Method of manufacturing aluminum-ceramic bonded substrate

Ultrasonic treatment of molten aluminum alloys with Cu, Ti, and B enhances the crack resistance of ceramic plates in aluminum-ceramic bonded substrates, addressing the issue of heat cycle-induced cracking.

JP2024136046APending Publication Date: 2024-10-04TOHOKU UNIV +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023047000
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Aluminum-ceramic bonded substrates face issues with increased crack resistance due to heat cycles, particularly when reinforced with aluminum-based members, leading to potential ceramic plate cracking.

Method used

Applying ultrasonic vibration to a molten aluminum alloy containing Cu, Ti, and B, followed by solidification, to enhance the crack resistance of ceramic plates in aluminum-ceramic bonded substrates.

Benefits of technology

Significantly improves the cracking resistance of ceramic plates against heat cycles by using a molten metal bonding method with ultrasonic-treated aluminum alloys, maintaining strength and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136046000001_ABST
    Figure 2024136046000001_ABST
Patent Text Reader

Abstract

To improve heat cycle resistance of an aluminum-ceramic bonded substrate using an aluminum alloy to which an alloying element contributing to strengthening is added.SOLUTION: An aluminum alloy solid material comprising a solidified material specified in (A) below is melted to form a molten aluminum alloy, and the molten aluminum is solidified in contact with the surface of a ceramic sheet arranged in a mold. (A) The solidified material is obtained by forming a metal melt having a composition consisting of 0.10-1.20% by mass of Cu, 0-0.40% of Mg, 0.01-0.20% of Ti, 0.001-0.10% of B, 0-0.50% of the total of elements other than Cu, Mg, Ti, B and Al, and the balance of Al, subjecting the metal melt to a treatment for imparting ultrasonic vibration to the metal melt when the temperature of the metal melt is in the range of 680-720°C, and then solidifying the metal melt subjected to the treatment.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an "aluminum-ceramic bonded substrate" in which a ceramic plate is bonded to a plate-like member made of an aluminum-based material, which is useful as an insulating circuit board for mounting semiconductor elements. [Background technology]

[0002] In semiconductor devices that generate a large amount of heat, such as power modules, an insulated circuit board is generally used in which a "circuit member" made of a plate-shaped metal is bonded to the surface of a ceramic plate, and a semiconductor element is mounted on the circuit member by a method such as soldering. Copper-based or aluminum-based metal materials with good electrical conductivity are used as the circuit member. Among these, insulated circuit boards using aluminum-based circuit members (aluminum-ceramic bonded boards) are advantageous in terms of the resistance of ceramic plates to damage in heat cycles that repeatedly raise and lower the temperature, and thus demand is expected to increase in automotive applications and other areas.

[0003] As a manufacturing method for aluminum-ceramic bonded substrates, a "molten metal bonding method" is known in which a ceramic plate and a circuit member made of an aluminum alloy are directly bonded by solidifying a molten aluminum alloy on the surface of the ceramic plate. According to the molten metal bonding method, a "base member" that improves the strength of an insulating circuit board and is responsible for heat conduction for heat dissipation can be formed on the back surface of the ceramic plate (the surface opposite to the surface on which the circuit members are formed) at the same time as the circuit members. In this specification, an aluminum-ceramic bonded substrate having a structure in which a circuit member is bonded to one surface of a ceramic plate and a base member is bonded to the other surface, and the circuit member, ceramic plate, and base member are integrated, is called an "integrated base aluminum-ceramic bonded substrate."

[0004] In the molten metal bonding method, the circuit components made of aluminum alloys become solidified structures, and unlike processed products such as rolled materials, the crystal grains tend to become coarse. If the crystal grain size of the circuit components is large, repeated deformation accompanying temperature rise and fall while the circuit components are restrained by the ceramic plate can cause steps to form in the grain boundaries exposed on the surface of the circuit components, resulting in unevenness on the semiconductor element mounting surface. If the surface steps are large, there is a risk of damage to the semiconductor elements mounted on that surface.

[0005] Patent Document 1 discloses a technique for applying an aluminum alloy containing Ti and B as a grain refinement technique for aluminum-based members in a molten metal joining method. In this technique, it is preferable to prevent solidification nuclei components such as TiAl3, AlB2, and TiB2 contained in the molten metal from dissolving by generating the molten aluminum alloy at a relatively low temperature, and to suppress the dissolution of Ti and B into Al by quickly pouring the molten metal into a mold (see paragraph 0020 of Patent Document 1). By utilizing this technique, the above-mentioned problems related to damage to semiconductor elements can be significantly reduced.

[0006] Meanwhile, Patent Document 2 describes that when casting aluminum, the effect of controlling the solidification structure can be obtained by irradiating the molten metal with ultrasonic waves. The molten metal can be irradiated with ultrasonic waves by inserting an ultrasonic horn into the molten metal flowing through a moving trough or into the molten metal in a mold (paragraph 0002). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2019-141879 A [Patent Document 2] JP 2011-177787 A Summary of the Invention [Problem to be solved by the invention]

[0008] Recently, there is an increasing demand for miniaturization of aluminum-ceramic bonded substrates, and therefore, high strength is also important. For example, the application of base-integrated aluminum-ceramic bonded substrates and high strength of the aluminum-based components that compose them are advantageous for miniaturizing aluminum-ceramic bonded substrates. In addition to utilizing the strength improvement effect of grain refinement by adding Ti and B, the addition of precipitation strengthening elements is also considered to be effective as a method for increasing the strength of aluminum-based components in cast products manufactured by the molten metal bonding method. However, as the strength of aluminum-based components increases, ceramic plates that are constrained at the joint surface with the aluminum-based components (insulating ceramic plates between circuit components and base components, and ceramic plates that are sometimes used as reinforcing members) are repeatedly subjected to severe restraining stress from the aluminum-based components when heat cycles are applied, making them more susceptible to cracking.

[0009] The present invention aims to provide a technology for significantly improving the crack generation resistance against heat cycles of a ceramic plate, which is a constituent member of an aluminum-ceramic bonding substrate made using an aluminum alloy to which alloy elements that contribute to strengthening have been added, and to provide a base-integrated aluminum-ceramic bonding substrate obtained by this technology. [Means for solving the problem]

[0010] As a result of research, the inventors found that the crack generation resistance of the ceramic plate against heat cycles can be significantly improved by applying ultrasonic vibration to a molten aluminum alloy containing a predetermined amount of Cu, Ti, and B, remelting the solidified product, and manufacturing an aluminum-ceramic bonded substrate by a molten metal bonding method. It was also confirmed that adding Mg together with Cu is also effective. The present invention was made based on these findings. That is, in order to achieve the above object, in the present invention, an aluminum alloy solid material is prepared in advance by a method of applying ultrasonic vibration to a molten aluminum alloy containing Cu, Ti, B, and if necessary, Mg, and then solidifying the molten aluminum alloy, and the aluminum alloy solid material is used as a raw material for forming the molten aluminum alloy in the molten metal bonding method. Specifically, the following inventions are disclosed in this specification.

[0011] [1] A method for producing an aluminum-ceramic bonding substrate, comprising melting an aluminum alloy solid material consisting of a solidified product as defined in (A) below to produce a molten aluminum alloy, and solidifying the molten aluminum alloy in contact with the surface of a ceramic plate placed in a mold, thereby bonding an aluminum alloy member to one or both sides of the ceramic plate. (A) A molten metal having a composition, by mass%, of Cu: 0.10-1.20%, Mg: 0-0.40%, Ti: 0.01-0.20%, B: 0.001-0.10%, the sum of elements other than Cu, Mg, Ti, B, and Al: 0-0.50%, and the balance being Al is formed, and when the temperature of the molten metal is in the range of 680-720°C, ultrasonic vibrations are applied to the molten metal, and then the molten metal that has been subjected to the above-mentioned treatment is solidified to obtain a solidified material. [2] The method for producing an aluminum / ceramic bonding substrate according to the above [1], wherein the treatment of applying ultrasonic vibration is a treatment of applying ultrasonic vibration having a vibration amplitude of 10 to 80 μm (pp). [3] The method for producing an aluminum-ceramic bonding substrate according to [1] or [2] above, wherein the aluminum-ceramic bonding substrate has a structure in which aluminum alloy members are bonded to both sides of a ceramic plate, one of the two aluminum alloy members being a circuit member for mounting a semiconductor element, and the other being a base member having a larger volume than the ceramic plate. [4] The method for producing an aluminum / ceramic bonding substrate according to [3] above, wherein the base member is provided with a reinforcing member on a portion other than the bonding surface with the ceramic plate. [5] The method for producing an aluminum / ceramic bonding substrate according to the above [4], wherein the reinforcing member is made of a ceramic plate.

[0012] Here, the "(pp)" in the vibration amplitude means that it is the amplitude measured in the peak-to-peak mode. The presence or absence of cracks in the ceramic plate can be checked by ultrasonic flaw detection. Effect of the Invention

[0013] According to the present invention, it is possible to obtain, by a molten metal bonding method, an aluminum-ceramic bonding substrate in which an aluminum alloy containing strengthening elements is used for circuit members or base members, in which the resistance to crack generation in the ceramic plate due to heat cycles is significantly improved. [Brief description of the drawings]

[0014] [Figure 1] 1 is a cross-sectional view showing a schematic example of one embodiment of a cross-sectional structure of an aluminum / ceramic bonding substrate according to the present invention. [Diagram 2] 1 is a cross-sectional view showing a schematic example of one embodiment of a cross-sectional structure of an aluminum / ceramic bonding substrate according to the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic example of an arrangement in a mold for producing an aluminum / ceramic bonding substrate having the cross-sectional structure shown in FIG. 1. [Figure 4]3 is a cross-sectional view showing a schematic example of an arrangement in a mold for producing an aluminum / ceramic bonding substrate having the cross-sectional structure shown in FIG. 2. [Diagram 5] FIG. 4 is a cross-sectional view showing a state in which molten metal has been introduced into the mold shown in FIG. 3 . [Figure 6] FIG. 5 is a cross-sectional view showing the state in which molten metal has been introduced into the mold shown in FIG. 4. [Figure 7] FIG. 1 is a cross-sectional view showing a schematic example of a configuration of a melting apparatus for producing an aluminum alloy solid material used in a molten metal joining method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] [Aluminum-ceramic bonding substrate] The aluminum-ceramic bonding substrate is an insulating substrate for mounting a semiconductor element, and has a laminated structure in which a plate-shaped aluminum alloy member serving as a circuit member is bonded to one surface of a ceramic plate. An aluminum alloy member responsible for heat transfer for heat dissipation may be bonded to the surface of the ceramic plate opposite the circuit member. The aluminum alloy member bonded to the surface of the ceramic plate opposite the circuit member may be referred to as a "back member" in this specification.

[0016] FIG. 1 shows a schematic example of one embodiment of the cross-sectional structure of an aluminum-ceramic bonded substrate of the present invention. A circuit member 20 made of a plate-shaped aluminum alloy member is bonded to one side of a ceramic plate 10. The circuit member 20 is formed by solidifying molten aluminum alloy on the surface of the ceramic plate 10 by a molten metal bonding method described later. A semiconductor element is mounted on the surface of the circuit member 20. Since the circuit member 20 is an aluminum alloy, the upper surface (semiconductor element mounting surface 22) of the circuit member 20 is usually plated with Ni or the like to improve solder wettability, and then the semiconductor element is bonded to the plated layer via a solder layer. The thickness of the ceramic plate 10 varies depending on the specifications of the semiconductor device, but can be set in the range of 0.3 to 1.5 mm, for example. The thickness of the circuit member 20 can be set in the range of 0.3 to 1.5 mm, for example. In FIG. 1, the thickness of each member is exaggerated.

[0017] Materials that have been conventionally used for insulating substrates for mounting semiconductors, as well as new ceramics that may be developed in the future and have excellent strength and thermal conductivity, can be used for the material of the ceramic plate 10. Known ceramics include those containing one or more of aluminum nitride (AlN), aluminum oxide (Al2O3), silicon nitride (Si3N4), and silicon carbide (SiC) as the main component (containing 50 mass% or more).

[0018] In the example of FIG. 1, a base member 50 using an aluminum alloy as a back member is bonded to the surface of the ceramic plate 10 opposite to the circuit member 20, thereby constructing a base-integrated aluminum-ceramic bonding substrate. The base member 50 is a heat dissipation member and a member that is responsible for the strength with which the ceramic plate bonded to the circuit member can be attached to the inside of a semiconductor device or to a housing, and it is preferable that the base member 50 has a larger volume than the ceramic plate 10. The base member 50 can be provided with a reinforcing member 110 as necessary in a portion other than the bonding surface with the ceramic plate 10. In the illustrated embodiment, the reinforcing member 110 is embedded in the aluminum alloy that constitutes the base member 50. As the reinforcing member 110, one or more of the above-mentioned ceramic materials, metal materials having a melting point higher than that of the aluminum alloy, and fire-resistant materials other than ceramics and metals (e.g., carbon materials) can be used. The reinforcing member 110 is preferably in the form of a plate or sheet. Even in the case of the base member 50 using the reinforcing member 110, the joint surface with the ceramic plate 10 is made of an aluminum alloy, and therefore this type of base member 50 also falls under the category of the aluminum alloy member as defined in this specification.

[0019] The aluminum alloy that is the constituent material of the circuit members and base member has the chemical composition described below.

[0020] FIG. 2 shows a schematic example of one embodiment of the cross-sectional structure of the aluminum-ceramic bonding substrate of the present invention, which has a base member having a structure in which pin-shaped protrusions are integrated as a back member. Here, a cross section of a portion in which two circuit members 20 are arranged side by side is shown. The two circuit members 20 are electrically insulated from each other by a groove portion 21 formed on the ceramic plate 10. In addition, a plurality of pin-shaped protrusions 53 are formed on the base member 50. Depending on the arrangement of the pin-shaped protrusions 53, some of the pin-shaped protrusions at the back may be visible between the pin-shaped protrusions 53 shown in FIG. 2, but the pin-shaped protrusions at the back are not shown here. The pin-shaped protrusions 53 have a heat sink function to enhance heat dissipation. In this example, the end of the base member 50 perpendicular to the thickness direction is integrated with a peripheral wall portion 51 that surrounds the end face of the ceramic plate 10. That is, the base member 50 in Fig. 2 is joined to the ceramic plate 10 on almost the entire surface of the ceramic plate 10 opposite to the surface on which the circuit members 20 are formed, on the end faces (side faces) of the ceramic plate 10, and around the surface on which the circuit members 20 are formed. The peripheral wall portion 51 and the circuit members 20 are electrically insulated from each other by a groove portion 52 formed on the ceramic plate 10. The base member 50 having the pin-shaped projections 53 and the peripheral wall portion 51 can also be formed by casting a molten aluminum alloy using the molten metal joining process for forming the circuit members 20. As a member for enhancing heat dissipation, for example, a heat dissipation fin made of a plate-shaped member can also be formed by casting using the molten metal joining process instead of the pin-shaped projections 53.

[0021] [Aluminum alloy] In the present invention, the aluminum alloy constituting the circuit member 20, and, if the base member 50 is provided, the aluminum alloy constituting the base member 50, has the following chemical composition. An aluminum alloy having a composition, by mass%, of Cu: 0.10 to 1.20%, Mg: 0 to 0.40%, Ti: 0.01 to 0.20%, B: 0.001 to 0.10%, the sum of elements other than Cu, Mg, Ti, B, and Al: 0 to 0.50%, and the balance being Al.

[0022] In this specification, "%" in the chemical composition of the alloy means "mass %" unless otherwise specified. In the present invention, Cu is used among elements that are considered to contribute to the high strength of aluminum alloys by precipitation strengthening. It has been found that when Cu is used, the crack generation resistance of ceramic plates against heat cycles can be significantly improved by applying the manufacturing technology of applying ultrasonic vibration described below. In order to fully exert this effect, a Cu content of 0.10% or more is ensured. When the Cu content is in the range of 0.10% to 1.20%, high strength and the above-mentioned crack generation resistance can be obtained while avoiding excessive reduction in electrical conductivity. The Cu content is more preferably 0.15 to 0.90%, and even more preferably 0.20% to 0.80%.

[0023] Mg is an optional element that contributes to high strength together with Cu and does not adversely affect the crack generation resistance of the ceramic plate in heat cycles, so it can be added as necessary. It is more effective to set the Mg content to 0.05% or more. In addition, excessive reduction in electrical conductivity can be avoided by setting the Mg content to 0.40% or less. The Mg content may be controlled to a range of 0.30% or less.

[0024] Since Ti and B have a grain refining effect, these elements are also contained in the present invention. The Ti content may be adjusted to the range of 0.01 to 0.20%, and the B content may be adjusted to the range of 0.001 to 0.10%. Elements other than Cu, Mg, Ti, B, and Al are permitted to be contained in a total content of 0.50% or less, with the balance being Al. The total content of elements other than Cu, Mg, Ti, B, and Al may be controlled to 0.20% or less.

[0025] [Molt metal joining method] In the present invention, a known molten metal joining method can be used, except that an aluminum alloy solid material consisting of a solidified product previously melted by a method described below is used as the raw material of the molten aluminum alloy used in the molten metal joining. The molten metal joining is mainly realized by a "member arrangement process" and a "joining process." Preferred embodiments of the molten metal joining method applicable to the present invention are exemplified below, but are not limited to these.

[0026] (Component placement process) The member placement step is a step of placing members, such as ceramic plates to which the molten aluminum alloy is to be joined, in the mold. FIG. 3 is a cross-sectional view showing a schematic example of the arrangement in a mold for producing an aluminum-ceramic bonded substrate having the cross-sectional structure shown in FIG. 1. The mold 1 is composed of an upper mold 1a and a lower mold 1b. The upper mold 1a and the lower mold 1b are made of a carbon material or a metal material having gas permeability. The mold 1 has a molten metal section 5 formed by the internal space of the upper mold 1a and the lower mold 1b. The molten metal section 5 is a space for storing molten metal to be supplied to the product shape space inside the mold. The molten aluminum alloy can also be obtained by melting an aluminum alloy solid material in the molten metal section 5. In that case, the molten metal section 5 also functions as a crucible. The upper part of the molten metal section 5 has a pressure port 2, and pressure is applied to the molten metal in the molten metal section 5 from the outside of the mold 1 through the pressure port 2 to send the molten metal in the molten metal section 5 to the product shape space. The lower mold 1b has a runner 3 for supplying the molten metal in the molten metal section 5 to each part in the mold. In the example of Fig. 3, a narrow cross-section flow path 103, which narrows the cross section of the flow path through which the molten metal passes, is provided in a part of the runner 3. When the molten aluminum alloy passes through the narrow cross-section flow path 103, the oxide film on the surface of the molten metal is removed.

[0027] The ceramic plate 10 is placed at a predetermined position (ceramic plate receiving portion) of the lower die 1b. In the example of FIG. 3, a plate-shaped reinforcing member 110 is placed on a support portion (not shown) provided inside the lower die 1b, and is placed at a predetermined position. A space A is formed between the ceramic plate 10 and the inner wall surface of the lower die 1b. The space A is connected to the molten metal storage portion 5 by a runner (not shown) in the lower die 1b. The aluminum alloy molten metal filled in the space A solidifies to form a plate-shaped circuit member (reference numeral 20 in FIG. 1). A space B is formed on the upper surface side of the ceramic plate 10 so as to surround the reinforcing member 110. The space B is connected to the molten metal storage portion 5 by a runner in the lower die 1b. The aluminum alloy molten metal filled in the space B solidifies to form a heat dissipation member (reference numeral 50 in FIG. 1) incorporating the reinforcing member 110. The ceramic plate 10 and the reinforcing member 110 are both restrained in position by a supporting member or a clamping member inside the mold so that they do not shift from their predetermined positions when molten metal is poured in the joining process. In Figure 3, the thickness of the ceramic plate 10, the thickness of the reinforcing member 110, the distance between the ceramic plate 10 and the lower mold 1b in space A, the distance between the ceramic plate 10 and the reinforcing member 110 in space B, and the distance between the reinforcing member 110 and the upper mold 1a in space B are each exaggerated.

[0028] FIG. 4 is a cross-sectional view showing a schematic example of the arrangement in a mold for producing an aluminum-ceramic bonded substrate having the cross-sectional structure shown in FIG. 2. In this case, the space B has a plurality of pin-shaped recesses 4 formed by the wall surface of the upper mold 1a. The aluminum alloy melt filled in the pin-shaped recesses 4 solidifies to form pin-shaped protrusions (reference numeral 53 in FIG. 2) having a heat sink function. The mold structure in FIG. 4 is basically the same as that in FIG. 3, except that the pin-shaped recesses 4 are formed, the arrangement of the ceramic plate 10, the space A, and the space B is different, and there is no structure for installing a reinforcing member (reference numeral 110 in FIG. 3). The ceramic plate 10 is restrained in position by a support member or a clamping member inside the mold so that it does not move from a predetermined position when the melt is poured in during the bonding process.

[0029] (Joining process) The joining process is a process in which a molten aluminum alloy is poured into a mold, and the molten aluminum alloy is solidified while being in contact with the surface of a ceramic plate or further a reinforcing member placed inside the mold, thereby forming a structure in which the aluminum alloy member derived from the molten aluminum alloy and the ceramic plate or further a reinforcing member are joined together.

[0030] 5 and 6 are cross-sectional views of the molds shown in FIGS. 3 and 4, respectively, in which molten metal has been introduced. Casting for molten metal joining is performed, for example, as follows. A mold 1 is prepared in which a ceramic plate 10 and, if necessary, a reinforcing member 110 are set as described above. When the molten metal storage section 5 is used as a crucible, an aluminum alloy solid material, which is a raw material for the molten aluminum alloy, is placed in the molten metal storage section 5 in the form of, for example, granules or small pieces. The mold 1 is placed in a heating furnace and heated in a non-oxidizing gas atmosphere such as nitrogen gas. When using an aluminum alloy molten metal obtained by melting an aluminum alloy solid material in a melting furnace outside the mold 1, the molten metal is introduced into the molten metal storage section 5 through the pressurizing port 2. When the molten metal storage section 5 is used as a crucible, an aluminum alloy solid material, which is a raw material, is melted in the molten metal storage section 5 to obtain an aluminum alloy molten metal.

[0031] After the mold has reached a predetermined temperature (e.g., 700-725°C), it is pressurized with an inert gas such as nitrogen gas at a pressure of, for example, 5-50 kPa from the pressurizing port 2, and the molten aluminum alloy 100 contained in the molten metal storage section 5 (i.e., the molten aluminum alloy solid material prepared by the method described below) is poured into the space in the mold via the runner 3 (a runner not shown in the space A). In the present invention, when obtaining the molten aluminum alloy to be poured into the mold, it is not necessary to adjust the composition using a solid metal such as a refiner, and it is sufficient to melt only a single type of aluminum alloy solid material prepared in advance, so that the pouring of the molten metal (pouring) can be started immediately once the aluminum alloy solid material is completely melted and reaches a predetermined pouring temperature.

[0032] In the example of FIG. 5 and FIG. 6, the molten aluminum alloy 100 passes through the narrow cross-section flow path 103, and thus an oxide film formed on the surface of the molten aluminum alloy is removed. After the entire space in the mold connected by the runner is filled with the molten aluminum alloy 100, solidification begins. As a method of solidification, it is preferable to perform directional solidification by contacting a part of the outer wall of the mold 1 (for example, the left end of FIG. 5 and FIG. 6) with a water-cooled copper block as a cooling device. In order to prevent casting defects such as shrinkage cavities, it is preferable to proceed with solidification while continuing to apply pressure at a pressure of, for example, 5 to 50 kPa with an inert gas such as nitrogen gas from the pressurizing port 2. The aluminum alloy member obtained by solidifying the molten aluminum alloy 100 in the space A and the space B is formed by remelting and then resolidifying an aluminum alloy solid material produced by a method described later.

[0033] [Method of manufacturing aluminum alloy solid materials] In the present invention, an aluminum alloy solid material consisting of a solidified product as specified in (A) below is used as the raw material of the aluminum alloy molten metal to be poured into a mold in the molten metal joining method. (A) A molten metal having a composition, by mass%, of Cu: 0.10-1.20%, Mg: 0-0.40%, Ti: 0.01-0.20%, B: 0.001-0.10%, the sum of elements other than Cu, Mg, Ti, B, and Al: 0-0.50%, and the balance being Al is formed, and when the temperature of the molten metal is in the range of 680-720°C, ultrasonic vibrations are applied to the molten metal, and then the molten metal that has been subjected to the above-mentioned treatment is solidified to obtain a solidified material. Hereinafter, the process of applying ultrasonic vibrations to molten metal may be simply referred to as "ultrasonic treatment."

[0034] An aluminum alloy solid material for use in the molten metal joining method can be produced, for example, by the following process. (Example of the manufacturing process for aluminum alloy solid materials) (Step 1) A molten metal having the composition described above in (A) is obtained. (Step 2) The molten metal is solidified to obtain a master alloy. (Step 3) The master alloy is remelted to obtain a molten metal. (Step 4) The molten metal is subjected to ultrasonic treatment. (Step 5) The molten metal after ultrasonic treatment is solidified to obtain a solidified product. Alternatively, ultrasonic treatment may be directly applied to the molten metal obtained by the above step 1. In this case, steps 2 and 3 can be omitted, but in mass production, it may be advantageous to prepare a master alloy to be subjected to ultrasonic treatment in advance via steps 2 and 3 in order to improve productivity. Below, a method for preparing an aluminum alloy solid material will be described using the above steps 1 to 5 as an example. The following are examples of preferred embodiments, and the present invention is not limited to these.

[0035] (Process 1) Pure Al can be used as the Al raw material, an Al-Cu mother alloy can be used as the Cu raw material, and when Mg is to be contained, metallic magnesium can be used as the Mg raw material. These raw materials are placed in a crucible so as to have a predetermined composition, and are melted by heating to obtain a molten Al-Cu-(Mg) alloy (molten metal). The temperature of the molten metal is raised to 730°C or higher, and an Al-Ti alloy containing, for example, about 10% by mass of Ti as the Ti raw material and an Al-B alloy containing, for example, about 4% by mass of B as the B raw material are respectively charged into the molten metal, and Ti and B are completely dissolved in the liquid phase of the Al alloy. In order to prevent the generation of TiB2, it is preferable that the molten metal temperature when the Ti raw material and the B raw material are charged is 730°C or higher, but it is more preferable to raise the temperature to a higher temperature range, for example, a temperature of 750 to 850°C. The amount of the Al-Ti alloy and the Al-B alloy charged is adjusted so that the molten metal has a target composition in the range of Ti: 0.01 to 0.20% by mass and B: 0.001 to 0.10% by mass. It is more preferable that the content ratio of Ti to B is set so that the mass ratio of Ti:B is 1:1 to 6:1. The gas phase space in contact with the molten metal may be an air atmosphere or an inert gas atmosphere such as nitrogen gas.

[0036] (Process 2) The molten metal obtained in step 1 is cast into a mold and solidified to obtain a master alloy.

[0037] (Step 3) The master alloy obtained in step 2 is remelted in a melting device equipped with a mechanism capable of applying ultrasonic vibration to obtain a molten Al-Cu-(Mg)-Ti-B alloy. FIG. 7 shows a schematic cross-sectional view of an example of the melting apparatus. A crucible 71 is installed inside a furnace 70. The mother alloy obtained in step 2 is placed in the crucible 71, and the mother alloy is heated and melted in the furnace 70 to form a molten metal 72. Sub-materials other than the mother alloy may be added to adjust the composition. When ultrasonic treatment is directly performed on the molten metal obtained in step 1, the furnace 70 can be used as the melting furnace used in step 1. For example, an electric furnace equipped with a heater (not shown) or a high-frequency induction furnace equipped with a high-frequency coil (not shown) can be used as the furnace 70. For example, an alumina crucible can be used as the crucible 71. A horn 74 equipped on an ultrasonic vibrator 73 incorporating a vibrator can be immersed in the molten metal 72 and pulled out of the molten metal 72 by operating from outside the furnace. For example, a thermocouple sensor 75 is installed in the crucible 71 to monitor the temperature of the molten metal 72. The gas phase space in contact with the molten metal may be an air atmosphere or an inert gas atmosphere such as nitrogen gas.

[0038] (Step 4) The horn 74 of the ultrasonic vibrator 73 is immersed in the molten metal 72 in the crucible 71 obtained in step 3. Then, after adjusting the temperature of the molten metal to a range of 680°C to 720°C, a process is performed in which ultrasonic vibration is applied to the molten metal 72 from the horn 74 while maintaining the temperature in that range. The vibration amplitude of the ultrasonic vibration applied to the molten metal 72 is, for example, effectively set to 10 to 80 μm (pp), and more preferably set to 40 to 70 μm (pp). The vibration amplitude described in this application is a value measured in a peak-to-peak (pp) mode. Since a particle dispersion effect is expected by forming a cavitation field in the molten metal, the lower limit of the vibration amplitude is preferably set to 10 μm (pp), which is close to the threshold amplitude at which fully developed cavitation begins, in the case of an aluminum alloy molten metal. In addition, it is necessary to avoid as much as possible the phenomenon (acoustic (or cavitation) shielding) in which a large number of cavitation bubbles are generated just below the end face of the horn, greatly reducing the energy transmitted from the horn to the molten Al, and considering that an excessive vibration amplitude increases the internal stress in the horn and increases the risk of the horn breaking, it is desirable to set the vibration amplitude to 80 μm (pp) or less. It is desirable to set the immersion position of the horn 74 so that the effect of the ultrasonic vibration is applied to the entire molten metal 72 to be treated. In order to apply the above vibration amplitude to the entire molten metal 72 to be treated, this can be achieved by adjusting the ultrasonic vibration output by the ultrasonic vibrator 73 in the range of, for example, 0.05 to 0.5 kW per kg of molten metal. The application time of the ultrasonic vibration can be set in the range of, for example, 0.5 to 15 minutes, and it is more effective to set it in the range of 1 to 10 minutes. Although the term "ultrasonic wave" is often used to mean a sound wave of 20 kHz or more, in this specification, the vibration of a frequency of 15 kHz or more generated by the vibrator is called ultrasonic vibration. According to past experiments, for example, ultrasonic vibrations of 15 kHz or more can produce a cavitation effect in the molten aluminum alloy. Although there is no particular upper limit, it is preferable to set it to, for example, 30 kHz or less in consideration of the occurrence of cavitation in the molten aluminum alloy.

[0039] (Step 5) After the process of applying ultrasonic vibrations is completed, the horn 74 is lifted from the molten metal 72. Thereafter, the molten metal 72 is poured into a mold or the like installed in the furnace 70 by, for example, tilting the crucible 71 and solidified therein, or the temperature of the molten metal 72 is lowered to solidify the molten metal 72 in the crucible 72, thereby obtaining a solidified product.

[0040] The effect of ultrasonic vibration on molten aluminum has not been fully elucidated at present, but the following is thought to be the case. It is thought that ultrasonic vibration prevents the aggregation of TiB2 particles, and small TiB2 particles are dispersed in the molten aluminum. This is thought to lead to a homogenization of the structure of the solidified product when the molten aluminum is solidified.

[0041] The solid aluminum alloy material is then cut into small pieces of a predetermined size suitable for remelting in the molten metal joining process, thereby obtaining an aluminum alloy solid material to be used as an aluminum raw material in the molten metal joining process.

[0042] The Al-Cu-(Mg)-Ti-B aluminum alloy solid material obtained in the above manner, when remelted by the molten metal joining method and then resolidified in contact with the surface of a ceramic plate, has the same high strength (hardness) as an aluminum alloy part obtained when an aluminum alloy of the same composition that has not been ultrasonically treated is used, but has an inherent property that significantly improves the crack generation resistance of a ceramic plate (including ceramic plates that are sometimes used as reinforcing members) when subjected to a heat cycle. The mechanism behind this is currently unclear. EXAMPLES

[0043] [Example 1] (Preparation of aluminum alloy solid materials) By carrying out the above-mentioned steps 1 to 5, an aluminum alloy solid material for application to the molten metal joining method was obtained as follows.

[0044] Step 1; An ingot of pure Al with a purity of 99.9% or more, an Al-Cu mother alloy as a Cu raw material, and metallic magnesium as an Mg raw material were placed in a crucible in an electric furnace, and the electric furnace was started to heat, and the above materials were melted to obtain a molten metal. The temperature of the molten metal was monitored by a thermocouple sensor installed in the crucible. The temperature of the molten metal was further increased and maintained at 800°C. An Al-5% by mass Ti-1% by mass B alloy was added to the molten Al-Cu-Mg alloy as a Ti raw material and a B raw material, and the Al-5% by mass Ti-1% by mass B alloy was completely melted by holding at 800°C for 60 minutes, and about 5.5 kg of a molten Al-Cu-Mg-Ti-B alloy was obtained. The raw materials were mixed so that the molten metal had a composition, in mass%, of Cu: 0.20%, Mg: 0.10%, Ti: 0.04%, B: 0.008%, and the balance of Al. The gas phase space in contact with the molten metal was air. Step 2; The resulting molten metal was poured into a mold to obtain a master alloy.

[0045] Step 3; This master alloy was placed in the crucible of an electric furnace having the configuration shown in FIG. 7 and remelted, with the molten metal temperature maintained in the range of 700 to 720°C. Step 4; In this state, the horn of the ultrasonic vibrator was immersed in the molten metal and ultrasonic vibration was applied to the molten metal. Here, ultrasonic vibration with a frequency of 20 kHz and a vibration amplitude of 40 μm was applied to the molten metal for 5 minutes. The ultrasonic vibration output was approximately 0.13 to 0.2 kW per kg of molten metal. The gas phase space in contact with the molten metal was air. Step 5; After applying ultrasonic vibration, the horn was lifted from the molten metal, and the molten metal in the crucible was poured into a mold at a molten metal temperature of 690° C. or less, and the molten metal was solidified.

[0046] The solidified material was removed from the mold, cut and divided into small pieces to obtain aluminum alloy solid materials for use in the molten metal joining method. The gas phase space in contact with the molten metal was air.

[0047] (Preparation of aluminum-ceramic bonded substrate) The above-mentioned aluminum alloy solid material produced by the method of applying ultrasonic vibration (having a composition, by mass%, of Cu: 0.20%, Mg: 0.10%, Ti: 0.04%, B: 0.008%, and the remainder Al) was used as the raw material for obtaining a molten aluminum alloy, and an aluminum-ceramic bonding substrate (base-integrated aluminum-ceramic bonding substrate) having the cross-sectional structure shown in Figure 1 was produced by a molten metal bonding method as follows.

[0048] A plate material made of AlN measuring 120 mm x 92 mm x 1 mm was prepared as the ceramic substrate (reference number 10 in FIG. 1). A plate material made of AlN measuring 126 mm x 94 mm x 1 mm was prepared as the reinforcing member (reference number 110 in FIG. 1). These were placed inside a mold made of a gas-permeable carbon material with a cross-sectional structure shown in FIG. 3. In the mold space (space A in FIG. 3) that becomes the circuit member (reference number 20 in FIG. 1), the distance between the mold wall and the ceramic substrate is 0.4 mm, and in the mold space (space B in FIG. 3) that becomes the heat dissipation member (reference number 50 in FIG. 1), the distance between the ceramic plate (reference number 10 in FIG. 3) and the reinforcing member (reference number 110 in FIG. 3) is 2.6 mm, and the distance between the reinforcing member (reference number 110 in FIG. 3) and the mold wall is 0.4 mm. The ceramic plate and the reinforcing member are both restrained in position by a supporting member or a clamping member inside the mold so that they do not shift from their predetermined positions when the molten metal is poured into them.

[0049] The aluminum alloy solid material prepared by the above method was placed in the molten metal reservoir of this mold (reference number 5 in FIG. 3) as the Al raw material, and then the mold was placed in a furnace and heated in a nitrogen atmosphere. The heating temperature was monitored by a thermocouple attached to the mold. After the Al raw material was melted, a pressure of 16 kPa was applied from the pressurizing port of the mold (reference number 2 in FIG. 5) at a temperature of 720°C by nitrogen gas, and the molten aluminum alloy was poured into the space inside the mold through a narrow cross-sectional passage (reference number 103 in FIG. 5) (a runner with a narrow cross-sectional passage not shown in space A). When about 4 minutes had elapsed from the start of pouring, directional solidification was started by contacting the outer wall of the mold end (the part corresponding to the left end in FIG. 5) with a water-cooled copper block as a cooling device. The solidification was allowed to proceed while continuing the pressurization by nitrogen gas and the supply of molten metal from the molten metal reservoir. After the temperature of the mold became about 50°C or lower, the inside of the furnace was opened to the atmosphere, and the cast product (laminated structure) was taken out of the mold. In this way, an aluminum / ceramic bonding substrate was obtained, the cross section of which had the structure shown in Figure 1. The dimensions of each component of this aluminum / ceramic bonding substrate (the dimensions of the product portion after removing unnecessary portions such as the runner portion by cutting when removed from the mold) were 114 mm x 86 mm x 0.4 mm for the circuit component (20 in Figure 1), 120 mm x 92 mm x 1.0 mm for the ceramic plate (10 in Figure 1), 140 mm x 100 mm x 4.0 mm for the heat dissipation component (50 in Figure 1), and 126 mm x 94 mm x 1.0 mm for the reinforcing member (110 in Figure 1) built into the heat dissipation component. Three base-integrated aluminum / ceramic bonded substrates having the same dimensions and shapes were produced by this method, with the test number being 3. The resulting aluminum / ceramic bonded substrates were used as test specimens for the following investigation.

[0050] (Hardness measurement of aluminum alloys) Here, the Vickers hardness was measured at four locations on the exposed aluminum alloy near the four corners of the bonding surface of the ceramic plate (reference number 10 in FIG. 1) of the base member (reference number 50 in FIG. 1) so that the formation of indentations for hardness measurement would not affect the results of the heat cycle test described below. As a result, the average Vickers hardness value of 12 locations (4 locations x 3 bodies) was 19.7 HV. If an aluminum-ceramic bonded substrate with the same structure and dimensions was produced using a conventionally known molten metal bonding method using an Al-Ti-B based alloy molten metal without added Cu and Mg, the Vickers hardness at the above measurement locations would be approximately 16 HV, so it can be evaluated that the strength of the aluminum alloy was improved by adding Cu and Mg.

[0051] (Measurement of electrical conductivity of aluminum alloys) As in the hardness measurement described above, the electrical conductivity (%IACS) was measured by the eddy current method using a conductivity meter (FOERSTER, SIGMATEST2.069) for four aluminum alloy exposed parts near the four corners of the joining surface of the ceramic plate (reference number 10 in Fig. 1) of the base member (reference number 50 in Fig. 1). As a result, the average electrical conductivity of 4 locations x 3 bodies = a total of 12 locations was 59.52%IACS.

[0052] (Heat cycle test) The test specimen, an aluminum-ceramic bonded substrate with integrated base, was placed in a heat cycle tester (a thermal shock tester TSA-103ES-W manufactured by Espec Corporation) and subjected to a heat cycle consisting of 30 minutes at -40°C, 10 minutes at 25°C, 30 minutes at 150°C, and 10 minutes at 25°C in an air atmosphere. Every 100 cycles, the test specimen was inspected using an ultrasonic tester (SAT) (FineSAT V manufactured by Hitachi Power Solutions Co., Ltd.) to observe the ceramic / aluminum alloy interface and the inside of the ceramics for the ceramic plate (reference number 10 in Fig. 1, hereafter referred to as the "insulating member") between the circuit member and the base member, and the ceramic plate (reference number 110 in Fig. 1) of the reinforcing member embedded in the base member, to check for the presence or absence of cracks. As a result, cracks were found in the ceramic plate of the reinforcing member in one of the test specimens (n=3) after 600 cycles. In addition, the hardness and electrical conductivity of the aluminum alloy were measured every 100 cycles by the above-mentioned method. These results are shown in Table 1 together with those of Comparative Example 1 below. The average hardness and average electrical conductivity shown in Table 1 are the average values ​​of measurements taken at 12 locations (4 locations x 3 specimens).

[0053] [Comparative Example 1] Three base-integrated aluminum-ceramic bonding substrates having the same structure and dimensions as those in Example 1 were fabricated (number of tests: n=3) by a conventional method of applying a non-ultrasonic-treated Al-Cu-Mg-Ti-B based alloy mother alloy to the molten metal bonding method. Specifically, the mother alloy obtained in steps 1 and 2 in Example 1 was used as a raw material for forming the molten aluminum alloy in the molten metal bonding method. Therefore, the composition of the aluminum alloy is the same as that in Example 1.

[0054] In the obtained base-integrated aluminum / ceramic bonding substrate, the hardness of the aluminum alloy was 20.1 HV as an average value of the 12 locations, and the electrical conductivity of the aluminum alloy was 60.06% IACS as an average value of the 12 locations. As a result of the heat cycle test, cracks were found in the ceramic plate of the reinforcing member in two of the specimens (n=3) after 100 cycles. These results are shown in Table 1.

[0055] [Table 1]

[0056] As can be seen from Table 1, in an integrated base aluminum-ceramic bonded substrate in which an aluminum alloy containing Cu is used as the circuit member and base member, the crack resistance of the ceramic plate against heat cycles was significantly improved by using a solidified product of ultrasonically treated molten metal as the raw material for forming the molten metal in the molten metal bonding process. No significant differences were found in the hardness (strength) and electrical conductivity of the aluminum alloy that could be related to the large difference in crack resistance described above between with and without ultrasonic treatment. The mechanism by which ultrasonic treatment improves crack resistance has not yet been elucidated. [Explanation of symbols]

[0057] 1. Mold 1a Upper mold 1b Lower mold 2 Pressure port 3 Yudo 4 Pin-shaped recess 5 Hot water storage section 10 Ceramic plate 20 Circuit Materials 21 Groove 22 Semiconductor element mounting surface 50 Base material 51 Peripheral wall section 52 Groove 53 Pin-like protrusion 70 Furnace 71 Crucible 72 Molten Metal 73 Ultrasonic transducer 74 Horn 75 Thermocouple Sensor 100 Molten metal 103 Narrow cross-section flow channel 110 Reinforcement member

Claims

1. A method for producing an aluminum-ceramic bonded substrate, comprising melting an aluminum alloy solid material consisting of a solidified product as defined in (A) below to produce a molten aluminum alloy, and solidifying the molten aluminum alloy in contact with a surface of a ceramic plate placed in a mold, thereby bonding an aluminum alloy member to one or both sides of the ceramic plate. (A) A molten metal having a composition, in mass%, of Cu: 0.10 to 1.20%, Mg: 0 to 0.40%, Ti: 0.01 to 0.20%, B: 0.001 to 0.10%, the sum of elements other than Cu, Mg, Ti, B, and Al: 0 to 0.50%, and the balance being Al is formed, and when the temperature of the molten metal is in the range of 680 to 720°C, ultrasonic vibrations are applied to the molten metal, and then the molten metal that has been subjected to the above-mentioned treatment is solidified to obtain a solidified material.

2. 2. The method for producing an aluminum / ceramic bonding substrate according to claim 1, wherein the treatment of applying ultrasonic vibration is a treatment of applying ultrasonic vibration having a vibration amplitude of 10 to 80 μm (pp).

3. 3. The method for producing an aluminum-ceramic bonding substrate according to claim 1 or 2, wherein the aluminum-ceramic bonding substrate has a structure in which aluminum alloy members are bonded to both sides of a ceramic plate, one of the two aluminum alloy members being a circuit member for mounting a semiconductor element, and the other being a base member having a larger volume than the ceramic plate.

4. 4. The method for producing an aluminum / ceramic bonding substrate according to claim 3, wherein said base member is provided with a reinforcing member on a portion other than the bonding surface with said ceramic plate.

5. 5. The method for producing an aluminum / ceramic bonding substrate according to claim 4, wherein the reinforcing member is made of a ceramic plate.

Citation Information

Patent Citations

  • Semiconductor-mounting radiation base plate and production method therefor

    CN109417059A

  • Combined member of aluminum-ceramics

    JP2008172197A

  • Ultrasonic horn and method for manufacturing aluminum alloy using the same

    JP2011177787A

  • Substrate for mounting electronic element

    JP2013093369A

  • Semiconductor mounting heat dissipation base board, and manufacturing method and manufacturing apparatus thereof

    JP2018163995A