Carbon material precursor, method for producing carbon material precursor, method for producing carbon material, composition for producing carbon material precursor, and method for producing composition for producing carbon material precursor

By integrating biomass fibers with acrylamide-based polymers and using water as a solvent, the method addresses sagging and fusion issues in carbon fiber production, ensuring high carbonization yield and improved strength and quality.

JP2024136272APending Publication Date: 2024-10-04KK TOYOTA CHUO KENKYUSHO
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023047345
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for producing carbon fiber using acrylamide-based polymers face issues such as sagging and fusion during stretching and flameproofing treatments due to softening at high temperatures, leading to reduced carbonization yield, strength, and appearance quality.

Method used

Incorporating biomass fibers with acrylamide-based polymers in the carbon material precursor, where the biomass fibers have a content of 0.1 to 40% by mass, and utilizing a solvent like water to maintain the polymer's solubility and stability, thereby suppressing softening and fusion.

Benefits of technology

The method effectively reduces sagging and fusion during processing, enhances heat resistance, maintains carbonization yield, and improves the strength and appearance quality of the carbon material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136272000003
    Figure 2024136272000003
  • Figure 2024136272000001
    Figure 2024136272000001
  • Figure 2024136272000002
    Figure 2024136272000002
Patent Text Reader

Abstract

To provide a carbon material precursor capable of decreasing occurrence of dripping and melting due to softening during drawing treatment or flame resistant treatment, a method for producing the carbon material precursor, a composition for producing the carbon material precursor used in production of the carbon material precursor, a method for producing the composition for producing the carbon material precursor, as well as a method for producing a carbon material using the carbon material precursor.SOLUTION: A carbon material precursor including a biomass fiber and an acrylamide-based polymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a carbon material precursor, a method for producing a carbon material precursor, a method for producing a carbon material, a composition for producing a carbon material precursor, and a method for producing a composition for producing a carbon material precursor. [Background technology]

[0002] Carbon materials are lightweight and have excellent mechanical properties, so carbon composite materials using carbon materials are attracting attention as materials to replace metal materials. As a method for producing carbon fiber, which is one of the carbon materials, a method is known in which a fiber bundle obtained by spinning polyacrylonitrile is subjected to a flame retardant treatment and then a carbonization treatment is performed (for example, Patent Document 1 and Patent Document 2). Polyacrylonitrile is difficult to dissolve in inexpensive, general-purpose solvents, so it is necessary to use expensive organic solvents such as dimethyl sulfoxide and N,N-dimethylacetamide when carrying out polymerization, spinning, etc., which results in high production costs for carbon fibers.

[0003] On the other hand, acrylamide-based polymers containing acrylamide-based monomers are water-soluble polymers and can be produced at low cost because water can be used as a solvent. They also have a small environmental impact, and are expected to reduce the production costs of carbon materials (e.g., Patent Documents 3 and 4).

[0004] However, in general, the stretching and flame-retarding treatment of the carbon material precursor is performed at a temperature of 160°C or higher, and an acrylamide-based polymer with a glass transition temperature of about 160°C rapidly softens during the stretching and flame-retarding treatment at a temperature of 160°C or higher. Therefore, when the carbon material precursor made of an acrylamide-based polymer is stretched and flame-retarded in the horizontal direction, the polymer is softened by heating, and fusion and sagging are likely to occur. If sagging occurs, the carbon material may come into contact with equipment or have a defective shape, and may not be able to apply sufficient tension during the stretching and flame-retarding treatment. If fusion occurs, the carbonization yield may decrease, the strength of the carbon material may decrease, and the appearance quality may decrease.

[0005] In Patent Document 5, therefore, the acrylamide polymer is crosslinked to suppress softening of the carbon material precursor and make it less likely to sag. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-183159 A [Patent Document 2] JP 2008-202208 A [Patent Document 3] JP 2019-26827 A [Patent Document 4] JP 2019-167516 A [Patent Document 5] JP 2019-172800 A Summary of the Invention [Problem to be solved by the invention]

[0007] It has become clear that although the technology described in Patent Document 5 can suppress the occurrence of sagging of the carbon material precursor during stretching treatment or flame-resistant treatment, the stretchability tends to decrease due to crosslinking, and that fusion is likely to occur due to melting occurring before the crosslinking reaction is completed or the crosslinking reaction occurring at the contact points between the carbon material precursors. If the materials are fused together, the flame retardant treatment and the subsequent carbonization treatment may not proceed sufficiently, which may result in a decrease in the carbonization yield, a decrease in the strength of the carbon material, and a decrease in the appearance quality.

[0008] In view of the above circumstances, an object of one embodiment of the present disclosure is to provide a carbon material precursor capable of reducing the occurrence of sagging and fusion due to softening during stretching and flame-resistant treatment, and a method for producing the same. Furthermore, an object of the present disclosure is to provide a composition for producing a carbon material precursor used in the production of the carbon material precursor of the present disclosure, a method for producing the composition for producing a carbon material precursor, and a method for producing a carbon material using the carbon material precursor of the present disclosure. [Means for solving the problem]

[0009] The specific means for achieving the objectives are as follows: <1> A carbon material precursor comprising a biomass fiber and an acrylamide-based polymer. <2> The content of the biomass fiber is 0.1 to 40% by mass relative to the content of the acrylamide-based polymer. <1> The carbon material precursor according to claim 1, <3> The biomass fiber is a fiber derived from at least one selected from the group consisting of cellulose and nitrogen-containing polysaccharide polymers. <1> or <2> The carbon material precursor according to claim 1, <4> The fiber diameter of the biomass fiber is within the range of 1 nm to 100 μm. <1> ~ <3> 13. The carbon material precursor according to claim 12. <5> <1> ~ <4> 1. A method for producing a carbon material precursor according to claim 1, comprising the steps of: and carbonizing the flame-resistant material. <6> A composition for producing a carbon material precursor, comprising biomass fibers, an acrylamide-based polymer, and a solvent. <7> The solvent comprises water. <6> The composition for producing a carbon material precursor according to claim 1. <8> A method for producing a composition for producing a carbon material precursor, comprising mixing biomass fiber, an acrylamide-based polymer, and a solvent. <9> The solvent comprises water. <8> A method for producing the composition for producing a carbon material precursor according to claim 1. <10> Using the liquid dispersion of the biomass fiber, <8> or <9> A method for producing the composition for producing a carbon material precursor according to claim 1. <11> A method for producing a carbon material precursor, comprising drying a composition for producing a carbon material precursor, the composition comprising biomass fibers, an acrylamide-based polymer, and a solvent. <12> The solvent comprises water. <11> A method for producing the carbon material precursor according to claim 1. <13> Using the liquid dispersion of the biomass fiber, <11> or <12> A method for producing the carbon material precursor according to claim 1. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a carbon material precursor capable of reducing the occurrence of sagging and fusion due to softening during stretching treatment and flame-resistant treatment, a method for producing a carbon material precursor, a composition for producing a carbon material precursor used in the production of a carbon material precursor, a method for producing a composition for producing a carbon material precursor, and a method for producing a carbon material using the carbon material precursor. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a diagram illustrating a method for evaluating the sagging state in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] In the present disclosure, a numerical range indicated using "~" includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with the value shown in the synthesis examples. In the present disclosure, the term "step" includes not only a step that is independent of other steps, but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.

[0013] In the present disclosure, each component may contain multiple types of the corresponding substance. When multiple types of substances corresponding to each component are present in the carbon material precursor, the content or amount of each component means the total content or amount of the multiple types of substances present in the carbon material precursor, unless otherwise specified.

[0014] In the present disclosure, the term "carbon material precursor" refers to a material that can be subjected to a carbonization treatment to obtain a carbon material. In the present disclosure, a "composition for producing a carbon material precursor" is a composition used in producing a carbon material precursor. In the present disclosure, the term "carbon material" refers to a material obtained by carbonization, regardless of its shape. For example, the carbon material may be in the form of fibers, plates, films, powders, particles, etc.

[0015] In the present disclosure, the term "acrylamide-based polymer" refers to a homopolymer of an acrylamide-based monomer or a copolymer of an acrylamide-based monomer and a monomer other than an acrylamide-based monomer (hereinafter referred to as other polymerizable monomer). In this disclosure, "biomass fiber" refers to fiber derived from biological sources.

[0016] <Carbon material precursor> The carbon material precursor of the present disclosure includes a biomass fiber and an acrylamide-based polymer, and is capable of reducing the occurrence of sagging and fusion due to softening during stretching or flame-resistant treatment.

[0017] The reason why the above effect is achieved is presumed to be as follows, but is not limited to this. Acrylamide-based polymers soften rapidly above their glass transition temperature (Tg) of approximately 160°C, but it is believed that the use of biomass fiber, which has excellent heat resistance and reinforcing properties, in combination with the polymers suppresses softening at temperatures above 160°C and thus prevents sagging. In particular, because biomass fiber has hydroxyl groups on its surface, these hydroxyl groups form hydrogen bonds with the acrylamide-based polymer, distributing the acrylamide-based polymer uniformly on the biomass fiber and maintaining this state, which is believed to effectively suppress softening and sagging at temperatures above 160°C.

[0018] In addition, since biomass fibers have hydroxyl groups on the surface, they are hydrophilic and easily dispersible in water, so water can be used as a solvent in the composition for producing a carbon material precursor. Therefore, the carbon material precursor of the present disclosure can be produced at low cost and has a small environmental impact, which are advantages in terms of production. Other advantages in terms of production will be described later.

[0019] (Acrylamide polymer) The carbon material precursor of the present disclosure includes an acrylamide-based polymer. The acrylamide-based polymer may be a homopolymer of an acrylamide-based monomer, or a copolymer of an acrylamide-based monomer and a monomer other than an acrylamide-based monomer (hereinafter referred to as another polymerizable monomer).

[0020] The content of acrylamide-based monomer units in the acrylamide-based polymer is preferably 30 mol % or more, more preferably 40 mol % or more, even more preferably 50 mol % or more, particularly preferably 55 mol % or more, and most preferably 60 mol % or more. When the content of the acrylamide-based monomer unit is 30 mol % or more, the solubility of the acrylamide-based polymer in an aqueous solvent or an aqueous mixed solvent tends to be improved. In addition, the upper limit of the content of acrylamide-based monomer units in the acrylamide-based polymer is not particularly limited, but from the viewpoint of fusion suppression and the like, it is preferably 99.9 mol % or less, more preferably 99 mol % or less, even more preferably 95 mol % or less, particularly preferably 90 mol % or less, and most preferably 85 mol % or less. The content of the acrylamide monomer unit is preferably 30 mol % to 99.9 mol %.

[0021] When the acrylamide polymer is a copolymer of an acrylamide monomer and another polymerizable monomer, the content of the other monomer units in the copolymer is preferably 0.1 mol % or more, more preferably 1 mol % or more, even more preferably 5 mol % or more, particularly preferably 10 mol % or more, and most preferably 15 mol % or more, from the viewpoint of fusion suppression and the like. From the viewpoint of improving the solubility of the acrylamide polymer in an aqueous solvent or an aqueous mixed solvent, the upper limit of the content of other monomer units is preferably 70 mol % or less, more preferably 60 mol % or less, even more preferably 50 mol %, particularly preferably 45 mol % or less, and most preferably 40 mol % or less. The content of the other monomer units is preferably 0.1 mol % to 70 mol %.

[0022] Examples of acrylamide monomers include acrylamide, ethacrylamide, crotonamide, itaconic acid diamide, cinnamic acid amide, maleic acid diamide, N-alkyl acrylamides such as N-methyl acrylamide, N-ethyl acrylamide, Nn-propyl acrylamide, N-isopropyl acrylamide, Nn-butyl acrylamide, and N-tert-butyl acrylamide, N-cycloalkyl acrylamides such as N-cyclohexyl acrylamide, dialkyl acrylamides such as N,N'-dimethyl acrylamide, dialkyl amino alkyl acrylamides such as dimethyl amino ethyl acrylamide and dimethyl amino propyl acrylamide, hydroxy alkyl acrylamides such as N-(hydroxy methyl) acrylamide and N-(hydroxy ethyl) acrylamide, N-aryl acrylamides such as N-phenyl acrylamide, diacetone acrylamide, and N,N'-methylene bisacrylamide, etc. N-alkylenebisacrylamides; methacrylamide; N-alkyl methacrylamides such as N-methyl methacrylamide, N-ethyl methacrylamide, Nn-propyl methacrylamide, N-isopropyl methacrylamide, N-n-butyl methacrylamide, and N-tert-butyl methacrylamide; N-cycloalkyl methacrylamides such as N-cyclohexyl methacrylamide; dialkyl methacrylamides such as N,N-dimethyl methacrylamide; dialkylaminoalkyl methacrylamides such as dimethylaminoethyl methacrylamide and dimethylaminopropyl methacrylamide; hydroxyalkyl methacrylamides such as N-(hydroxymethyl) methacrylamide and N-(hydroxyethyl) methacrylamide; N-aryl methacrylamides such as N-phenyl methacrylamide; diacetone methacrylamide; and N,N'-alkylene bismethacrylamides such as N,N'-methylene bismethacrylamide. Furthermore, from the viewpoint of the solubility of the acrylamide-based polymer in an aqueous solvent or an aqueous mixed solvent, among the above-mentioned acrylamide-based monomers, acrylamide, N-alkylacrylamide, dialkylacrylamide, methacrylamide, N-alkylmethacrylamide or dialkylmethacrylamide is preferred, and acrylamide is more preferred. The acrylamide monomers may be used alone or in combination of two or more.

[0023] Examples of other polymerizable monomers include vinyl cyanide monomers, unsaturated carboxylic acids and their salts, unsaturated carboxylic anhydrides, unsaturated carboxylic acid esters, aromatic vinyl monomers, vinyl halide monomers, vinyl alcohol monomers, vinyl carboxylate monomers, vinyl sulfonate monomers and their salts, and olefin monomers.

[0024] Examples of the vinyl cyanide monomer include acrylonitrile, methacrylonitrile, 2-hydroxyethyl acrylonitrile, chloroacrylonitrile, chloromethyl acrylonitrile, ethoxyacrylonitrile, and vinylidene cyanide. Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, crotonic acid, and isocrotonic acid. Examples of the salt of the unsaturated carboxylic acid include metal salts (for example, sodium salts, potassium salts, etc.), ammonium salts, and amine salts of the unsaturated carboxylic acid.

[0025] Examples of the unsaturated carboxylic acid anhydride include maleic anhydride and itaconic anhydride. Examples of the unsaturated carboxylate include methyl acrylate, methyl methacrylate, 2-hydroxyethyl acrylate, and 2-hydroxyethyl methacrylate. Examples of the aromatic vinyl monomer include styrene and α-methylstyrene. Examples of the vinyl halide monomer include vinyl chloride. The vinyl alcohol monomer includes vinyl alcohol. Examples of the vinyl carboxylate monomer include vinyl acetate and vinyl propionate. Examples of the sulfonic acid vinyl monomer include vinyl sulfonic acid, vinylbenzenesulfonic acid, and 2-acrylamido-2-methylpropanesulfonic acid. Examples of the salts of the sulfonic acid vinyl monomer include sodium salts, potassium salts, ammonium salts, and amine salts of the sulfonic acid vinyl monomer. Examples of the olefin monomer include ethylene, propylene, isopropylene, and butadiene.

[0026] Among the above-mentioned other polymerizable monomers, from the viewpoints of spinnability, fusion suppression, spinnability, etc. of the acrylamide polymer, vinyl cyanide monomers are preferred, and acrylonitrile is more preferred. Among the other polymerizable monomers described above, from the viewpoint of the solubility of the copolymer in an aqueous solvent or an aqueous mixed solvent, unsaturated carboxylic acids and salts thereof are preferred, and acrylic acid, maleic acid, fumaric acid or itaconic acid is more preferred. Among the other polymerizable monomers described above, from the viewpoint of suppressing fusion, unsaturated carboxylic acids or unsaturated carboxylic acid anhydrides are preferred, and acrylic acid, maleic acid, fumaric acid, itaconic acid or maleic anhydride are more preferred. The above-mentioned other polymerizable monomers may be used alone or in combination of two or more.

[0027] From the viewpoints of the solubility of the copolymer in an aqueous solvent or an aqueous mixed solvent, spinnability, fusion inhibition, and the like, the acrylamide-based polymer is particularly preferably a copolymer of an acrylamide-based monomer, a vinyl cyanide-based monomer, and an unsaturated carboxylic acid, and is most preferably a copolymer of acrylamide, acrylonitrile, and acrylic acid. From the viewpoints of spinnability, fusion suppression, etc., the content of vinyl cyanide monomer units in the copolymer is preferably 5 mol % to 40 mol %, and more preferably 10 mol % to 38 mol %. From the viewpoints of the solubility of the copolymer in an aqueous solvent or an aqueous mixed solvent, the fusion inhibition, etc., the content of unsaturated carboxylic acid units in the copolymer is preferably 1 mol % to 15 mol %, and more preferably 2 mol % to 10 mol %.

[0028] The weight average molecular weight of the acrylamide polymer is not particularly limited and is usually 5 million or less. From the viewpoint of the production and processability of the carbon material precursor, however, it is preferably 2 million or less, more preferably 1 million or less, even more preferably 500,000 or less, particularly preferably 200,000 or less, even more preferably 130,000 or less, and most preferably 100,000 or less. In addition, the lower limit of the weight average molecular weight of the acrylamide-based polymer is not particularly limited, but is usually 10,000 or more. From the viewpoint of the strength of the carbon material precursor and the carbon fiber, it is preferably 20,000 or more, more preferably 30,000 or more, and particularly preferably 40,000 or more.

[0029] In the present disclosure, the weight average molecular weight is measured by gel permeation chromatography under the following conditions: The measurement device may be HLC-8220GPC manufactured by Tosoh Corporation or a device equivalent thereto. (Measurement conditions) Column: TSKgel GMPWXL x 2 + TSKgel G2500PWXL x 1 Eluent: 100 mM sodium nitrate aqueous solution / acetonitrile (=80 / 20 (volume ratio)) ·Eluent flow rate: 1.0ml / min Column temperature: 40℃ Molecular weight standards: Standard polyethylene oxide / Standard polyethylene glycol Detector: Refractive index detector

[0030] The acrylamide polymer to be used may be a commercially available product, or may be one synthesized by a conventionally known method. The synthesis of an acrylamide polymer can be carried out by utilizing a known polymerization reaction such as radical polymerization, cationic polymerization, anionic polymerization, living radical polymerization, etc. Among the above polymerization reactions, radical polymerization is preferred from the viewpoint of reducing synthesis costs. The synthesis of an acrylamide polymer can be carried out by utilizing a polymerization method such as solution polymerization, suspension polymerization, precipitation polymerization, dispersion polymerization, or emulsion polymerization (for example, inverse phase emulsion polymerization). Furthermore, when synthesizing an acrylamide-based polymer by solution polymerization, it is preferable to use a solvent in which the raw material monomers and the resulting acrylamide-based polymer are soluble. From the viewpoint of low-cost and safe synthesis, it is more preferable to use an aqueous solvent or an aqueous mixed solvent, and even more preferable to use an aqueous solvent. Examples of the aqueous solvent include water, alcohol, and a mixture thereof, with water being particularly preferred. The aqueous mixed solvent means a mixed solvent of the above aqueous solvent and an organic solvent, and examples of the organic solvent include tetrahydrofuran, dimethylsulfoxide, and dimethylformamide.

[0031] In the synthesis of an acrylamide polymer by radical polymerization, it is preferable to use a polymerization initiator. As the polymerization initiator, a conventionally known radical polymerization initiator such as azobisisobutyronitrile, benzoyl peroxide, 4,4'-azobis(4-cyanovaleric acid), ammonium persulfate, potassium persulfate, etc. can be used. When an aqueous solvent or an aqueous mixed solvent is used as the solvent, a radical polymerization initiator soluble in the aqueous solvent or the aqueous mixed solvent, such as 4,4'-azobis(4-cyanovaleric acid), ammonium persulfate, or potassium persulfate, is preferred. From the viewpoint of controlling the molecular weight of the acrylamide polymer, it is preferable to use at least one of a polymerization accelerator and a molecular weight regulator in place of or together with the polymerization initiator, and it is more preferable to use a polymerization initiator and a polymerization accelerator in combination. The polymerization accelerator may, for example, be tetramethylethylenediamine. The molecular weight regulator may, for example, be an alkyl mercaptan compound such as n-dodecyl mercaptan. It is particularly preferable to use ammonium persulfate as a polymerization initiator in combination with tetramethylethylenediamine as a polymerization promoter.

[0032] The temperature of the polymerization reaction is not particularly limited, but from the viewpoint of controlling the molecular weight of the acrylamide polymer, it is preferably 35° C. or higher, more preferably 40° C. or higher, even more preferably 50° C. or higher, particularly preferably 70° C. or higher, and most preferably 75° C. or higher. The upper limit of the polymerization reaction temperature is not particularly limited, and can be 200° C. or lower.

[0033] The carbon material precursor may contain a polymer other than the acrylamide-based polymer. From the viewpoints of fusion inhibition, water resistance, etc., the content of the acrylamide polymer relative to the total mass of all polymers is preferably 50% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, even more preferably 99% by mass or more, and most preferably 100% by mass.

[0034] The polymer other than the acrylamide-based polymer is not particularly limited, but is preferably a polymer that dissolves or disperses in an aqueous solvent or an aqueous mixed solvent, more preferably a polymer that dissolves in an aqueous solvent or an aqueous mixed solvent, and even more preferably a water-soluble polymer. Examples of the other polymers preferably include polymers obtained by (co)polymerizing at least one selected from the group consisting of monomers such as unsaturated carboxylic acids and salts thereof, such as acrylic acid and methacrylic acid, unsaturated carboxylic acid esters, such as methyl acrylate, vinyl alcohol, vinyl acetate, and other vinyl carboxylates, vinylpyrrolidone, vinyl sulfonic acid and salts thereof, vinyl sulfonic acid esters, such as methyl vinyl sulfonate, vinylbenzenesulfonic acid and salts thereof, vinylbenzenesulfonic acid esters, carboxyvinyl, ethylene glycol, and polyalkylene glycols, such as propylene glycol, unsaturated carboxylic acid anhydrides, such as maleic anhydride, unsaturated dicarboxylic acids and salts thereof, such as maleic acid and fumaric acid, unsaturated dicarboxylic acid esters, such as monomethyl maleate and dimethyl maleate, 2-acrylamido-2-methylpropanesulfonic acid and salts thereof, and 2-acrylamido-2-methylpropanesulfonic acid esters; and hydrophilic polysaccharide polymers, such as acetyl cellulose and xanthan gum.

[0035] (Biomass fiber) The carbon material precursor of the present disclosure includes biomass fiber. The biomass fiber of the present disclosure is a fiber derived from a biological resource. The biological resource is not particularly limited, and examples thereof include cellulose (including lignocellulose containing lignin or hemicellulose, cellulose modified by chemical modification to carboxyl group, functional group containing a carboxyl group such as a carboxymethyl group, hydroxyethyl group, phosphoric acid group, polyphosphoric acid group, sulfonic acid group, functional group containing a sulfonic acid group such as a benzenesulfonic acid group, and salts thereof), nitrogen-containing polysaccharide polymers (chitin, chitosan, etc.), proteins (silk, spider silk, artificial proteins produced by microbial fermentation, etc.), etc. From the viewpoints of affinity with acrylamide-based polymers, heat resistance, reinforcing properties, carbonization yield, shape stability, etc., at least one selected from the group consisting of cellulose and nitrogen-containing polysaccharide polymers (chitin, chitosan). Here, chitosan has a structure almost identical to that of chitin, with chitin's amide groups replaced with amino groups, so biomass fibers derived from chitin and chitosan have equivalent properties (affinity with acrylamide polymers, heat resistance, reinforcing properties, carbonization yield, shape stability, etc.). The biomass fibers may be used alone or in combination of two or more kinds.

[0036] Biomass fibers can be produced by various production methods, and a preferred example of the production method is defibration of biological resources. Preferred examples of the defibration method include mechanical methods, chemical methods, and methods that combine these. Among these, biomass fibers produced by defibration using a mechanical method, or a combination of defibration using a mechanical method and defibration using a chemical method, are preferred.

[0037] Examples of defibration by mechanical means include methods of defibrating biological resources using a water jet, a high-pressure homogenizer, a grinder, an impact crusher, a bead mill, etc. It is also preferable to use biological resources that have been cut to a predetermined length using a beater, refiner, etc. for defibration.

[0038] When defibration by a mechanical method and defibration by a chemical method are used in combination, at least one of the biological resource and the biomass fiber can be chemically treated at one or more of the following times: before, during, and after defibration by the mechanical method. By chemically modifying at least one of the biological resource and the biomass fiber by chemical treatment and then defibration by a mechanical method, the biological resource can be further refined. Examples of defibration by chemical methods include a method in which all or a part of the hydroxyl groups on the surface of the biomass fiber are modified to easily ionized functional groups such as carboxyl groups and phosphate groups by a TEMPO oxidation treatment using 2,2,6,6-tetramethylpiperidine-1-oxyl (TEMPO), an oxidation treatment using sodium hypochlorite, a phosphoric acid esterification treatment, a sulfuric acid esterification treatment, etc., thereby making it easier to pulverize the biomass fibers by utilizing the electrostatic repulsion between the biomass fibers. Examples of the easily ionized functional groups include a carboxyl group, a functional group containing a carboxyl group such as a carboxymethyl group, a phosphoric acid group, a polyphosphoric acid group, a sulfonic acid group, a functional group containing a sulfonic acid group such as a benzenesulfonic acid group, and salts thereof (metal salts, ammonium salts, amine salts, etc.).

[0039] From the viewpoints of dispersibility in acrylamide polymers, heat resistance, reinforcing properties, carbonization yield, etc., the fiber diameter of the biomass fiber is preferably in the range of 1 nm to 100 μm, more preferably in the range of 2 nm to 50 μm, and even more preferably in the range of 3 nm to 20 μm.

[0040] The fiber diameter of the biomass fiber contained in the carbon fiber precursor is preferably in the range of 1 nm to 100 μm, more preferably in the range of 2 nm to 50 μm, and even more preferably in the range of 3 nm to 20 μm, from the viewpoints of heat resistance, reinforcing property, carbonization yield, and the like.

[0041] The average fiber length of the biomass fibers is not particularly limited, but is preferably in the range of 0.5 μm to 500 μm, and more preferably in the range of 1 μm to 200 μm.

[0042] The average fiber length of the biomass fibers contained in the carbon fiber precursor is not particularly limited, but is preferably in the range of 0.5 μm to 500 μm, and more preferably in the range of 1 μm to 200 μm.

[0043] The fiber diameter and average fiber length of the biomass fibers can be measured using a microscope, a transmission electron microscope (TEM), a scanning electron microscope (SEM), a scanning probe microscope (SPM), or the like.

[0044] When the biomass fiber is derived from cellulose and nitrogen-containing polysaccharide polymers (chitin, chitosan), the degree of polymerization is not particularly limited, but from the viewpoints of heat resistance, reinforcing property, carbonization yield, shape stability, and handleability of the composition for producing a carbon material precursor, it is preferably 50 to 10,000, more preferably 75 to 5,000, and even more preferably 100 to 2,000.

[0045] The degree of polymerization of cellulose and nitrogen-containing polysaccharide polymers (chitin, chitosan) is the number of glucose units linked together, which is the smallest structural unit, and is proportional to the fiber length of the biomass fiber. The degree of polymerization is determined by a viscosity method using a copper ethylenediamine solution. Specifically, 30 g of a suspension in which biomass fiber is diluted with ion-exchanged water to a content of 2±0.3% by mass is dispensed into a centrifuge tube and left to freeze overnight in a freezer. The suspension is then dried in a freeze dryer for 5 days or more, and then heated in a constant temperature dryer set at 105°C for 3 to 4 hours to obtain bone-dry biomass fiber. To measure the reference, 15 ml of pure water and 15 ml of 1 mol / L copper ethylenediamine are added to an empty 50 ml screw tube to prepare a 0.5 mol / L copper ethylenediamine solution. 10 ml of the above 0.5 mol / L copper ethylenediamine solution is placed in a Cannon-Fenske viscometer, left for 5 minutes, and the drop time at 25°C is measured to determine the solvent drop time. Next, to measure the viscosity of the biomass fiber, 0.14g to 0.16g of bone-dry biomass fiber is weighed into an empty 50ml screw tube and 15ml of pure water is added. 15ml of 1mol / L copper ethylenediamine is then added and stirred for 10 minutes at 1000rpm in a planetary super mixer to obtain a 0.5mol / L copper ethylenediamine solution in which the biomass fiber is dissolved. As in the reference measurement, 10ml of the prepared 0.5mol / L copper ethylenediamine solution is placed in a Cannon-Fenske viscometer and left for 5 minutes, after which the fall time at 25°C is measured. The fall time is measured three times and the average value is taken as the fall time of the biomass fiber solution. The degree of polymerization is calculated using the following formula from the mass of the bone-dry biomass fiber used in the measurement, the solvent dripping time, and the biomass fiber solution dripping time. Note that if the degree of polymerization is measured twice or more, the average value is used.

[0046] Mass of biomass fiber in an absolute dry state used in the measurement: a (g) (where a is 0.14 to 0.16) Cellulose concentration in solution: c = a / 30 (g / mL) Solvent drop time: t 0 (sec) Biomass fiber solution drop time: t (sec) Relative viscosity of the solution: η rel =t / t 0 Specific viscosity of the solution: η sp = η rel -1 ·Intrinsic viscosity:[η]=η sp / c(1+0.28η sp ) ·Polymerization degree: DP=[η] / 0.57

[0047] In the present disclosure, homemade or commercially available biomass fibers may be used. Examples of commercially available biomass fibers include RMa-10002, RMa-10005, IMa-10002, IMa-10005, BMa-10002, BMa-10005, BMa-10010, WFo-10002, WFo-10005, WFo-10010, AFo-10002, AFo-10005, AFo-10010, FMa-10002, FMa-10005, FMa-10010, WFo-UNDP, FMa-UNDP, CMF-05DP, and TFo- 10002, TFo-10005, SFo-20002, SFo-20005, SFo-20010, EFo-08002, EFo-08005, EFo-08010 and KCo-30005, PC110T, PC110A, PC100B, Roka Meijin, PC110S, FD100F, FD100G, FD200L, KY100S and KY100G manufactured by Daicel Miraize Ltd., nanoforest-S and nanoforest-M manufactured by Chuetsu Pulp Industry Co., Ltd., T-OP 100 manufactured by Toagosei Co., Ltd., I-2SX, C-2SP, I-2AX and I-2SXS manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and ELLEX-S, ELLEX-P and ELLEX-☆ manufactured by Daio Paper Corporation.

[0048] From the viewpoint of suppressing fusion and sagging during stretching or flame-resistant treatment, the content of the biomass fiber is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.75 mass% or more, based on the content of the acrylamide-based polymer, and from the viewpoint of manufacturability of the composition for producing a carbon material precursor, the content is preferably 40 mass% or less, more preferably 20 mass% or less, and even more preferably 15 mass% or less.

[0049] (Other Ingredients) The carbon material precursor of the present disclosure may further contain additive components such as organic solvents, surfactants, crosslinking agents, flame retardant accelerators (such as a group consisting of acids and their salts), chlorides such as sodium chloride and zinc chloride, hydroxides such as sodium hydroxide, various fillers such as glass fibers, carbon black, carbon nanotubes, and graphene, dispersants, smoothing agents, moisture absorbents, viscosity modifiers, plasticizers, release agents, spreading agents, antioxidants, antibacterial agents, preservatives, rust inhibitors, and pH adjusters. The content of the additive components can be appropriately adjusted.

[0050] When the carbon material precursor of the present disclosure contains a flame-resistant accelerator, the formation of a cyclic structure due to a dehydration reaction, a deammonification reaction, etc. is accelerated when the carbon material precursor is subjected to a flame-resistant treatment, and the fusion suppression, the carbonization yield, the strength of the carbon material, and the shape stability tend to be further improved. Note that at least a part of the flame-resistant component and its residue may remain in the carbon material according to the present disclosure.

[0051] Examples of the flame retardant accelerator include inorganic acids such as phosphoric acid, polyphosphoric acid, boric acid, sulfuric acid, nitric acid, and carbonic acid, and organic acids such as oxalic acid, citric acid, and sulfonic acid. Further examples include metal salts (sodium salts, potassium salts, etc.), ammonium salts, and amine salts of these acids. Among the above, from the viewpoints of fusion inhibition, carbonization yield, and strength and shape stability of the carbon material, the flame retardation accelerator is preferably phosphoric acid, polyphosphoric acid, boric acid, sulfuric acid, or an ammonium salt thereof, more preferably phosphoric acid, polyphosphoric acid, boric acid, or an ammonium salt thereof, and still more preferably phosphoric acid, polyphosphoric acid, an ammonium salt of phosphoric acid, or an ammonium salt of polyphosphoric acid.

[0052] From the viewpoints of fusion inhibition, carbonization yield, and strength and shape stability of the carbon material, the content of the flame retardant accelerator is preferably 0.1 parts by mass to 100 parts by mass, more preferably 0.2 parts by mass to 50 parts by mass, even more preferably 0.5 parts by mass to 30 parts by mass, and particularly preferably 1 part by mass to 20 parts by mass, relative to 100 parts by mass of the acrylamide-based polymer.

[0053] When the carbon material precursor of the present disclosure is in a fibrous form, a conventionally known oil such as a silicone-based oil may be applied to the surface from the viewpoint of improving bundling ability and suppressing fusion of the fibers.

[0054] <Composition for producing carbon material precursor> The composition for producing a carbon material precursor according to the present disclosure includes biomass fibers, an acrylamide-based polymer, and a solvent. The carbon material precursor-producing composition is dried to remove at least a part of the solvent, thereby obtaining a carbon material precursor. For example, a film-shaped carbon material precursor is obtained by drying a coating of the carbon material precursor-producing composition.

[0055] Examples of the solvent include aqueous solvents (water, alcohol, etc., and mixed solvents thereof), aqueous mixed solvents (mixed solvents of the aqueous solvents and organic solvents (tetrahydrofuran, etc.)), and the like, and preferably contain water. The solvent may be used alone or in combination of two or more kinds. From the viewpoint of reducing production costs and reducing environmental impact, the content of water relative to the total amount of solvent is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, particularly preferably 99 mass% or more, and may be 100 mass%.

[0056] The content of the solvent in the composition for producing a carbon material precursor can be appropriately adjusted from the viewpoints of coating, spinning, etc., and from the viewpoint of manufacturability, it is preferably 5 to 99%, more preferably 10 to 95%, and even more preferably 25 to 90%.

[0057] The acrylamide-based polymer in the composition for producing a carbon material precursor is the same as that described in the carbon material precursor.

[0058] The biomass fibers in the composition for producing a carbon material precursor are the same as those described for the carbon material precursor. Biomass fibers may be used as a liquid dispersion. Examples of liquids (also referred to as dispersion media in the present disclosure) include aqueous solvents (water, alcohol, etc., and mixtures thereof), aqueous mixed solvents (mixtures of the aqueous solvents and organic solvents (tetrahydrofuran, etc.)), and preferably contain water. Since acrylamide-based polymers are water-soluble, water can be used as a dispersion medium, reducing the environmental impact.

[0059] The content of the biomass fiber relative to the content of the acrylamide-based polymer in the composition for producing a carbon material precursor is the same as in the case of the carbon material precursor.

[0060] The composition for producing a carbon material precursor may contain the additive component described in the carbon material precursor. When the composition for producing a carbon material precursor contains the additive component, the content of the additive component is the same as that of the carbon material precursor.

[0061] <Method of producing composition for producing carbon material precursor> The method for producing the composition for producing a carbon material precursor is not particularly limited as long as the composition for producing a carbon material precursor can be obtained, and the composition may be prepared by mixing a biomass fiber, an acrylamide-based polymer, and a solvent. Water can be used as the solvent, which reduces the environmental load.

[0062] The acrylamide-based polymer in the method for producing the composition for producing a carbon material precursor is the same as that described for the carbon material precursor.

[0063] The biomass fiber in the method for producing a composition for producing a carbon material precursor is the same as that described for the carbon material precursor, and it is preferable to use a liquid dispersion of biomass fiber, and it is more preferable that the dispersion medium contains water. From the viewpoint of dispersibility of the biomass fiber, the content of the biomass fiber in the liquid dispersion of the biomass fiber is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less. Also, from the viewpoint of reducing the drying energy for obtaining a carbon material precursor, the content of the biomass fiber in the liquid dispersion of the biomass fiber is preferably 0.5% by mass or more, more preferably 0.75% by mass or more, and even more preferably 1.0% by mass or more.

[0064] The content of the biomass fiber relative to the content of the acrylamide-based polymer in the composition for producing a carbon material precursor is the same as in the case of the carbon material precursor.

[0065] The solvent in the method for producing a composition for producing a carbon material precursor is the same as that explained for the composition for producing a carbon material precursor, and preferably contains water.

[0066] Specific methods for mixing biomass fiber, an acrylamide polymer, and a solvent include dispersing biomass fiber powder in an acrylamide polymer solution, adding an acrylamide polymer to a biomass fiber liquid dispersion, adding an acrylamide polymer and a solvent to a biomass fiber liquid dispersion, mixing an acrylamide polymer solution with a biomass fiber liquid dispersion, mixing an acrylamide polymer, a biomass fiber liquid dispersion, and a solvent, mixing an acrylamide polymer, a biomass fiber powder, and a solvent, kneading biomass fiber powder with an acrylamide polymer and then adding a solvent, etc. From the viewpoints of environmental load and being able to disperse biomass fiber easily and at low cost, it is preferable to use a biomass fiber liquid dispersion, and it is more preferable for the dispersion medium to contain water.

[0067] Furthermore, the composition for producing a carbon material precursor may be prepared by adding the above-mentioned additive component. When the additive component is added, the content of the additive component per 100 parts by mass of the acrylamide-based polymer is the same as that of the carbon material precursor. The composition for producing a carbon material precursor may be prepared by adding the other additive components described above. The additive component and other additive components may be mixed together with the acrylamide-based polymer and mass fiber to prepare a composition for producing a carbon material precursor.

[0068] <Method of producing carbon material precursor> In the method for producing a carbon material precursor according to the present disclosure, the composition for producing a carbon material precursor according to the present disclosure is dried to obtain a carbon material precursor. The carbon material precursor thus obtained is inhibited from melting and sagging due to softening during stretching or flame-resistant treatment.

[0069] The composition for producing a carbon material precursor used in the method for producing a carbon material precursor can be obtained by the above-mentioned method for producing a composition for producing a carbon material precursor.

[0070] The drying temperature for the composition for producing a carbon material precursor may be any temperature that can remove at least a part of the solvent.

[0071] <Method of manufacturing carbon materials> The method for producing a carbon material according to the present disclosure includes subjecting a carbon material precursor according to the present disclosure to a flame-resistant treatment to obtain a flame-resistant material (hereinafter also referred to as a "flame-resistant treatment step"), and carbonizing the flame-resistant material (hereinafter also referred to as a "carbonization treatment step"). By using the carbon material precursor of the present disclosure, fusion and sagging due to softening during the flame-resistant treatment can be suppressed. The carbon material precursor used in the method for producing a carbon material of the present disclosure is as described above.

[0072] (Flame-resistant treatment process) The flame-resistant treatment of the carbon material precursor can be carried out by subjecting the carbon material precursor to a heat treatment in an oxidizing atmosphere.

[0073] The flame retardant treatment is not particularly limited, but is preferably carried out at a temperature in the range of 150°C to 500°C, more preferably at a temperature in the range of 175°C to 450°C, and even more preferably at a temperature in the range of 200°C to 420°C. The above temperature includes not only the maximum temperature during the flame-resistant treatment (flame-resistant treatment temperature) described below, but also the temperature during the temperature rise process up to the flame-resistant treatment temperature.

[0074] The maximum temperature during the flame retardant treatment (flame retardant treatment temperature) is preferably 200°C to 500°C, more preferably 250°C to 450°C, even more preferably 305°C to 440°C, particularly preferably 310°C to 430°C, and most preferably 315°C to 420°C. By setting the flame-retardant treatment temperature to 250° C. or higher, the heat resistance and carbonization yield of the flame-retardant material tend to be improved. Moreover, by setting the flame-retardant treatment temperature to 500° C. or less, thermal decomposition of the flame-retardant material tends to be suppressed.

[0075] In the flame-resistant treatment of the carbon material precursor, it is preferable to subject the carbon material precursor to a stretching treatment, which tends to orient the crosslinked acrylamide polymer contained in the carbon material precursor and improve the tensile strength of the flame-resistant product. The stretching treatment is preferably carried out at least during heating at the flame-proofing treatment temperature. From the viewpoint of improving the tensile strength of the flame-resistant product, it is preferable to carry out the stretching treatment also during the temperature rise process up to the flame-resistant treatment temperature. The stretching treatment may be carried out from the beginning or during the temperature rise process. In one embodiment, the stretching treatment is carried out at the flame retardant treatment temperature, and the other temperatures For the above, the stretching process does not need to be carried out. The stretching treatment may be carried out while controlling the moisture absorption rate during the spinning treatment or in a step prior to the flame retardant treatment.

[0076] The tension applied to the carbon material precursor during the stretching process is not particularly limited, but in the case of a fiber shape, it is preferably 0.05 mN / tex to 2000 mN / tex, more preferably 0.1 mN / tex to 500 mN / tex, even more preferably 0.1 mN / tex to 200 mN / tex, and particularly preferably 0.2 mN / tex to 100 mN / tex. By setting the tension applied to the carbon material precursor during the stretching process within the above numerical range, it is possible to improve the fusion suppression property and to suppress the occurrence of breakage and fluff in the flame-resistant material.

[0077] In the present disclosure, the tension (unit: mN / tex) applied to a fibrous carbon material precursor is the value obtained by dividing the tension (unit: mN) applied to the carbon material precursor during the flame-resistant treatment by the fineness (unit: tex) of the carbon material precursor in an absolute dry state, i.e., the tension per unit fineness of the carbon material precursor. The tension can be adjusted by adjusting the speed at the inlet and outlet of a heating device such as a flame-proofing furnace, or by using a load cell, a spring, a weight, an air cylinder, or the like.

[0078] The flame retardant treatment time (heating time at the flame retardant treatment temperature) is not particularly limited, but from the viewpoints of carbonization yield and production costs, it is preferably 1 to 120 minutes, more preferably 2 to 60 minutes, even more preferably 3 to 50 minutes, and particularly preferably 4 to 40 minutes. The flame-proofing treatment time may be set to a long time of more than 2 hours.

[0079] Furthermore, the carbon material precursor of the present disclosure may be subjected to a crosslinking treatment using an electron beam, ultraviolet light, heat, or the like from the viewpoint of improving heat resistance, strength, carbonization yield, shape stability, or moisture resistance, within a range that does not significantly impair the extensibility of the carbon material precursor.

[0080] (Carbonization process) The carbonization treatment refers to a treatment for carbonizing a carbon material precursor, and means carrying out a heat treatment in a low-oxygen environment (preferably an environment in which oxygen is blocked).

[0081] The carbonization method may be a method in which the flame-resistant material is subjected to a heat treatment in an inert gas (nitrogen, argon, helium, etc.) atmosphere at a temperature higher than that in the flame-resistant treatment. By the carbonization treatment, the flame-retardant material is carbonized to obtain a carbon material. The maximum heating temperature in the carbonization treatment is preferably 500°C or higher, more preferably 1000°C or higher, even more preferably 1100°C or higher, particularly preferably 1200°C or higher, and most preferably 1300°C or higher. Moreover, the upper limit of the maximum heating temperature is preferably 3000° C. or less, and more preferably 2500° C. or less. The maximum heating temperature in the carbonization treatment is preferably 500°C to 3000°C.

[0082] Furthermore, the heating time at the maximum temperature in the carbonization treatment is not particularly limited, but is preferably from 30 seconds to 60 minutes, and more preferably from 1 minute to 30 minutes.

[0083] In the present disclosure, the "carbonization treatment" may also include "graphitization" which is generally performed by heating at a temperature of 2000°C to 3000°C in an inert gas atmosphere. The carbonization process may include multiple heat treatments. For example, a heat treatment (preliminary carbonization treatment) can be first performed at a temperature less than 1000°C, then a heat treatment (carbonization treatment) can be performed at a temperature of 1000°C or higher, and finally a heat treatment (graphitization treatment) can be performed at a temperature of 2000°C or higher. EXAMPLES

[0084] The above embodiment will be specifically described below with reference to examples, but the above embodiment is not limited to these examples.

[0085] [Example 1] An aqueous solution was obtained by dissolving 100 parts by mass of a monomer composition containing 60 mol % of acrylamide (AM), 35 mol % of acrylonitrile (AN) and 5 mol % of acrylic acid (AA) and 5 parts by mass of tetramethylethylenediamine in 400 parts by mass of ion-exchanged water. Ammonium persulfate was added to the resulting aqueous solution while stirring under a nitrogen atmosphere, and the mixture was then heated at 80° C. for 150 minutes to carry out a polymerization reaction. The obtained aqueous solution was dropped into methanol to precipitate the copolymer, which was then recovered and vacuum dried at 80°C for 12 hours to obtain a water-soluble AM / AN / AA copolymer (AM / AN / AA = 60 mol% / 35 mol% / 5 mol%, "acrylamide-based polymer (a-1)").

[0086] 100 parts by mass of the obtained acrylamide-based polymer (a-1), 3 parts by mass of phosphoric acid, and 100 parts by mass of cellulose-derived biomass fiber IMa-10002 (manufactured by Sugino Machine Co., Ltd., 2 mass% water dispersion, average fiber diameter 10-50 nm (catalog value), degree of polymerization 800 (catalog value)) were added to ion-exchanged water to obtain a composition for producing a carbon material precursor. Note that, as a result of observation under a microscope, IMa-10002 contained some biomass fiber with a fiber diameter at the micron level (1-5 μm). The obtained composition for producing a carbon material precursor was dried on a petri dish made of Teflon (registered trademark) to prepare a film sample as a carbon material precursor.

[0087] [Example 2] A film sample was produced in the same manner as in Example 1, except that IMa-10002 was replaced with cellulose-derived biomass fiber WFo-10002 (manufactured by Sugino Machine Co., Ltd., 2 mass% aqueous dispersion, average fiber diameter 10-50 nm (catalog value), degree of polymerization 650 (catalog value)). Microscopic observation revealed that WFo-10002 contained some biomass fiber with a fiber diameter at the micron level (1-4 μm).

[0088] [Example 3] A film sample was produced in the same manner as in Example 1, except that IMa-10002 was changed to cellulose-derived biomass fiber FMa-10002 (manufactured by Sugino Machine Co., Ltd., 2 mass% aqueous dispersion, average fiber diameter 10 to 50 nm (catalog value), degree of polymerization 200 (catalog value)). Note that, as a result of observation under a microscope, FMa-10002 contained some biomass fiber with a fiber diameter at the micron level (1 to 5 μm).

[0089] [Example 4] A film sample was produced in the same manner as in Example 1, except that IMa-10002 was changed to a biomass fiber derived from chitin, a nitrogen-containing polysaccharide polymer (SFo-10002, manufactured by Sugino Machine Co., Ltd., 2 mass% aqueous dispersion, average fiber diameter 10-50 nm, degree of polymerization 300). Note that, as a result of observation under a microscope, SFo-10002 contained some biomass fiber with a fiber diameter at the micron level (1-3 μm).

[0090] [Comparative Example 1] A film sample was prepared in the same manner as in Example 1, except that no biomass fiber was used.

[0091] <Evaluation> (Heat resistance evaluation) The prepared film samples were processed into strips of 5 mm width and 30 mm length, and viscoelasticity measurements were performed using a horizontal dynamic viscoelasticity measuring device (IT Measurement and Control Co., Ltd., DVA-220). Measurements were performed under the following conditions: temperature: room temperature to 300°C, temperature rise: 10°C / min, data acquisition interval: 1°C, frequency: 1Hz, strain: 0.05%, static-dynamic ratio: 2.5, chuck distance: 20mm. The storage modulus at each temperature was calculated from the measurement data. The results are shown in Table 1.

[0092] (Sagging evaluation) The state of the rectangular sample after the above viscoelasticity measurement was observed. As shown in Figure 1, the length (L) of the straight line connecting the gripping parts of the gripping member 10 of the dynamic viscoelasticity measuring device and the base side of the rectangular sample 20 were measured. The results are shown in Table 1.

[0093] (Fusion evaluation) Two of the prepared film samples were placed on top of each other on a hot plate and heated from room temperature to 200°C, after which it was checked with tweezers whether the film samples could be peeled off from each other on the hot plate. After that, each time the temperature was raised by 25°C up to 300°C, it was checked with tweezers whether the film samples could be peeled off from each other on the hot plate. The temperature at which the film samples could no longer be peeled off from each other was taken as the fusion temperature. The results are shown in Table 1.

[0094] (Carbonization evaluation) The carbonization of the prepared film sample was evaluated using a differential thermobalance (Rigaku Corporation, ThermoPlusEV02). A platinum pan containing a film sample (approximately 1-2 mg) was set on the differential thermobalance, and the film sample was heated from room temperature to 350°C at a heating rate of 10°C / min in an air atmosphere, and then held at 350°C for 10 minutes to perform flame retardation, obtaining a flame-retarded film sample. The flame-retardant film sample was then carbonized in a nitrogen atmosphere by heating it from room temperature to 1200°C at a heating rate of 20°C / min while still in the platinum pan, while measuring the mass. The carbonization yield was calculated from the measured mass using the following formula. The results are shown in Table 1. Carbonization yield (%) = mass at each carbonization temperature / mass of film sample after flame retardation × 100

[0095] (Observation of biomass fibers in film) The cross section of the film was cut using a microtome and observed using a TEM to determine the range of fiber diameters of the biomass nanofibers in the film. From the observation results, the range of fiber diameters of the biomass fibers present in the film is shown in Table 1.

[0096] [Table 1]

[0097] As shown in Table 1, the results of the viscoelasticity measurement show that in the high temperature range of 160°C or higher, Examples 1 to 3 containing cellulose-derived biomass fiber have storage moduli that are about 1.5 to 4 times higher than Comparative Example 1, which does not contain any biomass fiber, and thus have improved heat resistance. This shows that tension can be easily applied during stretching and flame-retardant treatment. In particular, Examples 1 and 2, which have a high degree of polymerization, have higher storage moduli in the high temperature range than Example 3.

[0098] Furthermore, when observing the sagging state of the film sample (carbon material precursor) after heating to 300°C in the viscoelasticity measurement, it was found that Comparative Example 1 sagged 6 mm, whereas Examples 1 to 3 showed almost no sagging, indicating that softening was suppressed by the inclusion of biomass fiber.

[0099] Furthermore, in the results of the fusion evaluation, Comparative Example 1 was completely fused at 200°C, whereas Examples 1 to 3 were not fused even at 300°C, indicating that fusion is suppressed by the inclusion of biomass fiber.

[0100] In the examples, fusion is suppressed up to 300° C., which is above the glass transition temperature of the acrylamide polymer, about 160° C., and since a ring structure is formed near 300° C. and the polymer becomes infusible, fusion is similarly suppressed even at temperatures above 300° C. For the same reasons as above, it is believed that sagging is further suppressed at temperatures above 300° C.

[0101] The carbonization evaluation results show that Examples 1 and 2, which contain biomass fiber, have slightly higher carbonization yields than Comparative Example 1, and can be used as a carbon material precursor. Example 3 has a slightly lower carbonization yield than Comparative Example 1, but is almost the same, and a sufficiently high carbonization yield is obtained, so that it can be used as a carbon material precursor.

[0102] Furthermore, Example 4, which contains biomass fiber derived from chitin, a nitrogen-containing polysaccharide polymer, had a higher storage modulus in the high temperature range than Comparative Example 1, which did not contain biomass fiber, and had a storage modulus that was approximately the same as Examples 1 to 3, which used cellulose fiber. Dragging of the film sample and fusion between the film samples were also suppressed. Regarding the carbonization yield, Example 4, which contains biomass fiber derived from chitin, a nitrogen-containing polysaccharide polymer, had a higher carbonization yield than Comparative Example 1, indicating that it can be used as a carbon material precursor.

[0103] [Examples 5 to 8] Except for changing the amount of cellulose-derived biomass fiber added relative to 100 parts by mass of acrylamide polymer (a-1) as shown in Table 2, film samples were produced in the same manner as in Example 1. Heat resistance, sagging, adhesion, and carbonization were also evaluated in the same manner.

[0104] [Table 2]

[0105] As shown in Table 2, when the amount of biomass fiber added is increased to 5 parts by mass or 10 parts by mass, the storage modulus in the high temperature range increases further, making it easier to apply higher tension during stretching and flame-retardant treatment. Dragging of the film sample and fusion between film samples are also suppressed. The carbonization yield is also roughly the same as when the amount of biomass fiber added is 2 parts by mass, and a sufficiently high carbonization yield is obtained, indicating that it can be used as a carbon material precursor. [Explanation of symbols]

[0106] 10: gripping member of dynamic viscoelasticity measuring device, 20: rectangular sample

Claims

1. A carbon material precursor comprising a biomass fiber and an acrylamide-based polymer.

2. 2. The carbon material precursor according to claim 1, wherein the content of the biomass fiber is 0.1 to 40 mass % based on the content of the acrylamide-based polymer.

3. 3. The carbon material precursor according to claim 1, wherein the biomass fiber is a fiber derived from at least one selected from the group consisting of cellulose and nitrogen-containing polysaccharide polymers.

4. 3. The carbon material precursor according to claim 1, wherein the fiber diameter of the biomass fiber is within a range of 1 nm to 100 μm.

5. A method for producing a carbon material precursor according to claim 1 or 2 by subjecting the carbon material precursor to a flame-resistant treatment; and carbonizing the flame-resistant material.

6. A composition for producing a carbon material precursor, comprising biomass fibers, an acrylamide-based polymer, and a solvent.

7. The composition for producing a carbon material precursor according to claim 6 , wherein the solvent comprises water.

8. A method for producing a composition for producing a carbon material precursor, comprising mixing biomass fiber, an acrylamide-based polymer, and a solvent.

9. The method for producing a composition for producing a carbon material precursor according to claim 8 , wherein the solvent contains water.

10. The method for producing a composition for producing a carbon material precursor according to claim 8 or 9, wherein a liquid dispersion of the biomass fibers is used.

11. A method for producing a carbon material precursor, comprising drying a composition for producing a carbon material precursor, the composition comprising biomass fibers, an acrylamide-based polymer, and a solvent.

12. The method for producing a carbon material precursor according to claim 11 , wherein the solvent comprises water.

13. The method for producing a carbon material precursor according to claim 11 or 12, wherein a liquid dispersion of the biomass fibers is used.

Citation Information

Patent Citations

  • Silicone oil for fiber of carbon fiber precursor, fiber of carbon fiber precursor, flame resistant fiber, carbon fiber and method for producing the same

    JP2006183159A

  • Precursor fiber for carbon fiber, carbon fiber and method for producing thereof

    JP2008202208A

  • Carbon material precursor, carbon material precursor composition containing the same, and manufacturing method of carbon material using the same

    JP2019026827A

  • Carbon material precursor, carbon material precursor composition containing the same, and method for producing carbon material using these

    JP2019167516A

  • Carbon material precursor composition, method for producing same, and method for producing carbon material using same