Power storage device
Patent Information
- Application Number
- JP2023044821
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-21
AI Technical Summary
【0017】 この蓄電デバイスは、中間部P量も、端部P量の96~104%である。即ち、この蓄電デバイスでは、全体に亘り、Pを含む支持塩に由来するSEI被膜が均一に形成されており、電極体内の軸線方向に生じる局所的なIV抵抗の増加を抑え、電極体全体の抵抗増加を抑制した蓄電デバイスとなる。
Smart Images

Figure 2024134568000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electricity storage device. [Background technology]
[0002] Conventionally, in an electricity storage device such as a battery having an electrode body and an electrolyte in a case, it was necessary to consider the uneven penetration (uneven impregnation) of the electrolyte into the electrode body. For example, Patent Document 1 discloses a method for producing a lithium ion battery in which an electrolyte is impregnated in at least one of the separator and the electrode active material layer (B) before a lamination step in which an electrode active material layer (A), a separator, and an electrode active material layer (B) are laminated to obtain a lamination unit, thereby preventing or suppressing the uneven penetration of the electrolyte. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-212464 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as described in Patent Document 1, when a wound-type electrode body is used instead of a stacked unit, i.e., a laminated electrode body, it becomes necessary to handle a strip-shaped separator impregnated with an electrolyte or a strip-shaped electrode plate impregnated with an electrolyte, which makes handling difficult.
[0005] On the other hand, as a solvent for the electrolyte of an electricity storage device, ethylene carbonate (hereinafter also referred to as EC) which forms an SEI film may be used in addition to dimethyl carbonate (hereinafter also referred to as DMC), ethyl methyl carbonate (hereinafter also referred to as EMC), etc., in order to facilitate the formation of an SEI film on the negative electrode active material layer during initial charging. For example, an EC / DMC / EMC mixed solvent may be used for the electrolyte.
[0006] However, when an electrolyte containing EC is allowed to permeate into the inside of the electrode body from the end of the electrode body where the electrolyte has not yet permeated, it has been found that the permeation speed of EC is relatively slow compared to supporting electrolytes such as DMC, EMC, and LiPF6 dissolved in these electrolytes. EC has a melting point of about 34-37°C, which is relatively high compared to DMC (melting point 2-4°C) and EMC (melting point -53°C), and it also has a high viscosity, so it is thought that EC does not permeate easily compared to DMC when permeating into the inside of the electrode body along the negative electrode active material layer and separator.
[0007] For example, in a power storage device using a wound electrode assembly, in which the belt-shaped electrode plate is wide and the electrolyte permeates a long distance, even if the electrolyte is made to permeate from both ends in the axial direction and reaches the center in the axial direction to permeate the entire electrode assembly, there are cases in which the EC has not yet sufficiently reached the center in the axial direction. That is, during initial charging, there are cases in which the amount of EC per unit area (hereinafter also referred to as area density) present in various places in the electrode body is uneven, that is, there are cases in which the EC permeates unevenly.
[0008] In this state, when an initial charge is performed on an electric storage device such as a secondary battery to form an anode SEI coating on the anode active material layer, an anode SEI coating derived from EC and a supporting salt (e.g., LiPF6, etc.) is formed. However, as described above, the anode SEI coating derived from EC is less likely to be formed near the axial center of the electrode body where the EC content is low. In this case, to compensate for this, a relatively large amount of the anode SEI coating derived from the supporting salt is formed. However, the resistance of the anode SEI coating derived from the supporting salt is higher than that of the anode SEI coating derived from EC. For this reason, it has been found that the anode SEI coating derived from the supporting salt is locally increased near the axial center of the electrode body where the area density of EC is low, compared to the areas where the area density of EC is high, such as near both ends in the axial direction, resulting in a relatively high resistance anode active material layer. As a result, the resistance of the entire electric storage device is also high.
[0009] The present invention has been made in consideration of the above-mentioned current situation, and provides an electricity storage device in which the formation of a negative electrode SEI coating derived from a supporting salt in a negative electrode active material layer in a wound-type electrode body is generally uniform, and an increase in resistance is suppressed. [Means for solving the problem]
[0010] (1) One aspect of the present invention for solving the above problem includes an electrolytic solution containing ethylene carbonate, a solvent having a melting point lower than that of ethylene carbonate, and a supporting salt containing P; a wound-type electrode body having a strip-shaped positive electrode plate, a strip-shaped negative electrode plate having a strip-shaped negative electrode active material layer on which an SEI coating is formed, and a strip-shaped separator, the electrode body being an electric storage device in which the electrolytic solution permeates inside; and a case accommodating the electrode body and the electrolytic solution, wherein the electrode body is an electric storage device in which the width dimension of the negative electrode active material layer is 180 mm or more, and an amount of P contained in the SEI coating formed on the negative electrode active material layer is 90 to 105% of the amount of P at a center portion in the width direction, based on an amount of P at an end portion in the width direction of the negative electrode active material layer.
[0011] This energy storage device comprises an electrolyte solution containing a supporting salt containing EC and P, and an electrode body in which the width dimension of the negative electrode active material layer is 180 mm or more. As a result, as described above, uneven penetration of EC is likely to occur, and in the central portion where EC has difficulty reaching, an SEI coating derived from EC is difficult to form, and instead, an SEI coating derived from the supporting salt containing P tends to be formed in excess. However, in this electricity storage device, the amount of P in the central portion of the SEI coating of the negative electrode active material layer is within a range of 90 to 105% of the amount of P at the end portions. That is, the amount of P in the central portion is roughly equal to or slightly less than the amount of P at the end portions. In other words, in this electricity storage device, even in the central portion of the negative electrode active material layer, an excessive amount of the negative electrode SEI coating derived from the P-containing supporting salt is not formed, and the local increase in IV resistance occurring in the axial direction (width direction of the negative electrode plate) within the electrode body is suppressed, resulting in an electricity storage device that suppresses an increase in resistance of the entire electrode body.
[0012] Examples of the power storage device include secondary batteries such as lithium ion secondary batteries and sodium ion secondary batteries, and capacitors such as lithium ion capacitors. Examples of the wound electrode body include cylindrical wound electrode bodies and flat wound electrode bodies.
[0013] As the electrolyte, a non-aqueous electrolyte obtained by dissolving a supporting salt in an organic solvent can be used. Examples of organic solvents used in the electrolyte include ethylene carbonate (EC), as well as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), which can be mixed with EC to form a mixed solvent and have a lower melting point than EC.
[0014] The electrolyte may also contain, as a supporting salt, a lithium salt containing P, such as LiPF6, or a sodium salt, such as NaPF6.
[0015] In addition to the EC contained in the electrolyte, the electrode body may also contain a substance capable of forming a negative electrode SEI coating on the negative electrode active material particles during the initial charging process, such as EC, vinylene carbonate, LiBOB, etc., which are used separately from the electrolyte.
[0016] (2) The electric storage device according to (1) above, wherein the amount of P in an intermediate portion of the negative electrode active material layer that is located midway between the end portion and the central portion in the width direction is 96 to 104% of the amount of P in the end portion.
[0017] In this electricity storage device, the amount of P in the middle portion is also 96 to 104% of the amount of P at the end portions. That is, in this electricity storage device, an SEI coating derived from a supporting salt containing P is uniformly formed over the entire device, suppressing a local increase in IV resistance that occurs in the axial direction within the electrode body and suppressing an increase in resistance of the entire electrode body.
[0018] (3) In the electricity storage device according to (1) or (2) above, the amount of P may be the amount of P obtained by ICP-MS analysis using the negative electrode plate that has been removed from the electricity storage device and washed to remove the adhering electrolytic solution.
[0019] In this electricity storage device, the P amount in each portion of the negative electrode active material layer is obtained by ICP-MS analysis, so that accurate P amounts and relative P amounts can be obtained. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a partially cutaway perspective view of a battery according to an embodiment. [Diagram 2] FIG. 4 is an explanatory diagram illustrating a state in which a negative electrode SEI coating is formed on a negative electrode active material particle in a negative electrode active material layer in the embodiment. [Diagram 3] FIG. 2 is a perspective view of a flat wound electrode body and an unpermeated electrode body in the embodiment. [Figure 4] FIG. 2 is an explanatory diagram illustrating a flat wound type unpermeated electrode body developed to show a positive electrode plate, a negative electrode, and a separator according to the embodiment. [Diagram 5] 1 is a flowchart of a method for manufacturing a battery according to an embodiment. [Figure 6] FIG. 4 is an explanatory diagram showing a manufacturing process of an unpermeated negative electrode plate according to the embodiment. [Figure 7] FIG. 11 is an explanatory diagram showing a stripe pattern in which the non-containing negative electrode paste and the additional negative electrode paste are applied to a wide negative electrode foil by a die coater in the embodiment. [Figure 8] FIG. 11 is an explanatory diagram relating to Comparative Example 1, in which a flat wound type unpermeated electrode body is developed to show a positive electrode plate, a negative electrode, and a separator. [Figure 9] FIG. 11 is an explanatory diagram relating to Comparative Example 2, showing a flat wound type unpermeated electrode body developed to show a positive electrode plate, a negative electrode, and a separator. [Figure 10] FIG. 2 is an explanatory diagram showing an examination site in an electrode body of the battery according to the embodiment and comparative examples 1 and 2. [Figure 11]1 is a graph showing the relationship between the investigated sites in the electrode bodies of the batteries according to the embodiment and comparative examples 1 and 2 and the relative content of ethylene carbonate. [Figure 12] 1 is a graph showing the relationship between the relative P amount and an examination site in an electrode body of the batteries according to the embodiment and comparative examples 1 and 2. [Figure 13] 1 is a graph showing the relationship between the relative IV resistance value and the examined portion in the electrode body of the batteries according to the embodiment and comparative examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] (Embodiment) Hereinafter, a battery 1 (an example of an electricity storage device) which is a lithium ion secondary battery according to an embodiment of the present invention and its manufacture will be described with reference to Figures 1 to 7. The battery 1 is a rectangular, sealed lithium ion secondary battery, and is mounted in vehicles such as hybrid cars, plug-in hybrid cars, and electric cars, as well as in various devices.
[0022] The battery 1 of this embodiment includes a case 7, and an electrode assembly 2 and an electrolyte 6 housed inside the case 7. The case 7 is made of metal (aluminum in this embodiment) and has a rectangular box shape. The case 7 is made of a metal and has a square cylindrical case body 7H with a bottom and a lid 7L located at the upper BH1 in the height direction BH. A positive electrode terminal 8P and a negative electrode terminal 8N are fixed to the lid 7L via an insulating member 9. The lid 7L is perforated with a liquid injection hole 7LH for injecting the electrolyte 6, and is sealed by a liquid injection plug 7LP after the liquid is injected. The electrode assembly 2 is covered in a bag-shaped insulating film (not shown) inside the case 7. A part of the electrolyte 6 housed in the case 7 is impregnated in the electrode assembly 2, and the remaining part is collected at the bottom of the case 7.
[0023] The non-permeated electrode body 12 (see Figs. 3 and 4) not impregnated with the electrolyte 6 is a so-called flat wound electrode body, in which a strip-shaped non-permeated positive electrode plate 13 and a strip-shaped non-permeated negative electrode plate 14 (an example of an additional electrode plate) are wound via a pair of strip-shaped non-permeated separators 15, and pressed in the thickness direction CH to be flattened. For this reason, the electrode body 2 (see Figs. 1, 3, and 4) housed in the case 7 and having the non-permeated electrode body 12 impregnated with the electrolyte 6 is also housed in the case 7 and has a strip-shaped positive electrode plate 3 and a strip-shaped negative electrode plate 4, each of which is impregnated with the electrolyte 6, wound via a pair of strip-shaped separators 5, and is thinned and flattened in the thickness direction CH perpendicular to the paper surface in Fig. 1. This electrode body 2 is housed in the case 7 in a horizontal position in which the winding axis AX coincides with the width direction AH (the left-right direction in Fig. 1).
[0024] As described below, the electrode body 2 in the battery 1 is initially charged after the electrolyte solution 6 is impregnated into the unpermeated electrode body 12 housed in the case 7. For this reason, as shown in Fig. 2, a negative electrode SEI coating 4AC derived from ethylene carbonate 6VE, a solvent contained in the electrolyte solution 6, and a supporting salt 6S containing P are formed around the negative electrode active material particles 4AP constituting the negative electrode active material layer 4A formed on the negative electrode foil 4F of the electrode body 2. The formation of this negative electrode SEI coating 4AC enables the battery 1 to be charged and discharged stably with low resistance, compared to a case where the negative electrode SEI coating 4AC is not formed or is insufficiently formed.
[0025] Of the flat wound electrode body 2 and the unpermeated electrode body 12, one side XH1 of the axial direction XH along the winding axis AX (in this embodiment, this corresponds to one side AH1 in the width direction AH of the battery 1; upper side in FIG. 3) is provided with positive current collecting parts 2P, 12P formed by winding current collecting parts 3S, 13S of the positive plate 3 or the unpermeated positive plate 13. Conversely, the other side XH2 of the axial direction XH (in this embodiment, this corresponds to the other side AH2 in the width direction AH of the battery 1; lower side in FIG. 3) is provided with negative current collecting parts 2N, 12N formed by winding current collecting parts 4S, 14S of the negative plate 4 or the unpermeated negative plate 14. The portion between the positive electrode collector 2P, 12P and the negative electrode collector 2N, 12N is a main body portion 2H, 12H in which a positive electrode plate 3 and a negative electrode plate 4 are wound with a separator 5 between them, or an unpermeated positive electrode plate 13 and an unpermeated negative electrode plate 14 are wound with a unpermeated separator 15 between them.
[0026] The positive electrode terminal 8P is made of an aluminum plate bent into a predetermined shape. An inner connection part 8PI forming one end of the positive electrode terminal 8P is connected to a positive electrode current collector 2P arranged on one side AH1 in the width direction AH of the electrode body 2. On the other hand, the other end of the positive electrode terminal 8P is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8PO. In addition, the negative electrode terminal 8N is made of a copper plate bent into a predetermined shape. An inner connection part 8NI forming one end of this negative electrode terminal 8N is connected to a negative electrode current collector 2N arranged on the other side AH2 in the width direction AH of the electrode body 2. On the other hand, the other end of the negative electrode terminal 8N is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8NO.
[0027] The electrolyte 6 is a non-aqueous electrolyte containing an organic solvent 6V and a supporting salt 6S. In this embodiment, the organic solvent 6V is a mixture of ethylene carbonate (EC) 6VE and another solvent 6VL, dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC), in a weight ratio of 3:4:3. LiPF6 is used as the supporting salt 6S containing P. The concentration of LiPF6 in the electrolyte 6 is 1.1 mol / L.
[0028] As shown in FIG. 4, the strip-shaped unpermeated positive electrode plate 13 of the unpermeated electrode body 12 includes a positive electrode foil 13F made of aluminum foil and a positive electrode active material layer 13A laminated on both surfaces of the positive electrode foil 13F. The positive electrode active material layer 13A is made of positive electrode active material particles, conductive particles, and a binder (not shown). In this embodiment, lithium transition metal composite oxide particles, specifically, for example, lithium nickel cobalt manganese composite oxide particles, are used as the positive electrode active material particles. For example, acetylene black (AB) is used as the conductive particles. Also, for example, polyvinylidene fluoride (PVDF) is used as the binder. At the end of one side WH1 (upper side in FIG. 4) of the strip-shaped unpermeated positive electrode plate 13 in the width direction WH, the positive electrode active material layer 13A does not exist on the positive electrode foil 13F, and the positive electrode foil 13F is exposed to form a current collecting portion 13S. On the other hand, the remaining portion of the non-permeated positive electrode plate 13 is a positive electrode portion 13P in which positive electrode active material layers 13A are laminated on both surfaces of a positive electrode foil 13F. As can be seen from Fig. 3 and Fig. 4, the width direction WH (the vertical direction in Fig. 4) of the non-permeated positive electrode plate 13 etc. coincides with the axial direction XH, and one side WH1 coincides with one side XH1.
[0029] On the other hand, of the unpermeated electrode body 12, the strip-shaped unpermeated negative electrode plate 14 includes a negative electrode foil 14F made of copper foil and a negative electrode active material layer 14A laminated on both surfaces of the negative electrode foil 14F, and does not contain P. The negative electrode active material layer 14A is made of a negative electrode active material particle 14AP and a binder (not shown). In this embodiment, graphite particles are used as the negative electrode active material particle 14AP. For example, carboxymethyl cellulose (CMC) is used as the binder. Note that, at the end of the other side WH2 (lower in FIG. 4) of the width direction WH of the strip-shaped unpermeated negative electrode plate 14, the negative electrode active material layer 14A does not exist on the negative electrode foil 14F, and the negative electrode foil 14F is exposed as a current collecting portion 14S. On the other hand, the remaining part of the unpermeated negative electrode plate 14 is a negative electrode portion 14N in which the negative electrode active material layer 14A is laminated on both surfaces of the negative electrode foil 14F. In this embodiment, the width dimension AW of the negative electrode active material layers 4A, 14A in the width direction WH is AW=180 mm.
[0030] In addition, a pair of strip-shaped unpermeated separators 15 of the unpermeated electrode body 12 are made of a porous resin. As shown in FIG. 4, the unpermeated separators 15 are stacked so as to be interposed between the unpermeated negative electrode plate 14 and the unpermeated positive electrode plate 13 when wound. The unpermeated negative electrode plate 14 and the negative electrode portion 14N are slightly wider in the width direction WH than the unpermeated positive electrode plate 13 and the positive electrode portion 13P. Moreover, the negative electrode portion 14N is arranged so as to cover the entire positive electrode portion 13P in the width direction WH, that is, so that the negative electrode active material layer 14A facing the positive electrode active material layer 13A exists at any part of the positive electrode active material layer 13A. In addition, the unpermeated separator 15 is slightly wider in the width direction WH than the negative electrode portion 14N and the positive electrode portion 13P. Moreover, the unpermeated separator 15 is arranged so as to cover the entire width direction WH of the negative electrode portion 14N and the positive electrode portion 13P, i.e., so that the unpermeated separator 15 covering the positive electrode active material layer 13A and the negative electrode active material layer 14A is present in every portion of the positive electrode active material layer 13A and the negative electrode active material layer 14A.
[0031] When the unpermeated electrode body 12 is connected to the positive electrode terminal 8P and the negative electrode terminal 8N and housed in the case 7, and the electrolyte 6 is poured into the case 7, the electrolyte 6 permeates from the outside XHO in the axial direction XH of the unpermeated electrode body 12, i.e., from one side XH1 and the other side XH2, toward the inside of the unpermeated electrode body 12. Specifically, the electrolyte 6 permeates along the unpermeated positive electrode plate 13, the unpermeated negative electrode plate 14, and the unpermeated separator 15 from one side WH1 and the other side WH2 (upper and lower in FIG. 4) in the width direction WH that coincides with the axial direction XH, respectively, toward the center line ML of the width direction WH of the negative electrode active material layer 14A, i.e., toward the inner side WHI of the width direction WH.
[0032] However, as described above, when the electrolyte solution 6 permeates into the unpermeated electrode body 12, the ethylene carbonate 6VE, among the components of the organic solvent 6V, has a slower permeation speed than the other solvents 6VL (in this embodiment, DMC and EMC, which have a lower melting point than EC). For this reason, when considering the distance EL from both end edges 14AE1, 14AE2 in the width direction WH of the negative electrode active material layer 14A of the unpermeated negative electrode plate 14 as the starting point toward the inner side WHI in the width direction WH, it is considered that the concentration of ethylene carbonate 6VE in the electrolyte solution at the leading portion of the electrolyte solution 6 permeating toward the inner side WHI decreases as the distance EL increases. For this reason, when the electrolyte solution 6 has permeated up to the center line ML of the width direction WH of the negative electrode active material layer 14A, shown by a dotted line in Figure 4, and the permeation of the electrolyte solution 6 has been completed throughout the unpermeated electrode body 12, resulting in an electrode body 2 impregnated with the electrolyte solution 6 (for example, when the waiting time TT from the start of injection to the completion of permeation of the electrolyte solution 6 has elapsed), it is considered that the concentration of ethylene carbonate 6VE in the permeated electrolyte solution 6 located near the center line ML is relatively lower than that of the electrolyte solution 6 located outside (upper or lower in Figure 4) in the width direction WH rather than near the center line ML.
[0033] Here, the electrolyte 6 that permeates (advances) to the inner side WHI in the width direction WH along the negative electrode active material layer 14A has been described. However, the electrolyte 6 that permeates (advances) to the inner side WHI in the width direction WH along the positive electrode active material layer 13A of the non-permeated positive electrode plate 13 and the non-permeated separator 15 also causes non-uniformity in the concentration of ethylene carbonate 6VE in the electrolyte 6 due to differences in permeation speed. That is, when the electrolyte 6 is poured into the case 7 and permeates into the non-permeated electrode body 12, the amount of ethylene carbonate 6VE that reaches the vicinity of the center 2M in the axial direction XH of the electrode body 2 (see FIG. 3) impregnated with the electrolyte 6 tends to be small.
[0034] In particular, in the case where the electrode body 2 (unpermeated electrode body 12) has a width dimension AW of the negative electrode active material layers 4A and 14A of 180 mm or more (in the present embodiment, the width dimension AW=180 mm), the electrolyte solution 6 that has permeated from both ends 14AE1 and 14AE2 in the width direction WH of the negative electrode active material layer 14A must permeate (move) a distance EL of 90 mm or more along the negative electrode active material layer 14A before reaching the center line ML. Therefore, due to the difference in permeation speed with other solvents 6VL, the concentration of ethylene carbonate 6VE in the electrolyte solution 6 located near the center line ML becomes low, and the area density of ethylene carbonate 6VE present near the center line ML also becomes low.
[0035] In addition, when the electrolyte 6 permeated from both ends 14AE1, 14AE2 of the negative electrode active material layer 14A toward the inner side WHI reaches the vicinity of the center line ML and meets with each other, the electrolyte 6 does not move to the inner side WHI in the width direction WH by permeation thereafter. Therefore, it is considered that the unevenness in the concentration of the ethylene carbonate 6VE occurring between the electrolyte 6 located near the center line ML and the electrolyte 6 located outside (upper or lower in FIG. 4) in the width direction WH among the permeated electrolyte 6 is gradually eliminated by diffusion movement due to the concentration gradient of the ethylene carbonate 6VE. However, it is estimated that it takes longer to eliminate the unevenness in the concentration than the movement of the electrolyte 6 by permeation (for example, several days). For this reason, it is difficult to wait for a long time from the time when the electrolyte 6 has completely permeated the entire electrode body 2 until the unevenness in the concentration is eliminated before moving to the initial charge.
[0036] Therefore, if initial charging of the battery 1 is started immediately after the waiting time TT has elapsed until the electrolyte 6 has completely permeated the case 7, the initial charging will be performed in a state in which the concentration of ethylene carbonate 6VE in the electrode body 2 is uneven.
[0037] However, as described above, the ethylene carbonate 6VE contained in the electrolytic solution 6 serves as a raw material for forming the anode SEI coating 4AC around the anode active material particles 4AP constituting the anode active material layer 4A. For this reason, as described above, when the area density of the ethylene carbonate 6VE present in the vicinity of the center line ML of the anode active material layer 4A is low, the anode SEI coating 4AC derived from ethylene carbonate cannot be appropriately formed around the anode active material particles 4AP in the vicinity of the center line ML of the anode active material layer 4A, and this tends to cause problems such as an increase in the resistance of the battery 1.
[0038] In the battery 1 of this embodiment, as shown in Fig. 4, the negative electrode active material layer 14A of the non-permeated negative electrode plate 14 forming the non-permeated electrode body 12 is formed such that the central portion 14AM in the width direction WH, where the distance EL from both ends 14AE1, 14AE2 is equal to or greater than the additional portion distance ELF (in this embodiment, the additional portion distance ELF = 80 mm), is a strip-shaped additional negative electrode active material layer 14AF that contains a coating material CS in advance. On the other hand, the one side portion 14AS1 on one side WH1 in the width direction WH and the other side portion 14AS2 on the other side WH2 in the width direction WH are strip-shaped non-containing negative electrode active material layers 14AN1, 14AN2 that do not contain the coating material CS, as in the past. In this embodiment, ethylene carbonate CS1 is used as the coating material CS. This results in an unpermeated electrode body 12 having a coating material CS (ethylene carbonate CS1) that forms a negative electrode SEI coating 4AC on the negative electrode active material layer 4A pre-disposed in a central portion 12M in the axial direction XH.
[0039] To form the negative electrode active material layer 14A of the non-permeated negative electrode plate 14, the negative electrode active material layers 14AN1 and 14AN2 are formed using the same negative electrode paste PAN as before, which does not contain the film-forming material CS, as described later, while the additional negative electrode active material layer 14AF is formed in the central portion 14AM in the width direction WH using the additional negative electrode paste PAF containing the film-forming material CS. In this embodiment, the negative electrode paste PAN is a mixture of 99% by weight of graphite particles and 1% by weight of a binder (CMC) mixed with water as a solvent. The additional negative electrode paste PAF is the above-mentioned negative electrode paste PAN to which 5% by weight of ethylene carbonate CS1 is added as the film-forming material CS.
[0040] In this way, since the additional negative electrode active material layer 14AF is provided in the central portion 14AM of the negative electrode active material layer 14A, when the electrolyte 6 permeating from both ends 14AE1, 14AE2 in the width direction WH of the negative electrode active material layer 14A toward the inside WHI reaches the additional negative electrode active material layer 14AF, the electrolyte 6 further permeates toward the center line ML while the film-forming substance CS in the additional negative electrode active material layer 14AF is dissolved in the electrolyte 6. Therefore, even in the electrode body 2 in which the electrolyte 6 has completely permeated, the concentration of ethylene carbonate 6VE derived from the electrolyte 6 is reduced in the electrolyte 6 located near the center line ML of the negative electrode active material layer 14A, i.e., in the central portion 14AM. However, the electrolyte 6 in the central portion 14AM contains the film-forming substance CS (ethylene carbonate CS1) in the additional negative electrode active material layer 14AF.
[0041] Therefore, even if the initial charging step is performed in a state in which ethylene carbonate 6VE derived from the electrolyte 6 has not sufficiently reached the central portion 14AM as described above, the pre-deposited coating material CS can adequately form the anode SEI coating 4AC on the anode active material particles 4AP (see FIG. 2). Thus, it is possible to manufacture a battery 1 in which the non-uniformity of the formation of the anode SEI coating in the anode active material layer 4A is suppressed, the non-uniformity of the resistance of the anode active material layer 4A in the electrode body 2 is suppressed, and an increase in resistance is suppressed.
[0042] Particularly in this embodiment, ethylene carbonate CS1 is used as the film-forming substance CS. That is, ethylene carbonate CS1 is disposed in advance as the film-forming substance CS in the central portion 14AM of the negative electrode active material layer 14A where the ethylene carbonate 6VE derived from the electrolytic solution 6 is insufficient. Therefore, a negative electrode SEI film derived from ethylene carbonate can be appropriately formed over the entire negative electrode active material layer 4A without causing a shortage of ethylene carbonate in each portion of the negative electrode active material layer 4A.
[0043] Next, the manufacture of this battery 1 will be described with reference to Fig. 5 to Fig. 7. First, in an electrode body forming step S1, a wound-type unpermeated electrode body 12 is formed that is not permeated with the electrolytic solution 6. More specifically, in an unpermeated negative electrode plate forming step S11, an unpermeated negative electrode plate 14 having a strip-shaped negative electrode active material layer 14A is formed.
[0044] More specifically, the central portion 14AM in the width direction WH of the strip-shaped negative electrode active material layer 14A is a strip-shaped additional negative electrode active material layer 14AF containing the coating-forming substance CS, while one side portion 14AS1 and the other side portion 14AS2 of the strip-shaped non-containing negative electrode active material layer 14AN1 and 14AN2 not containing the coating-forming substance CS are formed in the strip-shaped negative electrode active material layer 14A (see FIG. 4). As described above, in this embodiment, ethylene carbonate CS1 is used as the coating-forming substance CS.
[0045] In this unpermeated negative electrode plate formation step S11, the negative electrode active material-free layers 14AN1 and 14AN2 are formed using the negative electrode paste PAN that contains the negative electrode active material particles 14AP and a binder but does not contain the film-forming material CS, while the additional negative electrode paste PAF that contains the negative electrode active material particles 4AP and the film-forming material CS is used to form the additional negative electrode active material layer 14AF.
[0046] Specifically, in the coating step S111, as shown in Fig. 6, a wide negative electrode paste layer 24AT is coated on a wide negative electrode foil 24F wound around a backup roll BR1 and having a width twice that of the negative electrode foil 4F of the negative electrode plate 4, using a die coater DC. More specifically, in the die coater DC, the uncontaining negative electrode paste PAN is stored in a storage tank DCT1, and the additional negative electrode paste PAF is stored in a storage tank DCT2. Using a die DCD provided with a plurality of partitions (not shown), the uncontaining negative electrode paste PAN supplied from the storage tank DCT1 and the additional negative electrode paste PAF supplied from the storage tank DCT2 are discharged in a stripe shape from a slit DCS of the die DCD, and coated on the wide negative electrode foil 24F wound around the backup roll BR1 (see Fig. 7). Specifically, a wide negative electrode paste layer 24AT having a width twice that of the negative electrode foil 14F is applied to both sides of the wide negative electrode foil 24F, leaving a portion to be the current collector 14S of the non-permeated negative electrode plate 14. The wide negative electrode paste layer 24AT is formed symmetrically with respect to the cutting center line CL shown by the dashed line in FIG. 7, and is applied in a five-stripe pattern in which two additional negative electrode paste layers 24ATF are interposed between three non-containing negative electrode paste layers 24ATN. The non-containing negative electrode paste layer 24ATN becomes the non-containing negative electrode active material layers 14AN1 and 14AN2 of the negative electrode active material layer 14A after drying and cutting as described below. The additional negative electrode paste layer 24ATF becomes the additional negative electrode active material layer 14AF after drying and cutting.
[0047] Thereafter, in a drying step S112, the wide negative electrode paste layer 24AT applied to the wide negative electrode foil 24F is dried in a drying oven DR to form a wide negative electrode active material layer 24A. The application step S111 and the drying step S112 are repeated for the front and back sides of the wide negative electrode foil 24F to form a wide unpermeated negative electrode plate 24 in which the wide negative electrode active material layer 24A is provided on both sides of the wide negative electrode foil 24F. FIG. 6 shows the application and drying of the wide negative electrode paste layer 24AT to a wide single-sided negative electrode plate 24S in which the wide negative electrode active material layer 24A is provided on one side of the wide negative electrode foil 24F.
[0048] Furthermore, in a cutting step S113, the wide unpermeated negative electrode plate 24 having the wide negative electrode active material layer 24A provided on both sides of the wide negative electrode foil 24F is cut along a cutting center line CL (see FIG. 7) to form two strip-shaped unpermeated negative electrode plates 14. Thereafter, the unpermeated negative electrode plates 14 are sorted by a sorting roll FR and wound up on winding rolls SR1 and SR2, respectively. Thus, the unpermeated negative electrode plate forming step S11 obtains the unpermeated negative electrode plate 14 (see FIG. 4).
[0049] Next, in a winding step S12, the unpermeated negative electrode plate 14 is wound together with a separately formed unpermeated positive electrode plate 13 and an unpermeated separator 15 to form a cylindrical wound-type electrode body (not shown). Furthermore, in a flattening step S13, this cylindrical electrode body is pressed to form a plate-like flat wound-type unpermeated electrode body 12 (see FIG. 3). Thus, the unpermeated electrode body 12 is obtained by the electrode body forming step S1.
[0050] Thereafter, in the accommodation step S2, the unpermeated electrode body 12 is accommodated in the case 7. Specifically, first, in a terminal connection step S21, the positive electrode current collector 12P of the unpermeated electrode body 12 is welded to the inside connection portion 8PI of the positive electrode terminal 8P fixed to the lid body 7L via the insulating member 9, and similarly, the positive electrode current collector 12P is welded to the inside connection portion 8NI of the negative electrode terminal 8N, respectively, to fix the unpermeated electrode body 12 to the lid body 7L via the positive electrode terminal 8P and the negative electrode terminal 8N (see FIG. 1).
[0051] In the subsequent insertion step S22, a bag-shaped resin cover (not shown) made of a resin film is placed over the unpermeated electrode body 12, and the unpermeated electrode body 12 is inserted into the case body 7H, and the case body 7H is sealed with the lid body 7L. Furthermore, in a sealing step S23, the periphery of the lid body 7L is hermetically welded and sealed to the case body 7H by laser welding all around. Thus, the unpermeated electrode body 12 is accommodated in the case 7 by the accommodation step S2.
[0052] Thereafter, in the liquid injection step S3, a predetermined amount of electrolyte 6 is injected into the case 7 through the liquid injection hole 7LH of the lid 7L. As a result, as described above, the electrolyte 6 is impregnated into the unpermeated electrode body 12 in the case 7. Note that in the liquid injection step S3, the electrolyte 6 is injected in a predetermined injection pattern. Furthermore, prior to the injection, the unpermeated battery 1 may be placed in a chamber and the pressure may be reduced or pressurized while the electrolyte 6 is impregnated into the unpermeated electrode body 12.
[0053] In the waiting step S4, it is waited until a predetermined waiting time TT has elapsed from the start of the injection. The waiting time TT is the time from the start of the injection until the electrolyte 6 has permeated the entire inside of the unpermeated electrode body 12 (until the electrode body 2 is impregnated with the electrolyte 6), and this waiting time TT is obtained in advance by disassembling battery samples with different elapsed times from the start of the injection and observing the permeation state of the electrolyte 6, for example.
[0054] After the waiting time TT has elapsed, the process proceeds to an initial charging step S5, in which a power source (not shown) is connected to the positive electrode terminal 8P and the negative electrode terminal 8N, and a voltage is applied to the electrode body 2 of the battery 1 through the positive electrode terminal 8P and the negative electrode terminal 8N to perform initial charging. That is, a voltage is applied between the positive electrode plate 3 and the negative electrode plate 4 of the electrode body 2 in a predetermined initial charging pattern, and a negative electrode SEI coating 4AC is formed on the negative electrode active material layer 4A of the negative electrode plate 4 (see FIG. 2). In this embodiment, initial charging is performed in an initial charging pattern of 0.5C-CCCV charging (SOC 90%). Thereafter, the liquid injection hole 7LH is sealed with a liquid injection plug 7LP.
[0055] As described above, in the battery 1 of this embodiment, the additional negative electrode active material layer 14AF is provided in the central portion 14AM of the negative electrode active material layer 14A of the unpermeated negative electrode plate 14 of the unpermeated electrode body 12. Therefore, in the electrode body 2 in which the waiting time TT has elapsed and the electrolyte 6 has permeated the entire unpermeated electrode body 12, it is possible to prevent a decrease in the area density of ethylene carbonate present near the center line ML of the negative electrode active material layer 4A of the negative electrode plate 4. Therefore, in the initial charging step S5, the negative electrode SEI coating 4AC can be appropriately formed on the negative electrode active material particles 4AP at any location of the negative electrode active material layer 4A.
[0056] Next, in a high-temperature aging step S6, the battery 1 is subjected to high-temperature aging by being left in an environment of 60° C. for 20 hours, and in an inspection step S7, the battery 1 is inspected, and the battery 1 is completed.
[0057] (Comparative forms 1 and 2) To compare with the battery 1 according to the embodiment, batteries 1C1 and 1C2 according to comparative embodiments 1 and 2 were also manufactured and examined as described below. First, the manufacture of the batteries 1C1 and 1C2 according to comparative embodiments 1 and 2 will be described with reference to FIGS.
[0058] The battery 1C1 according to the comparative embodiment 1 is a battery similar to the conventional battery. In the battery 1 of the embodiment, the non-permeated electrode body 12 was formed using the non-permeated negative electrode plate 14 in which the additional negative electrode active material layer 14AF was provided in the central portion 14AM of the negative electrode active material layer 14A, and the electrolyte 6 was impregnated. In contrast, in the battery 1C1 of the comparative embodiment 1, as shown in FIG. 8, the additional negative electrode active material layer 14AF was not provided in the negative electrode active material layer 14A, and the entire negative electrode active material layer 14A was made into the non-permeated negative electrode plate 14C1 in which the non-containing negative electrode active material layer 14AN that does not contain the coating material CS was formed. Then, the non-permeated electrode body 12C1 was formed using this non-permeated negative electrode plate 14C1. The rest was the same as the battery 1 of the embodiment 1, and the initial charging step S5 and the high-temperature aging step S6 were also performed in the same manner to obtain the battery 1C1 of the comparative embodiment 1.
[0059] On the other hand, the battery 1C2 according to the comparative embodiment 2 is a battery opposite to the non-permeated negative electrode plate 14C1 of the battery 1C1 of the comparative embodiment 1. That is, as shown in FIG. 9, the non-permeated negative electrode plate 14C2 was formed in which the negative electrode active material layer 14A was not provided with a non-containing negative electrode active material layer 14AN that did not contain a film-forming material CS, and the entire negative electrode active material layer 14A was made into an additional negative electrode active material layer 14AF that contained a film-forming material CS (ethylene carbonate CS1), and the non-permeated negative electrode plate 14C2 was used to form the non-permeated electrode body 12C2. The rest was the same as the battery 1 of the embodiment 1, and the initial charging step S5 and the high-temperature aging step S6 were also performed in the same manner to obtain the battery 1C2 of the comparative embodiment 2.
[0060] (Ethylene carbonate content survey) The manufactured batteries 1, 1C1, and 1C2 are disassembled in a glove box with an inert atmosphere, and the electrode bodies 2, 2C1, and 2C2 are taken out. Furthermore, the electrode bodies 2, 2C1, and 2C2 are unwound, and the negative electrode plate 4 is taken out and left to dry. The middle part of the winding (approximately the center in the longitudinal direction LH) of each negative electrode plate 4, and the parts corresponding to the positions shown by the inspection positions I, II, III, IV, and V in FIG. 10, are cut out to a size of 20 x 20 mm to obtain a total of 15 types of negative electrode samples for extraction. Each negative electrode sample for extraction is immersed in an extraction solvent to extract ethylene carbonate, and NMR measurements are performed on a standard solution with a known ethylene carbonate concentration and each extraction solution, and the content of ethylene carbonate contained in each extraction solution is calculated from the ratio of the detection intensity of ethylene carbonate in the standard solution and the extraction solution. Furthermore, in each of the electrode assemblies 2, 2C1, and 2C2, the ethylene carbonate content obtained at the inspection position I was defined as 100%, and the relative EC content (%) at each of the inspection positions I to V was obtained.
[0061] As shown in FIG. 10, the inspection positions I, II, III, IV, and V are flat plate-shaped portions of the negative electrode active material layer 4A of the negative electrode plate 4 in each electrode body 2, 2C1, and 2C2, and are arranged in the axial direction XH. The distances EL measured from the edge 4AE2 (see FIG. 4) of the current collector 4S side that becomes the negative electrode current collector 2N to the inner side XHI in the axial direction XH (inner side WHI in the width direction WH) are the distances EL1, EL2, EL3, EL4, and EL5, respectively (in the present embodiment, specifically, EL1=10 mm, EL2=30 mm, EL3=50 mm, EL4=70 mm, and EL5=90 mm). The inspection position V is a position on the center line ML of the negative electrode active material layer 4A. That is, the distance EL5 is 1 / 2 the width dimension AW (AW=180 mm in the present embodiment, etc.) of the negative electrode active material layer 4A in the width direction WH.
[0062] The results are shown in the graph of Figure 11. In the electrode body 2C1 of the battery 1C1 of Comparative Form 1, indicated by the thick dashed line, the content of ethylene carbonate 6VE gradually decreases from inspection position I to inspection position IV, i.e., from the edge 4AE2 to the inner side XHI in the axial direction XH. However, at inspection position V, i.e., at the central portion 2M in the axial direction XH of the electrode body 2C1 (see Figure 3), the content of ethylene carbonate 6VE is significantly reduced (in this Comparative Form 1, the content is reduced by approximately 30% compared to inspection position I).
[0063] This is believed to be due to the following reasons. As described above, the permeation speed of the ethylene carbonate 6VE contained in the electrolyte 6 is slower than that of other solvents 6VL (specifically, DMC, EMC). For this reason, it is believed that the greater the distance EL from the end edge 4AE2 to the inspection position V, the lower the concentration of the ethylene carbonate 6VE in the electrolyte 6 located at the tip of the permeation, among the electrolyte 6 permeating into the electrode body 2C1. In particular, when the distance EL exceeds 80 mm, the concentration of the ethylene carbonate 6VE decreases significantly. Moreover, in the vicinity of the inspection position V located on the center line ML of the negative electrode active material layer 4A, that is, in the central portion 2M of the electrode body 2C1, the electrolyte 6 that permeates from both end edges 4AE1, 4AE2 (see FIG. 8) of the negative electrode active material layer 4A to the inner side WHI in the width direction WH (the inner side XHI in the axial direction XH) meets and stops permeating, so that the content (area density) of the ethylene carbonate 6VE that reaches the central portion 2M tends to remain low.
[0064] On the other hand, in the electrode body 2C2 of the battery 1C2 of Comparative Form 2, indicated by a thick dashed dotted line, the ethylene carbonate content is maintained at a high value of nearly 100% from inspection position I to inspection position IV. In particular, the ethylene carbonate content is slightly higher at inspection positions II and III than at inspection position I near the edge 4AE2 of the outer side WHO in the width direction WH. However, at inspection position IV, the ethylene carbonate content is slightly reduced. However, at inspection position V, i.e., at the central portion 2M in the axial direction XH of the electrode body 2C1 (see FIG. 9), it is found that the ethylene carbonate content is significantly reduced (approximately 35% reduced compared to inspection position I in Comparative Form 2).
[0065] This is believed to be due to the following reason. The electrode body 2C2 of the battery 1C2 of Comparative Form 2 uses an unpermeated negative electrode plate 14C2 in which the entire negative electrode active material layer 14A is made of an additional negative electrode active material layer 14AF containing a coating-forming material CS (specifically, ethylene carbonate CS1). For this reason, in the range from the investigation positions I to III where the distance EL from the edge 4AE2 is relatively small, the decrease in concentration due to the slow permeation speed of ethylene carbonate 6VE contained in the electrolyte solution 6 (see the graph of Comparative Form 1) is compensated for by the dissolution of ethylene carbonate CS1 derived from the additional negative electrode active material layer 14AF in the electrolyte solution 6, and rather the concentration of ethylene carbonate increases with the permeation of the electrolyte solution 6.
[0066] However, as described above, the ethylene carbonate dissolved in the electrolyte solution 6 has a slower permeation rate and a higher viscosity than other solvents 6VL (specifically, DMC and EMC). Therefore, when the concentration of ethylene carbonate dissolved in the electrolyte solution 6 increases near the investigation positions II and III, the increase in viscosity causes the permeation rate of the ethylene carbonate to decrease rapidly, and the concentration of ethylene carbonate in the electrolyte solution 6 reaching the investigation position V decreases significantly. Therefore, even if the ethylene carbonate CS1 derived from the additional negative electrode active material layer 14AF near the investigation position V compensates, it is presumed that it cannot fully compensate for the large decrease in the ethylene carbonate content at the investigation position V, i.e., the central portion 2M.
[0067] In contrast, in the battery 1 (electrode body 2) of this embodiment shown by the thick solid line, the ethylene carbonate content gradually decreases at the inspection positions I to IV, generally similar to the battery 1C1 of Comparative Form 1, from inspection position I to inspection position IV, i.e., from the edge 4AE2 to the inner side XHI in the axial direction XH. However, unlike the battery 1C1 of Comparative Form 1, the ethylene carbonate content at inspection position V in the battery 1 of this embodiment is approximately the same as that at inspection position IV. That is, in the electrode body 2 of the battery 1 of this embodiment, the decrease in the ethylene carbonate content at the central portion 2M in the axial direction XH (see FIG. 3) is suppressed. Specifically, in this embodiment, the decrease in the content at inspection position V compared to inspection position I remains approximately 10% or less.
[0068] This is believed to be due to the following reason. In the electrode body 2 of the battery 1 of this embodiment, an unpermeated negative electrode plate 14 is used in which an additional negative electrode active material layer 14AF containing a film-forming substance CS (specifically, ethylene carbonate CS1) is formed only in a central portion 14AM of the negative electrode active material layer 14A, the central portion being at a distance EL of 80 mm or more including the inspection position V (see FIG. 4). For this reason, in the range from the inspection positions I to IV, it is believed that the decrease in concentration occurred due to the slow permeation speed of ethylene carbonate 6VE derived from the electrolyte solution 6, as in Comparative Form 1.
[0069] However, as described above, when the permeated electrolyte solution 6 reaches the additional negative electrode active material layer 14AF in the central portion 14AM of the negative electrode active material layer 14A, the ethylene carbonate CS1 originating from the additional negative electrode active material layer 14AF dissolves in and replenishes the electrolyte solution 6. This is thought to have allowed the ethylene carbonate content at the investigation position V to be kept at the same level as at the investigation position IV.
[0070] (P content survey) In order to investigate the origin of the negative electrode SEI coating 4AC formed on the negative electrode active material layer 4A of the batteries 1, 1C1, and 1C2, the amount of P MP contained in the negative electrode SEI coating 4AC was also investigated. Specifically, the negative electrode plates 4 taken out of the electrode bodies 2, 2C1, and 2C2 investigated by the above-mentioned ethylene carbonate content were cut out in the middle of the winding and in the areas corresponding to the investigation positions I, III, and V in FIG. 10 (the end 4AE, the middle part 4AM, and the center part 4AT of the negative electrode active material layer 4A) to a size of 20×20 mm to obtain a total of nine types of negative electrode samples for measuring the amount of P. Each sample was washed with EMC to remove the electrolyte 6 and then dried. Thereafter, each sample was put into an extraction solution and subjected to an acid treatment or the like, and the negative electrode active material layer 4A of each sample was subjected to an ICP-MS analysis, and the amount of P contained in the negative electrode active material layer 4A, i.e., the negative electrode SEI coating 4AC, was calculated. Furthermore, for each electrode body 2, 2C1, 2C2, the end P amount MPE obtained at investigation position I (end 4AE) was set to 100%, and the relative middle P amount MPM (%) and central P amount MPT (%) at each investigation position III, V (middle portion 4AM, central portion 4AT) were obtained.
[0071] The results are shown in the graph of Figure 12. In the electrode body 2C1 of the battery 1C1 of Comparative Form 1, indicated by the thick dashed line, it can be seen that the P amount gradually increases generally from inspection position I to inspection position V, that is, from the edge 4AE2 to the inner side XHI in the axial direction XH. Specifically, it can be seen that the middle portion P amount MPM corresponding to inspection position III (middle portion 4AM) is increased by about 2% compared to the end portion P amount MPE corresponding to inspection position I (end portion 4AE). It can also be seen that the center portion P amount MPT corresponding to inspection position V (center portion 2M in the axial direction XH of the electrode body 2C1 (see Figure 3)) is increased by about 8% compared to the end portion P amount MPE.
[0072] Considering this result together with the result of FIG. 11 described above, in the battery 1C1 of Comparative Example 1, when the initial charging step S5 was performed, the electrolyte 6 reached the center portion 2M of the electrode body 2C1, but it is considered that the area density of the ethylene carbonate 6VE was significantly reduced in the center portion 2M. For this reason, in the vicinity of the investigation position III (middle portion 4AM), similar to the investigation position I (end portion 4AE), it is considered that the generation of the negative electrode SEI coating 4AC derived from EC was sufficiently generated, and the negative electrode SEI coating derived from the supporting salt 6S (LiPF6 in this embodiment) containing P contained in the electrolyte 6 and therefore containing P was also generated to the same extent. However, in the center portion 2M of the electrode body 2C1, the generation of the negative electrode SEI coating 4AC derived from EC was not sufficient. However, instead, it is considered that the negative electrode SEI coating derived from the supporting salt 6S and containing P was excessively generated, so that the central portion P amount MPT increased compared to the end portion P amount MPE.
[0073] On the other hand, in the electrode body 2C2 of the battery 1C2 of comparative form 2 indicated by a thick dotted line, it can be seen that, contrary to the battery 1C1 of comparative form 1, the P amount decreases from the inspection position I toward the inspection position V, that is, from the edge 4AE2 toward the inner side XHI in the axial direction XH. Specifically, it can be seen that, compared to the end portion P amount MPE corresponding to inspection position I, the middle portion P amount MPM corresponding to inspection position III (middle portion 4AM) is reduced by approximately 4%, and the central portion P amount MPT corresponding to inspection position V (central portion 2M of the electrode body 2C2) is reduced by approximately 16%.
[0074] Considering this result together with the result of Fig. 11 described above, in the battery 1C2 of Comparative Form 2, when the initial charging step S5 was performed, the area density of ethylene carbonate dissolved in the electrolyte 6 was slightly higher near the investigation position III, and the generation of the negative electrode SEI coating 4AC derived from EC was sufficiently generated near the investigation position III (middle portion 4AM) similar to or greater than that at the investigation position I (end portion 4AE). Instead, it is considered that the generation of the negative electrode SEI coating derived from the supporting electrolyte 6S and containing P was somewhat suppressed.
[0075] However, as described above, due to the high viscosity of ethylene carbonate, not only the permeation rate of ethylene carbonate decreases, but also the permeation rate of the electrolyte 6 decreases. For this reason, it is presumed that the amount of electrolyte 6 reaching the inspection position V (center portion 4AT) also decreased. In other words, it is presumed that the electrolyte 6 did not reach the center portion 2M of the electrode body 2C2 sufficiently in the first place. For this reason, in the center portion 2M (inspection position V) of the electrode body 2C2, the negative electrode SEI coating 4AC derived from EC could not be sufficiently formed. In addition, the negative electrode SEI coating derived from the supporting salt 6S and containing P could not be sufficiently formed. For this reason, it is presumed that the central portion P amount MPT was greatly reduced compared to the end portion P amount MPE.
[0076] In contrast, in the electrode body 2 of the battery 1 of this embodiment shown by the thick solid line, the middle portion P amount MPM corresponding to the inspection position III is almost the same (about 1% increase) as the end portion P amount MPE corresponding to the inspection position I. On the other hand, the central portion P amount MPT corresponding to the inspection position V is about 6% smaller than the end portion P amount MPE.
[0077] Considering this result together with the result of FIG. 11 described above, the battery 1 of the embodiment uses an unpermeated negative electrode plate 14 in which the additional negative electrode active material layer 14AF is formed only on the central portion 14AM of the negative electrode active material layer 14A as described above (see FIG. 4). Therefore, when the initial charging step S5 is performed, the electrolyte 6 reaches the central portion 2M of the electrode body 2. In the vicinity of the investigation position III (middle portion 4AM), similarly to the investigation position I (end portion 4AE), the generation of the negative electrode SEI coating derived from EC in the negative electrode SEI coating 4AC is sufficiently generated, and it is considered that the negative electrode SEI coating derived from the supporting salt 6S (LiPF6 in this embodiment) containing P contained in the electrolyte 6 and therefore containing P is also generated to the same extent. Moreover, the decrease in the concentration of EC in the central portion 2M (investigation position V) was suppressed by the supplementation of ethylene carbonate CS1 derived from the additional negative electrode active material layer 14AF. For this reason, in the central portion 2M of the electrode body 2C2, the negative electrode SEI coating 4AC derived from EC was sufficiently formed, which suppressed the formation of the negative electrode SEI coating derived from the supporting electrolyte 6S and containing P. For this reason, it is estimated that the central portion P amount MPT was reduced by about 6% compared to the end portion P amount MPE.
[0078] (IV resistance value survey) In order to study the influence of the difference in the concentration of ethylene carbonate and the difference in the amount of P on the battery characteristics, the following investigations were also carried out. The manufactured batteries 1, 1C1, and 1C2 were charged to SOC 50%, disassembled in a glove box under an inert atmosphere, and the electrode bodies 2, 2C1, and 2C2 were taken out. Furthermore, the electrode bodies 2, 2C1, and 2C2 were unwound, and the positive electrode plate, the negative electrode plate facing it, and the separator sandwiched between them were cut out in the middle of the winding and in the areas corresponding to the investigation positions I, III, and V in FIG. 10, each with a size of 20×20 mm, to obtain a total of nine types of small cell samples consisting of a small positive electrode plate, a small negative electrode plate, and a small separator. These were washed and dried with EMC, stacked with a small separator sandwiched between the small positive electrode plate and the small negative electrode plate, surrounded by a laminate film, and new electrolyte 6 was poured in and sealed to form a new small cell (not shown).
[0079] For the small cells (total of nine types) corresponding to the investigation positions I, III, and V of each electrode body 2, 2C1, and 2C2, constant current discharge was performed with current A at a magnitude equivalent to discharge current rates of 0.2C, 0.5C, 1C, and 2C in an environment of 25°C, and the voltage drop ΔV was obtained after 10 seconds. The obtained data was plotted on a graph with current A on the X-axis and voltage drop ΔV on the Y-axis, and the slope of the approximated straight line was taken as the IV resistance value of each small cell (IV resistance = voltage drop ΔV / current A). Furthermore, for each form, the relative IV resistance value of the small cells at each investigation position I, III, and V was obtained, with the IV resistance value obtained for the small cell at investigation position I set to 100%.
[0080] The results are shown in the graph of Figure 13. Among the small cells of electrode body 2C1 of battery 1C1 of comparative form 1, indicated by the thick dashed line, the small cells at inspection positions I and III had almost the same relative IV resistance value. However, it can be seen that the small cell at inspection position V had a significantly increased relative IV resistance value compared to the small cells at inspection positions I and III (in comparative form 1, an increase of approximately 18% compared to inspection position I).
[0081] This is believed to be due to the following reasons. As described above, the ethylene carbonate content does not change much at the check positions I to III in the electrode body 2C1 of the battery 1C1 of Comparative Form 1 (see FIG. 11). Specifically, the ethylene carbonate content at check positions II and III is reduced by at most about -7% compared to check position I. The middle P content MPM at check position III also hardly increases compared to the end P content MPE at check position I (see FIG. 12). When the battery 1C1 of Comparative Form 1 is initially charged in the initial charge step S5, an ethylene carbonate-derived anode SEI coating is appropriately formed as an anode SEI coating 4AC on the anode active material particles 4AP in the anode active material layer 4A of the anode plate 4 near the check positions I and III. Therefore, an anode SEI coating derived from the supporting salt 6S is also formed to the same extent near the check positions I and III. Thus, it is considered that the relative IV resistance values of the small cells using small positive plates, small negative plates, and small separators at investigation positions I and III were comparable to each other.
[0082] However, as described above, the content of ethylene carbonate was significantly decreased (-28% decrease) at the survey position V of the electrode body 2C1 (see FIG. 11). Therefore, in the negative electrode active material layer 4A of the negative electrode plate 4 after the initial charge, near the survey position V, i.e., near the center line ML (see FIG. 10), the negative electrode SEI film 4AC derived from ethylene carbonate was not sufficiently formed as the negative electrode SEI film 4AC on the negative electrode active material particles 4AP, and instead, a large amount of negative electrode SEI film derived from the supporting salt 6S containing P with a relatively high resistance was generated. Therefore, it is considered that the relative IV resistance value was 18% higher in the small cell using the small positive electrode plate, small negative electrode plate, and small separator at the survey position V than in the small cell at the survey position I. This is also consistent with the fact that the central P amount MPT at the survey position V increased by about 8% compared to the end P amount MPE at the survey position I (see FIG. 12). This shows that in the electrode body 2C1 of the battery 1C1 of Comparative Form 1, the IV resistance value is locally high at the center portion 2M, and the IV resistance value is also high throughout the electrode body 2C1.
[0083] In the electrode body 2C2 of the battery 1C2 of Comparative Form 2 shown by the thick dashed dotted line, the small cells at the inspection positions I and III had almost the same relative IV resistance values. However, it can be seen that the small cell at the inspection position V had a significantly increased relative IV resistance value compared to the small cells at the inspection positions I and III (in Comparative Form 2, an increase of approximately 24% compared to inspection position I).
[0084] This is believed to be due to the following reasons. As described above, the content of ethylene carbonate contained in the electrolyte 6 hardly changes at the check positions I to III in the electrode body 2C2 of the battery 1C2 of the comparative embodiment 2 (see FIG. 11). Therefore, when the battery 1C2 of the comparative embodiment 2 is initially charged in the initial charge step S5, the negative electrode SEI coating 4AC derived from ethylene carbonate is appropriately formed on the negative electrode active material particles 4AP in the negative electrode active material layer 4A of the negative electrode plate 4 near the check positions I and III. Accordingly, the formation of the negative electrode SEI coating derived from the supporting salt 6S is suppressed near the check position III. Therefore, it is believed that the middle part P amount MPM at the check position III is reduced by about 4% compared to the end part P amount MPE at the check position I (see FIG. 12). And, as a result, it is believed that the relative IV resistance values became approximately the same in the small cells using the small positive electrode plate, small negative electrode plate, and small separator at the check positions I and III.
[0085] However, as described above, the ethylene carbonate content at the investigation position V of the electrode body 2C2 was greatly decreased (-36% decrease) (see FIG. 11). In addition, the central P amount MPT at the investigation position V was decreased by about 16% compared with the end P amount MPE at the investigation position I (see FIG. 12). Since the electrolyte 6 did not sufficiently reach the central portion 2M of the electrode body 2C2, the negative electrode SEI coating derived from ethylene carbonate could not be sufficiently formed as the negative electrode SEI coating 4AC on the negative electrode active material particles 4AP near the central portion 4AT (investigation position V) of the negative electrode active material layer 4A of the negative electrode plate 4 after the initial charge. In addition, the negative electrode SEI coating derived from the supporting salt 6S could not be sufficiently formed, that is, the negative electrode SEI coating 4AC was not sufficiently formed. As a result, it is considered that the relative IV resistance value of the small cell using the small positive electrode plate, small negative electrode plate, and small separator at the investigation position V was 24% higher than that of the small cell at the investigation position I. This shows that, also in the electrode body 2C2 of the battery 1C2 of Comparative Example 2, the IV resistance value is locally high at the center portion 2M, and the IV resistance value is also high throughout the electrode body 2C2.
[0086] In contrast, in the battery 1 (electrode body 2) of this embodiment indicated by the thick solid line, no significant change occurs in the relative IV resistance value at any of the investigation positions I, III, and V.
[0087] This is believed to be due to the following reasons. As described above, in the electrode body 2 of the battery 1 of this embodiment, the content of ethylene carbonate contained in the electrolyte 6 is not so low not only at the inspection positions II to IV but also at the inspection position V, as compared to the inspection position I. Specifically, the content at the inspection position V is only -9% lower than the inspection position I (see FIG. 11). The middle part P amount MPM at the inspection position III is also almost not increased compared to the end part P amount MPE at the inspection position I. On the other hand, the central part P amount MPT at the inspection position V is reduced by about 6% (see FIG. 12). From these, when the battery 1 of this embodiment is initially charged, the negative electrode SEI coating 4AC derived from ethylene carbonate can be appropriately formed on the negative electrode active material particles 4AP not only near the inspection positions I and III but also near the inspection position V in the negative electrode active material layer 4A of the negative electrode plate 4. Accordingly, the generation of the negative electrode SEI coating derived from the supporting salt 6S is suppressed near the inspection position V. For this reason, it is considered that the relative IV resistance values of the small cells using the small positive electrode plate, small negative electrode plate, and small separator at the inspection positions I, III, and V are approximately the same. From this, it is found that in the electrode body 2 of the battery 1 of this embodiment, the uneven formation of the negative electrode SEI coating in the negative electrode active material layer 4A in the wound type electrode body 2 can be suppressed, the IV resistance value does not become locally high in the central portion 2M, and the increase in the IV resistance value of the electrode body 2 as a whole can be suppressed. In other words, it is found that the battery 1 of this embodiment has a lower IV resistance than the batteries 1C1 and 1C2 of the comparative embodiments 1 and 2.
[0088] As described above, the battery 1 of this embodiment is provided with an electrolyte 6 containing ethylene carbonate 6VE and a supporting salt 6S containing P, and is provided with an electrode body 2 in which the width dimension AW of the negative electrode active material layer 4A is 180 mm or more. Therefore, as shown in Comparative Form 1, uneven penetration of EC is likely to occur, and in the central portion 2M where EC has difficulty reaching, an SEI coating derived from EC is difficult to form, and instead, an SEI coating derived from the supporting salt containing P tends to be formed in excess. However, in the battery 1 of this embodiment, the central P amount MPT of the P amount MP contained in the negative electrode SEI coating 4AC of the negative electrode active material layer 4A is within a range of 90 to 105% (specifically, 94%) of the end P amount MPE. That is, the central P amount MPT is roughly equal to or slightly less than the end P amount MPE. In other words, in this battery 1, even in the central portion 4AT of the negative electrode active material layer 4A, the negative electrode SEI coating derived from the P-containing supporting salt 6S is not excessively formed, and the battery 1 suppresses a local increase in IV resistance occurring in the axial direction XH (width direction WH of the negative electrode plate 4) in the electrode body 2 and suppresses an increase in the resistance of the entire electrode body 2.
[0089] In particular, in the battery 1 of this embodiment, the amount of P in the middle portion MPM is also 96 to 104% (specifically, 101%) of the amount of P in the end portion MPE. That is, in the battery 1, the negative electrode SEI coating 4AC derived from the supporting salt 6S containing P is uniformly formed over the entire battery 1, and the battery 1 suppresses an increase in local IV resistance occurring in the axial direction XH in the electrode body 2 and suppresses an increase in the resistance of the entire electrode body 2.
[0090] Although the present invention has been described above with reference to an embodiment, it goes without saying that the present invention is not limited to the embodiment and can be modified as appropriate without departing from the spirit of the present invention. For example, in the embodiment, a battery 1 was formed using an unpermeated negative electrode plate 14 in which an additional negative electrode active material layer 14AF in which ethylene carbonate CS1 was added as a film-forming substance CS was provided in a central portion 14AM of the negative electrode active material layer 14A. However, instead of ethylene carbonate CS1, vinylene carbonate, LiBOB, or the like may be added as the film-forming substance CS to generate a negative electrode SEI film and suppress excessive generation of the negative electrode SEI film derived from the supporting salt 6S. [Explanation of symbols]
[0091] 1, 1C1, 1C2 battery (energy storage device) 2,2C1,2C2 electrode body 2M central part 3 Positive plate 4 Negative plate 4A negative electrode active material layer 4AE End 4AT central part 4AM Middle Section AW (negative electrode active material layer) width dimension 4AE1,4AE2 (widthwise) edges 4AP negative electrode active material particles 4AC negative electrode SEI coating MP amount MPE end P amount MPT center P amount MPM Middle P amount 6 Electrolyte 6V Organic Solvent 6VE Ethylene Carbonate 6VL Other Solvents 6S supporting salt (supporting salt containing P) 7 Cases 14A Anode active material layer 14AE1, 14AE2 (widthwise) edges ML Centerline 14AM Central part 14AS1 One side part (edge side part) 14AS2 Other side part (edge side part) EL Distance 14AF Additional negative electrode active material layer 14AN1,14AN2,14AN-free negative electrode active material layer 14AP negative electrode active material particles XH Axial direction XHI Inside XHO outside WH width direction WHI Inside
Claims
1. an electrolyte solution including ethylene carbonate, a solvent having a melting point lower than that of ethylene carbonate, and a supporting salt containing P; A wound electrode body having a strip-shaped positive electrode plate, a strip-shaped negative electrode plate having a strip-shaped negative electrode active material layer on which an SEI coating is formed, and a strip-shaped separator, the electrolyte solution permeating into the inside of the wound electrode body; A case that accommodates the electrode body and the electrolyte, The electrode body has a width dimension of the negative electrode active material layer of 180 mm or more. An electricity storage device, The amount of P contained in the SEI coating formed on the negative electrode active material layer is Based on the amount of end P at the end in the width direction of the negative electrode active material layer, The amount of P in the central portion in the width direction is 90 to 105% of the amount of P in the end portion. Energy storage device.
2. The power storage device according to claim 1 , The amount of P in an intermediate portion located midway between the end portion and the central portion in the width direction of the negative electrode active material layer is 96 to 104% of the amount of P in the end portion. Energy storage device.
3. The electricity storage device according to claim 1 or 2, The amount of P is The amount of P obtained by ICP-MS analysis using the negative electrode plate that was removed from the electricity storage device and washed to remove the adhering electrolyte is Energy storage device.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery and manufacturing method thereof
JP2013182712A
Method for manufacturing nonaqueous electrolyte secondary battery
JP2014157748A
Negative electrode for secondary battery and manufacturing method therefor, and secondary battery using the same
JP2015018775A
Lithium ion secondary battery and manufacturing method of the same