Method for producing molding material and molding material
Microwave-assisted acylation of cellulose with specific ions and solvent conditions enhances the durability and moldability of cellulose derivatives, addressing shear-induced decomposition issues and producing high-strength molded products.
Patent Information
- Application Number
- JP2023047142
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Molded bodies made from cellulose derivatives suffer from low durability due to shear force-induced decomposition during kneading and molding, leading to reduced mechanical strength.
A method involving microwave irradiation of a mixture containing cellulose, an acylating agent, and a solvent to perform an acylation reaction, resulting in a cellulose derivative with specific molecular weight distribution and conductivity, incorporating ions like imidazolium, pyridinium, or chloride ions, to enhance tensile strength and moldability.
The method produces a molding material with improved tensile strength and moldability, preventing charge buildup and ensuring high-quality molded articles.
Smart Images

Figure 2024136147000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a molding material and a molding material. [Background technology]
[0002] As a measure to combat the depletion of petroleum and global warming, attempts are being considered to replace conventional plastic materials with molding materials that use cellulose, a plant-derived, abundant natural material.
[0003] For example, a molding material containing cellulose fibers and resin is known. However, a molded article produced using such a molding material has a problem of low durability.
[0004] In response to this, cellulose derivatives have been proposed in which the hydrogen atoms of the hydroxyl groups of cellulose are substituted in a specified ratio with short-chain organic groups having 2 carbon atoms, medium-chain organic groups having 3 to 5 carbon atoms, and long-chain organic groups having 6 to 30 carbon atoms, for the purpose of application to molded articles with improved thermoplasticity, water resistance, impact strength, etc. (see Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2017 / 061190 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when producing a molded body using the cellulose derivative described in Patent Document 1, a problem arises in that part of the cellulose skeleton is decomposed by shear forces due to heat and mechanical stirring during kneading, molding, etc., resulting in the generation of low molecular weight components, which reduces the mechanical strength of the produced molded body. [Means for solving the problem]
[0007] The present invention has been made to solve the above-mentioned problems, and can be realized as the following application examples.
[0008] A method for producing a molding material according to an application example of the present invention includes an acylation step of irradiating a mixture containing cellulose, an acylating agent, and a solvent with microwaves having a frequency of 0.4 GHz or more and 6.0 GHz or less to carry out an acylation reaction of the cellulose, the solvent is an ionic liquid or a liquid containing a salt, The mixture contains the acylating agent in an amount of 0.2 equivalents or more based on the total hydroxyl groups of the cellulose.
[0009] The molding material according to the application example of the present invention comprises a cellulose derivative in which at least a part of the hydroxyl groups of cellulose is acylated; at least one ion selected from the group consisting of imidazolium ions, pyridinium ions, lithium ions, and chloride ions; The cellulose derivative has a content of low molecular weight components having a molecular weight of ¼ or less of a peak top molecular weight in a molecular weight distribution measured by gel permeation chromatography of 15% or less; The electrical conductivity at a temperature of 23°C and a relative humidity of 50% is 1.0 x 10 -6 S / cm or more. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a table summarizing the manufacturing conditions for the molding materials not containing a thermoplastic resin for each of the Examples and Comparative Examples, as well as the measurement and evaluation results for the molding materials not containing a thermoplastic resin and the molding materials containing a thermoplastic resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Preferred embodiments of the present invention will now be described in detail. [1] Molding material First, the molding material of the present invention will be described.
[0012] The molding material of the present invention contains a cellulose derivative in which at least a portion of the hydroxyl groups of cellulose has been acylated, and at least one ion selected from the group consisting of imidazolium ions, pyridinium ions, lithium ions, and chloride ions. The cellulose derivative contained in the molding material has a content of low molecular weight components having a molecular weight of 1 / 4 or less of the peak top molecular weight in a molecular weight distribution measured by gel permeation chromatography of 15% or less. The electrical conductivity of the molding material at a temperature of 23°C and a relative humidity of 50% is 1.0 x 10 -6 S / cm or more.
[0013] This makes it possible to provide a molding material that can be suitably used to produce a molded body having excellent tensile strength. It is also possible to provide a molding material that has excellent moldability when producing a molded body. It is also possible to suitably prevent charging of a molded body produced using the molding material.
[0014] On the other hand, if the above conditions are not met, satisfactory results will not be obtained. For example, even if the molding material contains a cellulose derivative in which at least some of the hydroxyl groups of the cellulose are acylated, if the molding material does not contain the above-mentioned specified ions, the tensile strength of the molded body produced using the molding material and the moldability when producing the molded body cannot be sufficiently excellent.
[0015] Moreover, if the content of the low molecular weight component in the cellulose derivative is too high, the tensile strength of a molded article produced using the molding material cannot be made sufficiently excellent.
[0016] If the electrical conductivity at a temperature of 23° C. and a relative humidity of 50% is too low, a molded article produced using the molding material will easily become charged with electricity.
[0017] The molding material of the present invention can be suitably produced by the method described below. [1-1] Cellulose derivatives The molding material of the present invention contains a cellulose derivative in which at least a portion of the hydroxyl groups of cellulose are acylated.
[0018] That is, the cellulose derivative contained in the molding material of the present invention has a chemical structure in which at least a portion of the -OH of cellulose is converted to an -OCOR structure when R is a hydrocarbon group.
[0019] By containing such a cellulose derivative together with specific ions as described in detail below, it is possible to improve the moldability when producing a molded body and the tensile strength of a molded body produced using the molding material.
[0020] The cellulose derivative may contain one type of acyl group in the molecule, or may contain multiple types of acyl groups.
[0021] The above R may be any hydrocarbon group, and may be an aromatic hydrocarbon group, but is preferably an aliphatic hydrocarbon group.
[0022] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0023] Furthermore, the R may be, for example, a straight-chain hydrocarbon group or a branched-chain hydrocarbon group.
[0024] The number of carbon atoms in R is preferably 1 or more and 18 or less, more preferably 2 or more and 6 or less, and even more preferably 2 or more and 4 or less.
[0025] This makes it possible to improve the moldability when producing a molded body and the tensile strength of a molded body produced using the molding material. In particular, even when the molding material contains cellulose, the affinity between cellulose and the cellulose derivative can be improved, and the moldability when producing a molded body and the tensile strength of a molded body produced using the molding material can be improved.
[0026] When the cellulose derivative contains multiple types of acyl groups in the molecule, it is preferable that the weighted average value of the carbon chain lengths of the R constituting these multiple types of acyl groups satisfies the above condition.
[0027] Furthermore, the R may be any hydrocarbon group, but is preferably an alkyl group. This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0028] The DS value of the cellulose derivative, i.e., the degree of substitution, which is the proportion of hydroxyl groups esterified with acyl groups among all hydroxyl groups in cellulose, is preferably 0.2 or more and 3.0 or less, more preferably 1.0 or more and 2.8 or less, and even more preferably 2.0 or more and 2.6 or less.
[0029] This makes it possible to improve the moldability when producing a molded body and the tensile strength of a molded body produced using the molding material. In particular, even when the molding material contains cellulose, the affinity between cellulose and the cellulose derivative can be improved, and the moldability when producing a molded body and the tensile strength of a molded body produced using the molding material can be improved.
[0030] The molding material of the present invention needs to contain at least one type of the cellulose derivative, and may contain a plurality of types of the cellulose derivatives.
[0031] The weight average molecular weight of the cellulose derivative determined by gel permeation chromatography is preferably from 10,000 to 500,000, more preferably from 100,000 to 450,000, and even more preferably from 200,000 to 400,000.
[0032] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0033] In the molecular weight distribution of the cellulose derivative measured by gel permeation chromatography, the content of low molecular weight components having a molecular weight of 1 / 4 or less of the peak top molecular weight is 15% or less, and the content of the low molecular weight components is preferably 12% or less, more preferably 10% or less, even more preferably 7% or less, and most preferably 5% or less. This makes the above-mentioned effects more pronounced.
[0034] The glass transition temperature of the cellulose derivative is preferably 80°C or higher and 200°C or lower, more preferably 90°C or higher and 180°C or lower, and even more preferably 100°C or higher and 170°C or lower.
[0035] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0036] The cellulose derivative can be suitably synthesized by acylation of cellulose with an acylating agent, which will be described in detail later.
[0037] The content of the cellulose derivative in the molding material of the present invention is preferably 10.0% by mass or more and 99.8% by mass or less, more preferably 20.0% by mass or more and 99.5% by mass or less, and even more preferably 40.0% by mass or more and 99.0% by mass or less.
[0038] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0039] [1-2] Specific ions The molding material of the present invention contains a specific ion, which is at least one type of ion selected from the group consisting of an imidazolium ion, a pyridinium ion, a lithium ion, and a chloride ion.
[0040] The specific ion contained in the molding material of the present invention is at least one ion selected from the group consisting of imidazolium ions, pyridinium ions, lithium ions and chloride ions, with imidazolium ions being preferred among them.
[0041] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0042] The specific ion may form a salt with, for example, a cellulose derivative in the molding material.
[0043] The content of the specific ion in the molding material of the present invention is preferably from 0.01% by mass to 5.0% by mass, more preferably from 0.05% by mass to 1.0% by mass, and even more preferably from 0.1% by mass to 0.5% by mass.
[0044] This makes it possible to improve the moldability when producing a molded article and the tensile strength of a molded article produced using the molding material.
[0045] [1-3]Thermoplastic resin The molding material of the present invention may further contain a thermoplastic resin in addition to the cellulose derivative and the specific ion.
[0046] This leads to better thermoplasticity of the molding material of the present invention, and better moldability when producing a molded article. In addition, the uniformity in the molding material and in a molded article produced using the molding material is improved, and the molded article exhibits better physical properties, such as tensile strength.
[0047] Examples of the thermoplastic resin include polyolefins such as polyethylene and polypropylene, and polyesters such as aliphatic polyesters and aromatic polyesters. One or more selected from these may be used in combination.
[0048] Aliphatic polyester is a polyester that does not have an aromatic chemical structure, and all of the constituent monomers do not have an aromatic chemical structure. Examples of aliphatic polyesters include those in which both the polyvalent carboxylic acid component and the polyhydric alcohol component as the constituent monomers have an aliphatic alkylene group. In addition, the aliphatic polyester may be one that is composed of a monomer that has a hydroxyl group and a carboxyl group in the molecule. Examples of aliphatic polyesters that are composed of a monomer that has a hydroxyl group and a carboxyl group in the molecule include polylactic acid.
[0049] When the aliphatic polyester has a chemical structure in which a polycarboxylic acid component having an aliphatic alkylene group and a polyhydric alcohol component having an aliphatic alkylene group are polymerized, the aliphatic polyester preferably has a chemical structure in which an alkylene dicarboxylic acid having an alkylene group with a carbon chain length of 2 or more and 6 or less and an alkylene diol having an alkylene group with a carbon chain length of 2 or more and 8 or less are condensed.
[0050] In particular, when the molding material of the present invention contains polylactic acid as a thermoplastic resin, it is advantageous in the following respects. That is, since polylactic acid can be produced from biological raw materials, consumption of underground resources can be suppressed even when it is kneaded with a thermoplastic resin. In addition, the effects of improving moldability and improving the physical properties of a molded body produced using the molding material as described above are also fully exhibited.
[0051] When the molding material of the present invention contains a thermoplastic resin, the content of the thermoplastic resin in the molding material of the present invention is preferably 10.0 mass% or more and 80.0 mass% or less, more preferably 15.0 mass% or more and 75.0 mass% or less, and even more preferably 20.0 mass% or more and 58.0 mass% or less. This makes the above-mentioned effects more pronounced.
[0052] When the molding material of the present invention contains polylactic acid, the proportion of polylactic acid in the total thermoplastic resin contained in the molding material of the present invention is preferably 50.0 mass% or more, more preferably 60.0 mass% or more, and even more preferably 70.0 mass% or more. This makes the above-mentioned effects more pronounced.
[0053] When the molding material of the present invention contains a thermoplastic resin, when the content of the cellulose derivative in the molding material of the present invention is XC [mass%] and the content of the thermoplastic resin is XR [mass%], it is preferable to satisfy the relationship of 0.12≦XR / XC≦4.1, it is more preferable to satisfy the relationship of 0.18≦XR / XC≦3.1, and it is even more preferable to satisfy the relationship of 0.26≦XR / XC≦1.3. This makes the above-mentioned effects more pronounced.
[0054] [1-4] Solvent The molding material of the present invention may contain a solvent. Such a solvent is capable of dissolving, for example, the cellulose derivative.
[0055] Examples of the solvent include 1-allyl-3-butylimidazolium bromide, 1-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide, N-methyl-N-propylpyrrolidinium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, dimethylpropylimidazolium iodide, butylmethylimidazolium iodide, and methylimidazolium iodide. 1,2-Dimethyl-3-n-propylimidazoinium salt, 1-Methyl-3-n-hexylimidazolinium iodide salt, 1,2-Dimethyl-3-ethylimidazolium trifluoromethanesulfonate, 1-Methyl-3-butylimidazolium nonafluorobutylsulfonate, 1-Methyl-3-ethylimidazolium bis(trifluoromethyl)sulfonylimide, 1-Methyl-3-n-hexylimidazolium bis(trifluoromethyl)sulfonylimide, 1-Methyl-3-n-hexyl Silimidazolium dicyanamide, lithium bisfluorosulfonylimide, lithium bistrifluorosulforomethanesulfonylimide, 1-methyl-3-propylimidazolium bis(trifluorosulfonyl)imide, 1-ethyl-3-butylimidazolium tetrafluoroborate, 1-hexyl-3-methylimidazolium hexafluorophosphate and other ionic liquids, water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol and other monohydric alcohols, ethylene glycol, propane glycol, butanediol and other dihydric alcohols, diethylene glycol, dipropylene glycol and other ether bond-containing dihydric alcohols, glycerin and other trihydric alcohols, dimethylformamide, dimethylacetamide, dimethylsulfoxide, acetonitrile, methylformamide, ethyl acetate, tetrahydrofuran and other aprotic polar solvents, and the like, among which one or more of them can be used in combination.
[0056] When the molding material of the present invention contains a solvent, the solvent may dissolve the specific ions in the molding material. In other words, a liquid containing specific ions may function as a solvent that dissolves the cellulose derivative.
[0057] When the molding material of the present invention contains a solvent, the content of the solvent in the molding material of the present invention is preferably 0.1% by mass or more and 80.0% by mass or less, more preferably 0.2% by mass or more and 70.0% by mass or less, and even more preferably 0.5% by mass or more and 65.0% by mass or less.
[0058] When the molding material of the present invention contains a solvent, the solvent may be removed, for example, during the production of the molded article.
[0059] [1-5] Other ingredients The molding material of the present invention may contain components other than the components described above. Hereinafter, in this section, such components are also referred to as "other components".
[0060] Examples of other components include flame retardants, colorants, insect repellents, anti-fungal agents, antioxidants, UV absorbers, aggregation inhibitors, release agents, cellulose, derivatives other than the above-mentioned cellulose derivatives, hemicellulose, lignin, acylating agents, organic acids, and ions other than the above-mentioned specific ions.
[0061] However, the content of other components in the molding material of the present invention is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, and even more preferably 5.0% by mass or less.
[0062] [1-6] Characteristics of molding materials As described above, the electrical conductivity of the molding material of the present invention at a temperature of 23° C. and a relative humidity of 50% is 1.0×10 -6 S / cm or more, but 1.0×10 -4 S / cm or more, and 1.0×10 -2It is more preferable that the viscosity is at least 1.0 S / cm, and even more preferable that the viscosity is at least 1.0 S / cm.
[0063] This makes it possible to more effectively prevent charging of a molded body produced using the molding material.
[0064] The electrical conductivity of the molding material of the present invention at a temperature of 23° C. and a relative humidity of 50% is 1.0×10 11 S / cm or less, and preferably 1.0×10 7 S / cm or less is more preferable, and 1.0×10 3 It is more preferable that the viscosity is less than or equal to S / cm. This makes it possible to improve moldability when producing a molded article.
[0065] [2] Manufacturing method of molding material Next, the method for producing the molding material of the present invention will be described.
[0066] The method for producing a molding material of the present invention includes an acylation step in which an acylation reaction of the cellulose is carried out while irradiating a mixture containing cellulose, an acylating agent, and a solvent with microwaves of 0.4 GHz or more and 6.0 GHz or less.
[0067] The solvent contained in the mixture is an ionic liquid or a liquid containing a salt, and the mixture contains the acylating agent in a ratio of 0.2 equivalents or more relative to the total hydroxyl groups of the cellulose.
[0068] This makes it possible to provide a method for producing a molding material that can be suitably used to produce a molded article having excellent tensile strength. It also makes it possible to provide excellent moldability when producing a molded article. It also makes it possible to suitably prevent the resulting molded article from being charged.
[0069] On the other hand, if the above conditions are not met, satisfactory results will not be obtained. For example, even if a process for reacting cellulose with an acylating agent is included, if this process is carried out without microwave irradiation, a problem occurs in which part of the cellulose is decomposed by shear forces due to heat and mechanical stirring, resulting in the generation of low molecular weight components and a decrease in the mechanical strength of the molded body.
[0070] Furthermore, even if microwaves are irradiated in the above process, if the frequency of the microwaves is below the lower limit, the proportion of low molecular weight components in the cellulose derivative will be too high, and the tensile strength of the molded body produced using the molding material will not be sufficiently excellent.
[0071] Furthermore, even if microwaves are irradiated in the above process, if the frequency of the microwaves exceeds the upper limit, the proportion of low molecular weight components in the cellulose derivative becomes too high, and the tensile strength of the molded body produced using the molding material cannot be made sufficiently excellent.
[0072] Furthermore, even if a process for reacting cellulose with an acylating agent is included, if an ionic liquid or a liquid containing a salt is not used as a solvent in the process, the proportion of low molecular weight components in the cellulose derivative becomes too high, and the tensile strength of the molded body produced using the molding material cannot be made sufficiently excellent.
[0073] Furthermore, if the amount of acylating agent used in the acylation step is less than the lower limit, the acylation reaction does not proceed properly, and the tensile strength of the molded body produced using the molding material cannot be made sufficiently excellent.
[0074] [2-1] Acylation process The method for producing a molding material of the present invention includes an acylation step in which an acylation reaction of the cellulose is carried out while irradiating a mixture containing cellulose, an acylating agent, and a solvent with microwaves of 0.4 GHz or more and 6.0 GHz or less.
[0075] [2-1-1] Cellulose Cellulose is a plant-derived, abundant natural material. Therefore, using cellulose as a raw material can suitably address environmental issues and save buried resources, and is also preferable from the viewpoints of stable supply of molding materials and molded articles produced using the same, cost reduction, etc. In addition, cellulose has particularly high theoretical rigidity, and the cellulose derivative obtained by derivatizing it through chemical modification also has excellent theoretical rigidity. Therefore, it is advantageous from the viewpoint of improving the rigidity of molded articles.
[0076] The cellulose used in the acylation step may be one that has been previously purified, or may contain impurities such as hemicellulose, lignin, etc. More specifically, the cellulose may be virgin pulp, or recycled waste paper, old cloth, etc.
[0077] The cellulose content in the mixture subjected to the acylation step is preferably 20.0% by mass or more and 95.0% by mass or less, more preferably 30.0% by mass or more and 90.0% by mass or less, and even more preferably 50.0% by mass or more and 87.0% by mass or less.
[0078] This allows cellulose as a raw material to be acylated at a higher reaction rate, and also allows the amounts of solvent and acylating agent used to be effectively reduced.
[0079] [2-1-2] Acylating agent The acylating agent has a function of reacting with cellulose to acylate at least a portion of the hydroxyl groups of the cellulose.
[0080] The number of carbon atoms in the acyl group of the acylating agent is not particularly limited, but is preferably 2 or more and 7 or less.
[0081] Examples of the acylating agent include carboxylic acid anhydrides, carboxylic acid halides, and carboxylic acids, and at least one selected from the group consisting of these can be used.
[0082] Examples of the carboxylic acid anhydride include acetic anhydride, propionic anhydride, butanoic anhydride, etc. Examples of the carboxylic acid halide include acyl fluorides such as acetyl fluoride, propionyl fluoride, butyryl fluoride, acyl chlorides such as acetyl chloride, propionyl chloride, butyryl chloride, acyl bromides such as acetyl bromide, propionyl bromide, butyryl bromide, acyl iodides such as acetyl iodide, propionyl iodide, butyryl iodide, etc. Examples of the carboxylic acid include acetic acid, propionic acid, butanoic acid, etc.
[0083] The acylating agent may be used in a ratio of 0.2 equivalents or more relative to the total hydroxyl groups of the cellulose contained in the mixture, but it is preferable that the acylating agent be used in a ratio of 0.5 equivalents or more, more preferably 1.0 equivalents or more, and even more preferably 3.0 equivalents or more.
[0084] This allows a sufficient proportion of the hydroxyl groups in the cellulose to be acylated, thereby improving the moldability when using the resulting molding material to produce a molded article, and the tensile strength of the molded article produced using the molding material.
[0085] The acylating agent is preferably used in a ratio of 8.0 equivalents or less, more preferably 7.5 equivalents or less, and even more preferably 7.0 equivalents or less, based on the total hydroxyl groups of the cellulose contained in the mixture. In other words, the mixture contains the acylating agent in a ratio of 8.0 equivalents or less, more preferably 7.5 equivalents or less, and even more preferably 7.0 equivalents or less, based on the total hydroxyl groups of the cellulose.
[0086] This effectively prevents the hydroxyl groups of cellulose from being excessively acylated, and the cellulose derivative contained in the molding material forms hydrogen bonds at an appropriate ratio, improving the moldability of the molding material. In addition, the amount of acylating agent used can be reduced, which is advantageous in terms of reducing the manufacturing cost of the molding material and saving resources.
[0087] [2-1-3] Solvent The solvent contained in the mixture has, for example, a function of dissolving at least a portion of the components contained in the mixture, such as the acylating agent, or a function of dissolving at least a portion of the cellulose derivative which is the reaction product.
[0088] The solvent constituting the mixture is an ionic liquid or a liquid containing a salt. Examples of the ionic liquid include 1-allyl-3-butylimidazolium bromide, 1-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide, N-methyl-N-propylpyrrolidinium bis(fluorosulfonyl)imide, 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide, dimethylpropylimidazolium iodide, butylmethylimidazolium iodide, 1,2-dimethyl-3-n-propylimidazoinium iodide salt, 1-methyl-3-n-hexylimidazolinium iodide salt, 1,2-dimethyl-3-ethylimidazolium trifluoromethanesulfonate, 1-methyl-3-butyl Examples of the imidazolium nonafluorobutyl sulfonate include 1-methyl-3-ethylimidazolium bis(trifluoromethyl)sulfonylimide, 1-methyl-3-n-hexylimidazolium bis(trifluoromethyl)sulfonylimide, 1-methyl-3-n-hexylimidazolium dicyanamide, lithium bisfluorosulfonylimide, lithium bistrifluorosulfomethanesulfonylimide, 1-methyl-3-propylimidazolium bis(trifluorosulfonyl)imide, 1-ethyl-3-butylimidazolium tetrafluoroborate, and 1-hexyl-3-methylimidazolium hexafluorophosphate. One or more selected from these may be used in combination.
[0089] When an ionic liquid is used, it is preferable to use an ionic liquid having an imidazolium salt structure.
[0090] This makes it possible to improve the solubility of cellulose and the cellulose derivative, allowing the acylation reaction to proceed more smoothly, and also allows the produced cellulose derivative to be contained in the reaction product with higher uniformity.
[0091] Examples of the cation constituting the salt include monovalent cations such as alkali metal ions such as lithium ion, sodium ion, and potassium ion; ammonium ion, imidazolium ion, and pyridinium ion; and divalent cations such as alkaline earth metal ions such as magnesium ion and calcium ion.
[0092] Examples of anions constituting the salt include halide ions such as fluoride ion, chloride ion, bromide ion, and iodide ion; monovalent anions such as nitrate ion; divalent anions such as sulfate ion; and trivalent anions such as phosphate ion. The salt solution is not particularly limited, but examples thereof include an aqueous solution.
[0093] When the solvent is a liquid containing a salt, examples of the component that dissolves the salt include monohydric alcohols such as water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol; dihydric alcohols such as ethylene glycol, propane glycol, and butanediol; dihydric alcohols containing an ether bond such as diethylene glycol and dipropylene glycol; trihydric alcohols such as glycerin; and aprotic polar solvents such as dimethylformamide, dimethylacetamide, dimethylsulfoxide, acetonitrile, methylformamide, ethyl acetate, and tetrahydrofuran. These can be used alone or in combination of two or more.
[0094] The content of the solvent in the mixture subjected to the acylation step is preferably 2.0% by mass or more and 75.0% by mass or less, more preferably 3.0% by mass or more and 60.0% by mass or less, and even more preferably 4.0% by mass or more and 30.0% by mass or less.
[0095] This makes it possible to more suitably proceed with the acylation reaction of cellulose without using an excess of solvent.
[0096] [2-1-4] Other ingredients The mixture to be subjected to the acylation step may contain components other than the above-mentioned components. Hereinafter, in this section, such components are also referred to as "other components".
[0097] Examples of other components include catalysts, hemicellulose, lignin, organic acids, and ions other than the specific ions.
[0098] However, the content of other components in the mixture subjected to the acylation step is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, and even more preferably 5.0% by mass or less.
[0099] [2-1-5] Reaction conditions In the acylation step, the mixture is irradiated with microwaves having a frequency of 0.4 GHz or more and 6.0 GHz or less to carry out an acylation reaction of the cellulose.
[0100] The frequency of the microwaves irradiated to the mixture in this step may be from 0.4 GHz to 6.0 GHz, preferably from 0.5 GHz to 5.8 GHz, more preferably from 0.6 GHz to 3.0 GHz, and even more preferably from 0.7 GHz to 2.0 GHz.
[0101] This allows the acylation reaction of cellulose to proceed more favorably, the proportion of low molecular weight components of the cellulose derivative contained in the molding material produced can be reduced, and the tensile strength of the molded article produced using the molding material can be improved. Also, the moldability when producing a molded article using the molding material can be improved.
[0102] The microwave irradiation time for the mixture in this step is preferably from 15 minutes to 600 minutes, more preferably from 30 minutes to 450 minutes, and even more preferably from 60 minutes to 300 minutes.
[0103] This makes it possible to reduce the proportion of low molecular weight components of the cellulose derivative contained in the molding material produced, and to improve the tensile strength of the molded article produced using the molding material. Also, the productivity of the molding material can be improved.
[0104] In this step, there may be a period during which the reaction is allowed to proceed without irradiating the mixture with microwaves.
[0105] When the time period is as above, the time period during which microwave irradiation is not performed in this step is preferably 60 minutes or less, more preferably 30 minutes or less, and even more preferably 15 minutes or less.
[0106] The temperature of the mixture in this step is preferably from 5°C to 70°C, more preferably from 10°C to 60°C, and even more preferably from 15°C to 50°C.
[0107] [2-2] Cellulose derivative separation process The method for producing a molding material of the present invention may include at least an acylation step, but may also include a cellulose derivative separation step of separating the cellulose derivative from the composition obtained in the acylation step.
[0108] This allows the cellulose derivative to be separated from excess solvent, unreacted acylating agent and cellulose, reaction products between the acylating agent and water, etc., and the purity and content of the cellulose derivative can be increased.
[0109] The cellulose derivative can be separated, for example, by precipitating the cellulose derivative from the composition obtained in the acylation step and filtering the cellulose derivative.
[0110] The cellulose derivative can be precipitated, for example, by concentrating the composition obtained in the acylation step, or by adding a poor solvent for the cellulose derivative to the composition obtained in the acylation step.
[0111] In addition, in the cellulose derivative separation process, it is not necessary to substantially completely remove components other than the cellulose derivative, and the cellulose derivative separated may contain other components such as the solvent in a predetermined proportion.
[0112] However, the cellulose derivative separated in this step preferably has a purity of 90% by mass or more, and more preferably 95% by mass or more.
[0113] [2-3] Mixing process The method for producing a molding material of the present invention may further include a kneading step of kneading the cellulose derivative with a thermoplastic resin.
[0114] This leads to better thermoplasticity of the molding material produced, and better moldability when producing a molded article. In addition, the uniformity in the molding material and in the molded article produced using the molding material is improved, and the molded article exhibits better physical properties, such as tensile strength.
[0115] Examples of the thermoplastic resin include polyolefins such as polyethylene and polypropylene, aliphatic polyesters such as polylactic acid, and polyesters such as aromatic polyesters. One or more selected from these can be used in combination.
[0116] In particular, if the thermoplastic resin contains polylactic acid, it is advantageous in the following respects. That is, since polylactic acid can be produced from biological raw materials, consumption of underground resources can be suppressed even when it is kneaded with a thermoplastic resin. In addition, the effects of improving moldability and improving the physical properties of molded bodies produced using the molding material as described above are also fully exhibited.
[0117] When the thermoplastic resin used in this process contains polylactic acid, the proportion of polylactic acid in the entire thermoplastic resin used in this process is preferably 50.0 mass% or more, more preferably 60.0 mass% or more, and even more preferably 70.0 mass% or more. This makes the above-mentioned effects more pronounced.
[0118] The amount of the thermoplastic resin used in this step is not particularly limited, but when the amount of the cellulose derivative used in this step is XC [parts by mass] and the amount of the thermoplastic resin used in this step is XR [parts by mass], it is preferable to satisfy the relationship of 0.12≦XR / XC≦4.1, it is more preferable to satisfy the relationship of 0.18≦XR / XC≦3.1, and it is even more preferable to satisfy the relationship of 0.26≦XR / XC≦1.3. This makes the above-mentioned effects more pronounced.
[0119] In this step, components other than the thermoplastic resin may be kneaded with the cellulose derivative together with the thermoplastic resin. Hereinafter, in this section, such components are also referred to as "other components".
[0120] Examples of other components include flame retardants, colorants, insect repellents, anti-fungal agents, antioxidants, UV absorbers, aggregation inhibitors, release agents, cellulose, derivatives other than the above-mentioned cellulose derivatives, and ions other than the above-mentioned specific ions.
[0121] However, the content of other components in the material subjected to this step is preferably 10.0% by mass or less, more preferably 7.0% by mass or less, and even more preferably 5.0% by mass or less.
[0122] The other components may be previously mixed with the thermoplastic resin before being subjected to the kneading step.
[0123] For the kneading in this step, for example, a single-screw kneader, a twin-screw kneader, a multi-screw kneader, a mixer, or a roll Banbury mixer can be used.
[0124] The strand-like molding material obtained by kneading may be pelletized, for example, using a pelletizer of the strand type or watering hot cut type to form a pellet-like molding material.
[0125] [2-4] Other processes The method for producing the molding material of the present invention may include steps other than those described above. Examples of such steps include a pretreatment step for removing impurities from the cellulose fibers, an intermediate treatment step such as a washing step for washing the cellulose derivative prior to kneading with a thermoplastic resin, and a post-treatment step for molding the kneaded product into a predetermined shape.
[0126] [3] Molded body Next, a molded article produced by using the molding material of the present invention will be described.
[0127] The molded article according to the present invention contains a cellulose derivative in which at least some of the hydroxyl groups of cellulose have been acylated, and at least one ion selected from the group consisting of imidazolium ions, pyridinium ions, lithium ions, and chloride ions. The cellulose derivative has a molecular weight distribution measured by gel permeation chromatography in which the content of low molecular weight components having a molecular weight of ¼ or less of the peak top molecular weight is 15% or less. The molded article according to the present invention has a conductivity of 1.0×10 at a site made of a material containing the cellulose derivative and the ions at a temperature of 23° C. and a relative humidity of 50%. -6 S / cm or more.
[0128] This makes it possible to provide a molded article having excellent tensile strength, and also makes it possible to suitably prevent the molded article from becoming statically charged.
[0129] The molded article according to the present invention as described above can be suitably produced by using the molding material according to the present invention described above.
[0130] Each component constituting the molded product preferably satisfies the conditions described above in [1-1] to [1-5], provided that the content of the solvent in the molded product is preferably 1.0 mass % or less.
[0131] The shape of the molded product is not particularly limited, and may be any shape, such as a sheet, a block, a sphere, or a three-dimensional shape.
[0132] The molded article may be used for any purpose, and examples thereof include various housings such as printer housings, ink cartridges, and various containers.
[0133] In particular, the molded article according to the present invention is effectively prevented from generating dust, and therefore can be suitably applied to ink cartridges and the like where dust generation is particularly problematic.
[0134] Furthermore, since the molded article according to the present invention is effectively prevented from being charged, it can be suitably applied to members that are prone to be charged due to friction, such as electrical appliances and precision instruments.
[0135] The molded article according to the present invention may be produced by any method, but can be suitably produced, for example, by injection molding, press molding, or the like using the molding material according to the present invention as described above.
[0136] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these. EXAMPLES
[0137] Next, specific examples of the present invention will be described. [4] Manufacturing of molding materials [4-1] Manufacturing of molding materials that do not contain thermoplastic resins Example 1 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 4 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.4 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0138] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0139] Example 2 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred for 2 hours at 35°C under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0140] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0141] Example 3 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 4 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 5.8 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0142] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0143] Example 4 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide (Kanto Chemical Co., Ltd.) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical Co., Ltd.), and 6 equivalents of propionic anhydride (Kanto Chemical Co., Ltd.) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 4 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves having a frequency of 0.915 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0144] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0145] Example 5 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of lithium chloride (Kanto Chemical) as a salt, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 4 hours in a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0146] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0147] Example 6 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 9 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred for 2 hours at 35°C under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0148] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0149] Example 7 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 8 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 2 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0150] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0151] Example 8 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 0.2 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred for 2 hours at 35°C under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0152] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0153] Comparative Example 1 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 6 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.3 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0154] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0155] Comparative Example 2 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred at 35°C for 6 hours under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 20 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0156] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0157] Comparative Example 3 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 10 parts by mass of dimethylacetamide (Kanto Chemical) and 6 equivalents of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups of the cellulose were added, and the mixture was stirred at 35°C for 6 hours in a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by a microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0158] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0159] Comparative Example 4 To 100 parts by mass of cellulose (Nippon Paper Industries, dissolving pulp, degree of polymerization 750, approximately 3 mm square sheet), 5 parts by mass of 1-allyl-3-butylimidazolium bromide (Kanto Chemical) as an ionic liquid, 10 parts by mass of dimethylacetamide (Kanto Chemical), and 0.1 equivalent of propionic anhydride (Kanto Chemical) as an acylating agent relative to the total hydroxyl groups possessed by the cellulose were added, and the mixture was stirred for 2 hours at 35°C under a nitrogen atmosphere to carry out an acylation reaction. At this time, microwaves with a frequency of 0.915 GHz generated by microwave oscillation means were irradiated to the reaction solution via a waveguide.
[0160] After the reaction was completed, the cellulose derivative was precipitated. The precipitated cellulose derivative was filtered off, washed with 500 parts by mass of water and filtered off three times, and then vacuum dried at 80° C. for 4 hours to obtain a molding material.
[0161] [4-2] Manufacturing of molding materials containing thermoplastic resins The molding materials of each of the above-mentioned Examples and Comparative Examples, i.e., each molding material not containing a thermoplastic resin, were mixed with the same mass of polylactic acid (Tomoe Engineering Co., Ltd., PLA (polylactic acid) L105) to obtain a mixture, and the mixture was kneaded and extruded using a twin-screw extruder (Technovel Co., Ltd., KZW15TW-45MG-NH) at a maximum heating temperature of 220°C, to obtain pellet-shaped molding materials, i.e., molding materials containing a thermoplastic resin.
[0162] [5] Measurement and evaluation [5-1] Electrical conductivity For each of the molding materials not containing a thermoplastic resin in each of the Examples and Comparative Examples, the volume conductivity was measured in an environment at a temperature of 23° C. and a relative humidity of 50%.
[0163] The volume conductivity was determined as follows: Each sample was left for 1 hour in a chamber in an environment of 23°C temperature and 50% relative humidity, and then a direct current of 100V was applied using brass electrodes and an ammeter in accordance with JIS K6723, the current value after charging for 1 minute was measured, and the volume conductivity was calculated using the following formula: The main electrode had a diameter of 50 mm and a height of 35 mm, the guard electrode had an outer diameter of 80 mm, an inner diameter of 70 mm, and a height of 10 mm, and the counter electrode was 300 x 150 x 2 mm.
[0164] ρ=(πd2 / 4t)Rv ρ: Volume resistivity (Ω cm) d: diameter of main electrode (cm) t: thickness of test piece (cm) Rv: Volume resistance (Ω)
[0165] [5-2]Molecular weight distribution For the cellulose derivatives contained in the molding materials not containing thermoplastic resin of each of the Examples and Comparative Examples, the weight average molecular weight and molecular weight distribution were measured by gel permeation chromatography in the following manner.
[0166] That is, the solution in which the molding material was dissolved in solution A, which was prepared by adding LiBr to N-methyl-2-pyrrolidone to make 0.1 mol / L, was measured at 55°C with a gel permeation chromatography (GPC) (main body: Shimadzu Corporation HPLC Prominence) connected to a column with RI (differential refractometer). The column consisted of a guard column (Agilent Technologies PolyPore GUARD size 50×7.5mm) and a main column (front column: Agilent Technologies PolyPore size 300×7.5mm, rear column: Agilent Technologies PolyPore size 300×7.5mm). The measurement conditions were mobile phase: solution A, column temperature: 55°C. The molecular weight and molecular weight distribution of the polymer were calculated using the relationship between the known molecular weight of Agilent Technologies polymethyl methacrylate (MM-10 set) and the GPC measurement value (retention time) of the cellulose derivative.
[0167] [5-3] Formability The molding materials not containing thermoplastic resin of each of the Examples and Comparative Examples were evaluated for moldability in an injection molding machine.
[0168] Good molding transportability means that the molding material can be supplied stably when it is fed into the molding machine and the load is not excessive. Good injectability means that the molding material can be molded into the desired shape without deterioration such as the generation of air bubbles or coloring. Molding materials that have good molding transportability and injectability are rated "A", molding materials that have issues with either one but can be molded are rated "B", molding materials that have issues with both but can be molded are rated "C", and molding materials that cannot be molded are rated "D".
[0169] [5-4] Tensile strength of molded body Using the molding materials not containing a thermoplastic resin of each of the Examples and Comparative Examples, molded articles were produced as follows, and the tensile strength was measured.
[0170] First, the molding material was kneaded at a maximum heating temperature of 220°C using a twin-screw extruder (KZW15TW-45MG-NH manufactured by Technobel Co., Ltd.) and extruded to form pellets. The pellet-shaped molding material was molded into the standard shape (test piece type 2) for evaluating the physical properties of plastics described in JIS K7127 using an injection molding machine (SE-EV-A manufactured by Sumitomo Heavy Industries, Ltd.) to obtain a tensile test piece. The tensile strength of the tensile test piece was determined using a tensile tester (Instron Tester Model 5567 manufactured by Instron Co., Ltd.) under the conditions of a ball line distance of 25 mm and a test speed of 50 mm / min, and was evaluated according to the following criteria. The higher the tensile strength, the better. The evaluation is as follows.
[0171] A: Tensile strength is 40 MPa or more. B: The tensile strength is 30 MPa or more and less than 40 MPa. C: Tensile strength is 20 MPa or more and less than 30 MPa. D: The tensile strength is less than 20 MPa.
[0172] In addition, tensile test pieces were produced in the same manner as above, except that instead of the pellet-shaped molding material not containing thermoplastic resin in each of the above-mentioned Examples and Comparative Examples, a pellet-shaped molding material containing thermoplastic resin, i.e., the molding material produced in [4-2] above, was used, and the tensile strength was measured and evaluated in the same manner and by the same criteria as above.
[0173] The measurement and evaluation results are shown together in FIG. 1, together with the manufacturing conditions of the molding materials not containing thermoplastic resin according to each of the examples and comparative examples.
[0174] In FIG. 1, the column for the amount of acylating agent used shows the amount of acylating agent used relative to the total hydroxyl groups in the cellulose used as the raw material, expressed as an equivalent amount.
[0175] As is clear from Fig. 1, excellent results were obtained in each of the Examples, whereas satisfactory results were not obtained in each of the Comparative Examples.
Claims
1. The method includes an acylation step of irradiating a mixture containing cellulose, an acylating agent, and a solvent with microwaves having a frequency of 0.4 GHz or more and 6.0 GHz or less to carry out an acylation reaction of the cellulose, the solvent is an ionic liquid or a liquid containing a salt, The mixture contains the acylating agent in an amount of 0.2 equivalents or more relative to the total hydroxyl groups of the cellulose.
2. The method for producing a molding material according to claim 1 , wherein the mixture contains the acylating agent in an amount of 8.0 equivalents or less based on the total hydroxyl groups of the cellulose.
3. 3. The method for producing a molding material according to claim 1, further comprising a kneading step of kneading the cellulose derivative obtained in the acylation step with a thermoplastic resin.
4. The method for producing a molding material according to claim 3 , wherein the thermoplastic resin comprises polylactic acid.
5. a cellulose derivative in which at least a portion of the hydroxyl groups of cellulose are acylated; at least one ion selected from the group consisting of imidazolium ions, pyridinium ions, lithium ions, and chloride ions; The cellulose derivative has a molecular weight distribution measured by gel permeation chromatography, in which a content of low molecular weight components having a molecular weight of ¼ or less of a peak top molecular weight is 15% or less; The electrical conductivity at a temperature of 23°C and a relative humidity of 50% is 1.0 x 10 -6 A molding material having a viscosity of 1.0 S / cm or more.
6. The electrical conductivity of the molding material at a temperature of 23° C. and a relative humidity of 50% is 1.0×10 7 The molding material according to claim 5, having a viscosity of 0.2 S / cm or less.
7. The molding material according to claim 5 or 6, further comprising a thermoplastic resin.
8. The molding material according to claim 7 , wherein the thermoplastic resin comprises polylactic acid.
Citation Information