd.) was added thereto and stirred for 1 hour. Then, 40 ml of ethanol was added and stirred for 3 hours. Then, in the separation step S2, ultracentrifugation was performed at 15,000 rpm for 10 minutes using a centrifuge to settle the solid phase. To remove unreacted sodium silicate, the separated particles were washed twice with distilled water. Further, in the dissolution step S3, the particles obtained by solid phase separation were redispersed in an aqueous solvent, and hydrochloric acid adjusted to 3 mol / L was added to lower the pH to about 3, dissolving calcium carbonate. Furthermore, ultracentrifugation was performed again at 15,000 rpm for 10 minutes using a centrifuge to separate the solid and liquid. The separated solid phase was washed twice with water and once with ethanol, and dried at 80° C. to obtain hollow silica particles of Example 2.

[0054] <Evaluation> The shape of the hollow silica particles obtained in Example 1 and Example 2 was observed using a scanning electron microscope in secondary electron (SEI) mode and transmission electron (TED) mode. As a result, as shown in Fig. 18, hollow silica particles and solid silica particles with a large particle size were observed in both Example 1 and Example 2. However, the solid silica particles in Example 1 had a larger particle size than the solid silica particles in Example 2.

[0055] The evaluation results can be explained as follows. In Example 1, when a sodium silicate aqueous solution was added to an ethanol / water mixed solvent in which calcium carbonate particles were dispersed, silica precursors were generated uniformly in the liquid. It is considered that the silica precursors thus generated aggregated in the liquid before being adsorbed on the calcium carbonate surface, generating solid silica particles with large particle diameters (see FIG. 18, Example 1).

[0056] On the other hand, in Example 2, the sodium silicate aqueous solution is added to the water solvent in which calcium carbonate particles are dispersed, so that the sodium silicate aqueous solution is diluted. Also, since the solvent is only water and ethanol is not mixed, the dehydration and condensation reaction is slowed down, and solid silica particles are adsorbed to calcium carbonate before they are generated in the liquid. Then, ethanol is added, and the silica precursors adsorbed to calcium carbonate dehydrate and condense with each other, growing a silica shell. Therefore, the silica shell grows selectively on the surface of calcium carbonate. As a result, it is considered that the formation of solid silica particles in the liquid becomes difficult, and the solid silica particles have a small particle size (see FIG. 18 Example 2).

[0057] (Examples 3-1, 3-2, and 3-3) Jeoren et al. have reported that amino groups and zwitterions (NH3 + and CO - They have succeeded in producing polystyrene particles with a silica shell by adding an aqueous sodium silicate solution to polystyrene particles modified with dimethylsilane (see paper below). Jeroen JLM Cornelissen, Eric. F. Connor, Ho-Cheol Kim, Victor Y. Lee, Teddie Magibitang, Philip M. Rice, Willi Volksen, Linda K. Sundberg and Robert D. Miller, “Versatile synthesis of nanometer sized hollow silica spheres”, CHEM. COMMUN. , 1010-1011, (2003) Therefore, in Examples 3-1, 3-2, and 3-3, hollow silica particles were synthesized using calcium carbonate to which ammonia was adsorbed, and the effect of ammonia adsorption on the formation of the silica shell was examined.

[0058] -Ammonia adsorption experiment on calcium carbonate First, the adsorption isotherm of ammonia adsorption to calcium carbonate was obtained. The amount of ammonia molecules adsorbed to calcium carbonate was measured by subtracting the amount of substance after adsorption from the amount of substance in the original ammonia aqueous solution, and the difference was calculated as the amount of substance of the adsorbed ammonia molecules. In order to measure the molar concentration of the ammonia aqueous solution after adsorption, an acidic solution of a specified concentration was added to the ammonia aqueous solution, and then neutralization titration was performed with a basic solution. A process diagram for measuring the amount of ammonia molecules adsorbed to calcium carbonate by this back titration method is shown in Figure 19. Details are explained below.

[0059] Calcium carbonate P [g] was added to 50 ml of a solution prepared by adding distilled water to a 28 wt.% ammonia aqueous solution (manufactured by Wako Pure Chemical Industries) to a specified concentration Q [mol / L], and stirred for 12 hours. Then, the solution was centrifuged at 15,000 rpm for 10 minutes to separate the solid and liquid. 10 ml of the separated supernatant solution was taken, and R [ml] of hydrochloric acid adjusted to 1.0 mol / L was added to it to make the supernatant solution acidic. Neutralization titration was performed using the solution and a sodium hydroxide aqueous solution adjusted to 1.0 mol / L, and the ammonia adsorption amount V [mol] was calculated using the following calculation formula (1).

number

[0060] In addition, the equilibrium concentration C [mol / L / g] of the aqueous ammonia solution per unit mass of calcium carbonate to obtain this adsorption amount was calculated using the following calculation formula (2).

number

[0061] The adsorption amount V and the equilibrium concentration C thus determined were plotted to prepare an adsorption isotherm. Figure 20 shows an adsorption isotherm that shows the relationship between the amount of ammonia adsorbed and the equilibrium concentration of the aqueous ammonia solution calculated by back titration. This graph shows that the amount of adsorption increases until the equilibrium concentration reaches a certain value, after which the amount of adsorption becomes saturated. The adsorption phenomenon is a chemical adsorption that uses the concentration gradient as the driving force, and the adsorbent is adsorbed to the adsorption carrier as a single layer. For this reason, when one layer of adsorption layer is formed, the adsorption phenomenon no longer occurs. The equilibrium concentration at this saturated adsorption was 6.058 mol / L, and the amount of adsorption was 0.166 mol / g.

[0062] Synthesis of hollow silica particles using calcium carbonate adsorbed with ammonia The synthesis method is shown in Figure 21. 75 ml of diluted ammonia solution prepared by mixing 28 wt.% ammonia solution and distilled water to 9.087 mol / L (6.058 mol / L x 1.5 g) was added to 1.5 g of calcium carbonate, and the mixture was stirred at 8000 rpm for 10 minutes using a homogenizer to prepare a uniform suspension. The suspension was stirred for 12 hours using a magnetic stirrer in a closed space to prepare a suspension of calcium carbonate saturated with ammonia. Then, a silica precursor solution prepared by diluting 1 ml of water glass with 10 ml of distilled water was added to the suspension to adsorb the silica precursor to calcium carbonate. A predetermined amount of ethanol (21 ml in Example 3-1, 38 ml in Example 3-2, and 51 ml in Example 3-3) was added to the suspension in which the silica precursor was present near the surface of the calcium carbonate by these steps, and the suspension was stirred for 3 hours to form a silica shell, synthesizing calcium carbonate particles with a silica shell. Ultracentrifugation was performed for 10 minutes at 15,000 rpm using a centrifuge to separate the solid and liquid, and the calcium carbonate particles with a silica shell were precipitated. To remove unreacted sodium silicate, the separated particles were washed twice with distilled water. The silica shell-attached calcium carbonate particles thus obtained were redispersed in an aqueous solvent, and hydrochloric acid adjusted to 3 mol / L was added to lower the pH to about 3, dissolving the calcium carbonate core particles. Then, the mixture was ultracentrifuged at 15,000 rpm for 10 minutes using a centrifuge to separate the solid and liquid. The separated solid phase was washed twice with water and once with ethanol to remove impurities. The washed particles were dried in a dryer at 80°C to obtain hollow silica particles. The mixed amount of water / ammonia aqueous solution and the amount of ethanol added in the diluted ammonia aqueous solution are shown in Table 2.

[0063] [Table 2]

[0064] <Evaluation> The hollow silica particles of Examples 3-1, 3-2, and 3-3 prepared as described above were observed by a scanning electron microscope. The evaluation method was the same as that of Test Example 1, and therefore the description is omitted. In addition, to estimate the structure of the silica shell, nitrogen adsorption measurements were performed using an automatic specific surface area measurement device (Belsorp-mini II, Microtrac BEL) and true density measurements were performed using a pycnometer (ULTRAPYCNOMETER, Quantachrome), and the pore size inside the silica shell was calculated.

[0065] Shape observation using a scanning electron microscope (SEM) 22 shows scanning electron microscope photographs of hollow silica particles of Examples 3-1, 3-2, and 3-3. In Example 3-1 (ethanol addition rate 25 vol%), black spheres were observed in the transmission electron image (TED). These particles are particles that electron beams cannot penetrate, and therefore they are found to be solid silica particles. These particles are also found to be solid particles from the secondary electron image (SEI). In contrast, in Example 3-2 (ethanol addition rate 45 vol%), no black spheres were observed in the transmission electron image (TED). This indicated that no solid silica particles were present, and hollow silica particles were produced. In addition, black shadow areas were observed in the transmission electron image (TED), which are believed to be overlapping areas of the silica shells of the hollow silica particles. In Example 3-3 (ethanol addition rate: 60 vol%), similarly to Example 3-2, no solid silica particles were observed, but irregularities were observed on the particle surfaces.

[0066] The unevenness observed on the particle surface in Example 3-3 is considered to be a state in which the primary particles constituting the silica shell of the hollow silica particles are exposed. The reason for the formation of the unevenness is presumed to be as follows. That is, in Examples 3-1, 3-2, and 3-3, hollow silica particles are synthesized using calcium carbonate with ammonia adsorbed thereon, so that ammonia serves as a catalyst for the condensation of the silica precursor, and silica is selectively formed on the calcium carbonate surface. This facilitates the formation of the first layer of the silica shell. And, the presence of this first layer promotes the growth of silica, and a shell shell is formed. Therefore, in Example 3-3, the formation of solid silica particles in the mixed liquid is suppressed. Therefore, the particle diameter of the primary particles constituting the silica shell becomes large, and as shown in the schematic diagram of FIG. 23, a shell shell in which the primary particle shape is exposed is formed. On the other hand, in Examples 3-1 and 3-2, where the amount of ethanol added was low, solid particles were observed because the solvent with a low amount of ethanol had a high polarity due to its high dielectric constant, allowing solid silica particles to grow from the silica precursor.

[0067] Nitrogen adsorption measurement and true density measurement Nitrogen adsorption measurements and true density measurements were performed to calculate the pore size in the silica shell. The t method was applied to the adsorption isotherm obtained from the nitrogen adsorption measurement to calculate the micropore diameter. The t method is a method for evaluating pore diameter and pore volume using the phenomenon of filling micropores with nitrogen molecules (micropore filling). If the pore radius is t, the pore radius can be calculated from the following formula (3). In this case, Va is the amount of adsorption, and Vm is the amount of monomolecular adsorption. For this measurement, solid silica particles without micropores were used as the standard isotherm.

number

[0068] The t-plot is shown in Figure 24. The horizontal axis is the adsorption layer thickness t, and 2t corresponds to the micropore diameter. The vertical axis is the amount of adsorption, from which the micropore volume can be determined. In the t-plot, the thickness of the adsorption layer at the intersection of the straight lines plotted before and after the slope of the straight line changes due to micropore filling is the pore radius. The micropore volume was calculated from the intercept of the straight line plotted after the slope changed (see the table in Figure 24). As a result, it was found that the micropore diameter increased with an increase in the ethanol addition rate. This is thought to be due to an increase in the primary silica particle diameter (see Figure 25). The above results demonstrate that it is possible to control the primary particle diameter by controlling the ethanol addition rate.

[0069] <Synthesis of hollow silica particles using organic solvents other than ethanol> In the above-mentioned Examples 1, 2, 3-1, 3-2, and 3-3, ethanol was used as the organic solvent for adjusting the dielectric constant, but in Examples 4 to 12, hollow silica particle synthesis experiments were performed using the solvents shown in Table 3.

[0070] [Table 3]

[0071] Each organic solvent was mixed in a mixing ratio based on the following calculation formula (4) such that the dielectric constant εmix of the mixed solvent with water would be 62. The other procedures were the same as in Example 1.

number

[0072] FIG. 26 shows an electron microscope photograph of Example 12 synthesized in a water-NMP mixed solvent system. From this photograph, it was found that hollow silica particles can be formed by adjusting the mixing ratio of water and NMP so that the dielectric constant εmix of the mixed solvent is 62. Similarly, hollow silica particles were formed in Examples 4 to 11 synthesized in mixed solvent systems of other organic solvents and water. From the above results, it was found that hollow silica particles can be formed by adjusting the dielectric constant εmix to 62 by mixing water and an organic solvent.

[0073] The present invention is not limited to the above-mentioned embodiment. Various modifications within the scope of the claims and within the scope of those skilled in the art are also included in the present invention. [Industrial Applicability]

[0074] Hollow silica particles have properties such as a high specific surface area, low density, and low thermal conductivity compared to solid silica particles. These properties can be utilized as functional materials such as catalyst carriers, light scattering materials, and heat insulating materials. [Explanation of symbols]

[0075] S1...Mixing process, S2...Separation process, S3...Dissolution process

Claims

1. a mixing step of mixing water, an organic solvent that is soluble in water and has a dielectric constant smaller than that of water, calcium carbonate, and an aqueous solution of sodium silicate in a predetermined ratio; A separation step of separating a solid phase from the mixed solution; a dissolving step of treating the separated solid phase with an acid to dissolve calcium carbonate; A method for producing hollow silica particles comprising the steps of:

2. 2. The method for producing hollow silica particles according to claim 1, wherein the mixed solution has a relative dielectric constant of 50 to 75.

3. 3. The method for producing hollow silica particles according to claim 1, wherein the calcium carbonate has ammonia adsorbed thereon.

4. 3. The organic solvent according to claim 1 or 2, wherein the organic solvent is an alkyl alcohol having 3 or less carbon atoms.

2. A method for producing hollow silica particles according to claim 1 .

5. The method for producing hollow silica particles according to claim 4, wherein the alkyl alcohol is ethanol.

Citation Information

Patent Citations

  • High dispersion silica NANO hollow particle and its producing method

    JP2005263550A

  • Method for preparing hollow silica particle

    JP2008222459A