Optical component

A copolymer with controlled fluorine content and cyclic structures addresses the trade-offs in optical components, providing enhanced heat resistance, scratch resistance, and high Abbe numbers for improved optical performance in imaging devices and smartphones.

JP2024137025AInactive Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048373
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing optical components with high Abbe numbers suffer from trade-offs between heat resistance and scratch resistance, limiting their performance in high-temperature environments and durability.

Method used

The use of a copolymer containing structural units derived from monomers with different cyclic structures, specifically monomers represented by general formulas (A) and (B), with controlled fluorine content and molar ratios, to enhance heat resistance and scratch resistance while maintaining high Abbe numbers.

Benefits of technology

The copolymer achieves an improved balance of high Abbe number, heat resistance, and scratch resistance, suitable for optical components in imaging devices and smartphones, reducing chromatic aberrations and enhancing durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137025000001
    Figure 2024137025000001
  • Figure 2024137025000002
    Figure 2024137025000002
  • Figure 2024137025000003
    Figure 2024137025000003
Patent Text Reader

Abstract

To provide an optical component with a higher Abbe number and an improved performance balance of the resistance to heat and the resistance to scratching.SOLUTION: The present invention relates to an optical component having at least two optical lenses. The outermost optical lens of the optical component includes a copolymer (Z) having a constituent unit (x) derived from a monomer (X) having at least three cyclic structures and four cyclic structures at most and a constituent unit (y) derived from a monomer (Y) having at least six cyclic structures and seven cyclic structures at most. The content of fluorine atoms measured by 19F-NMR in the copolymer (Z) is from 20 mass% to 70 mass% when the total of the copolymer (Z) is 100 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical component. [Background technology]

[0002] In various optical components (lenses), lens materials with high Abbe numbers are required to achieve clearer image quality and to reduce size. High Abbe number lens materials have small chromatic aberration, so they can be used in the outermost layer of a combined lens to reduce color shift. As a technique relating to a high Abbe number, for example, the technique described in Patent Document 1 can be mentioned.

[0003] Patent Document 1 describes an optical component material that has a refractive index of 1.48 or less for D-line wavelength light and contains a fluorine-containing cyclic olefin polymer having at least a repeating structural unit represented by general formula (1). The fluorine-containing cyclic olefin polymer is soluble in organic solvents that do not contain fluorine atoms, has high surface polarity, and has a small water contact angle, so that it can be suitably used as an antireflection film, and also describes that the Abbe number is 60 or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-177046 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention provides an optical component having an improved balance of performance including a high Abbe number, heat resistance, and scratch resistance. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems, and have found that an optical component having an improved Abbe number, heat resistance, and scratch resistance can be obtained by including a copolymer in which the lens of the outermost layer of the optical component includes structural units derived from two types of monomers having different cyclic structures, and the content of fluorine atoms in the copolymer is within a predetermined range, and thus the present invention has been completed. The present inventors also discovered that an optical component having an outermost optical lens containing a copolymer (Z) including a structural unit derived from a compound represented by general formula (A) and a structural unit derived from a compound represented by general formula (B) can be obtained, thereby obtaining an optical component having an improved Abbe number, heat resistance, and scratch resistance, and thus completing the present invention. According to the present invention, there is provided the following optical component.

[0007] [1] An optical component having two or more optical lenses, the optical lens of the outermost layer in the optical component comprises a copolymer (Z) including a structural unit (x) derived from a monomer (X) having a cyclic structure with 3 to 4 rings and a structural unit (y) derived from a monomer (Y) having a cyclic structure with 6 to 7 rings, In the copolymer (Z), 19 The optical component has a fluorine atom content, as measured by F-NMR, of 20% by mass or more and 70% by mass or less, when the entire copolymer (Z) is taken as 100% by mass. [2] The monomer (X) contains a compound represented by the following general formula (A): The optical component according to [1], wherein the monomer (Y) contains a compound represented by the following general formula (B): [ka] (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group,1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [ka] (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure. [3] In the general formula (A), R 1 ~R 4 at least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms; In the general formula (B), R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms. [4] the number of cyclic structures / total number of carbon atoms in the monomer (X) is 0.20 or more and 0.45 or less, The optical component according to any one of [1] to [3], wherein the number of cyclic structures / the total number of carbon atoms in the monomer (Y) is 0.30 or more and 0.50 or less. [5] The optical component according to any one of [1] to [4], wherein in the copolymer (Z), a molar ratio (x / y) of the structural unit (x) derived from the monomer (X) to the structural unit (y) derived from the monomer (Y) is 0.25 or more and 4.0 or less. [6] The optical component according to any one of [1] to [5], wherein the total content of the structural unit (x) and the structural unit (y) in the copolymer (Z) is 50% by mass or more and 100% by mass or less, when the entire copolymer (Z) is taken as 100% by mass. [7] An optical component having two or more optical lenses, The optical lens of the outermost layer of the optical component is A structural unit derived from a compound represented by the following general formula (A), An optical component comprising a copolymer (Z) containing a structural unit derived from a compound represented by the following general formula (B): [ka] (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [ka] (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure. [8] The optical component according to [7], wherein in the copolymer (Z), a molar ratio (x' / y') of the structural unit (x') derived from the compound represented by general formula (A) to the structural unit (y') derived from the compound represented by general formula (B) is 0.25 or more and 4.0 or less. [9] The optical component according to [7] or [8], wherein the total content of the structural unit (x') derived from the compound represented by general formula (A) and the structural unit (y') derived from the compound represented by general formula (B) in the copolymer (Z) is 50% by mass or more and 100% by mass or less, when the entire copolymer (Z) is 100% by mass.

[10] The optical component according to any one of [1] to [9], wherein the weight average molecular weight (Mw) of the copolymer (Z) in terms of polystyrene measured by gel permeation chromatography (GPC) is 500 or more and 1,000,000 or less.

[11] The optical component according to any one of [1] to

[10] , wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) and the number average molecular weight (Mn) of the copolymer (Z) in terms of polystyrene, as measured by gel permeation chromatography (GPC), is 1.0 or more and 5.0 or less.

[12] The optical component according to any one of [1] to

[11] , wherein the outermost optical lens has an Abbe number vd of 60 or more and 120 or less, as measured in accordance with ASTM D542.

[13] The optical component according to any one of [1] to

[12] , wherein the copolymer (Z) has a glass transition temperature of 120° C. or higher.

[14] The optical component according to any one of [1] to

[13] , wherein the refractive index nd of the outermost optical lens for d-line wavelength light measured in accordance with ASTM D542 is 1.30 or more and 1.48 or less.

[15] The optical component according to any one of [1] to

[14] , wherein the pencil hardness of the outermost optical lens is in the range of B to 2H as defined by ISO 15184.

[16] The optical component according to any one of [1] to

[15] , wherein the thickness of the outermost optical lens is 0.5 mm or more and 15 mm or less. Effect of the Invention

[0008] According to the present invention, it is possible to provide an optical component having an improved balance of performance including a high Abbe number, heat resistance, and scratch resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the present invention will be described based on the embodiment. In this embodiment, "A to B" indicating a numerical range means A or more and B or less unless otherwise specified. In addition, when a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily.

[0010] 1.Optical components The optical component of the present embodiment has two or more optical lenses, and the outermost optical lens contains a copolymer (Z) including a structural unit (x) derived from a monomer (X) having a cyclic structure with 3 to 4 rings and a structural unit (y) derived from a monomer (Y) having a cyclic structure with 6 to 7 rings, and in the copolymer (Z), 19 The content of fluorine atoms measured by F-NMR is from 20% by mass to 70% by mass, when the entire copolymer (Z) is taken as 100% by mass. Alternatively, the optical component of the present embodiment has two or more optical lenses, and the outermost optical lens contains a copolymer (Z) that includes a structural unit derived from a compound represented by general formula (A) and a structural unit derived from a compound represented by general formula (B).

[0011] For example, in the optical components (lenses) of imaging devices installed in automobiles and in the optical components (lenses) of smartphone cameras, lens materials with high Abbe numbers are required to achieve clearer image quality and to reduce size. Since high Abbe number lens materials have small chromatic aberration, they can be used in the outermost layer of a combination lens to reduce color shift. In addition to having a large Abbe number, high Abbe number lens materials are sometimes required to be heat-resistant and scratch-resistant to withstand high temperature environments because they are used in the outermost layer. In recent years, optical lenses for imaging devices and smartphone cameras have been using, for example, resin lenses using amorphous polymers. In resin lenses using amorphous polymers, it is considered to be designed to introduce fluorine atoms in order to improve the Abbe number. However, according to the investigations of the present inventors, it has become clear that the introduction of fluorine atoms reduces the heat resistance of the resin and also softens the resin, which may make the lens more susceptible to scratches.

[0012] According to the research of the present inventors, it has been found that by making the lens of the outermost layer of an optical component contain a copolymer containing structural units derived from two types of monomers having different cyclic structures and setting the content of fluorine atoms in the copolymer within a predetermined range, it is possible to obtain an optical component having an improved Abbe number while also improving heat resistance and scratch resistance. Although the reason for this is unclear, the copolymer can improve heat resistance by containing structural units derived from two different monomers with cyclic structures. It is also believed that the trade-off between high Abbe number and heat resistance and scratch resistance of the lens can be improved by the monomers with cyclic structures containing fluorine and the fluorine content in the copolymer being within an appropriate range.

[0013] Furthermore, according to the investigations of the present inventors, it has been found that when the outermost lens of an optical component contains a copolymer (Z) containing a structural unit derived from a compound represented by general formula (A) and a structural unit derived from a compound represented by general formula (B), an optical component can be obtained that has an improved Abbe number, heat resistance, and scratch resistance. The reason for this is unclear, but it is believed that the compound represented by general formula (A) has a high fluorine content and can improve the Abbe number, while the compound represented by general formula (B) has a large number of rings and a rigid structure, which limits the movement of the copolymer chain when heat is applied, thereby improving heat resistance and scratch resistance. Therefore, it is believed that the copolymer contains a structural unit derived from the compound represented by general formula (A) and a structural unit derived from the compound represented by general formula (B), thereby improving the trade-off between a high Abbe number and heat resistance and scratch resistance of the lens.

[0014] From the viewpoint of improving heat resistance, the monomer (X) has a cyclic structure having 3 to 4 rings, and preferably has a cyclic structure having 3 rings. From the viewpoint of improving heat resistance, the monomer (Y) has a cyclic structure having 6 to 7 rings, and preferably has a cyclic structure having 6 rings. The number of cyclic structures refers to the total number of cyclic structures contained in the compound, including the cyclic structure with the maximum number of ring members that does not pass through a bridging portion and passes through a condensed ring portion, and the cyclic structure with the minimum number of ring members that passes through a bridging portion. For example, 5,6-difluoro-5-fluoro-6-(trifluoromethyl)bicyclo(2.2.1)hept-2-ene has three cyclic structures, and 8,8,9-trifluoro-9-trifluoromethyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-Dodecene has a cyclic structure with six rings.

[0015] Copolymer (Z) in this embodiment contains monomer (X) and monomer (Y) having different cyclic structures and fluorine contents, and thereby the performance balance of high Abbe number, heat resistance, and scratch resistance of the outermost lens layer containing copolymer (Z) can be improved. The reason for this is unclear, but the inclusion of monomer (X) having a high fluorine content improves the Abbe number, while the inclusion of monomer (Y) having a large number of cyclic structures and a rigid structure improves the heat resistance and scratch resistance.

[0016] From the viewpoints of improving heat resistance, setting the fluorine content in the copolymer (Z) in an appropriate range, and improving the Abbe number, the monomer (X) preferably contains a compound represented by the following general formula (A).

[0017] [ka]

[0018] In formula (A), preferably, R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure.

[0019] In formula (A), R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 1 ~R 4 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 1 ~R4 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 4 is a trifluoromethyl group, and R 1 ~R 3 is fluorine. This allows the fluorine content in the copolymer (Z) to fall within an appropriate range, and in turn allows the performance balance of a high Abbe number, heat resistance, and scratch resistance to be further improved.

[0020] From the viewpoint of improving the heat resistance and scratch resistance in the copolymer (Z), the monomer (Y) preferably contains a compound represented by the following general formula (B).

[0021] [ka]

[0022] In formula (B), preferably, R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

[0023] In formula (B), R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 5 ~R 8 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 5 ~R 8 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 8 is a trifluoromethyl group, and R 5 ~R 7 is fluorine. This allows the fluorine content in the copolymer (Z) to fall within an appropriate range, and in turn allows the performance balance of a high Abbe number, heat resistance, and scratch resistance to be further improved.

[0024] The ratio of the number of cyclic structures to the total number of carbon atoms in the monomer (X) (number of cyclic structures / total number of carbon atoms) is preferably 0.20 or more, more preferably 0.25 or more, and even more preferably 0.30 or more, from the viewpoint of improving the bulkiness of the polymer and thereby further improving the heat resistance, and is preferably 0.45 or less, more preferably 0.40 or less, from the viewpoint of easy availability of the monomer. The ratio of the number of cyclic structures to the total number of carbon atoms in the monomer (Y) (number of cyclic structures / total number of carbon atoms) is preferably 0.30 or more, more preferably 0.35 or more, preferably 0.40 or more, and even more preferably 0.45 or more, from the viewpoint of improving the bulkiness of the polymer and thereby further improving the heat resistance, and is preferably 0.50 or less, more preferably 0.48 or less, from the viewpoint of easy availability of the monomer.

[0025] In the copolymer (Z), the molar ratio (x / y) of the structural unit (x) derived from the monomer (X) to the structural unit (y) derived from the monomer (Y) is preferably 0.25 or more, more preferably 0.30 or more, even more preferably 0.40 or more, even more preferably 0.50 or more, even more preferably 0.60 or more, and preferably 4.0 or less, more preferably 3.5 or less, even more preferably 3.0 or less, even more preferably 2.5 or less, even more preferably 2.0 or less, even more preferably 1.5 or less, even more preferably 1.0 or less. In the copolymer (Z), the molar ratio (x / y) of the structural unit (x) derived from the monomer (X) to the structural unit (y) derived from the monomer (Y) is preferably 0.25 or more and 4.0 or less, more preferably 0.40 or more and 3.5 or less, even more preferably 0.50 or more and 3.0 or less, even more preferably 0.50 or more and 2.5 or less. This makes it possible to further improve the balance of performance among high Abbe number, heat resistance, and scratch resistance. The molar ratio (x / y) of the structural unit (x) derived from the monomer (X) to the structural unit (y) derived from the monomer (Y) is 19 It is measured by F-NMR.

[0026] Copolymer (Z) 19 The fluorine content as measured by F-NMR, when the entire copolymer (Z) is taken as 100 mass%, from the viewpoint of improving the Abbe number, is 20 mass% or more, preferably 25 mass% or more, more preferably 30 mass% or more, even more preferably 35 mass% or more, and even more preferably 40 mass% or more, and from the viewpoints of improving the strength of the obtained lens, reducing its susceptibility to scratches, increasing the glass transition temperature, and improving moldability, is 70 mass% or less, more preferably 65 mass% or less, even more preferably 60 mass% or less, even more preferably 55 mass% or less, and even more preferably 50 mass% or less. The fluorine content of the copolymer (Z) is 19 It is measured using the mole fractions [A] and [B] of monomer (X) and monomer (Y) measured by F-NMR.

[0027] From the viewpoint of further improving the performance balance of high Abbe number, heat resistance, and scratch resistance, the total content of the structural unit (x) derived from monomer (X) and the structural unit (y) derived from monomer (Y) in copolymer (Z) is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and is, for example, 100% by mass or less, when the entire copolymer (Z) is taken as 100% by mass.

[0028] The copolymer (Z) may contain structural units derived from compounds other than the monomers (X) and (Y) as long as the effects of the present invention are not impaired. When copolymer (Z) contains structural units derived from other compounds, the content of the structural units derived from other compounds, when the entire copolymer (Z) is taken as 100 mass%, from the viewpoint of further improving the performance balance of high Abbe number, heat resistance, and scratch resistance, is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, even more preferably 20 mass% or less, and even more preferably 10 mass% or less, and may be, for example, 0 mass% or more, 1 mass% or more, or 5 mass% or more.

[0029] Copolymer (Z) in the optical lens of the outermost layer in the optical component of this embodiment contains a constitutional unit derived from a compound represented by the following general formula (A) from the viewpoints of setting the fluorine content in copolymer (Z) within an appropriate range and improving the Abbe number.

[0030] [ka]

[0031] In formula (A), preferably, R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure.

[0032] In formula (A), R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 1 ~R 4 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 1 ~R 4 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 4 is a trifluoromethyl group, and R 1 ~R 3 is fluorine. This allows the fluorine content in the copolymer (Z) to fall within an appropriate range, and in turn allows the performance balance of a high Abbe number, heat resistance, and scratch resistance to be further improved.

[0033] Copolymer (Z) in the outermost optical lens in the optical component of this embodiment contains a constitutional unit derived from a compound represented by the following general formula (B) from the viewpoint of improving the heat resistance and scratch resistance of copolymer (Z).

[0034] [ka]

[0035] In formula (B), preferably, R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

[0036] In formula (B), R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 5 ~R 8 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 5 ~R 8 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 8 is a trifluoromethyl group, and R 5 ~R 7is fluorine. This allows the fluorine content in the copolymer (Z) to fall within an appropriate range, and in turn allows the performance balance of a high Abbe number, heat resistance, and scratch resistance to be further improved.

[0037] In the copolymer (Z), the molar ratio (x' / y') of the structural unit (x') derived from the compound represented by the general formula (A) to the structural unit (y') derived from the compound represented by the general formula (B) is preferably 0.25 or more, more preferably 0.30 or more, even more preferably 0.40 or more, even more preferably 0.50 or more, even more preferably 0.60 or more, and preferably 4.0 or less, more preferably 3.5 or less, even more preferably 3.0 or less, even more preferably 2.5 or less, even more preferably 2.0 or less, even more preferably 1.5 or less, even more preferably 1.0 or less. In the copolymer (Z), the molar ratio (x' / y') of the structural unit (x') derived from the compound represented by the general formula (A) to the structural unit (y') derived from the compound represented by the general formula (B) is preferably 0.25 or more and 4.0 or less, more preferably 0.40 or more and 3.5 or less, even more preferably 0.50 or more and 3.0 or less, even more preferably 0.50 or more and 2.5 or less. This makes it possible to further improve the balance of performance among high Abbe number, heat resistance, and scratch resistance. The molar ratio (x' / y') of the structural unit (x') derived from the compound represented by general formula (A) to the structural unit (y') derived from the compound represented by general formula (B) is 19 It is measured by F-NMR.

[0038] From the viewpoint of further improving the performance balance of high Abbe number, heat resistance, and scratch resistance, the total content of the structural unit (x') derived from the compound represented by general formula (A) and the structural unit (y') derived from the compound represented by general formula (B) in copolymer (Z) is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and for example, 100% by mass or less, when the entire copolymer (Z) is taken as 100% by mass.

[0039] The weight average molecular weight (Mw) of the copolymer (Z) in terms of polystyrene as measured by gel permeation chromatography (GPC) is preferably 500 or more, more preferably 1,000 or more, even more preferably 10,000 or more, even more preferably 50,000 or more, even more preferably 80,000 or more, and even more preferably 100,000 or more, from the viewpoint of further expressing the physical properties as a polymer and improving the performance balance of high Abbe number, heat resistance, and scratch resistance, and is preferably 1,000,000 or less, more preferably 500,000 or less, even more preferably 300,000 or less, and even more preferably 150,000 or less, from the viewpoint of further maintaining fluidity during thin film formation or injection molding.

[0040] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the copolymer (Z) in terms of polystyrene, measured by gel permeation chromatography (GPC), is, for example, 1.0 or more, and from the viewpoint of obtaining thin film formability with a uniform thickness and good injection moldability, is preferably 1.4 or more, more preferably 1.5 or more, even more preferably 2.0 or more, even more preferably 2.5 or more, and even more preferably 3.0 or more, and is, for example, 5.0 or less, preferably 4.5 or less, and more preferably 4.0 or less.

[0041] The Abbe number vd of the outermost optical lens measured according to ASTM D542 is preferably 60 or more, more preferably 63 or more, even more preferably 65 or more, even more preferably 68 or more, and even more preferably 70 or more, from the viewpoint of further reducing the chromatic aberration of the obtained optical component, and is preferably 120 or less, more preferably 110 or less, even more preferably 100 or less, and even more preferably 85 or less, from the viewpoint of further improving the refractive index. The Abbe number vd of the outermost optical lens measured according to ASTM D542 is preferably 60 or more and 120 or less, more preferably 63 or more and 110 or less, even more preferably 65 or more and 100 or less, and even more preferably 70 or more and 85 or less, from the viewpoint of further reducing the chromatic aberration of the obtained optical component. If the Abbe number of the outermost optical lens is 60 or more, it is possible to obtain the required chromatic aberration correction effect, for example, when used in combination with a high refractive index lens.

[0042] The Abbe number vd is a value expressed by the following formula (2) in accordance with ASTM D542, and indicates the degree of change in refractive index in the visible light region. Abbe number (νd) = (nd-1) / (nf-nc) (2) Here, in formula (2), nd represents the d-line refractive index (wavelength 587.6 nm), nf represents the F-line refractive index (wavelength 486.1 nm), and nc represents the C-line refractive index (wavelength 656.3 nm). Therefore, a substance with a high Abbe number indicates that it has a small change in refractive index and a high degree of linearity in the visible light region.

[0043] The glass transition temperature of the copolymer (Z) is preferably 120° C. or higher, more preferably 125° C. or higher, even more preferably 130° C. or higher, even more preferably 135° C. or higher, and even more preferably 140° C. or higher, from the viewpoint of improving the moldability, it is preferably 170° C. or lower, more preferably 165° C. or lower, and even more preferably 160° C. or lower. The glass transition temperature of the copolymer (Z) is preferably 120° C. or higher and 170° C. or lower, more preferably 125° C. or higher and 170° C. or lower, even more preferably 130° C. or higher and 165° C. or lower, even more preferably 135° C. or higher and 165° C. or lower, and even more preferably 140° C. or higher and 160° C. or lower, from the viewpoint of improving the heat resistance.

[0044] In order to obtain an optical lens with an improved performance balance of the Abbe number, glass transition temperature, refractive index, and scratch resistance, for example, as described below, it is important to adjust the purification conditions of the monomer (X) solution and the monomer (Y) solution before the polymerization of the monomer (X) and the monomer (Y) to reduce the content of the by-product fluorine-free cyclic diolefin compound. By reducing the content of the fluorine-free cyclic diolefin compound contained in the monomer (X) solution and the monomer (Y) solution, the polymerization and hydrogenation of the monomer (X) and the monomer (Y) can be performed while suppressing gelation, so that the polymerization unevenness and composition unevenness of the obtained copolymer (Z) can be suppressed, and as a result, a lens with an improved performance balance of the Abbe number, glass transition temperature, refractive index, and scratch resistance can be obtained.

[0045] The optical component of the present embodiment is an optical component having two or more optical lenses. The number of optical lenses is preferably three or more, more preferably four or more, and is preferably nine or less, more preferably eight or less. The outermost optical lens of the optical component contains the copolymer (Z) of this embodiment. When the copolymer (Z) of this embodiment is used as an optical lens, it has an excellent balance of performance such as a high Abbe number, heat resistance, and scratch resistance, and therefore can be suitably used for optical components. In this embodiment, the outermost layer refers to, for example, the side of an imaging lens opposite to the side of a person observing, that is, the outermost layer on the object side. The outermost optical lens has another lens on the inside.

[0046] The refractive index nd of the outermost optical lens to d-line wavelength light, measured in accordance with ASTM D542, is preferably 1.30 or more, more preferably 1.35 or more, and preferably 1.48 or less, more preferably 1.45 or less. By having the refractive index nd to d-line wavelength light within the above range, light shows excellent linearity within this refractive index range.

[0047] The optical lens of the outermost layer has a light transmittance in the visible light region, measured in accordance with JIS K 7361-1: 1997, of preferably 80% or more, more preferably 85% or more, and preferably 100% or less. When the light transmittance in the visible light region is 80% or more, it is preferable that the image does not appear blurred even when the film is applied as an anti-reflection film to the surface of a CRT or liquid crystal display.

[0048] The pencil hardness of the outermost layer of the optical lens, as defined by ISO 15184, is preferably B or more, more preferably HB or more, and is preferably 2H or less, more preferably H or less, from the viewpoint of further reducing the susceptibility of the lens to scratches.

[0049] The thickness of the outermost optical lens is preferably 0.5 mm or more, more preferably 0.8 mm or more, even more preferably 1 mm or more, even more preferably 3 mm or more, and is preferably 15 mm or less, more preferably 10 mm or less, even more preferably 8 mm or less, even more preferably 5 mm or less. The thickness of the outermost optical lens is preferably 0.5 mm or more and 15 mm or less, more preferably 0.8 mm or more and 10 mm or less, even more preferably 1 mm or more and 8 mm or less, even more preferably 3 mm or more and 5 mm or less.

[0050] The content of copolymer (Z) in the outermost optical lens of this embodiment, when the entire outermost optical lens of this embodiment is taken as 100 mass%, from the viewpoint of further improving the balance of performance of optical properties such as high Abbe number, heat resistance, scratch resistance, transparency and refractive index, is preferably 60 mass% or more, more preferably 70 mass% or more, even more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, even more preferably 98 mass% or more, and preferably 100 mass% or less.

[0051] Furthermore, the outermost optical lens of this embodiment may contain components other than the copolymer (Z) as long as the effects of the present invention are not impaired. Examples of other components include resins other than the copolymer (Z) and known additives. Examples of the other resin include at least one resin selected from the group consisting of amorphous transparent resins such as polycarbonate, acrylic resin, amorphous polyarylate, and alicyclic hydrocarbon resin. Examples of the additives include ultraviolet absorbers, antioxidants, flame retardants, antistatic agents, colorants, secondary antioxidants, lubricants, release agents, anti-fogging agents, weather resistance stabilizers, light resistance stabilizers, and metal deactivators.

[0052] In the optical component of this embodiment, the lens provided on the inside of the outermost optical lens preferably includes one or more lenses selected from the group consisting of high refractive index lenses, concave lenses, convex lenses, aspheric lenses, and lenses with one concave side and one convex side. The refractive index nd of the high refractive index lens for d-line wavelength light, measured in accordance with ASTM D542, is preferably 1.50 or more, more preferably 1.52 or more, even more preferably 1.54 or more, and is preferably 1.70 or less, more preferably 1.68 or less, even more preferably 1.65 or less.

[0053] The optical component according to the present embodiment has an excellent balance of performances including a high Abbe number, heat resistance, and scratch resistance. Therefore, it can be suitably used as an optical component in an optical system that requires highly accurate and clear identification of an image. Furthermore, since it has a high Abbe number, it is possible to further miniaturize the optical component. The optical component is a component used in optical equipment, etc., and specifically, it can be suitably used as an optical component such as an in-vehicle camera lens or a camera lens for a mobile device (mobile phone, smartphone, tablet, etc.). Examples of the in-vehicle camera lens or the camera lens for a mobile device include a view camera lens, a sensing camera lens, a lens for converging light in a head-up display, and a lens for diffusing light in a head-up display.

[0054] 2. Method for producing copolymer (Z) Specifically, the method for producing the copolymer (Z) includes a synthesis step of synthesizing the monomer (X) and the monomer (Y) using a fluorine-containing olefin and a cyclic polyene, respectively, and a polymerization step of polymerizing the monomer (X) and the monomer (Y) to obtain the copolymer (Z). From the viewpoint of obtaining an optical lens with an improved balance of the performance of the Abbe number, the glass transition temperature, the refractive index, and the scratch resistance, it is preferable to carry out a purification step of purifying the monomer (X) and the monomer (Y) respectively and reducing the content of the fluorine-free cyclic diolefin compound before the polymerization step. If necessary, a hydrogenation step of hydrogenating the obtained copolymer (Z) may be carried out.

[0055] The synthesis process of the monomer (X) and the monomer (Y) can be carried out by an appropriate known method. For example, a monomer (X) solution and a monomer (Y) solution can be obtained by subjecting a fluorine-containing olefin (e.g., hexafluoropropene) to a Diels-Alder reaction with a cyclic polyene (e.g., cyclopentadiene, dicyclopentadiene, furan, etc.). In the purification step, an acid catalyst and at least one hydroxyl group-containing compound selected from the group consisting of water and alkyl alcohols are added to the monomer (X) solution or monomer (Y) solution obtained in the synthesis step to react with each other, and the monomer (X) or monomer (Y) is separated from the resulting reaction solution. More specifically, by using an acid catalyst, the fluorine-free cyclic diolefin compound contained in the obtained monomer (X) solution or monomer (Y) solution reacts with the hydroxyl group-containing compound, and the hydroxyl group-containing compound is added to the fluorine-free cyclic diolefin compound (e.g., dicyclopentadiene, tricyclopentadiene, etc.) to produce a fluorine-free hydrate compound or a fluorine-free ether compound. Next, the monomer (X) or monomer (Y) is separated from at least one selected from the group consisting of the fluorine-free hydrate compound and the fluorine-free ether compound by distillation. Since the boiling point difference between the fluorine-free hydrate compound or fluorine-free ether compound and the monomer (X) or monomer (Y) is larger than the boiling point difference between the fluorine-free cyclic diolefin compound and the monomer (X) or monomer (Y), the monomer (X) or monomer (Y) with improved purity can be obtained by distillation.

[0056] The acid catalyst is not particularly limited as long as it is a Bronsted acid, and examples thereof include at least one selected from the group consisting of inorganic acids, organic acids, and solid acids. Examples of inorganic acids include hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid. Examples of the organic acid include methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, 10-camphorsulfonic acid, trifluoroacetic acid, and the like. The solid acid may be, for example, a strongly acidic cation exchange resin having a sulfonic acid group. Among these, strong acid cation exchange resins are preferred from the viewpoint of separating the acid catalyst by filtration after the reaction without carrying out a step of neutralizing and extracting the acid used with an alkaline solution such as an aqueous sodium hydroxide solution, etc. Furthermore, strong acid cation exchange resins having a macroporous structure with a large surface area are preferred from the viewpoint of increasing the contact area with the reaction substrate.

[0057] From the viewpoint of further improving the reactivity between the fluorine-free cyclic diolefin compound and the hydroxyl group-containing compound, the alkyl alcohol is preferably at least one selected from the group consisting of 1-propanol, 2-propanol, 1-butanol, 2-butanol, 2-methyl-1-propanol, 2-methyl-2-propanol, 1-pentanol, 2-pentanol, 1-hexanol, 2-hexanol, 1-heptanol, 2-heptanol, 1-octanol, 1-nonanol, and 1-decanol, and more preferably at least one selected from the group consisting of 1-propanol, 1-butanol, 1-pentanol, and 1-hexanol.

[0058] In the polymerization step, the purified monomer (X) and monomer (Y) can be polymerized in the presence of a known polymerization catalyst. For example, a ring-opening metathesis polymerization catalyst can be used as the polymerization catalyst. The polymerization temperature, polymerization pressure, polymerization time, etc. are appropriately adjusted. In the hydrogenation step, the olefin portion of the main chain of the copolymer (Z) obtained in the polymerization step is hydrogenated using a catalyst. As the hydrogenation catalyst, a known homogeneous metal complex catalyst or a heterogeneous metal-supported catalyst can be used. By undergoing the above-mentioned purification process, it is possible to obtain a copolymer (Z) which can suppress gelation in the polymerization process and hydrogenation process and can give a uniform cured product in which polymerization unevenness, composition unevenness, and the like are suppressed.

[0059] The method for producing the copolymer (Z) containing a structural unit derived from the compound represented by general formula (A) and a structural unit derived from the compound represented by general formula (B) is similar to the method for producing the copolymer (Z) containing the structural unit (x) derived from the monomer (X) and the structural unit (y) derived from the monomer (Y) described above.

[0060] 3. Optical lens molding method The method for molding the optical lens from the copolymer (Z) in this embodiment is not particularly limited, and examples thereof include injection molding, press molding, compression molding, injection compression molding, extrusion molding, etc. In addition, the molding temperature when melt molding the optical lens of this embodiment is preferably 330° C. or lower. If it is 330° C. or lower, the mass loss amount when heated for 5 minutes is less than 0.1%, and the generation amount of highly corrosive fluorine-containing gas such as hydrogen fluoride accompanying the mass loss is small.

[0061] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements that do not impair the effects of the present invention are included in the present invention. EXAMPLES

[0062] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.

[0063] <Synthesis of Copolymer (Z)> Example 1 In a nitrogen atmosphere, 5.8 kg of dicyclopentadiene (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter also referred to as "DCp") and 16.6 kg of hexafluoropropene (manufactured by Takachiho Chemical Industry Co., Ltd.) were placed in a 25 L autoclave equipped with a magnetic stirrer, and the mixture was heated and stirred at 160° C. for 24 hours, and then heated and stirred at 180° C. for 15 hours. After cooling, 3.9 kg of unreacted hexafluoropropene was recovered, and 17.9 kg of the reaction liquid was taken out. The resulting reaction solution was then distilled to obtain 5,6-difluoro-5-fluoro-6-(trifluoromethyl)bicyclo(2.2.1)hept-2-ene (hereinafter referred to as "NBF 6 ") and DCp were obtained, and 15.5 kg of a composition containing 8,8,9-trifluoro-9-trifluoromethyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-Dodecene (hereinafter referred to as "TDF 6 ") and NBF 6 2.2 kg of a composition (X1) containing DCp and tricyclopentadiene (hereinafter also referred to as "TCPD") was obtained.

[0064] Next, 250 g of composition (X1), 170 g of 1-propanol, which is a hydroxyl group-containing compound, and 25 g of a cation exchange resin (AMBERLYST 15JS-HG·DRY, manufactured by Organo Corporation), which is a solid acid catalyst, were placed in a 1000 mL glass reactor equipped with a stirrer and a condenser, and the mixture was heated and stirred at 110°C for 12 hours under a nitrogen atmosphere to carry out an etherification reaction of DCp and TCPD in composition (X1). Next, the resulting reaction liquid was cooled to room temperature, and the solid acid catalyst was removed by filtration under reduced pressure to obtain NBF before distillation purification. 6 and T.D.F. 6 The composition containing NBF before distillation and purification was obtained. 6 and T.D.F. 6 A Sneader fractionating column and a Liebig condenser were attached to a round-bottom flask containing a composition containing 6 and T.D.F. 6 was obtained by fractional distillation.

[0065] In a 5 L autoclave equipped with a magnetic stirrer under nitrogen atmosphere, the NBF obtained above was 6 495g (2.3mol) of the TDF obtained above 6 970g (3.4mol) of 1-hexene and 32.2g (0.38mol) of 1-hexene were dissolved in 1.5kg of tetrahydrofuran (hereinafter referred to as THF) and stirred. i 2 C6 H 3 )(CHCMe 2 Ph)(OBu t ) 2 The mixture was reacted at 70° C. for 48 hours. Then, 248 mg (3.4 mmol) of n-butyl aldehyde was added and cooled to obtain 3.0 kg of a ring-opening metathesis polymerized polymer solution. 1 The polymerization rate of the obtained polymer was 100% by H-NMR. The obtained polymer solution was diluted with 3.0 kg of THF, and palladium alumina was added to the polymer solution to carry out a hydrogenation reaction of the olefin part of the polymer at 160°C, thereby obtaining a THF solution of a fluorine-containing cyclic olefin polymer. 1 The hydrogenation rate of the polymer obtained by H-NMR was 100%. Palladium alumina was removed from the obtained polymer solution by filtration through a 0.1 μm filter. A fluorine-containing cyclic olefin polymer was precipitated from the obtained polymer solution using water / methanol = 50 / 50 (wt / wt), filtered, and dried under reduced pressure at 80 ° C to obtain a white powder solid (copolymer Z1).

[0066] Example 2 NBF 6 779g (3.6mol), TDF 6 678 g (2.4 mol), 33.7 g (0.40 mol) of 1-hexene, Mo(N-2,6-Pr i 2 C 6 H 3 )(CHCMe 2 Ph)(OBu t ) 2 A white powder solid of copolymer Z2 was obtained in the same manner as in Example 1, except that the amount of copolymer Z2 was changed to 660 mg (1.20 mmol). 1 The polymerization rate of the polymer obtained by H-NMR was 100%. 1 The hydrogenation rate of the polymer obtained was 100% by H-NMR.

[0067] <Synthesis of homopolymer (W)> Comparative Example 1 NBF 6 1450g (6.7mol), 1-hexene 4.1g (0.048mol), Mo(N-2,6-Pr i 2 C 6 H 3 )(CHCMe 2 Ph)(OBu t ) 2 was changed to 740 mg (1.35 mmol), and TDF 6 A white powder solid of homopolymer W1 was obtained in the same manner as in Example 1, except that no toluene was used and precipitation was performed with methanol. 1 The polymerization rate of the polymer obtained by H-NMR was 100%. 1 The hydrogenation rate of the polymer obtained was 100% by H-NMR.

[0068] Comparative Example 2 TDF 6 1460g (5.2mol), 1-hexene 101.8g (1.21mol), Mo(N-2,6-Pr i 2 C 6 H 3 )(CHCMe 2 Ph)(OBu t ) 2 was changed to 570 mg (1.04 mmol), and NBF 6 A white powder solid of homopolymer W2 was obtained in the same manner as in Example 1, except that no hexane was used and precipitation was performed with methanol. 1 The polymerization rate of the polymer obtained by H-NMR was 100%. 1 The hydrogenation rate of the polymer obtained was 100% by H-NMR.

[0069] The physical properties of the copolymer (Z) and homopolymer (W) obtained in each example were measured by the following methods.

[0070] [Polymer conversion] In each example, after polymerization of the monomer, the polymer before hydrogenation was dissolved in deuterated tetrahydrofuran and subjected to 400 MHz- 1Using H-NMR spectrum, the polymerization rate of the polymer was calculated from the integral value of the signal originating from hydrogen bonded to the double bond carbon of the monomer at δ=6.0-6.5 ppm and hydrogen bonded to the double bond carbon of the main chain of the polymer at δ=5.0-6.0 ppm.

[0071] [Hydrogenation rate] The copolymer (Z) and homopolymer (W) obtained in each example were dissolved in deuterated tetrahydrofuran and subjected to 400 MHz- 1 Using H-NMR spectrum, the hydrogenation rate was calculated from the integral value of the signals of hydrogen bonded to the double bond carbon of the main chain of the polymer at δ=5.0-6.0 ppm and hydrogen originating from the hydrogenated polymer at δ=0.7-3.0 ppm.

[0072] [Molar ratio of structural unit (x) to structural unit (y) and fluorine content (mass%)] The fluorine atom content in the copolymer (Z) and homopolymer (W) obtained in each example, and the molar ratio of the structural unit (x) to the structural unit (y) in the copolymer (Z) are as follows: 19 Measurements were performed by F-NMR. Using a JEOL ECA500 nuclear magnetic resonance spectrometer, 19 F-NMR spectrum was measured and δ = 0.00 ppm of CFCl 3 The -CF of copolymer Z and homopolymer W, respectively, at δ=-150 to -200 ppm and -CF of δ=-100 to -150 ppm were used as the reference signal. 2 , or δ=-60~-100ppm -CF 3 The molar ratio (x / y) of the structural unit (x) to the structural unit (y) was calculated using the integral value of fluorine derived from the above. The fluorine content (mass%) was calculated from formula (1). Measurement solvent: Deuterated tetrahydrofuran Sample concentration: Approximately 5% ·Measurement temperature: room temperature Number of times: 256 Base peak: Automatically set by the instrument to CFCl 3 Set to 0.00 ppm Equation (1): Fluorine atom content (mass%) = {(F(A)n × 19 × [A]) / (F(A)w × [A] + F(B)w × [B]) + (F(B)n × 19 × [B]) / (F(A)w × [A] + F(B)w × [B])} × 100 (1) Here, in formula (1), F(A)n represents the number of fluorine atoms in the structural unit derived from the compound represented by general formula (A), F(B)n represents the number of fluorine atoms in the structural unit derived from the compound represented by general formula (B), F(A)w represents the formula weight of the structural unit derived from the compound represented by general formula (A), and F(B)w represents the formula weight of the structural unit derived from the compound represented by general formula (B). In addition, in formula (1), [A] and [B] represent -CF and -CF of the structural unit derived from the compound represented by general formula (A). 2 , and -CF 3 and the integral value of fluorine derived from the compound represented by general formula (B) of the structural units -CF and -CF 2 , and -CF 3 represents the mole fraction of each of the structural units derived from the compounds represented by general formulas (A) and (B), calculated from the integral value of fluorine derived from, and 19 represents the molecular weight of fluorine. In the present Examples and Comparative Examples, the structural unit (x) is a structural unit derived from a compound represented by general formula (A) (i.e., monomer (X)), and the structural unit (y) is a structural unit derived from a compound represented by general formula (B) (i.e., monomer (Y)).

[0073] [Weight average molecular weight (Mw), molecular weight distribution (Mw / Mn)] For the copolymer (Z) and homopolymer (W) obtained in each example, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polymer dissolved in tetrahydrofuran (THF) were measured by gel permeation chromatography (GPC) under the following conditions, calibrating the molecular weight with a polystyrene standard (manufactured by Resonac Holdings, Inc., product name: Shodex STANDARD SM-105). Detector: JASCO 830-RI and 875-UV Column: Shodex k-806M, 804, 803, 802.5 Flow rate: 1.0ml / min

[0074] [Glass transition temperature Tg] Viscoelasticity measurements were performed on the copolymer (Z) and homopolymer (W) obtained in each example using RSA-III manufactured by TA Instruments. The glass transition temperature (Tg) was evaluated as the peak top temperature of the loss tangent (tan δ=E'' / E'), which is the storage modulus E' and loss modulus E'', when the temperature was raised from 20°C to approximately 200°C under nitrogen at 1 Hz and a heating rate of 3°C / min in tension mode.

[0075] <Method for producing hot-pressed pieces of copolymer (Z) and homopolymer (W)> The copolymer (Z) and homopolymer (W) obtained in each example were premelted in a vacuum oven under vacuum (Tg+110°C) for 30 minutes. After premelting was completed, the sheet-shaped polymer pieces were taken out and filled into a mold (1 mm or 3 mm thick), and heated in air under conditions of (Tg+120°C), 10 MPa, and 1 minute to produce pressed pieces.

[0076] The following physical properties were measured using the hot-pressed pieces of each example obtained. A 3 mm-thick pressed piece was used to measure the refractive index nd and Abbe number νd, and a 1 mm-thick pressed piece was used to measure the light transmittance and pencil hardness.

[0077] [Refractive index nd and Abbe number νd] The refractive index and Abbe number νd of the heat-pressed specimen obtained in each example were determined in accordance with ASTM D542. The refractive index was measured using a KPR-3000 manufactured by Shimadzu Corporation. Using a heat-pressed specimen with a thickness of 3 mm, the refractive indexes of d-line, C-line, and F-line at 25°C were measured using the V-block method, and the Abbe number νd was calculated using the following formula (2). Abbe number (νd) = (nd-1) / (nf-nc) (2) In the formula (2), nd represents the d-line refractive index (wavelength 587.6 nm), nf represents the F-line refractive index (wavelength 486.1 nm), and nc represents the C-line refractive index (wavelength 656.3 nm).

[0078] [Light transmittance] The heat-pressed pieces obtained in each example were used to measure the light transmittance in the visible light region according to JIS K 7361-1:1997 using a spectrophotometric colorimeter / haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., COH7700).

[0079] [Pencil hardness] The pencil hardness as specified in ISO 15184 was measured using the hot-pressed specimens obtained in each example.

[0080] [Table 1]

Claims

1. An optical component having two or more optical lenses, the optical lens of the outermost layer in the optical component comprises a copolymer (Z) including a structural unit (x) derived from a monomer (X) having a cyclic structure with 3 to 4 rings and a structural unit (y) derived from a monomer (Y) having a cyclic structure with 6 to 7 rings, In the copolymer (Z), 19 The content of fluorine atoms as measured by F-NMR is 20% by mass or more and 70% by mass or less, when the entirety of the copolymer (Z) is taken as 100% by mass.

2. The monomer (X) includes a compound represented by the following general formula (A): The optical component according to claim 1 , wherein the monomer (Y) includes a compound represented by the following general formula (B): 【Chemistry 1】 (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a group that does not contain fluorine, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. 【Chemistry 2】 (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a group that does not contain fluorine, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

3. In the general formula (A), R 1 ~R 4 at least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms; In the general formula (B), R 5 ~R 8 3. The optical component according to claim 2, wherein at least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms.

4. the number of cyclic structures / the total number of carbon atoms in the monomer (X) is 0.20 or more and 0.45 or less, 4. The optical component according to claim 1, wherein the number of cyclic structures / the total number of carbon atoms in the monomer (Y) is 0.30 or more and 0.50 or less.

5. In the copolymer (Z), the molar ratio (x / y) of the structural unit (x) derived from the monomer (X) to the structural unit (y) derived from the monomer (Y) is 0.25 or more and 4.0 or less. The optical component according to any one of claims 1 to 4.

6. When the entire copolymer (Z) is taken as 100 mass%, the total content of the structural unit (x) and the structural unit (y) in the copolymer (Z) is 50 mass% or more and 100 mass% or less. The optical component according to any one of claims 1 to 5.

7. An optical component having two or more optical lenses, The optical lens of the outermost layer of the optical component is A structural unit derived from a compound represented by the following general formula (A), An optical component comprising a copolymer (Z) containing a structural unit derived from a compound represented by the following general formula (B): 【Chemistry 3】 (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a group that does not contain fluorine, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. 【Chemistry 4】 (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a group that does not contain fluorine, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

8. The optical component according to claim 7, wherein in the copolymer (Z), the molar ratio (x' / y') of the structural unit (x') derived from the compound represented by the general formula (A) to the structural unit (y') derived from the compound represented by the general formula (B) is 0.25 or more and 4.0 or less.

9. 9. The optical component according to claim 7 or 8, wherein the total content of the structural unit (x') derived from the compound represented by the general formula (A) in the copolymer (Z) and the structural unit (y') derived from the compound represented by the general formula (B) is 50% by mass or more and 100% by mass or less, when the entire copolymer (Z) is 100% by mass.

10. The optical component according to any one of claims 1 to 9, wherein the copolymer (Z) has a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of 500 or more and 1,000,000 or less.

11. The copolymer (Z) has a ratio (Mw / Mn) of the weight average molecular weight (Mw) and the number average molecular weight (Mn) in terms of polystyrene, measured by gel permeation chromatography (GPC), of 1.0 or more and 5.0 or less. The optical component according to any one of claims 1 to 10.

12. 12. The optical component according to claim 1, wherein the outermost optical lens has an Abbe number vd of 60 or more and 120 or less, as measured in accordance with ASTM D542.

13. The optical component according to any one of claims 1 to 12, wherein the copolymer (Z) has a glass transition temperature of 120°C or higher.

14. 14. The optical component according to claim 1, wherein the refractive index nd of the outermost optical lens with respect to d-line wavelength light measured in accordance with ASTM D542 is 1.30 or more and 1.48 or less.

15. The optical component according to any one of claims 1 to 14, wherein the pencil hardness of the outermost optical lens is in the range of B to 2H as defined by ISO 15184.

16. 16. The optical component according to claim 1, wherein the thickness of the outermost optical lens is 0.5 mm or more and 15 mm or less.

Citation Information

Patent Citations

  • Optical part using fluorine-containing cyclic olefin polymer

    JP2007177046A