Three-dimensional molding method and three-dimensional molding apparatus
The method enhances three-dimensional modeling by filling cavities with a high-melting-point powder and providing an escape route to prevent deformation during sintering, thus improving the quality of objects with internal cavities.
Patent Information
- Application Number
- JP2023199303
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2023-11-24
- Publication Date
- 2024-10-03
AI Technical Summary
The molding quality in three-dimensional modeling methods using powder layering is compromised due to deformation of the green body during sintering, particularly when a cavity is present inside the object.
A method involving a three-dimensional modeling process that includes forming an object with a cavity, filling the cavity with a second powder having a higher melting point than the sintering temperature, and providing an opening to allow discharge of the second powder during sintering, thereby preventing deformation of the green body.
The method improves modeling quality by preventing deformation and damage to the green body during sintering by allowing the second powder to escape through the opening, maintaining the structural integrity of the object.
Smart Images

Figure 2024134506000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a three-dimensional object fabrication method and a three-dimensional object fabrication apparatus. [Background technology]
[0002] Known methods of three-dimensional modeling using powder lamination (powder lamination modeling) include the binder jet (BJ) method, in which a modeling liquid is applied to a powder layer.
[0003] Patent Document 1 discloses a method of filling a cavity formed inside a green body with powder and sintering the body with an object attached to the cavity. Summary of the Invention [Problem to be solved by the invention]
[0004] However, in the method of Patent Document 1, there is a possibility that the molding quality may decrease due to deformation of the green body during sintering.
[0005] The present invention aims to improve the molding quality. [Means for solving the problem]
[0006] A three-dimensional modeling method according to one aspect of the present invention is a method for producing a modeled object having an internal cavity, the modeled object including an opening connecting the cavity to an outside of the modeled object, and includes a modeling process for modeling the modeled object with a first powder, a filling process for filling the cavity with a second powder through the opening, a sintering process for sintering the modeled object with the second powder filled in the cavity in the filling process, and a removal process for removing the second powder within the cavity through the opening. Effect of the Invention
[0007] According to the present invention, the molding quality can be improved. [Brief description of the drawings]
[0008] [Figure 1]A diagram showing an example of a model and a green body. [Diagram 2] FIG. 1 is a block diagram showing a schematic configuration of a three-dimensional object forming apparatus according to an embodiment of the present invention; [Diagram 3] FIG. 1 is a diagram showing an example of the configuration of a modeling unit; [Figure 4] Hardware configuration of the control unit [Diagram 5] 1 is a flowchart of a three-dimensional modeling method according to an embodiment of the present invention. [Figure 6] Schematic diagram showing a first example of the structure of a molded object [Figure 7] Schematic diagram showing a second example of the structure of the object [Figure 8] Schematic diagram showing a third example of the structure of a molded object [Figure 9] FIG. 4 is a schematic diagram showing a fourth example of the structure of a molded object. [Figure 10] FIG. 5 is a schematic diagram showing a fifth example of the structure of a molded object. [Figure 11] FIG. 6 is a schematic diagram showing a sixth example of the structure of a molded object; [Figure 12] FIG. 7 is a schematic diagram showing a seventh example of the structure of a molded object. [Figure 13] FIG. 13 is a schematic diagram showing an eighth example of the structure of a molded object. [Figure 14] FIG. 9 is a schematic diagram showing a ninth example of the structure of a molded object. [Figure 15] Cross section along the line AA in Figure 14(C) [Figure 16] FIG. 10 is a schematic diagram showing a tenth example of the structure of a molded object. [Figure 17] FIG. 1 shows a first example of a method for preventing the sealing member from coming off. [Figure 18] FIG. 13 is a diagram showing a second example of a method for preventing the sealing member from coming off. [Figure 19] A diagram showing an example of a gyroid structure provided in the internal cavity of a molded object. [Figure 20] A diagram showing the range of acceptable opening diameters [Figure 21] FIG. 13 shows a modified example of the molding part. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment will be described with reference to the drawings. In order to facilitate understanding of the description, the same components in each drawing are denoted by the same reference numerals as much as possible, and duplicated description will be omitted.
[0010] In the following description, the molded object 62 includes the first powder. The molded object 62 is an assembly formed by stacking a plurality of molded layers 61, and is in a state before the molding is completed. The powder 50 includes a metal, and for example, aluminum or an aluminum alloy can be used as the metal. The powder 50 may be made of other metals, or may be made of materials other than metals, such as ceramics. The molded object 62 that has been subjected to a drying process and from which the excess powder 50 has been removed is called a "green body 63." Furthermore, the finished product after the green body 63 has been subjected to degreasing and sintering processes is called a "three-dimensional molded object 64."
[0011] In the following description, the second powder 52 is a different type of powder from the powder 50 used to form the molded object 62. The second powder 52 is filled into the cavity 81 inside the green body 63 during the sintering process. The melting point of the second powder 52 is higher than the sintering temperature in the sintering process. The second powder 52 has a higher melting point than the first powder 50. For example, when the first powder 50 contains a metal, such as aluminum or an aluminum alloy, the second powder 52 may be made of zirconia, lumina, or the like.
[0012] In addition, the term "mixed powder" used in the following description refers to a plurality of powders mixed by the powder mixing unit 2. The mixed powder includes new powder (hereinafter referred to as "new powder") and recovered powder (hereinafter referred to as "recovered powder"). The new powder is powder that has not been used for modeling in the modeling unit 3. The recovered powder is powder that has been used for modeling in the modeling unit 3. The recovered powder may be recovered from the modeling unit 3 or from the powder removal unit 5. The "mixing ratio" refers to the ratio of the powder content in the mixed powder to the powder content in the modeling unit 3. The ratio of new powder to recovered powder is shown. The "mixing ratio" can be any type, such as volume ratio or weight ratio. The ratio can be applied.
[0013] Fig. 1 is a schematic diagram showing an example of a shaped object 62 and a green body 63. Fig. 1(A) is a schematic diagram showing the shaped object 62. Fig. 1(B) is a schematic diagram showing the green body 63.
[0014] 1(A), multiple powders 50 are arranged in the Y and Z directions in the modeling tank 12. A modeling liquid 60 is applied to some of the multiple powders 50 in the modeling tank 12 to form a modeling layer 61, and the modeling layers 61 are stacked in the Z direction to form a modeled object 62. The areas of the multiple powders 50 other than the modeled object 62 are areas to which the modeling liquid 60 is not applied.
[0015] The modeling tank 12 is dried by the drying section 4, and the powder 50 is removed by the powder removing section 5 from the area where the modeling liquid 60 has not been applied, to obtain a green body 63 as shown in FIG. 1(B).
[0016] As a result, the green body 63 has a cavity 81 inside and includes an opening 82 connecting the cavity 81 with the outside of the green body 63. Hereinafter, the shape of the green body 63 will be described as including the cavity 81 and the opening 82 inside.
[0017] <Basic configuration of 3D modeling device> A basic configuration of a three-dimensional object forming apparatus 1 according to the embodiment will be described with reference to FIGS.
[0018] 2 is a block diagram showing a schematic configuration of a three-dimensional object forming apparatus 1 according to an embodiment of the present invention. As an example of the three-dimensional object forming apparatus 1 according to an embodiment of the present invention, a binder jet (BJ) method is described below in which a modeling liquid 60 is applied to a modeling region on the surface of a powder layer 51. In the BJ method, a three-dimensional object can be formed by selectively applying the modeling liquid 60 to the powder layer 51, solidifying it, and sintering it. The modeling liquid 60 contains, for example, a resin such as a binder and an ink such as a solvent.
[0019] The three-dimensional modeling apparatus 1 includes a powder mixing unit 2, a modeling unit 3, a drying unit 4, a powder removing unit 5, a filling unit 6, a sintering unit 7, a removing unit 8, a collecting unit 9, and a control unit 100.
[0020] The powder mixing unit 2 mixes the powder 50. In this way, a mixed powder is generated as the powder to be supplied to the modeling unit 3. The powder mixing unit 2 mixes new powder (new powder) that has not yet been used for modeling with powder (recovered powder) that has already been used for modeling and collected by the collection unit 9. Furthermore, the powder mixing unit 2 can mix the mixed powder at a desired mixing ratio based on a control command from the control unit 100 and supply it to the modeling unit 3.
[0021] The modeling unit 3 models a modeled object 62 containing the powder 50. The powder 50 includes at least mixed powder supplied from the powder mixing unit 2. In this embodiment, the modeling unit 3 performs modeling by the BJ method. Note that a part of the powder 50 used in the modeling unit 3 is collected in the collection unit 9 as collected powder. More specifically, the modeling unit 3 forms a powder layer 51. Note that the powder layer 51 may be a flattened layer. Also, a modeling layer 61 is formed by applying a modeling liquid 60 to the powder layer 51. The modeling layer 61 is a layered modeled object in which the powder 50 is bonded by applying the modeling liquid 60. Note that the powder layer 51 and the modeling layer 61 each refer to a single layer.
[0022] An example of the operation of the modeling unit 3 will now be described with reference to Fig. 3. Fig. 3 is a diagram showing an example of the configuration of the modeling unit 3.
[0023] In the following description, the X, Y, and Z directions are perpendicular to each other. The X and Y directions are horizontal, and the Z direction is vertical. The X direction is the axial direction of the rotation axis of the flat section 31. The Y direction is the movement direction of the flat section 31, and is the arrangement direction of the supply tank 11, the modeling tank 12, and the surplus powder tank 15 in the powder tank 10. The Z direction is the ascending and descending direction of the supply stage 13 and the modeling stage 14. In the following description, for convenience of explanation, the positive Z direction may be referred to as the upper side, and the negative Z direction may be referred to as the lower side.
[0024] The modeling section 3 includes a powder tank 10, a lamination unit 30, and an application section 40.
[0025] The powder tank 10 forms a powder layer 51 containing powder 50. The application unit 40 applies a modeling liquid 60 to the powder layer 51 to form a modeling layer 61. In the modeling unit 3, a plurality of modeling layers 61 are stacked to form a model 62.
[0026] The powder tank 10 includes a supply tank 11, a modeling tank 12, a supply stage 13, a modeling stage 14, and a surplus powder tank 15. The powder tank 10 has a box-like shape. The tops of the supply tank 11, the modeling tank 12, and the surplus powder tank 15 are open.
[0027] The supply tank 11 of the powder tank 10 is a tank that supplies the powder 50 to the modeling tank 12. The supply tank 11 holds the powder 50 to be supplied to the modeling tank 12. A supply stage 13 is provided at the bottom of the supply tank 11. The supply stage 13 moves up and down in the vertical direction (Z direction). The side of the supply stage 13 is disposed so as to contact the inner side of the supply tank 11.
[0028] The powder 50 required for modeling is supplied from the supply tank 11 to the modeling tank 12 of the powder tank 10. A powder layer 51 and a modeling layer 61 are formed in the modeling tank 12. Furthermore, a plurality of modeling layers 61 are stacked in the modeling tank 12, and a model 62 is formed.
[0029] A supply stage 13 and a modeling stage 14 are provided at the bottom of the supply tank 11 and the modeling tank 12, respectively, and move up and down in the vertical direction (Z direction). The side of the modeling stage 14 is disposed so as to contact the inner side of the modeling tank 12. The upper surfaces of the supply stage 13 and the modeling stage 14 are kept horizontal.
[0030] The surplus powder tank 15 of the powder tank 10 is a tank that holds surplus powder 50 among the powder 50 flattened by the flat portion 31 when forming the powder layer 51. A means for sucking the powder 50 may be provided at the bottom of the surplus powder tank 15, or a means for removing the surplus powder tank 15 may be provided. The surplus powder tank 15 is disposed next to the modeling tank 12. The surplus powder 50 held in the surplus powder tank 15 is collected by the collection unit 9 using any of the above-mentioned methods, and is resupplied from the collection unit 9 to the powder mixing unit 2 as collected powder.
[0031] The powder 50 held in the supply tank 11 is appropriately replenished by the mixed powder supplied by the powder mixing unit 2 at any timing, such as before modeling in the modeling unit 3 starts or when the amount of powder 50 in the supply tank 11 decreases. Note that, although the powder tank 10 has been exemplified as having two tanks, the supply tank 11 and the modeling tank 12, the supply tank 11 may not be provided and the powder 50 may be directly supplied from the powder mixing unit 2 to the modeling tank 12.
[0032] Methods for transporting the powder 50 from the powder mixing section 2 to the supply tank 11 include a screw conveyor method using a screw, a pneumatic transport method using air, and the like.
[0033] In addition, the powder tank 10 divides the inner space of a single box into three spaces along the Y direction to form the supply tank 11, the modeling tank 12, and the surplus powder tank 15. Alternatively, the powder tank 10 may be configured such that the supply tank 11, the modeling tank 12, and the surplus powder tank 15 are each formed as a separate box. In this case, it is preferable to install the supply tank 11 and the modeling tank 12 so that the surfaces facing in the Y direction of the supply tank 11 and the modeling tank 12 are in close contact with the surfaces facing in the Y direction of the modeling tank 12 and the surplus powder tank 15. This makes it possible to prevent the powder 50 from leaking out when moving the powder 50 between the tanks, and to ensure the movement of the powder 50. In addition, it is possible to easily transport the modeling tank 12 containing the modeled object modeled in the modeling unit 3 to the drying unit 4 or the powder removing unit 5.
[0034] The lamination unit 30 also has a flat portion 31 and a powder removal portion 32 .
[0035] The flat part 31 of the lamination unit 30 flattens the modeling layer 61 and the powder layer 51. The flat part 31 flattens the modeling layer 61 by rotating the recoater as a rotating body. The flat part 31 rotates to supply the powder 50 from the supply stage 13 of the supply tank 11 to the modeling tank 12, forming the powder layer 51. The flat part 31 moves back and forth in the Y direction along the stage surface (the surface on which the powder 50 is loaded) of the modeling stage 14. More specifically, the flat part 31 moves horizontally from the outside of the supply tank 11 to pass above the supply tank 11 and the modeling tank 12. As a result, the powder 50 is transferred and supplied onto the modeling tank 12, and the flat part 31 flattens the powder 50 while passing over the modeling tank 12, forming the powder layer 51. The flat part 31 is a member longer than the inner dimensions of the modeling tank 12 and the supply tank 11. Note that the flat part 31 may be a blade or a bar as a plate-shaped member.
[0036] Powder removing part 32 of lamination unit 30 removes powder 50 adhering to flat part 31. Powder removing part 32 moves together with flat part 31 while being in contact with the peripheral surface of flat part 31.
[0037] The application unit 40 includes a carriage 41 and a head 42 .
[0038] The head 42 applies the modeling liquid 60 to the powder layer 51. The head 42 is, for example, an inkjet head, and is provided with a nozzle row in which a plurality of nozzles are arranged. A colored model may be formed by applying a cyan modeling liquid, a magenta modeling liquid, a yellow modeling liquid, and a black modeling liquid, or a modeling liquid of one color may be applied from a plurality of nozzles. The modeling liquid 60 may be applied by an inkjet method or a dispenser method.
[0039] At least one head 42 is mounted on a carriage 41, and moves back and forth in the X (main scanning), Y (sub-scanning), and Z directions by a motor, a guide member, and the like. An example of the operation of the modeling unit 3 has been described above.
[0040] Returning to FIG. 2, the three-dimensional modeling apparatus 1 will be described. The drying unit 4 dries the model 62 formed by the modeling unit 3. Specifically, the drying unit 4 dries the solvent and the like contained in the modeling liquid 60 contained in the model 62. In the drying unit 4, the modeling tank 12 containing the model 62 formed by the modeling unit 3 is heated and decompressed to dry it. As a result, the powder 50 is fixed by the binder contained in the modeling liquid 60.
[0041] The powder removal unit 5 removes excess powder 50 from the model 62 dried by the drying unit 4. The powder removal unit 5 uses any method, such as blowing air to remove the powder. The powder removal unit 5 removes the powder 50 that has not been applied with the modeling liquid 60 from the modeling tank 12 and has not adhered thereto. As a result, the powder removal unit 5 obtains a three-dimensional object that is adhered with the binder, i.e., a green body (G body) 63. The powder 50 removed by the powder removal unit 5 is collected by the collection unit 9 as collected powder.
[0042] The filling unit 6 fills the second powder 52 into the cavity 81 inside the green body 63 obtained in the powder removing unit 5. The filling unit 6 inserts, for example, a hollow tube into the cavity 81 from an opening 82, and inserts the second powder 52 through the tube. In this manner, the second powder 52 can be filled into the cavity 81. Note that the filling unit 6 may use any method other than the above-mentioned method to fill the cavity 81 with the second powder 52.
[0043] The sintering unit 7 sinters the green body 63 to generate a final three-dimensional object (S body) 64. The sintering unit 7 removes the binder from the green body 63 (debinding) and sinters the green body 63, for example, in a sintering furnace. Particularly in this embodiment, the sintering unit 7 debinding and sinters the green body 63 in a state in which the second powder 52 has been filled into the internal cavity 81 by the filling unit 6.
[0044] The removal unit 8 removes the second powder 52 remaining from the cavity 81 of the three-dimensional object 64 after the degreasing and sintering processes are performed by the sintering unit 7. The removal unit 8 can use any method, such as blowing air to blow away the second powder 52.
[0045] The recovery unit 9 recovers at least a portion of the powder 50 in the modeling unit 3 as recovered powder. The recovery unit 9 also recovers the powder 50 from the powder removing unit 5. The recovery unit 9 supplies the recovered powder to the powder mixing unit 2.
[0046] The control unit 100 controls the above-mentioned operations of each unit of the 3D modeling apparatus 1.
[0047] FIG. 4 is a diagram showing an example of a hardware configuration of the control unit 100. As shown in FIG. 4, the control unit 100 of the 3D printing apparatus 1 includes a CPU 101 (Central Processing Unit), a ROM 102 (Read Only Memory) for storing a program for executing control and other fixed data, and a RAM 103 (Random Access Memory) for temporarily storing printing data and the like. The control unit 100 also receives printing data from a printing data creation device 104 such as an external computer. The printing data creation device 104 creates printing data by slicing a 3D object 64 in a final form into printing layers 61. The control unit 100 performs a printing operation for each printing layer 61. The printing data creation device 104 may be separate from the 3D printing apparatus 1 or may be integrated with the 3D printing apparatus 1. The control unit 100 may be located inside the 3D printing apparatus 1 or outside the 3D printing apparatus 1.
[0048] <3D modeling method> Fig. 5 is a flowchart of a three-dimensional object forming method according to an embodiment of the present invention. The flowchart shown in Fig. 5 shows a flow of a series of operations for forming a three-dimensional object 64 performed by the three-dimensional object forming apparatus 1 according to this embodiment.
[0049] In step S1, the control unit 100 receives shaping data from the shaping data creating device 104. The control unit 100 outputs a control command based on the shaping data to each element of the three-dimensional object forming apparatus 1.
[0050] In step S2, the new powder and the recovered powder are mixed in a predetermined ratio by the powder mixing unit 2 based on the control command input from the control unit 100 in step S1 to prepare a mixed powder. The mixed powder mixed in the powder mixing unit 2 is supplied to the modeling unit 3 and used as powder 50 for modeling the model 62. Note that the powder 50 may not be a mixed powder, and may consist of only new powder or only recovered powder.
[0051] In step S3, the modeling unit 3 creates a modeled object 62 using the powder 50 supplied from the powder mixing unit 2 in step S2 based on the control command input from the control unit 100 in step S1 (modeling process). The modeling process includes a process of forming a powder layer 51 with the first powder 50 and a process of applying a modeling liquid 60 to the powder layer 51. In particular, in this embodiment, the modeling unit 3 uses the powder 50 to model a modeled object 62 having an internal cavity 81 and an opening 82 connecting the cavity 81 to the outside. The modeling tank 12 in which the modeled object 62 is accommodated is transported from the modeling unit 3 to the drying unit 4. In addition, surplus powder overflowing from the modeling tank 12 in the modeling unit 3 is collected by the collection unit 9 and supplied to the powder mixing unit 2.
[0052] In step S4, the drying unit 4 dries the model 62 formed in step S3. The drying unit 4 dries the model at a drying temperature and for a drying time according to a control command from the control unit 100. The modeling tank 12 containing the model 62 after drying is transported from the drying unit 4 to the powder removing unit 5.
[0053] In step S5, the powder removing unit 5 removes the excess powder 50 (excess powder) from the shaped object 62 dried in step S4 to produce a green body 63 (powder removing step). The green body 63 from which the excess powder has been removed is transported from the powder removing unit 5 to the filling unit 6. The excess powder is also collected by the collecting unit 9 and supplied to the powder mixing unit 2.
[0054] In step S6, the filling unit 6 fills the cavity 81 of the green body 63 created in step S5 with the second powder 52 through the opening 82 (filling step). The filling unit 6 inserts, for example, a hollow tube into the cavity 81 through the opening 82, and inserts the second powder 52 through the tube. In this manner, the second powder 52 can be filled into the cavity 81. Note that in the filling step of step S6, instead of the filling unit 6, an operator may manually fill the second powder 52 into the cavity 81. The green body 63 filled with the second powder 52 is transported from the filling unit 6 to the sintering unit 7.
[0055] In step S7, the sintering unit 7 performs a degreasing process on the green body 63 filled with the second powder 52 in step S6 (degreasing process). By this process, the binder component of the molding liquid 60 is removed from the green body 63.
[0056] In the degreasing process of step S7, the green body 63 is degreased using a degreasing device included in the sintering unit 7, for example. Specifically, the green body 63 is heated to a temperature equal to or higher than the thermal decomposition temperature of the resin, so that the resin contained in the green body 63 is degreased. In detail, the degreasing process may be performed by decomposing a resin component including an acrylic material at a temperature higher than the thermal decomposition temperature and lower than the melting point or solidus temperature of pure aluminum or an aluminum alloy material. Depending on the resin component contained in the green body 63, it is possible to set a plurality of heating and holding temperatures. Alternatively, instead of heating, a degreasing method using solvent extraction may be applied in which the green body 63 is immersed in a solvent to extract the resin.
[0057] In step S8, the sintering unit 7 fills the cavity 81 with the second powder 52 in step S6 and sinters the green body 63 that has been degreased in step S7 (sintering process). During the sintering process, for example, from the start of sintering to the end of sintering, a part of the second powder 52 is discharged from the cavity 81 through the opening 82. The green body 63 is sintered by the sintering process to generate a three-dimensional object 64. The three-dimensional object 64 in a state in which the cavity 81 is filled with the second powder 52 after the sintering process is transported from the sintering unit 7 to the removal unit 8.
[0058] In the sintering process of step S8, the degreased green body 63 is sintered, for example, using a sintering device included in the sintering unit 7. Specifically, the green body 63 is heated at a temperature higher than that in the degreasing process to obtain a three-dimensional object 64 (sintered body of the green body) integrated with pure aluminum or aluminum alloy material. Here, the aluminum alloy material includes Al-Cu, Al-Mn, Al-Mg, Al-Si, Al-Si-Mg, Al-Si-Cu, Al-Zn-Mg, Al-Li alloys, or alloy materials similar thereto.
[0059] In the sintering process, the degreased green body 63 is heated to a temperature between the aluminum liquidus and solidus at a rate of 1°C / h (hour) to 200°C / h, and then the temperature is maintained for about 1 to 10 hours. More specifically, the maximum temperature is preferably a temperature at which 10 to 50% of the aluminum liquid phase is generated. The rate of temperature rise may be changed midway. The degreasing and sintering processes are carried out in vacuum, Ar, H 2 , N 2 After heating, the inside of the apparatus is cooled and the sintered body is taken out.
[0060] For example, when degreasing a green body 63 containing AlSi10Mg and acrylic resin, it is heated to a temperature equal to or higher than the decomposition temperature of the acrylic resin and equal to or lower than the solidus temperature (about 570°C) of AlSi10Mg. Furthermore, when sintering, the green body 63 is heated at a temperature equal to or higher than the solidus temperature (about 570°C) and equal to or lower than the liquidus temperature (about 600°C) for 1 to 10 hours.
[0061] The degreasing process in step S8 and the sintering process in step S9 may be carried out consecutively using the same degreasing / sintering apparatus such as the sintering section 7 of this embodiment, or may be carried out using separate degreasing and sintering apparatuses.
[0062] In step S9, the removal unit 8 removes the second powder 52 from the cavities 81 of the three-dimensional object 64 that has been sintered in step S8 (removal process). The removal unit 8 can remove the second powder 52 from the cavities 81 by using any method, such as blowing air to blow away the second powder 52. In the removal process of step S9, the second powder 52 may be manually removed from the cavities 81 by an operator instead of the removal unit 8. In addition, in the removal process, it is preferable to also remove other holders such as a green body setter, a ceramic paper block setter, and a ceramic powder setter outside the object. When the process of step S9 is completed, this control flow ends.
[0063] Fig. 6 is a schematic diagram showing a first example of the structure of a molded object. Fig. 6(A) is a cross-sectional view of the molded object, and Fig. 6(B) is a schematic diagram showing a part 52A of the second powder being discharged from a cavity 81 through an opening 82. The molded object has an internal cavity 81 and a single opening 82 that connects the cavity 81 with the outside of the molded object. The cavity 81 is filled with the second powder 52.
[0064] As shown in FIG. 6(A), the green body 63 is sintered by the sintering unit 7 in a state where the second powder 52 is filled in the cavity 81 through the opening 82. When the sintering is completed, a three-dimensional object 64 is generated as shown in FIG. 6(B). During sintering, the volume of the internal cavity 81 is reduced as the external shape of the green body 63 shrinks. Therefore, the amount of the second powder 52 that can be filled in the cavity 81 also changes as the shrinkage occurs. In particular, in this embodiment, as the cavity 81 of the green body 63 shrinks, a part 52A of the second powder that can no longer be contained in the cavity 81 is discharged from the opening 82 to the outside of the green body 63. This suppresses the effect of the shrinkage of the external shape of the green body 63, and improves the molding quality.
[0065] Moreover, the opening 82 is smaller than the diameter of the cavity 81. The opening 82 is provided on the side surface of the green body 63. Furthermore, the opening 82 is provided at the longitudinal end of the cavity 81. For example, the cavity 81 is formed so that the longitudinal direction is the Y direction. The opening 82 is formed at the end of the cavity 81 on the negative Y direction side. Since the opening 82 is formed on the longitudinal side where the cavity 81 has a greater degree of shrinkage, the second powder 52 can be easily discharged to the outside through the opening 82.
[0066] Here, the advantages of filling the second powder 52 into the cavity 81 inside the shaped object 62 will be described. The green body 63 degreased in the degreasing step becomes very brittle, and there is a risk that the green body 63 will collapse due to a certain stress. In addition, since the green body 63 is very brittle during sintering, the green body 63 may suffer from problems such as deformation and breakage.
[0067] This problem is particularly noticeable when the shaped object 62 has an internal cavity 81. In the 3D modeling apparatus 1 according to this embodiment, when a 3D object 64 having an internal cavity 81 is to be manufactured, the internal cavity 81 of the green body 63 is filled with the second powder 52 in the filling step. This improves the strength of the green body 63 in the sintering step, and prevents deformation and damage of the green body 63.
[0068] However, while the green body 63 densifies and shrinks during the sintering process, the second powder 52 does not shrink. Therefore, if the entire second powder 52 remains in the cavity 81 of the green body 63 from the start to the end of the sintering process, the cavity 81 may expand and deform the green body 63.
[0069] Therefore, in this embodiment, an opening 82 through which the second powder 52 is discharged is provided in the shaped object 62. Specifically, the opening 82 connecting the cavity 81 inside the shaped object 62 to the outside is provided in advance by the shaping unit 3. As a result, when the green body 63 shrinks during the sintering process, the second powder 52 flows in accordance with the shrinkage of the green body 63, and a part 52A of the second powder is discharged from the opening 82. This makes it possible to prevent deformation or damage of the green body 63 due to the effect of the second powder 52 filled in the cavity 81.
[0070] The second powder 52 preferably has a higher melting point than the powder 50. When the powder 50 is made of aluminum or an aluminum alloy, the second powder 52 is preferably made of ceramic, and it is particularly preferable to use alumina (melting point: 2072°C) or zirconia (melting point: 2715°C).
[0071] In addition, the second powder 52 filled in the cavity 81 needs to be discharged from the cavity 81 through the opening 82 to the outside of the green body 63 as it shrinks during sintering, so the second powder 52 needs to have fluidity. Indices that represent the fluidity include sphericity, particle size distribution, and angle of repose.
[0072] In addition, since it is preferable for the second powder 52 to fill the voids 81 as completely as possible, the smaller the particle size, the better. The above are the characteristics required for the second powder 52 in this embodiment.
[0073] The shape of the cavity 81 may be any shape depending on the part to be manufactured. For example, when the three-dimensional object 64 is a heat sink, the cavity 81 forms a flow path inside the heat sink. The smaller the volume of the cavity 81, the less the amount of the second powder 52 will be as the green body 63 shrinks, and therefore the occurrence of deformation or damage can be prevented. In addition, the larger the cross-sectional area of the opening 82, the better. In addition, since the shape of the opening 82 shrinks during the sintering process, it is preferable that the diameter of the opening 82 is a dimension that can be maintained even after shrinkage.
[0074] When the three-dimensional object 64 is a heat sink, the opening 82 can serve as both the inlet and outlet of the fluid of the heat sink. In this case, the opening 82 is preferably circular, which is easy to process in order to connect components. The diameter of the opening 82 is preferably, for example, about 12 mm. If the opening 82 can serve as both the inlet and outlet of the fluid in this way, there is no need to add a relief hole to the modeling data, and modeling efficiency can be improved.
[0075] The three-dimensional object fabrication method according to this embodiment is a method for manufacturing a shaped object 62 having a cavity 81 therein, the shaped object 62 including an opening 82 connecting the cavity 81 to the outside of the shaped object 62, and includes a fabrication step S3 of fabricating the shaped object 62 with powder 50, a filling step S6 of filling the cavity 81 with a second powder 52 through the opening 82 of the shaped object 62 fabricated in the fabrication step S3, a sintering step S8 of sintering the green body 63 in which the cavity 81 has been filled with the second powder 52 in the filling step S6, and a removal step S9 of removing the second powder 52 in the cavity 81 through the opening 82. The melting point of the second powder 52 is higher than the sintering temperature in the sintering step S8.
[0076] With this configuration, the cavity 81 of the shaped object 62 is filled with the second powder 52 in the filling step S6 and then sintered in the sintering step S8. Even if the green body 63 shrinks during the sintering step and stress that deforms the cavity 81 occurs, the deformation can be suppressed by the second powder 52 filled in the cavity 81. In addition, the cavity 81 also shrinks as the green body 63 shrinks during the sintering step. Therefore, if there is no escape route for the second powder 52 filled in the cavity 81, the inner wall of the cavity 81 is pressed outward by the second powder 52 inside the cavity as the cavity 81 shrinks, and there is a risk that the green body 63 will be deformed so as to be curved outward. In contrast, in this embodiment, as the cavity 81 shrinks, a part 52A of the second powder 52 is discharged to the outside of the green body 63 through the opening 82. As a result, even if the green body 63 and the cavity 81 shrink during the sintering process, the cavity 81 can be maintained filled with an appropriate amount of the second powder 52, thereby preventing deformation or damage to the green body 63.
[0077] Furthermore, the shape of the opening 82 is not limited as long as the opening 82 can discharge the part 52A of the second powder 52 during the sintering process. Therefore, according to the three-dimensional object manufacturing method according to this embodiment, the object manufacturing quality can be improved.
[0078] In addition, the three-dimensional modeling apparatus 1 of this embodiment is equipped with a modeling unit 3 that performs the modeling process, a filling unit 6 that performs the filling process S6, a sintering unit 7 that performs the sintering process S8, and a removal unit 8 that performs the removal process S9, and can therefore achieve the same effects as the three-dimensional modeling method of this embodiment.
[0079] Next, a configuration in which a plurality of loopholes are provided will be described with reference to FIGS.
[0080] Fig. 7 is a schematic diagram showing a second example of the structure of the shaped object. In Fig. 7, two openings 82, 83 are provided as multiple holes as compared to Fig. 6. This makes it possible to disperse the pressure on the second powder 52 when the green body 63 contracts. Fig. 7(A) is a cross-sectional view in the YZ axis direction, and Fig. 7(B) is a side view seen from the Y negative direction side.
[0081] As shown in FIG. 7(A), the opening 83 is smaller than the opening 82. The openings 82 and 83 face each other through a cavity 81. As shown in FIG. 7(B), the cross-sectional shapes of the openings 82 and 83 are perfect circles, and the circular shape of the opening 83 is smaller than the circular shape of the opening 82. The cross-sectional shapes of the openings 82 and 83 may be perfect circles, ellipses, polygons, etc. The opening 82 is on an axis extending from a part of the opening 83. The positions of the openings 82 and 83 are preferably such that when one opening 83 is projected along the axial direction of the other opening 82, a part or the whole of the other opening 83 overlaps with the one opening 82. For example, the opening 83 overlaps with a part of the projection of the opening 82. This allows the second powder 52 to be discharged from a pair of directions on the same axis (Y direction in FIG. 7).
[0082] Furthermore, for example, when cavity 81 has a symmetrical shape, openings 82 and 83 preferably have the same shape and diameter, and are preferably coaxial. When cavity 81 does not have a symmetrical shape, it is preferable to adjust the shape and diameter of openings 82 and 83 to match the shape of cavity 81. By making the shapes and diameters the same or adjusting them, the amount and speed of discharge of second powder 52 can be made uniform.
[0083] 8A and 8B are schematic diagrams showing a third example of the structure of a shaped object, in which Fig. 8A is a cross-sectional view in the YZ axis direction, Fig. 8B is a side view seen from the Y negative direction, and Fig. 8C is a plan view seen from the Z positive direction.
[0084] 6 and 7, in Fig. 8, four openings 82, 83, 84, and 85 are provided as a plurality of loopholes. Of the four openings, two openings 82 and 83 forming a first pair are disposed opposite each other, and two openings 84 and 85 forming a second pair are disposed opposite each other.
[0085] As shown in FIG. 8(B), when the first pair of two openings 82, 83 is projected along the axial direction of one opening 82, a part or all of the opening 83 overlaps with the opening 82. Also, as shown in FIG. 8(C), the opening 85 is smaller than the opening 84. The openings 84, 85 face each other through a cavity 81. As shown in FIG. 8(A), the opening 84 is on an axis extending from a part of the opening 85. Also, when the second pair of two openings 84, 85 is projected along the axial direction of one opening 84, a part or all of the opening 85 overlaps with the opening 84.
[0086] 8, two pairs of holes are provided as four holes, but the number of openings may be an even number, for example, six or eight. In other words, when one opening is projected along the axial direction of the other opening in each of the multiple pairs of openings, a part or the whole of the other opening may overlap with one opening.
[0087] This configuration makes it possible to discharge the second powder 52 from multiple directions during the sintering process.
[0088] It is also preferable that the line connecting the centers of the first pair of openings 82, 83 is perpendicular to the line connecting the centers of the second pair of openings 84, 85. This configuration allows the second powder 52 to easily escape in many shrinkage directions of the green body 63 in the sintering step S8.
[0089] Note that FIG. 8 illustrates a configuration in which four holes, i.e., two pairs of openings, face each other in the Y direction (the long direction of cavity 81) and the Z direction (the short direction of cavity 81), respectively; however, another pair of openings may be provided whose facing direction is the X direction.
[0090] Fig. 9 is a schematic diagram showing a fourth example of the structure of the shaped object. Fig. 9 is a cross-sectional view in the YZ axis direction. In Fig. 9, three openings 86, 87, and 88 may be provided as a plurality of escape holes, in contrast to Figs. 6 to 8. Note that Fig. 9 illustrates a configuration in which three openings are provided, but the number of openings may be an odd number, and may be, for example, five or seven.
[0091] The openings 86, 87, and 88 are provided at positions equidistant from the center O of the cavity 81. With this configuration, the amount of the second powder 52 that escapes through the openings as the green body 63 shrinks during the sintering process can be made uniform.
[0092] As described above, the multiple openings prevent stress from concentrating at one point in the cavity 81 when the second powder 52 tries to escape during shrinkage in the sintering process, making it easier for the second powder 52 to escape and making the shrinkage of the green body 63 even more uniform.
[0093] Next, the structure for providing the taper will be described with reference to FIGS.
[0094] Fig. 10 is a schematic diagram showing a fifth example of the structure of the shaped object. Fig. 10(A) is a cross-sectional view in the YZ axis direction, and Fig. 10(B) is an enlarged view of the dotted circle A in Fig. 10(A). In Fig. 10, a taper 89 is provided at the end of the opening 82 on the cavity 81 side, in comparison with Fig. 6.
[0095] The taper 89 serves to alleviate blockage of the second powder 52 and promote its discharge.
[0096] 10(B) shows angle θ as the inclination angle of taper 89. Angle θ is set at a predetermined angle from a horizontal line extending from the axial direction of opening 82. It is preferable that the dimension of taper 89 is large, and it may be continuous from cavity 81 to the surface of green body 63 at the maximum.
[0097] Fig. 11 is a schematic diagram showing a sixth example of the structure of the shaped object. Fig. 11 is a cross-sectional view in the YZ axis direction. As shown in Fig. 11, a taper 90 is preferably provided at the outer end of the opening 82. In this case, the opening 82 is formed so as to widen from the inside to the outside of the cavity 81 due to the taper 90. In other words, the cross-sectional area of the opening 82 increases from the inside to the outside of the cavity 81.
[0098] This configuration reduces the resistance between the second powder 52 and the wall surface of the green body 63, making it easier to discharge the second powder 52. Also, the second powder 52 can be easily filled into the cavity 81.
[0099] By providing the tapers 89 and 90, the second powder 52 does not remain in the sintering step S8, and can be easily discharged.
[0100] Fig. 12 is a schematic diagram showing a seventh example of the structure of the shaped object. Fig. 12 is a cross-sectional view in the YZ axis direction. In the example of Fig. 12, the shape of the green body 63 has a protruding portion 63C that partially protrudes in the Y direction (horizontal direction) from the outer wall of the green body 63 in the installation posture during the debinding and sintering processes. In the case of such a shape, the method of filling the second powder 52 into the cavity 81 as in each of the above examples does not act on the protruding portion 63C during the debinding and sintering processes, so there is a risk that the protruding portion 63C will be deformed or damaged.
[0101] 12, a holder 91 may be used below the protruding portion 63C. This allows the position of the protruding portion 63C to be maintained by the holder 91, which can suppress deformation and damage of the protruding portion 63C during the degreasing step S7 and the sintering step S8, and can further improve the effect of preventing deformation and damage of the entire green body 63.
[0102] In the degreasing step S7 and the sintering step S8, the protruding portion 63C also shrinks in the same manner as the green body 63, and therefore the position of the protruding portion 63C in the Z direction may fluctuate. In consideration of this point, it is preferable that the holder 91 is formed of the powder 50 of the same material as the shaped object 62. In this way, the holder 91 also shrinks in the same manner as the protruding portion 63C and the green body 63 during the degreasing and sintering steps, so that the relative positional relationship with the protruding portion 63C can be maintained, and the attitude of the protruding portion 63C can be continuously maintained by the holder 91. Furthermore, the contact surface of the holder 91 with the protruding portion 63C (the upper surface in the example of FIG. 12) is preferably formed of the same material as the second powder 52 so as not to melt at the sintering temperature and fuse to the protruding portion 63C.
[0103] Next, a configuration for providing a sealing member 63B on a molded object will be described with reference to Figures 13 to 19. Note that the following description will be based on the second example of the molded object structure shown in Figure 7, i.e., a molded object having two openings 82, 83 provided as multiple escape holes, but the structure of a molded object other than the second example may also be applied.
[0104] Fig. 13 is a schematic diagram showing an eighth example of the structure of the object. As shown in Fig. 13, the eighth example of the object (green body 63) includes a main body 63A and a sealing member 63B that is separate from the main body 63A. The main body 63A is provided with a filling opening 92 that is separate from the openings 82, 83. The sealing member 63B can seal the filling opening 92.
[0105] The main body 63A and the sealing member 63B are both formed from the first powder 50. For example, the main body 63A and the sealing member 63B can be formed as parts of the object 62 in the forming process of step S3, and then formed as parts of the green body 63 through the drying process of step S4 and the powder removal process of step S5.
[0106] As shown in FIG. 13(A), in the first stage of the filling process in step S6, the second powder 52 is filled into the cavity 81 inside the main body 63A of the green body 63 through the filling opening 92. The filling opening 92 is formed to have a larger opening area than the openings 82 and 83. When the outer shape of the main body 63A of the shaped object and the spatial shape of the cavity 81 are both rectangular parallelepiped shapes as exemplified in this embodiment, it is preferable to form an opening in the entirety of any one of the four faces of the rectangular parallelepiped shape of the main body 63A except for a pair of opposing faces on which the openings 82 and 83 are provided, and use this opening as the filling opening 92. In the example of FIG. 13, the filling opening 92 is formed in a face facing the Z positive direction among the six faces of the main body 63A, and the shape of the filling opening 92 is formed in a rectangular shape along the inner circumferential surface of the cavity 81 when viewed in the Z direction. By providing the filling opening 92 in this manner, the second powder 52 can be filled into the cavity 81 in a shorter time during the filling process compared to filling the second powder 52 through the openings 82, 83, making the filling operation easier.
[0107] As shown in FIG. 13(A), in the filling step of step S6, in the second stage, after the cavity 81 is filled with the second powder 52, the filling opening 92 is sealed by the sealing member 63B. The sealing member 63B has a flat surface 63B1 that can come into surface contact with the end surface 63A1 of the main body 63A where the filling opening 92 is provided. The shape of the flat surface 63B1 is preferably formed so as to extend at least outward from the outer edge of the filling opening 92. In the example of FIG. 13, the shape of the flat surface 63B1 of the sealing member 63B is rectangular, which is the same as the shape of the surface (the outer edge shape of the end surface 63A1) facing the Z positive direction where the filling opening 92 is provided, among the six faces of the rectangular parallelepiped shape of the main body 63A. In the example of FIG. 13, the sealing member 63B is a flat plate-like member having a pair of main surfaces facing the Z direction and one main surface facing the Z negative direction side being a flat surface 63B1. The outer edge shape of sealing member 63B as viewed in the Z direction is formed to be the same shape as the outer edge shape of main body 63A. By forming sealing member 63B in this manner, it is possible to completely block filling opening 92 in its entirety. Therefore, even in a structure in which filling opening 92 separate from openings 82, 83 is provided, second powder 52 filled in cavity 81 in the sintering process of step S8 can be discharged from openings 82, 83, as in the first to seventh examples described above.
[0108] 13B, when the sintering step S8 is performed with the filling opening 92 of the main body 63A sealed with the sealing member 63B formed as described above, the sealing member 63B is bonded to the outer edge of the filling opening 92 to form a three-dimensional object 64 integrated with the main body 63A. In this case, in the example of FIG. 13, the outer edge shape of the sealing member 63B as viewed in the Z direction is formed to be the same as the outer edge shape of the main body 63A, so that the joint portion between the main body 63A and the sealing member 63B can be made flush, resulting in a natural integrated structure.
[0109] 13, in the powder removal process of step S5, it is preferable to remove excess powder 50 in cavity 81 through filling opening 92. This allows excess powder 50 in cavity 81 to be removed through filling opening 92, which has a larger opening area than openings 82 and 83, making it possible to remove excess powder 50 from cavity 81 in a shorter time in the powder removal process, and thus facilitating the powder removal work in addition to the filling process.
[0110] Fig. 14 is a schematic diagram showing a ninth example of the structure of the object. Fig. 15 is a cross-sectional view taken along line AA in Fig. 14(C). As shown in Figs. 14 and 15, the ninth example of the object (green body 63) is provided with a structure to prevent the sealing member 63B from coming off, in comparison with the eighth example of Fig. 13.
[0111] 14 and 15, in the ninth example, a pair of erected portions 63A4, 63A5 are provided on the Z positive side of the end face 63A1 on which the filling opening 92 is provided of the main body 63A. The pair of erected portions 63A4, 63A5 are provided on portions corresponding to a pair of opposite sides of the rectangular four sides of the end face 63A1, and in the example of Fig. 14, they are provided extending in the X direction along the side faces 63A2, 63A3 on which the openings 82, 83 are provided, respectively. On the other hand, the width dimension of the sealing member 63B in the Y direction is formed so as to fit between the pair of erected portions 63A4, 63A5.
[0112] In the pair of standing portions 63A4, 63A5, grooves 63A6, 63A7 are provided on the opposing surfaces on the center side of the main body 63A facing each other along the extending direction of the standing portions 63A4, 63A5, respectively. Meanwhile, in the sealing member 63B, streaks 63B2, 63B3 are provided on the side surface facing the opposing surface along the longitudinal direction of the side surface. The streaks 63B2, 63B3 are formed so as to be able to be engaged with the grooves 63A6, 63A7, respectively. In addition, the grooves 63A6, 63A7 are provided up to the ends of the standing portions 63A4, 63A5 in the X direction, thereby allowing the streaks 63B2, 63B3 to be inserted from the X direction.
[0113] As shown in FIG. 14(A), in the filling process of step S6, the second powder 52 is filled into the cavity 81 inside the main body 63A of the green body 63 through the filling opening 92 as a first stage.
[0114] 14(B), in the filling process of step S6, as a second stage, after filling cavity 81 with second powder 52, stripes 63B2, 63B3 of sealing member 63B are inserted into grooves 63A6, 63A7 of main body 63A from, for example, the X positive direction side. As a result, sealing member 63B is slid toward the X negative direction side between a pair of upright portions 63A4, 63A5 of main body 63A while gradually closing filling opening 92.
[0115] As shown in FIG. 14(C), in the filling process of step S6, as a third stage, sealing member 63B is slid further toward the negative X direction and reaches the end of main body 63A on the negative X direction side, and finally filling opening 92 is sealed by sealing member 63B.
[0116] As shown in Fig. 15, in a state where the filling opening 92 is sealed by the sealing member 63B, the ribs 63B2 and 63B3 of the sealing member 63B are engaged with the grooves 63A6 and 63A7 of the main body 63A, so that the sealing member 63B can be prevented from moving in the Z positive direction relative to the main body 63A. That is, the portions indicated by the dotted circles A and B in Fig. 15, i.e., the portion A where the ribs 63B2 are engaged with the groove 63A6 and the portion B where the ribs 63B3 are engaged with the groove 63A7 at both ends of the sealing member 63B in the Y direction, function as a structure for preventing the sealing member 63B from coming off.
[0117] By providing a structure to prevent the sealing member 63B from coming off in this manner, it is possible to prevent the second powder 52 filled in the cavity 81 from leaking through the contact surface between the main body 63A and the sealing member 63B when the green body 63 shrinks in the sintering process of step S8. This makes it possible to prevent the second powder 52 from being interposed in the gap between the main body 63A and the sealing member 63B during the sintering process, thereby reducing the influence of the second powder 52 on the bonding between the main body 63A and the sealing member 63B. As a result, the bonding between the main body 63A and the sealing member 63B in the sintering process can be more reliably achieved.
[0118] 14 and 15 are merely examples, and other structures may be used as long as they are shaped in a molding process. Examples of other structures include light press-fitting and screw fastening.
[0119] Fig. 16 is a schematic diagram showing a tenth example of the structure of a molded object. As shown in Fig. 16, in the tenth example of the molded object, unlike the ninth example of Figs. 14 and 15, a sealing member 63B is provided on one part of one surface of a main body 63A, rather than on the entirety thereof.
[0120] In the example of FIG. 16, the retaining structure between sealing member 63B and main body 63A is similar to that of the ninth example, but the dimension of sealing member 63B in the X direction is shorter than the dimension of the surface of main body 63A on which filling opening 92 is provided in the X direction.
[0121] In the tenth example, the same anti-dislodgement structure as in the ninth example is provided, and therefore the same effect as in the ninth example can be achieved.
[0122] FIG. 17 is a diagram showing a first example of a method for preventing the sealing member 63B from coming off. FIG. 17 illustrates an example of a sintering process using the shaped object of the eighth example. As shown in FIG. 17, in the sintering process, the green body 63 is accommodated in a sintering vessel 93 and sintered. In the example of FIG. 17, the green body 63 is placed upside down so that the sealing member 63B is disposed on the bottom surface 93A side of the sintering vessel 93 with respect to the main body 63A in a state where the sealing member 63B seals the filling opening 92 of the main body 63A. Furthermore, the second powder 52 is filled into the sintering vessel 93 to a height that covers the contact surface between the main body 63A and the sealing member 63B.
[0123] By performing the sintering process using the configuration shown in Figure 17, even if the molded object does not have an anti-slip structure like the ninth or tenth example, it is possible to prevent the second powder 52 filled in the cavity 81 from leaking through the contact surface between the main body 63A and the sealing member 63B when the green body 63 shrinks in the sintering process in step S8.
[0124] Fig. 18 is a diagram showing a second example of a method for preventing the sealing member 63B from coming off. Fig. 18 also shows an example of placement of the green body 63 in the sintering process using the eighth example of the shaped object, and unlike Fig. 17, the sintering container 93 is omitted.
[0125] 18, the green body 63 is also placed upside down so that the sealing member 63B is disposed on the bottom surface 93A side of the sintering vessel 93 with respect to the main body 63A, with the sealing member 63B sealing the filling opening 92 of the main body 63A (see FIG. 17). Furthermore, at this time, a weight 94 is placed on the surface of the green body 63 facing upward, i.e., on the bottom surface 63A8 of the main body 63A. As a result, the green body 63 is placed in a state where a load is applied to the bottom surface 93A side of the sintering vessel 93 (the lower side in FIG. 18).
[0126] By performing the sintering process using the configuration shown in Figure 18, even if the molded object does not have an anti-slip structure like the ninth or tenth example, it is possible to prevent the second powder 52 filled in the cavity 81 from leaking through the contact surface between the main body 63A and the sealing member 63B when the green body 63 shrinks in the sintering process of step S8.
[0127] 18 shows an example of a method of placing a weight 94, but other methods may be used as long as the green body 63 can be placed in a state where a load is applied to the bottom surface 93A of the sintering vessel 93. For example, a configuration in which the top surface 93B (see FIG. 17) of the sintering vessel 93 can be moved in the vertical direction may be one in which the top surface 93B is lowered to press the green body 63 downward.
[0128] Fig. 19 is a diagram showing an example in which a gyroid structure 95 is provided in an internal cavity 81 of a shaped object. In the eighth to tenth examples in Figs. 13 to 18, a sealing member 63B is provided mainly for the purpose of facilitating the filling of the second powder 52 into the cavity 81 in the filling step of step S6. On the other hand, the sealing member 63B may be provided only for the purpose of facilitating the removal of the excess powder 50 in the cavity 81 in the powder removal step of step S5.
[0129] 19, in a configuration in which a gyroid structure 95 is provided in a cavity 81 inside the molded object, the cavity 81 can maintain its shape by the gyroid structure 95. For this reason, it is not necessarily necessary to fill the cavity 81 with the second powder 52 in order to suppress deformation of the molded object in the sintering process of step S8. On the other hand, in a configuration in which a gyroid structure 95 is provided inside the cavity 81, the inside of the cavity 81 has a complex shape, so that it is troublesome to remove the excess powder 50 inside the cavity 81 in the powder removal process of step S5, and the time required is relatively long.
[0130] Therefore, even in the structure illustrated in FIG. 19, by making the sealing member 63B separate from the main body 63A, the powder removal opening 96 having a larger opening area than the openings 82 and 83 can be provided in the main body 63A, and the cavity 81 can be opened by the powder removal opening 96. This powder removal opening 96 corresponds to the filling opening 92 in the eighth to tenth examples. In the example of FIG. 19, in the powder removal process of step S5, the excess powder 50 in the cavity 81 is removed through the powder removal opening 96, and after removal, the powder removal opening 96 is sealed by the sealing member 63B. In the example of FIG. 19, the filling process of step S6 is not performed, and the sintering process of step S8 is performed in a state in which the cavity 81 is not filled with the second powder 52 and the powder removal opening 96 of the main body 63A is sealed by the sealing member 63B. For this reason, the removal process of step S9 is not performed either.
[0131] Therefore, in the example of Figure 19, excess powder 50 in cavity 81 can be removed through powder removal opening 96, which has a larger opening area than openings 82, 83, so that the time required to remove excess powder 50 from cavity 81 in the powder removal process can be significantly reduced, making the powder removal work easier.
[0132] Next, the appropriate size of the opening 82 will be described with reference to FIG.
[0133] Fig. 20 is a diagram showing the range of hole diameters of openings 82. The horizontal axis of Fig. 20 shows the taper angle provided to openings 82, and the vertical axis shows the ratio of the total area of the holes of openings 82 to the volume of cavity 81 (total area of holes / volume of cavity). Here, "total area of holes" refers to the area of the cross section when viewed from the axial direction of the holes of openings 82. When multiple openings 82 are provided, it is the total value of the cross-sectional areas of all the holes.
[0134] Several test objects were created using several combinations of "taper angle" and "total area of holes / volume of cavity," and the degree of deformation of the objects after the sintering process was confirmed. Each plot in Figure 20 corresponds to several test objects, and the type of plot indicates the result of the degree of deformation. A circle plot indicates a result of "no deformation," that is, no deformation such as warping occurred in the object after the sintering process. A triangle plot indicates a result of "small deformation (can be dealt with by shape correction)," that is, some deformation occurred in the object after the sintering process, but the deformation was small enough to be covered by shape correction processing such as correcting the shape of the model to be printed in advance. A square plot indicates a result of "large deformation."
[0135] The results in Fig. 20 show that it is preferable to set the ratio of the area of the opening 82 to the volume of the internal cavity 81 to 0.013 or more (area of opening ÷ volume of internal cavity ≧ 0.013). By setting the ratio to 0.013 or more, deformation due to inhibited shrinkage of the second powder 52 during sintering can be suppressed. To prevent deformation, it is effective to correct the shape of the model to be molded in advance.
[0136] 20 shows that by setting the above-mentioned ratio to 0.029 or more, deformation due to inhibition of shrinkage of the second powder 52 during sintering does not occur. For this reason, for example, in the case of molding a portion that requires high surface accuracy, such as a mounting surface, it is preferable to set the ratio to 0.029 or more.
[0137] Fig. 21 is a diagram showing a modified example of the modeling unit. The modeling unit 3A according to the modified example shown in Fig. 21 includes a powder supply unit 70 instead of the supply tank 11 of the modeling unit 3 shown in Fig. 2. Descriptions common to Fig. 3 will be omitted as appropriate.
[0138] The powder supplying unit 70 supplies powder 50 to the powder layer 51 in the modeling tank 12. The powder supplying unit 70 is movable in the horizontal direction (Y1 and Y2 directions) and scans above the modeling tank 12 to supply powder 50 to the modeling tank 12.
[0139] The powder supply section 70 includes a hopper 71 , a vibration source 72 , and a trough 73 .
[0140] The hopper 71 holds the powder 50 to be supplied to the modeling tank 12 .
[0141] The trough 73 supplies the powder 50 to the modeling tank 12. The trough 73 is a supply path that supplies the powder 50 held in the hopper 71 to the modeling tank 12. It is preferable that the length (width) of the trough 73 in the X direction is the same as the length (width) of the modeling tank 12 in the X direction. The vibration source 72 vibrates the trough 73. As the trough 73 is vibrated by the vibration source 72, the powder 50 falls from the opening of the trough 73 into the modeling tank 12.
[0142] The modeling section 3A includes an application section 40, a lamination unit 30, and an excess powder tank 15. As part of the modeling section, a powder supply section 70 supplies powder to form a powder layer 51 containing powder 50. The application section 40 applies a modeling liquid 60 to the powder layer 51 to form a modeling layer 61. In the modeling section 3A, a plurality of modeling layers 61 are laminated to form a modeled object.
[0143] The present embodiment has been described above with reference to specific examples. However, the present disclosure is not limited to these specific examples. Any design modifications made by a person skilled in the art to these specific examples are also included within the scope of the present disclosure as long as they have the features of the present disclosure. The elements of each of the above-mentioned specific examples and their arrangements, conditions, shapes, etc. are not limited to those exemplified and can be changed as appropriate. The combination of each of the elements of each of the above-mentioned specific examples can be changed as appropriate as long as no technical contradiction occurs.
[0144] In the above embodiment, a single 3D modeling apparatus 1 has been described as an example, but a 3D modeling system including multiple apparatuses may be used. The 3D modeling system includes a powder mixing apparatus, a modeling apparatus, a drying apparatus, a powder removing apparatus, a filling apparatus, a sintering apparatus, a removing apparatus, a collecting apparatus, and a control apparatus, which correspond to the powder mixing unit 2, the modeling unit 3, the drying unit 4, the powder removing unit 5, the filling unit 6, the sintering unit 7, the removing unit 8, the collecting unit 9, and the control unit 100, which are the components of the 3D modeling apparatus 1. In the 3D modeling system, the multiple apparatuses are connected to each other so that they can communicate with each other, and the multiple apparatuses can work together to perform 3D modeling operations.
[0145] For example, aspects of the present invention are as follows. <1> A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a molding step of molding the object using a first powder; a filling step of filling the cavity with a second powder through the opening; a sintering step of sintering the shaped object in which the cavity is filled with the second powder in the filling step; a removing step of removing the second powder in the cavity through the opening; Including, Three-dimensional modeling method. <2> The first powder is a metal. <1> The three-dimensional object forming method according to claim 1, <3> The melting point of the second powder is higher than the sintering temperature of the sintering step. <1> or <2> The three-dimensional object forming method according to claim 1, <4> The molding process includes: forming a powder layer with the first powder; applying a modeling liquid to the powder layer; <1> ~ <3> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <5> In the sintering step, A portion of the second powder is discharged from the cavity through the opening. <1> ~ <4> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <6> The diameter of the opening is smaller than the diameter of the cavity. <1> ~ <5> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <7> The opening is provided on a side surface of the object. <1> ~ <6> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <8> The opening is provided at a longitudinal end of the cavity. The above <1> ~ <7> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <9> The object includes a plurality of the openings. The above <1> ~ <8> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <10> The openings include at least a first opening and a second opening, The first opening is smaller than the second opening. The above <1> ~ <9> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <11> The openings include at least a first opening and a second opening, The first opening and the second opening face each other across the cavity. The above <1> ~ <10> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <12> The openings include at least a first opening and a second opening, The first opening is on an axis extending from a portion of the second opening. The above <1> ~ <11> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <13> The openings include at least a first opening, a second opening, a third opening, and a fourth opening, the first opening and the second opening face each other across the cavity, the third opening and the fourth opening face each other across the cavity; The above <1> ~ <12> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <14> The openings include at least a first opening, a second opening, a third opening, and a fourth opening, the first opening is on an axis extending from a portion of the second opening; The third opening is on an axis extending from a portion of the fourth opening. The above <1> ~ <13> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <15> The openings include at least a first opening, a second opening, a third opening, and a fourth opening, an axis extending from a center of the second opening toward the first opening; an axis extending from a center of the fourth opening toward the third opening; are orthogonal, The above <1> ~ <14> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <16> The object includes a plurality of the openings, Each of the plurality of openings is provided at a position equidistant from the center of the cavity. The above <1> ~ <15> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <17> The object has a taper at least on one end of the opening on the cavity side or the outside side. The above <1> ~ <16> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <18> the cavity is a flow path formed in the object, The openings are the inlet and outlet of the flow path. The above <1> ~ <17> 13. The three-dimensional object fabrication method according to any one of claims 1 to 12. <19> An apparatus for manufacturing a shaped object having a cavity therein, comprising: the object includes an opening that connects the cavity with an outside of the object, a molding unit that molds the object using a first powder; a filling section that fills the cavity with a second powder through the opening; a sintering section that sinters the shaped object having the cavity filled with the second powder by the filling section; a removal unit that removes the second powder in the cavity through the opening; Equipped with Three-dimensional modeling device. <20> A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a filling opening separate from the opening, and a sealing member that seals the filling opening; a molding step of molding the object using a first powder; a filling step of filling a second powder into the cavity through the filling opening and sealing the filling opening with the sealing member after the filling; a sintering step of sintering the shaped object in which the cavity is filled with the second powder in the filling step; a removing step of removing the second powder in the cavity through the opening; Including, Three-dimensional modeling method. <21> a powder removing step of removing excess powder from the shaped object after the shaping step and before the filling step, In the powder removing step, the excess powder in the cavity is removed through the filling opening. The above <20> The three-dimensional object forming method according to claim 1, <22> A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a powder removal opening separate from the opening, and a sealing member that seals the powder removal opening, a molding step of molding the object using a first powder; a powder removing step of removing excess powder from the shaped object; a sintering step of sintering the shaped object; Including, In the powder removing step, the excess powder in the cavity is removed through the powder removing opening, and after the removal, the powder removing opening is sealed by the sealing member. Three-dimensional modeling method. <23> The ratio of the area of the opening to the volume of the cavity is 0.013 or more. The above <6> The three-dimensional object forming method according to claim 1, [Explanation of symbols]
[0146] 1 Three-dimensional modeling device 3. Modeling Department 6 Filling section 7 Sintering section 8 Removal section 50 Powder (First Powder) 52 Second Powder 62 Sculptures 63 Green Body 63B Sealing member 64 Three-dimensional sculpture 81 Cavity 82 Opening 92 Filling opening 96 Powder removal opening S3 Molding process S5 Powder removal process S6 Filling process S8 Sintering process S9 removal process [Prior art documents] [Patent documents]
[0147] [Patent Document 1] Special Publication No. 2018-501398
Claims
1. A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a molding step of molding the object using a first powder; a filling step of filling the cavity with a second powder through the opening; a sintering step of sintering the shaped object in which the cavity is filled with the second powder in the filling step; a removing step of removing the second powder in the cavity through the opening; Including, Three-dimensional modeling method.
2. The method for fabricating a three-dimensional object according to claim 1 , wherein the first powder is a metal.
3. The three-dimensional object fabrication method according to claim 1 , wherein the melting point of the second powder is higher than a sintering temperature in the sintering step.
4. The molding process includes: forming a powder layer with the first powder; The three-dimensional object fabrication method according to claim 1 , further comprising: applying a modeling liquid to the powder layer.
5. In the sintering step, The three-dimensional object fabrication method according to claim 1 , wherein a part of the second powder is discharged from the cavity through the opening.
6. The three-dimensional object fabrication method according to claim 1 , wherein a diameter of the opening is smaller than a diameter of the cavity.
7. The three-dimensional object fabrication method according to claim 1 , wherein the opening is provided on a side surface of the object.
8. The opening is provided at a longitudinal end of the cavity. The three-dimensional object fabrication method according to claim 1 .
9. The object includes a plurality of the openings. The three-dimensional object fabrication method according to claim 1 .
10. The openings include at least a first opening and a second opening, The first opening is smaller than the second opening. The three-dimensional object fabrication method according to claim 1 .
11. The openings include at least a first opening and a second opening, The first opening and the second opening face each other across the cavity. The three-dimensional object fabrication method according to claim 1 .
12. The openings include at least a first opening and a second opening, The first opening is on an axis extending from a portion of the second opening. The three-dimensional object fabrication method according to claim 1 .
13. The openings include at least a first opening, a second opening, a third opening, and a fourth opening, the first opening and the second opening face each other across the cavity, the third opening and the fourth opening face each other across the cavity; The three-dimensional object fabrication method according to claim 1 .
14. The openings include at least a first opening, a second opening, a third opening, and a fourth opening, the first opening is on an axis extending from a portion of the second opening; The third opening is on an axis extending from a portion of the fourth opening. The three-dimensional object fabrication method according to claim 1 .
15. The openings include at least a first opening, a second opening, a third opening, and a fourth opening, an axis extending from a center of the second opening toward the first opening; an axis extending from a center of the fourth opening toward the third opening; are orthogonal, The three-dimensional object fabrication method according to claim 1 .
16. The object includes a plurality of the openings, Each of the plurality of openings is provided at a position equidistant from the center of the cavity. The three-dimensional object fabrication method according to claim 1 .
17. The object has a taper at least on one end of the opening on the cavity side or the outside side. The three-dimensional object fabrication method according to claim 1 .
18. the cavity is a flow path formed in the object, The openings are the inlet and outlet of the flow path. The three-dimensional object fabrication method according to claim 1 .
19. An apparatus for manufacturing a shaped object having a cavity therein, comprising: the object includes an opening that connects the cavity with an outside of the object, a molding unit that molds the object using a first powder; a filling section that fills the cavity with a second powder through the opening; a sintering section that sinters the shaped object having the cavity filled with the second powder by the filling section; a removal unit that removes the second powder in the cavity through the opening; Equipped with Three-dimensional modeling device.
20. A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a filling opening separate from the opening, and a sealing member that seals the filling opening; a molding step of molding the object using a first powder; a filling step of filling a second powder into the cavity through the filling opening and sealing the filling opening with the sealing member after the filling; a sintering step of sintering the shaped object in which the cavity is filled with the second powder in the filling step; a removing step of removing the second powder in the cavity through the opening; Including, Three-dimensional modeling method.
21. a powder removing step of removing excess powder from the shaped object after the shaping step and before the filling step, In the powder removing step, the excess powder in the cavity is removed through the filling opening. The three-dimensional object fabrication method according to claim 20.
22. A method for manufacturing a shaped object having an internal cavity, comprising the steps of: the object includes an opening that connects the cavity with an outside of the object, a powder removal opening separate from the opening, and a sealing member that seals the powder removal opening, a molding step of molding the object using a first powder; a powder removing step of removing excess powder from the shaped object; a sintering step of sintering the shaped object; Including, In the powder removing step, the excess powder in the cavity is removed through the powder removing opening, and after the removal, the powder removing opening is sealed by the sealing member. Three-dimensional modeling method.
23. The ratio of the area of the opening to the volume of the cavity is 0.013 or more. The three-dimensional object fabrication method according to claim 6 .