Thick steel plate and producing method thereof

A thick steel plate with a Si-enriched layer and Ni segregation region, combined with controlled manufacturing processes, addresses irregular scale peeling during laser cutting, enhancing laser cuttability and stability.

JP2024135079APending Publication Date: 2024-10-04NIPPON STEEL CORPORATION
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023045592
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing thick steel plates used in large structures face issues with irregular scale peeling during laser cutting due to varying heat absorption properties and poor adhesion, leading to unstable cutting and increased man-hours.

Method used

A thick steel plate with a Si-enriched layer and Ni segregation region at the steel plate/scale interface, controlled scale thickness deviation, and specific manufacturing processes to enhance adhesion and stability during laser cutting.

Benefits of technology

The solution effectively suppresses scale peeling during laser irradiation, improving laser cuttability and ensuring stable, high-quality cuts with reduced defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135079000005
    Figure 2024135079000005
  • Figure 2024135079000006
    Figure 2024135079000006
  • Figure 2024135079000007
    Figure 2024135079000007
Patent Text Reader

Abstract

To provide a thick steel plate, in which adhesion of scale is heightened, scale is suppressed or prevented from peeling during laser irradiation, thereby laser cutting property is improved and a producing method thereof.SOLUTION: Provided are a thick steel plate comprising a steel plate and a scale formed on a surface of the steel plate, further comprising a Si-enriched layer formed at the interface between the steel plate and the scale, the Si-enriched layer having an average thickness of 1.0 μm or more, a Ni segregation region having a length of 2.0 μm or more present along at least a part of the interface between the steel plate and the scale or along at least a part of a grain boundary in the vicinity of the surface of the steel plate, the Ni concentration in the Ni segregation region of 2.0 times or more the average Ni concentration in the steel plate, the thickness deviation of the scale of 0.70 or less, and the length of cracks present in the vicinity of the interface between the steel plate and the scale of 20 μm or less, and a method for producing the thick steel plate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thick steel plate and a manufacturing method thereof, and more particularly to a thick steel plate that is used by laser cutting in forming a structure, and a manufacturing method thereof. [Background technology]

[0002] A large amount of thick steel plates are used in large steel structures such as ships, building materials, industrial machinery, and bridges. In the construction of these steel structures, cutting and welding account for a large part of the construction labor. Therefore, there is a demand for precision cutting to reduce the cutting labor as well as the welding labor.

[0003] In addition to conventional gas cutting, laser cutting and plasma cutting are known as methods for cutting steel plates. Laser cutting has been popularized mainly for cutting thin steel plates because it has superior cut surface accuracy, a smaller heat-affected zone due to cutting, and can reduce labor hours through automation compared to conventional gas cutting. In recent years, with the practical application of high-power laser cutting machines, laser cutting is sometimes used for cutting thick steel plates used in the large steel structures.

[0004] The manufacturing of steel plates, such as thick steel plates, generally includes a process of hot rolling slabs, and it is known that hot-rolled steel plates oxidize in the atmosphere and form scales (iron oxide) on their surfaces. Laser cutting of steel plates involves applying heat to the steel plate by irradiating it with a laser, melting the steel plate, and cutting it, so the melting state changes significantly depending on the change in heat absorption at the point irradiated with the laser. The heat absorption of steel plates varies greatly depending on the state of the surface scale and the interface between the scale and the base steel, so depending on the state, the steel plate cannot be cut stably or abnormal cut parts are created on the cut surface, which increases the labor hours and deteriorates the cutting accuracy. In particular, when the surface scale peels off irregularly due to laser irradiation, the heat absorption also varies irregularly and significantly, making the laser cutting particularly unstable and causing the eruption of molten material from the cut part, which is called burning.

[0005] As a method for improving laser cuttability, for example, Patent Document 1 proposes a steel material having a dry coating film on the surface of the steel sheet containing a coloring pigment consisting of titania powder, zinc powder, aluminum powder, and one or more of black iron oxide pigment and black calcined pigment. Patent Document 1 teaches that the laser cuttability can be improved by adding titania powder with high laser absorption to the coating film of the coated steel material to increase the laser absorption rate. Patent Document 2 also presents a steel material having a coating composition on the surface of which contains an alkoxysilane having two or more alkoxy groups and / or its hydrolysate or condensate (e.g., tetraalkoxysilane), zinc powder, and powder of aluminum phosphate (preferably aluminum tripolyphosphate) or a mixed powder of aluminum phosphate and zinc phosphate.

[0006] On the other hand, Patent Document 3 presents a steel sheet in which the ratio of magnetite phase (Fe3O4) in the scale on the steel sheet surface is set to 85% or more to increase adhesion and the thickness of the scale is limited to 6 μm or less in order to improve laser cuttability.

[0007] Furthermore, Patent Documents 4 and 5 propose improving laser cuttability by reducing peeling at the interface between the scale and the base steel that exists before laser cutting in thick steel plate and by reducing voids that exist in the scale.

[0008] Patent Document 6 describes that stable cuttability can be ensured by having a layer of Si-enriched regions with an Si content of 0.4% or more in the scale and a layer of Al-enriched regions with an Al / Si ratio of 0.3 or more on the surface side of the Si-enriched regions. Patent Document 7 proposes forming an internal oxide layer with concentrated alloy elements on the base steel side of the interface between the scale and base steel of the steel plate, thereby improving the spalling resistance of the scale. Furthermore, Patent Document 8 proposes forming a region with concentrated alloy elements at the interface between the scale and base steel of a thick steel plate and, in addition, reducing voids present in the scale, thereby improving laser cuttability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2013 / 065349 [Patent Document 2] JP 2008-156377 A [Patent Document 3] JP 2003-221640 A [Patent Document 4] JP 2002-332540 A [Patent Document 5] JP 2005-271074 A [Patent Document 6] International Publication No. 2012 / 014851 [Patent Document 7] Japanese Patent Application Publication No. 09-078180 [Patent Document 8] JP 2002-332541 A Summary of the Invention [Problem to be solved by the invention]

[0010] In order to reduce costs in a society with a declining population, there is an increasing demand for automation of laser cutting of steel plates. On the other hand, to cope with the thickening of the objects to be cut due to the enlargement of structures and the increase in cutting speed by high-power fiber lasers, steel plates with better laser cuttability than before are required. Specifically, in order to improve laser cuttability, there is a demand for steel plates with a scale that has excellent adhesion and does not peel off irregularly when irradiated with a higher-power laser than before.

[0011] In the steel sheet described in Patent Document 3, measures have been taken against irregular peeling of scale, but descaling with high-pressure water is required in every rolling pass, and there is still room for improvement in terms of addressing the fundamental issue of cost reduction. In addition, Patent Document 7 considers improving scale peeling resistance, but there is still room for improvement in terms of increasing laser output.

[0012] Therefore, an object of the present invention is to provide a thick steel plate that has improved adhesion of scale, suppresses or prevents scale peeling during laser irradiation, and therefore has improved laser cuttability, and a manufacturing method thereof. [Means for solving the problem]

[0013] In order to achieve the above object, the inventors have investigated the surface layer of a steel sheet necessary for stable cutting in laser cutting. As a result, they have found that when defects occur on the laser cut surface, scale peels off irregularly at the location irradiated with the laser. It is presumed that this is because the thermal stress caused by the laser irradiation causes partial scale peeling in areas where adhesion is low at the interface between the steel sheet (base steel) and the scale.

[0014] The present inventors conducted various studies aimed at improving the adhesion between steel sheet and scale in order to suppress the occurrence of defects on the laser cut surface. First, a Si-enriched layer is generated at the steel sheet / scale interface, and Ni-segregated regions are generated at the steel sheet / scale interface or at grain boundaries near the surface of the steel sheet in a heating furnace. Next, the surface of the steel sheet can be homogenized by removing the scale above the Si-enriched layer and Ni-segregated region by descaling, leaving the Si-enriched layer and the Ni-segregated region. Then, stable scale growth can be promoted by appropriately controlling the subsequent cooling process. As a result, it was found that a scale with excellent adhesion can be obtained over the entire surface layer of the steel sheet.

[0015] The present invention which has achieved the above object is as follows. (1) A steel plate and a scale formed on a surface of the steel plate, Further comprising a Si-enriched layer formed at the interface between the steel sheet and the scale, The average thickness of the Si-enriched layer is 1.0 μm or more, a Ni segregation region having a length of 2.0 μm or more is present along at least a part of the interface between the steel sheet and the scale or at least a part of the grain boundary in the vicinity of the surface of the steel sheet, The Ni concentration in the Ni segregation region is 2.0 times or more the average Ni concentration in the steel sheet, The scale thickness deviation is 0.70 or less, A thick steel plate, wherein the length of a crack present in the vicinity of the interface between the steel plate and the scale is 20 μm or less. (2) The steel plate according to (1) above, wherein the average thickness of the scale is 20 to 70 μm. (3) The steel plate comprises, in mass%, C: 0.02-0.30%, Si: 0.15-1.20%, Mn: 0.30-2.20%, P: 0.003-0.060%, S: 0.010% or less, Ni: 0.05-1.50%, Al: 0.001 to 0.100%, N: 0.010% or less, O: 0.0035% or less, Cu: 0-1.00%, Cr: 0-1.00%, Mo: 0-1.00%, W: 0 to 0.50%, Nb: 0 to 0.500%, Ti: 0 to 0.500%, V: 0 to 1.000%, B: 0~0.0100%, Sn: 0 to 0.500%, Sb: 0 to 0.500%, Ca: 0 to 0.0100%, Mg: 0 to 0.0100%, Hf: 0~0.0100%, Te: 0~0.0100%, Sr: 0 to 0.0100%, REM: 0 to 0.0100%, and The steel plate according to (1) or (2) above, having a chemical composition consisting of the balance: Fe and impurities. (4) The chemical composition is, in mass%, Cu: 0.01 to 1.00%, Cr: 0.01 to 1.00%, Mo: 0.01 to 1.00%, W: 0.003 to 0.50%, Nb: 0.003 to 0.500%, Ti: 0.003 to 0.500%, V: 0.003 to 1.000%, B: 0.0003~0.0100%, Sn: 0.003 to 0.500%, Sb: 0.003 to 0.500%, Ca: 0.0003~0.0100%, Mg: 0.0003~0.0100%, Hf: 0.0003~0.0100%, Te: 0.0003~0.0100%, Sr: 0.0003 to 0.0100%, and REM: 0.0003~0.0100% The steel plate according to (3) above, comprising one or more selected from the group consisting of: (5) a step of heating the slab, the step of heating the slab to a temperature at which the surface temperature of the slab becomes 1180°C to 1300°C and maintaining the temperature for 40 to 240 minutes; a hot rolling step of hot rolling the slab, the hot rolling step being performed at a rolling completion temperature of 1050°C to (T0-30)°C and a cumulative rolling reduction of 15 to 30%, followed by performing high-pressure water descaling in a temperature range of 1000°C to (T0-30)°C, and then performing rolling two or more times in which the rolling reduction in one pass is 30% or less compared to the plate thickness before rolling in each pass, controlling the interpass time of the rolling after the high-pressure water descaling to satisfy the following formula (2), and setting the rolling completion temperature in the final rolling pass to 850°C or more; A step of cooling the obtained steel sheet, in which the elapsed time from the completion of the hot rolling step to the start of water cooling is controlled so as to satisfy the following formula (3), and the water cooling stop temperature is set to 550 to 650 ° C. The method for producing a thick steel plate according to any one of the above (1) to (4), comprising: T0 is the temperature calculated by the following formula (1). T0=1175-8.4[Mn]-135[P] 0.5 -52[Al]-24[Cr]...Formula (1) [Mn], [P], [Al] and [Cr] are the contents [mass%] of each element in the slab. y n ≦1.00...Equation (2) y m =y m-1 ·exp[E1·k m-1 ·exp{E2·(J m-1 +J m )}]+E3·R m ·exp(E4·J m ) y0=0.00 y m is an index showing the degree of cracking in the scale that occurs in the mth rolling out of a total of n rolling steps performed from after high-pressure water descaling to the completion of rolling, E1, E2, E3 and E4 are constants, each of which is −2.57 × 10 -10 , -1.02×10 -2 , 2.70×10 1 and -8.33 × 10 -3 and k m is the elapsed time [seconds] from the mth rolling to the (m+1)th rolling, J m is the rolling temperature of the material at the mth rolling step [℃], R m is the reduction ratio [%] of the thickness before rolling in the mth rolling pass, y n is obtained by calculating y1, y2, y3, etc., in that order using the above formula. 1.0≦z 10 ≦10.0...Equation (3) z1=F1·exp{F2 / (H1-F3)}·(-H1 2 +F4H1+F5) 0.5 Δp 0.5 p n =z n 2 Formula 1 -2 ·exp{2·F2 / (H1-F3)}·(-H n+1 2 +F4H n+1 +F5) -1 z n =F1·exp{F2 / (H n -F 3)}·(-H n 2 +F4H n +F5) 0.5 ·(p n-1 +Δp) 0.5 z n is an index showing the degree of scale growth after the elapsed time from the end of the hot rolling process to the start of water cooling is divided into 10 equal parts during the cooling process, and n indicates that the calculation corresponds to the nth of the 10 equal parts. F1, F2, F3, F4 and F5 are constants, each equal to 1.63 × 10 -6 , -2.50×10 2 , 3.25×10 2 , 2.94×10 2 and 1.36×10 6 and H n is the average steel plate temperature [℃] in the nth region of the 10 equal divisions, Δp is one tenth of the elapsed time [seconds], z 10 is obtained by calculating z1, z2, z3, etc., in that order using the above formula. Effect of the Invention

[0016] According to the present invention, by increasing the adhesion of the scale, peeling of the scale during laser irradiation can be suppressed or prevented, and therefore a thick steel plate and a manufacturing method thereof can be provided with improved laser cuttability. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram of a thick steel plate according to an embodiment of the present invention. [Diagram 2] The layer distribution (hematite, magnetite, and wüstite) inside the scale is shown by crystal orientation analysis using the EBSD method. [Diagram 3] The Si concentration map obtained by EPMA is shown. [Figure 4] The oxygen concentration map obtained by EPMA is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, a thick steel plate and a manufacturing method thereof according to an embodiment of the present invention will be described in more detail. However, these descriptions are intended to exemplify preferred forms of the present invention and are not intended to limit the present invention to specific embodiments.

[0019] [Preferable chemical composition] In the embodiment of the present invention, the chemical composition of the steel plate is not particularly limited, and may be appropriately determined within a range useful for application in laser cutting. As described above, the present invention aims to provide a thick steel plate that enhances the adhesion of the scale, suppresses or prevents scale peeling during laser irradiation, and therefore has improved laser cuttability. The present invention achieves the above-mentioned objective by providing a steel plate and a scale formed on the surface of the steel plate, further including a Si-enriched layer formed at the interface between the steel plate and the scale, the average thickness of the Si-enriched layer being 1.0 μm or more, a Ni segregation region having a length of 2.0 μm or more along at least a part of the interface between the steel plate and the scale or at least a part of the grain boundary near the surface of the steel plate, the Ni concentration of the Ni segregation region being 2.0 times or more the average Ni concentration of the steel plate (base steel), and the thickness deviation of the scale being 0.70 or less. Therefore, it is clear that the chemical composition of the steel plate itself is not an essential technical feature for achieving the objective of the present invention. Hereinafter, a preferred chemical composition of the steel plate according to the embodiment of the present invention will be described, but these descriptions are intended to be merely illustrative and are not intended to limit the present invention to a steel plate having such a specific chemical composition. In the following description, the unit of content of each element, "%", means "mass %" unless otherwise specified.

[0020] [C: 0.02~0.30%] C is an element that greatly increases strength, and in order to increase strength, it is preferable to contain 0.02% or more, and more preferably 0.04% or more. On the other hand, if C exceeds 0.30%, the toughness of the steel plate is greatly deteriorated, so the C content is preferably 0.30% or less. In addition, C is an element that impairs weldability and the toughness of the welded portion, and from this viewpoint, the C content is preferably 0.20% or less, and more preferably 0.18% or less.

[0021] [Si:0.15~1.20%] Si is an element that forms a Si-enriched layer at the interface between the steel sheet and the scale, and by containing an appropriate amount of Si in the steel sheet, the scale and the Si-enriched layer having the characteristics of the thick steel sheet according to the embodiment of the present invention can be formed. In order to sufficiently form the Si-enriched layer at the steel sheet / scale interface, the Si content is preferably 0.15% or more. In order to improve the scale adhesion, the Si content is preferably 0.20% or more, and more preferably 0.30% or more. On the other hand, if the Si content is high, the Si-enriched layer is excessively formed at the steel sheet / scale interface, and the formation behavior of the scale on the surface of the steel sheet becomes non-uniform, and the laser cuttability deteriorates, so the Si content is preferably 1.20% or less. In addition, Si is an element that impairs the toughness of the steel sheet, and from this viewpoint, the Si content is preferably 1.00% or less, and more preferably 0.80% or less.

[0022] [Mn: 0.30~2.20%] Mn is an element that contributes to improving strength, and in order to fully obtain this effect, the Mn content is preferably 0.30% or more. From the viewpoint of increasing strength, the Mn content is preferably 0.40% or more, and more preferably 0.50% or more. On the other hand, if Mn is contained excessively, the formation of a Si-enriched layer is excessively promoted, the behavior of the scale formation on the surface of the steel sheet becomes non-uniform, and the laser cuttability deteriorates, so that the Mn content is preferably limited to 2.20% or less. From this viewpoint, the Mn content is preferably 2.00% or less, and more preferably 1.80% or less.

[0023] [P:0.003~0.060%] P is an element that is inevitably contained in a general steelmaking process, and limiting it to less than 0.003% places a large load on the smelting process and is economically undesirable. From this viewpoint, the P content is preferably 0.003% or more. In addition, P is an element that promotes the formation of a Si-enriched layer, and from this viewpoint, the P content is preferably 0.005% or more, and more preferably 0.008% or more. On the other hand, if P is contained excessively, the formation of a Si-enriched layer is excessively promoted, the behavior of the scale formation on the surface of the steel sheet becomes non-uniform, and the laser cuttability is deteriorated. From this viewpoint, the P content is preferably limited to 0.060% or less, more preferably 0.050% or less, and even more preferably 0.040% or less.

[0024] [S:0.010% or less] S is an element that is inevitably contained in general steelmaking methods and forms coarse sulfides that reduce toughness. From this viewpoint, the S content is preferably limited to 0.010% or less, more preferably 0.006% or less, and even more preferably 0.004% or less. [Ni: 0.05~1.50%] Ni is an element that segregates along at least a part of the interface between the steel sheet and the scale or along at least a part of the grain boundary near the surface of the steel sheet, thereby improving the adhesion between the steel sheet and the scale and improving the laser cuttability of the steel sheet. To achieve this effect, the Ni content is preferably 0.05% or more, and more preferably 0.08% or more. On the other hand, if the Ni content is excessive, there is a concern that scratches will occur on the surface of the cast slab and cause problems in rolling, so the Ni content is preferably limited to 1.50% or less. In addition, since Ni deteriorates weldability, the Ni content is more preferably 1.30% or less.

[0025] [Al: 0.001~0.100%] Al is a deoxidizing element, and in order to obtain this effect, the Al content is preferably 0.001% or more. In order to fully exert the deoxidizing effect, the Al content is preferably 0.005% or more. Furthermore, Al is an element that promotes the formation of a Si-enriched layer, and from this viewpoint, the Al content is preferably 0.010% or more. On the other hand, if an excessive amount of Al is contained, the formation of a Si-enriched layer is excessively promoted and the laser cuttability is impaired, so that the Al content is preferably limited to 0.100% or less, more preferably 0.060% or less, and even more preferably 0.050% or less.

[0026] [N:0.010% or less] N is an element that is inevitably contained in a general steelmaking process. If a large amount of N is contained, coarse nitrides are formed, which impairs the toughness of the steel plate, so the N content is preferably limited to 0.010% or less. In addition, N is an element that impairs the toughness of a welded portion, and from this viewpoint, the N content is preferably set to 0.009% or less, and more preferably to 0.008% or less. There is no particular lower limit for the N content, but since limiting it to less than 0.001% places a large load on the smelting process and is economically undesirable, it is preferable to set it to 0.001% or more.

[0027] [O:0.0035% or less] O is an element that is inevitably contained in a general steelmaking process. If a large amount of O is contained, coarse oxides are formed, which impairs the toughness of the steel sheet, so the O content is preferably limited to 0.0035% or less. O is also an element that impairs the toughness of a welded portion, and from this viewpoint, the O content is preferably limited to 0.0030% or less, and more preferably to 0.0025% or less. There is no particular lower limit for the O content, but since limiting it to less than 0.0002% places a large load on the smelting process and is economically undesirable, it is preferable to set it to 0.0002% or more.

[0028] The basic chemical composition of the steel sheet according to the embodiment of the present invention is as described above. Furthermore, the steel sheet may contain one or more of the following optional elements as necessary. The steel sheet may contain one or more selected from the group consisting of Cu: 0-1.00%, Cr: 0-1.00%, Mo: 0-1.00%, and W: 0-0.50%. The steel sheet may also contain one or more selected from the group consisting of Nb: 0-0.500%, Ti: 0-0.500%, and V: 0-1.000%. The steel sheet may also contain B: 0-0.0100%. The steel sheet may also contain one or two selected from the group consisting of Sn: 0-0.500% and Sb: 0-0.500%. The steel sheet may also contain one or more elements selected from the group consisting of Ca: 0-0.0100%, Mg: 0-0.0100%, Hf: 0-0.0100%, Te: 0-0.0100%, Sr: 0-0.0100%, and REM: 0-0.0100%. These optional elements will be described in detail below.

[0029] [Cu: 0-1.00%] Cu is an element that enhances the adhesion between the steel sheet and the scale and enhances the laser cuttability of the steel sheet. The Cu content may be 0%, but when it is contained, it may be 0.001% or more. To obtain this effect, the Cu content is preferably 0.01% or more, and more preferably 0.04% or more. On the other hand, if the Cu content is excessive, there is a concern that scratches will occur on the surface of the cast slab and cause problems in rolling, so the Cu content is preferably limited to 1.00% or less. In addition, since Cu deteriorates weldability, the Cu content is more preferably 0.50% or less.

[0030] [Cr:0~1.00%] Cr is an element that contributes to improving strength. The Cr content may be 0%, but when it is contained, it may be 0.001% or more or 0.01% or more. Cr is also an element that promotes the formation of fayalite that mainly constitutes the Si-enriched layer, and from this viewpoint, the Cr content is preferably 0.05% or more, and more preferably 0.15% or more. On the other hand, if Cr is contained excessively, there is a concern that coarse Cr carbonitrides will be generated and the toughness of the steel plate will be greatly deteriorated. From this viewpoint, it is preferable to limit the Cr content to 1.00% or less. Cr is also an element that impairs weldability and the toughness of the welded part, and from this viewpoint, the Cr content is preferably 0.60% or less.

[0031] [Mo:0~1.00%] Mo is an element that contributes to improving strength. It is also an element that is effective in suppressing the oxidation of Fe on the surface of the steel sheet during cutting by laser cutting or the like, and the heat generation associated therewith, by concentrating at the interface between the steel sheet and the scale. The Mo content may be 0%, but when it is contained, it may be 0.001% or more or 0.01% or more. From the viewpoint of enhancing these effects, the Mo content is preferably 0.02% or more, and more preferably 0.05% or more. On the other hand, if Mo is contained excessively, there is a concern that the weldability and the toughness of the welded part may be impaired. From this viewpoint, the Mo content is preferably limited to 1.00% or less, and more preferably 0.30% or less.

[0032] [W:0~0.50%] W is an element that contributes to improving strength. The content of W may be 0%, but when it is contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the content of W is preferably 0.05% or more, and more preferably 0.15% or more. On the other hand, if W is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the content of W is preferably limited to 0.50% or less, and more preferably 0.30% or less.

[0033] [Nb: 0~0.500%] Nb is an element that contributes to improving strength. The Nb content may be 0%, but when it is contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the Nb content is preferably 0.005% or more, and more preferably 0.010% or more. On the other hand, if Nb is contained excessively, coarse Nb carbonitrides are generated, and there is a concern that the toughness of the steel plate and welded parts will be significantly deteriorated. From this viewpoint, the Nb content is preferably limited to 0.500% or less, and more preferably 0.100% or less.

[0034] [Ti: 0~0.500%] Ti is an element that contributes to improving strength. The Ti content may be 0%, but when it is contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the Ti content is preferably 0.005% or more, and more preferably 0.010% or more. On the other hand, if Ti is contained excessively, coarse Ti carbonitrides are generated, and there is a concern that the toughness of the steel plate and welded parts may be significantly deteriorated. From this viewpoint, the Ti content is preferably limited to 0.500% or less, and more preferably 0.200% or less.

[0035] [V:0~1.000%] V is an element that contributes to improving strength. The V content may be 0%, but when contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the V content is preferably 0.030% or more, and more preferably 0.080% or more. On the other hand, if V is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the V content is preferably limited to 1.000% or less, and more preferably 0.600% or less.

[0036] [B:0~0.0100%] B is an element that contributes to improving strength. The content of B may be 0%, but when it is contained, it may be 0.0001% or more. From the viewpoint of increasing strength, the content of B is preferably 0.0003% or more, and more preferably 0.0008% or more. On the other hand, if B is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the content of B is preferably limited to 0.0100% or less, and more preferably 0.0035% or less.

[0037] [Sn:0~0.500%] Sn has the effect of concentrating at the interface between the steel sheet and the scale, and promoting the formation of a Si-concentrated layer. The Sn content may be 0%, but in order to increase the adhesion of the scale and improve the laser cuttability, Sn may be contained in an amount of 0.500% or less. In order to fully obtain this effect, the Sn content is preferably 0.001% or more, 0.003% or more, or 0.005% or more, and more preferably 0.025% or more. On the other hand, if a large amount of Sn is contained, the weldability and the toughness of the welded part are impaired, so the Sn content is preferably limited to 0.500% or less. From this viewpoint, the Sn content is preferably 0.300% or less, and more preferably 0.200% or less.

[0038] [Sb: 0~0.500%] Sb has the effect of concentrating at the interface between the steel sheet and the scale and promoting the formation of a Si-concentrated layer. The Sb content may be 0%, but in order to increase the adhesion of the scale and improve the laser cuttability, the Sb content is preferably 0.001% or more or 0.003% or more. In order to fully obtain this effect, the Sb content is preferably 0.005% or more, and more preferably 0.025% or more. On the other hand, if a large amount of Sb is contained, the weldability and the toughness of the welded part are impaired, so the Sb content is preferably limited to 0.500% or less. From this viewpoint, the Sb content is preferably 0.300% or less, and more preferably 0.200% or less.

[0039] [Ca: 0~0.0100%] [Mg: 0~0.0100%] [Hf:0~0.0100%] [Te:0~0.0100%] [Sr:0~0.0100%] [REM:0~0.0100%] Ca, Mg, Hf, Te, Sr and REM are elements that refine sulfides and improve the toughness of steel plate. The contents of Ca, Mg, Hf, Te, Sr and REM may be 0%, but to obtain this effect, the contents of Ca, Mg, Hf, Te, Sr and REM are preferably 0.0001% or more or 0.0003% or more, respectively. On the other hand, if these elements are contained excessively, the effect is saturated, and therefore, the inclusion of more Ca, Mg, Hf, Te, Sr and REM in the steel plate than necessary leads to an increase in manufacturing costs. Therefore, it is preferable to limit the contents of Ca, Mg, Hf, Te, Sr and REM to 0.0100% or less, and more preferably to 0.0040% or less. Here, REM is a general term for Sc, Y and lanthanides (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu), and the total content of these 17 elements is defined as the REM content.

[0040] In the steel sheet according to the embodiment of the present invention, the balance other than the above elements consists of Fe and impurities. The impurities are components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when the steel sheet is industrially manufactured.

[0041] The chemical composition of steel sheets can be measured by a general analytical method. For example, the chemical composition of steel sheets can be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S are measured using the combustion-infrared absorption method.

[0042] Next, the characteristics of the steel plate according to the embodiment of the present invention in terms of scale will be described.

[0043] A schematic diagram of a thick steel plate according to an embodiment of the present invention is shown in Fig. 1. Referring to Fig. 1, it can be seen that the thick steel plate according to the embodiment of the present invention includes a steel plate and a scale formed on the surface of the steel plate, and further includes a Si-enriched layer formed at the interface between the steel plate and the scale, and has a Ni segregated region having a predetermined length along at least a part of the interface between the steel plate and the scale or at least a part of the grain boundary near the surface of the steel plate.

[0044] [Average thickness of Si-enriched layer: 1.0 μm or more] In the thick steel plate according to the embodiment of the present invention, a Si-enriched layer is formed at the interface between the steel plate and the scale. The Si-enriched layer is a layer formed mainly by so-called fayalite. From the viewpoint of enhancing the adhesion of the scale, it is preferable that the interface is sufficiently covered by the Si-enriched layer. If the coverage of the interface by the Si-enriched layer is insufficient, peeling of the scale cannot be suppressed at the portion where the Si-enriched layer is not present at the interface, the adhesion of the scale is reduced, and further, the growth behavior of the scale differs between the portion where fayalite is present and the portion where it is not present at the interface, and the laser cuttability is deteriorated due to the deviation in the scale thickness. When the interface between the steel plate and the scale is appropriately covered by the Si-enriched layer, the thickness deviation of the scale can be reliably controlled within a desired range, that is, 0.70 or less as described in detail later. Therefore, in the thick steel plate according to the embodiment of the present invention, it is not necessary to specify the coverage ratio of the interface by the Si-enriched layer. It is sufficient that more than 50 area % of fayalite is present in the Si-enriched layer, and in addition to fayalite, other phases (wustite, magnetite, hematite) may also be present.

[0045] The average thickness (t) of the Si-enriched layer is 1.0 μm or more. If the thickness of the Si-enriched layer is thin, the effect of increasing the adhesion of the scale is insufficient, and the laser cuttability is not sufficiently improved. For this reason, the average thickness of the Si-enriched layer is 1.0 μm or more. On the other hand, if the average thickness of the Si-enriched layer is excessively thick, cracks are likely to occur in the fayalite and its vicinity due to thermal stress caused by laser irradiation, and the adhesion of the scale is deteriorated, and the laser cuttability is deteriorated. The average thickness of the Si-enriched layer is preferably 10.0 μm or less. From the above viewpoints, the average thickness of the Si-enriched layer is preferably 1.0 to 10.0 μm, and more preferably 1.5 to 8.0 or 7.0 μm.

[0046] [Ni segregation region that exists along at least a part of the interface between the steel sheet and the scale or along at least a part of the grain boundary near the surface of the steel sheet: length 2.0 μm or more] The thick steel plate according to the embodiment of the present invention has a Ni segregation region. The Ni segregation region refers to a region in which Ni is concentrated to 2.0 times or more the average Ni concentration of the steel plate (base steel). If Ni is less than 2.0 times the average Ni concentration of the steel plate, sufficient scale adhesion cannot be obtained. There is no particular upper limit for the Ni concentration of the Ni segregation region, but the Ni concentration of the region is at most 10.0 times the average Ni concentration of the steel plate, and may be 8.0 times or less. The length of the Ni segregation region refers to the length of the Ni segregation region that exists continuously in a cross section perpendicular to the interface between the scale and the steel plate. When the Ni segregation region exists at the interface between the steel plate and the scale, the length (L1) along the interface between the steel plate and the scale may be measured. For example, when the interface is curved, the length along the curve may be taken as the length of the Ni segregation region. When the Ni segregation region exists along the grain boundary near the surface of the steel plate, the length along the grain boundary may be taken as the length of the Ni segregation region (L2). The Ni segregation region may be identified by, for example, performing Ni mapping analysis using a Field Emission Scanning Electron Microscope (FE-SEM). Alternatively, it may be identified by element mapping using an Electron Probe MicroAnalizer (EPMA). In the present invention, the "average Ni concentration of the steel sheet" refers to a value measured by the above-mentioned Inductively Coupled Plasma-Atomic Emission Spectrometry (ICP-AES).

[0047] The Ni segregation region exists at the interface between the steel sheet and the scale or along the grain boundaries near the surface of the steel sheet. The presence of the Ni segregation region at these locations improves the adhesion between the steel sheet (base steel) and the scale interface. The Ni segregation region does not need to exist over the entire surface of these locations, but only needs to exist in at least a part of these locations. The length (L) of the Ni segregation region must be 2.0 μm or more. If the length is less than 2.0 μm, the adhesion between the steel sheet (base steel) and the scale interface is insufficient, and irregular scale peeling is likely to occur during laser irradiation. There is no upper limit to the length of the Ni segregation region. However, in the Ni segregation region that is generated at the interface between the steel sheet and the scale or along the grain boundaries near the surface of the steel sheet, Ni is easily diffused, so it tends to become long, and can reach as long as 7.0 μm in some cases. The diffusion of Ni occurs mainly during slab heating, and the higher the heating temperature and the longer the heating time, the longer the length of the Ni segregation region becomes. However, if heating is performed for an excessively long time, the scale thickness generated on the slab becomes too thick, making descaling during rolling difficult. If one attempts to control the scale thickness so as to perform appropriate descaling, the length of the Ni segregated region is usually 15.0 μm or less.

[0048] [Scale thickness deviation: 0.70 or less] In the thick steel plate according to the embodiment of the present invention, the scale thickness is uniform, so that the occurrence of thermal stress is suppressed, the scale adhesion is improved, and the scale adhesion is excellent. If the scale thickness varies greatly, the amount of heat consumed by melting the scale due to laser irradiation changes irregularly, thermal stress is generated irregularly, and the scale adhesion is deteriorated. From this viewpoint, in the thick steel plate according to the embodiment of the present invention, the deviation of the scale thickness obtained by dividing the difference between the maximum and minimum thicknesses of the measured scale by the average thickness is limited to 0.70 or less. Since the smaller the scale thickness deviation, the higher the scale adhesion, the scale thickness deviation is preferably 0.60 or less, more preferably 0.55 or less, and even more preferably 0.50 or less. There is no particular lower limit for the scale thickness deviation, but since the effect of reducing the scale thickness deviation is saturated when it is less than 0.03, it is preferably 0.03 or more from an economical viewpoint, and may be 0.05 or more or 0.08 or more.

[0049] [The length of the crack near the interface between the steel plate and the scale is 20 μm or less] The thick steel plate according to the embodiment of the present invention has excellent laser cuttability because the length of the cracks existing near the interface between the steel plate and the scale is 20 μm or less. Cracks are relatively likely to occur in places where there is no Si-enriched layer or Ni segregation region, and are often sandwiched between the steel plate (base steel) and the scale. Even if the variation in the thickness of the scale is small, if there are cracks, the scale is likely to peel off due to thermal stress accompanying laser irradiation, making the melting phenomenon by the laser unstable, and large irregularities are likely to occur on the cut surface, making it easy for cutting defects to occur. However, if the cracks are small, the scale will not peel off due to thermal stress, stable melting by the laser is possible, and a smooth cut surface can be obtained. From this viewpoint, in the thick steel plate according to the embodiment of the present invention, the length of the cracks existing near the interface between the steel plate and the scale is 20 μm or less. The shorter the crack length, the more preferable it is, and the length is preferably 15 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. There is no particular lower limit set for the crack length. The length of the crack can be determined by taking a photograph of a cross section perpendicular to the interface between the scale and the steel sheet using an optical microscope and then determining the length of the crack from the electronic image.

[0050] [Average scale thickness: 20~70μm] The average thickness (T) of the scale formed on the surface of the thick steel plate according to the embodiment of the present invention is preferably 20 to 70 μm. By making the scale thicker, a sudden increase in the temperature of the steel plate during laser irradiation is suppressed, and it is possible to reliably suppress the occurrence of poor cutting caused by an increase in the amount of molten steel. From this viewpoint, the average thickness of the scale is preferably 20 μm or more, and more preferably 30 μm or more. On the other hand, if the scale becomes too thick, the thermal stress generated at the steel plate (base steel) / scale interface during laser irradiation increases, and the adhesion of the scale may decrease. For this reason, from the viewpoint of further increasing the adhesion of the scale, the average thickness of the scale is preferably 70 μm or less, and more preferably 60 μm or less.

[0051] The scale in the steel plate according to the embodiment of the present invention may further contain hematite (Fe2O3), wustite (FeO), alloy oxides, ferrite, and metal particles, so long as the above characteristics are satisfied.

[0052] The features of the scale described above are evaluated by crystal orientation analysis and structural observation of the cross section of the scale. Specifically, a small piece is cut from half of the thickness of the steel plate in the width direction, and the cross section parallel to the rolling direction and perpendicular to the plate surface is used as the observation surface. The observation surface is wet polished and polished with colloidal silica to a mirror finish, and the section from the outermost surface of the steel plate to the steel plate / scale interface is observed using a Field Emission Scanning Electron Microscope (FE-SEM), analyzed using a crystal orientation analyzer that uses the electron backscattering diffraction (EBSD) method mounted on the FE-SEM, and element mapping is performed using an Electron Probe MicroAnalizer (EPMA).

[0053] The crystal orientation analysis using the EBSD method reveals the layer distribution inside the scale, as shown in FIG. 2. The EBSD method also detects the presence of a Si-enriched layer (mainly composed of fayalite). However, the crystal structure of fayalite is particularly complex, and the detection pattern obtained by the EBSD method is weak, so the thickness of the Si-enriched layer cannot be determined from the map shown in FIG. 2. When element mapping is performed by EPMA at the location where the Si-enriched layer is detected by the EBSD method, a Si-enriched area is observed, as shown in FIG. 3. Here, at each measurement point, the measurement point where the detected Si concentration is 5.0 mass% or more is determined to be fayalite. In addition, as shown in FIG. 4, when fayalite is present within 2.0 μm in the sheet thickness direction from the steel sheet / scale interface determined from the oxygen concentration map obtained by the element mapping, the scale is determined to be covered with fayalite. The region where the fayalite identified in this way exists at a ratio of more than 50 area% at the interface between the steel sheet and the scale is determined to be the Si-enriched layer. Furthermore, from the element concentration maps of iron, oxygen, and substitutional elements (Si, Mn, Ni, Cu, and Cr), measurement points where the total amount of these elements is less than 50 at% are determined to be voids, and points where these exist continuously in the scale are determined to be cracks in the scale.

[0054] For each observation sample, the surface layer on the observation surface was evaluated in a range of 100 μm in length parallel to the rolling direction, and the measurement step for crystal orientation analysis by EBSD method and element mapping by EPMA was 0.3 μm. The thickness of the scale and each layer in the scale was determined by drawing five lines in a direction perpendicular to the plate surface of each observation sample, evaluating the length of the line segment corresponding to the scale and the Si-enriched layer on each line, and taking the simple average of the values ​​on the five lines to determine the thickness of the Si-enriched layer for that sample. Similarly, the difference between the maximum and minimum values ​​of the scale thickness measured at five locations was calculated, and this difference was divided by the average value of the scale thickness at the five locations to determine the deviation of the scale thickness. The average value of the scale thickness at the five locations was determined to be the average thickness of the scale.

[0055] The thick steel plate according to the embodiment of the present invention may have any thickness that allows the application of laser cutting, and may have a plate thickness of, for example, 6 to 40 mm, without being particularly limited. The plate thickness may be, for example, 8 mm or more, 10 mm or more, 15 mm or more, or 20 mm or more. Similarly, the plate thickness may be, for example, 35 mm or less, 30 mm or less, or 25 mm or less.

[0056] Next, a method for manufacturing a steel plate according to an embodiment of the present invention will be described below in the order of steps. The following description is an example of a characteristic method for manufacturing a steel plate according to an embodiment of the present invention, and is not intended to limit the steel plate to one manufactured by the manufacturing method described below.

[0057] The method for manufacturing a thick steel plate according to an embodiment of the present invention includes: A step of heating the slab, the step being to heat the slab to a temperature where the surface temperature of the slab is 1180°C to 1300°C and hold the temperature for 40 to 240 minutes; a hot rolling step of hot rolling the slab, the hot rolling step being performed at a rolling completion temperature of 1050°C to (T0-30)°C and a cumulative rolling reduction of 15 to 30%, followed by performing high-pressure water descaling in a temperature range of 1000°C to (T0-30)°C, and then performing rolling two or more times in which the rolling reduction in one pass is 30% or less compared to the plate thickness before rolling in each pass, controlling the interpass time of the rolling after the high-pressure water descaling to satisfy the following formula (2), and setting the rolling completion temperature in the final rolling pass to 850°C or more; A step of cooling the obtained steel sheet, in which the elapsed time from the completion of the hot rolling step to the start of water cooling is controlled so as to satisfy the following formula (3), and the water cooling stop temperature is set to 550 to 650 ° C. The present invention is characterized in that it includes: T0 is the temperature calculated by the following formula (1). T0=1175-8.4[Mn]-135[P] 0.5 -52[Al]-24[Cr]...Formula (1) [Mn], [P], [Al] and [Cr] are the contents [mass%] of each element in the slab. y n ≦1.00...Equation (2) y m =y m-1 ·exp[E1·k m-1 ·exp{E2·(J m-1 +J m )}]+E3·R m ·exp(E4·J m ) y0=0.00 y m is an index showing the degree of cracking in the scale that occurs in the mth rolling out of a total of n rolling steps performed from after high-pressure water descaling to the completion of rolling, E1, E2, E3 and E4 are constants, each of which is −2.57 × 10 -10 , -1.02×10 -2 , 2.70×10 1 and -8.33 × 10 -3 and k m is the elapsed time [seconds] from the mth rolling to the (m+1)th rolling, J m is the rolling temperature of the material at the mth rolling step [℃], R m is the reduction ratio [%] of the thickness before rolling in the mth rolling pass, y n is obtained by calculating y1, y2, y3, etc., in that order using the above formula. 1.0≦z 10 ≦10.0...Equation (3) z1=F1·exp{F2 / (H1-F3)}·(-H1 2 +F4H1+F5) 0.5 Δp 0.5 p n =z n 2 Formula 1 -2 ·exp{2·F2 / (H1-F3)}·(-H n+1 2 +F4H n+1 +F5) -1 z n =F1·exp{F2 / (H n -F3)}·(-H n 2 +F4H n +F5) 0.5 ·(p n-1 +Δp) 0.5 z n is an index showing the degree of scale growth after the elapsed time from the end of the hot rolling process to the start of water cooling is divided into 10 equal parts during the cooling process, and n indicates that the calculation corresponds to the nth of the 10 equal parts. F1, F2, F3, F4 and F5 are constants, each equal to 1.63 × 10 -6 , -2.50×10 2 , 3.25×10 2 , 2.94×10 2 and 1.36×10 6 and H n is the average steel plate temperature [℃] in the nth region of the 10 equal divisions, Δp is one tenth of the elapsed time [seconds], z 10 is obtained by calculating z1, z2, z3, etc., in that order using the above formula.

[0058] [Casting process] The manufacturing method of the slab applied to the thick steel plate according to the embodiment of the present invention is not particularly specified, and it can be manufactured by, for example, a continuous casting method or a blooming method. In addition, for the purpose of stabilizing the laser cuttability and improving the appearance of the product, the surface of the slab after casting may be ground to remove the scale and the steel plate / scale interface.

[0059] [Heating process] In order to perform hot rolling, the manufactured slab is heated to a temperature at which the surface temperature of the slab is 1180°C to 1300°C, and is subjected to a heat treatment in which the surface temperature is held for 40 to 240 minutes. This heat treatment causes the fayalite in the scale on the surface of the slab to settle to the steel sheet / scale interface, forming a Si-enriched layer at the steel sheet / scale interface, and forming Ni segregation regions at the steel sheet / scale interface or at grain boundaries near the surface of the steel sheet. If the heating temperature is below 1180°C or the holding time is less than 40 minutes, the desired Si-enriched layer and / or Ni segregation region cannot be obtained. On the other hand, if the heating temperature exceeds 1300°C, the scale grows inhomogeneously, and the scale cannot be sufficiently removed in the descaling after heating, so that the scale remains on the Si-enriched layer, and the thickness of the scale becomes inhomogeneous, deteriorating the laser cuttability. Furthermore, if the holding time exceeds 240 minutes, the scale becomes thick, and the scale cannot be completely removed by descaling after heating, and the thickness of the scale becomes non-uniform, deteriorating the laser cuttability, as in the case of a heating temperature exceeding 1300° C. The heating temperature is preferably 1200 to 1280° C., more preferably 1220 to 1260° C. Furthermore, the holding time is preferably 60 to 180 minutes, more preferably 90 to 150 minutes.

[0060] [Hot rolling process] On the surface of the slab that has been subjected to the heat treatment, there is a heterogeneous scale that is easily peeled off. Therefore, by performing hot rolling and descaling with high pressure water to remove the heterogeneous scale that has grown on the Si-enriched layer and exposing the Si-enriched layer on the surface of the steel plate, the subsequent scale formation behavior can be homogenized, and then by performing appropriate rolling and cooling treatment, the scale structure in the thick steel plate according to the embodiment of the present invention can be obtained.

[0061] In order to sufficiently remove the scale by descaling, hot rolling is performed prior to descaling to crush the scale that has grown on the Si-enriched layer. The rolling prior to descaling is performed once or multiple times at a rolling completion temperature in the range of 1050°C to (T0-30)°C, and the rolling reduction is a cumulative 15 to 30% relative to the slab thickness. In other words, when rolling prior to descaling is performed multiple times, the cumulative rolling reduction calculated based on the plate thickness after the multiple rolling times is 15 to 30% relative to the slab thickness. Note that T0 is the temperature that is an index at which fayalite starts to settle inside the scale, and is the temperature calculated by the following formula (1). T0=1175-8.4[Mn]-135[P] 0.5 -52[Al]-24[Cr]...Formula (1) Here, [Mn], [P], [Al] and [Cr] are the contents [mass%] of each element in the slab.

[0062] If the rolling completion temperature before descaling is below 1050°C, the Si-enriched layer is crushed together with the scale above it, and the Si-enriched layer is removed by descaling, degrading laser cuttability. On the other hand, if the rolling completion temperature before descaling is above (T0-30)°C, the adhesion between the Si-enriched layer and the scale growing on it is high, the scale is not crushed sufficiently, the degree to which the scale remains after descaling becomes inhomogeneous, and the subsequent scale formation behavior becomes inhomogeneous, degrading laser cuttability.

[0063] In addition, if the cumulative reduction rate of the hot rolling is less than 15%, the scale is not crushed sufficiently, the scale remains inhomogeneous after descaling, and the subsequent scale formation behavior becomes inhomogeneous, deteriorating the laser cuttability. On the other hand, if the cumulative reduction rate of the hot rolling exceeds 30%, the Si-enriched layer is crushed, the Si-enriched layer is removed by descaling, and the laser cuttability is deteriorated. In order to suppress the crushing of the Si-enriched layer, the cumulative reduction rate of the hot rolling is preferably 25% or less.

[0064] After the hot rolling, the obtained rolled material is subjected to descaling with high pressure water. Descaling can be performed, for example, using high pressure water with a collision pressure of 10 to 15 MPa. Here, if the temperature at which high pressure water descaling is performed is below 1000°C, some of the scale that has grown inhomogeneously remains, and the subsequent formation of scale becomes inhomogeneous. On the other hand, if the temperature at which high pressure water descaling is performed exceeds (T0-30)°C, some of the Si-enriched layer is peeled off by high pressure water descaling, and as a result, the desired average thickness of the Si-enriched layer cannot be obtained. From the above viewpoint, the temperature at which high pressure water descaling is performed after the hot rolling is limited to the range of 1000°C to (T0-30)°C.

[0065] After the descaling, the surface layer of the steel sheet is mainly covered with a Si-enriched layer. In order to make the steel sheet have a thickness appropriate for the application, the steel sheet is rolled. However, if the reduction rate per pass of the rolling exceeds 30%, large cracks are generated in the scale formed, impairing the laser cuttability, so the reduction rate per pass is limited to 30% or less. The smaller the reduction rate per pass, the smaller the cracks formed in the scale. From this viewpoint, it is preferable to limit the reduction rate per pass to 25% or less, and more preferably to 20% or less. On the other hand, if the reduction rate is excessively small in all rolling, the number of rolling passes required to obtain a plate thickness appropriate for the application increases, the temperature at which the rolling is performed decreases, and the rolling completion temperature decreases excessively, so it is preferable to set the average reduction rate in the rolling after high-pressure water descaling to 10% or more.

[0066] By setting the reduction rate per rolling pass to 30% or less, the size of cracks occurring in the formed scale can be suppressed, but continuous rolling causes the cracks to grow and impairs laser cuttability. Therefore, when performing continuous rolling, by leaving a sufficient elapsed time between rolling passes, the growth of the scale is promoted and the formed cracks are filled, thereby suppressing the formation of large cracks and improving laser cuttability. From the above viewpoints, in the rolling performed after the high-pressure water descaling, rolling is performed so that the interpass time between rolling passes satisfies the following formula (2).

[0067] After the high-pressure water descaling, in order to prevent a portion of the Si-enriched layer from being crushed by the rolling and being incorporated into the scale and remaining in the scale, high-pressure water descaling may be performed once or more times during the continuous rolling to remove excess scale. y n ≦1.00...Equation (2) y m =y m-1 ·exp[E1·k m-1 ·exp{E2·(J m-1 +J m )}]+E3·R m ·exp(E4·J m ) y0=0.00

[0068] y m is an index showing the degree of cracking in the scale that occurs in the mth rolling out of the total n rollings performed from after high-pressure water descaling to the completion of rolling. By successively calculating y1, y2, y3, etc. according to the above formula, the degree of cracking at the completion of rolling can be calculated. n You can get y n If is large, the crack in the scale will become large, so as shown in the above formula (2), y n Limit the value of y to 1.00 or less. To reduce the cracks in the scale, n The value of k is preferably 0.70 or less, and more preferably 0.50 or less. m is the elapsed time from the mth rolling to the (m+1)th rolling [seconds], and J m is the rolling temperature [℃] at the mth rolling, and R m is the reduction ratio [%] of the thickness before the mth rolling in the mth rolling. E1, E2, E3, and E4 are constants, each of which is -2.57×10 -10 , -1.02×10 -2 , 2.70×10 1 and -8.33 × 10 -3 It is.

[0069] The rolling completion temperature in the final rolling pass after high-pressure water descaling is 850°C or higher. If rolling is performed at a temperature below 850°C, some of the scale will peel off, and the peeled scale will be pushed in, making the scale thickness non-uniform and impairing laser cuttability. The rolling completion temperature is preferably 875°C or higher, and more preferably 900°C or higher. There is no particular upper limit, but for example, the rolling completion temperature in the final rolling pass may be 1000°C or lower.

[0070] [Cooling process] In order to control the time elapsed from the completion of the hot rolling process to the start of water cooling and reduce the size of the cracks formed inside the scale, the time elapsed from the completion of the hot rolling process to the start of water cooling is managed by formula (3). Here, if the time elapsed from the completion of the hot rolling process to the start of water cooling is too short, z 10 If z is less than 1.0, the growth of the scale is excessively suppressed, and the laser cutting ability is impaired. 10 On the other hand, if the time from the end of the hot rolling process to the start of water cooling is too long, z 10 If z exceeds 10.0, excessive oxygen is supplied to the scale, and some cracks become coarser. 10 z should be 10.0 or less. To improve the structure of the scale and the laser cutting properties, 10 is preferably 2.0 or more and 8.0 or less, and more preferably 3.0 or more and 7.0 or less. 1.0≦z 10 ≦10.0...Equation (3) Here, z n is calculated as follows: z1=F1·exp{F2 / (H1-F3)}·(-H1 2 +F4H1+F5) 0.5 Δp 0.5 p n =z n 2 Formula 1 -2 ·exp{2·F2 / (H1-F3)}·(-H n+1 2 +F4H n+1 +F5)-1 z n =F1·exp{F2 / (H n -F3)}·(-H n 2 +F4H n +F5) 0.5 ·(p n-1 +Δp) 0.5

[0071] These calculations were carried out by dividing the time elapsed from the end of the hot rolling process to the start of water cooling into 10 equal parts, and calculating the degree of scale growth (z n ), where the subscript n indicates that the calculation is the nth of 10 equal intervals. F1, F2, F3, F4, and F5 are constants, each of which is 1.63 × 10 -6 , -2.50×10 2 , 3.25×10 2 , 2.94×10 2 and 1.36×10 6 It is. n is the average steel sheet temperature [°C] in the nth region of the 10 equal sections, that is, the arithmetic average of the temperature measurements at each predetermined time in the entire nth region. Δp is one-tenth of the elapsed time [seconds]. 10 is obtained by calculating z1, z2, z3, etc., in that order using the above formula.

[0072] Water cooling is stopped when the steel plate temperature reaches 550-650°C. If the water cooling stop temperature is too high, the scale grows non-uniformly, resulting in an inhomogeneous thickness of the scale and poor laser cuttability. On the other hand, if the water cooling stop temperature is too low, thermal stress causes cracks in the scale during water cooling, impairing laser cuttability. For this reason, the water cooling stop temperature is set to 550-650°C.

[0073] Regarding the cooling conditions of the steel plate after completion of water cooling, it is preferable to naturally cool or air-cool the steel plate, since excessive heat retention after water cooling may impair the toughness of the steel plate. Alternatively, the steel plate after water cooling or during water cooling may be wound into a coil shape, and further water-cooled, air-cooled, and / or naturally cooled after satisfying the characteristics of the manufacturing method described above. Furthermore, after completion of cooling of the steel plate, a tempering treatment may be performed within a range that does not impair the characteristics of the thick steel plate according to the embodiment of the present invention.

[0074] Furthermore, in addition to the above-mentioned heating step, hot rolling step, and cooling step, a flattening step using a hot leveler or the like may be further included.

[0075] The thick steel plate manufactured as described above includes a steel plate and a scale formed on the surface of the steel plate, and further includes a Si-enriched layer formed at the interface between the steel plate and the scale, the average thickness of the Si-enriched layer being 1.0 μm or more, a Ni segregated region having a length of 2.0 μm or more is present along at least a part of the interface between the steel plate and the scale or along at least a part of the grain boundary near the surface of the steel plate, the Ni concentration in the Ni segregated region is 2.0 times or more the average Ni concentration in the steel plate (base steel), and the scale thickness deviation is 0.70 or less. Therefore, irregular peeling of the scale during laser irradiation in a laser cutting operation can be suppressed or prevented, and cutting into any shape can be stably proceeded, and the plate can be used for structures such as construction, architecture, industrial machinery, and bridges.

[0076] The present invention will be described in more detail below with reference to examples. The following conditions are examples of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to these example conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention. EXAMPLES

[0077] Steel plates according to the embodiment of the present invention were manufactured under various conditions, and the degree of scale spalling and laser cuttability when the obtained steel plates were irradiated with a laser were examined.

[0078] First, a slab having the chemical composition shown in Table 1 was used, and a heating process, a hot rolling process, and a cooling process were carried out under the conditions shown in Table 2 to obtain thick steel plates as experimental examples, including examples of the present invention and comparative examples.

[0079] [Table 1-1]

[0080] [Table 1-2]

[0081] [Table 2]

[0082] [Evaluation of scale adhesion] The scale adhesion of the obtained thick steel plate was evaluated by a test simulating the state of laser irradiation on the thick steel plate. First, a thick steel plate containing scale on the surface was cut into 100 mm x 100 mm, and the center of the surface of the thick steel plate kept at room temperature (20 to 30 ° C) was irradiated with a laser over a length of 10 mm under the following conditions. A 1 mm long area in the center of the laser irradiation mark on the surface was observed with an optical microscope to evaluate the degree of scale peeling in the same area. When the area ratio of scale peeling in the area by one irradiation exceeded 30%, it was marked as "X", when it was more than 5% and 30% or less, it was marked as "○", and when it was 5% or less, it was marked as "◎". A thick steel plate that obtained "○" or "◎" was judged to be a thick steel plate with excellent scale adhesion and in which scale peeling during laser irradiation was suppressed or prevented, and was judged to have passed. The results are shown in Table 3. Laser power: 500W Pulse frequency: 60kHz Focus diameter: 0.70mm Irradiation speed: 3m / sec

[0083] [Laser cuttability evaluation] The laser cuttability was evaluated based on the measurement results of the scar roughness of the cut surface. The inventors' study has revealed that defects such as notches and burning that occur during laser cutting are likely to occur when the scar roughness exceeds the limit scar roughness (Ram) shown in formula (4). In other words, the risk of defect occurrence can be quantitatively evaluated by comparing the limit scar roughness with the scar roughness of the evaluation target. The scar roughness was measured by measuring the roughness Ra (arithmetic mean roughness) at a position 0.5 mm from the surface layer on the laser incidence side in a 5 mm central area of ​​the four laser cut surfaces of the measurement sample using a digital microscope (manufactured by Hirox Co., Ltd.), and the average value of the roughness of these four surfaces was taken as the scar roughness (Ra). The average scar roughness Ra (μm) of the cut surface of the steel plate was measured, and if it satisfied formula (5), the laser cuttability was evaluated as "good", and if it did not, it was evaluated as "x". Ram = -0.34×t + 17.2 (4) Ra < Ram (5)

[0084] [Table 3]

[0085] Among the experimental examples listed in Tables 1 to 3, experimental example 30 is a comparative example in which the heating temperature of the slab in the heating process was low, and a sufficient Si-enriched layer and Ni segregated region were not obtained, resulting in poor scale adhesion and insufficient laser cuttability. In Experimental Example 31, the heating temperature of the slab in the heating process was high, the thickness of the scale was thick, and the thickness deviation was large. Therefore, the scale adhesion was poor, and sufficient laser cuttability was not obtained. Experimental Example 32 is a comparative example in which the heating time in the heating step was short, so that a sufficient Si-enriched layer was not obtained at the steel sheet / scale interface, resulting in poor scale adhesion and insufficient laser cuttability. In Experimental Example 33, the heating time in the heating step was long, the scale thickness was thick, and as a result, the thickness deviation was large. Therefore, this is a comparative example in which the scale adhesion was poor and sufficient laser cuttability was not obtained. Experimental Example 34 is a comparative example in which the rolling completion temperature before descaling was low, and a sufficient Si-enriched layer was not obtained at the scale / steel sheet interface, resulting in poor scale adhesion and insufficient laser cuttability. In Experimental Example 35, the rolling completion temperature before descaling was high, and the scale adhesion was high, but the scale could not be sufficiently crushed by descaling, and the scale thickness deviation became large. Therefore, this is a comparative example in which the scale adhesion was inferior and sufficient laser cuttability was not obtained. In Experimental Example 36, the cumulative reduction ratio of the rolling prior to descaling was small, and the scale could not be sufficiently crushed by descaling, resulting in a large deviation in scale thickness. As a result, the scale adhesion was poor, and sufficient laser cuttability was not obtained. In Experimental Example 37, the cumulative reduction ratio of the rolling prior to descaling was large, and the Si-enriched layer was pulverized, so that a sufficient Si-enriched layer was not obtained. As a result, the scale adhesion was inferior, and sufficient laser cuttability was not obtained. In Experimental Example 38, the descaling temperature was low, some unevenly grown scale remained, and the scale thickness deviation became large. As a result, the scale adhesion was poor and sufficient laser cuttability was not obtained. In Experimental Example 39, the descaling temperature was high, and part of the Si-enriched layer peeled off due to descaling. As a result, the desired average thickness of the Si-enriched layer was not obtained, the scale adhesion was poor, and sufficient laser cuttability was not obtained. Example 40 is a comparative example in which the maximum reduction ratio in rolling after descaling was large, causing some of the scale to peel off from the steel sheet during rolling, large cracks exceeding 20 μm to occur in the scale, and resulting in poor laser cuttability. Experimental Example 41 is a comparative example in which the time between rolling passes after descaling was short, and formula (2) was not satisfied. In this case, the scale became slightly thicker, and cracks of more than 20 μm occurred at the interface between the scale and the steel sheet, resulting in poor laser cuttability. In Experimental Example 42, the rolling completion temperature in the final rolling pass was low, and part of the scale peeled off and was pushed in, resulting in a large deviation in scale thickness. This resulted in poor scale adhesion, and insufficient laser cuttability. Experimental Example 43 is a comparative example in which the time that elapsed from the completion of the hot rolling process to the start of water cooling was long, and formula (3) was not satisfied. In this case, excessive oxygen was supplied to the scale, the scale became slightly thicker, and cracks exceeding 20 μm were generated at the interface between the scale and the steel sheet, resulting in poor laser cuttability. Experimental Example 44 is a comparative example in which the water-cooling stop temperature was low, and cracks that occurred during cooling were not sufficiently repaired, and cracks of more than 20 μm were generated at the interface between the scale and the steel plate due to thermal stress during water cooling, resulting in inferior laser cuttability. Experimental Example 45 is a comparative example in which the water cooling stop temperature was high, the scale grew non-uniformly, and the deviation in scale thickness was large. As a result, the scale adhesion was poor, and sufficient laser cuttability was not obtained.

[0086] The experimental examples excluding the above comparative examples, i.e., experimental examples 1 to 29, are examples of the present invention, and steel sheets were obtained that had excellent scale adhesion, and in which scale spalling during laser irradiation was suppressed or prevented, and therefore had excellent laser cuttability. In particular, in examples 1 to 24 of the present invention, in which the average thickness of the scale was controlled to 20 to 70 μm, the degree of scale spalling was 5% or less in terms of area ratio, and particularly excellent scale adhesion was achieved. Furthermore, in many of the examples of the present invention, the length of the cracks present near the interface between the steel sheet and the scale was 5 μm or less.

Claims

1. A steel plate and a scale formed on a surface of the steel plate, The steel sheet further includes a Si-enriched layer formed at an interface between the steel sheet and the scale, The average thickness of the Si-enriched layer is 1.0 μm or more, a Ni segregation region having a length of 2.0 μm or more is present along at least a part of the interface between the steel sheet and the scale or at least a part of the grain boundary in the vicinity of the surface of the steel sheet, The Ni concentration in the Ni segregation region is 2.0 times or more the average Ni concentration in the steel plate, The scale thickness deviation is 0.70 or less, A thick steel plate, wherein the length of a crack present in the vicinity of the interface between the steel plate and the scale is 20 μm or less.

2. The steel plate according to claim 1, wherein the average thickness of the scale is 20 to 70 μm.

3. The steel plate comprises, in mass%, C: 0.02-0.30%, Si: 0.15-1.20%, Mn: 0.30-2.20%, P: 0.003-0.060%, S: 0.010% or less, Ni: 0.05-1.50%, Al: 0.001-0.100%, N: 0.010% or less, O: 0.0035% or less, Cu: 0 to 1.00%, Cr: 0-1.00%, Mo: 0-1.00%, W: 0-0.50%, Nb: 0 to 0.500%, Ti: 0 to 0.500%, V: 0-1.000%, B: 0 to 0.0100%, Sn: 0-0.500%, Sb: 0 to 0.500%, Ca: 0-0.0100%, Mg: 0 to 0.0100%, Hf: 0-0.0100%, Te: 0 to 0.0100%, Sr: 0 to 0.0100%, REM: 0 to 0.0100%, and The steel plate according to claim 1 or 2, having a chemical composition consisting of the balance being Fe and impurities.

4. The chemical composition, in mass%, Cu: 0.01 to 1.00%, Cr: 0.01-1.00%, Mo: 0.01-1.00%, W: 0.003-0.50%, Nb: 0.003 to 0.500%, Ti: 0.003 to 0.500%, V: 0.003-1.000%, B: 0.0003 to 0.0100%, Sn: 0.003 to 0.500%, Sb: 0.003 to 0.500%, Ca: 0.0003-0.0100%, Mg: 0.0003 to 0.0100%, Hf: 0.0003-0.0100%, Te: 0.0003 to 0.0100%, Sr: 0.0003 to 0.0100%, and REM: 0.0003-0.0100% The steel plate according to claim 3, comprising one or more selected from the group consisting of:

5. A step of heating the slab to a temperature where the surface temperature of the slab is 1180°C to 1300°C and held for 40 to 240 minutes; A process for hot rolling the slab, the rolling completion temperature being 1050° C. to (T 0 -30) ° C., and a cumulative rolling reduction of 15 to 30% is applied, followed by rolling at 1000 ° C. to (T 0a hot rolling process in which high-pressure water descaling is performed at a temperature range of −30° C., followed by rolling two or more times with a rolling reduction rate in one pass of 30% or less compared to the plate thickness before rolling in each pass, the interpass time of the rolling after the high-pressure water descaling is controlled to satisfy the following formula (2), and the rolling completion temperature in the final rolling pass is 850° C. or more; A step of cooling the obtained steel sheet, in which the elapsed time from the completion of the hot rolling step to the start of water cooling is controlled so as to satisfy the following formula (3), and the water cooling stop temperature is set to 550 to 650 ° C. The method for producing a steel plate according to claim 1 or 2, comprising: T 0 is the temperature calculated by the following formula (1). T 0 =1175-8.4[Mn]-135[P] 0.5 -52[Al]-24[Cr]...Formula (1) [Mn], [P], [Al] and [Cr] are the contents [mass %] of each element in the slab. y n ≦1.00...Formula (2) y m = y m-1 ・exp [E 1 ・k m-1 ・exp{E 2 ・(J m-1 +J m )}]+E 3 ・R m ・exp(E 4 J m ) y 0 = 0.00 y m is an index representing the degree of cracking in the scale occurring in the mth rolling out of a total of n rollings performed from after high-pressure water descaling to the completion of rolling, E 1 , E 2 , E 3 and E 4 are constants, and −2.57×10 -10 , −1.02×10 -2 , 2.70×10 1 and -8.33 x 10 -3 and k m is the elapsed time [seconds] from the mth rolling to the (m+1)th rolling, J m is the rolling material temperature [°C] at the mth rolling, R m is the reduction ratio [%] of the plate thickness before rolling in the mth rolling, y n is expressed by the above formula: 1 From y 2 , y 3 This can be obtained by calculating in this order. 1.0≦z 10 ≦10.0...Formula (3) Z 1 = F 1 ・exp{F 2 / (H 1 -F 3 ))・(-H 1 2 +F 4 H 1 +F 5 ) 0.5 Δp 0.5 p n = z n 2 ・F 1 -2 ・exp{2・F 2 / (H 1 -F 3 ))・(-H n+1 2 +F 4 H n+1 +F 5 ) -1 Z n = F 1 ・exp{F 2 / (H n -F 3)}・(-H n 2 +F 4 H n +F 5 ) 0.5 ・(p n-1 +Δp) 0.5 Z nis an index representing the degree of growth of scale after each section is completed by dividing the elapsed time from the completion of the hot rolling process to the start of water cooling into 10 equal sections in the cooling process, and n indicates that the calculation corresponds to the nth section out of the 10 equal sections. F 1 , F 2 , F 3 , F 4 and F 5 are constants, 1.63 × 10 -6 , −2.50×10 2 , 3.25×10 2 , 2.94×10 2 and 1.36 x 10 6 and H n is the average steel sheet temperature [°C] in the n-th region of the 10 equally divided sections, Δp is one tenth of the elapsed time [seconds], Z 10 is calculated by the above formula: 1 From Z 2 , z 3 This can be obtained by calculating in this order.

Citation Information

Patent Citations

  • Method for improving surface quality of silicon-containing steel

    CN106399856A

  • Steel material excellent in high density energy line cutting property and its production

    JP1997078180A

  • Wire rod excellent in cutting property with high density energy beam and its production

    JP1998251805A

  • Steel sheet excellent in surface properties, and method for producing the same

    JP2013082979A

  • Steel material, steel structure for burying underground and manufacturing method of steel material

    JP2016166388A