Method for producing block copolymer

A two-step radical polymerization method using polyfunctional thiol compounds addresses the limitations of existing block copolymer synthesis, enabling efficient production of diverse block copolymers suitable for large-scale applications by controlling monomer conversion rates and structures.

JP2024136726APending Publication Date: 2024-10-04MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023047936
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for synthesizing block copolymers, such as those using living anionic polymerization or radical polymerization with macromonomers, are costly, require controlled environments, and restrict the types of monomers and structures that can be used, making them unsuitable for large-scale production and applications like polymer dispersants.

Method used

A two-step radical polymerization method using a secondary or higher polyfunctional thiol compound as a chain transfer agent, allowing for the production of block copolymers with diverse monomer types and structures by controlling the conversion rates of vinyl monomers in each step.

Benefits of technology

This method enables the production of block copolymers with desired structures efficiently, using various monomer compositions, and avoids the limitations of previous methods, facilitating large-scale production and applications requiring low viscosity and easy dispersion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136726000007
    Figure 2024136726000007
  • Figure 2024136726000008
    Figure 2024136726000008
  • Figure 2024136726000001
    Figure 2024136726000001
Patent Text Reader

Abstract

To provide a method for producing a block copolymer that is applicable to various vinyl monomer species, enables polymerization in various monomer compositions, and facilitates easy production of a block copolymer with a desired structure.SOLUTION: A method for producing a block copolymer includes: a first step where, in the presence of a secondary or more polyfunctional thiol compound, a first vinyl monomer is radical polymerized to obtain a polymer; and a second step where, in the presence of the secondary or more polyfunctional thiol compound and the polymer obtained in the first step, a second vinyl monomer is radical polymerized.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a block copolymer. [Background technology]

[0002] Known common methods for synthesizing block copolymers include living polymerization methods such as living anionic polymerization, reversible addition-fragmentation chain transfer polymerization, and atom transfer radical polymerization. However, these polymerization methods use relatively expensive reagents, and the reaction is difficult to control in the presence of oxygen and water, making them unsuitable for large-scale production of block copolymers in factories, for example.

[0003] In recent years, therefore, studies have been conducted on methods for synthesizing block copolymers that are less expensive and easier to handle. For example, Patent Document 1 discloses a method for synthesizing a block copolymer by using a macromonomer as a copolymerization component and carrying out radical polymerization of a vinyl monomer. Patent Document 2 discloses a method for synthesizing a star block copolymer by radically polymerizing a vinyl monomer in two stages using a multifunctional thiol compound as a chain transfer agent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-88763 A [Patent Document 2] JP 2001-139646 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, as described in Patent Document 1, in the method of synthesizing a block copolymer by copolymerization of a macromonomer, the molecular weight generally tends to be very large. Therefore, the block copolymer obtained by the method described in Patent Document 1 is not suitable for use as a polymer dispersant, for example, where low viscosity and easy dispersion are required. In addition, the types of monomers that can be copolymerized with the macromonomer are also limited, and the structure of the block copolymer that can be synthesized is likely to be restricted.

[0006] The method described in Patent Document 2 is a method for synthesizing a star block copolymer using a chain transfer agent, and therefore it is possible to reduce the molecular weight of the block copolymer. However, when the conversion rate of the vinyl monomer in the first radical polymerization is 100%, most of the thiol groups of the multifunctional thiol compound react, and therefore, even if the second radical polymerization is performed, the vinyl monomer used in the second radical polymerization is homopolymerized, and almost no star block copolymer is obtained. Therefore, in the method described in the cited document 2, it is necessary to stop the polymerization at a stage where the conversion rate of the first-stage vinyl monomer is low, and then add the second-stage vinyl monomer to carry out the polymerization, which tends to limit the structure and composition of the star block copolymer that can be synthesized.

[0007] An object of the present invention is to provide a method for producing a block copolymer, which is applicable to various types of vinyl monomers, enables polymerization with various monomer compositions, and enables easy production of a block copolymer having a desired structure. [Means for solving the problem]

[0008] The present invention has the following aspects. [1] A first step of radically polymerizing a first vinyl monomer in the presence of a secondary or higher polyfunctional thiol compound to obtain a polymer; and a second step of radically polymerizing a second vinyl monomer in the presence of the secondary or higher polyfunctional thiol compound and the polymer obtained in the first step. [2] The method for producing the block copolymer according to [1] above, wherein the secondary or higher functional thiol compound has a valence of 2 to 100. [3] The method for producing a block copolymer according to [1] or [2] above, wherein the first vinyl monomer comprises at least one selected from the group consisting of a (meth)acrylic acid ester and an aromatic vinyl compound. [4] The method for producing a block copolymer according to any one of the above [1] to [3], wherein the conversion of the first vinyl monomer is 51% or more. [5] The method for producing a block copolymer according to any one of the above [1] to [4], wherein the second vinyl monomer comprises at least one selected from the group consisting of a (meth)acrylic acid ester and an aromatic vinyl compound, and is a vinyl monomer different from the first vinyl monomer. [6] The method for producing a block copolymer according to any one of [1] to [5] above, wherein in the first step, the first vinyl monomer is charged all at once before being polymerized, and in the second step, the second vinyl monomer is charged all at once before being polymerized. Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for producing a block copolymer which is applicable to various types of vinyl monomers, enables polymerization with various monomer compositions, and enables simple production of a block copolymer having a desired structure. [Brief description of the drawings]

[0010] [Figure 1] 1 is a gel permeation chromatography (GPC) chromatogram of the block copolymer in Example 5. [Diagram 2] 1 is a gel permeation chromatography (GPC) chromatogram of a block copolymer in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The following describes in detail the forms for implementing the present invention, but the present invention is not limited to the embodiments described below, and various modifications are possible without departing from the gist of the present invention. In this specification and claims, a numerical range expressed by "to" means a numerical range including the numerical values ​​before and after "to" as the lower and upper limits. In the present specification and claims, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic. Similarly, "(meth)acrylate" is a general term for acrylate and methacrylate.

[0012] [Method of manufacturing block copolymer] The method for producing a block copolymer according to the present embodiment includes the following first and second steps.

[0013] <1st process> The first step is a step of obtaining a polymer by radical polymerization of a first vinyl monomer in the presence of a secondary or higher polyfunctional thiol compound. In the following description, the polyfunctional thiol compound used in the first step is referred to as a "polyfunctional thiol compound (T)", and the polymer obtained in the first step is referred to as a "polymer (P)". The conditions for the radical polymerization in the first step will be described later.

[0014] The polyfunctional thiol compound (T) serves as a chain transfer agent. The number of series of the multifunctional thiol compound (T) is 2 or more. If the number of series of the multifunctional thiol compound (T) is 1, the chain transferability to the vinyl monomer becomes too high, and most of the thiol groups contained in the multifunctional thiol compound (T) react with the first vinyl monomer in the first step. As a result, the number of unreacted thiol groups remaining in the second step decreases, and the production rate of the target block copolymer decreases. The number of series of the polyfunctional thiol compound (T) may be 2 or 3, but the tertiary polyfunctional thiol compound (T) has a lower chain transferability to vinyl monomers than the secondary polyfunctional thiol compound (T), and the thiol group tends to be less reactive. Therefore, the number of series of the polyfunctional thiol compound (T) is preferably 2.

[0015] The polyfunctional thiol compound (T) is not particularly limited as long as it is secondary or higher, but is preferably a fatty acid polythiol compound, and from the viewpoint of suppressing decomposition of the linking group due to chain transfer, an aliphatic polythiol compound having no disulfide bond is more preferable, and an aliphatic polythiol compound having no sulfur atoms other than the thiol group is even more preferable.

[0016] The valence of the polyfunctional thiol compound (T), i.e., the average number of thiol groups per molecule, is preferably more than 1.5, more preferably 2 or more, and even more preferably 2.5 or more. If the valence of the polyfunctional thiol compound (T) is equal to or more than the above lower limit, the number of thiol groups remaining at the end of the first step increases, and the production ratio of the block copolymer produced at the end of the second step increases. The valence of the polyfunctional thiol compound (T) is preferably 1000 or less, more preferably 500 or less, and even more preferably 100 or less. If the valence of the polyfunctional thiol compound (T) is equal to or less than the upper limit, the number of polymer chains linked to the thiol group moiety at the end of the first step is reduced. As a result, the effect of steric hindrance by the polymer chains is reduced in the second step, and the production rate of the block copolymer is increased. The upper and lower limits of the valence of the polyfunctional thiol compound (T) can be combined in any combination. For example, the valence of the polyfunctional thiol compound (T) is preferably more than 1.5 and not more than 1000, more preferably 2 to 500, even more preferably 2 to 100, and particularly preferably 2.5 to 100.

[0017] The polyfunctional thiol compound (T) preferably has a structure represented by any one of the following general formulas (1) to (3).

[0018] [ka]

[0019] [ka]

[0020] [ka]

[0021] In general formula (1), R 1 is a monovalent hydrocarbon group, a hydroxyl group, or a monovalent electron-withdrawing group, and R 2 is an n1-valent organic group, where n1 is an integer from 1 to 6. In general formula (2), R 3 is a monovalent hydrocarbon group, a hydroxyl group, or a monovalent electron-withdrawing group, and R 4 is an n2-valent organic group, where n2 is an integer of 1 to 6. In general formula (3), R 5 is a monovalent hydrocarbon group, a hydroxyl group, or a monovalent electron-withdrawing group, and R 6 is a monovalent hydrocarbon group.

[0022] R 1 , R 3 , R 5 The monovalent hydrocarbon group in is not particularly limited, but is preferably a monovalent electron-donating group such as an alkyl group, more preferably an alkyl group having 6 or less carbon atoms, further preferably a methyl group or ethyl group, and particularly preferably a methyl group. R 1 , R 3 , R 5 The monovalent electron-withdrawing group in is not particularly limited, but is preferably an ester group, more preferably an ester group having an alkyl group having 6 or less carbon atoms, further preferably an ethyl ester group or methyl ester group, and particularly preferably a methyl ester group.

[0023] Each of n1 and n2 is an integer of 1 to 6, and preferably an integer of 2 to 6. R 2 is an n1-valent organic group, and R4 is an n2-valent organic group. R 2 and R 4 Examples of the organic group in include a monovalent hydrocarbon group, a divalent hydrocarbon group, a trivalent hydrocarbon group, a tetravalent hydrocarbon group, a pentavalent hydrocarbon group, a hexavalent hydrocarbon group, a group derived from a trivalent heterocyclic compound, etc. Among these, a divalent hydrocarbon group, a trivalent hydrocarbon group, a tetravalent hydrocarbon group, a pentavalent hydrocarbon group, a hexavalent hydrocarbon group, a group derived from a trivalent heterocyclic compound, etc. are preferred, and a divalent hydrocarbon group, a trivalent hydrocarbon group, a tetravalent hydrocarbon group, a hexavalent hydrocarbon group, a group derived from a trivalent heterocyclic compound, etc. are more preferred. R 2 , R 4 The hydrocarbon group in may contain an ether group, a thioether group, an amino group or a phenyl group.

[0024] R 2 , R 4 The divalent hydrocarbon group in is not particularly limited, but is preferably an alkylene group, more preferably an alkylene group having 1 to 6 carbon atoms, further preferably an ethylene group, n-propylene group, or n-butylene group, and particularly preferably an n-butylene group. R 2 , R 4 The trivalent hydrocarbon group in is not particularly limited, but is preferably a branched trivalent alkylene group, more preferably a branched trivalent alkylene group having 5 to 10 carbon atoms, and particularly preferably having 4 substituted carbons. R 2 , R 4 The tetravalent hydrocarbon group in is not particularly limited, but is preferably a branched tetravalent alkylene group, more preferably a branched tetravalent alkylene group having 5 to 10 carbon atoms, and particularly preferably having 4 substituted carbons. R 2 , R 4 The hexavalent hydrocarbon group in is not particularly limited, but is preferably a hexavalent hydrocarbon group containing an ether group, and more preferably -CH2-C(CH2)(CH2)-CH2-O-CH2-C(CH2)(CH2)-CH2-. R 2 , R4 The group derived from a trivalent heterocyclic compound in the above formula is a group obtained by removing three hydrogen atoms from a heterocyclic compound. The heterocyclic compound is not particularly limited, but preferably has a nitrogen atom, more preferably has a nitrogen atom and a carbon atom, and particularly preferably has a nitrogen atom and a carbonyl group.

[0025] R 6 The monovalent hydrocarbon group in is not particularly limited, but is preferably a branched monovalent alkylene group or a branched monovalent alkylene group, more preferably a branched monovalent alkylene group having 1 to 6 carbon atoms or a branched monovalent alkylene group having 1 to 6 carbon atoms, and particularly preferably a branched monovalent alkylene group having 1 to 6 carbon atoms. R 6 The monovalent hydrocarbon group in may contain an ether group, a thioether group, an amino group, a phenyl group or a hydroxyl group.

[0026] Specific examples of the polyfunctional thiol compound (T) include pentaerythritol tetrakis (3-mercaptobutyrate), 1,4-bis (3-mercaptobutyloxy) butane, 1,3,5-tris (3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6-trione, trimethylolpropane tris (3-mercaptobutyrate), dipentaerythritol hexakis (3-mercaptobutyrate), etc. Among these, pentaerythritol tetrakis (3-mercaptobutyrate) is preferred from the viewpoint of increasing the production ratio of block copolymers. These polyfunctional thiol compounds (T) may be used alone or in combination of two or more kinds.

[0027] The first vinyl monomer may be a vinyl monomer having no polar group, such as a (meth)acrylic acid ester or an aromatic vinyl compound; a vinyl monomer having a polar group, etc. Among these, a vinyl monomer having no polar group is preferred, a (meth)acrylic acid ester or an aromatic vinyl compound is more preferred, and a (meth)acrylic acid ester is even more preferred. These first vinyl monomers may be used alone or in combination of two or more. Examples of the polar group include a carboxylic acid group, an amino group, an amide group, a sulfonic acid group, and a phosphoric acid group.

[0028] Examples of the (meth)acrylic acid ester include linear or branched carbonized (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, i-pentyl (meth)acrylate, n-hexyl (meth)acrylate, heptyl (meth)acrylate, n-octyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. Alkyl (meth)acrylates having a hydrogen skeleton; alkyl (meth)acrylates having an alicyclic skeleton, such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecanyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, and dicyclopentanyl (meth)acrylate; (meth)acrylates having an aromatic ring introduced in the side chain, such as phenyl (meth)acrylate and benzyl (meth)acrylate; polyethylene glycol mono(meth)acrylate, polypropylene (Meth)acrylates having a polyethylene glycol group, such as polyethylene glycol mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, diethylene glycol monomethyl ether (meth)acrylate, diethylene glycol monoethyl ether (meth)acrylate, and polyethylene glycol methyl ether (meth)acrylate; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. hydroxyalkyl (meth)acrylates such as 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, etc.; (meth)acrylates having an oxyethylene group such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, ethoxyethyl (meth)acrylate, propoxymethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxymethyl (meth)acrylate, butoxyethyl (meth)acrylate, etc.Among these, alkyl(meth)acrylates having a linear or branched hydrocarbon skeleton are preferred, methyl(meth)acrylate and ethyl(meth)acrylate are more preferred, and methyl(meth)acrylate is even more preferred. These (meth)acrylic acid esters may be used alone or in combination of two or more kinds.

[0029] Examples of aromatic vinyl compounds include styrene, α-methylstyrene, divinylbenzene, vinyltoluene, p-styrenesulfonic acid, etc. Among these, styrene is preferred. These aromatic vinyl compounds may be used alone or in combination of two or more.

[0030] Examples of vinyl monomers having a polar group include vinyl monomers in which a polar group is directly linked to a vinyl group, such as (meth)acrylic acid, vinyl sulfonic acid, and vinyl phosphonic acid; vinyl monomers in which a polar group is connected to a side chain, such as dimethylaminoethyl (meth)acrylate; and vinyl monomers in which a polar group has been introduced onto an aromatic ring, such as vinylbenzenesulfonic acid. These vinyl monomers having a polar group may be used alone or in combination of two or more kinds.

[0031] The first vinyl monomer preferably contains at least a methacrylic acid ester. The ratio of the methacrylic acid ester in the first vinyl monomer is preferably 20 mol% or more, more preferably 30 mol% or more, even more preferably 50 mol% or more, and particularly preferably 70 mol% or more, based on the total moles of the first vinyl monomer. If the ratio of the methacrylic acid ester is equal to or more than the above lower limit, the polyfunctional thiol compound (T) and the first vinyl monomer react appropriately, and sufficient unreacted thiol groups remain at the stage where the first step is completed. Therefore, in the second step, the second vinyl monomer reacts with the remaining thiol groups, and the production ratio of the target block copolymer increases. The upper limit of the proportion of the methacrylic acid ester in the first vinyl monomer is preferably 100 mol % based on the total number of moles of the first vinyl monomer. The upper and lower limits of the ratio of the methacrylic acid ester in the first vinyl monomer can be combined in any combination. For example, the ratio of the methacrylic acid ester in the first vinyl monomer is preferably 20 to 100 mol%, more preferably 30 to 100 mol%, further preferably 50 to 100 mol%, and particularly preferably 70 to 100 mol%, based on the total number of moles of the first vinyl monomer.

[0032] The first vinyl monomer may further contain at least one of an acrylic acid ester and an aromatic vinyl compound in addition to the methacrylic acid ester. The total ratio of the acrylic acid ester and aromatic vinyl compound in the first vinyl monomer is preferably 80 mol% or less, more preferably 70 mol% or less, even more preferably 50 mol% or less, and particularly preferably 30 mol% or less, based on the total moles of the first vinyl monomer. If the total ratio of the acrylic acid ester and aromatic vinyl compound is equal to or less than the upper limit value, the polyfunctional thiol compound (T) and the first vinyl monomer react appropriately, and sufficient unreacted thiol groups remain at the stage where the first step is completed. Therefore, in the second step, the second vinyl monomer reacts with the remaining thiol groups, and the production ratio of the target block copolymer increases. The lower limit of the total proportion of the acrylic acid ester and the aromatic vinyl compound in the first vinyl monomer is 0 mol % based on the total number of moles of the first vinyl monomer. The upper and lower limits of the ratio of the acrylic acid ester and the aromatic vinyl compound in the first vinyl monomer can be arbitrarily combined. For example, the total ratio of the acrylic acid ester and the aromatic vinyl compound in the first vinyl monomer is preferably 0 to 80 mol%, more preferably 0 to 70 mol%, further preferably 0 to 50 mol%, and particularly preferably 0 to 30 mol%, based on the total number of moles of the first vinyl monomer.

[0033] The conversion rate of the first vinyl monomer is preferably 51% or more, more preferably 75% or more, and even more preferably 90% or more. When the conversion rate of the first vinyl monomer is equal to or more than the lower limit, the first vinyl monomer remaining in the first step and the second vinyl monomer used in the second step are less likely to mix, and more accurate block chains are more likely to be obtained. The upper limit of the conversion rate of the first vinyl monomer is 100%. The upper and lower limits of the conversion rate of the first vinyl monomer can be combined in any desired manner. For example, the conversion rate of the first vinyl monomer is preferably 51 to 100%, more preferably 75 to 100%, and even more preferably 90 to 100%. The conversion rate of the first vinyl monomer is determined as follows. At the end of the first step, the reaction solution is sampled and dissolved in deuterated chloroform for 1H-NMR measurement. The monomer conversion rate is calculated by comparing the integral values ​​of the monomer peak and the polymer peak from the NMR chart obtained.

[0034] <Second process> The second step is a step of radically polymerizing a second vinyl monomer in the presence of a polyfunctional thiol compound (T) and a polymer (P). The conditions for the radical polymerization in the second step will be described later.

[0035] The polyfunctional thiol compound (T) used in the second step is the same as the polyfunctional thiol compound (T) used in the first step, and the polyfunctional thiol compound (T) used in the first step may be used continuously in the second step.

[0036] The second vinyl monomer may be the same as the first vinyl monomer. Among these, vinyl monomers without polar groups are preferred, and (meth)acrylic acid esters and aromatic vinyl compounds are more preferred. Among (meth)acrylic acid esters, alkyl (meth)acrylates with linear or branched hydrocarbon skeletons, alkyl (meth)acrylates with alicyclic skeletons, (meth)acrylates with aromatic rings introduced into side chains, and (meth)acrylates with oxyethylene groups are preferred, and methyl (meth)acrylate, ethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate are more preferred, and methyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and methoxyethyl (meth)acrylate are even more preferred. Among the aromatic vinyl compounds, styrene is preferred. Furthermore, when the polymer obtained in the second step, ie, the target block copolymer, is a miktoarm star polymer, it is preferable that the second vinyl monomer is a vinyl monomer different from the first vinyl monomer. The second vinyl monomer may be used alone or in combination of two or more kinds.

[0037] The proportion of the aromatic vinyl compound in the second vinyl monomer is preferably 100 mol% or less, more preferably 80 mol% or less, even more preferably 70 mol% or less, and particularly preferably 50 mol% or less, based on the total moles of the second vinyl monomer. If the proportion of the aromatic vinyl compound is equal to or less than the upper limit, it is possible to prevent all of the thiol groups from reacting before the polymerization of the aromatic vinyl compound is completed, and it is possible to prevent the formation of a block copolymer that is not linked to a thiol group, thereby increasing the proportion of the block copolymer that is the target product. The lower limit of the aromatic vinyl compound in the second vinyl monomer is 0 mol % based on the total number of moles of the second vinyl monomer. The upper and lower limits of the proportion of the aromatic vinyl compound in the second vinyl monomer can be arbitrarily combined. For example, the proportion of the aromatic vinyl compound in the second vinyl monomer is preferably 0 to 100 mol%, more preferably 0 to 80 mol%, further preferably 0 to 70 mol%, and particularly preferably 0 to 50 mol%, based on the total number of moles of the second vinyl monomer.

[0038] The ratio of the (meth)acrylic acid ester in the second vinyl monomer is preferably 0 mol% or more, more preferably 20 mol% or more, even more preferably 30 mol% or more, and particularly preferably 50 mol% or more, based on the total number of moles of the second vinyl monomer. If the ratio of the (meth)acrylic acid ester is equal to or more than the above lower limit, it is possible to prevent all of the thiol groups from reacting before the polymerization of the aromatic vinyl compound is completed, and it is possible to prevent the formation of a block copolymer that is not linked to a thiol group, thereby increasing the production ratio of the target block copolymer. The upper limit of the (meth)acrylic acid ester in the second vinyl monomer is 100 mol % based on the total number of moles of the second vinyl monomer. The upper and lower limits of the proportion of the (meth)acrylic acid ester in the second vinyl monomer can be arbitrarily combined. For example, the proportion of the (meth)acrylic acid ester in the second vinyl monomer is preferably 0 to 100 mol%, more preferably 20 to 100 mol%, further preferably 30 to 100 mol%, and particularly preferably 50 to 100 mol%, based on the total number of moles of the second vinyl monomer.

[0039] The conversion rate of the second vinyl monomer is preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more. If the conversion rate of the second vinyl monomer is equal to or more than the lower limit, a block copolymer can be synthesized with a composition close to the charging ratio. The upper limit of the conversion rate of the second vinyl monomer is 100%. The upper and lower limits of the conversion rate of the second vinyl monomer can be combined in any desired manner. For example, the conversion rate of the second vinyl monomer is preferably 50 to 100%, more preferably 70 to 100%, and even more preferably 90 to 100%. The conversion rate of the second vinyl monomer is determined as follows. At the end of the second step, the reaction solution is sampled and dissolved in deuterated chloroform for 1H-NMR measurement. The monomer conversion rate is calculated by comparing the integral values ​​of the monomer peak and the polymer peak from the NMR chart obtained.

[0040] <Radical polymerization> The form of radical polymerization in the first and second steps is not particularly limited, but examples thereof include solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization.

[0041] In the first step, it is preferable to charge the first vinyl monomer all at once before polymerization. In the second step, it is preferable to charge the second vinyl monomer all at once before polymerization. By charging the first vinyl monomer and the second vinyl monomer at once, respectively, polymerization can be carried out by suspension polymerization, which is an industrially used polymerization method.

[0042] The amount of the polyfunctional thiol compound (T) used in the radical polymerization is preferably 0.2 to 100 parts by mass, more preferably 1 to 70 parts by mass, based on 100 parts by mass of the total of the first vinyl monomer and the second vinyl monomer. If the amount of the polyfunctional thiol compound (T) used is equal to or greater than the lower limit, unreacted thiol remains at the end of the first step, and the proportion of block copolymer produced in the second step increases. If the amount of the polyfunctional thiol compound (T) used is equal to or less than the upper limit, the molecular weight of the produced polymer is unlikely to be extremely low, and the resulting block copolymer can be prevented from acting as a plasticizer.

[0043] In the first and second steps, radical polymerization is carried out using a radical polymerization initiator and a polymerization solvent. Examples of the radical polymerization initiator used in the radical polymerization include peroxides such as dibenzoyl peroxide and tert-butyl permaleate; and azo compounds such as 2,2'-azobisisobutyronitrile and azobisisovaleronitrile. These radical polymerization initiators may be used alone or in combination of two or more.

[0044] The amount of radical polymerization initiator used in radical polymerization is preferably 0.0001 to 10 parts by mass, more preferably 0.001 to 1 part by mass, based on 100 parts by mass of the total of the first vinyl monomer and the second vinyl monomer. If the amount of radical polymerization initiator used is equal to or greater than the lower limit, the monomer conversion rate during polymerization is likely to increase. If the amount of radical polymerization initiator used is equal to or less than the upper limit, polymerization via the multifunctional thiol compound (T) is likely to occur, and the production rate of block copolymers is increased.

[0045] Examples of polymerization solvents used in radical polymerization include aromatic hydrocarbon solvents such as toluene, ethylbenzene, and xylene; aliphatic hydrocarbon solvents such as pentane, hexane, heptane, octane, and cyclohexane; ketone solvents such as acetone, methyl isobutyl ketone, and methyl ethyl ketone; ester solvents such as butyl acetate; and alcohol solvents such as methanol and ethanol. These polymerization solvents may be used alone or in combination of two or more.

[0046] The amount of the polymerization solvent used in the radical polymerization is preferably 50 to 500 parts by mass, more preferably 100 to 300 parts by mass, based on 100 parts by mass of the total of the first vinyl monomer and the second vinyl monomer. When the amount of the polymerization solvent used is equal to or more than the lower limit, abnormal polymerization due to heat generated by polymerization is unlikely to occur. When the amount of the polymerization solvent used is equal to or less than the upper limit, the monomer conversion rate is likely to increase.

[0047] The polymerization temperatures for the radical polymerization in the first and second steps can be appropriately set, but are preferably from −100 to 250° C., for example, as this is a suitable temperature range for using a radical polymerization initiator. The polymerization times for the radical polymerization in the first step and the second step can be appropriately set, and can be, for example, 0.5 to 48 hours.

[0048] <Block copolymer> The block copolymer obtained by the present invention is a polymeric compound containing a block chain in which a plurality of polymer chains are linked by a multifunctional thiol compound (T), and is also called a star polymer. In particular, when the first vinyl monomer and the second vinyl monomer are different types, or when at least one of the first vinyl monomer and the second vinyl monomer contains two or more types of vinyl monomers, a block copolymer in which different types of polymer chains are linked by a multifunctional thiol compound (T) is obtained, and such a block copolymer is also called a miktoarm star polymer.

[0049] The relative weight average molecular weight of the block copolymer (hereinafter referred to as "relative M w The relative M of the block copolymer is preferably 1000 or more, more preferably 2000 or more, and even more preferably 3000 or more. w When is equal to or larger than the above lower limit, the molecular weight is sufficiently large, and the block copolymer can be prevented from acting as a plasticizer. In addition, the relative M w is preferably 300,000 or less, more preferably 150,000 or less, and even more preferably 100,000 or less. w If is equal to or less than the upper limit, the polymer chain is reduced in molecular weight due to chain transfer of the polyfunctional thiol compound (T), and the production ratio of the block copolymer is increased. Relative M of block copolymers w The upper and lower limits can be arbitrarily combined. For example, the relative M wis preferably 1,000 to 300,000, more preferably 2,000 to 150,000, and even more preferably 3,000 to 100,000.

[0050] In addition, the relative M w is preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more. w When is equal to or larger than the above lower limit, the molecular weight is sufficiently large, and the target block copolymer can be prevented from acting as a plasticizer. In addition, the relative M w is preferably 100,000 or less, more preferably 50,000 or less, and even more preferably 25,000 or less. w When is equal to or less than the upper limit, steric hindrance is unlikely to become large when radical polymerization is carried out in the second step, and the unreacted thiol group and the second vinyl monomer are likely to react with each other, thereby increasing the production ratio of the block copolymer. Relative M of polymer chain of polymer (P) w The upper and lower limits can be arbitrarily combined. For example, the relative M w is preferably 500 to 100,000, more preferably 1,000 to 50,000, and further preferably 1,500 to 25,000.

[0051] Relative M of polymer chains of block copolymer obtained in the second step w is preferably 500 or more, more preferably 1000 or more, and even more preferably 1500 or more. w When is equal to or larger than the above lower limit, the molecular weight is sufficiently large, and the target block copolymer can be prevented from acting as a plasticizer. In addition, the relative M of the polymer chain of the block copolymer w is preferably 200,000 or less, more preferably 100,000 or less, and even more preferably 50,000 or less. wWhen the ratio is equal to or less than the upper limit, the amount of homopolymer formed by homopolymerization of the second vinyl monomer without the involvement of unreacted thiol groups can be reduced, and the proportion of block copolymer formed can be increased. Relative M of polymer chains in block copolymers w The upper and lower limits can be arbitrarily combined. For example, the relative M w is preferably 500 to 200,000, more preferably 1,000 to 100,000, and further preferably 1,500 to 50,000.

[0052] In addition, relative M w is a polymethyl methacrylate equivalent measured by gel permeation chromatography (GPC). w is the molecular weight calculated by the method described in the Examples below.

[0053] In addition, whether or not a block chain is formed can be confirmed by comparing the GPC chromatogram measurement charts, that is, by comparing the peak top molecular weight Mpa of the polymer chain of the polymer (P) obtained in the first step with the peak top molecular weight Mpb of the block copolymer obtained in the second step, it can be confirmed whether or not a block chain is formed.

[0054] When block chains are produced, the polymer produced in the second step is linked to the polymer (P) produced in the first step, so that the peak top molecular weight Mpa of the polymer chain of the polymer (P) produced in the first step shifts to the higher molecular weight side with the production of block chains, and the peak top molecular weight Mpb of the finally obtained block copolymer is obtained, resulting in a single-peak GPC chromatogram chart. On the other hand, when the production of block chains is small, the polymer chain of the polymer (P) produced in the first step remains even after the second step, so the peak top of the finally obtained block copolymer is obtained in a double-peak GPC chromatogram chart. In this way, when a GPC measurement of a block copolymer gives a single-peaked GPC chromatogram chart, it can be determined that block chains have been produced.

[0055] <Action and effect> As described above, according to the method for producing a block copolymer of the present embodiment, a secondary or higher polyfunctional thiol compound is used as a chain transfer agent, and radical polymerization of vinyl monomers is carried out in two stages to produce a block copolymer. The block copolymer thus obtained has a structure in which the polymer chains of each monomer composition are linked by the polyfunctional thiol group. In addition, there is no limitation on the vinyl monomer used, and for example, (meth)acrylic acid esters, aromatic vinyl compounds, and vinyl monomers containing polar groups can be used. Therefore, the method for producing a block copolymer of the present embodiment can be applied to various types of vinyl monomers, polymerization can be performed with various monomer compositions, and a block copolymer having a desired structure can be simply produced. EXAMPLES

[0056] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the examples described below, and various modifications are possible without departing from the gist of the present invention.

[0057] [Raw materials] The raw materials and their abbreviations used in the examples and comparative examples are shown below.

[0058] <Multifunctional thiol compounds (T)> ·MTPE-1: Pentaerythritol tetrakis(3-mercaptobutyrate) (manufactured by Resonac Co., Ltd.) PEMP: Pentaerythritol tetrakis(3-mercaptopropionate) (manufactured by SC Organic Chemicals Co., Ltd.) DPMP: Dipentaerythritol-3-mercaptopropionic acid ester (manufactured by SC Organic Chemical Co., Ltd.)

[0059] <Vinyl Monomer> MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name "Acrylic Ester M") ·MEA: Methoxyethyl acrylate ·BA: Butyl acrylate CHMA: Cyclohexyl methacrylate ·MAA: Methacrylic acid PhMA: Phenyl methacrylate Styrene: Styrene

[0060] <Polymerization initiator> AIBN: 2,2'-azobisisobutyronitrile

[0061] <Polymerization solvent> DMF: Dimethylformamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0062] [Measurement and evaluation methods] <Relative M w Measurements > Relative M of block copolymers w was measured by gel permeation chromatography (GPC) under the following measurement conditions: Equipment: HLC-8220 (Tosoh Corporation) Column: TSK GUARD COLUMN SUPER HH (4.6 x 35 mm, Tosoh Corporation) and two TSK-GEL SUPER HM-H (6.0 x 150 mm, Tosoh Corporation) connected in series Detector: Refractive index (RI) detector Column and detector temperature: 40℃ Eluent: Tetrahydrofuran ·Flow rate: 0.6mL / min Sample concentration: 2mg / mL (tetrahydrofuran solution) Standard substance: Polymethyl methacrylate (Polymer Laboratories; Mp (peak molecular weight) = 141,500, 55,600, 11,100, 1,590)

[0063] <Confirmation of block chain generation> The content of the block chain in the block copolymer was calculated by the following method. The solution of the polymer (P) obtained in the first step was reprecipitated using a poor solvent to recover the polymer (P). The recovered polymer (P) was subjected to GPC measurement, and the peak top molecular weight (Mpa) was calculated. Next, the solution of the block copolymer obtained in the second step was subjected to GPC measurement, and the peak top molecular weight Mpb was calculated. Next, Mpb / Mpa was calculated, and the degree of change in peak top molecular weight was determined. In addition, the obtained GPC chromatogram charts were compared to confirm whether the GPC chromatogram of the block copolymer obtained in the second step had a peak relatively shifted toward the high molecular weight side compared to the peak of the GPC chromatogram of the polymer (P) obtained in the first step, and whether it was monomodal. The polymer (P) obtained in the first step had a Mpb / Mpa value of 1.05 or more, and the peak was shifted relatively toward the higher molecular weight side compared to the peak in the GPC chromatogram of the polymer (P) obtained in the first step. The polymer (P) was determined to have produced a block chain when the peak was monomodal.

[0064] [Example 1] In a 50 mL Schlenk flask equipped with a stirrer and a nitrogen inlet tube, 35 parts by mass of methyl methacrylate (MMA) as the first vinyl monomer, 10 parts by mass of pentaerythritol tetrakis (3-mercaptobutyrate) (MTPE-1) as the multifunctional thiol compound (T) relative to 35 parts by mass of the first vinyl monomer, 0.3 mol% of 2,2'-azobisbutyronitrile (AIBN) as a radical polymerization initiator relative to the first vinyl monomer, and toluene were added as a polymerization solvent. The first vinyl monomer, the multifunctional thiol compound (T), the radical polymerization initiator, and the polymerization solvent were mixed in the Schlenk flask to prepare a mixed solution with a solid content (first vinyl monomer, multifunctional thiol compound (T), and radical polymerization initiator) concentration of 0.5% by mass. The prepared mixed solution was heated to 80°C while stirring under a nitrogen atmosphere. The mixed solution was heated and stirred for 5 hours to obtain a solution of polymer (P) (first step). The obtained solution of polymer (P) was subjected to GPC measurement. Note that, when reprecipitating the solution of polymer (P), a poor solvent shown in Table 1 was used.

[0065] Subsequently, 100 parts by mass of styrene as a second vinyl monomer and 0.5 mol% of 2,2'-azobisbutyronitrile (AIBN) as a radical polymerization initiator relative to the second vinyl monomer were added to the solution of the obtained polymer (P), and toluene was further added as a polymerization solvent. The second vinyl monomer, the radical polymerization initiator, and the polymerization solvent were mixed in the Schlenk flask to prepare a mixed solution with a solid content (second vinyl monomer and radical polymerization initiator) concentration of 0.5% by mass. The prepared mixed solution was heated to 80°C while stirring under a nitrogen atmosphere. The mixed solution was heated and stirred for 5 hours to obtain a solution of a block copolymer (second process). The obtained solution of the block copolymer was subjected to GPC measurement. The GPC measurement results (peak top molecular weight Mpa, peak top molecular weight Mpb, peak comparison in GPC chromatogram, peak shape in GPC chromatogram, and peak top shift rate) are shown in Table 1.

[0066] The conversion rate of the first vinyl monomer is shown in Table 1. The conversion rate was determined as follows. The reaction solution obtained in the first step was sampled and homogenized by adding deuterated chloroform. The reaction rate was then calculated by comparing the integral values ​​of the peaks specific to the monomer and the peaks specific to the polymer in proton NMR measurements. For example, in the case of polymerization of MMA, the NMR peaks were calculated using the following formula. Methyl group integral value of the methyl ester group of PMMA / (Methyl group integral value of the methyl ester part of MMA + Methyl group integral value of the methyl ester part of PMMA) × 100

[0067] [Example 2] In the first step, except that the amount of the polyfunctional thiol compound (T) was changed to 15 parts by mass relative to 35 parts by mass of the first vinyl monomer, a solution of a block copolymer was produced in the same manner as in Example 1, and a GPC measurement was carried out. The results are shown in Table 1.

[0068] [Example 3] A solution of a block copolymer was produced in the same manner as in Example 1, except that in the first step, the amount of the first vinyl monomer was changed to 70 parts by mass, and in the second step, the amount of the second vinyl monomer was changed to 50 parts by mass, and a GPC measurement was performed. The results are shown in Table 1.

[0069] [Example 4] In the first step, the amount of the first vinyl monomer was changed to 70 parts by mass, and the amount of the multifunctional thiol compound (T) was changed to 15 parts by mass relative to 70 parts by mass of the first vinyl monomer, and in the second step, the amount of the second vinyl monomer was changed to 50 parts by mass. Except for this, a solution of the block copolymer was produced in the same manner as in Example 1, and a GPC measurement was performed. The results are shown in Table 1.

[0070] [Example 5] In the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, and the amount of the multifunctional thiol compound (T) was changed to 8.12 parts by mass relative to 50 parts by mass of the first vinyl monomer, and in the second step, 50 parts by mass of butyl acrylate (BA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%. Except for this, a solution of a block copolymer was produced in the same manner as in Example 1, and a GPC measurement was performed. The results are shown in Table 2. The GPC chromatogram is also shown in FIG. 1.

[0071] [Example 6] In the first step, the amount of the first vinyl monomer was changed to 40 parts by mass, and the amount of the multifunctional thiol compound (T) was changed to 2.17 parts by mass relative to 40 parts by mass of the first vinyl monomer, and in the second step, 60 parts by mass of methoxyethyl acrylate (MEA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%. Except for this, a solution of the block copolymer was produced in the same manner as in Example 1, and GPC measurement was performed. The results are shown in Table 2.

[0072] [Example 7] A solution of a block copolymer was produced in the same manner as in Example 1, except that in the first step, 40 parts by mass of methyl methacrylate (MMA) and 10 parts by mass of methacrylic acid (MAA) were used as the first vinyl monomer, dimethylformamide (DMF) was used as the polymerization solvent, and in the second step, 50 parts by mass of methyl methacrylate (MMA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%, and the solution was subjected to GPC measurement. The results are shown in Table 2.

[0073] [Example 8] In the first step, the amount of the first vinyl monomer was changed to 40 parts by mass, and the amount of the multifunctional thiol compound (T) was changed to 2.17 parts by mass relative to 40 parts by mass of the first vinyl monomer, and in the second step, 50 parts by mass of cyclohexyl methacrylate (CHMA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%. Except for this, a solution of a block copolymer was produced in the same manner as in Example 1, and a GPC measurement was performed. The results are shown in Table 2.

[0074] [Example 9] A solution of a block copolymer was produced in the same manner as in Example 1, except that in the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, in the second step, 50 parts by mass of phenyl methacrylate (PhMA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%, and a GPC measurement was performed. The results are shown in Table 2.

[0075] [Comparative Example 1] In the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, and 7.33 parts by mass of pentaerythritol tetrakis (3-mercaptopropionate) (PEMP) was used as the polyfunctional thiol compound (T) relative to 50 parts by mass of the first vinyl monomer, and in the second step, 50 parts by mass of butyl acrylate (BA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%. Except for this, a solution of a block copolymer was produced in the same manner as in Example 1, and GPC measurement was performed. The results are shown in Table 3. The GPC chromatogram is also shown in FIG. 2.

[0076] [Comparative Example 2] In the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, and 5.33 parts by mass of dipentaerythritol-3-mercaptopropionate (DPMP) was used as the polyfunctional thiol compound (T) relative to 50 parts by mass of the first vinyl monomer, and in the second step, 64 parts by mass of butyl acrylate (BA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%. Except for this, a solution of a block copolymer was produced in the same manner as in Example 1, and a GPC measurement was performed. The results are shown in Table 3.

[0077] [Comparative Example 3] In the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, and 2.67 parts by mass of dipentaerythritol-3-mercaptopropionate (DPMP) was used as the polyfunctional thiol compound (T) relative to 50 parts by mass of the first vinyl monomer, and in the second step, 64 parts by mass of butyl acrylate (BA) was used as the second vinyl monomer, and the amount of the radical polymerization initiator was changed to 0.3 mol%, except that a solution of a block copolymer was produced in the same manner as in Example 1 and GPC measurement was performed. The results are shown in Table 3.

[0078] [Reference example A] In the first step, the amount of the first vinyl monomer was changed to 50 parts by mass, and 7.33 parts by mass of pentaerythritol tetrakis(3-mercaptopropionate) (PEMP) was used as the polyfunctional thiol compound (T) relative to 50 parts by mass of the first vinyl monomer, except that the first step was carried out in the same manner as in Example 1. However, when the conversion rate of methyl methacrylate (MMA) reached 66%, the Schlenk flask was removed from the oil bath and returned to room temperature, and then reprecipitation was carried out. The second step was carried out in the same manner as in Example 1, except that 64 parts by mass of butyl acrylate (BA) was added as a second vinyl monomer to the obtained reprecipitated polymer and the amount of the radical polymerization initiator was changed to 0.3 mol %, to produce a block copolymer solution, which was then subjected to GPC measurement. The results are shown in Table 3.

[0079] [Table 1]

[0080] [Table 2]

[0081] [Table 3]

[0082] The following can be said from the above-mentioned Examples and Comparative Examples. As shown in each example, by using a secondary multifunctional thiol compound (T) and performing two-stage radical polymerization, the peak of the GPC chromatogram generated in the first stage was shifted to the high molecular weight side and became a single-peak, as shown in FIG. 1. On the other hand, when two-stage radical polymerization was carried out using a primary polyfunctional thiol compound (T), as shown in Figure 2, the polymer peak generated in the first stage did not shift to the high molecular weight side, resulting in a bimodal peak. In addition, although the results of Reference Example A were comparable to those of the other Examples, it was time-consuming because reprecipitation was required between the first and second steps. In addition, since the second vinyl monomer was added at a stage where the conversion rate of the vinyl monomer was low to carry out polymerization, the structure and composition of the block copolymer that could be synthesized are likely to be limited. From the above, it has been demonstrated that the present invention makes it possible to efficiently and simply produce a block copolymer, which is a polymer compound containing block chains.

Claims

1. A first step of radically polymerizing a first vinyl monomer in the presence of a secondary or higher polyfunctional thiol compound to obtain a polymer; and a second step of radically polymerizing a second vinyl monomer in the presence of the secondary or higher polyfunctional thiol compound and the polymer obtained in the first step.

2. The method for producing a block copolymer according to claim 1, wherein the secondary or higher functional thiol compound has a valence of 2 to 100.

3. The method for producing a block copolymer according to claim 1 , wherein the first vinyl monomer comprises at least one selected from the group consisting of a (meth)acrylic acid ester and an aromatic vinyl compound.

4. The method for producing a block copolymer according to claim 1 , wherein the conversion rate of the first vinyl monomer is 51% or more.

5. The method for producing a block copolymer according to claim 1, wherein the second vinyl monomer comprises at least one selected from the group consisting of a (meth)acrylic acid ester and an aromatic vinyl compound, and is a vinyl monomer different from the first vinyl monomer.

6. 2. The method for producing a block copolymer according to claim 1, wherein the first vinyl monomer is charged all at once before being polymerized in the first step, and the second vinyl monomer is charged all at once before being polymerized in the second step.

Citation Information

Patent Citations

  • Acrylic block polymer and its use and production method

    JP2001139646A

  • Photosensitive resin composition for sandblasting, and phtosensitive film for sandblasting using the composition

    JP2004126073A

  • Impact resistance improver, thermoplastic resin composition and film

    JP2018012820A

  • Photo-curable composition and molded article

    WO2014148148A1

  • Adhesive polymer and medical adhesive patch

    WO2017057693A1