Piping materials
High-purity polyethylene resin piping materials with controlled particle and metal content address the issue of impurity elution, ensuring high purity and quality in semiconductor and pharmaceutical applications.
Patent Information
- Application Number
- JP2023045123
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing piping materials for high-purity chemicals and ultrapure water in the semiconductor and pharmaceutical industries suffer from high elution of fine particles such as organic and metal impurities, leading to decreased yield and defects in semiconductor devices.
Development of high-purity polyethylene resin piping materials with stringent specifications to minimize the elution of fine particles and metal impurities, including specific requirements for particle count, molecular weight distribution, and metal content.
The solution effectively suppresses the elution of fine particles and metal impurities, ensuring high purity of chemicals and water, thereby enhancing the yield and quality of semiconductor devices and pharmaceutical products.
Abstract
Description
[Technical field]
[0001] The present invention relates to piping materials such as pipes, joints, valves, etc. that constitute transport lines for high-purity chemicals or ultrapure water used in the semiconductor device industry, precision industrial parts, pharmaceuticals, etc. [Background technology]
[0002] In recent years, with the remarkable development of the electronics industry, the demand for high-purity chemicals or ultrapure water has been increasing. High-purity chemicals are used as indispensable chemicals for the manufacture of electronic circuits such as large-scale integrated LSIs. Specific examples of high-purity chemicals used include sulfuric acid, hydrochloric acid, nitric acid, hydrofluoric acid, ammonium fluoride, hydrogen peroxide, isopropyl alcohol, xylene, TMAH (tetramethylammonium hydroxide), methanol, acetic acid, phosphoric acid, ammonia water, PGMEA (propylene glycol methyl ether acetate), DMSO (dimethyl sulfoxide), and NMP (N-methyl-2-pyrrolidone) for applications such as wafer cleaning and etching, wiring and insulating film etching, jig cleaning, developing solution, resist dilution solution, resist stripping solution, and drying. In addition, in the manufacture of precision devices such as semiconductor devices or liquid crystal display devices, ultrapure water refined to an extremely high purity is also used in wet processes such as cleaning. Since particles such as organic impurities and metal impurities contained in high-purity chemicals or ultrapure water cause a decrease in the yield of semiconductor devices and defects, the demand for reducing the particles has become increasingly strict in recent years. Impurities can also be mixed into the high-purity chemicals or ultrapure water by elution from piping materials such as pipes, joints, and valves that constitute the transport lines of the high-purity chemicals or ultrapure water.
[0003] Generally, fluororesins are chemically inactive and have the characteristic that they release very little impurities into the high-purity chemicals or ultrapure water, and therefore are generally used as piping materials for pipes, joints, valves, and the like that constitute the transport lines of the high-purity chemicals or ultrapure water (see, for example, Patent Document 1). Also, a pipe material for ultrapure water having an HDPE layer containing high-density polyethylene and a fluorine-based lubricant has been proposed (see, for example, Patent Documents 2 and 3). Furthermore, a polyethylene resin composition used for a piping material for ultrapure water has been proposed (see, for example, Patent Document 4).
[0004] The fluororesin piping proposed in Patent Document 1 has problems in that it is difficult to mold fluororesin, resulting in low productivity and low freedom of design, and also has a problem of high cost because fluororesin is more expensive than general resins. Furthermore, the polyethylene resin compositions used in the ultrapure water pipe materials or ultrapure water piping materials proposed in Patent Documents 2 to 4 have low elution of metals into ultrapure water, but there is no description of organic impurities that are the cause of fine particles contained in the high purity chemicals or ultrapure water, or of their quantitative evaluation. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-234576 A [Patent Document 2] JP 2022-159129 A [Patent Document 3] JP 2022-157376 A [Patent Document 4] JP 2022-145138 A Summary of the Invention [Problem to be solved by the invention]
[0006] Therefore, an object of the present invention is to provide piping materials such as piping, joints, valves, etc. made of high-purity polyethylene resin having an extremely low content of particulates such as organic impurities and metallic impurities, and more specifically, to provide piping materials such as piping, joints, valves, etc. that constitute transport lines for high-purity chemicals or ultrapure water used in the semiconductor device industry, precision industrial parts field, and in the production of high-purity chemicals or ultrapure water used in pharmaceuticals, etc. [Means for solving the problem]
[0007] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have discovered that a piping material made of a high-purity polyethylene resin having an extremely low content of fine particles such as organic impurities and metallic impurities can be suitably used in the transport of high-purity chemicals or ultrapure water used in the semiconductor device industry, precision industrial parts field, and pharmaceuticals, etc., by suppressing the leaching of fine particles such as organic impurities and metallic impurities, and have thus completed the present invention.
[0008] That is, the present invention is as shown below [1]. [1] A piping material comprising a polyethylene resin that satisfies the following requirements (1) to (3): (1) An 800 mL container obtained by blow molding polyethylene resin is filled with 600 mL of ultrapure water in a clean room, the lid is put on, and after storing it at a set temperature of 40°C for 35 days, the number of eluted particles of 0.1 μm or more is 25 particles / mL or less. (2) In the molecular weight distribution curve obtained using gel permeation chromatography (GPC), the molecular weight of components with a molecular weight of 1,000 or less is 0.50% by weight or less. (3) Metal content is 20 ppm or less Effect of the Invention
[0009] According to the present invention, it is possible to provide a piping material capable of suppressing the elution of fine particles such as organic impurities and metallic impurities during the transport of high-purity chemicals or ultrapure water, and the industrial value of this material is extremely high. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below.
[0011] The polyethylene resin constituting the piping material of the present invention can be any polyethylene-based resin that satisfies the following requirements (1) to (3) without any limitations. (1) An 800 mL container obtained by blow molding polyethylene resin is filled with 600 mL of ultrapure water in a clean room, the lid is put on, and after storing it at a set temperature of 40°C for 35 days, the number of eluted particles of 0.1 μm or more is 25 particles / mL or less. (2) In the molecular weight distribution curve obtained using gel permeation chromatography (GPC), the molecular weight of components with a molecular weight of 1,000 or less is 0.50% by weight or less. (3) Metal content is 20 ppm or less
[0012] Examples of the polyethylene resin include high density polyethylene, medium density polyethylene, branched low density polyethylene, linear low density polyethylene, and ultra-high molecular weight polyethylene, and among these, high density polyethylene is preferable because it provides a piping material having excellent mechanical strength, durability, etc. The density of the polyethylene resin is not particularly limited, but is usually 0.925 to 0.975 g / cm. 3 It is preferable that the molecular weight is 0.935 to 0.965 because the number of fine particles is suppressed and mechanical strength and durability are easily obtained. These polyethylene resins can be used alone or in combination or in combination.
[0013] Here, the polyethylene resin may be an ethylene homopolymer or an ethylene-α-olefin copolymer. In the case of an ethylene-α-olefin copolymer, the α-olefin may be, for example, propylene, 1-butene, 4-methyl-1-pentene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-hexadecene, 1-octadecene, etc., and a Ziegler catalyst is suitable as a highly active polymerization catalyst. As a specific example, a catalyst consisting of a solid catalyst component containing titanium, magnesium, and a halogen as essential components and an organoaluminum compound may be used as the Ziegler catalyst. By producing polyethylene using a Ziegler polymerization catalyst, it is possible to obtain a polyethylene resin composition containing less metals. The polyethylene resin constituting the piping material of the present invention may also be produced by a two-stage polymerization method.
[0014] Furthermore, the melt flow rate (JIS K6922-1, hereinafter referred to as HLMFR) of the polyethylene resin at 190°C under a load of 21.6 kg is not particularly limited, but is usually preferably 0.1 to 50 g / 10 min, and more preferably 1 to 30 g / 10 min, in order to suppress the number of fine particles and to improve the moldability and surface smoothness of the molded product.
[0015] The ratio Mw / Mn of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the polyethylene resin determined by gel permeation chromatography (GPC) is not particularly limited, but is usually preferably 3 to 20, and more preferably 5 to 15 because this suppresses the number of fine particles and improves moldability.
[0016] The number of particles of 0.1 μm or more eluted from the polyethylene resin constituting the piping material of the present invention is 25 particles / mL or less, more preferably 20 particles / mL or less. If the number of particles of 0.1 μm or more is 25 particles / mL or less, the amount of particles eluted from the piping material into high-purity chemicals or ultrapure water is small, so that the impurity concentration in the high-purity chemicals or ultrapure water can be suppressed. The number of particles can be measured by filling an 800 mL container obtained by blow molding a polyethylene resin with 600 mL of ultrapure water in a clean room, closing the lid, storing at a set temperature of 40° C. for 35 days, and then measuring the number of particles of 0.1 μm or more in the filled water with a particle counter.
[0017] In addition, in the molecular weight distribution curve obtained by gel permeation chromatography (GPC) of the polyethylene resin constituting the piping material of the present invention, the component having a molecular weight of 1,000 or less is 0.50% by weight or less. If the component having a molecular weight of 1,000 or less exceeds 0.50% by weight, the low molecular weight component increases, and the amount of fine particles eluted from the piping material into high purity chemicals or ultrapure water increases.
[0018] Furthermore, the polyethylene resin constituting the piping material of the present invention has a metal content of 20 ppm. If the metal content is 20 ppm or less, the metal impurity concentration of high purity chemicals or ultrapure water can be suppressed.
[0019] In addition, since the polyethylene resin can become fine particles in high-purity chemicals or ultrapure water, it is preferable that the polyethylene resin does not contain additives such as antioxidants, heat stabilizers, ultraviolet inhibitors, light stabilizers, and antistatic agents.
[0020] The polyethylene resin may contain a fluororesin within the scope of the present invention in order to improve the surface smoothness of the molded article. Examples of the fluororesin include homopolymers or copolymers of fluorinated olefins such as vinylidene fluoride, vinyl fluoride, tetrafluoroethylene, and hexafluoropropylene. The amount of the fluororesin added is preferably 0.01 to 0.05% by weight, since it keeps the impurity concentration low and improves the surface smoothness of the molded article.
[0021] The piping material of the present invention can be used for piping, joints, valves, etc.
[0022] The piping material of the present invention can be molded into any desired shape using an extrusion molding machine, an injection molding machine, a transfer molding machine, a compression molding machine, a blow molding machine, or the like. EXAMPLES
[0023] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. It is not something that is done.
[0024] ~Measurement of the number of eluted particles from polyethylene resin~ A container with an internal volume of 800 mL obtained by blow molding polyethylene resin was used. The container was filled with 600 mL of ultrapure water in a clean room, covered, and stored in a clean oven (Yamato Scientific Co., Ltd., DE411) set at 40°C for 35 days, after which the number of particles of 0.1 μm or more in the filled water was measured using a particle counter (Rion Co., Ltd., controller: KE-40B1, particle sensor: KS-42A). The number of particles in the water is shown in particles / mL.
[0025] -Evaluation of metal content in polyethylene resin- The sample was incinerated and then fused in an alkali to prepare a solution, which was used as a measurement solution. The amount of metal contained in the sample was measured by ICP-AES measurement.
[0026] ~Measurement of the number of particles dissolved from piping materials~ Polyethylene resin was continuously extruded by extrusion molding into a cylindrical shape with a wall thickness of 3 mm and an outer diameter of 50 mm, and then cut into a length of 20 cm to prepare a pipe. The pipe was covered with a glass cap, filled with 200 mL of ultrapure water in a clean room, and stored in a clean oven (Yamato Scientific Co., Ltd., DE411) set at a temperature of 40°C for 35 days, after which the number of particles of 0.1 μm or more in the filled water was measured using a particle counter (Rion Co., Ltd., controller: KE-40B1, particle sensor: KS-42A). The number of particles in the water is shown in particles / mL.
[0027] <Synthesis Example 1 (Synthesis of Polyethylene Resin A)> A Ziegler catalyst mainly composed of Mg, Al, Ti and Cl prepared according to Example 1 described in JP-A-7-41513, a solvent (hexane), ethylene (concentration 9-10 g / kg-solvent), hydrogen (concentration 0.1-0.3 g / kg-solvent), and triisobutylaluminum (concentration 0.10-0.20 g / kg-solvent) were continuously fed to a polymerization vessel, and ethylene polymerization was carried out under conditions of a temperature of 80-85°C, a total pressure of 3,000 kPa, and an average residence time of 2 hours. The hexane slurry containing the polymer from the first stage was continuously fed to a separate second stage polymerization vessel after removing unreacted hydrogen and ethylene in a flash tank. In the second-stage polymerization reactor, ethylene (concentration: 10-13 g / kg-solvent), hydrogen (0.03-0.05 g / kg-solvent), and 1-butene (8.5-10 g / kg-solvent) were further supplied, and ethylene polymerization was carried out under the conditions of a temperature of 75-85°C, a total pressure of 2,000 kPa, and an average residence time of 2 hours. The hexane slurry in the second-stage polymerization reactor was sent to a flash tank to remove unreacted hydrogen, ethylene, and 1-butene, and then a drying process was carried out to obtain a mixture powder of an ethylene-based copolymer. The powder polymerized in the above two stages was pelletized without the addition of any additives, to obtain polyethylene A. The polyethylene resin had a density of 0.955 g / cm 3The melt flow rate at 190°C under a load of 21.6 kg was 10.5 g / 10 min, the number of fine particles was 8, the molecular weight distribution curve obtained using GPC showed that the components having a molecular weight of 1,000 or less were 0.15% by weight, the Mw / Mn calculated from GPC was 10, and the metal content was 8 PPM. <Synthesis Example 2 (Synthesis of Polyethylene Resin B)> A Ziegler catalyst mainly composed of Mg, Al, Ti and Cl prepared according to Example 1 described in JP-A-7-41513, a solvent (hexane), ethylene (concentration 9-10 g / kg-solvent), hydrogen (concentration 0.1-0.3 g / kg-solvent), and triisobutylaluminum (concentration 0.10-0.20 g / kg-solvent) were continuously fed to a polymerization vessel, and ethylene polymerization was carried out under conditions of a temperature of 80-85°C, a total pressure of 3,000 kPa, and an average residence time of 2 hours. The hexane slurry containing the polymer from the first stage was continuously fed to a separate second stage polymerization vessel after removing unreacted hydrogen and ethylene in a flash tank. In the second-stage polymerization reactor, ethylene (concentration: 10-13 g / kg-solvent), hydrogen (0.01-0.015 g / kg-solvent), and 1-butene (11-13 g / kg-solvent) were further supplied, and ethylene polymerization was carried out under the conditions of a temperature of 75-85°C, a total pressure of 2,000 kPa, and an average residence time of 2 hours. The hexane slurry in the second-stage polymerization reactor was sent to a flash tank to remove unreacted hydrogen, ethylene, and 1-butene, and then a drying process was carried out to obtain a mixture powder of an ethylene-based copolymer. The powder obtained by the two-stage polymerization in the above manufacturing process was pelletized without the addition of any additives, to obtain polyethylene B. The polyethylene resin had a density of 0.945 g / cm 3 The melt flow rate at 190°C under a load of 21.6 kg was 15 g / 10 min, the number of fine particles was 10, the molecular weight distribution curve obtained using GPC showed that the components having a molecular weight of 1,000 or less were 0.3 wt%. The Mw / Mn calculated from GPC was 12, and the metal content was 9 PPM.
[0028] <Synthesis Example 3 (Synthesis of Polyethylene Resin C)> Polyethylene resin C was obtained in the same manner as in Synthesis Example 1, except that the polymerization temperature in the first stage was 70 to 80°C and the polymerization pressure was a total pressure of 1,000 kPa. The polyethylene resin had a density of 0.955 g / cm 3 The melt flow rate at 190°C under a load of 21.6 kg was 20 g / 10 min, the number of fine particles was 40, and in the molecular weight distribution curve obtained using GPC, the components having a molecular weight of 1,000 or less were 1.0 wt %, the Mw / Mn calculated from GPC was 18, and the metal content was 55 PPM.
[0029] <Synthesis Example 4 (Synthesis of Polyethylene Resin D)> The hexane slurry containing the polymer was subjected to removal of unreacted hydrogen and ethylene in a flash tank, and then a polyethylene resin D was obtained in the same manner as in Synthesis Example 1, except that solvent purification was not performed. The polyethylene resin had a density of 0.96 g / cm. 3 The melt flow rate at 190°C under a load of 21.6 kg was 14.5 g / 10 min, the number of fine particles was 40, the molecular weight distribution curve obtained using GPC showed that the components having a molecular weight of 1,000 or less were 2.1% by weight, the Mw / Mn calculated from GPC was 19, and the metal content was 30 PPM.
[0030] <Synthesis Example 5 (Synthesis of Polyethylene Resin E)> A polyethylene resin E was obtained in the same manner as in Synthesis Example 1, except that a Phillips catalyst containing Cr and SiO2 as main components, prepared according to Example 1 described in JP-A-53-91092, was used. The polyethylene resin had a density of 0.955 g / cm. 3 The melt flow rate at 190°C under a load of 21.6 kg was 18 g / 10 min, the number of fine particles was 60, and in the molecular weight distribution curve obtained using GPC, the components having a molecular weight of 1,000 or less were 0.8% by weight, the Mw / Mn calculated from GPC was 12.5, and the metal content was 60 PPM.
[0031] Example 1 Using the polyethylene resin A obtained in Synthesis Example 1, the polyethylene resin was continuously extruded into a cylindrical shape with a wall thickness of 3 mm and an outer diameter of 50 mm by extrusion molding, and then cut into a length of 20 cm to prepare a pipe. Then, isopropyl alcohol was passed through the pipe, and then the isopropanol was replaced with ultrapure water, and this operation was repeated three times before use in the test. Next, the number of particles of 0.1 μm or more in the liquid was measured in a clean room. The number of particles was 7, and the pipe had excellent purity with few particles.
[0032] Example 2 Using the polyethylene resin B obtained in Synthesis Example 2, the polyethylene resin was continuously extruded into a cylindrical shape with a wall thickness of 3 mm and an outer diameter of 50 mm by extrusion molding, and then cut into a length of 20 cm to prepare a pipe. Then, isopropyl alcohol was passed through the pipe, and then the isopropanol was replaced with ultrapure water, and this operation was repeated three times before use in the test. Next, the number of particles of 0.1 μm or more in the liquid was measured in a clean room. The number of particles was 9, and the pipe had excellent purity with few particles.
[0033] Example 3 A pipe was produced by adding 0.03 parts by weight of vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer (trade name) Dynamer FX5911 (manufactured by 3M Japan Ltd.) to 100 parts by weight of the polyethylene resin A obtained in Synthesis Example 1, and extrusion molding was carried out in the same manner as in Example 1. The number of fine particles in the pipe was 7, and the purity was excellent with few fine particles.
[0034] Comparative Example 1 A pipe was produced in the same manner as in Example 1, except that the polyethylene resin C obtained in Synthesis Example 3 was used, and the number of fine particles was measured. The number of fine particles in the pipe was 30, and the purity was poor with a large number of fine particles.
[0035] Comparative Example 2 A pipe was produced in the same manner as in Example 1, except that polyethylene resin D obtained in Synthesis Example 4 was used, and the number of fine particles was measured. The number of fine particles in the pipe was 45, and the purity was poor with a large number of fine particles.
[0036] Comparative Example 3 A pipe was produced in the same manner as in Example 1, except that polyethylene resin E obtained in Synthesis Example 5 was used, and the number of fine particles was measured. The number of fine particles in the pipe was 45, and the purity was poor with a large number of fine particles. [Industrial Applicability]
[0037] The present invention provides piping materials such as pipes, joints, valves, etc. that constitute transport lines for high-purity chemicals or ultra-pure water used in the semiconductor device industry, precision industrial parts, and pharmaceuticals.
Claims
[Claim 1] A piping material characterized by being made of a polyethylene resin that satisfies the following requirements (1) to (3). (1) A container with an internal volume of 800 mL obtained by blow molding polyethylene resin is filled with 600 mL of ultrapure water in a clean room, the container is covered, and the container is stored at a set temperature of 40° C. for 35 days. After that, the number of particles of 0.1 μm or more eluted is 25 particles / mL or less. (2) In a molecular weight distribution curve obtained using gel permeation chromatography (GPC), the content of components having a molecular weight of 1,000 or less is 0.50% by weight or less. (3) Metal content is 20 ppm or less
Citation Information
Patent Citations
Multilayer tube
JP2010234576A
Piping material for ultrapure water, and polyethylene-based resin composition for piping material for ultrapure water
JP2022145138A
Pipe for ultrapure water
JP2022157376A
Pipe material for ultrapure water
JP2022159129A