Galvanized steel sheet excellent in press-moldability, chemical conversion treatability and appearance quality and method for manufacturing galvanized steel sheet
A zinc-based plated steel sheet with controlled manganese and halogen ion content in an inorganic film addresses press formability and appearance issues by ensuring uniform chemical conversion films and improved sliding properties, enhancing the steel's overall performance.
Patent Information
- Application Number
- JP2023046169
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-23
AI Technical Summary
Zinc-based plated steel sheets used in automobile bodies face issues with press formability, chemical conversion treatment properties, and appearance quality due to the retention of rust preventive oil, leading to uneven chemical conversion films and impaired appearance after painting.
A zinc-based plated steel sheet with an inorganic film containing specific amounts of manganese, phosphorus, and halogen ions (Cl, S, F, Br) is treated with a solution of manganese ions, permanganate ions, and alkali metal or ammonium salts to enhance press formability, chemical conversion treatment properties, and appearance quality.
The solution ensures uniform chemical conversion films, improved sliding properties, and enhanced appearance quality by promoting rapid degreasing and uniform crystal size of the chemical conversion coating, maintaining the steel sheet's original characteristics.
Smart Images

Figure 2024135472000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a zinc-based plated steel sheet having excellent press formability, chemical conversion treatability and appearance quality, and a method for producing the same. [Background technology]
[0002] Zinc-plated steel sheets are used in automobile bodies and the like for the purpose of improving their corrosion resistance, appearance, etc. In the body manufacturing process by automobile manufacturers and the like, the car body is manufactured by press-forming the steel sheet, so the zinc-plated steel sheet that is formed into the complex shapes for the automobile body is required to have excellent press formability, and thus coating treatment technologies have been developed to impart high lubricity to the steel sheet surface.
[0003] Among them, phosphoric acid-based coatings have been used as lubricating coatings because they have excellent lubricity and can relatively easily form a uniform and adhesive coating by utilizing the chemical reaction between the plating surface and the treatment liquid. For example, Patent Document 1 shows a zinc-plated steel sheet having a prephosphate coating mainly composed of zinc phosphate. In this treatment, it is necessary to perform surface conditioning using a titanium colloid-containing aqueous solution and zinc phosphate colloid-containing water as a pretreatment for forming a dense coating.
[0004] On the other hand, manganese phosphate-based coatings are known to have a high lubricating effect even when thin, because they are hard among phosphoric acid-based coatings and have a high effect of suppressing plating from seizing the die even when formed under high surface pressure. For example, Patent Documents 2 to 7 disclose techniques for improving the press formability of steel sheets by applying a phosphoric acid-based inorganic lubricating coating mainly composed of manganese phosphate to the plating surface.
[0005] After manufacturing, plated steel sheets are shipped with anti-rust oil applied, and are then painted after press forming and joining by the automobile manufacturer. In the painting process, the steel sheet is first subjected to an alkaline degreasing treatment to remove the oil that has adhered to its surface, but if the steel sheet has been stored with the oil applied for a long time and the anti-rust oil and the steel sheet are strongly adsorbed, or if the degreasing liquid has been used continuously and a large amount of oil or metal ions have been mixed into the liquid, weakening its degreasing power, degreasing may not be performed sufficiently, adversely affecting the appearance after subsequent chemical conversion treatment or painting.
[0006] Specifically, if oil remains on the steel sheet surface even after degreasing, the formation reaction of the chemical conversion coating is inhibited at that portion, making the chemical conversion coating non-uniform, which results in uneven appearance after painting. In particular, in steel sheets provided with a lubricating coating for the purpose of improving press formability, including the above-mentioned phosphoric acid coating, this problem is likely to occur because the coating itself may have the effect of increasing lubricating oil retention, and therefore a technology for improving this problem has been required. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 4100358 [Patent Document 2] Patent No. 2131655 [Patent Document 3] Patent No. 2691797 [Patent Document 4] Patent No. 3199980 [Patent Document 5] Patent No. 4786769 [Patent Document 6] Patent No. 5146607 [Patent Document 7] Patent No. 5168417 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention overcomes the above-mentioned problems and provides a zinc-based plated steel sheet excellent in press formability, chemical conversion treatability and appearance quality, and a method for producing the same. [Means for solving the problem]
[0009] The gist of the present invention is as follows. (1) Mn: 1.0 mg / m on the surface of the zinc coating of hot-dip galvanized steel sheet 2 More than 100mg / m 2 Below, P:10.0mg / m 2 More than 100mg / m 2 The sum of the moles of one or more of Cl, S, F, and Br derived from chlorides, sulfates, fluorides, and bromides [A] is 1.0 x 10 -5 mol / m 2 Above 5.0×10 -3 mol / m 2 A zinc-based plated steel sheet having excellent press formability, chemical conversion treatability and appearance quality, characterized in that it is provided with an inorganic coating comprising the following and unavoidable impurities: (2) A zinc-based plated steel sheet excellent in press formability, chemical conversion treatability and appearance quality according to (1), characterized in that in the inorganic coating, a ratio [A] / [P] of the sum of the number of moles [A] in a range from the outermost layer to 2 nm, as measured with an X-ray photoelectron spectroscopy analyzer, to the number of moles of P [P], is 0.01 or more and 5.0 or less. (3) Manganese ions or permanganate ions are 0.01 mol / L or more and 2.5 mol / L or less, phosphate ions are 0.6 mol / L or more and 3.0 mol / L or less, and one or more of chloride ions, sulfate ions, fluoride ions, and bromide ions added to the solution as salts such as alkali metal salts, ammonium salts, and zinc compounds, rather than as acids, are added to the solution at a molar concentration of [A L ] and the molar concentration of phosphate ions [P L ] and the ratio [A L ] / [P L1. A method for producing a zinc-based plated steel sheet excellent in press formability, chemical conversion property and appearance quality, comprising contacting a plated surface with an aqueous solution containing residual unavoidable impurities for a period of 0.1 to 10 seconds, followed by drying to obtain the zinc-based plated steel sheet according to (1) or (2). Effect of the Invention
[0010] According to the present invention, it is possible to provide a zinc-based plated steel sheet excellent in press formability, chemical conversion treatability and appearance quality. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the relationship between [A] in a coating and chemical conversion treatability and sliding properties. [Diagram 2] FIG. 1 is a graph showing the relationship between the [AS] / [PS] ratio in a coating and chemical conversion treatability and sliding properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The details of the present invention are described below.
[0013] As a result of extensive investigations aimed at solving the above-mentioned problems, it was discovered that by incorporating an appropriate amount of a compound containing halogen ions such as fluoride ions, chloride ions, and bromide ions, and oxoacid ions such as sulfate ions (hereinafter referred to as ions group A) in an inorganic lubricating coating mainly composed of manganese phosphate as described in Patent Document 2, etc., it is possible to improve chemical conversion treatability without impairing sliding properties.
[0014] The metal salts of the above-mentioned ions of group A have a higher solubility in an alkaline aqueous solution than manganese phosphate, which is the main component of the inorganic coating. Therefore, it is believed that good chemical conversion properties can be obtained by dissolving and removing part of the coating together with the rust-preventive oil during alkaline degreasing treatment.
[0015] Furthermore, detailed investigations into the relationship between the state of the outermost surface of the inorganic coating and its chemical conversion properties and the surface appearance after painting revealed that the higher the ratio of group A ions to phosphate ions on the outermost surface, the more uniform the crystal size of the chemical conversion coating formed and the more beautiful the surface appearance after painting. This is thought to be because the presence of group A ions on the outermost surface speeds up the desorption reaction of the rust-preventive oil, so even if there are areas where the steel sheet and the rust-preventive oil are strongly adsorbed locally, the degreasing liquid will penetrate from the surrounding area and the rust-preventive oil can be removed from the entire surface, thereby increasing the uniformity of degreasing properties and chemical conversion properties.
[0016] In addition, since the degreasing treatment is performed after the steel sheet is pressed and assembled, the loss of part of the inorganic lubricating film during the degreasing treatment does not in any way impair the inherent property guaranteed by the lubricating film, that is, improving the sliding properties when the steel sheet is pressed.
[0017] The inorganic coating on the surface of the hot-dip galvanized base contains 1.0 mg / m2 of manganese. 2 More than 100mg / m 2 The manganese content is within the following range: 1.0 mg / m 2 If the manganese content is less than 100 mg / m, adhesion of the plating to the die cannot be sufficiently suppressed, and sufficient formability cannot be ensured. 2 If the temperature exceeds this range, the effect of inhibiting adhesion of the plating becomes saturated, and the chemical conversion treatability also deteriorates in the present invention.
[0018] In addition, the coating contains 10.0 mg / m 2 More than 100mg / m 2 The phosphorus content is within the following range: 10.0 mg / m 2 If the phosphorus content is less than 100 mg / m, the alloy will not adhere well to the rust-preventive oil during sliding processing, and sufficient moldability cannot be ensured. 2 If the temperature exceeds this range, the compatibility with the rust-preventive oil becomes saturated and the chemical conversion treatability also deteriorates in the present invention.
[0019] The appropriate amount of ions of group A to be contained in the film is expressed as the sum of the number of moles of ions of group A contained in the film per unit area [A], as shown in Figure 1. [A] is 1.0 × 10 -5 mol / m 2 Above 5.0×10 -3 mol / m 2 When the content of [A] is 1.0×10 or less, the effect of improving chemical conversion treatability can be obtained while ensuring good sliding properties. -5 mol / m 2 If the content is less than this, the effect of improving the chemical conversion treatability cannot be obtained, and if the content exceeds this, it becomes difficult to continuously form a hard manganese phosphate coating that ensures the sliding properties, and press formability deteriorates.
[0020] In addition, by increasing the proportion of group A ions in the outermost layer of the inorganic coating as shown in Figure 2, the uniformity of the degreasing and chemical conversion reaction is increased as described above, and the size of the chemical conversion coating crystals can be made more uniform, which is preferable. In order to achieve this, the total number of moles of one or more types of group A ions present in the outermost layer of the inorganic coating [A S ] and the number of moles of P present in the outermost layer [P S ] ratio [A S ] / [P S ] is 0.01 or more. On the other hand, this is [A S ] / [P S If [ ] becomes too large, the sliding properties tend to become somewhat inferior, so the upper limit is set to 5.0 or less.
[0021] Here, the outermost layer of the inorganic coating is defined as the average value of measurements of atomic concentration at three points, measured at equal intervals from the point where the atomic concentration of C is 10% or less toward the steel sheet side, to a depth of 2 nm, at 1 nm intervals. The atomic concentration is a value obtained by dividing the area intensity, when the background is removed from the peak of each element detected at the measurement site by the X-ray photoelectron spectrometer, by the relative sensitivity coefficient set for each device, and can be calculated using analysis software.
[0022] Furthermore, even if the coating contains unavoidable impurities in addition to the components contained in hot-dip galvanizing, there is no effect on the properties of the steel sheet such as sliding properties, chemical conversion properties, etc. Examples of unavoidable impurities include Li, Be, C, F, Na, Mg, Al, Si, Cl, K, Ca, Ni, Mo, V, W, Ti, Fe, Rb, Sr, Y, Zn, Nb, Cs, Ba, Cr, Cd, Pb, Sn, As, and lanthanides.
[0023] The hot-dip galvanized steel sheet on which the inorganic coating is formed may be one having a metal coating containing 50% or more Zn by mass concentration on the surface of a hot-rolled or cold-rolled steel sheet. The composition of the coating may be not only pure Zn, but also Zn-Fe, Zn-Ni, Zn-Al, Zn-Mn, Zn-Cr, etc., which contain Zn as the main component and one or more alloy elements and impurity elements such as Fe, Ni, Co, Al, Pb, Sn, Sb, Cu, Ti, Si, B, P, N, S, and O. In particular, the so-called alloyed hot-dip galvanized steel sheet, which is obtained by immersing a steel sheet in a Zn coating bath containing a small amount of Al and then subjecting it to heat treatment to contain about 5 to 20% Fe in the coating phase based on the total coating mass, is excellent in corrosion resistance after painting and spot weldability, and is suitable as the automotive steel sheet used in the present invention.
[0024] There are no particular restrictions on the coating weight of the plating, but considering the corrosion resistance of steel sheets for automobiles, the total of all components constituting the plating must be 20 g / m 2 If the coating weight is too high, the coating peels off during processing of the steel sheet and may remain on the die, causing imprint marks. Therefore, the upper limit is set to 100 g / m. 2 It is preferable that the present invention is not affected by the properties of the steel sheet that is the base material for hot-dip galvanizing, and there are no restrictions on the strength class, composition, or structure. Furthermore, there are no restrictions on the raw materials used in manufacturing the steel sheet or the manufacturing method of the steel sheet.
[0025] The method for producing this coating involves bringing a solution containing manganese ions or permanganate ions and phosphoric acid, and one or more of chloride ions, sulfate ions, fluoride ions, and bromide ions, which are added to the aqueous solution not as an acid but as a salt such as an alkali metal salt, ammonium salt, or zinc compound, into contact with the plating surface and then drying.
[0026] The acids of the above-mentioned oxo acid ion group and halogen ion group are strong acids or acids with extremely strong plating etching power. If they are mixed into the treatment solution in an acidic state, the dissolution reaction on the steel sheet surface may proceed excessively when the solution comes into contact with the steel sheet, potentially resulting in poor appearance. Therefore, they need to be added to the treatment solution as a salt.
[0027] Desirable types of salts include alkali metal salts, ammonium salts, zinc compounds, etc. The cations contained in these and compounds of ion group A have high solubility in aqueous solutions, so they do not adversely affect the effect of improving the chemical conversion treatability, and at the same time, they do not adversely affect other steel sheet properties such as sliding properties and corrosion resistance.
[0028] The composition of the treatment solution used may be adjusted to obtain an appropriate film state by taking into consideration the method of contacting the plating surface with a solution containing manganese ions or permanganate ions, phosphoric acid, and ions of group A, and the contact time. Preferably, the molar concentration of phosphorus [P L ] is 0.6 mol / L or more and 3.0 mol / L or less, and the total molar concentration of one or more of the ions in group A [A L ] and the molar concentration of phosphorus [A L ] / [P L It is preferable that the value of the viscosity of the solution is 0.2 or more and 1.5 or less, and that the solution is brought into contact with the plating surface for a period of 0.1 to 10 seconds, and then dried.
[0029] In the present invention, the inorganic film mainly composed of manganese phosphate formed on the plating surface is formed by a mechanism in which poorly soluble phosphate compounds precipitate by utilizing the increase in pH caused by dissolution of the plating surface when the plating surface is brought into contact with an acidic solution containing phosphoric acid. On the other hand, since the A group ions themselves cannot form poorly soluble compounds in response to pH fluctuations, it is necessary to incorporate the A group ions with the formation of the phosphate compounds. Therefore, in order to allow the A group ions to exist in an appropriate state in the inorganic film, it is necessary to control the formation rate of the phosphate compounds and the concentration of the A group ions in the solution.
[0030] [P L If the concentration is less than 0.6 mol / L, the film formation speed is low, so that the A group ions are expelled during the time-consuming process of forming the phosphate compound, and the A group ions cannot be sufficiently incorporated into the film. If the concentration is more than 3.0 mol / L, the amount of film formed becomes too large, and in a general film formation process, the amount of phosphate film becomes excessive, making it impossible to ensure chemical conversion treatment properties.
[0031] In addition, [A L ] / [P L If the ratio is less than 0.2, the necessary amount of ion group A cannot be incorporated into the coating, and sufficient improvement in chemical conversion treatability cannot be obtained. Conversely, if the ratio exceeds 1.5, sludge will adhere to the plating surface due to excessive dissolution of ion group A, causing the surface to discolor.
[0032] The time from when the above-mentioned treatment solution comes into contact with the steel sheet surface until it dries should be between 0.1 and 10 seconds. If it is less than 0.1 seconds, a sufficient phosphate film cannot be formed, and sliding properties cannot be ensured. On the other hand, if it is more than 10 seconds, the plating surface will be over-dissolved by ions of group A, causing sludge to adhere to the plating surface and discoloring the surface.
[0033] Methods for contacting the steel sheet with the treatment solution include a method in which the steel sheet is immersed in the treatment solution and then the amount of applied solution is made uniform by a wringer roll or gas wiping, and a roll coating method.
[0034] In addition, after contacting the steel sheet with the treatment solution, it is not necessarily required to rinse with water. If it is rinsed with water, the method is not particularly specified, but it can be done by immersion or spraying with water. In this case, excessive rinsing with water may cause the [A S ] / [P S ] may decrease, so it is important to adjust the washing time, water temperature, water pressure, etc. appropriately.
[0035] The treatment liquid or moisture is dried using a blower, a hot air oven, an IH heater, etc. The drying temperature is not particularly limited as long as the moisture can be removed within a specified time, but from the viewpoint of economic rationality, it is preferably 200° C. or less.
[0036] The content of each element and ion in the film can be measured by dissolving the film in chromic acid using ICP emission spectrometry or the like. For oxoacid ions, the molar concentration in the film can be obtained by measuring the content of chlorine, sulfur, and other halogen ions, which are elements that make up oxoacids, using the above method. In addition, the amount of elements present on the film surface can be quantitatively evaluated using fluorescent X-rays using a calibration curve created using ICP emission spectrometry or the like. For the type of oxoacid, the state of chlorine and sulfur on the film surface and in the film can be identified using photoelectron spectroscopy (XPS) or the like. Note that before the above analysis, the sample is ultrasonically cleaned using hexane or ethanol to remove surface oil and dirt. EXAMPLES
[0037] The present invention will now be described in a non-limiting manner with reference to examples. The galvannealed steel sheets to which the inorganic coating was applied were galvannealed steel sheets (AS, Fe: 10 mass%, Al: 0.2 mass%, balance Zn) and galvannealed steel sheets (GI). The treatment solution having the conditions shown in Table 1 was applied with a roll coater and then dried at 50°C in a hot air drying furnace to form a coating.
[0038] [Table 1]
[0039] <Chemical conversion treatment> The specimen was a plated steel sheet with the above-mentioned inorganic lubricant coating applied with rust-preventive oil (Noxrust 550HN, manufactured by Nihon Parkerizing Co., Ltd.) at 2.0 g / m on one side. 2 The specimen was used. In order to deteriorate the ability of the degreasing liquid, the specimen was immersed for 90 seconds in the degreasing liquid Fine Cleaner 4380 (40°C, manufactured by Nihon Parkerizing Co., Ltd.) to which 5g / L of the above-mentioned rust-preventive oil and 100ppm each of iron and zinc were added. The specimen was then immersed for 30 seconds in the surface conditioner Parkore Z (manufactured by Nihon Parkerizing Co., Ltd.), and then immersed for 90 seconds in PB-3080 (manufactured by Nihon Parkerizing Co., Ltd., liquid temperature 43°C). The quality of the chemical conversion coating was judged by SEM observation (secondary electron beam image), and the evaluation criteria below were evaluated as ◎ and ○. Evaluation criteria: ◎: A dense chemical conversion film with crystal size of 1 to 10 μm is formed. ○: There is some variation in the crystal size, but a dense, opaque chemical coating of 1 to 10 μm is formed. △: The chemical conversion coating is formed without any transparency, but there are crystals larger than 10 μm in size. ×: The chemical conversion film is not formed in part.
[0040] <Sliding properties> After the coating process, the sample was cut to a width of 17 mm and a length of 300 mm, and coated with Noxrust 550HN (manufactured by Nippon Parkerizing Co., Ltd.) at 1 g / m 2 After oiling, a drawbead test was performed at a pulling speed of 500 mm / min. The pressing load was changed from 200 to 800 kgf (1.96 × 103 to 7.84 × 103 N) to measure the pull-out load, and the slope was calculated from a plot with the pressing load as the horizontal axis. This was multiplied by 2 to obtain the coefficient of friction. The following evaluation criteria of ◎ and ○ were used to determine pass. Evaluation criteria: ◎: Friction coefficient is less than 0.15 ○: Friction coefficient is less than 0.20 △: Friction coefficient is 0.20 or more and less than 0.30 ×: Friction coefficient is more than 0.30
[0041] <Appearance evaluation> After the formation of the coating, the zinc-plated steel sheet was visually evaluated for uneven appearance. The observation area was 210 mm × 300 mm, and the evaluation was performed according to the following criteria, with ○ being evaluated as passing. Evaluation criteria: ○: No unevenness that can be visually confirmed exists. △: The area ratio of clear unevenness that can be visually confirmed is less than 50%. ×: The area ratio of the unevenness clearly visible to the naked eye is 50% or more.
[0042] As shown in Table 1, for the samples (Levels 1 to 31) produced under conditions within the range of the present invention, galvanized steel sheets having good chemical conversion treatability, excellent sliding properties, and good appearance were obtained.
[0043] Of these, levels 8 and 17 passed the chemical conversion treatment test, but the [A S ] / [P S ] was slightly low, so there was some unevenness in the crystal size of the chemical conversion coating.
[0044] On the other hand, in the comparative examples of levels 32 to 34, the total amount of element A in the coating was less than the range of the present invention, and sufficient chemical conversion treatability was not obtained. Also, in level 35, the total amount of element A in the coating was greater than the range of the present invention, and sufficient sliding properties were not obtained.
[0045] In levels 36 and 37, the amount of P or Mn in the coating was less than the range of the present invention, and sufficient sliding properties could not be obtained. In levels 38 and 39, strong acids such as sulfuric acid and hydrochloric acid were added to the treatment solution, which caused uneven treatment and resulted in uneven appearance.
Claims
1. On the surface of the zinc coating of the hot-dip galvanized steel sheet, Mn: 1.0 mg / m 2 More than 100mg / m 2 Below, P: 10.0mg / m 2 More than 100mg / m 2 The sum of the moles of one or more of Cl, S, F, and Br derived from chlorides, sulfates, fluorides, and bromides [A] is 1.0×10 -5 mol / m 2 Above 5.0 x 10 -3 mol / m 2 A zinc-based plated steel sheet having excellent press formability, chemical conversion treatability and appearance quality, characterized in that it is provided with an inorganic coating comprising the following and unavoidable impurities:
2. 2. The zinc-based plated steel sheet according to claim 1, wherein in the inorganic coating, a ratio [A] / [P] of the sum [A] of the number of moles in a range from the outermost layer to 2 nm, as measured with an X-ray photoelectron spectroscopy analyzer, to the number of moles of P [P], is 0.01 or more and 5.0 or less.
3. Manganese ions or permanganate ions are 0.01 mol / L or more and 2.5 mol / L or less, phosphate ions are 0.6 mol / L or more and 3.0 mol / L or less, and one or more of chloride ions, sulfate ions, fluoride ions, and bromide ions, which are added to the solution not as acids but as salts such as alkali metal salts, ammonium salts, and zinc compounds, are added to the solution at a molar concentration of their sum [A L ] and the molar concentration of phosphate ions [P L ] to the ratio [A L ] / [P L 3. A method for producing a zinc-based plated steel sheet excellent in press formability, chemical conversion treatability and appearance quality, comprising contacting a plated surface with an aqueous solution containing residual unavoidable impurities for a period of 0.1 to 10 seconds, followed by drying to obtain the zinc-based plated steel sheet according to claim 1 or 2.
Citation Information
Patent Citations
Galvanized steel sheet excellent in weldability, workability in pressing and chemical convertibility
JP1992088176A
Galvannealed steel sheet having excellent coating finishability, pressability and chemical conversion treatability
JP1994088190A
Galvanized steel sheet excellent in lubricity, chemical conversion treatment property and compatibility with adhesive
JP1996296066A
Galvanized steel sheet excellent in corrosion resistance, chemically treating solution and chemical conversion treating method
JP2002030459A
Surface treating solution and surface treating method for galvanized steel sheet having excellent corrosion resistance after working
JP2002105659A