Method for manufacturing circuit board
A resin sheet with controlled water vapor permeability and thermal curing conditions addresses adhesion issues in circuit boards with high inorganic filler content, ensuring effective adhesion and dielectric properties in thin layers.
Patent Information
- Application Number
- JP2023045599
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
The adhesion between insulating layers and conductor layers in circuit boards deteriorates when using resin compositions with high inorganic filler content and a thickness of 15 μm or less, which is necessary for good dielectric properties and low thermal expansion.
A manufacturing method involving a resin sheet with a support having a specific water vapor permeability coefficient, thermally curing the resin composition layer under controlled temperature conditions, and peeling off the support to form an insulating layer with good adhesion to the conductor layer.
The method ensures good adhesion between the insulating and conductor layers, maintaining dielectric properties and low thermal expansion while reducing surface roughness, even with high inorganic filler content in thin resin composition layers.
Smart Images

Figure 2024135084000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a circuit board. [Background technology]
[0002] Resin compositions containing a thermosetting resin and its curing agent produce cured products that have excellent insulation properties, heat resistance, adhesion, and other properties, and therefore have been widely used as insulating materials for circuit boards, such as printed wiring boards and rewiring boards for semiconductor packages.
[0003] On the other hand, with the recent increase in communication speed, insulating materials for circuit boards are required to have excellent dielectric properties (low dielectric tangent) in order to reduce transmission loss when operating in a high-frequency environment. In addition, insulating materials with a low thermal expansion coefficient are required to suppress the occurrence of cracks and circuit distortion due to the difference in thermal expansion between the insulating layer and the conductor layer in the circuit board, or to suppress the occurrence of warping when forming a large-area insulating layer in the manufacture of circuit boards such as wafer level packages (WLPs) and panel level packages (PLPs). As insulating materials that exhibit good dielectric properties and a low thermal expansion coefficient, resin compositions containing a high content of inorganic fillers such as silica particles are known (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2022-93188 A Summary of the Invention [Problem to be solved by the invention]
[0005] As a manufacturing technique for circuit boards, a manufacturing method using a build-up method in which insulating layers and conductor layers (circuit layers) are alternately stacked is known. In the manufacturing method using the build-up method, a resin composition layer is generally laminated on a substrate using a resin sheet or the like, and the resin composition layer is cured to form an insulating layer. Thereafter, the insulating layer is roughened (desmeared) and subjected to a plating process to provide a conductor layer and form a wiring pattern.
[0006] The present inventors have found that when an insulating layer is formed using a resin composition with a high content of inorganic filler in order to achieve good dielectric properties and a low coefficient of thermal expansion, if a thin resin composition layer is used to reduce the height of a circuit board, sufficient adhesion between the insulating layer and the conductor layer may not be obtained. In particular, it has been confirmed that when a thin resin composition layer with a thickness of 15 μm or less contains a high content of inorganic filler, the adhesion between the insulating layer and the conductor layer is significantly deteriorated.
[0007] The present invention aims to provide a novel technology that can provide a circuit board having an insulating layer that has good adhesion to a conductor layer, even when the insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content. [Means for solving the problem]
[0008] As a result of extensive investigations into the above problems, the present inventors have found that the above problems can be solved by a method for manufacturing a circuit board having the following configuration, and have thus completed the present invention.
[0009] That is, the present invention includes the following. <1> (I) a step of laminating a resin sheet including a support and a resin composition layer provided on the support, the resin composition layer having an inorganic filler content of 60% by mass or more and a thickness of 15 μm or less, on a substrate such that the resin composition layer is bonded to the substrate; (II) a step of thermally curing the resin composition layer to form an insulating layer; and (III) peeling off the support; A method for manufacturing a circuit board, comprising the steps of: The water vapor permeability coefficient of the support, calculated from the water vapor permeability of the support measured under conditions of a temperature of 40°C and a relative humidity difference of 90% using a method in accordance with JIS K7129, is 0.5 g / m 2 mm -1 - 24 hours or less, The method, in the step (II), wherein the resin composition layer is subjected to a heat treatment in which it is maintained at a temperature T1, and then subjected to a heat treatment in which it is maintained at a temperature T2 higher than the temperature T1. <2> Temperature T2 is 150°C or higher; <1> The method according to <3> The difference between temperature T1 and temperature T2 (T2-T1) is 20°C or more. <1> or <2> The method according to <4> Temperature T1 is 50°C or higher; <1> ~ <3> 13. The method according to claim 12, wherein <5> In step (II), the resin composition layer is heated to a temperature T2 at a heating rate of 0.5° C. / min or more and 30° C. / min or less. <1> ~ <4> 13. The method according to claim 12, wherein <6> The resin composition layer contains a thermosetting resin; <1> ~ <5> 13. The method according to claim 12, wherein <7> The resin composition layer contains one or more curing agents selected from the group consisting of active ester-based curing agents, phenol-based curing agents, naphthol-based curing agents, and carbodiimide-based curing agents. <1> ~ <6> 13. The method according to claim 12, wherein <8> Further comprising the step of forming a via hole in the insulating layer by a laser. <1> ~ <7> 13. The method according to claim 12, wherein <9> Further comprising a step of forming a conductor layer on a surface of the insulating layer. <1> ~ <8> 13. The method according to claim 12, wherein <10> The peel strength between the insulating layer and the conductor layer is 0.3 kgf / cm or more. <9> The method according to Effect of the Invention
[0010] According to the present invention, a novel technique can be provided that can provide a circuit board having an insulating layer that has good adhesion to a conductor layer, even when the insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Before describing the method for producing a circuit board of the present invention in detail, the resin sheet used in the method will be described.
[0012] <Resin sheet> In the method for producing a circuit board of the present invention, a resin sheet is used that includes a support and a resin composition layer that is provided on the support and has an inorganic filler content of 60% by mass or more and a thickness of 15 μm or less. The resin sheet has a water vapor permeability coefficient of the support that is calculated from the water vapor permeability of the support measured under conditions of a temperature of 40° C. and a relative humidity difference of 90% by a method conforming to JIS K7129, and is 0.5 g / m 2 mm -1 - It is characterized by being 24 hours or less.
[0013] Hereinafter, preferred embodiments of the present invention will be described from the viewpoint of obtaining the effects of the present invention more effectively.
[0014] -Support- The inventors have discovered that even when an insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content, in order to obtain an insulating layer with good adhesion to a conductor layer, it is important to use a resin sheet having a support whose water vapor permeability coefficient is a certain value or less.
[0015] In detail, the water vapor permeability (g / m) of the support measured under conditions of a temperature of 40°C and a relative humidity difference of 90% according to a method in accordance with JIS K7129. 2 The water vapor permeability coefficient (g / m2) of the support is calculated by multiplying the thickness (mm) of the support by the water vapor permeability coefficient (g / m2) of the support. 2 mm -1 24h) is 0.5g / m 2 mm-1 Even when an insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content, from the viewpoint of providing an insulating layer having better adhesion to a conductor layer and further providing an insulating layer having a low surface roughness after roughening treatment (desmear treatment), the water vapor permeability coefficient of the support is preferably 0.45 g / m 2 mm -1 24 hours or less, preferably 0.4g / m 2 mm -1 24 hours or less, preferably 0.35 g / m 2 mm -1 ·24 hours or less, 0.3g / m 2 mm -1 ·24 hours or less, 0.28g / m 2 mm -1 ·24 hours or less, 0.26g / m 2 mm -1 ·24h or less, 0.24g / m 2 mm -1 ·24 hours or less, 0.22g / m 2 mm -1 24 hours or less, or 0.2g / m 2 mm -1 The lower limit of the water vapor permeability coefficient is not particularly limited, and is, for example, 0.05 g / m 2 mm -1 ·Over 24 hours, 0.06g / m 2 mm -1 ·Over 24 hours, 0.08g / m 2 mm -1 ·Over 24 hours, 0.1g / m 2 mm -1 It may be 24 hours or more.
[0016] Examples of a support that satisfies such a water vapor permeability coefficient include: (1) a support having a water vapor permeability coefficient of 0.5 g / m 2 mm -1 (2) A base film having a release layer for an overall weight of 0.5 g / m 2 mm -1(3) A base film with a release layer that has a water vapor permeability coefficient of 0.5 g / m2 or less for 24 hours. 2 mm -1 (4) A base film with a barrier layer that has a water vapor transmission coefficient of 0.5 g / m2 as a whole by providing a barrier layer on the side opposite the release layer of the base film with a release layer. 2 mm -1 Supports having a layer structure of release layer / base film / barrier layer that have a water vapor transmission coefficient of 24h or less are examples of such supports.
[0017] Examples of the base film used as the support include a thermoplastic resin film, a metal foil, and a release paper, with a thermoplastic resin film and a metal foil being preferred, and a thermoplastic film (including one having a barrier layer) being particularly preferred. When forming a via hole in an insulating layer with a laser or the like, it is desirable to form the via hole with a support in order to reduce damage to the insulating layer surface, but when a thermoplastic film is used as the support, there is no need to perform pretreatment such as blackening treatment as with metal foil, and the via hole can be easily formed with a laser.
[0018] When a thermoplastic resin film is used as the base film, examples of the thermoplastic resin include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polycarbonate (PC), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate, polyethylene naphthalate, and polyimide are preferred.
[0019] When a metal foil is used as the base film, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0020] The surface of the base film that is bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment. As the base film, as described above, a base film with a release layer having a release layer on one surface (the surface that is bonded to the resin composition layer) may be used. Examples of the release agent used in the release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The base film with a release layer may be a commercially available product, and examples thereof include "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0021] The thickness of the base film is not particularly limited as long as a support that satisfies the above water vapor permeability coefficient can be obtained, but is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 12 μm or more, 14 μm or more, or 15 μm or more, and the upper limit is preferably 75 μm or less, more preferably 60 μm or less, and even more preferably 50 μm or less. When a base film with a release layer is used, it is preferable that the thickness of the entire base film with a release layer is within the above range.
[0022] As described above, the support may have a barrier layer. By providing a barrier layer, it is possible to suppress the permeation of water vapor, and it is easy to obtain a support that satisfies the above water vapor permeability coefficient. The barrier layer is not particularly limited as long as it satisfies the above water vapor permeability coefficient together with the base film, and examples thereof include inorganic films and organic films. Examples of inorganic films include metal foils such as aluminum and copper; silica vapor deposition films; silicon nitride films; silicon oxide films; magnesium oxide films; and the like. Examples of organic films include polyvinyl alcohol films, ethylene-vinyl alcohol copolymer films, polyvinylidene chloride films, and the like. The barrier layer may have a single layer structure or a multilayer structure, and may have a multilayer structure composed of, for example, an inorganic film and an organic film.
[0023] Examples of methods for forming an inorganic film include chemical vapor deposition using heat, plasma, ultraviolet light, etc., and physical vapor deposition using deposition, sputtering, etc. Examples of methods for forming an organic film include a method in which an organic compound is applied to a substrate using a coating device such as a die coater, a comma coater, a gravure coater, or a bar coater.
[0024] The thickness of the barrier layer is not particularly limited as long as it satisfies the above water vapor permeability coefficient together with the base film, but from the viewpoint of obtaining the effects of the present invention significantly, the thickness is preferably 0.1 μm or more, more preferably 0.2 μm or more, 0.4 μm or more, or 0.5 μm or more, even more preferably 0.6 μm or more, 0.8 μm or more, or 1 μm or more, and the upper limit is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less.
[0025] The barrier layer may be bonded to the base film via an adhesive layer. The adhesive that can be used for the adhesive layer is not particularly limited as long as it can bond the base film and the barrier layer, and any adhesive may be used. Examples of such adhesives include water-based, solvent-based, hot melt-based, and active energy ray curable adhesives that can be cured by active energy rays such as ultraviolet rays.
[0026] The thickness of the adhesive layer is not particularly limited, but from the viewpoint of obtaining the effects of the present invention remarkably, it is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, even more preferably 5 μm or less.
[0027] -Resin composition layer- In the present invention, a resin composition layer having an inorganic filler content of 60% by mass or more and a thickness of 15 μm or less is used.
[0028] From the viewpoint of providing an insulating layer exhibiting good dielectric properties and a low thermal expansion coefficient, the content of the inorganic filler in the resin composition layer is 60% by mass or more when the non-volatile components in the resin composition layer are 100% by mass. As described above, the present inventors have confirmed that when an inorganic filler is highly mixed in a thin resin composition layer having a thickness of 15 μm or less, the adhesion between the insulating layer and the conductor layer is significantly deteriorated. In this regard, according to the method for producing a circuit board of the present invention in which a resin sheet having a support having a water vapor permeability coefficient in the above range is used and the resin composition layer is cured under specific conditions as described below, even when an inorganic filler is highly mixed in a thin resin composition layer having a thickness of 15 μm or less, an insulating layer having good adhesion to the conductor layer can be provided. For example, the content of the inorganic filler in the resin composition layer may be increased to 65% by mass or more, 66% by mass or more, 68% by mass or more, or 70% by mass or more. The upper limit of the content of the inorganic filler is not particularly limited, but may be, for example, 90% by mass or less, 85% by mass or less, etc.
[0029] Examples of inorganic filler materials include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum silicate, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as silica. The inorganic filler may be used alone or in combination of two or more.
[0030] Examples of commercially available inorganic fillers include "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellfiers" and "MGH-005" manufactured by Pacific Cement Corporation; and "Sferique" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.
[0031] The average particle size of the inorganic filler is not particularly limited, but is preferably 5 μm or less, more preferably 3 μm or less, or 2 μm or less, and even more preferably 1 μm or less, 0.8 μm or less, or 0.7 μm or less. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.07 μm or more, 0.1 μm or more, or 0.2 μm or more. The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0032] The specific surface area of the inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, 3m 2 / g or more or 5m 2 The upper limit of the specific surface area is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 80m 2 / g or less, more preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area of the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.
[0033] The inorganic filler is preferably surface-treated with a suitable surface treatment agent. By performing the surface treatment, the moisture resistance and dispersibility of the inorganic filler can be improved. Examples of the surface treatment agent include silane coupling agents such as vinyl silane coupling agents, epoxy silane coupling agents, styryl silane coupling agents, (meth)acrylic silane coupling agents, amino silane coupling agents, isocyanurate silane coupling agents, ureido silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, and acid anhydride silane coupling agents; alkoxysilane compounds such as methyltrimethoxysilane and phenyltrimethoxysilane; silazane compounds; and oligomers thereof. The surface treatment agent may be used alone or in combination of two or more.
[0034] -Thermosetting resin- The resin composition layer preferably contains a thermosetting resin.
[0035] Examples of the thermosetting resin include epoxy resin, benzocyclobutene resin, epoxy acrylate resin, urethane acrylate resin, urethane resin, cyanate resin, unsaturated polyester resin, melamine resin, silicone resin, etc. The thermosetting resin may be used alone or in combination of two or more kinds.
[0036] Among these, from the viewpoint of being able to provide an insulating layer having good adhesion to a conductor layer even when a high content of an inorganic filler is incorporated in a thin resin composition layer having a thickness of 15 μm or less, and further from the viewpoint of being able to provide an insulating layer having low surface roughness after roughening treatment (desmear treatment), it is preferable that the thermosetting resin contains an epoxy resin.
[0037] Examples of epoxy resins include bisphenol type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, and tetraphenylethane type epoxy resins. Bisphenol type epoxy resins refer to epoxy resins having a bisphenol structure, and examples thereof include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, and bisphenol AF type epoxy resins. Biphenyl type epoxy resin refers to an epoxy resin having a biphenyl structure, where the biphenyl structure may have a substituent such as an alkyl group, an alkoxy group, or an aryl group. Therefore, bixylenol type epoxy resin and biphenyl aralkyl type epoxy resin are also included in biphenyl type epoxy resin. The epoxy resin may be used alone or in combination of two or more kinds.
[0038] The epoxy resin is preferably an aromatic epoxy resin, where the aromatic epoxy resin means an epoxy resin having an aromatic ring in the molecule.
[0039] The epoxy resin preferably has two or more epoxy groups in one molecule. When the non-volatile component of the epoxy resin is taken as 100 mass%, the ratio of the epoxy resin having two or more epoxy groups in one molecule is preferably 50 mass% or more, more preferably 60 mass% or more, and further preferably 70 mass% or more.
[0040] Epoxy resins include epoxy resins that are liquid at a temperature of 20°C (hereinafter referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter referred to as "solid epoxy resins").
[0041] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.
[0042] Preferred liquid epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins such as alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, and epoxy resins having a butadiene structure.
[0043] Specific examples of liquid epoxy resins include "HP-4032", "HP-4032D", and "HP-4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (p-aminophenol type epoxy resins, glycidyl ether type epoxy resins) manufactured by Mitsubishi Chemical Corporation. amine type epoxy resin); "ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd. (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); "EX-721" manufactured by Nagase ChemteX Corporation (glycidyl ester type epoxy resin); "Celloxide 2021P" manufactured by Daicel Corporation (alicyclic epoxy resin with an ester skeleton); "PB-3600" manufactured by Daicel Corporation (epoxy resin with a butadiene structure); "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd., etc.
[0044] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.
[0045] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred.
[0046] Specific examples of solid epoxy resins include "HP-4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200HH", "HP-7200H", and "HP-7200" (dicyclopentadiene epoxy resins) manufactured by DIC Corporation. type epoxy resin); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", and "HP6000" (naphthylene ether type epoxy resin) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku; "NC-7000-L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku; "NC-3000-H", "NC-3000", and "NC-3000" manufactured by Nippon Kayaku 0-L, "NC-3100" (biphenyl type epoxy resin); "ESN475V" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX4000HK" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd. "YX8800" (anthracene type epoxy resin) manufactured by Osaka Gas Chemicals; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (solid bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical.
[0047] The resin composition layer may contain only liquid epoxy resin as the epoxy resin, may contain only solid epoxy resin, or may contain a combination of liquid epoxy resin and solid epoxy resin. Even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, the resin composition layer preferably contains a solid epoxy resin from the viewpoint of providing an insulating layer having good adhesion to the conductor layer. When a liquid epoxy resin and a solid epoxy resin are used in combination, the ratio of the amounts (liquid epoxy resin:solid epoxy resin) is preferably 1:0.5 to 1:50, more preferably 1:1 to 1:30, and even more preferably 1:2 to 1:20 by mass.
[0048] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 80 g / eq. to 2000 g / eq., and even more preferably 110 g / eq. to 1000 g / eq. The epoxy equivalent is the mass of an epoxy resin containing one equivalent of an epoxy group. This epoxy equivalent can be measured according to JIS K7236.
[0049] The weight average molecular weight (Mw) of the epoxy resin is preferably from 100 to 5000, more preferably from 250 to 3000, and further preferably from 400 to 1500. The Mw of the epoxy resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).
[0050] Even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, the content of the thermosetting resin in the resin composition layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, 20% by mass or more, or 25% by mass or more, when the resin component in the resin composition layer is 100% by mass. The upper limit of the content is not particularly limited and may be determined depending on the properties required for the resin composition, and may be, for example, 80% by mass or less, 70% by mass or less, 65% by mass or less, or 60% by mass or less.
[0051] In the present invention, the "resin component" in the resin composition layer refers to the non-volatile components constituting the resin composition layer, excluding the inorganic filler described below.
[0052] - Hardener - The resin composition layer preferably contains a curing agent. The curing agent usually has a function of reacting with the thermosetting resin to cure the resin composition layer.
[0053] Examples of the curing agent include active ester curing agents, phenolic curing agents, naphthol curing agents, acid anhydride curing agents, cyanate ester curing agents, carbodiimide curing agents, amine curing agents, etc. The curing agents may be used alone or in combination of two or more.
[0054] Among them, from the viewpoint of being able to provide an insulating layer having good adhesion to the conductor layer even when a thin resin composition layer having a thickness of 15 μm or less is highly blended with an inorganic filler, and from the viewpoint of being able to provide an insulating layer having low surface roughness after roughening treatment (desmear treatment), it is preferable that the curing agent contains one or more selected from the group consisting of active ester curing agents, phenolic curing agents, naphthol curing agents, and carbodiimide curing agents. Therefore, in one embodiment, the resin composition layer contains one or more selected from the group consisting of active ester curing agents, phenolic curing agents, naphthol curing agents, and carbodiimide curing agents, and more preferably contains an active ester curing agent.
[0055] As the active ester curing agent, a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester curing agent, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferable. The active ester curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester curing agent derived from a carboxylic acid compound is preferable, an active ester curing agent obtained from a carboxylic acid compound and a hydroxy compound is more preferable, and an active ester curing agent obtained from a carboxylic acid compound and an aromatic hydroxy compound is even more preferable.
[0056] As the carboxylic acid compound, either an aromatic carboxylic acid compound or an aliphatic carboxylic acid may be used, and examples thereof include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid.
[0057] Examples of aromatic hydroxy compounds include (i) polyaddition products of unsaturated aliphatic cyclic compounds containing two double bonds in one molecule and phenols, (ii) various bisphenol compounds, (iii) aromatic polyols having two or more hydroxyl groups bonded to the carbon atoms on the aromatic ring, and (iv) aromatic monools having one hydroxyl group bonded to the carbon atoms on the aromatic ring. Examples of polyaddition products of unsaturated aliphatic cyclic compounds and phenols include polyaddition products of unsaturated aliphatic cyclic compounds such as dicyclopentadiene, tetrahydroindene, norbornadiene, limonene, and vinylcyclohexene with phenols that may have a substituent (e.g., phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, halophenol, etc.), and specifically, for example, dicyclopentadiene-phenols polyaddition products. Examples of bisphenol compounds include bisphenol A, bisphenol F, bisphenol AF, bisphenol AP, bisphenol B, bisphenol BP, bisphenol C, and bisphenol M. Examples of aromatic polyols having two or more hydroxy groups bonded to carbon atoms on an aromatic ring include hydroquinone, resorcinol, catechol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, and phenol novolak. Examples of aromatic monools having one hydroxy group bonded to a carbon atom on an aromatic ring include phenol, cresol, xylenol, ethylphenol, propylphenol, vinylphenol, allylphenol, phenylphenol, benzylphenol, halophenol, naphthol, methylnaphthol, dimethylnaphthol, ethylnaphthol, propylnaphthol, vinylnaphthol, allylnaphthol, phenylnaphthol, benzylnaphthol, and halonaphthol.
[0058] Suitable specific examples of the active ester curing agent include an active ester compound containing a dicyclopentadiene-type diphenol structure, an active ester compound containing a naphthalene structure, an active ester compound containing an acetylated product of phenol novolac, and an active ester compound containing a benzoylated product of phenol novolac. Among them, an active ester compound containing a naphthalene structure and an active ester compound containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentalene-phenylene.
[0059] Commercially available active ester curing agents include active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB-9451", "EXB-9460", "EXB-9460S", "HPC-8000-65T", "HPC-8000H-65TM", and "HPC-8000L-65TM" (manufactured by DIC Corporation); active ester resins containing a naphthalene structure such as "EXB-8100L-65T", "EXB-8150-60T", "EXB-8150-62T", "EXB-9416-70BK", "HPC-8150-60T", and "HPC-8150-62T"; Examples of such active ester resins include "HP-B-8151-62T" and "HP-C-8151-62T" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester resin which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester resins which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation) as an active ester resin containing a styryl group and a naphthalene structure.
[0060] As the phenol-based curing agent and naphthol-based curing agent, those having a novolac structure are preferred from the viewpoint of heat resistance and water resistance. Also, from the viewpoint of adhesion to the conductor layer, nitrogen-containing phenol-based curing agents and nitrogen-containing naphthol-based curing agents are preferred, and triazine skeleton-containing phenol-based curing agents and triazine skeleton-containing naphthol-based curing agents are more preferred.
[0061] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Chemical Industry Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; and "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", and "SN-37" manufactured by Nippon Steel Chemical & Material Co., Ltd. 5" and "SN-395" manufactured by DIC Corporation; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "EXB-9500", "HPC-9500", "KA-1160", "KA-1163", and "KA-1165" manufactured by Gun-ei Chemical Co., Ltd.; and the like.
[0062] Specific examples of carbodiimide-based curing agents include Carbodilite (registered trademark) V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.); V-09 (carbodiimide group equivalent: 200 g / eq.), and Stavaxol (registered trademark) P (carbodiimide group equivalent: 302 g / eq.), all manufactured by Nisshinbo Chemical Inc.
[0063] Examples of the acid anhydride curing agent include a curing agent having one or more acid anhydride groups in one molecule. Specific examples of the acid anhydride curing agent include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include polymeric acid anhydrides such as anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and styrene-maleic acid resins, which are copolymers of styrene and maleic acid. Commercially available acid anhydride hardeners include "MH-700" manufactured by New Japan Chemical Co., Ltd.
[0064] Examples of cyanate ester curing agents include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0065] Examples of the amine-based curing agent include curing agents having one or more amino groups in one molecule, such as aliphatic amines, polyether amines, alicyclic amines, aromatic amines, etc. Specific examples of the amine-based curing agent include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)- ... bis(4-aminophenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, etc. The amine-based curing agent may be a commercially available product, for example, "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd., and "Epicure W" manufactured by Mitsubishi Chemical Corporation.
[0066] Even when a thin resin composition layer having a thickness of 15 μm or less is highly blended with an inorganic filler, from the viewpoint of being able to provide an insulating layer having good adhesion to a conductor layer, and further from the viewpoint of being able to provide an insulating layer having low surface roughness after roughening treatment (desmear treatment), the content of the curing agent in the resin composition is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, 30% by mass or more, or 35% by mass or more, when the resin component in the resin composition is 100% by mass. The upper limit of the content is not particularly limited and may be determined according to the properties required for the resin composition, but may be, for example, 70% by mass or less, 65% by mass or less, or 60% by mass or less.
[0067] Among them, even when a thin resin composition layer having a thickness of 15 μm or less is highly blended with an inorganic filler, from the viewpoint of obtaining an insulating layer having better adhesion to the conductor layer, and further from the viewpoint of obtaining an insulating layer having a lower surface roughness after roughening treatment (desmear treatment), it is preferable that the curing agent contains an active ester curing agent. When the resin composition layer contains an active ester curing agent as a curing agent, the content of the active ester curing agent in the curing agent is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, 75% by mass or more, or 80% by mass or more, when the non-volatile components of the curing agent are taken as 100% by mass, from the viewpoint of obtaining the effects of the present invention more effectively and from the viewpoint of obtaining a cured product exhibiting particularly excellent dielectric properties. The upper limit of the content of the active ester curing agent in the curing agent is not particularly limited, and may be 100% by mass, but may be, for example, 95% by mass or less, 90% by mass or less, etc.
[0068] In the case where the resin composition layer in the multilayer resin sheet of the present invention contains an active ester-based curing agent as a curing agent, the mass ratio of the active ester-based curing agent to the thermosetting resin (active ester-based curing agent / thermosetting resin) is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more, or 0.75 or more, from the viewpoint of being able to enjoy the effects of the present invention more effectively and from the viewpoint of exhibiting particularly excellent dielectric properties. The upper limit of the mass ratio (active ester-based curing agent / thermosetting resin) may be, for example, 5 or less, 4.5 or less, 4 or less, etc.
[0069] -Thermoplastic resin- The resin composition layer may further contain a thermoplastic resin.
[0070] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polystyrene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polyetheretherketone resin, polyester resin, etc. The thermoplastic resin may be used alone or in combination of two or more kinds.
[0071] The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is preferably 8000 or more, more preferably 10000 or more, even more preferably 20000 or more or 30000 or more. The upper limit is preferably 100000 or less, more preferably 70000 or less, even more preferably 60000 or less. The polystyrene-equivalent Mw of the thermoplastic resin is measured by a GPC method. Specifically, the polystyrene-equivalent Mw of the thermoplastic resin is measured at a column temperature of 40° C. using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K. as a mobile phase, chloroform or the like, and can be calculated using a calibration curve of standard polystyrene.
[0072] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd., and "YL7800BH40", "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0073] Examples of polyvinyl acetal resins include polyvinyl formal resins and polyvinyl butyral resins, and polyvinyl butyral resins are preferred.Specific examples of polyvinyl acetal resins include Denka Butyral 4000-2, Denka Butyral 5000-A, Denka Butyral 6000-C, Denka Butyral 6000-EP, and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series, all of which are manufactured by Sekisui Chemical Co., Ltd.
[0074] As the polyimide resin, a resin having an imide structure (preferably a cyclic imide structure) can be used, and for example, an imide compound of an acid anhydride and a diamine compound or a diisocyanate compound can be used. Specific examples of the polyimide resin include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of the polyimide resin include modified polyimides such as linear polyimides (polyimides described in JP-A-2006-37083) obtained by reacting a bifunctional hydroxyl group-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride, and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).
[0075] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.
[0076] A specific example of polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. A specific example of polyphenylene ether resin is "OPE-2St 1200" oligophenylene ether-styrene resin manufactured by Mitsubishi Gas Chemical Co., Ltd. A specific example of polyetheretherketone resin is "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd. A specific example of polyetherimide resin is "Ultem" manufactured by GE Corporation.
[0077] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0078] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin-based elastomers such as polypropylene and ethylene-propylene block copolymer.
[0079] Examples of polystyrene resins include homopolymers of styrene, copolymers of styrene and diene compounds (butadiene, isoprene, etc.), and hydrogenated products thereof.
[0080] Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polybutylene naphthalate resin, polytrimethylene terephthalate resin, polytrimethylene naphthalate resin, and polycyclohexane dimethyl terephthalate resin.
[0081] When the resin composition layer contains a thermoplastic resin, even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, the content of the thermoplastic resin is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on the resin component in the resin composition layer being 100% by mass, from the viewpoint of obtaining an insulating layer having better adhesion to the conductor layer. The upper limit is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0082] The resin composition layer may further contain one or more selected from the group consisting of a radical polymerizable resin, a curing accelerator, and a polymerization initiator.
[0083] -Radical polymerizable resin- The type of radical polymerizable resin is not particularly limited as long as it has one or more (preferably two or more) radical polymerizable unsaturated groups in one molecule. For example, the radical polymerizable resin may be a resin having one or more radical polymerizable unsaturated groups selected from maleimide group, vinyl group, allyl group, styryl group, vinylphenyl group, acryloyl group, methacryloyl group, fumaroyl group, and maleoyl group.
[0084] There is no particular limitation on the type of maleimide resin, so long as it has one or more (preferably two or more) maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule. Examples of maleimide resins include (1) maleimide resins having an aliphatic skeleton (preferably an aliphatic skeleton having 36 carbon atoms derived from dimer diamine), such as "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", and "BMI-689" (all manufactured by DigiCner Molecules), and "SLK6895-T90" (manufactured by Shin-Etsu Chemical Co., Ltd.); (2) maleimide resins having an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; and (3) maleimide resins having an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).
[0085] The (meth)acrylic resin is not particularly limited in type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) (meth)acryloyl groups in one molecule. Here, the term "(meth)acryloyl group" is a general term for acryloyl and methacryloyl groups. Examples of methacrylic resins include (meth)acrylate monomers, as well as (meth)acrylic resins such as "A-DOG" (manufactured by Shin-Nakamura Chemical Co., Ltd.), "DCP-A" (manufactured by Kyoeisha Chemical Co., Ltd.), "NPDGA", "FM-400", "R-687", "THE-330", "PET-30", and "DPHA" (all manufactured by Nippon Kayaku Co., Ltd.).
[0086] The styryl resin is not particularly limited in type, and may be a monomer or oligomer, as long as it has one or more (preferably two or more) styryl groups or vinylphenyl groups in one molecule. Examples of the styryl resin include styrene monomers, as well as styryl resins such as "OPE-2St", "OPE-2St 1200", and "OPE-2St 2200" (all manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0087] When the resin composition layer contains a radical polymerizable resin, even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, the content of the radical polymerizable resin in the resin composition layer is preferably 2% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, 6% by mass or more, 8% by mass or more, or 10% by mass or more, based on the resin component in the resin composition being 100% by mass. The upper limit of the content is not particularly limited and may be determined according to the properties required for the resin composition, but may be, for example, 50% by mass or less, 40% by mass or less, or 30% by mass or less.
[0088] -Curing accelerator- Examples of the curing accelerator include amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, metal-based curing accelerators, peroxide-based curing accelerators, etc. The curing accelerators may be used alone or in combination of two or more.
[0089] When the resin composition layer contains a curing accelerator, the content of the curing accelerator in the resin composition may be determined according to the properties required of the resin composition. However, from the viewpoint of being able to provide an insulating layer with better adhesion to the conductor layer even when a high content of inorganic filler is used in a thin resin composition layer having a thickness of 15 μm or less, the content of the curing accelerator is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less, assuming that the resin component in the resin composition is 100% by mass, and the lower limit may be 0.01% by mass or more, 0.05% by mass or more, 0.1% by mass or more, etc.
[0090] -Polymerization initiator- Examples of the polymerization initiator include peroxides such as t-butylcumyl peroxide, t-butyl peroxyacetate, α,α'-di(t-butylperoxy)diisopropylbenzene, t-butyl peroxylaurate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneodecanoate, and t-butyl peroxybenzoate.
[0091] Commercially available polymerization initiators include, for example, “Perbutyl C”, “Perbutyl A”, “Perbutyl P”, “Perbutyl L”, “Perbutyl O”, “Perbutyl ND”, “Perbutyl Z”, “Percumyl P”, and “Percumyl D” manufactured by NOF Corporation.
[0092] When the resin composition layer contains a polymerization initiator, the content of the polymerization initiator is, from the viewpoint of better enjoying the effects of the present invention, preferably 0.01 mass % or more, more preferably 0.02 mass % or more, and even more preferably 0.03 mass % or more, relative to 100 mass % of the resin component in the resin composition, and the upper limit is preferably 1 mass % or less, or 0.5 mass % or less.
[0093] -Optional additives- The resin composition layer may further contain any additive. Examples of such additives include organic fillers such as rubber particles; organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; triazole-based adhesion imparting agents, tetrazole-based adhesion imparting agents, triazine Examples of the additives include adhesion imparting agents such as phenol-based adhesion imparting agents; antioxidants such as hindered phenol-based antioxidants; fluorescent whitening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. The content of such additives may be determined according to the properties required for the resin composition layer and thus the insulating layer.
[0094] As described above, the thickness of the resin composition layer is 15 μm or less from the viewpoint of providing a thin insulating layer and thus contributing to the reduction of the height of the circuit board. As described above, the present inventors have confirmed that when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, the adhesion between the insulating layer and the conductor layer is significantly deteriorated. In this regard, according to the method for producing a circuit board of the present invention in which a resin sheet having a support having a water vapor permeability coefficient in the above range is used and the resin composition layer is cured under specific conditions as described below, even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, an insulating layer having good adhesion to the conductor layer can be obtained. For example, the thickness of the resin composition layer may be as thin as 14 μm or less, 12 μm or less, or 10 μm or less. The lower limit of the thickness of the resin composition layer can usually be 3 μm or more, 5 μm or more, etc.
[0095] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress adhesion of dirt and the like to the surface of the resin composition layer and scratches.
[0096] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.
[0097] The organic solvent may be the same as the organic solvent described as a component of the resin composition. The organic solvent may be used alone or in combination of two or more kinds.
[0098] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 1 minute to 10 minutes.
[0099] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0100] The present invention will be described in detail below with reference to preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0101] [Circuit board manufacturing method] The method for producing a circuit board of the present invention (hereinafter also simply referred to as the "method of the present invention") is as follows: (I) a step of laminating a resin sheet including a support and a resin composition layer provided on the support, the resin composition layer having an inorganic filler content of 60% by mass or more and a thickness of 15 μm or less, on a substrate such that the resin composition layer is bonded to the substrate; (II) a step of thermally curing the resin composition layer to form an insulating layer; and (III) peeling off the support; A method for manufacturing a circuit board, comprising the steps of: The water vapor permeability coefficient of the support, calculated from the water vapor permeability of the support measured under conditions of a temperature of 40°C and a relative humidity difference of 90% using a method in accordance with JIS K7129, is 0.5 g / m 2 mm -1 - 24 hours or less, The method, in the step (II), wherein the resin composition layer is subjected to a heat treatment in which it is maintained at a temperature T1, and then subjected to a heat treatment in which it is maintained at a temperature T2 higher than the temperature T1.
[0102] As described above, the present inventors have found that when an insulating layer is formed using a resin composition with a high content of inorganic filler in order to achieve good dielectric properties and a low coefficient of thermal expansion, if a thin resin composition layer is used to reduce the height of a circuit board, sufficient adhesion between the insulating layer and the conductor layer may not be obtained. In particular, it has been confirmed that when a thin resin composition layer with a thickness of 15 μm or less contains a high content of inorganic filler, the adhesion between the insulating layer and the conductor layer is significantly deteriorated.
[0103] In contrast, according to the method of the present invention, which uses a resin sheet having a support having a water vapor permeability coefficient in the above-mentioned specific range and thermally cures a resin composition layer under the above-mentioned specific conditions to form an insulating layer, even when a thin resin composition layer having a thickness of 15 μm or less contains a high amount of inorganic filler, an insulating layer having good adhesion to a conductor layer can be obtained.Furthermore, an insulating layer having low surface roughness after roughening treatment (desmear treatment) can be obtained.
[0104] In the case where the insulating layer had poor adhesion to the conductor layer, the surface of the insulating layer after the roughening treatment (desmearing treatment) was observed, and it was confirmed that a large amount of inorganic filler was present and exposed on the insulating layer surface due to the high content of inorganic filler. In contrast, it was confirmed that the insulating layer obtained by the method of the present invention, which uses a resin sheet having a support with a water vapor permeability coefficient in the above-mentioned specific range and thermally cures the resin composition layer under the above-mentioned specific conditions, has a tendency that there is little inorganic filler present and exposed on the insulating layer surface after the roughening treatment, and a resin-rich phase is present. Thus, it is presumed that the insulating layer obtained by the method of the present invention has a resin-rich phase formed on its surface while maintaining the bulk properties such as good dielectric properties and low thermal expansion coefficient due to the high content of inorganic filler, and a surface that contributes to adhesion to the conductor layer is reproduced. In addition, when a thin resin composition layer having a thickness of 15 μm or less contains a high content of inorganic filler, it has been confirmed that an insulating layer having good adhesion to a conductor layer cannot be achieved by simply using a resin sheet having a support whose water vapor permeability coefficient is in the above-mentioned specific range or by simply heat-curing the resin composition layer under the above-mentioned specific conditions to form an insulating layer (see Comparative Example described later). In other words, the problems and effects of the present invention can be solved and achieved synergistically only by using a resin sheet having a support whose water vapor permeability coefficient is in the above-mentioned specific range and by heat-curing the resin composition layer under the above-mentioned specific conditions to form an insulating layer.
[0105] Each step will be described below.
[0106] -Process (I)- In step (I), a resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer having an inorganic filler content of 60 mass% or more and a thickness of 15 μm or less, is laminated on a substrate so that the resin composition layer is bonded to the substrate.
[0107] The resin sheet used in step (I) is as described above in the <Resin Sheet> section, including the water vapor permeability coefficient of the support and the composition and thickness of the resin composition layer. When the resin sheet has a protective film, the protective film is peeled off to expose the resin composition layer, and then step (I) is carried out.
[0108] In step (I), the "substrate" on which the resin sheet is laminated mainly refers to a substrate such as a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, or a substrate having a patterned conductor layer (circuit) formed on one or both sides of the substrate. In addition, the "substrate" of the present invention also includes an inner layer circuit substrate of an intermediate product on which an insulating layer and / or a conductor layer is to be formed when manufacturing a circuit substrate.
[0109] In addition, when manufacturing a rewiring board for a semiconductor package, the circuit board is stIn the case of manufacturing by the 1st chip method, a semiconductor wafer having a circuit element having a predetermined function and an electrode pad surface on which a plurality of electrode pads electrically connected to the circuit element are formed may be used as the "substrate". The semiconductor wafer is preferably a silicon (Si)-based wafer, but is not limited thereto. For example, a wafer such as a gallium arsenide (GaAs)-based, an indium phosphide (InP)-based, a gallium phosphide (GaP)-based, a gallium nitride (GaN)-based, a gallium telluride (GaTe)-based, a zinc selenium (ZnSe)-based, or a silicon carbide (SiC)-based wafer may be used. The chip 1st method is a method in which a semiconductor chip is first provided and a rewiring layer is formed on the electrode pad surface (for example, JP 2002-289731 A, JP 2006-173345 A, etc.). In such a chip 1st method, particularly when manufacturing a package with a fan-out structure, the semiconductor wafer is first divided into individual pieces, and the individual semiconductor chips are arranged on a carrier substrate at a distance from each other, and then the pieces are sealed with resin. A rewiring layer is then formed on the exposed electrode pad surface and the sealing resin layer around it (for example, JP 2012-15191 A, JP 2015-126123 A, etc.). st In the case of manufacturing the circuit board by the 1st rewiring layer method, a substrate with a peelable layer or a substrate on which a patterned conductor layer (circuit) is formed on the substrate with a peelable layer may be used as the "substrate". The 1st rewiring layer method is a method in which a rewiring layer is first provided, and a semiconductor chip is provided on the rewiring layer in such a state that the electrode pad surface can be electrically connected to the rewiring layer (for example, JP 2015-35551 A, JP 2015-170767 A, etc.). In the 1st rewiring layer method, after providing a semiconductor chip on the rewiring layer, the substrate with a peelable layer is peeled off to expose the rewiring layer. As the substrate with a peelable layer, a known substrate used when manufacturing a circuit board by the 1st rewiring layer method may be used, and the type is not particularly limited, but examples thereof include a glass substrate with a peelable layer, a metal substrate with a peelable layer, and a plastic substrate with a peelable layer.
[0110] The substrate and the resin sheet can be laminated by thermocompression bonding the resin sheet to the substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the substrate (hereinafter also referred to as "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). The thermocompression bonding member may be directly pressed onto the resin sheet, or may be pressed via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate.
[0111] The lamination of the substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the heat-pressure bonding temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the heat-pressure bonding pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the heat-pressure bonding time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.
[0112] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0113] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0114] -Process (II)- In step (II), the resin composition layer is thermally cured to form an insulating layer.
[0115] The method of the present invention is characterized in that in step (II), the resin composition layer is subjected to a heat treatment at a temperature T1 and then to a heat treatment at a temperature T2 higher than the temperature T1. Hereinafter, the heat treatment at a temperature T1 is also referred to as a "pre-cure step", and the heat treatment at a temperature T2 is also referred to as a "post-cure step".
[0116] --Pre-curing process (heat treatment at temperature T1)-- Usually, before the pre-cure step, the resin composition layer is at a temperature rise start temperature T0, which is lower than the temperature T1. The temperature rise start temperature T0 may be, for example, room temperature. Thus, the step (II) may include a step of raising the temperature of the resin composition layer from the temperature rise start temperature T0 to the temperature T1 before the pre-cure step. From the viewpoint of obtaining the effects of the present invention significantly, the temperature rise rate in this temperature rise step is preferably 0.5°C / min or more, more preferably 1°C / min or more, even more preferably 1.5°C / min or more, even more preferably 2°C / min or more, and particularly preferably 2.5°C / min or more, and the upper limit is preferably 30°C / min or less, more preferably 25°C / min or less, even more preferably 20°C / min or less, even more preferably 15°C / min or less, and particularly preferably 10°C / min or less. The temperature rise rate in the temperature rise step may be constant or may be changed.
[0117] In the pre-cure step, the resin composition layer is subjected to a heat treatment in which the resin composition layer is held at a temperature T1. The heating temperature T1 in this pre-cure step is set in a temperature range higher than room temperature and lower than the temperature T2. From the viewpoint of obtaining the effects of the present invention significantly, the specific range of the heating temperature T1 is preferably 50°C or higher, more preferably 60°C or higher, even more preferably 70°C or higher, and even more preferably 80°C or higher, and the upper limit is preferably less than 150°C, more preferably 140°C or lower, and even more preferably 130°C or lower. In the pre-cure step, holding the resin composition layer at a temperature T1 is not limited to maintaining the temperature of the resin composition layer at a constant temperature, but also includes fluctuating the temperature of the resin composition layer within a range that does not significantly impair the effects of the present invention. For example, the temperature of the resin composition layer in the pre-cure step may fluctuate within a range of ±10°C, ±8°C, or ±5°C. However, even when the temperature of the resin composition layer fluctuates in this manner, the temperature of the resin composition layer in the pre-cure step is preferably within the above-mentioned preferred range, for example, within a range of 50° C. or more and less than 150° C. In particular, it is particularly preferable that the temperature of the resin composition layer does not fluctuate and is constant in the pre-cure step.
[0118] The time for which the resin composition layer is held at the heating temperature T1 in the pre-cure process depends on the composition of the resin composition layer and the value of the heating temperature T1, but from the viewpoint of obtaining the effects of the present invention significantly, it is preferably 10 minutes or more, more preferably 15 minutes or more, and even more preferably 20 minutes or more, and the upper limit is preferably 150 minutes or less, more preferably 120 minutes or less, and even more preferably 120 minutes or less.
[0119] --Post-cure process (heat treatment at temperature T2)-- Usually, before the post-cure step, the resin composition layer is at a temperature lower than the temperature T2. Therefore, the step (II) may include a step of raising the temperature of the resin composition layer to the temperature T2 after the pre-cure step and before the post-cure step. From the viewpoint of obtaining the effects of the present invention significantly, the temperature raising rate in this temperature raising step is preferably 0.5°C / min or more, more preferably 1°C / min or more, even more preferably 1.5°C / min or more, even more preferably 2°C / min or more, and particularly preferably 2.5°C / min or more, and the upper limit is preferably 30°C / min or less, more preferably 25°C / min or less, even more preferably 20°C / min or less, even more preferably 15°C / min or less, and particularly preferably 10°C / min or less. Therefore, in one embodiment, in the step (II), the resin composition layer is raised to the temperature T2 at a temperature raising rate of 0.5°C / min or more and 30°C / min or less. The temperature raising rate in the temperature raising step may be constant or may be changed.
[0120] In the post-cure step, the resin composition layer is subjected to a heat treatment in which the resin composition layer is held at a temperature T2. The heating temperature T2 in the post-cure step is set to a temperature higher than the temperature T1. From the viewpoint of obtaining the effects of the present invention remarkably, the specific range of the heating temperature T2 is preferably 150°C or higher, more preferably 155°C or higher, even more preferably 160°C or higher, and particularly preferably 170°C or higher, and the upper limit is preferably 250°C or lower, more preferably 230°C or lower, even more preferably 220°C or lower, even more preferably 210°C or lower, and particularly preferably 200°C or lower. In the post-cure step, holding the resin composition layer at a temperature T2 includes not only maintaining the temperature of the resin composition layer at a constant temperature, but also fluctuating the temperature of the resin composition layer within a range that does not significantly impair the effects of the present invention. For example, the temperature of the resin composition layer in the post-cure step may fluctuate within a range of ±10°C, ±8°C, or ±5°C. However, even when the temperature of the resin composition layer fluctuates in this manner, the temperature of the resin composition layer in the post-cure step is preferably within the above-mentioned preferred range, for example, within the range of 150° C. or more and 250° C. or less. Among these, it is particularly preferable that the temperature of the resin composition layer does not fluctuate and is constant in the post-cure step.
[0121] The difference T2-T1 between the heating temperature T1 in the precure step and the heating temperature T2 in the postcure step is preferably within a specific range from the viewpoint of obtaining the effects of the present invention significantly. Specifically, the difference T2-T1 is preferably 20°C or more, more preferably 30°C or more, and even more preferably 40°C or more, and the upper limit is preferably 150°C or less, more preferably 140°C or less, even more preferably 130°C or less, and particularly preferably 120°C or less. When the temperature of the resin composition layer varies in the precure step and / or the postcure step, it is preferable that the difference between the median temperature of the resin composition in the precure step and the median temperature of the resin composition in the postcure step is within the above range.
[0122] The time for which the resin composition layer is held at the heating temperature T2 in the post-cure process depends on the composition of the resin composition layer and the value of the heating temperature T2, but from the viewpoint of obtaining the effects of the present invention significantly, it is preferably 10 minutes or more, more preferably 15 minutes or more, and even more preferably 20 minutes or more, and the upper limit is preferably 150 minutes or less, more preferably 120 minutes or less.
[0123] After the heat treatment at temperature T1 in the precure step, the resin composition layer may be cooled once and then subjected to a heat treatment at heating temperature T2 in the postcure step. Alternatively, after the heat treatment at temperature T1 in the precure step, the resin composition layer may be subjected to a heat treatment at temperature T2 in the postcure step without being cooled.
[0124] The heat treatment in the precure step and the heat treatment in the postcure step may be performed using the same heat treatment device. The heat treatment in the precure step may be performed using a first heat treatment device, and the heat treatment in the postcure step may be performed using a second heat treatment device different from the first heat treatment device. The heat treatment device is not particularly limited as long as it can thermally cure the resin composition layer. For example, an oven, a hot press, or the like may be used as the heat treatment device. For example, after the heat treatment in the precure step is performed using an oven adjusted to a temperature T1, the laminate of the substrate and the resin sheet may be transferred to an oven adjusted to a temperature T2, and the heat treatment in the postcure step may be performed. Alternatively, the heat treatment in the precure step may be performed using a heat treatment device capable of temperature programming, and then the temperature may be increased from T1 to T2, and the heat treatment in the postcure step may be performed.
[0125] Step (II) may further include any step in addition to the above-mentioned pre-cure step, post-cure step, and the temperature-raising step before them. For example, step (II) may include a step of subjecting the resin composition layer to a heat treatment in which the resin composition layer is maintained at a temperature other than temperatures T1 and T2. That is, step (II) is not limited to a two-step heat treatment, and may include three or more steps of heat treatment.
[0126] Step (II) is preferably carried out in a nitrogen atmosphere. When the nitrogen atmosphere contains oxygen, the oxygen concentration in the nitrogen atmosphere is preferably 5% by mass or less, more preferably 3% by mass or less, further preferably 1% by mass or less, and may be 0% by mass.
[0127] The pressure condition of the nitrogen atmosphere in which step (II) is carried out may be normal pressure or reduced pressure. In one example, the specific pressure condition of the nitrogen atmosphere is preferably 0.1 hPa or more, more preferably 1.3 hPa or more, and the upper limit is preferably 5000 hPa or less, more preferably 2500 hPa or less.
[0128] -Process (III)- In step (III), the support is peeled off, thereby exposing the insulating layer.
[0129] The support may be peeled off by pulling the support relative to the insulating layer. For example, the insulating layer and the base material may be transported while the support is fixed, and the support may be peeled off. Alternatively, the support may be pulled while the insulating layer and the base material are fixed, and the support may be peeled off.
[0130] The temperature at which step (III) is carried out is not particularly limited. From the viewpoint of reducing the energy required for manufacturing the circuit board, step (III) is usually carried out at room temperature or a temperature close to it. Therefore, usually, after step (II), the laminate consisting of the base material, the insulating layer and the support is cooled, and then step (III) is carried out. The temperature at which step (III) is carried out is preferably in the range of 10°C or more and 40°C or less. In addition, the cooling rate when cooling from temperature T2 is not particularly limited, but is preferably 0.5°C / min or more, more preferably 1°C / min or more, even more preferably 1.5°C / min or more, even more preferably 2°C / min or more, and particularly preferably 2.5°C / min or more, and the upper limit is preferably 30°C / min or less, more preferably 25°C / min or less, even more preferably 20°C / min or less, even more preferably 15°C / min or less, and particularly preferably 10°C / min or less.
[0131] The method of the present invention may include other steps as long as it includes the above steps (I) to (III) in that order. For example, the method of the present invention may further include the steps of (A) forming a via hole in the insulating layer by a laser, (B) roughening the insulating layer (desmearing), and (C) forming a conductor layer on the surface of the insulating layer.
[0132] In step (A), a via hole is formed in an insulating layer by a laser.
[0133] As a laser light source for forming a via hole in an insulating layer, for example, a carbon dioxide laser (CO2 laser), a UV-YAG laser, an excimer laser, or the like may be used.
[0134] The laser processing conditions (e.g., laser wavelength, pulse number, pulse width, output) are not particularly limited as long as they can form via holes having a good via shape and a small amount of internal smear, and may be appropriately determined within the range of general processing conditions depending on the specifications of the laser processing machine used.
[0135] The dimensions and shape of the via hole may be appropriately determined according to the design of the circuit board. For example, the shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 30 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less, and the lower limit may be, for example, 2 μm or more, 4 μm or more, 5 μm or more, etc. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole on the surface of the insulating layer.
[0136] In the method of the present invention, step (A) may be carried out after the above step (II), for example, between step (II) and step (III) or after step (III).
[0137] In step (B), the insulating layer is roughened (desmeared). This makes it possible to remove resin residues (smears) in the via holes. The procedure and conditions of the desmearing are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer for a circuit board can be adopted. For example, the desmearing can be performed by carrying out a swelling treatment using a swelling liquid, a desmear (roughening) treatment using an oxidizing agent liquid, and a neutralization treatment using a neutralizing liquid in this order.
[0138] The swelling liquid used in the desmear treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigant P" and "Swelling Dip Securigant SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.
[0139] The oxidizing agent used in the desmear treatment is not particularly limited, and examples thereof include an alkaline permanganate solution obtained by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.
[0140] The neutralizing solution used in the desmear treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Securigant P" manufactured by Atotech Japan. The neutralizing treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in the neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in the neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.
[0141] Here, when the desmear treatment is performed after peeling off the support, that is, when step (B) is performed after step (III), the desmear treatment also serves as a roughening treatment for the exposed surface of the insulating layer. As described above, according to the method of the present invention, a resin-rich phase tends to be formed on the surface of the insulating layer after the roughening treatment, which is advantageous because it can reproduce a surface that contributes to adhesion with the conductor layer. Therefore, in one embodiment, the desmear treatment is performed after peeling off the support.
[0142] Next, in step (C), a conductor layer is formed on the surface of the insulating layer.
[0143] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.
[0144] First, a plating seed layer is formed on the surface of the insulating layer by electroless plating. The plating seed layer includes at least a conductive seed layer. The conductive seed layer is a layer that functions as an electrode in the electrolytic plating method. The conductive material constituting the conductive seed layer is not particularly limited as long as it exhibits sufficient conductivity, and suitable examples include copper, palladium, gold, platinum, silver, aluminum, and alloys thereof. The plating seed layer may also include a diffusion barrier layer. The diffusion barrier layer is a layer that prevents the conductive material constituting the conductive seed layer from diffusing into the insulating layer and causing insulation breakdown. In addition, the material constituting the diffusion barrier layer is not particularly limited as long as it can suppress or prevent the diffusion of the conductive material constituting the conductive seed layer, and suitable examples include titanium, tungsten, tantalum, and alloys thereof. After a conductive layer is formed on the plating seed layer in a desired pattern, unnecessary parts other than the conductive layer formation part are removed by etching or the like. At this time, the thinner the plating seed layer is, the easier it is to remove the unnecessary parts of the plating seed layer, and the erosion of the conductive pattern when removing the unnecessary parts can be minimized, which is advantageous in realizing fine wiring. The thickness of the plating seed layer is preferably 1000 nm (1 μm) or less, more preferably 800 nm or less, 600 nm or less, 500 nm or less, 400 nm or less, or 300 nm or less. Since the method of the present invention can realize an insulating layer with low surface roughness, the thickness of the plating seed layer may be even thinner. For example, the thickness of the plating seed layer may be 250 nm or less, 200 nm or less, 150 nm or less, 140 nm or less, 120 nm or less, or 100 nm or less. When the plating seed layer includes a diffusion barrier layer, the "thickness of the plating seed layer" in the present invention refers to the average thickness of the entire plating seed layer including not only the conductive seed layer but also the diffusion barrier layer.
[0145] The plating seed layer may be formed by dry plating or wet plating. Examples of dry plating include physical vapor deposition (PVD) methods such as sputtering, ion plating, and vacuum deposition, and chemical vapor deposition (CVD) methods such as thermal CVD and plasma CVD. Examples of wet plating include electroless plating. From the viewpoint of forming a thin plating seed layer with a more uniform thickness, dry plating or electroless plating is preferred.
[0146] Next, an etching resist (plating resist) is formed on the formed plating seed layer, which exposes a part of the plating seed layer corresponding to a desired wiring pattern. After forming a metal layer by electrolytic plating on the exposed plating seed layer, the etching resist is removed. The conductive material used for the metal layer is not particularly limited. In a preferred embodiment, the metal layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The metal layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy).
[0147] Thereafter, unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern (hereinafter also referred to as a "conductor pattern") can be formed.
[0148] The thickness of the conductor layer depends on the desired design of the circuit board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0149] According to the method of the present invention, it is possible to form a fine conductor circuit with an L / S of, for example, 5 / 5 μm or less, 4 / 4 μm or less, 3 / 3 μm or less, 2 / 2 μm or less, 1.5 / 1.5 μm or less, or 1 / 1 μm or less while maintaining good adhesion between the insulating layer and the conductor layer.
[0150] According to the method of the present invention, even when an insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content, an insulating layer having good adhesion to a conductor layer can be obtained. For example, the peel strength to the conductor layer measured by the method described in the <Measurement of Adhesion (Peel Strength)> section below can be preferably 0.26 kgf / cm or more, 0.28 kgf / cm or more, or 0.3 kgf / cm or more.
[0151] According to the method of the present invention, even when an insulating layer is formed using a resin composition layer having a thickness of 15 μm or less and a high inorganic filler content, an insulating layer having a low surface roughness after roughening treatment (desmear treatment) can be obtained. For example, the arithmetic mean roughness Ra measured by the method described in the section <Measurement of arithmetic mean roughness Ra> below can be preferably 500 nm or less, 400 nm or less, 300 nm or less, 250 nm or less, 200 nm or less, or 150 nm or less.
[0152] If necessary, the formation of the insulating layers and the conductor layers in the above steps (I) to (III) and steps (A) to (C) may be repeated to form a multi-layer circuit board.
[0153] As described above, the circuit board manufactured by the method of the present invention can be suitably used as a printed wiring board or a circuit board for a semiconductor package (circuit board for a semiconductor package). The semiconductor package in which the circuit board manufactured by the method of the present invention is used may be either a fan-in type package or a fan-out type package. When the semiconductor package is a fan-out type package, it is advantageous because a conductor circuit can be formed in a large area with a fine pattern, in addition to the inherent feature of the fan-out type package that the rewiring layer can be formed in a large area. EXAMPLES
[0154] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" means "parts by mass" unless otherwise specified. Unless otherwise specified, the measurements were performed at room temperature and atmospheric pressure.
[0155] [Example 1] 10 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical & Material Co., Ltd., a 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent 169) and 50 parts of naphthol type epoxy resin ("ESN475V" manufactured by Nippon Steel Chemical & Material Co., Ltd., epoxy equivalent approximately 330) were heated and dissolved in 40 parts of solvent naphtha with stirring. This was cooled to room temperature to prepare a dissolved composition of the epoxy resin.
[0156] The epoxy resin solution composition was mixed with 5 parts of a phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of methyl ethyl ketone (MEK) and cyclohexanone with a non-volatile content of 30% by mass), 5 parts of a triazine skeleton-containing cresol novolac resin ("LA3018-50P" manufactured by DIC Corporation, a reactive group equivalent of about 151, a 2-methoxypropanol solution with a non-volatile content of 50% by mass), 70 parts of an active ester-based hardener ("HPC-8000-65T" manufactured by DIC Corporation, a reactive group equivalent of about 223, a toluene solution with a non-volatile content of 65% by mass), and 70 parts of a (meth)acrylic resin ("A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd., ( 20 parts of a carbodiimide curing agent (Nisshinbo Chemical's "V-03", carbodiimide equivalent 216, toluene solution with 50% non-volatile components) 15 parts of a curing accelerator (1-benzyl-2-phenylimidazole (1B2PZ), MEK solution with 10% non-volatile components) 6 parts of a polymerization initiator (NOF Corp.'s "Perkmyl D", MEK solution with 20% non-volatile components)) 2 parts of an amino-silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM573")-treated spherical silica (Admatechs' "SO-C2", average particle size 0.5 μm, specific surface area 5.9 m) 2 Resin varnish 1 was prepared by mixing 370 parts of toluene (1 / g), 10 parts of cyclohexanone, and 10 parts of MEK and dispersing the mixture uniformly in a high-speed rotating mixer.
[0157] The support was prepared by preparing a PET film ("AL5" manufactured by Lintec Corporation, thickness 40 μm) with a release layer on one side, and providing an organic barrier layer (polyvinyl alcohol) with a thickness of 2 μm on the side opposite the release layer of the film (layer structure of support: release layer / PET film / organic barrier layer). Resin varnish 1 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 1 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including the support and the resin composition layer.
[0158] [Example 2] 25 parts of liquid bisphenol A type epoxy resin ("jER828EL" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 180), 20 parts of biphenyl type epoxy resin ("NC-3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 269), 15 parts of naphthalene type tetrafunctional epoxy resin ("HP-4700" manufactured by DIC Corporation, epoxy equivalent 162), 15 parts of dicyclopentadiene type epoxy resin ("HP-7200HH" manufactured by DIC Corporation, epoxy equivalent 280), and 30 parts of phenoxy resin ("YX6954" manufactured by Mitsubishi Chemical Corporation, weight average molecular weight 38000, 1:1 solution of MEK and cyclohexanone with non-volatile component of 30% by mass) were dissolved by heating in 15 parts of MEK and 15 parts of cyclohexanone with stirring. To this was added 40 parts of a phenol novolac hardener (DIC Corporation's "LA-7054", phenolic hydroxyl equivalent 124, MEK solution with 60% non-volatile components), 0.1 parts of a hardening accelerator (Shikoku Chemical Industry Co., Ltd.'s "2E4MZ", 2-ethyl-4-methylimidazole), and spherical silica (Admatechs Corporation's "SO-C2", average particle size 0.5 μm, specific surface area 5.9 m) surface-treated with an amino silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM573"). 2 The mixture was mixed and uniformly dispersed in a high-speed mixer to prepare Resin Varnish 2.
[0159] The support was prepared by preparing a PET film ("AL5" manufactured by Lintec Corporation, thickness 40 μm) with a release layer on one side, and providing an organic barrier layer (polyvinyl alcohol) with a thickness of 2 μm on the side opposite the release layer of the film. Resin varnish 2 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 2 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including the support and the resin composition layer.
[0160] [Example 3] A PEN film (Toyobo Co., Ltd. "Teonex Q83", thickness 25 μm) with a release layer on one side was prepared as a support. The above-mentioned resin varnish 1 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 1 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including a support and a resin composition layer.
[0161] [Example 4] A polyimide (PI) film (Ube Industries, Ltd., "Upilex-S", thickness 13 μm) with a release layer was prepared as a support. The above-mentioned resin varnish 1 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying would be 10 μm. Thereafter, the resin varnish 1 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including a support and a resin composition layer.
[0162] [Comparative Example 1] As a support, a PET film ("AL5" manufactured by Lintec Corporation, thickness 38 μm) having a release layer on one side was prepared. The above-mentioned resin varnish 1 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 1 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including the support and the resin composition layer.
[0163] [Comparative Example 2] A PET film ("AL5" manufactured by Lintec Corporation, thickness 40 μm) with a release layer on one side was prepared, and a 2 μm-thick organic barrier layer (polyvinyl alcohol) was provided on the side opposite the release layer of the film to prepare a support. The above-mentioned resin varnish 1 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 1 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including a support and a resin composition layer.
[0164] [Comparative Example 3] A PET film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. The above-mentioned resin varnish 3 was uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 10 μm. Thereafter, the resin varnish 3 was dried at 80°C to 100°C (average 90°C) for 2 minutes to obtain a resin sheet including the support and the resin composition layer.
[0165] [Preparation of samples for measurement and evaluation] (1) Surface preparation of inner layer board Both sides of the glass cloth-based epoxy resin double-sided laminate (copper foil thickness 18μm, substrate thickness 0.8mm, Panasonic "R1515A") on which the inner layer circuit was formed were etched 1μm deep using MEC's "CZ8100" to roughen the copper surface. Then, it was dried at 190℃ for 30 minutes.
[0166] (2) Lamination of resin sheets The resin sheets obtained in the examples and comparative examples were laminated on both sides of the inner layer substrate using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd. 2-stage build-up laminator "CVP700") so that the resin composition layer was bonded to the inner layer substrate. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 100°C and a pressure of 0.74 MPa for 30 seconds. The laminated resin sheets were then heat pressed at atmospheric pressure, 100°C, and a pressure of 0.5 MPa for 60 seconds to smooth them. In this way, a laminate having a layer structure of support / resin composition layer / inner layer substrate / resin composition layer / support was obtained.
[0167] (3) Curing of the resin composition layer Next, the laminate was placed in a nitrogen oven with the support still attached. After placing, the door was closed, and nitrogen was circulated until the oxygen concentration in the oven reached 0.5%. After confirming that the oxygen concentration in the oven reached 0.5%, the resin composition layer was thermally cured under the following curing conditions. Specifically, the temperature in the oven was raised from 30°C to temperature T1 (see Table 1; 130°C in Example 1) at a heating rate of 10°C / min, and then subjected to a heat treatment in which the temperature was held at T1 for 30 minutes, and then further heated to temperature T2 (see Table 1; 175°C in Example 1) at a heating rate of 10°C / min, and then subjected to a heat treatment in which the temperature was held at T2 for 30 minutes. In this way, the resin composition layer was thermally cured to obtain a laminate having a layer structure of support / insulating layer / inner layer substrate / insulating layer / support. Thereafter, the temperature was lowered to 30°C at 5°C / min, and the laminate was taken out of the nitrogen oven.
[0168] (4) Roughening treatment The support was peeled off from the laminate to expose the insulating layer. The laminate was then immersed in a swelling liquid (Atotech Japan's "Swelling Dip Securigant P", an aqueous solution of diethylene glycol monobutyl ether and sodium hydroxide) at 60°C for 10 minutes, then in an oxidizing agent liquid (Atotech Japan's "Concentrate Compact P", an aqueous solution of potassium permanganate at about 6% by mass and sodium hydroxide at about 4% by mass) at 80°C for 20 minutes, and finally in a neutralizing liquid (Atotech Japan's "Reduction Solution Securigant P", an aqueous solution of sulfuric acid) at 40°C for 5 minutes. The obtained substrate is referred to as "Evaluation Substrate A".
[0169] <Measurement of arithmetic mean roughness Ra> For evaluation board A, the arithmetic mean roughness Ra was calculated using a non-contact surface roughness meter (Beeco Instruments' "WYKO NT3300") in VSI mode with a 50x lens over a measurement range of 121μm x 92μm. Each was measured by calculating the average value of 10 randomly selected points.
[0170] <Measurement of adhesion (peel strength)> (1) Preparation of evaluation board Evaluation substrate A was immersed in an electroless plating solution containing PdCl2 at 40°C for 5 minutes, and then immersed in an electroless copper plating solution at 25°C for 20 minutes. After heating at 150°C for 30 minutes to perform an annealing treatment, a plating resist was formed, and the plating resist was etched to form a pattern, and then copper sulfate electrolytic plating was performed to form a conductor layer with a thickness of 30 μm. Next, an annealing treatment was performed at 200°C for 60 minutes. The obtained substrate is called "evaluation substrate B".
[0171] (2) Peel strength measurement A 10 mm wide, 150 mm long cut was made in the conductor layer of evaluation board B, and one end of this was peeled off and held with a gripping tool (TSE Autocom type testing machine "AC-50C-SL"), and the load (kgf / cm) was measured when 100 mm was peeled off vertically at a speed of 50 mm / min at room temperature (25°C).
[0172] <Method for measuring water vapor permeability coefficient> The water vapor permeability coefficient of the support was determined by the following procedure. First, the water vapor permeability (g / m 2 The water vapor transmission rate was measured at a temperature of 40°C and a relative humidity of 90% using a water vapor transmission rate measuring device (MOCON's "PERMATRAN-W3 / 34") in accordance with JIS K7129. The water vapor transmission rate was multiplied by the thickness of the support (mm) to obtain the water vapor transmission coefficient of the support (g / m 2 mm -1 -24h) was calculated.
[0173] [Table 1]
Claims
1. (I) A step of laminating a resin sheet including a support and a resin composition layer having an inorganic filler content of 60% by mass or more and a thickness of 15 μm or less provided on the support, onto a substrate such that the resin composition layer is bonded to the substrate; (II) a step of thermally curing the resin composition layer to form an insulating layer; and (III) peeling off the support; A method for manufacturing a circuit board, comprising the steps of: The water vapor permeability coefficient of the support calculated from the water vapor permeability of the support measured under conditions of a temperature of 40° C. and a relative humidity difference of 90% according to a method in accordance with JIS K7129 is 0.5 g / m 2 ・mm -1 - 24 hours or less, In the step (II), the resin composition layer is subjected to a heat treatment in which it is maintained at a temperature T1, and then subjected to a heat treatment in which it is maintained at a temperature T2 higher than the temperature T1.
2. 2. The method according to claim 1, wherein the temperature T2 is 150° C. or higher.
3. 2. The method according to claim 1, wherein the difference T2-T1 between the temperature T1 and the temperature T2 is 20° C. or more.
4. 2. The method according to claim 1, wherein the temperature T1 is 50° C. or higher.
5. The method according to claim 1, wherein in the step (II), the resin composition layer is heated to a temperature T2 at a heating rate of 0.5° C. / min or more and 30° C. / min or less.
6. The method of claim 1 , wherein the resin composition layer comprises a thermosetting resin.
7. The method of claim 1 , wherein the resin composition layer comprises one or more curing agents selected from the group consisting of active ester-based curing agents, phenol-based curing agents, naphthol-based curing agents, and carbodiimide-based curing agents.
8. The method of claim 1 further comprising the step of laser forming a via hole in the insulating layer.
9. The method according to any one of claims 1 to 8, further comprising the step of forming a conductive layer on a surface of the insulating layer.
10. The method according to claim 9, wherein the peel strength between the insulating layer and the conductor layer is 0.3 kgf / cm or more.
Citation Information
Patent Citations
Method for manufacturing laminate
JP2013030761A
Manufacturing method of printed wiring board and resin sheet with inorganic layer
JP2021015913A
Resin sheet
JP2021154641A
Resin composition
JP2022093188A
Cited By
Wiring laminate, wiring board, circuit board, and method for manufacturing wiring laminate
WO2026186851A1