Concrete repair material and concrete repair method

A lithium silicate-based repair material and method enhance the durability of carbonated concrete by densifying the surface and protecting it, addressing the ineffectiveness of existing methods on carbonated concrete with improved water resistance and adhesive strength.

JP2024134451AActive Publication Date: 2024-10-03RINACOZMO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044766
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Existing concrete repair methods are ineffective for concrete that has undergone carbonation, leading to issues such as increased deterioration and potential secondary disasters from peeling flakes.

Method used

A concrete repair material containing 13 to 17% lithium silicate and 1.5 to 2.5% sodium hydroxide is applied to the concrete surface, followed by drying to form a protective layer, which is then optionally reinforced with a polymer cement mortar or coating, to densify and protect the concrete.

Benefits of technology

The repair method effectively suppresses water and chloride ion intrusion, maintaining adhesive strength and reducing dynamic friction, even on carbonated concrete, with a water permeability suppression rate of 65.3 to 74.8% and improved compatibility with other construction methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134451000001_ABST
    Figure 2024134451000001_ABST
Patent Text Reader

Abstract

To provide a concrete repair method that is even more effective for concrete with advanced neutralization.SOLUTION: In a concrete repair method that can be performed on concrete that is in a latent period of deterioration and concrete that is in a period of deterioration after the latent period, when a concrete surface is in a state of surface dryness, a concrete repair material that contains 13 to 17 mass% of lithium silicate and 1.5 to 2.5 mass% of sodium hydroxide in an aqueous solution is applied and dried to form a concrete repair surface, and in a water permeability test on the concrete repair surface, the inhibition rate is 65.3% to 74.8%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a concrete repair material for, for example, existing or newly constructed concrete, and a method for repairing concrete. [Background technology]

[0002] Patent Document 1 (claim 1, etc.) listed below discloses an invention relating to a method for repairing concrete, in which a surface protective agent consisting of an aqueous solution containing an alkali metal silicate and a carboxylic acid is applied to the surface of polymer cement mortar. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4664949 Summary of the Invention [Problem to be solved by the invention]

[0004] Patent Document 1 does not clarify whether or not the method is effective for concrete in which neutralization has progressed.

[0005] An object of the present invention is to provide a concrete repair material that is more effective even on concrete in which neutralization has progressed, and a method for repairing concrete. [Means for solving the problem]

[0006] The concrete repair material according to the present invention comprises: The aqueous solution contains 13 to 17% by mass of lithium silicate and at most 1.5 to 2.5% by mass of sodium hydroxide. The method for repairing concrete according to the present invention is a method for repairing concrete that can be performed on concrete in which the deterioration process is in the latent period and on concrete in which the deterioration process is in the latent period or later, When the concrete surface is in a dry state, the concrete repair material is applied to the concrete surface and dried to form a concrete repair surface; In the water permeability test of the repaired concrete surface, the inhibition rate was 65.3 to 74.8%. Effect of the Invention

[0007] According to the present invention, it is possible to provide a concrete repair material and a concrete repair method that are more effective even on concrete in which neutralization has progressed. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is an explanatory diagram showing a schematic diagram of a mechanism of concrete repair using a repair material according to one embodiment of the present invention. [Diagram 2] 1 is a table showing test results regarding adhesion of a repair material according to an embodiment to various adhesives. [Diagram 3] 3 is a table showing the test results following FIG. 2. [Figure 4] 1 is a table showing measurement results of dynamic friction coefficients for the repair material of the embodiment together with comparative examples. [Diagram 5] 1 is a table showing the results of a water permeability test for the repair material of the embodiment together with a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Concrete is inherently very durable. For this reason, it has traditionally been said that its service life is 50 to 100 years. However, in recent years, it has been discovered that concrete deteriorates faster than expected.

[0010] In particular, concrete deterioration and combined deterioration caused by freeze-thaw and salt damage are causing structures to appear that do not last their expected service life. There is also concern about secondary disasters caused by concrete pieces peeling off from structures. For these reasons, various measures are being taken to investigate the causes of deterioration and to improve the quality of new and existing concrete.

[0011] Specifically, the composition of cement constituting the newly placed concrete is changed and the unit water content is reduced. Further, for the aggregate components, for existing concrete, methods such as coating the deteriorated surface with polymer cement, coating with a silicate (silicic acid)-based waterproofing agent-containing mortar, and injection, penetration, and film coating methods using organic resins and cement-based materials are carried out.

[0012] Although all of these measures are effective, they may not be sufficient for dealing with concrete in which carbonation has progressed. The inventors have studied a concrete modification method that can obtain good effects even for concrete in which carbonation has progressed to a certain extent. Hereinafter, a concrete modification method (base concrete modification method, repair method, repair technique) according to an embodiment of the present invention and a concrete repair material used therefor will be described.

[0013] ><Regarding the base concrete repair method (modification method) using OSMO-KK (trade name)> ><Overview> (1) The concrete repair material according to this embodiment has 13 to 17% by mass of lithium silicate and 1.5 to 2.5% by mass of sodium hydroxide (caustic soda) in an aqueous solution (silicate aqueous solution). (2) The concrete repair method according to this embodiment is a concrete repair method that can be performed on concrete in which the deterioration process is up to the latent period and concrete in which the deterioration process is after the latent period, when the concrete surface is in a surface dry state, applying the concrete repair material of (1) above and drying it to form a concrete repair surface, and the suppression rate is 65.3 to 74.8% in the water permeability test of the concrete repair surface. (3) In the concrete repair method of (2) above, a primary application of the concrete repair material of (1) above is performed on the surface layer portion of the concrete repair surface and dried to form a protective layer. (4) In the concrete repair method of (3) above, the surface layer of the concrete reinforcement surface is secondarily coated with the concrete repair material of (1) above, and dried to form a protective layer. (5) In the concrete repair method according to this embodiment, the average value of the adhesion strength between the concrete using the concrete repair material described in (1) above and the coating material attached to the concrete is 1.1 N / mm 2 or more and 3.4 N / mm 2 or less. (6) In the concrete repair method according to this embodiment, the decrease in the average value of the dynamic friction coefficient when using the concrete repair material described in (1) above is within 8.4%.

[0014] The concrete repair method (repair method, modification method) according to the embodiment is a concrete repair method (modification method) by combining the modification of the concrete base using a solidified lithium silicate-based surface impregnating material and the surface coating material.

[0015] OSMO-KK (trade name of the concrete repair material (modification material), hereinafter abbreviated) is the concrete repair material according to this embodiment. OSMO-KK is the name of a solidified lithium silicate-based surface impregnating material developed by the inventors. OSMO-KK is manufactured by a unique method of dissolving an alkali metal salt (such as sodium silicate and potassium silicate) in an aqueous solution of lithium silicate (Li4SiO4). The preferred composition of OSMO-KK will be described later. The name of OSMO-KK can also be changed to other names.

[0016] <<Each step of the concrete repair method using OSMO-KK>> An example of the concrete repair method (repair method) using OSMO-KK will be described. The concrete repair method according to this embodiment can be divided into a first step and a second step. In the first step, OSMO-KK is applied to the surface layer of the concrete in which neutralization has progressed to a certain extent. In the second step, protection is provided for the concrete surface to which OSMO-KK has been applied.

[0017] Specifically, in the first step, a solidifying silicate-based surface impregnating material (OSMO-KK) is applied to the base concrete (base concrete). By applying the surface impregnating material, the surface layer of the concrete is densified. By densifying the surface layer of the concrete, the intrusion of deterioration factors such as water, chloride ions, and carbon dioxide is suppressed.

[0018] In the subsequent second step, as described above, the concrete surface (concrete surface) is protected. Various general methods can be used to protect the concrete surface. General methods include, for example, application of polymer cement mortar (hereinafter referred to as "PCM"), application of a paint material, application of a covering material, and application of a spalling prevention sheet. Any one of these, or a combination of two or more of these, can be used. All of these methods form a covering layer on the surface (surface layer) of the concrete repair surface.

[0019] For example, when applying a PCM, it is possible to form a coating layer by applying an impregnating material and / or a coating agent on top of the applied PCM. When a coating agent is applied, a coating film is formed on the PCM.

[0020] <<Mechanism of concrete repair>> Concrete renovation (concrete modification and repair) targets include newly constructed concrete structures as well as existing concrete structures that have been in service for many years. Concrete structures that have been in service for many years have been exposed to carbon dioxide for a long period of time. For this reason, carbonation is usually progressing.

[0021] There are two types of silicate-based surface impregnating materials: reactive and solidifying. The more common type is the reactive type. In methods using reactive silicate-based surface impregnating materials, a product called CSH (calcium silicate hydrate) gel is produced through a chemical reaction between calcium hydroxide and an agent, densifying the surface layer of the concrete. However, in concrete that has been neutralized, calcium hydroxide has been converted to calcium carbonate by carbon dioxide, making it difficult for a chemical reaction to occur with the reactive agent.

[0022] In the concrete repair method of this embodiment, OSMO-KK is used. As described above, OSMO-KK is a solidified silicate-based surface impregnation material produced by dissolving an alkali metal salt in lithium silicate.

[0023] Even with OSMO-KK, some CSH gel is produced by the chemical reaction between the agent and calcium hydroxide. However, the main modification mechanism when using a solidifying silicate-based surface impregnation material is the densification of concrete using the hardly soluble solidified material produced by the drying of the agent itself. For this reason, the effect of modification does not depend on the presence or absence of calcium hydroxide.

[0024] Furthermore, the OSMO-KK used in this embodiment is capable of densifying even concrete in which neutralization has progressed, due to the action of lithium silicate, alkali metal salts, etc., as shown diagrammatically in FIG.

[0025] The left side of Fig. 1 shows a state in which cracks have occurred in cement paste containing aggregate. By impregnating the neutralized layer (surface layer) of such a concrete matrix 10 with OSMO-KK, a sparingly soluble product is formed in the cracks, as shown on the right side of Fig. 1, and the concrete matrix 10 is repaired. Therefore, according to the concrete modification method of this embodiment, a satisfactory modification effect is exhibited even on concrete in which neutralization has progressed.

[0026] OSMO-KK penetrates into the concrete through tiny gaps and microcracks in the surface layer of the concrete. More specifically, part of the main component of OSMO-KK reacts with calcium hydroxide in the early stages of impregnation, and then the remaining main component becomes a poorly soluble solid as it dries, filling the voids.

[0027] Even when the concrete has become neutralized and the calcium hydroxide on the surface of the concrete has disappeared, the agent itself dries and hardens. According to OSMO-KK, the sparingly soluble product fills the voids in the concrete, densifying the surface of the concrete. As a result of permeability tests using test specimens in which neutralization had been accelerated according to the invention, a permeability inhibition effect (inhibition rate) of approximately 71% was confirmed. More specifically, in three permeability tests, test results of 65.3%, 73.6%, and 74.8% were obtained, with an average value of 71.2%. The dry solid content is calculated as the amount of dry solids per square meter of construction area. 2 It was 58g per serving.

[0028] It is recommended that OSMO-KK can be used alone up to the incubation period. The incubation period is the period when no visible changes are observed and the chloride ion concentration at the cover of the steel material drops to the corrosion threshold concentration (1.2 kg / m 3 ) during this period. During this period, the rebar is not corroded. If deterioration has progressed beyond this stage, it is advisable to remove chloride ions and repair the cross section. By doing this, it becomes possible to more reliably repair concrete that has deteriorated beyond the incubation period using OSMO-KK.

[0029] In addition, when using OSMO-KK, apply the original solution twice in a dry state (total 300g / m 2 =150g / m 2 It is recommended to apply at least 1000 times the amount of water (1000 times the amount of water per ...

[0030] In this embodiment, the components of OSMO-KK are lithium silicate, caustic soda, caustic potash, and water. The ratio of each component (OSMO-KK composition) is 15% by weight lithium silicate, 2% by weight caustic soda (sodium hydroxide), 1% by weight caustic potash (potassium hydroxide), and 83% by weight water.

[0031] The composition of OSMO-KK is not limited to the above example, and can be, for example, 13 to 17 wt % lithium silicate, 1.5 to 2.5 wt % caustic soda, 0.5 to 1.5 wt % caustic potash, and the remainder water.

[0032] More preferably, the mixture may contain 14 to 16% by weight of lithium silicate, 1.75 to 2.25% by weight of caustic soda, 0.75 to 1.25% by weight of caustic potash, and the remainder water.

[0033] Increasing the proportion of lithium silicate makes it difficult for the solidified silicate-based surface impregnating material to impregnate concrete. For example, making the agent more concentrated increases the viscosity, making impregnation more difficult. Any agent that does not soak into the concrete surface will drip off. This reduces the amount of agent that can be supplied to the inside of the concrete. Any agent that does not drip off will form a glassy film on the concrete surface, which can inhibit the adhesion of adhesives and whiten the concrete surface. However, by setting the composition appropriately as described above, a solidified silicate-based surface impregnating material with a viscosity that allows it to easily impregnate into tiny voids and microcracks in the concrete can be obtained.

[0034] Thus, one of the reasons why OSMO-KK has a moderately good impregnation property (ease of impregnation) even though it is a solidified silicate-based surface impregnation material is thought to be that it is manufactured by dissolving an alkali metal salt in lithium silicate. Although the mechanism of action is not clearly understood, the inventors believe that the alkali metal salt (sodium silicate, potassium silicate, etc.) may have contributed to improving the impregnation property of the impregnation material.

[0035] As a result of obtaining good impregnation, good test results were obtained in tests of adhesive strength, dynamic friction coefficient, etc., as shown in Figures 2 to 5 below. Therefore, according to the OSMO-KK of this embodiment, it is possible to densify the surface layer of concrete in which neutralization has progressed. Note that the impregnation depth in this embodiment is, for example, about 2 to 4 mm (more preferably 2.5 to 3.5 mm, and even more preferably about 3 mm) from the surface of the concrete.

[0036] <Advantages of the concrete repair method according to the embodiment> As described above, according to the concrete repair method of this embodiment, OSMO-KK is used as a solidified lithium silicate-based surface impregnation material. OSMO-KK is produced by dissolving an alkali metal salt in lithium silicate. Therefore, even if the concrete is neutralized, it can exhibit a good modification effect. For example, even in cases where a sufficient modification effect cannot be obtained using the type of method disclosed in the above-mentioned Patent Document 1, the OSMO-KK of this embodiment can exhibit a sufficient modification effect.

[0037] Furthermore, the concrete repair method according to this embodiment allows the inside of the concrete to be modified. In other words, in the concrete repair method according to this embodiment, paint is not applied to the surface, but the inside of the concrete is protected by an impregnating material.

[0038] Furthermore, when combined with a process (the second process mentioned above) of protecting the concrete surface with a protective material (PCM, paint, covering material, or anti-peeling sheet, etc.), both the inside and outside (surface) of the concrete can be protected.

[0039] In addition, for example, when a water-repellent substance is applied to the surface of concrete, it becomes difficult for adhesives to adhere to the surface, making it difficult to combine with other methods. However, according to the concrete repair method of the present embodiment, the concrete can be modified without imparting properties that inhibit adhesion to adhesives, so it is compatible with other methods and can be easily combined with other methods.

[0040] In other words, there are generally two types of surface impregnating materials: silane-based and silicate-based. Silane-based materials are more common, but because they are water-repellent impregnating materials, they are not compatible with adhesives. However, the OSMO-KK used in this embodiment is a silicate-based impregnating material, so it is compatible with adhesives and can be easily combined with other construction methods.

[0041] <Adhesive strength test results> Figures 2 and 3 show the results of adhesive strength tests that were obtained by an external testing agency. The "substrate" listed in the test results is concrete not impregnated with OSMO-KK (blank), or concrete with the surface impregnated with OSMO-KK (impregnating material-coated test specimen). In Figures 2 and 3, the company and product names listed in the "Product Name" column are not those listed in the actual test results, but have been changed to generalized names such as "Company A," "Company B," "CC-B specification paint material," "acrylic base preparation material (filler)," "epoxy base coat material (sealer)," and "epoxy resin adhesive."

[0042] According to the test results shown in Figures 2 and 3, the adhesive strength was 1.0 N / mm 2 When a material with a lithium silicate-based impregnating material on its surface is pulled by a tensile tester, a glassy substance forms on the surface of the material, making it impossible to measure in the tensile test.

[0043] In contrast, in the test results shown in Figs. 2 and 3, the adhesive strength is, for example, 3.55 N / mm 2 , 2.60N / mm 2 , 3.13N / mm 2 , 3.56N / mm 2 , 3.23N / mm 2 , 3.28N / mm 2 etc., and all results are 1.0N / mm 2 More specifically, the average adhesive strength after multiple tests (three tests in this case) is 1.1 N / mm 2 More than 3.4N / mm 2In practice, the adhesive strength is 1.0 N / mm 2 Therefore, with OSMO-KK, measurements can be made using lithium silicate-based impregnating materials while still ensuring sufficient adhesive strength.

[0044] The adhesive strength in the test results in Figures 2 and 3 is the adhesive strength between the concrete on which OSMO-KK was used and the coating material attached to the concrete (here, "CC-B specification paint material," "acrylic base preparation material (filler)," "epoxy base coating material (sealer)," and "epoxy resin adhesive," etc.). In Figures 2 and 3, the coating material is shown as the "coating material." The test is performed by fixing (adhering) a test jig to the coating material (coating material) and pulling the coating material (coating material), and observing the condition of the "substrate" and the coating material (coating material).

[0045] In addition, the above-mentioned "CC-B specification paint material," which is a type of coating material (applied material), has layers, for example, of epoxy resin primer, epoxy resin putty, flexible epoxy resin paint undercoat, and flexible fluororesin paint topcoat, which are layered in order on the concrete structure (substrate).

[0046] In addition, the "epoxy resin adhesive" has a base resin and a curing agent that contains polythiol or aliphatic polyamine, a mixed viscosity (20°C) of 5000±2000 mPa s, a base:curing agent ratio of 4:1 (by weight), and a pot life (20°C, 1 kg) of 40±10 minutes.

[0047] <Dynamic friction coefficient test results> Furthermore, impregnating concrete with OSMO-KK does not significantly change the dynamic friction coefficient of the concrete. Figure 4 shows the results of dynamic friction coefficient measurements that were obtained by an external testing agency, along with comparative examples. "Impregnating material 1" and "Impregnating material 2" in the chart in Figure 4 show the measurement results of concrete slabs impregnated with OSMO-KK. "Uncoated 1" and "Uncoated 2" in the chart in Figure 4 show the measurement results of concrete that was not impregnated with OSMO-KK (comparative examples).

[0048] FIG. 4 also shows the results of measurements taken three times for each of "Impregnating material 1," "Impregnating material 2," "Uncoated 1," and "Uncoated 2" at various measurement speeds (20 km / h, 40 km / h, 60 km / h), and the average of the three measurements (shown as "Average A"). Further to the right of this, the average of "Impregnating material 1" and "Impregnating material 2," and the average of "Uncoated 1" and "Uncoated 2" (these averages are shown as "Average B"). Further to the right of this, the "ratio" (Impregnating material / Uncoated) of the average of "Impregnating material 1" and "Impregnating material 2" and the average of "Uncoated 1" and "Uncoated 2" is shown.

[0049] The ratio value at a speed of 20km / h is 91.6%, at a speed of 40km / h is 93.6%, and at a speed of 60km / h is 97.0%.

[0050] As shown above, the "ratio" (impregnated material / uncoated) is above 91.6% in all cases. Therefore, the decrease in the dynamic friction coefficient caused by applying the impregnated material is kept to within 8.4 (= 100 - 91.6)%.

[0051] <Waterproofing test results> Furthermore, concrete impregnated with OSMO-KK has improved water impermeability (water permeability control). The reasons for this improvement in water permeability include the proportions of lithium silicate, caustic soda (sodium hydroxide), and caustic potash (potassium hydroxide) in the agent, as well as the amount applied per unit area. With this appropriate composition and application amount, it has become possible to supply a sufficient amount of lithium silicate to the surface layer of the concrete.

[0052] The chart in Figure 5 shows the results of a permeability test conducted by an external organization. The test results in Figure 5 are from a permeability test in which a silicate-based surface impregnating material was applied over two types of PCM (PCM1, PCM2). "As is" specimens show PCM1 and PCM2 that were not coated with OSMO-KK, while "with OSMO-KK" shows PCM1 and PCM2 that were coated with OSMO-KK.

[0053] According to the test results in FIG. 5, the average permeability of PCM1 and PCM2 without OSMO-KK was 5.2% and 16.49%, respectively, while the average permeability of PCM1 and PCM2 with OSMO-KK was 3.32% and 7.48%, respectively. In addition, the permeability ratio, which is the ratio of the average permeability (with OSMO-KK / original specimen) of multiple tests (three times in this case), was 64% for PCM1 and 45% for PCM2. If 100-permeability ratio (%) is the inhibition rate, the inhibition rates of PCM1 and PCM2 were 36% (=100%-64%) and 55% (=100%-45%), respectively. In addition, as mentioned above, in a permeability test of the concrete repair surface conducted by the applicant separately from the experiment in FIG. 5, the inhibition rate was about 71%.

[0054] The lower the amount of water permeability compared to the original test specimen, the higher the inhibition rate. From the test results in Figure 5, it is believed that OSMO-KK is effective when applied to concrete with a low cement content. The fact that it is effective even with a low cement content suggests that it is also effective for concrete that has been neutralized and has reduced calcium hydroxide.

[0055] For example, as disclosed in the above-mentioned Patent Document 1, in the case of a sodium silicate-based impregnating material containing carboxylic acid and a repair method using the same, it is believed that the use of a sodium silicate-based impregnating material using carboxylic acid makes it possible to carry out thin-coat repair of polymer cement mortar. Furthermore, this type of repair material and repair method is believed to be able to supplement conventional methods.

[0056] However, the effectiveness of this type of repair material and repair method on concrete with advanced neutralization has not been confirmed.In addition, this type of repair material is not thought to change the roughness coefficient (a value that indicates the roughness of the walls and bottom of the waterway).

[0057] Furthermore, the OSMO-KK of this embodiment is not intended to impart alkali to concrete, but rather to repair concrete.

[0058] <Other> It should be noted that the above-described embodiments are merely examples of the implementation of the present invention, and the technical scope of the present invention should not be interpreted as being limited thereby. In other words, the present invention can be implemented in various forms without departing from the gist or main characteristics thereof. [Explanation of symbols]

[0059] 10: Concrete base material

Claims

1. A concrete repair material comprising an aqueous solution containing 13-17% by weight lithium silicate and 1.5-2.5% by weight sodium hydroxide.

2. A method for repairing concrete that can be performed on concrete whose deterioration process is in the latent period and on concrete whose deterioration process is in the latent period or later, comprising the steps of:

2. When the concrete surface is in a dry state, the concrete repair material according to claim 1 is applied to the concrete surface and dried to form a concrete repair surface; The method for repairing concrete has a water permeability test on the repaired surface of the concrete, and the water permeability test results in a water inhibition rate of 65.3 to 74.8%.

3. 3. The method for repairing concrete according to claim 2, further comprising the steps of: first applying the concrete repair material according to claim 1 to a surface layer of the concrete surface to be repaired; and then drying the applied material to form a protective layer.

4. 4. The method for repairing concrete according to claim 3, further comprising the step of: secondly applying the concrete repair material according to claim 1 to a surface layer of the reinforced concrete surface; and drying the applied material to form a protective layer.

5. The average adhesive strength between the concrete using the concrete repair material according to claim 1 and the coating material attached to the concrete is 1.1 N / mm 2 3.4N / mm or more 2 Below are methods for repairing concrete.

6. A method for repairing concrete, in which the average decrease in dynamic friction coefficient is within 8.4% when the concrete repair material according to claim 1 is used.