Laminate and method for manufacturing the same

The laminate structure with a copper-nickel resistive film and silver conductive film, separated by a non-silver-copper connection layer, addresses material cost and performance issues in ceramic substrates, achieving low TCR and robust insulation.

JP2024134523AActive Publication Date: 2024-10-03MITSUBOSHI BELTING LTD

Patent Information

Application Number
JP2024024626
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-02-21
Publication Date
2024-10-03
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

Conventional ceramic substrates with resistive films face challenges in reducing material costs, achieving low temperature coefficient of resistance (TCR), and ensuring excellent insulation and protection performance due to issues such as alloying, oxidation, and bubble formation in the insulating protective film.

Method used

A laminate structure comprising a ceramic substrate with a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, where a connection layer made of a metal component excluding silver and copper is interposed between the conductive and resistive films, allowing for the use of less expensive materials and preventing direct contact that leads to alloying and oxidation.

Benefits of technology

The laminate achieves reduced TCR, improved insulation properties, and enhanced protection against oxidation, resulting in a ceramic substrate with cost-effective and stable resistive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134523000001_ABST
    Figure 2024134523000001_ABST
Patent Text Reader

Abstract

To provide a laminate capable of suppressing the cost of a metal based paste material, having a small TCR of a resistance film and including a protective film excellent in insulation properties and protection performance.SOLUTION: A laminate including a ceramic substrate 2, a conductor film 3 including silver, a resistance film 5 including copper and nickel and insulation protective films 6 and 7 intervenes a connection layer 4 including a metal component without including silver and copper between the conductor film and the resistance film. The metal component of the connection layer may include at least one kind selected from a group consisting of lanthanum hexaboride, nickel, gold and ruthenium oxide; the connection layer may further include a glass component; in the connection layer, the volume ratio of the metal component to the glass component may be the metal component / the glass component=60 / 40 to 10 / 90; the average thickness of the connection layer may be 5-50 μm; the conductor film may be formed of silver, silver palladium alloy or silvery platinum alloy; and the insulation protective film may include a glass component.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate (ceramic substrate with a resistive film) having a conductive film, a resistive film, and an insulating protective film, and a method for manufacturing the same. [Background technology]

[0002] Traditionally, "resistors" used in ceramic heaters, chip resistors, and substrates for mounting light-emitting diodes (LEDs) are composed of ceramic substrates with resistive film. A ceramic substrate with resistive film is a laminate of multiple metal films formed by applying multiple metal paste materials by screen printing to a ceramic base material and firing them at high temperature. The multiple metal films are composed of a conductive film, a resistive film, and an insulating protective film.

[0003] In a ceramic substrate with a resistive film, the conductive film acts as wiring or electrodes, acting as a conductive path within the substrate and as a connection to the outside. The resistive film not only lowers the power supply voltage to a specified voltage in the circuit and detects the current value flowing through the circuit from the potential difference across the resistor (its role as a resistor itself), but also acts as a heating element that generates Joule heat in ceramic heaters. For this reason, the resistive film is required to have high resistance accuracy, a small temperature coefficient of resistance, and resistance to load power. The insulating protective film protects the resistive film from the external environment, suppresses resistance changes during long-term use, and protects it from unintended electrical contact. For this reason, the insulating protective film is required to have heat resistance, moisture resistance, insulation, etc.

[0004] The metal paste materials used for each film are often silver-based paste for the conductor film, and resistive paste mainly composed of precious metals such as silver, platinum, palladium, ruthenium, etc., or alloys of these metals, for the resistive film. Insulating materials such as epoxy resin and glass are used for the insulating protective film, and glass paste is used when heat resistance is particularly required.

[0005] Precious metal paste is used as a material for conductor films and resistive films because it can be fired in air. Precious metal paste does not oxidize in air, so there is no need to fire it in a controlled atmosphere such as inert gas, reducing gas, or vacuum, and it has been widely used because it can be fired stably by a relatively simple method. However, precious metals have a major problem in that the material cost is high. In particular, silver-palladium alloys with a small temperature coefficient of resistance (TCR) are used for resistive films, but palladium is particularly expensive among precious metals, and increasing the composition ratio of palladium to minimize the TCR inevitably increases the cost. Moreover, even if a silver-palladium alloy with a high palladium ratio is used, it is difficult to meet the high requirement of a TCR within ±100 ppm / ℃ or a narrower range.

[0006] Therefore, in Patent Document 1 (Japanese Patent No. 2986539), a thick-film resistor composition is prepared by adding glass frit and titania or alumina to a silver-palladium paste having a silver:palladium ratio of 45:55 to reduce the TCR.

[0007] In addition, in Patent Document 2 (JP 2002-75600 A), when single precious metals such as gold, silver, platinum, and palladium are used as the heating resistor of a ceramic heater, a TCR of 2,000 ppm / °C or less is obtained by using an alloy composition of these metal species in order to improve the heat generation variation that occurs during rapid heating due to the large TCR of the single precious metals.

[0008] Furthermore, Patent Document 3 (Patent Publication No. 3642100) proposes a chip resistor using a copper-nickel alloy resistive film obtained by firing a resistive paste made of copper / nickel alloy powder, copper powder, glass frit, and an organic vehicle as a resistive paste that is not a precious metal, in a nitrogen gas atmosphere. If a copper-nickel alloy is used as the resistive film in this chip resistor, it is relatively easy to achieve a small TCR, so it can be constructed from an inexpensive base metal. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 2986539 [Patent Document 2] JP 2002-75600 A [Patent Document 3] Patent No. 3642100 Summary of the Invention [Problem to be solved by the invention]

[0010] However, even in the thick-film resistor composition of Patent Document 1, the glass frit and oxide components affect the adhesion to the ceramic substrate, and if the selection of these components is limited, the selection of the applicable ceramic substrate material is also limited. In particular, when adhering a thick-film paste film to a nitride ceramic such as aluminum nitride or silicon nitride, it has been difficult to find a glass frit or oxide component that achieves both adhesion and TCR due to the poor wettability of the oxide components.

[0011] Moreover, even with the resistive heating element of Patent Document 2, the TCR could only be suppressed to 500 ppm / ° C. at most, and since a precious metal was used, it was expensive.

[0012] Furthermore, in the chip resistor of Patent Document 3, when a copper-nickel alloy paste is used for the resistive film, a copper paste is usually used for the conductive film. In this case, the insulating protective film (glass paste) must be fired in nitrogen gas to prevent the copper from oxidizing. However, the binder resin component contained in the paste is difficult to decompose in nitrogen gas, and the decomposed gas remains in the film as bubbles. If bubbles are generated in the film, the insulation property is greatly reduced. In addition, when used at high temperatures such as for heating elements, if bubbles are present in the insulating protective film, the concealment against oxygen permeation is low, and the resistive film (copper-nickel alloy) is oxidized during use, causing a problem of an increase in resistance value. In order to avoid this problem, it is possible to use a silver paste that does not oxidize even in the air for the conductive film and fire the insulating protective film (glass paste) in the air, but in this case, the conductive film (silver) and the resistive film (copper-nickel alloy) cannot be connected, and the physical and electrical connection is broken. That is, when these films are heated during firing, a phenomenon occurs in which part of the conductive film (silver) is absorbed into the resistive film (copper-nickel alloy), a phenomenon known as "eating," and the connection with the remaining conductive film (silver) is broken. This phenomenon occurs whether the silver film and the copper-nickel alloy film are fired separately or simultaneously.

[0013] As described above, with conventional technology, it was difficult to obtain a ceramic substrate with a resistive film (resistor) that had all of the following characteristics: reducing the cost of the metal paste material, keeping the TCR of the resistive film small, and providing sufficient insulating and protective performance of the insulating protective film.

[0014] Therefore, an object of the present invention is to provide a laminate having a protective film which reduces the cost of metal-based paste material, has a small TCR of a resistive film, and is excellent in insulating properties and protective performance, and a manufacturing method thereof. [Means for solving the problem]

[0015] In order to achieve the above object, the inventors have discovered that in a laminate comprising a ceramic substrate, a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, by interposing a connection layer containing a metal component that does not contain silver or copper between the conductive film and the resistive film, it is possible to reduce the cost of metal-based paste material, and provide a laminate having a protective film with a small TCR of the resistive film and excellent insulating properties and protective performance, and have completed the present invention.

[0016] That is, the laminate according to aspect [1] of the present invention is a laminate comprising a ceramic substrate, a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, and a connecting layer containing a metal component not containing silver or copper is interposed between the conductive film and the resistive film.

[0017] The embodiment [2] of the present invention is an embodiment in which, in the embodiment [1], the metal component of the connection layer includes at least one selected from the group consisting of lanthanum hexaboride, nickel, gold, and ruthenium oxide.

[0018] Aspect [3] of the present invention is an aspect of aspect [1] or [2], wherein the connection layer further contains a glass component, and the volume ratio of the metal component to the glass component is metal component / glass component=60 / 40 to 10 / 90.

[0019] The embodiment [4] of the present invention is any one of the above embodiments [1] to [3], wherein the average thickness of the connection layer is 5 to 50 μm.

[0020] An embodiment [5] of the present invention is any one of the above embodiments [1] to [4], wherein the conductor film is formed of silver, a silver-palladium alloy, or a silver-platinum alloy.

[0021] An aspect [6] of the present invention is any one of the aspects [1] to [5] above, wherein the insulating protective film contains a glass component.

[0022] An aspect [7] of the present invention is any of the aspects [1] to [6], wherein the insulating protective film covers a partial area of ​​the conductor film and also covers at least a partial area of ​​the resistive film.

[0023] An embodiment [8] of the present invention is any one of the embodiments [1] to [7] above, wherein the insulating protective film has a multilayer structure.

[0024] The present invention includes, as an aspect [9], A conductive film forming process in which a conductive film paste for forming a conductive film containing silver is applied onto a ceramic substrate and fired in air to form a conductive film; a connection layer forming step of applying a connection layer paste for forming a connection layer containing a metal component not containing silver and copper to an area including a part of the conductor film, and firing the paste in air or a nitrogen atmosphere to form a connection layer; a resistive film forming step of applying a resistive film paste containing copper and nickel to at least a portion of the connection layer and a portion of the ceramic substrate, and firing the paste in a nitrogen atmosphere to form a resistive film; a first insulating protective film forming step of applying a first insulating protective film paste to a partial region of the conductor film and at least a partial region of the resistive film, and firing the paste in a nitrogen atmosphere to form a first insulating protective film; Also included is a method for manufacturing a laminate, which includes a second insulating protective film formation step of applying a second insulating protective film paste for forming a second insulating protective film on the first insulating protective film, and firing the paste in air to form the second insulating protective film. Effect of the Invention

[0025] In the present invention, in a laminate comprising a ceramic substrate, a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, a connection layer containing a metal component that does not contain silver or copper is interposed between the conductive film and the resistive film, thereby reducing the cost of metal-based paste material and providing a laminate with a protective film having a small TCR of the resistive film and excellent insulating and protective performance. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the laminate of the present invention. [Diagram 2] FIG. 2 is an enlarged view of an end portion of the laminate of FIG. [Diagram 3] FIG. 3 is a schematic plan view of the laminate of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] [Laminate] The laminate (ceramic substrate with resistive film) of the present invention is a laminate including a ceramic substrate, a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, and is characterized in that the conductive film and the resistive film are bonded via a connecting layer containing a metal component not containing silver or copper. An example of the laminate of the present invention having such a structure will be described in detail with reference to the attached drawings as necessary.

[0028] FIG. 1 is a schematic cross-sectional view showing an example of a laminate of the present invention, FIG. 2 is an enlarged view of an end portion of the laminate of FIG. 1, and FIG. 3 is a schematic plan view of the laminate of FIG. 1 (a view of the planar shape of the laminate 1 observed from the insulating protective film 7 side).

[0029] As shown in FIG. 1, the laminate 1 of this example comprises a ceramic substrate 2 having a square (rectangular) planar shape, a pair of conductor films 3 formed (or laminated) on a partial region of the surface of the ceramic substrate 2, a resistive film 5 formed by bridging both conductor films 3 to electrically connect the pair of conductor films 3, a first insulating protective film 6 formed on an area including the entire surface (exposed surface) of the resistive film 5 to protect the resistive film 5 from the external environment, and a second insulating protective film 7 laminated on top of the insulating protective film 6, and a pair of connecting layers 4 are interposed between the conductor film 3 and the resistive film 5 at the joint between the two films to prevent the two films from coming into contact with each other.

[0030] In detail, the connection layer 4 is formed not only in the region (opposing region) where the conductive film 3 and the resistive film 5 are in contact, i.e., the region of the surface of the conductive film 3 that is in contact with the resistive film 5 on the opposing surface area and side end face, but also in the region 4a adjacent to the side end face where the ceramic substrate 2 and the resistive film 5 are in contact.

[0031] In addition, the first and second insulating protective films 6, 7 cover the entire surface of the resistive film 5 and are laminated on a partial area of ​​the ceramic substrate 2, and by covering the entire surface of the resistive film 5, they have the role of protecting the resistive film 5 from the external environment.

[0032] Furthermore, the first and second insulating protective films 6, 7 cover only partial areas of the surface of the conductor film 3, thereby exposing the remaining area of ​​the conductor film 3 (the connection area on the opposite side in the opposing direction of the pair of conductor films), and the conductor film 3 is formed in a structure that can be joined or connected to an external conductor in the exposed area.

[0033] The laminate of the present invention is not limited to the forms and structures shown in Figures 1 to 3 as long as it comprises a ceramic substrate, a conductive film, a resistive film, and an insulating protective film, and the conductive film and the resistive film are joined via a connecting layer.

[0034] That is, the laminate of the present invention is characterized in its form and structure by the presence of a connection layer between the conductor film and the resistive film in a laminate formed of a ceramic substrate, a conductor film laminated on a partial region of the surface of the ceramic substrate, a resistive film laminated on a partial region of the surface of the ceramic substrate in a state of being electrically connected to the conductor film, and an insulating protective film that laminates at least a partial region of the surface of the resistive film. In the present invention, the conductor film and the resistive film are joined without direct contact due to the presence of a connection layer that does not contain silver or copper, so that the problem of the physical and electrical connection being interrupted between the conductor film (silver-based) and the resistive film (copper-nickel-based) due to the so-called "eat-up phenomenon" can be eliminated. That is, in the present invention, since the eat-up phenomenon can be suppressed even when a copper-nickel-based resistive film is used, it is possible to use an inexpensive base metal-based resistive film. In addition, since the copper-nickel-based base metal material has excellent TCR characteristics, the TCR of the resistive film can be reduced. Furthermore, since the conductor film that is not covered by the insulating protective film and is partially exposed becomes silver-based, which is resistant to oxidation, the glass paste that serves as the insulating protective film can be fired in the air. Therefore, the resin component in the paste can be smoothly decomposed, and the decomposition gas can be prevented from being trapped in the glass film to generate bubbles, so that an insulating protective film with excellent insulating properties and protective performance can be formed. In other words, the configuration of the present invention makes it possible to obtain a laminate that is a ceramic substrate with a resistive film, which has a small TCR of the resistive film and is provided with an insulating protective film with excellent insulating properties and protective performance, while reducing the cost of the paste material.

[0035] (Connection Layer) The shape of the connection layer is not particularly limited as long as it is interposed between the conductive film and the resistive film and has a shape (a layer corresponding to the contact area) that is interposed between the two films in the contact area of ​​the two films so that the two films do not come into contact with each other; however, it is preferable that the connection layer be formed in an opposing area including at least the surface and side end faces of the conductive film in a form that allows the conductive film to be connected to an external conductor, and it is particularly preferable that the connection layer be formed in an adjacent area adjacent to the side end faces (a part of the contact area between the ceramic substrate and the resistive film) in addition to the opposing areas.

[0036] That is, the connection layer only needs to be formed (interposed) between the surface of the conductive film laminated opposite to each other on the ceramic substrate and the resistive film, and it is preferable that the connection layer is formed not only between the surface and the resistive film, but also between the side end faces of the conductive film (particularly, both end faces where the conductive films face each other) and the resistive film, and it is particularly preferable that the connection layer is formed in an adjacent region of the ceramic substrate adjacent to the side end face of the conductive film, in addition to between the surface and the resistive film and between the side end face and the resistive film. That is, as shown in Figures 1 and 2, if the connection layer is formed in the region extending from the surface of the conductive film via the side end face to the adjacent region (if the connection layer is interposed not only in the contact region between the conductive film and the resistive film but also in the adjacent region), it is possible to prevent the conductive film from coming into direct contact with the resistive film, and the connection layer can be easily formed by coating, resulting in excellent productivity.

[0037] The connection layer includes a metal component (first metal component) that does not include silver and copper. The metal component is not particularly limited as long as it is a metal element or alloy other than silver and copper, or a metal compound that does not include silver and copper.

[0038] Examples of preferred metal elements include molybdenum, tungsten, manganese, nickel, platinum, gold, and aluminum. These metal elements can be used alone or in combination. Among these metal elements, molybdenum, tungsten, aluminum, nickel, and gold are particularly preferred.

[0039] Preferred alloys include alloys made by combining at least two or more metals selected from the group consisting of the above-mentioned metal elements, etc. Among such alloys, molybdenum manganese alloys are particularly preferred.

[0040] Preferred metal compounds include, for example, metal borides such as lanthanum hexaboride (LaB6), and metal oxides such as ruthenium oxide. These metal compounds can be used alone or in combination. Among these metal compounds, lanthanum hexaboride and ruthenium oxide are preferred.

[0041] In particular, among these metal components, molybdenum, tungsten, manganese, nickel, gold, aluminum, molybdenum-manganese alloy, lanthanum hexaboride, and ruthenium oxide (RuO2) are preferred, and at least one selected from the group consisting of lanthanum hexaboride, nickel, gold, and ruthenium oxide is more preferred because the firing temperature and atmosphere are similar to those of metal pastes for forming conductive films (silver-based) and resistive films (copper-nickel-based), and lanthanum hexaboride and / or nickel are most preferred because of their excellent economic efficiency.

[0042] The connection layer may further contain a glass component (first glass component) as an inorganic binder in addition to the metal component. The main role of the glass component is to assist in sintering the metal component particles, which are the raw material of the metal component, in the manufacturing process of the laminate, and to adhere the sintered film to the ceramic substrate, but when the metal component is ruthenium oxide or lanthanum hexaboride, the glass frit, which is the raw material of the glass component, softens and melts, and hardens the film so as to envelop the metal component particles, and at the same time, it also plays a role of connecting electrical conduction between the particles.

[0043] Examples of glass components include borosilicate glass, such as borosilicate glass represented by the composition formula SiO2-B2O3-MO (wherein M represents an element other than Si and B), zinc borosilicate glass represented by the composition formula ZnO-SiO2-B2O3-MO (wherein M represents an element other than Zn, Si, and B), bismuth borosilicate glass represented by the composition formula BiO2-SiO2-B2O-MO (wherein M represents an element other than Bi, Si, and B), aluminosilicate glass represented by the composition formula Al2O3-SiO2-MO (wherein M represents an element other than Al and Si), and aluminoborosilicate glass represented by the composition formula Al2O3-SiO2-B2O3-MO (wherein M represents an element other than Al, Si, and B). These glass components can be used alone or in combination of two or more kinds. Among these, borosilicate glass and zinc borosilicate glass are preferred.

[0044] The softening point (or melting point) of the glass component is preferably lower than the firing temperature for forming the connection layer. The softening point of the glass component is, for example, 400 to 800° C., preferably 420 to 780° C., and more preferably 450 to 750° C. If the softening point is too low, the strength of the connection layer may be reduced, and conversely, if it is too high, the melt fluidity may be reduced, and the function as a binder may be reduced.

[0045] The volume ratio of the first metal component to the first glass component can be selected from the range of about first metal component / first glass component=90 / 10 to 1 / 99 (particularly 60 / 40 to 10 / 90), for example 70 / 30 to 5 / 95 (e.g. 50 / 50 to 30 / 70), preferably 65 / 35 to 7 / 93, further preferably 60 / 40 to 10 / 90, more preferably 55 / 45 to 12 / 88, most preferably 50 / 50 to 15 / 85. If the volume ratio of the first metal component is too low, there is a risk of the electrical properties being degraded, whereas if it is too high, there is a risk of the adhesion to the ceramic substrate being degraded.

[0046] The mass ratio of the first metal component to the first glass component can be selected from a range of about 90 / 10 to 1 / 99 (first metal component / first glass component), for example, 70 / 30 to 10 / 90, preferably 60 / 40 to 30 / 70, more preferably 60 / 40 to 40 / 60, and even more preferably 55 / 45 to 45 / 55. If the volume ratio of the first metal component is too low, there is a risk of the electrical properties being degraded, whereas if it is too high, there is a risk of the adhesion to the ceramic substrate being degraded.

[0047] The connection layer may contain a non-conductor such as a semiconductor or an insulator (e.g., a filler such as ceramics, an organic vehicle remaining after firing, etc.) within a range that does not impair the effects of the present invention. The total proportion of the first metal component and the first glass component in the connection layer may be 90 mass % or more, preferably 95 mass % or more, more preferably 99 mass % or more, and particularly may be 100 mass % (formed only of the first metal component and the first glass component).

[0048] The connection layer may have a single-layer structure, or may have a multi-layer structure in which a plurality of layers having different compositions are laminated.

[0049] In the laminate of the present invention, the connection layer can electrically connect the conductor film and the resistive film, but preferably has low electrical resistance. The reason why low electrical resistance is preferable varies depending on the application. For example, in applications such as voltage adjustment and current detection, the resistance value of the entire conductive path in the substrate is mainly controlled by the resistive film. However, in resistive film materials that require a small TCR (temperature coefficient of resistance), if the resistance of the connection layer becomes so high that it cannot be ignored compared to the resistance of the resistive film, the TCR characteristics are greatly affected by the connection layer. On the other hand, in applications as a heating element, if the resistance of the connection layer is high, the heating temperature will be higher only in the connection layer than in the surrounding area, and the temperature uniformity will decrease. Considering these points, the surface resistance of the connection layer is, for example, 10 kΩ / □ or less, preferably 1 kΩ / □ or less, more preferably 100 Ω / □ or less, and more preferably 10 Ω / □ or less.

[0050] In the present application, the sheet resistance of the connection layer can be measured by a two-terminal method.

[0051] The thickness (average thickness) of the connection layer can be selected from the range of about 3 to 200 μm, for example, 3 to 100 μm, preferably 4 to 70 μm, further preferably 5 to 50 μm, more preferably 10 to 25 μm, and most preferably 15 to 20 μm. If the connection layer is too thin, there is a risk that the erosion phenomenon cannot be suppressed, and conversely, if it is too thick, there is a risk that the electrical properties of the laminate will deteriorate.

[0052] In the present application, the average thickness of the connection layer and each of the other films can be measured using a stylus film thickness meter.

[0053] (Conductor film) Since the conductive film contains silver, oxidation in the atmosphere can be suppressed, and therefore the conductive film can be fired in the atmosphere even when the surface of the conductive film is exposed during the manufacturing process of the laminate. Therefore, for example, in the firing process of the insulating protective film, firing can be performed in the atmosphere without considering oxidation of the conductive film, and the productivity of the laminate can be improved.

[0054] The conductor film may be formed (laminated) in a partial region of the ceramic substrate as a conductive path for wiring or an electrode, but usually a plurality of conductor films are formed (laminated), and may be formed as a pair of opposing conductor films, for example, as shown in Figures 1 to 3. The shape of the conductor film may be a layer, and the planar shape is not limited to a rectangular shape as shown in Figures 1 to 3, and can be selected according to the purpose.

[0055] The conductive film may contain silver as a metal component (second metal component), and preferably contains silver in the form of simple silver or an alloy containing silver (silver-containing alloy).

[0056] In the silver-containing alloy, examples of other metals that are alloyed with silver include transition metals (e.g., periodic table Group 4A metals such as titanium and zirconium; periodic table Group 5A metals such as vanadium and niobium; periodic table Group 6A metals such as molybdenum and tungsten; periodic table Group 7A metals such as manganese; periodic table Group 8 metals such as iron, cobalt, ruthenium, rhodium, palladium, rhenium, iridium, and platinum; periodic table Group 1B metals such as gold), periodic table Group 2B metals (e.g., zinc, cadmium, etc.), periodic table Group 3B metals (e.g., aluminum, gallium, indium, etc.), periodic table Group 4B metals (e.g., germanium, tin, lead, etc.), and periodic table Group 5B metals (e.g., antimony, bismuth, etc.). These metals can be used alone or in combination of two or more. Among these metals, palladium and / or platinum are preferred because they can suppress the sulfurization of silver.

[0057] In the silver-containing alloy, the proportion of silver may be 50% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more in the silver-containing alloy. If the proportion of silver is too low, depending on the type of other metal, the conductor film may be easily oxidized, while in the case of precious metals such as palladium and platinum, the economical efficiency may decrease.

[0058] The proportion of other metals in the silver-containing alloy may be 50 mass % or less, preferably 20 mass % or less, and more preferably 10 mass % or less.

[0059] The proportion of silver (including silver in the alloy) in the second metal component may be 50 mass% or more, preferably 80 mass% or more, even more preferably 90 mass% or more, and even more preferably 99 mass% or more, and in particular may be 100 mass% (formed only of silver).

[0060] As the second metal component, simple silver, a silver-palladium alloy, or a silver-platinum alloy is preferable, and simple silver is particularly preferable.

[0061] The conductor film may further contain a glass component (second glass component) as an inorganic binder in addition to the second metal component. Examples of the second glass component include the glass components exemplified as the first glass component in the section on the connection layer. The glass components may be used alone or in combination of two or more. Among the glass components, borosilicate zinc glass is preferred.

[0062] The softening point of the second glass component, including the preferred embodiments, can also be selected from the ranges described for the softening point of the first glass component.

[0063] The mass ratio of the second metal component to the second glass component (second metal component / second glass component) can be selected within a range of about 99.9 / 0.1 to 90 / 10, for example 99 / 1 to 95 / 5, preferably 98.5 / 1.5 to 96 / 4, and more preferably 98 / 2 to 97 / 3. If the proportion of the second metal component is too low, the electrical properties may be degraded, whereas if it is too high, the adhesion to the ceramic substrate may be degraded.

[0064] The conductive film may contain a non-conductor such as a semiconductor or an insulator (e.g., a filler such as ceramics, an organic vehicle remaining after firing, etc.) so long as the effect of the present invention is not impaired. The proportion of the second metal component and the second glass component in the conductive film is 90 mass % or more, preferably 95 mass % or more, more preferably 99 mass % or more, and may particularly be 100 mass % (formed only of the second metal component and the second glass component).

[0065] The thickness (average thickness) of the conductor film may be 3 μm or more (for example, 3 to 200 μm), for example, 3 to 100 μm, preferably 5 to 50 μm, further preferably 10 to 25 μm, and further preferably 10 to 15 μm. If the thickness of the conductor film is too thin, the electrical properties of the laminate may deteriorate.

[0066] (resistive film) The resistive film is electrically connected to the conductive film, and is formed to drop the power supply voltage to a predetermined voltage in the circuit, or to detect the current value flowing through the circuit from the potential difference across the resistor. Therefore, the shape of the resistive film is not particularly limited as long as it is joined to the conductive film via the connection layer so as to be electrically connected (a layer formed to bridge a plurality of connection layers), but is preferably formed on at least a part of the surface of the connection layer and the area between the opposing connection layers (a part of the area on the ceramic substrate), and is particularly preferably formed on the entire surface of the connection layer, the side end faces of the opposing connection layers (both end faces where the connection layers face each other), and the area of ​​the ceramic substrate between the opposing connection layers. The planar shape of the resistive film is not particularly limited as long as it can be joined to the conductive film via the connection layer and exhibit its function, and is not limited to a rectangular shape as shown in Figures 1 to 3, and can be selected according to the purpose.

[0067] The resistive film contains copper and nickel as metal components (third metal components). Copper and nickel are less expensive materials than precious metals, and a resistive film made of a copper-nickel alloy has a small TCR characteristic of within ±100 ppm / °C by appropriately selecting the composition ratio of copper and nickel, so that an extremely excellent resistive film can be formed in which the resistance hardly changes with temperature changes. Therefore, the resistive film may contain copper and nickel, but it is preferable that the resistive film contains copper and nickel in the form of an alloy containing copper and nickel (copper-nickel-containing alloy).

[0068] In the copper-nickel-containing alloy, examples of metals that can be alloyed with copper and nickel include the other metals exemplified as other metals that can be alloyed with silver in the second metal component of the conductor film.

[0069] In the copper-nickel-containing alloy, the proportion of copper and nickel in the copper-nickel-containing alloy may be 50% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 99% by mass or more, and particularly 100% by mass (copper-nickel alloy formed only of copper and nickel). If the proportion of copper and nickel is too small, it may be difficult to reduce the TCR.

[0070] The proportion of other metals in the copper-nickel alloy may be 50 mass % or less, preferably 20 mass % or less, further preferably 10 mass % or less, and further preferably 1 mass % or less.

[0071] The resistive film may further contain a glass component (third glass component) as an inorganic binder in addition to the third metal component. Examples of the third glass component include the glass components exemplified as the first glass component in the section on the connection layer. The glass components may be used alone or in combination of two or more. Among the glass components, borosilicate glass, particularly zinc borosilicate glass, is preferred.

[0072] The softening point of the third glass component, including the preferred embodiments, can also be selected from the ranges described for the softening point of the first glass component.

[0073] The mass ratio of the third metal component to the third glass component (third metal component / third glass component) can be selected from a range of about 99.9 / 0.1 to 80 / 20, for example 99 / 1 to 90 / 10, preferably 98 / 2 to 93 / 7, and more preferably 97 / 3 to 95 / 5. If the ratio of the third metal component is too low, the electrical properties may be degraded, whereas if it is too high, the adhesion to the ceramic substrate may be degraded.

[0074] The resistive film may contain a non-conductor such as a semiconductor or an insulator (e.g., a filler such as ceramics, an organic vehicle remaining after firing, etc.) within a range that does not impair the effects of the present invention. The total proportion of the third metal component and the third glass component in the resistive film is 90 mass % or more, preferably 95 mass % or more, more preferably 99 mass % or more, and may particularly be 100 mass % (formed only of the third metal component and the third glass component).

[0075] The thickness (average thickness) of the resistive film may be 5 μm or more (for example, 5 to 200 μm), for example, 5 to 100 μm, preferably 10 to 50 μm, further preferably 15 to 30 μm, and further preferably 20 to 25 μm. If the thickness of the resistive film is too thin, the electrical properties of the laminate may deteriorate.

[0076] (insulating protective film) The insulating protective film contains a glass component (fourth glass component) and has heat resistance, moisture resistance, and insulating properties. By covering the resistive film with an insulating protective film having such properties, it is possible to suppress changes in resistance value during long-term use and to protect the resistive film from external environmental factors such as sudden electrical contact.

[0077] The shape of the insulating protective film is not particularly limited as long as it covers at least a part of the resistive film, but it is preferable to cover the entire surface (exposed surface) of the resistive film from the viewpoint of effectively protecting the resistive film from the external environment. When the insulating protective film covers the entire surface of the resistive film, it is preferable to also cover the area adjacent to the resistive film (the surface of the ceramic substrate and the conductor film) from the viewpoint of improving the protective function of the insulating protective film and excellent productivity. In other words, the insulating protective film preferably includes the surface of the resistive film and covers an area larger than the resistive film, but is preferably formed on a part of the conductor film and the ceramic substrate. This is because the conductor film can be electrically connected to an external conductor by leaving an exposed area on the conductor film where the insulating protective film is not laminated.

[0078] The fourth glass component may be the glass components exemplified in the section on the connection layer. The glass components may be used alone or in combination of two or more. Among the glass components, borosilicate glass, aluminosilicate glass, and aluminoborosilicate glass are preferred because of their excellent insulating properties, gas barrier properties, and resistance to plating solutions.

[0079] The softening point (or melting point) of the fourth glass component is preferably lower than the firing temperature for forming the connection layer. The softening point of the glass component is, for example, 400 to 800° C., preferably 420 to 780° C., and more preferably 450 to 750° C. If the softening point is too low, the strength of the insulating protective film may decrease, and conversely, if it is too high, the melt flowability may decrease.

[0080] The fourth glass component preferably contains a filler in view of excellent insulation and gas barrier properties. When the fourth glass component contains a filler, defects due to air bubbles can be suppressed from occurring in the insulating protective film. Examples of fillers include silica, alumina, barium oxide, yttrium oxide, zinc oxide, aluminum oxide, magnesium oxide, and boron oxide. These fillers can be used alone or in combination of two or more. Of these, silica and alumina are preferred.

[0081] The content of the filler in the fourth glass component is 3 to 25 mass %, preferably 5 to 15 mass %, and more preferably 7 to 13 mass %.

[0082] The fourth glass component may be required to have plating resistance when plating an exposed conductive film, and may be an acid-resistant glass or an alkali-resistant glass from the viewpoint of excellent resistance to plating solutions.

[0083] The insulating protective film may contain a non-conductor such as a semiconductor or an insulator (e.g., an organic vehicle remaining after firing) as long as the effect of the present invention is not impaired. The proportion of the fourth glass component in the insulating protective film is 90 mass % or more, preferably 95 mass % or more, more preferably 99 mass % or more, and may particularly be 100 mass % (formed only of the fourth glass component).

[0084] The insulating protective film may have a single layer structure, but a laminated structure of two or more layers is preferable. By forming the insulating protective film into a laminated structure, the second and subsequent layers after covering the resistive film can be fired in the air during the manufacturing process of the insulating protective film, so that the generation of bubbles in the glass can be suppressed and an insulating protective film with excellent insulating properties and protective performance can be formed. The multi-layer structure may be a multi-layer structure of two or more layers, but from the viewpoint of productivity, etc., a two- to four-layer structure is preferable, a two- to three-layer structure is more preferable, and a two-layer structure is even more preferable. The materials (compositions) of the layers in the laminated structure may be different compositions or the same composition.

[0085] The thickness of the insulating protective film (average thickness of the total thickness in the case of a laminated structure) may be 10 μm or more, for example, 20 to 200 μm, preferably 30 to 150 μm, further preferably 60 to 130 μm, and further preferably 80 to 120 μm. If the insulating protective film is too thin, the protective function of the insulating protective film may be reduced.

[0086] (Ceramic substrate) The ceramic substrate is not particularly limited as long as it contains ceramics as a raw material and is a material that can withstand the firing temperature, and various ceramics, glass materials, ceramic green sheets, etc. are commonly used.

[0087] Examples of the material of the ceramic substrate (or ceramic substrate) include metal oxides (alumina or aluminum oxide, zirconia, sapphire, ferrite, zinc oxide, niobium oxide, mullite, beryllia, etc.), silicon oxides (quartz, silicon dioxide, etc.), metal nitrides (aluminum nitride, titanium nitride, etc.), silicon nitride, boron nitride, carbon nitride, metal carbides (titanium carbide, tungsten carbide, etc.), silicon carbide, boron carbide, metal double oxides [metal titanates (barium titanate, strontium titanate, lead titanate, niobium titanate, calcium titanate, magnesium titanate, etc.), metal zirconates (barium zirconate, calcium zirconate, lead zirconate, etc.)], etc. These ceramics can be used alone or in combination of two or more kinds. The ceramics may be low-temperature co-fired ceramics (LTCC).

[0088] Of these ceramic substrates, from the viewpoint of high reliability in the electrical and electronic fields, an alumina substrate, an alumina-zirconia substrate, an aluminum nitride substrate, a silicon nitride substrate, and a silicon carbide substrate are preferred, an alumina substrate, an aluminum nitride substrate, and a silicon nitride substrate are more preferred, and from the viewpoint of excellent adhesion to a resistive film or a conductive film, an aluminum nitride substrate and an alumina substrate are more preferred, and an alumina substrate is most preferred.

[0089] The thickness of the ceramic substrate may be appropriately selected depending on the application, and is, for example, 0.001 to 10 mm, preferably 0.01 to 5 mm, more preferably 0.05 to 3 mm, and even more preferably 0.1 to 1 mm.

[0090] [Laminate properties] The laminate of the present invention has low temperature dependency of resistance value and is excellent in stability. Specifically, the absolute value of the temperature coefficient of resistance (TCR) of the laminate of the present invention is, for example, 300 ppm / °C or less (for example, about 10 to 300 ppm / °C), preferably 200 ppm / °C or less, further preferably 100 ppm / °C or less, more preferably 80 ppm / °C or less, and most preferably 70 ppm / °C or less. If the TCR is too large, there is a risk that the stability of the laminate as a ceramic substrate with a resistive film will decrease.

[0091] In the present application, the TCR of the laminate can be measured by the method described in the Examples below. In addition, in the present application, ppm / °C means a value expressed in the unit " / °C" in 10 6 It means doubling.

[0092] The laminate of the present invention is also excellent in voltage resistance. The laminate of the present invention may have a voltage resistance value of 1.5 kV or more (e.g., about 1.5 to 5 kV), preferably 1.8 kV or more (e.g., about 1.8 to 3 kV), and more preferably 2.0 kV or more, as a result of measuring the durability of the insulating protective film against voltage. If the voltage resistance value is too low, there is a risk that the stability of the laminate as a ceramic substrate with a resistive film will decrease.

[0093] In the present application, the withstand voltage value of the laminate can be measured by the method described in the examples described later.

[0094] [Method of manufacturing laminate] The method for producing the laminate of the present invention includes a conductive film forming step, a connection layer forming step, a resistive film forming step, and an insulating protective film forming step, and the insulating protective film forming step is preferably a step of forming a plurality of steps. For example, when the insulating protective film has a two-layer structure, the insulating protective film forming step is preferably a step of forming a first insulating protective film by firing in a nitrogen atmosphere and a step of forming a second protective film by firing in air. Each step will be described in detail below.

[0095] (Conductor film formation process) In the conductor film forming step, a conductor film paste for forming a conductor film containing silver is applied onto (a portion of) the ceramic substrate, and then fired to form the conductor film.

[0096] The conductive film paste contains second metal particles that are the raw material of the second metal component, and second glass particles that are the second glass component.

[0097] The second metal particles may be single metal particles or alloy particles. In addition, when the metal component is an alloy, the alloy may be formed using alloy particles, or the single metal particles may be mixed to form the alloy.

[0098] The shape of the second metal particles is not particularly limited, and may be spherical (true spherical or approximately spherical), ellipsoidal (elliptical sphere), polyhedral (triangular pyramid, regular hexahedral or cubic, rectangular parallelepiped, octahedral, etc.), plate-like (flat, scale or thin plate-like, etc.), rod-like or bar-like, fibrous, irregular, etc. The shape of the metal particles is usually spherical, ellipsoidal, polyhedral, irregular, etc.

[0099] The median particle size (D50) of the second metal particles can be selected, for example, within a range of about 0.05 to 100 μm (particularly 0.05 to 50 μm). From the viewpoints of improving sinterability and facilitating finishing into a paste with a viscosity suitable for coating (particularly screen printing), it is preferably 0.08 to 10 μm, further preferably 0.1 to 5 μm, even more preferably 0.2 to 4 μm, and most preferably 0.3 to 3 μm.

[0100] In this application, the median particle size (or average particle size) of metal particles (including glass particles described later) means the median particle size (volume basis) based on the particle size distribution measured using a laser diffraction scattering type particle size distribution measuring device.

[0101] The conductive film paste may further contain a second organic vehicle in addition to the second metal particles.

[0102] The second organic vehicle may be an organic binder and / or an organic solvent. The second organic vehicle may be either an organic binder or an organic solvent, but is usually a combination of an organic binder and an organic solvent (a solution of the organic binder in the organic solvent).

[0103] The organic binder (second organic binder) is not particularly limited, and examples thereof include thermoplastic resins (olefin resins, vinyl resins, acrylic resins, styrene resins, polyether resins, polyester resins, polyamide resins, cellulose derivatives, etc.), thermosetting resins (thermosetting acrylic resins, epoxy resins, phenol resins, unsaturated polyester resins, polyurethane resins, etc.). These organic binders can be used alone or in combination of two or more. Among these organic binders, resins that are easily burned off during the firing process and have low ash content, such as acrylic resins (polymethyl methacrylate, polybutyl methacrylate, etc.), cellulose derivatives (nitrocellulose, ethyl cellulose, butyl cellulose, cellulose acetate, etc.), polyethers (polyoxymethylene, etc.), and rubbers (polybutadiene, polyisoprene, etc.), are commonly used.

[0104] The organic solvent (second organic solvent) is not particularly limited, and may be any organic compound that imparts appropriate viscosity to the paste and can be easily evaporated by drying after the paste is applied to the substrate, and may be a high-boiling organic solvent. Examples of such organic solvents include aromatic hydrocarbons (e.g., paraxylene), esters (e.g., ethyl lactate, texanol), ketones (e.g., isophorone), amides (e.g., dimethylformamide), aliphatic alcohols (e.g., octanol, decanol, diacetone alcohol), cellosolves (e.g., methyl cellosolve, ethyl cellosolve), cellosolve acetates (e.g., ethyl cellosolve acetate, butyl cellosolve acetate), carbitols (e.g., carbitol, methyl carbitol, ethyl carbitol), carbitol acetates (e.g., ethyl carbitol acetate, butyl carbitol acetate), and the like. acetate), aliphatic polyhydric alcohols (ethylene glycol, diethylene glycol, dipropylene glycol, butanediol, triethylene glycol, glycerin, etc.), alicyclic alcohols [for example, cycloalkanols such as cyclohexanol; terpene alcohols (monoterpene alcohols, etc.) such as terpineol and dihydroterpineol], aromatic alcohols (metacresol, etc.), aromatic carboxylic acid esters (dibutyl phthalate, dioctyl phthalate, etc.), nitrogen-containing heterocyclic compounds (dimethylimidazole, dimethylimidazolidinone, etc.), etc. These organic solvents can be used alone or in combination of two or more.

[0105] When the second organic binder and the second organic solvent are combined to form the second organic vehicle, the proportion of the second organic binder is 3 to 60 mass %, preferably 5 to 50 mass %, and more preferably 10 to 30 mass % based on the total mass of the second organic vehicle.

[0106] The volume fraction of the second organic vehicle is, for example, 30 to 70 volume %, preferably 40 to 60 volume %, and more preferably 45 to 55 volume %, based on the total volume of the paste for conductive film.

[0107] The conductive film paste may further contain conventional additives within the range that does not impair the effects of the present invention. Examples of conventional additives include curing agents (such as acrylic resin curing agents), colorants (such as dyes and pigments), hue improvers, dye fixing agents, gloss imparting agents, metal corrosion inhibitors, stabilizers (such as antioxidants and ultraviolet absorbers), surfactants or dispersants (such as anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants), dispersion stabilizers, viscosity adjusters or rheology adjusters, moisturizers, thixotropic agents, leveling agents, defoamers, bactericides, and fillers. These additives may be used alone or in combination of two or more.

[0108] The method for preparing the paste for the conductive film is not particularly limited as long as it is possible to prepare a paste containing the above-mentioned components, but it can usually be prepared by dispersing second metal particles in a second organic vehicle using a conventional method.

[0109] Examples of the coating method for applying the conductive film paste to the ceramic substrate include flow coating, spin coating, spray coating, screen printing, flexographic printing, casting, bar coating, curtain coating, roll coating, gravure coating, dipping, slitting, photolithography, and inkjet printing. The coating may be formed on a part of the surface of the ceramic substrate, and is usually formed on a part of the surface in a pattern. When a pattern is formed (drawn) with a coating film, a sintered pattern (conductive film) can be formed by firing the formed pattern (drawn pattern). The drawing method (or printing method) for drawing a pattern (coating layer) is not particularly limited as long as it is a printing method capable of forming a pattern, and examples thereof include screen printing, inkjet printing, intaglio printing (e.g., gravure printing), offset printing, intaglio offset printing, and flexographic printing. Among these methods, screen printing is preferred.

[0110] After coating, the coating may be naturally dried or may be dried by heating. The heating temperature can be selected depending on the type of organic solvent, and is, for example, about 50 to 200° C., preferably about 100 to 150° C. The heating time is, for example, about 5 minutes to 1 hour, and preferably about 10 to 30 minutes.

[0111] The coated film is heated and baked (or heat-treated) at a predetermined temperature to obtain a conductive film.

[0112] The firing temperature (maximum temperature) for forming the conductor film is, for example, 600 to 1000° C., preferably 800 to 900° C. If the firing temperature is too low, the metal particles may not be sintered, resulting in a decrease in electrical conductivity. On the other hand, if the firing temperature is too high, the metal particles may be excessively sintered, causing the conductor film to curl up and reducing adhesion to the ceramic substrate.

[0113] The firing atmosphere may be either an inert gas (eg, nitrogen gas, argon gas, helium gas, etc.) or air, but air is preferred.

[0114] (Connection layer formation process) In the connection layer formation process, a connection layer paste for forming a connection layer made of a metal component that does not contain silver or copper is applied to an area including a portion of the conductor film on the ceramic substrate on which the conductor film is laminated, and then the paste is fired to form the connection layer.

[0115] The connecting layer paste contains first metal particles that are a raw material for a first metal component, and first glass particles that are a raw material for a first glass component.

[0116] The first metal particles may be particles of a single metal or particles of an alloy. When the metal component is an alloy, the alloy may be formed by using alloy particles or by mixing single metal particles.

[0117] The shape of the first metal particles can be selected from the shapes exemplified for the second metal particles, including normal shapes, and the median particle size (D50) of the first metal particles can be selected from the ranges described for the median particle size (D50) of the second metal particles, including the preferred ranges.

[0118] The shape of the first glass particles, including normal shapes, can be selected from the shapes exemplified for the second metal particles, and the median particle size (D50) of the first glass particles can be selected from the ranges described for the median particle size (D50) of the second metal particles, including the preferred ranges.

[0119] The paste for the connection layer may further contain a first organic vehicle in addition to the first metal particles and the first glass particles. The first organic vehicle may be an organic vehicle exemplified as the second organic vehicle. The ratio of the first organic binder to the entire first organic vehicle and the volume fraction of the first organic vehicle may be selected from the ratios and volume fractions described for the second organic vehicle, including the preferred ranges.

[0120] The connection layer paste may further contain conventional additives within the range that does not impair the effects of the present invention. Examples of conventional additives include the conventional additives described above as conventional additives in the conductive film paste.

[0121] The ratio of each component is not particularly limited, and can be appropriately adjusted depending on printability, electrical properties, adhesion to the ceramic substrate, and the like.

[0122] The method for preparing the connecting layer paste is not particularly limited as long as it is possible to prepare a paste containing the above-mentioned components, but it can usually be prepared by dispersing first metal particles and first glass particles in a first organic vehicle using a conventional method.

[0123] The coating method of the paste for the connection layer may be the same as that described above for the paste for the conductive film. The coating is formed in the area including the contact area between the conductive film and the resistive film. The preferred coating method is the same as that described above for the paste for the conductive film.

[0124] After coating, the coating may be naturally dried or may be dried by heating. The heating temperature and heating time may be selected from the ranges described above as the heating temperature and heating time for the conductive film paste, including the preferred ranges.

[0125] The coated film is heated and baked (or heat-treated) at a predetermined temperature to obtain a connection layer.

[0126] The firing temperature (maximum temperature) for forming the connection layer can be selected from the range of, for example, about 600 to 1000° C., preferably 800 to 1000° C., and more preferably 850 to 900° C. If the firing temperature is too low, the glass particles may not be sintered, and the effect of inhibiting alloying between the conductor film and the resistive film may be insufficient. On the other hand, if the firing temperature is too high, the softened glass particles may seep onto the conductor film, and the conductivity may decrease.

[0127] The firing atmosphere may be either an inert gas (eg, nitrogen gas, argon gas, helium gas, etc.) or air, and can be selected depending on the type of the first metal component.

[0128] When the connection layer is formed to have a laminated structure, the connection layer forming step can be repeated to form a connection layer having a multi-layer structure.

[0129] (Resistance film formation process) In the ceramic substrate on which the conductor film and the connection layer are laminated, a resistive film paste containing copper and nickel is applied to at least a portion of the connection layer and a portion of the ceramic substrate (at least a portion of the connection layer and a portion of the ceramic substrate continuous with this portion), and the resistive film is formed by firing in a nitrogen atmosphere. When a plurality of conductor films and connection layers are formed, it is preferable to apply the resistive film paste to the surface of the connection layer (particularly, the entire surface) and the region between the opposing connection layers (a portion of the ceramic substrate surface, a region bridging the connection layers) and then fire in a nitrogen atmosphere.

[0130] The resistive film paste contains third metal particles that are a raw material for a third metal component, and third glass particles that are a raw material for a third glass component.

[0131] The third metal particles may be single metal particles or alloy particles. In addition, when the metal component is an alloy, the alloy may be formed by using alloy particles, or the single metal particles may be mixed to form the alloy.

[0132] The shape of the third metal particles can be selected from the shapes exemplified for the second metal particles, including normal shapes, and the median particle size (D50) of the third metal particles can be selected from the ranges described for the median particle size (D50) of the second metal particles, including the preferred ranges.

[0133] The shape of the third glass particles, including normal shapes, can be selected from the shapes exemplified for the second metal particles, and the median particle size (D50) of the third glass particles can be selected from the range described for the median particle size (D50) of the second metal particles, including the preferred range.

[0134] The paste for resistive film may further contain a third organic vehicle in addition to the third metal particles and the third glass particles. The third organic vehicle may be an organic vehicle exemplified as the second organic vehicle. The ratio of the third organic binder to the entire third organic vehicle and the volume fraction of the third organic vehicle may be selected from the ratios and volume fractions described for the second organic vehicle, including the preferred ranges.

[0135] The resistive film paste may further contain conventional additives within the range not impairing the effects of the present invention. Examples of conventional additives include the conventional additives described above as conventional additives in the conductive film paste.

[0136] The method for preparing the resistive film paste is not particularly limited as long as it is possible to prepare a paste containing the above-mentioned components, but it can usually be prepared by dispersing third metal particles and third glass particles in a third organic vehicle using a conventional method.

[0137] Examples of the coating method of the resistive film paste include the coating method described above as the coating method of the conductive film paste. The coating is formed in the region that bridges the connection layer in order to electrically connect the conductive films formed in the multiple regions via the connection layer. The preferred coating method is the same as the coating method of the conductive film paste.

[0138] After coating, the coating may be naturally dried or may be dried by heating. The heating temperature and heating time may be selected from the ranges described above as the heating temperature and heating time for the conductive film paste, including the preferred ranges.

[0139] The coated film is heated and baked (or heat-treated) at a prescribed temperature to obtain a resistive film.

[0140] The firing temperature (maximum temperature) for forming the resistive film can be selected from the range of, for example, about 600 to 1000° C., preferably 800 to 1000° C., and more preferably 850 to 900° C. If the firing temperature is too low, the metal particles may not be sintered, resulting in a decrease in electrical conductivity. On the other hand, if the firing temperature is too high, the metal particles may segregate, resulting in a failure to obtain the desired electrical characteristics.

[0141] The firing atmosphere may be either an inert gas (eg, nitrogen gas, argon gas, helium gas, etc.) or air, but a nitrogen atmosphere is preferred since it is possible to suppress oxidation of copper.

[0142] (First insulating protective film forming process) In the ceramic substrate on which the conductor film, the connection layer, and the resistive film are laminated, a first insulating protective film paste for forming a first insulating protective film is applied to a partial region of the conductor film and at least a partial region of the resistive film, and then fired to form the first insulating protective film. By applying the first insulating protective film paste only to a partial region of the conductor film, the remaining part of the conductor film can be used as a connection region with an external conductor, while it is preferable to cover the entire surface of the resistive film with the first insulating protective film paste in order to improve protection.

[0143] The first insulating protective film paste contains fourth glass particles that are a raw material for a fourth glass component.

[0144] The shape of the fourth glass particles can be selected from the shapes exemplified for the second metal particles, including normal shapes, and the median particle size (D50) of the fourth glass particles can be selected from the range described for the median particle size (D50) of the second metal particles, including the preferred range.

[0145] The first insulating protective film paste may further contain a fourth organic vehicle in addition to the fourth glass particles. Examples of the fourth organic vehicle include the organic vehicles exemplified as the second organic vehicle. The ratio of the fourth organic binder to the entire fourth organic vehicle and the volume fraction of the fourth organic vehicle can be selected from the ratios and volume fractions described for the second organic vehicle, including the preferred ranges.

[0146] The first insulating protective film paste may further contain conventional additives within the range that does not impair the effects of the present invention. Examples of conventional additives include the conventional additives described above as conventional additives in the conductive film paste.

[0147] The method for preparing the first insulating protective film paste is not particularly limited as long as it is possible to prepare a paste containing the above-mentioned components, but it can usually be prepared by dispersing the fourth glass particles in the fourth organic vehicle using a conventional method.

[0148] The coating method of the first insulating protective film paste may be the coating method described as the coating method of the conductive film paste. The coating is laminated on the surface of the resistive film, and is usually laminated on the entire surface of the resistive film. The preferred coating method is the same as the coating method of the conductive film paste.

[0149] After coating, the coating may be naturally dried or may be dried by heating. The heating temperature and heating time may be selected from the ranges described above as the heating temperature and heating time for the conductive film paste, including the preferred ranges.

[0150] The coated film is heated and baked (or heat-treated) at a prescribed temperature to obtain the first insulating protective film.

[0151] The firing temperature (maximum temperature) for forming the first insulating protective film can be selected from the range of, for example, about 600 to 1000° C., preferably 800 to 1000° C., and more preferably 850 to 900° C. If the firing temperature is too low, the glass particles may not be sintered, and the insulating and protective functions may be impaired. On the other hand, if the firing temperature is too high, the softened glass frit may not cover the base film completely, exposing the conductive film or resistive film, and thus impairing the insulating and protective functions.

[0152] The firing atmosphere may be either an inert gas (such as nitrogen gas, argon gas, or helium gas) or air, but a nitrogen atmosphere is preferred since it can suppress oxidation of copper in the resistive film.

[0153] (Second insulating protective film forming process) In the second insulating protective film forming process, a paste for a second insulating protective film for forming a second insulating protective film is applied onto the first insulating protective film, and then fired in air to form the second insulating protective film.

[0154] In the second insulating protective film forming step, the second insulating protective film can be formed in the same manner as in the first insulating protective film forming step, except for the firing atmosphere. In the second insulating protective film forming step, the fourth glass particles may be different from the fourth glass particles in the first insulating protective film forming step, but are usually the same from the viewpoint of simplicity, etc., and the same is true for the fourth organic vehicle and the conventional additives. The conditions and methods other than the firing atmosphere may also be different from those in the first insulating protective film forming step, but are usually the same from the viewpoint of simplicity, etc.

[0155] On the other hand, regarding the sintering atmosphere, in the first insulating protective film forming step, a nitrogen atmosphere is preferable to suppress oxidation of the copper of the resistive film, but in the second insulating protective film forming step, air is preferable because the resistive film is protected by the first insulating protective film. When the second insulating protective film is sintered in a nitrogen atmosphere, air bubbles caused by the organic vehicle and the like are likely to occur, but by sintering in air, the generation of air bubbles can be suppressed and the stability of the laminate can be improved.

[0156] (Other processes) When the insulating protective film has a laminated structure of three or more layers, the insulating protective film forming process will have three or more steps, but the steps other than the first insulating protective film forming step are preferably fired in air, as in the second insulating protective film forming step. For example, when the insulating protective film has a three-layer structure, the manufacturing method for the laminate has the insulating protective film lamination steps of the first insulating protective film forming step, the second insulating protective film forming step, and the third insulating protective film forming step, but the firing atmosphere is preferably a nitrogen atmosphere in the first insulating protective film forming step, and the firing atmosphere is preferably air in the second insulating protective film forming step and the third insulating protective film forming step. EXAMPLES

[0157] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0158] [Materials used] Ag particles: Silver particles with a median particle size (D50) of 2 μm (specific gravity 10.5) AgPd particles: Ag and Pd alloy particles with a median particle size (D50) of 1 μm (mass ratio of Ag to Pd: Ag / Pd=90 / 10, specific gravity 10.6) AgPt particles: Ag and Pt alloy particles with a median particle size (D50) of 1 μm (mass ratio of Ag to Pt: Ag / Pt=90 / 10, specific gravity 11.1) Au particles: gold particles with a median particle size (D50) of 1 μm (specific gravity 19.3) LaB6 particles: Lanthanum hexaboride particles with a median particle size (D50) of 1 μm (specific gravity 4.8) RuO2 particles: Ruthenium oxide particles with a median particle size (D50) of 1 μm (specific gravity 7.1) Cu particles: Copper particles with a median particle size (D50) of 2 μm (specific gravity 8.9) Ni particles: Nickel particles with a median particle size (D50) of 0.5 μm (specific gravity 8.9) Glass particles A: Glass particles with a median particle size (D50) of 3 μm and a composition of zinc borosilicate glass (specific gravity 3.0) Glass particles B: median particle size (D50) 3 μm, glass particles made of borosilicate glass (specific gravity 3.0) Organic vehicle A: A 30% by mass solution of acrylic resin prepared by dissolving acrylic resin in a mixed solvent of terpineol and butyl carbitol acetate (mass ratio 1 / 1) Organic vehicle B: A 10% by weight solution of ethyl cellulose prepared by dissolving ethyl cellulose in a Texanol solvent. Alumina substrate: 96% alumina substrate

[0159] [Sample preparation] Example 1 A laminate in which a conductive film, a connection layer, a resistive film and an insulating protective film were formed on an alumina substrate in the arrangement shown in FIGS. 1 to 3 was produced as follows.

[0160] First, the paste for conductive film (85% by mass of Ag particles, 2% by mass of glass particles A, 13% by mass of organic vehicle B) was screen-printed onto a 0.6 cm x 0.9 cm rectangle, dried for 20 minutes in a 100°C air drier to remove the solvent, and then fired in a belt furnace to form a conductive film. Firing was performed in air at a peak temperature of 900°C, with a peak temperature retention time of 10 minutes and a total loading-unloading time of 60 minutes. The thickness of the obtained conductive film was measured with a stylus-type film thickness gauge and was about 10 to 15 μm.

[0161] Next, the connection layer paste (40% by mass of LaB6 particles, 40% by mass of glass particles B, 20% by mass of organic vehicle A) was screen-printed on the conductor film in a rectangular area of ​​0.3 cm x 0.5 cm, dried for 20 minutes in a 100°C air dryer to remove the solvent, and then fired in a belt furnace to form a connection layer. The firing was performed in a nitrogen atmosphere at a peak temperature of 900°C, with a peak temperature holding time of 10 minutes and a total loading-unloading time of 60 minutes. The average thickness of the connection layer was 18 μm.

[0162] Furthermore, on the connection layer, a resistive film paste (52% by mass Cu particles, 32% by mass Ni particles, 4% by mass glass particles A, 12% by mass organic vehicle A) was screen-printed in a rectangular area of ​​0.3 x 9 cm, dried for 20 minutes in a 100°C air dryer to remove the solvent, and then fired in a belt furnace to form a resistive film. The firing was performed in a nitrogen atmosphere at a peak temperature of 900°C, with a peak temperature retention time of 10 minutes and a total loading-unloading time of 60 minutes. The resistive film had a thickness of approximately 20-25 μm.

[0163] Finally, in order to prevent oxidation of the resistive film, the first insulating protective film paste (glass particle B 75% by mass, organic vehicle A 25% by mass) was screen-printed on the resistive film in a rectangular area of ​​3 x 12 cm so as to overlap with the resistive film, and then dried for 20 minutes in a 100°C air blower to remove the solvent, and then fired in a belt furnace to form a first insulating protective film. The firing was performed in a nitrogen atmosphere at a peak temperature of 900°C, with a peak temperature retention time of 10 minutes and a total loading-discharging time of 60 minutes. On the formed first insulating protective film, the second insulating protective film paste (glass particle B 75% by mass, organic vehicle A 25% by mass) was further screen-printed on a rectangular area of ​​3 cm x 12 cm, and the process of drying for 20 minutes in a 100°C air blower to remove the solvent was repeated twice, and then fired in a belt furnace to form a second insulating protective film. The firing was performed in air at a peak temperature of 900°C, with a peak temperature hold time of 10 minutes and a total loading-unloading time of 60 minutes. The thickness of each insulating protective film was approximately 50 to 55 μm.

[0164] Through the above steps, a ceramic substrate with a resistive film (laminate) was obtained in which the conductive film, the connection layer, the resistive film, the first insulating protective film, and the second insulating protective film were laminated on the alumina substrate.

[0165] Example 2 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that Ni particles were used instead of the LaB6 particles contained in the connection layer paste.

[0166] Example 3 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that RuO2 particles and organic vehicle B were used instead of LaB6 particles and organic vehicle A contained in the connecting layer paste, and the firing was carried out in air.

[0167] Example 4 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that Au particles and organic vehicle B were used instead of LaB6 particles and organic vehicle A contained in the connecting layer paste, the compounding ratio was changed to 64 mass % Au particles, 16 mass % glass particles B, and 20 mass % organic vehicle B, and the firing was carried out in air.

[0168] Example 5 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that AgPd particles were used instead of the Ag particles contained in the conductive film paste.

[0169] Example 6 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that AgPt particles were used instead of the Ag particles contained in the conductive film paste.

[0170] Example 7 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that glass particles A were used instead of glass particles B contained in the connection layer paste.

[0171] Example 8 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that the compounding ratio of LaB6 particles and glass particles B contained in the connecting layer paste was changed to 20 mass % LaB6 particles, 60 mass % glass particles B, and 20 mass % organic vehicle A.

[0172] Example 9 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that the compounding ratio of LaB6 particles and glass particles B contained in the connecting layer paste was changed to 48 mass % LaB6 particles, 32 mass % glass particles B, and 20 mass % organic vehicle A.

[0173] Example 10 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that the conditions for screen printing the connecting layer paste were adjusted so that the average thickness of the connecting layer after firing was 6 μm.

[0174] Example 11 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that the conditions for screen printing the connecting layer paste were adjusted so that the average thickness of the connecting layer after firing was 48 μm.

[0175] Comparative Example 1 A connecting layer was not formed, and a conductive film (silver) and a resistive film (copper nickel) were formed in the same manner as in Example 1. Observation at this stage confirmed that the conductive film (silver) and the resistive film (copper nickel) were in a physically and electrically disconnected state (disconnected state) due to a reaction (alloying) between them, so an insulating protective film was not formed.

[0176] Comparative Example 2 By using Ag particles and organic vehicle B instead of LaB6 particles and organic vehicle A contained in the paste for the connection layer, a conductor film (silver), a connection layer (silver), and a resistive film (copper nickel) were formed in the same manner as in Example 1. The connection layer was fired in air. Observation at this stage confirmed that the connection layer (silver) and the resistive film (copper nickel) were physically and electrically disconnected (disconnected) due to a reaction (alloying) between them, so an insulating protective film was not formed.

[0177] Comparative Example 3 By using Cu particles instead of LaB6 particles contained in the connection layer paste, a conductor film (silver), a connection layer (copper), and a resistive film (copper nickel) were formed in the same manner as in Example 1. Observation at this stage confirmed that the connection layer (copper) and the conductor film (silver) were in a physically and electrically disconnected state (disconnected state) due to a reaction (alloying) between them, so an insulating protective film was not formed.

[0178] Comparative Example 4 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that a connection layer was not formed, AgPd particles and organic vehicle B were used instead of Cu particles, Ni particles and organic vehicle A contained in the resistive film paste, and all firing was performed in air. All firing was performed in air because no copper component was included. The thickness of the silver-palladium resistive film was about 10 to 15 μm.

[0179] Comparative Example 5 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that Cu particles and organic vehicle A were used instead of Ag particles and organic vehicle B contained in the conductive film paste, no connection layer was formed, and all firing was performed under a nitrogen atmosphere.

[0180] Comparative Example 6 Except for using AgPd particles and organic vehicle B instead of Cu particles, Ni particles and organic vehicle A contained in the resistive film paste, and firing the resistive film and insulating protective film in air, a ceramic substrate with a resistive film was obtained in the same manner as in Example 1. The thickness of the silver-palladium resistive film was about 10 to 15 μm.

[0181] Comparative Example 7 A ceramic substrate with a resistive film was obtained in the same manner as in Example 1, except that Cu particles and organic vehicle A were used instead of Ag particles and organic vehicle B contained in the conductive film paste, and all firing was performed under a nitrogen atmosphere because the conductive film contains copper components.

[0182] The evaluation methods for the ceramic substrates with resistive film obtained in Examples 1 to 11 and Comparative Examples 1 to 7 are shown below.

[0183] [Conductive film and resistive film connection check] The ceramic substrates with resistive film produced in each of the examples and comparative examples were observed under a microscope and rated according to the following criteria.

[0184] (Judgment criteria) A: The conductive film and resistive film do not react with each other and are not disconnected physically or electrically. C: The conductive film and resistive film have reacted, causing a physical and electrical disconnection.

[0185] [Whether or not there are air bubbles in the insulating protective film] The insulating protective film of the ceramic substrate with resistive film produced in each Example and Comparative Example was observed under a microscope to determine the presence or absence of bubbles with a diameter of 20 μm or more. In order to improve insulation properties and concealment against oxygen permeation, it is preferable that the insulating protective film has no bubbles.

[0186] (Judgment criteria) Judgment a: When there are no bubbles with a diameter of 20 μm or more in the insulating protective film C: When there are bubbles with a diameter of 20 μm or more in the insulating protective film

[0187] [Temperature coefficient of resistance TCR] The evaluation sample was placed in a thermostatic chamber at 25°C and left to stand for 5 minutes or more, and then the average resistance value (volume resistivity) was measured by a four-terminal method. Next, the evaluation sample was placed in a thermostatic chamber at 75°C and left to stand for 5 minutes or more, and then the average resistance value (volume resistivity) was measured by a four-terminal method. Based on the average resistance value after standing at 75°C (average resistance value at 75°C) and the average resistance value after standing at 25°C (average resistance value at 25°C), the temperature coefficient of resistance TCR as a rate of change was calculated by the following formula, and the evaluation was made according to the following criteria.

[0188] TCR(ppm / ℃)=10 6 ×[Average resistance value at 75℃ (Ω) - Average resistance value at 25℃ (Ω)] / [Average resistance value at 25℃ (Ω) × (75 - 25) (℃)]

[0189] Generally, a lower TCR is preferable. When considering chip resistor applications, a value of 100 ppm / °C or less is desirable, but when considering applications to fixing heaters, a value up to about 300 ppm / °C is considered to be acceptable.

[0190] (Judgment criteria) a: Absolute value of TCR is less than 300ppm / ℃ C: Absolute value of TCR is 300ppm / ℃ or more

[0191] [Voltage resistance] For the evaluation sample, one of the two electrodes extended from the dielectric strength measuring instrument was connected to the conductive film, and the other was connected to copper foil cut to a size that could completely cover the insulating protective film. Next, the copper foil was placed on the insulating protective film and a voltage was applied. The applied voltage was increased at a rate of about 0.1 kV / sec., and the voltage at which the insulating protective film broke down was taken as the withstand voltage value. For example, assuming use as a fixing heater, it is preferable that the withstand voltage can withstand 1.8 kV for more than one minute without dielectric breakdown.

[0192] (Judgment criteria) a rating: Withstand voltage is 2.0 kV or more C rating: Withstand voltage value is less than 2.0 kV

[0193] [Paste material cost] For the conductor film, connection layer, and resistive film, the fewer the number of precious metals silver, palladium, ruthenium, gold, and platinum contained, the lower the cost of the paste material and the more preferable (e.g., Example 1 contains one silver component, Example 3 contains two components, silver and ruthenium, and Comparative Example 4 contains three components, silver and a silver-palladium alloy).

[0194] (Judgment criteria) Classification a: When the conductive film, connection layer, or resistive film contains one of silver, palladium, ruthenium, gold, or platinum B: When the conductive film, connection layer, or resistive film contains two of the following metals: silver, palladium, ruthenium, gold, or platinum C: Conductive film, connection layer, or resistive film contains three or more of the following metals: silver, palladium, ruthenium, gold, or platinum

[0195] [Overall Judgment] Based on the judgment of each evaluation item, an overall evaluation was made according to the following criteria.

[0196] (Judgment criteria) A rank: When all evaluation items are rated A B rank: There is no C rating in any evaluation item, and even one B rating C rank: If there is at least one C rating in each evaluation item

[0197] Table 1 shows the evaluation results of the resistive film-attached ceramic substrates obtained in Examples 1 to 7 and Comparative Examples 1 to 7.

[0198] [Table 1]

[0199] Example 1 This is an example where a connection layer (lanthanum hexaboride) was provided between the conductive film (silver) and resistive film (copper nickel), and the conductive film and resistive film were formed without any disconnection. The TCR was small at 66 ppm / ℃, and the withstand voltage value was large at 2.3 kV, both of which were at good levels. As the only precious metal used was the silver in the conductive film, it is also advantageous in terms of material costs.

[0200] Example 2 This is an example in which the connection layer was changed to nickel compared to Example 1. As in Example 1, good levels of TCR and withstand voltage were obtained. Since the only precious metal used was the silver conductor film, it is also advantageous in terms of material costs.

[0201] (Examples 3 and 4) In Example 3, in which the connection layer was changed to ruthenium oxide compared to Example 1, and Example 4, in which it was changed to gold, good levels of TCR and withstand voltage were obtained, similar to those of Example 1. However, in terms of material costs, Example 3 contains silver in the conductor film and ruthenium in the connection layer, while Example 4 contains silver in the conductor film and gold in the connection layer, making them somewhat less advantageous than Example 1.

[0202] (Examples 5 and 6) In Example 5, in which the conductor film was changed to silver-palladium compared to Example 1, and Example 6, in which the conductor film was changed to silver-platinum, good levels of TCR and withstand voltage were obtained, similar to those of Example 1. However, in terms of material costs, Example 5 contains silver and palladium in the conductor film, and Example 6 contains silver and platinum in the conductor film, so they are somewhat disadvantageous compared to Example 1.

[0203] Example 7 In Example 7, in which the glass component of the connection layer was changed to glass particles A in comparison with Example 1, good levels of TCR and withstand voltage were obtained, similar to those of Example 1. Since the only precious metal used was silver in the conductor film, it is also advantageous in terms of material costs.

[0204] Comparative Example 1 In the case of a structure in which a conductive film (silver) and a resistive film (copper-nickel) are directly laminated, the formation of an alloy leads to disconnection, which is not preferable.

[0205] Comparative Example 2 This is an example in which a connection layer (silver) was provided in addition to Comparative Example 1. The connection layer (silver) and the resistive film (copper-nickel) were alloyed together, resulting in disconnection, which was not preferable.

[0206] Comparative Example 3 This is an example in which a connection layer (copper) was provided in comparison with Comparative Example 1. The connection layer (copper) and the conductor film (silver) were alloyed together, resulting in disconnection, which was not preferable.

[0207] Comparative Example 4 In the case of a structure in which the conductive film (silver) and the resistive film (silver-palladium) are directly laminated, the withstand voltage value was at a good level of 2.5 kV, but the TCR was at a high level of 601 ppm / ℃. It is also disadvantageous in terms of material cost because it uses a large amount of precious metals.

[0208] Comparative Example 5 In the case of a structure in which the conductor film (copper) and resistive film (copper nickel) are directly laminated, the TCR was at a good level of 50 ppm / ℃, but the withstand voltage value was at a low level of 0.8 kV (less than 2.0 kV). The reason for the low withstand voltage value is thought to be that, due to the use of copper, which is easily oxidized, in the conductor film, the insulating protective film had to be fired in a nitrogen atmosphere, and the decomposition gas of the resin remained in the film in large amounts as bubbles that reduced the withstand voltage.

[0209] Comparative Example 6 This is an example in which a connection layer (lanthanum hexaboride) was provided in comparison with Comparative Example 4. As with Comparative Example 4, the withstand voltage value was at a good level of 2.4 kV, but the TCR was at a high level of 615 ppm / ℃. This is an example in which the combination of a conductor film (silver) and a resistive film (silver palladium) cannot satisfy the TCR characteristics even if a connection layer (lanthanum hexaboride) is provided. In addition, since a large amount of precious metals is used, it is also disadvantageous in terms of material costs.

[0210] Comparative Example 7 This is an example in which a connection layer (lanthanum hexaboride) was provided in comparison with Comparative Example 5. As with Comparative Example 5, the TCR was at a good level of 56 ppm / °C, but the withstand voltage value was at a low level of 0.7 kV (less than 2.0 kV). This is an example in which the combination of a conductor film (copper) and a resistive film (copper nickel) cannot satisfy the withstand voltage characteristics even if a connection layer (lanthanum hexaboride) is provided.

[0211] Table 2 shows the evaluation results of the ceramic substrates with resistive film obtained in Examples 1 and 8 to 11.

[0212] [Table 2]

[0213] (Examples 8 and 9) In Example 8, in which the volume ratio of the metal component and the glass component of the connecting layer was changed to metal component / glass component = 17 / 83 compared to Example 1, and in Example 9, in which the volume ratio was changed to metal component / glass component = 49 / 51, good levels of TCR and withstand voltage values ​​were obtained, similar to those of Example 1.

[0214] (Examples 10 and 11) In Example 10, in which the average thickness of the connection layer was changed to 6 μm compared to Example 1, and in Example 11, in which the average thickness was changed to 48 μm, similarly good levels of TCR and withstand voltage were obtained as in Example 1. [Industrial Applicability]

[0215] The laminate of the present invention can be used in chip resistors, modules with built-in resistors, substrates with built-in resistors, ceramic heaters, substrates for mounting LEDs, and the like. [Explanation of symbols]

[0216] 1...Laminate 2. Ceramic substrate 3...Conductor film 4…Connecting layer 5...Resistance film 6...First insulating protective film 7...Second insulating protective film

Claims

1. A laminate comprising a ceramic substrate, a conductive film containing silver, a resistive film containing copper and nickel, and an insulating protective film, wherein a connecting layer containing a metal component not containing silver or copper is interposed between the conductive film and the resistive film.

2. 2. The laminate according to claim 1, wherein the metal component of said connection layer comprises at least one selected from the group consisting of lanthanum hexaboride, nickel, gold and ruthenium oxide.

3. 3. The laminate according to claim 1, wherein the connection layer further contains a glass component, and a volume ratio of the metal component to the glass component is metal component / glass component=60 / 40 to 10 / 90.

4. 3. The laminate according to claim 1, wherein the average thickness of the connection layer is 5 to 50 μm.

5. 3. The laminate according to claim 1, wherein the conductive film is made of silver, a silver-palladium alloy or a silver-platinum alloy.

6. 3. The laminate according to claim 1, wherein the insulating protective film contains a glass component.

7. 3. The laminate according to claim 1, wherein the insulating protective film covers a partial area of ​​the conductor film and at least a partial area of ​​the resistive film.

8. 3. The laminate according to claim 1, wherein the insulating protective film has a multi-layer structure.

9. A conductive film forming process in which a conductive film paste for forming a conductive film containing silver is applied onto a ceramic substrate and fired in air to form a conductive film; a connection layer forming step of applying a connection layer paste for forming a connection layer containing a metal component not containing silver and copper to an area including a part of the conductor film, and firing the paste in air or a nitrogen atmosphere to form a connection layer; a resistive film forming step of applying a resistive film paste containing copper and nickel to at least a portion of the connection layer and a portion of the ceramic substrate, and firing the paste in a nitrogen atmosphere to form a resistive film; a first insulating protective film forming step of applying a first insulating protective film paste to a partial region of the conductor film and at least a partial region of the resistive film, and firing the paste in a nitrogen atmosphere to form a first insulating protective film; a second insulating protective film forming step of applying a second insulating protective film paste for forming a second insulating protective film on the first insulating protective film, and firing the paste in air to form a second insulating protective film.

Citation Information

Patent Citations

  • Chip resistor

    JP1991138901A

  • Molding device for optical member

    JP1993043261A

  • Thick film chip resistor

    JP1993205903A

  • Resistor and its manufacture

    JP1997246004A

  • Circuit board

    JP2000049435A

Cited By

  • Method for manufacturing electronic component, electronic component, and thin film resistor

    JP2026090161A

  • Method for manufacturing electronic components, electronic components, and thin-film resistors

    JP7939414B2