Alloy steel and mechanical component therewith
The alloy steel with controlled chemical composition and surface hardened layer addresses the challenge of high hardness and cost in bearing steels by achieving 800 HV hardness at lower quenching temperatures, enhancing mechanical parts' performance and reducing manufacturing costs.
Patent Information
- Application Number
- JP2023046131
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing bearing steels face challenges in achieving high hardness without excessive deformation and increased manufacturing costs due to high heat treatment temperatures, limiting their application in smaller, thinner, and lighter mechanical parts.
An alloy steel composition with specific ranges of C, Si, Mn, Cr, Mo, V, and optionally Nb or W, forming a hardened layer on the surface, achieving 800 HV hardness at lower quenching temperatures, thereby reducing deformation and manufacturing costs.
The alloy steel achieves high surface hardness and indentation resistance, suitable for sliding and bearing parts, while minimizing deformation and cost through optimized chemical composition and lower quenching temperatures.
Abstract
Description
[Technical field]
[0001] The present invention relates to an alloy steel composed of chromium, molybdenum, etc., with a content of additive elements other than iron of less than 5%, and to a machine part using the same. [Background technology]
[0002] Currently, bearing steel (SUJ2) is widely used for mechanical parts used in automobiles and industrial machinery, such as rolling bearings. Its surface and internal hardness is about 61-62HRC on the Rockwell C scale. In recent years, there has been a demand for smaller, thinner, and lighter mechanical parts, but because it is not easy to change the shape of the rolling elements and inner and outer rings that make up rolling bearings, there is an urgent need to reconsider this from the perspective of materials.
[0003] For example, Patent Document 1 discloses a rolling bearing made of alloy steel, and explains that the hardness of both the surface and the interior is ensured to be 63 HRC or higher on the Rockwell C scale, and that the bearing has sufficient static strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-49057 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the steel type disclosed in Patent Document 1, the desired structure is formed by setting the heat treatment temperature (quenching temperature) to at least 1100°C, resulting in a hardness of 63 HRC or more on the Rockwell C scale. However, there are problems in that the amount of deformation of the product increases after heat treatment, and the manufacturing cost also increases.
[0006] Therefore, the objective of the present invention is to provide an alloy steel that can achieve high hardness (surface hardness of 800 HV or more in Vickers hardness) even when quenched at a temperature (900°C or less) equivalent to the quenching temperature of conventional bearing steel, and to provide a mechanical part using the alloy steel. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, the alloy steel of the present invention is an alloy steel consisting of, by weight percent, 0.40-0.90% C, 0.70-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-1.50% Mo, and 0.05-0.80% V, with the remainder being Fe and unavoidable impurities, and a hardened layer is formed on the surface of the alloy steel.
[0008] Alternatively, the alloy steel may be composed, by weight, of 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-0.70% Mo, 0.05-0.40% V, with the remainder being Fe and unavoidable impurities, and having a hardened layer formed on the surface.
[0009] Other chemical components are, by weight, C: 0.40-0.90%, Si: 0.70-2.50%, Mn: 0.10-1.00%, Cr: 1.00-4.00%, Mo: 0.20-1.50%, and Nb: 0.025-0.20%, with the remainder being Fe and unavoidable impurities, and a hardened layer is formed on the surface of the alloy steel.
[0010] Alternatively, the alloy steel may be composed, by weight, of 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-0.70% Mo, 0.025-0.20% Nb, with the remainder being Fe and unavoidable impurities, and having a hardened layer formed on the surface.
[0011] Other chemical components are, by weight, C: 0.40-0.90%, Si: 0.70-2.50%, Mn: 0.10-1.00%, Cr: 1.00-4.00%, W+2Mo: 0.40-3.0%, and V: 0.05-0.80%, with the remainder being Fe and unavoidable impurities, and a hardened layer is formed on the surface of the alloy steel.
[0012] Alternatively, the alloy steel may be composed, by weight, of 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.40-3.0% W+2Mo, and 0.05-0.40% V, with the remainder being Fe and unavoidable impurities, and having a hardened layer formed on the surface.
[0013] The hardened layer formed on the surface of the alloy steel may be either a carburized layer or a carbonitrided layer, and the surface hardness is preferably 800 HV or more in Vickers hardness. Effect of the Invention
[0014] The alloy steel of the present invention can obtain sufficient surface hardness (800HV or more) by carburizing or carbonitriding even at a quenching temperature in the same temperature range as that of bearing steel (900°C or less) during manufacturing. In addition, the manufacturing cost of the alloy steel can be reduced by reducing the content of rare metals such as Cr, Mo, and V in the alloy steel to 5% by weight or less. Furthermore, since the alloy steel has excellent resistance to indentations (the material surface is less likely to be dented), it can be applied to sliding parts and bearing parts where a load (dynamic or static) is concentrated at a specific location. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As an embodiment of the present invention, the chemical components and the hardness of the surface and the inside of the alloy steel will be described. The C (carbon) content in the alloy steel of the present invention is 0.40 to 0.90% by weight. Carbon ensures the hardness of the steel after quenching and tempering, and plays a role in ensuring a high fatigue life when used as a material for mechanical parts. If the C content in the steel is below 0.40%, the required hardness of the surface and the inside cannot be obtained, and if it exceeds 0.90%, the amount of retained austenite (γ amount) increases, deteriorating the fatigue life of the mechanical parts.
[0016] The content of silicon (Si) is 0.70-2.50% by weight. Silicon plays a role in increasing the temper softening resistance of steel. If the Si content in steel is below 0.70%, the necessary temper softening resistance cannot be obtained, and if it exceeds 2.50%, the hot forgeability is significantly deteriorated. The Si content is preferably 1.50-2.50%.
[0017] The content of Mn (manganese) is 0.10 to 1.00% by weight. Manganese increases the hardenability of steel, and is effective in improving fatigue life when used as a mechanical part material. If the Mn content in steel is below 0.10%, the hardenability of the steel deteriorates, and if it exceeds 1.00%, the hot forgeability deteriorates significantly.
[0018] Cr (chromium) is 1.00 to 4.00% by weight. Chromium increases the hardenability of steel, thermally stabilizes cementite, and inhibits the cementite from dissolving in the matrix at high temperatures. If the Cr content in steel is below 1.00%, the hardenability of the steel deteriorates, and if it exceeds 4.00%, coarse carbides are generated in the steel.
[0019] Mo (molybdenum) is 0.20 to 1.50% by weight. Molybdenum forms carbides in steel and contributes to ensuring hardness. If the Mo content in steel is below 0.20%, the necessary tempering hardness and softening resistance cannot be obtained. If the Mo content exceeds 1.50%, coarse carbides are generated. Preferably, Mo is 0.20 to 0.70%.
[0020] The content of V (vanadium) is 0.05 to 0.80% by weight. V has the role of increasing temper softening resistance by adding it in combination with silicon in the steel. If the V content in the steel is less than 0.10%, the necessary temper softening resistance cannot be obtained, and if it exceeds 0.80%, coarse carbides are generated. The V content is preferably 0.05 to 0.40%.
[0021] The same effect can be obtained by including Nb (niobium) as a substitute element for V. In this case, the Nb content is preferably in the range of 0.025 to 0.40% by weight. W (tungsten) can also be included in the range of 0.40 to 3.00% by weight as the W equivalent (W+2Mo). In this case, tungsten forms carbides in the steel like molybdenum, and contributes to ensuring hardness. If the W equivalent in the steel is below 0.40%, the required tempering hardness and softening resistance cannot be obtained. On the other hand, if the W equivalent exceeds 3.00%, coarse carbides are generated.
[0022] In addition, the surface of the alloy steel of the present invention is formed with a hardened layer, either a carburized layer or a carbonitrided layer, and the surface hardness of this carburized layer or carbonitrided layer is preferably 800 HV or more in Vickers hardness.
Claims
1. An alloy steel consisting of, by weight, 0.40-0.90% C, 0.70-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-1.50% Mo, 0.05-0.80% V, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
2. An alloy steel comprising, by weight, 0.40-0.90% C, 0.70-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-1.50% Mo, 0.025-0.20% Nb, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
3. An alloy steel consisting of, by weight, 0.40-0.90% C, 0.70-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.40-3.0% W+2Mo, 0.05-0.80% V, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
4. An alloy steel consisting of, by weight, 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-0.70% Mo, 0.05-0.40% V, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
5. An alloy steel consisting of, by weight, 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.20-0.70% Mo, 0.025-0.20% Nb, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
6. An alloy steel consisting of, by weight, 0.40-0.90% C, 1.50-2.50% Si, 0.10-1.00% Mn, 1.00-4.00% Cr, 0.40-3.0% W+2Mo, 0.05-0.40% V, with the remainder being Fe and unavoidable impurities, wherein a hardened layer is formed on the surface of the alloy steel.
7. 2. The alloy steel according to claim 1, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
8. 3. The alloy steel according to claim 2, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
9. 4. The alloy steel according to claim 3, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
10. 5. The alloy steel according to claim 4, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
11. 6. The alloy steel according to claim 5, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
12. 7. The alloy steel according to claim 6, wherein the hardened layer is either a carburized layer or a carbonitrided layer, and the surface hardness is 800 HV or more in Vickers hardness.
13. A machine part made of the alloy steel according to any one of claims 1 to 12.
Citation Information
Patent Citations
Rolling bearing excellent in wear resistance
JP1996049057A