Fluorine-containing cyclic olefin copolymer, fluorine-containing cyclic olefin resin composition, molding, optical component, method for producing fluorine-containing cyclic olefin copolymer, and method for producing lens molding

By controlling the molecular weight distribution and structural units in fluorine-containing cyclic olefin copolymers, the generation of hydrogen fluoride during molding is minimized, ensuring safer and more durable optical components.

JP2024137036AInactive Publication Date: 2024-10-04MITSUI CHEMICALS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048388
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fluorine-containing cyclic olefin polymers generate significant amounts of hydrogen fluoride during heat molding, posing health risks and damaging molding machines.

Method used

Reducing the content of components with a weight average molecular weight of 10,000 or less in the fluorine-containing cyclic olefin copolymer to a predetermined value or less, optimizing the molecular weight distribution and structural units to minimize hydrogen fluoride generation.

Benefits of technology

Significantly reduces hydrogen fluoride generation during heat molding, enhancing safety and machine longevity while maintaining optical properties such as high Abbe number and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137036000001
    Figure 2024137036000001
  • Figure 2024137036000002
    Figure 2024137036000002
  • Figure 2024137036000003
    Figure 2024137036000003
Patent Text Reader

Abstract

To provide a fluorine-containing cyclic olefin copolymer reduced in the amount of hydrogen fluoride generated during heat molding.SOLUTION: In the fluorine-containing cyclic olefin copolymer, the content of a component having a weight average molecular weight (Mw) measured by gel permeation chromatography of 10,000 or less is 10.0 mass% or less based on 100 mass% of the whole fluorine-containing cyclic olefin copolymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fluorine-containing cyclic olefin copolymer, a fluorine-containing cyclic olefin resin composition, a molded article, an optical part, a method for producing a fluorine-containing cyclic olefin copolymer, and a method for producing a lens molded article. [Background technology]

[0002] Various optical components (lenses) require lens materials with high Abbe numbers to achieve clearer image quality and to reduce size. In order to improve the Abbe number, designs that introduce fluorine atoms into resins are sometimes used. Examples of technologies related to high Abbe numbers include those described in Patent Document 1.

[0003] Patent Document 1 describes an optical component material that has a refractive index of 1.48 or less for D-line wavelength light and contains a fluorine-containing cyclic olefin polymer having at least a repeating structural unit represented by general formula (1). The fluorine-containing cyclic olefin polymer is soluble in organic solvents that do not contain fluorine atoms, has high surface polarity, and has a small water contact angle, so that it can be suitably used as an antireflection film, and also describes that the Abbe number is 60 or more. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-177046 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention provides a fluorine-containing cyclic olefin copolymer which generates a reduced amount of hydrogen fluoride during heat molding. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to solve the above problems, and as a result have found that the amount of hydrogen fluoride generated during hot molding can be reduced by controlling the content of components having a weight average molecular weight (Mw) of 10,000 or less in a fluorine-containing cyclic olefin copolymer to a predetermined value or less, thereby completing the present invention. According to the present invention, there are provided a fluorine-containing cyclic olefin copolymer, a fluorine-containing cyclic olefin resin composition, a molded article, an optical part, a method for producing a fluorine-containing cyclic olefin copolymer, and a method for producing a lens molded article, all of which are shown below.

[0007] [1] A fluorine-containing cyclic olefin copolymer, The fluorine-containing cyclic olefin copolymer has a content of a component having a weight average molecular weight (Mw) of 10,000 or less as measured by gel permeation chromatography, which is 10.0% by mass or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100% by mass. [2] The fluorine-containing cyclic olefin copolymer according to [1], which has an amount of hydrogen fluoride generated of less than 60 ppm as measured by ion chromatography according to the <Amount of Hydrogen Fluoride Generated> below. <Amount of hydrogen fluoride generated> (1) 0.1 g of the fluorine-containing cyclic olefin copolymer was placed in a platinum boat and inserted into a quartz tube in a heating furnace heated to 250° C. while passing nitrogen gas at a rate of 0.2 L / min. (2) The fluorine-containing cyclic olefin copolymer is heated in a heating furnace at 250° C. for 30 minutes, and the hydrogen fluoride generated during the heating is dissolved in 5 mL of ultrapure water in an impinger. (3) The hydrogen fluoride dissolved in the ultrapure water is converted into hydrogen ions (H + ) and fluorine ion (F - ) and the amount of fluorine ions generated is measured using an ion chromatograph. (4) The amount of hydrogen fluoride generated is calculated according to the following formula (1). Amount of hydrogen fluoride generated (ppm) = (amount of fluoride ions generated (mg)) ÷ (total mass of copolymer (kg)) × (20 / 19) (1) Here, the number 19 represents the atomic weight of fluorine, and the number 20 represents the molecular weight of hydrogen fluoride. [3] The fluorine-containing cyclic olefin copolymer according to [1] or [2], which has a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of 50,000 or more and 100,000 or less. [4] The fluorine-containing cyclic olefin copolymer according to any one of [1] to [3], having a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) in terms of polystyrene, measured by gel permeation chromatography (GPC), of 2.8 or less. [5] A structural unit (x) derived from a compound (X) represented by the following general formula (A), The fluorine-containing cyclic olefin copolymer according to any one of [1] to [4], which contains a structural unit (y) derived from a compound (Y) represented by the following general formula (B): [ka] (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [ka] (In the above formula (B), R 5~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure. [6] In the general formula (A), R 1 ~R 4 at least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms; In the general formula (B), R 5 ~R 8 at least one of which is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms. [7] The fluorine-containing cyclic olefin copolymer according to [5] or [6], wherein the molar ratio (x / y) of the structural unit (x) to the structural unit (y) in the fluorine-containing cyclic olefin copolymer is 0.25 or more and 4.0 or less. [8] The fluorine-containing cyclic olefin copolymer according to any one of [5] to [7], wherein the total content of the structural unit (x) and the structural unit (y) in the fluorine-containing cyclic olefin copolymer is 50% by mass or more and 100% by mass or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100% by mass. [9] A fluorine-containing cyclic olefin resin composition comprising the fluorine-containing cyclic olefin copolymer according to any one of [1] to [8].

[10] A molded article comprising the fluorine-containing cyclic olefin copolymer according to any one of [1] to [8] or the fluorine-containing cyclic olefin resin composition according to [9].

[11] The molded article according to

[10] , which is an optical lens.

[12] An optical component having two or more optical lenses, An optical component, wherein the optical lens in the outermost layer of the optical component is the molded article according to

[11] .

[13] A method for producing a fluorine-containing cyclic olefin copolymer, comprising the steps of: Hildebrand solubility parameter δ (SP value) is 20MPa 1 / 2 More than 38MPa 1 / 2 A method for producing a fluorine-containing cyclic olefin copolymer, comprising the step of precipitating the fluorine-containing cyclic olefin copolymer using a solvent selected from the group consisting of:

[14] The method for producing a fluorine-containing cyclic olefin copolymer according to

[13] , wherein the fluorine-containing cyclic olefin copolymer has a weight average molecular weight (Mw) of 50,000 or more and 100,000 or less in terms of polystyrene measured by gel permeation chromatography (GPC).

[15] The method for producing a fluorine-containing cyclic olefin copolymer according to

[13] or

[14] , wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the fluorine-containing cyclic olefin copolymer in terms of polystyrene, as measured by gel permeation chromatography (GPC), is 2.8 or less.

[16] The method for producing a fluorine-containing cyclic olefin copolymer according to any one of

[13] to

[15] , wherein the fluorine-containing cyclic olefin copolymer contains a structural unit (x) derived from a compound (X) represented by the following general formula (A) and a structural unit (y) derived from a compound (Y) represented by the following general formula (B): [ka] (In the above formula (A), R 1 ~R 4at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [ka] (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

[17] The method for producing a fluorine-containing cyclic olefin copolymer according to any one of

[13] to

[16] , wherein the fluorine-containing cyclic olefin copolymer contains a component having a weight average molecular weight (Mw) of 10,000 or less as measured by gel permeation chromatography in an amount of 10.0 mass% or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100 mass%.

[18] A method for producing a lens molding, comprising the step of molding a fluorine-containing cyclic olefin copolymer according to any one of [1] to [8] or a fluorine-containing cyclic olefin resin composition according to [9] into a lens. Effect of the Invention

[0008] According to the present invention, it is possible to provide a fluorine-containing cyclic olefin copolymer which generates a reduced amount of hydrogen fluoride during hot molding. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the present invention will be described based on the embodiment. In this embodiment, "A to B" indicating a numerical range means A or more and B or less unless otherwise specified. In addition, when a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily.

[0010] <Fluorine-containing cyclic olefin copolymer> In the fluorine-containing cyclic olefin copolymer of the present embodiment, the content of components having a weight average molecular weight (Mw) of 10,000 or less as measured by gel permeation chromatography is 10.0% by mass or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100% by mass. The content of components having a weight average molecular weight (Mw) of 10,000 or less in the fluorine-containing cyclic olefin copolymer is preferably 9.8 mass% or less, more preferably 9.6 mass% or less, even more preferably 9.0 mass% or less, even more preferably 8.0 mass% or less, even more preferably 7.0 mass% or less, and even more preferably 6.5 mass% or less, from the viewpoint of further reducing the amount of hydrogen fluoride generated during heat molding. There is no lower limit for the content of components having a weight average molecular weight (Mw) of 10,000 or less, but it may be, for example, 0% by mass or more, 1.0% by mass or more, 2.0% by mass or more, 3.0% by mass or more, or 4.0% by mass or more. From the viewpoint of further reducing the amount of hydrogen fluoride generated during heat molding, the content of components having a weight average molecular weight (Mw) of 10,000 or less in the fluorine-containing cyclic olefin copolymer is preferably 0% by mass or more and 10.0% by mass or less, more preferably 1.0% by mass or more and 9.8% by mass or less, even more preferably 2.0% by mass or more and 9.6% by mass or less, and even more preferably 3.0% by mass or more and 8.0% by mass or less.

[0011] In this embodiment, the content of components having a weight average molecular weight (Mw) of 10,000 or less in the fluorine-containing cyclic olefin copolymer is measured by gel permeation chromatography and is calculated as polystyrene. The measurement method may be the method described in the examples. Specifically, the measurement is performed as follows. For the fluorine-containing cyclic olefin copolymer, the weight average molecular weight (Mw) of the polymer dissolved in THF was measured using gel permeation chromatography (GPC) using a polystyrene standard of weight average molecular weight (Mw) = 1.32 × 10 3 , 2.78×10 3 , 1.07×10 4 , 2.20×10 4 , 6.60×10 4 , 1.56×10 5 , 4.60×10 5 The molecular weight is calibrated and measured using the seven samples. Using the weight average molecular weight (Mw) results obtained, the total amount of components having a weight average molecular weight (Mw) of 10,000 or less can be divided by the weight of the fluorine-containing cyclic olefin copolymer used in the measurement to calculate the content of components having a weight average molecular weight (Mw) of 10,000 or less. The GPC measurement conditions may be, for example, as follows: Detector: JASCO 830-RI and 875-UV Column: Shodex k-806M, 804, 803, 802.5 (manufactured by Resonac Holdings, Inc.) Solvent: Tetrahydrofuran Flow rate: 1.0mL / min Column temperature: 40℃ Concentration: 7.5mg / mL Injection volume: 100μL Polystyrene standard: Manufactured by Resonac Holdings Co., Ltd., Product name: Shodex STANDARD SM-105

[0012] Optical components (lenses) in imaging devices installed in automobiles and in smartphone cameras require lens materials with high Abbe numbers to achieve clearer image quality and to reduce size. High Abbe lens materials have small chromatic aberration, so they can be used in the outermost layer of a combination lens to reduce color shift. Resin lenses made of amorphous polymers are used in the optical lenses of recent imaging devices and smartphone cameras. Fluorine atoms are introduced into the polymer to design resin lenses with high Abbe numbers, but the introduction of fluorine atoms reduces heat resistance, and hydrogen fluoride (HF) may be generated during the granulation and injection molding processes that involve heating during molding into camera lenses. Hydrogen fluoride is harmful to human health and corrodes molding machines, so suppressing the generation of hydrogen fluoride is an issue.

[0013] According to the studies of the present inventors, it has been found that the amount of hydrogen fluoride generated during hot molding can be reduced by adjusting the content of components having a weight average molecular weight (Mw) of 10,000 or less in the fluorine-containing cyclic olefin copolymer to a predetermined value or less. The reason for this is unclear, but it is believed that when the content of low molecular weight components with a weight average molecular weight (Mw) of 10,000 or less is low, the elimination of the fluorocarbon substituents (-CF, -CF2 or -CF3) of the fluorine-containing cyclic olefin copolymer during heating is relatively difficult, and therefore the amount of hydrogen fluoride generated during heat molding is reduced. In addition, in the case of a copolymer in which two or more compounds are polymerized, the polymerization tends to be nonuniform, so the content of low molecular weight components with a weight average molecular weight (Mw) of 10,000 or less tends to be high, but even in this case, the amount of hydrogen fluoride generated during heat molding can be reduced by setting the content of low molecular weight components with a weight average molecular weight (Mw) of 10,000 or less to a predetermined value or less.

[0014] The amount of hydrogen fluoride generated when the fluorine-containing cyclic olefin copolymer is heated under specific conditions is preferably less than 60 ppm, more preferably 55 ppm or less, even more preferably 50 ppm or less, even more preferably 45 ppm or less, even more preferably 40 ppm or less, even more preferably 35 ppm or less, even more preferably 30 ppm or less, even more preferably 25 ppm or less. There is no lower limit to the amount of hydrogen fluoride generated when the fluorine-containing cyclic olefin copolymer is heated, but it may be, for example, 0 ppm or more, 1 ppm or more, 5 ppm or more, or 10 ppm or more. The unit (ppm) of the amount of hydrogen fluoride generated when a fluorine-containing cyclic olefin copolymer is heated represents the amount of fluorine generated (mg) per 1 kg of the fluorine-containing cyclic olefin copolymer, ie, mg / kg.

[0015] The amount of hydrogen fluoride generated when the fluorine-containing cyclic olefin copolymer is heated is measured by ion chromatography as follows. (1) 0.1 g of a fluorine-containing cyclic olefin copolymer is placed in a platinum boat and inserted into a quartz tube in a heating furnace heated to 250° C. while nitrogen gas is passed through the boat at a rate of 0.2 L / min. (2) The fluorine-containing cyclic olefin copolymer is heated in a heating furnace at 250°C for 30 minutes, and the hydrogen fluoride generated during the heating process is dissolved in 5 mL of ultrapure water in an impinger. (3) Hydrogen fluoride dissolved in ultrapure water converts into hydrogen ions (H + ) and fluorine ion (F - ) and the amount of fluorine ions generated is measured using an ion chromatograph. (4) Calculate the amount of hydrogen fluoride generated using the following formula (1). Amount of hydrogen fluoride generated (ppm) = (amount of fluoride ions generated (mg)) ÷ (total mass of copolymer (kg)) × (20 / 19) (1) Here, the above number 19 represents the atomic weight of fluorine, the above number 20 represents the molecular weight of hydrogen fluoride, and the amount of fluorine ions generated is calculated using a calibration curve prepared using a standard substance (fluorine compound).

[0016] From the viewpoint of improving heat resistance, the fluorine-containing cyclic olefin copolymer of the present embodiment preferably contains a structural unit (x) derived from a compound (X) represented by the following general formula (A) and a structural unit (y) derived from a compound (Y) represented by the following general formula (B).

[0017] [ka]

[0018] In formula (A), preferably, R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a non-fluorine-containing group, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure.

[0019] In formula (A), R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 1 ~R 4 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 1 ~R 4 At least one of these is fluorine or a perfluoroalkyl group having 1 to 2 carbon atoms, and more preferably, R 1 ~R 4 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 1 ~R 4 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 4 is a trifluoromethyl group, and R 1 ~R 3 is fluorine. This makes it possible to further improve the balance between the optical properties such as the Abbe number of an optical lens and the heat resistance. From the viewpoint of further improving the balance between the optical properties such as the Abbe number of an optical lens or the like and the heat resistance, compound (X) preferably contains 5,6-difluoro-5-fluoro-6-(trifluoromethyl)bicyclo(2.2.1)hept-2-ene (hereinafter also referred to as "NBF6").

[0020] [ka]

[0021] In formula (B), preferably, R5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a non-fluorine-containing group, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

[0022] In formula (B), R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 10 carbon atoms, and more preferably R 5 ~R 8 At least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms, and more preferably R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 4 carbon atoms, and more preferably, R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 3 carbon atoms, and more preferably, R 5 ~R 8 At least one of these is fluorine or a perfluoroalkyl group having 1 to 2 carbon atoms, and more preferably, R 5 ~R 8 At least one of R is fluorine or a trifluoromethyl group, and more preferably R 5 ~R 8 Any one of the groups is a trifluoromethyl group and the remaining three groups are fluorine. More preferably, R 8 is a trifluoromethyl group, and R 5 ~R 7 is fluorine. This makes it possible to further improve the balance between the optical properties such as the Abbe number of an optical lens and the heat resistance. From the viewpoint of further improving the balance between the optical properties such as the Abbe number of an optical lens or the like and the heat resistance, the compound (Y) is 8,8,9-trifluoro-9-trifluoromethyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ]-3-dodecene (hereinafter also referred to as "TDF6").

[0023] In the fluorine-containing cyclic olefin copolymer, the molar ratio (x / y) of the structural unit (x) derived from the compound (X) to the structural unit (y) derived from the compound (Y) is preferably 0.25 or more, more preferably 0.30 or more, even more preferably 0.40 or more, even more preferably 0.50 or more, even more preferably 0.60 or more, and preferably 4.0 or less, more preferably 3.5 or less, even more preferably 3.0 or less, even more preferably 2.5 or less, even more preferably 2.0 or less, even more preferably 1.5 or less, even more preferably 1.0 or less. In the fluorine-containing cyclic olefin copolymer, the molar ratio (x / y) of the structural unit (x) derived from the compound (X) to the structural unit (y) derived from the compound (Y) is preferably 0.25 or more and 4.0 or less, more preferably 0.40 or more and 3.5 or less, even more preferably 0.50 or more and 3.0 or less, even more preferably 0.60 or more and 2.0 or less. This makes it possible to further improve the balance of performance among high Abbe number, heat resistance, and scratch resistance. The molar ratio (x / y) of the structural unit (x) derived from the compound (X) to the structural unit (y) derived from the compound (Y) in the fluorine-containing cyclic olefin copolymer is 19 It can be measured by F-NMR.

[0024] From the viewpoint of further improving the balance between the performance of optical properties such as Abbe number and heat resistance, the total content of the constituent unit (x) derived from the compound (X) and the constituent unit (y) derived from the compound (Y) in the fluorine-containing cyclic olefin copolymer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and is, for example, 100% by mass or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100% by mass.

[0025] The fluorine-containing cyclic olefin copolymer may contain structural units derived from compounds other than the compound (X) and the compound (Y) as long as the effects of the present invention are not impaired. When the fluorine-containing cyclic olefin copolymer contains constituent units derived from other compounds, the content of the constituent units derived from other compounds, when the entire fluorine-containing cyclic olefin copolymer is taken as 100 mass%, is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, even more preferably 20 mass% or less, and even more preferably 10 mass% or less, and may be, for example, 0 mass% or more, 1 mass% or more, or 5 mass% or more.

[0026] The fluorine content of the fluorine-containing cyclic olefin copolymer, when the entire fluorine-containing cyclic olefin copolymer is taken as 100 mass%, from the viewpoint of further improving the Abbe number, is preferably 20 mass% or more, more preferably 25 mass% or more, even more preferably 30 mass% or more, even more preferably 35 mass% or more, and even more preferably 40 mass% or more, and from the viewpoints of improving the strength of the obtained lens, reducing its susceptibility to scratches, increasing the glass transition temperature, and improving the moldability, it is preferably 70 mass% or less, more preferably 65 mass% or less, even more preferably 60 mass% or less, even more preferably 55 mass% or less, and even more preferably 50 mass% or less. The fluorine content of the fluorine-containing cyclic olefin copolymer is 19 It can be measured by F-NMR.

[0027] The weight average molecular weight (Mw) of the fluorine-containing cyclic olefin copolymer measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 50,000 or more, more preferably 55,000 or more, and even more preferably 60,000 or more, from the viewpoint of further expressing the physical properties as a polymer, and from the viewpoint of further maintaining the fluidity during thin film formation and injection molding, it is preferably 100,000 or less, more preferably 90,000 or less, more preferably 80,000 or less, and even more preferably 70,000 or less. From the viewpoint of further expressing the physical properties as a polymer and further maintaining the fluidity during thin film formation and injection molding, the weight average molecular weight (Mw) of the fluorine-containing cyclic olefin copolymer measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 50,000 or more and 100,000 or less, more preferably 55,000 or more and 90,000 or less, and even more preferably 60,000 or more and 80,000 or less.

[0028] The ratio (Mw / Mn) of the polystyrene-equivalent weight average molecular weight (Mw) to number average molecular weight (Mn) of the fluorine-containing cyclic olefin copolymer measured by gel permeation chromatography (GPC) is, for example, 1.0 or more, and from the viewpoint of obtaining thin film formability with a uniform thickness and good injection moldability, is preferably 1.2 or more, more preferably 1.5 or more, even more preferably 2.0 or more, and even more preferably 2.1 or more, and from the viewpoint of further reducing the amount of hydrogen fluoride generated during hot molding, is preferably 2.8 or less, more preferably 2.7 or less, even more preferably 2.6 or less, even more preferably 2.5 or less, and even more preferably 2.4 or less. From the viewpoint of obtaining a thin film formability with a uniform thickness and good injection moldability, the ratio (Mw / Mn) of the weight average molecular weight (Mw) in terms of polystyrene and the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) is preferably 1.0 or more and 2.8 or less, more preferably 1.5 or more and 2.7 or less, even more preferably 2.0 or more and 2.6 or less, and even more preferably 2.1 or more and 2.5 or less.

[0029] The fluorine-containing cyclic olefin resin composition of the present embodiment contains the fluorine-containing cyclic olefin copolymer of the present embodiment. When the fluorine-containing cyclic olefin resin composition contains a fluorine-containing cyclic olefin copolymer, the content of the fluorine-containing cyclic olefin copolymer in the fluorine-containing cyclic olefin resin composition is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, even more preferably 98 mass% or more, and preferably 100 mass% or less, when the entire fluorine-containing cyclic olefin resin composition is taken as 100 mass%, from the viewpoint of further reducing the amount of hydrogen fluoride generated during hot molding.

[0030] Furthermore, the fluorine-containing cyclic olefin resin composition of the present embodiment may contain other components in addition to the fluorine-containing cyclic olefin copolymer, as long as the effects of the present invention are not impaired. Examples of other components include resins other than the fluorine-containing cyclic olefin copolymer and known additives. Examples of the other resin include at least one resin selected from the group consisting of amorphous transparent resins such as polycarbonate resin, acrylic resin, amorphous polyarylate, and alicyclic hydrocarbon resin. Examples of the additives include ultraviolet absorbers, antioxidants, flame retardants, antistatic agents, colorants, secondary antioxidants, lubricants, release agents, anti-fogging agents, weather resistance stabilizers, light resistance stabilizers, and metal deactivators.

[0031] <Molded body> The molded article of the present embodiment is a molded article containing the fluorine-containing cyclic olefin copolymer of the present embodiment or the fluorine-containing cyclic olefin resin composition of the present embodiment, and can be obtained, for example, by molding the fluorine-containing cyclic olefin resin composition of the present embodiment into a predetermined shape while curing it. Since the molded article of the present embodiment contains the fluorine-containing cyclic olefin copolymer or the fluorine-containing cyclic olefin resin composition of the present embodiment, the amount of hydrogen fluoride generated during heat molding can be reduced, and therefore the molded article of the present embodiment can be suitably used as an optical material. The heating temperature when molding the molded body of this embodiment is, for example, 100°C or higher and 300°C or lower, and from the viewpoint of further improving the performance balance between reducing the amount of hydrogen fluoride generated during hot molding and moldability, the heating temperature is preferably 150°C or higher, more preferably 200°C or higher, even more preferably 250°C or higher, and preferably 280°C or lower. The molded article of the present embodiment may be an optical lens.

[0032] <Optical components> The optical component of this embodiment has, for example, two or more optical lenses, and the outermost optical lens is the molded article of this embodiment. Since the optical lens of the outermost layer in an optical component is the molded body of this embodiment, the amount of hydrogen fluoride generated during heat molding can be reduced, making it suitable for use as an optical material, and ultimately reducing the effects of health hazards to the human body and corrosion, etc., on molding machines. In this embodiment, the outermost layer refers to, for example, the side of an imaging lens opposite to the side of a person observing, that is, the outermost layer on the object side. The outermost optical lens has another lens on the inside.

[0033] The number of optical lenses in the optical component is preferably three or more, more preferably four or more, and is preferably nine or less, more preferably eight or less. In the optical component of this embodiment, the lens provided inside the outermost optical lens may be a high refractive index lens, a lens with low light absorption, a lens with low light reflection, etc. Preferably, the lens includes at least one type selected from the group consisting of a high refractive index lens and a lens with low light absorption. The refractive index nd of the high refractive index lens for d-line wavelength light, measured in accordance with ASTM D542, is preferably 1.50 or more, more preferably 1.52 or more, even more preferably 1.54 or more, and is preferably 1.70 or less, more preferably 1.68 or less, even more preferably 1.65 or less.

[0034] The optical component according to the present embodiment can reduce the amount of hydrogen fluoride generated during heat molding, and therefore can be suitably used as an optical component. Optical components are components used in optical equipment, and specifically, they can be suitably used as optical component materials such as cameras, video cameras, projection televisions, projector lenses, laser printers, microlens arrays, sensor lenses, pickup lenses, prisms, fθ lenses, imaging lenses, light guide plates, and other imaging and projection optical lenses; optical fibers, optical fiber connectors, optical waveguides, and other information transmission components. Furthermore, the optical component according to the present embodiment can be suitably used as an optical component such as an in-vehicle camera lens or a camera lens for a mobile device (such as a mobile phone, a smartphone, or a tablet). Examples of in-vehicle camera lenses and camera lenses for mobile devices include a view camera lens, a sensing camera lens, a light converging lens for a head-up display, and a light diffusing lens for a head-up display.

[0035] <Lens molding method> The method for molding a lens of this embodiment includes a step of molding the fluorine-containing cyclic olefin copolymer of this embodiment or the fluorine-containing cyclic olefin resin composition of this embodiment into a lens.

[0036] <Method of producing fluorine-containing cyclic olefin copolymer> In the method for producing the fluorine-containing cyclic olefin copolymer of the present embodiment, the Hildebrand solubility parameter δ (SP value) (hereinafter, also simply referred to as “SP value”) is preferably 20 MPa 1 / 2 More than 38MPa 1 / 2 The method includes a step of precipitating the fluorine-containing cyclic olefin copolymer using a solvent selected from the group consisting of: The Hildebrand solubility parameter δ (SP value) of the solvent is preferably 20 MPa. 1 / 2 More preferably, 23MPa 1 / 2 More preferably, 25 MPa 1 / 2 More preferably, 26 MPa 1 / 2 or more, and preferably 38 MPa 1 / 2Less than or equal to 35MPa, more preferably 1 / 2 Less than 33MPa, more preferably 33MPa 1 / 2 Less than 30MPa, more preferably 30MPa 1 / 2 The following is the result. When the SP value of the solvent is equal to or more than the above lower limit, the upper limit of the molecular weight of the low molecular weight component having a weight average molecular weight of 10,000 or less that can be dissolved in the solvent can be increased without dissolving all of the fluorine-containing cyclic olefin copolymer components, and the amount of low molecular weight components that contain a high content of structural units derived from compound (X), which is thought to be a source of hydrogen fluoride in the fluorine-containing cyclic olefin copolymer, can be reduced. When the SP value of the solvent is equal to or less than the above upper limit, the low molecular weight components having a weight average molecular weight of 10,000 or less can be more easily dissolved.

[0037] When a polymerization solution of a fluorine-containing cyclic olefin copolymer is dropped into a poor solvent for the copolymer, only the copolymer component precipitates, and the copolymer can be isolated. At this time, low molecular weight components contained in the polymerization solution are removed. According to the study by the present inventors, it has been found that the low molecular weight component contains a large amount of NBF6. When a relatively large amount of the low molecular weight component is removed, the amount of hydrogen fluoride generated during heating is reduced, and therefore, it is believed that the source of hydrogen fluoride generation during heating of the fluorine-containing cyclic olefin copolymer is the low molecular weight component containing a large amount of NBF6. Therefore, it is believed that by making the solvent during the precipitation slightly closer to a good solvent, the upper limit of the molecular weight of the low molecular weight component that can be removed during precipitation can be increased, and the amount of hydrogen fluoride generated during heating can be suppressed.

[0038] The Hildebrand solubility parameter δ (SP value) is a value defined by the regular solution theory introduced by Hildebrand, and is an index that indicates the degree to which a substance dissolves in another substance. In general, the closer the SP values ​​of two components are, the more easily the two components dissolve in each other. The Hildebrand solubility parameter δ (SP value) is expressed by the following formula (2).

[0039]

number

[0040] where ΔH is the molar heat of vaporization of the solvent (Jmol ?1 ), V is the molar volume of the solvent (m 3 Mol -1 ), R is the gas constant (8.314 JK ?1 Mol ?1 ), and T is temperature (K). In this embodiment, the SP value of the solvent is the value shown in Table 1 of "Solubility Parameters: Theory and Application" by Burke, John, 1984, Book and Paper Group Annual 3: pp. 13-58.

[0041] Examples of the solvent used in the method for producing the fluorine-containing cyclic olefin copolymer of the present embodiment include the following. Acetone (SP value: 19.7MPa 1 / 2 ), 1-propanol (SP value: 24.9 MPa 1 / 2 ), ethanol (SP value: 26.2MPa 1 / 2 ), 1-butanol (SP value: 28.7 MPa 1 / 2 ), methanol (SP value: 29.7MPa 1 / 2 ), water (SP value: 48.0MPa 1 / 2 ). In addition, when a mixed solvent is used, the SP value can be calculated by the additivity rule. In this embodiment, the above-mentioned solvents can be mixed at an appropriate mixing ratio to adjust the SP value. From the viewpoint of facilitating removal of the solvent by distillation after precipitation of the fluorine-containing cyclic olefin copolymer, the boiling point of the solvent is preferably 130° C. or lower, more preferably 120° C. or lower.

[0042] The SP value of the fluorine-containing cyclic olefin copolymer is preferably 10.0 MPa. 1 / 2More preferably, 12.0MPa 1 / 2 and preferably 18.0 MPa or more. 1 / 2 Less than or equal to 16.0MPa, more preferably 1 / 2 The following is the result. The SP value of the fluorine-containing cyclic olefin copolymer can be estimated by the Hoftzyer and Krevelen method (Hansen solubility parameter δ), which will be specifically described in the Examples section.

[0043] In the method for producing the fluorine-containing cyclic olefin copolymer of the present embodiment, the step of precipitating the fluorine-containing cyclic olefin copolymer using a solvent having an SP value in the above range can be carried out, for example, by dissolving the fluorine-containing cyclic olefin copolymer of the present embodiment in another solvent that does not impair the effects of the present invention, and then dropping the copolymer into a container containing the solvent. Alternatively, the fluorine-containing cyclic olefin copolymer can be dropped into the solvent and stirred. Stirring can be carried out, for example, under conditions of 1000 rpm or more and 5000 rpm or less. Other solvents for dissolving the fluorine-containing cyclic olefin copolymer include, for example, tetrahydrofuran (THF) and toluene, and the fluorine-containing cyclic olefin copolymer can be dissolved in the solvent to a concentration of 5% by mass or more and 20% by mass or less. The time for mixing the solvent and the fluorine-containing cyclic olefin copolymer, and optionally stirring, is until the copolymer precipitates, for example, 5 minutes or more and 15 minutes or less. In addition, after the step of precipitating the fluorine-containing cyclic olefin copolymer using a solvent having an SP value in the above range, the fluorine-containing cyclic olefin copolymer may be isolated and dried by vacuum heating. There is no limitation on the isolation method, but it can be performed, for example, by suction filtration. In addition, the vacuum heating conditions are, for example, 0 Torr to 100 Torr, 70°C to 90°C, and 5 hours to 15 hours.

[0044] In the production method of the fluorine-containing cyclic olefin copolymer of the present embodiment, the preferred numerical ranges of the polystyrene-equivalent weight average molecular weight (Mw) and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) of the fluorine-containing cyclic olefin copolymer are the same as those of the above-mentioned fluorine-containing cyclic olefin copolymer. Moreover, the fluorine-containing cyclic olefin copolymer in the production method of the fluorine-containing cyclic olefin copolymer of the present embodiment preferably contains a constituent unit (x) derived from the compound (X) represented by the above general formula (A) and a constituent unit (y) derived from the compound (Y) represented by the above general formula (B), and the preferred numerical range of the molar ratio (x / y) of the constituent unit (x) derived from the compound (X) to the constituent unit (y) derived from the compound (Y) is the same as that of the above-mentioned fluorine-containing cyclic olefin copolymer. The preferred embodiments of these configurations are as described above in the section on the fluorine-containing cyclic olefin copolymer, and therefore will not be described here.

[0045] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements that do not impair the effects of the present invention are included in the present invention. EXAMPLES

[0046] Hereinafter, the present embodiment will be described in detail with reference to examples, etc. However, the present embodiment is not limited to the description of these examples.

[0047] <Synthesis of fluorine-containing cyclic olefin copolymer> The fluorine-containing cyclic olefin copolymer 1 used in each of the Examples and Comparative Examples was synthesized as follows. In a 5 L autoclave equipped with a magnetic stirrer under a nitrogen atmosphere, 495 g (2.3 mol) of 5,6-difluoro-5-fluoro-6-(trifluoromethyl)bicyclo(2.2.1)hept-2-ene (NBF6) as compound (X) and 8,8,9-trifluoro-9-trifluoromethyl-tetracyclo[4.4.0.1]hept-2-ene (Y) were added. 2,5 .1 7,10 970 g (3.4 mol) of 1-dodecene (TDF6) and 44.0 g (0.52 mol) of 1-hexene were dissolved in 1.5 kg of tetrahydrofuran (hereinafter referred to as THF) and stirred. i 2C6H3)(CHCMe2Ph)(OBu t 630 mg (1.15 mmol) of 2 was added and reacted at 70° C. for 48 hours. Then, 248 mg (3.4 mmol) of n-butylaldehyde was added and cooled to obtain 3.0 kg of a ring-opening metathesis polymerized polymer solution. 1 The polymerization rate of the polymer obtained by H-NMR was 100%, Mw by GPC was 66,000, and Mw / Mn was 2.8. The obtained polymer solution was diluted with 3.0 kg of THF, and palladium alumina was added to this polymer solution to carry out a hydrogenation reaction of the olefin portion of the polymer at 160°C, thereby obtaining a THF solution of fluorine-containing cyclic olefin copolymer 1. 1 The hydrogenation rate of the obtained polymer was 100% by H-NMR. The palladium alumina was removed from the THF solution of the obtained copolymer by filtration with a 0.1 μm filter. The obtained fluorine-containing cyclic olefin copolymer 1 19 F-NMR analysis revealed that the molar ratio of structural unit (x) to structural unit (y) was x / y=38.9 / 61.1, and the fluorine content was 44.1% by mass.

[0048] [Molar ratio of structural unit (x) to structural unit (y) and fluorine content (mass%) of fluorine-containing cyclic olefin copolymer 1] The molar ratio x / y of the structural unit (x) to the structural unit (y) of the fluorine-containing cyclic olefin copolymer 1 and the content of fluorine atoms are as follows:19 Measurements were performed by F-NMR. Using a JEOL ECA500 nuclear magnetic resonance spectrometer, 19 F-NMR spectrum was measured, and the molar ratios [A] and [B] of the structural unit (x) and the structural unit (y) were calculated using the integral value of fluorine derived from -CF at δ = -150 to -200 ppm, -CF2 at δ = -100 to -150 ppm, or -CF3 at δ = -60 to -100 ppm of the fluorine-containing cyclic olefin copolymer 1, with CFCl3 at δ = 0.00 ppm as the reference signal. In addition, the fluorine content (mass%) was calculated from the following formula (4). Measurement solvent: Deuterated tetrahydrofuran Sample concentration: Approximately 5% ·Measurement temperature: Room temperature (20℃) Number of times: 256 Base peak: CFCl3 set to 0.00 ppm automatically by the instrument Equation (4): Fluorine atom content (mass%) = {(F(A)n × 19 × [A]) / (F(A)w × [A] + F(B)w × [B]) + (F(B)n × 19 × [B]) / (F(A)w × [A] + F(B)w × [B])} × 100 (4) In formula (4), F(A)n represents the number of fluorine atoms in the structural unit represented by general formula (A), F(B)n represents the number of fluorine atoms in the structural unit represented by general formula (B), F(A)w represents the formula weight of the structural unit represented by general formula (A), and F(B)w represents the formula weight of the structural unit represented by general formula (B).

[0049] Example 1 600 g of methanol was placed in a 1 L homogenizer, and 60 g of the THF solution of fluorine-containing cyclic olefin copolymer 1 obtained above with a solution concentration of 10% by mass was dropped therein using a Pasteur pipette, and the mixture was stirred at room temperature (20°C) and a rotation speed of 3,000 rpm to precipitate fluorine-containing cyclic olefin copolymer 1. The precipitated fluorine-containing cyclic olefin copolymer 1 was isolated by suction filtration, and then dried at 80°C for 10 hours in a vacuum oven.

[0050] Example 2 The same procedure as in Example 1 was carried out, except that methanol was changed to a mixed solvent of acetone / methanol = 30 / 70 (mass ratio).

[0051] Comparative Example 1 The same procedure as in Example 1 was carried out, except that methanol was changed to a mixed solvent of water / methanol=50 / 50 (mass ratio).

[0052] [Hildebrand solubility parameter δ (SP value) of the solvent] The Hildebrand solubility parameter δ (SP value) of the solvent used in each example was taken from Table 1 in "Solubility Parameters: Theory and Application," Book and Paper Group Annual 3:13-58, by Burke, John, 1984. In the case of a mixed solvent, the SP value was calculated by multiplying the SP value of each solvent by its mass ratio and adding the resulting values. As an example, in the case of acetone / methanol=30 / 70 (mass ratio), the SP value is 19.7×30 / 100+29.7×70 / 100=26.7.

[0053] [Solubility parameter δ (SP value) of fluorine-containing cyclic olefin copolymer 1] The solubility parameter δ (SP value) of the fluorine-containing cyclic olefin copolymer 1 used in the examples and comparative examples was estimated by the Hoftzyer and Krevelen method (Equation 3.1, Equation 3.2, Equation 3.3) as the Hansen solubility parameter (δd: dispersion term, δp: polar term, δh: hydrogen bond term), and further converted to the Hildebrand solubility parameter δ using Equation (3.4). δd = ΣEdi / Vm (3.1) δp = (ΣEpi 2 ) 1 / 2 / Vm...(3.2) δh=(ΣEhi / Vm) 1 / 2 (3.3) δ 2 = δd 2 +δp 2 +δh 2(3.4) Here, Ed in formula (3.1) is the cohesive energy related to the dispersion term of each substituent, Ep in formula (3.2) is the cohesive energy related to the polar term of each substituent, Eh in formula (3.3) is the cohesive energy related to the hydrogen bond term of each substituent, and Vm in the above formulas (3.1) to (3.3) is the molecular volume. δd, δp, and δh have unique values ​​depending on the substituent and basic skeleton. The SP values ​​of the NBF6 and TDF6 monomers were calculated by calculating the δd, δp and δh values ​​for the methylene group, difluoromethylene group, tertiary carbon, quaternary carbon and fluorine group, and the δ value, i.e., the SP value, was calculated from formula (3.4). The results are shown below. SP value of NBF6: 14.8 (MPa) 1 / 2 SP value of TDF6: 13.7 (MPa) 1 / 2 Using the SP values ​​of the above NBF6 and TDF6 monomers and the molar ratio of NBF6 and TDF6 in fluorine-containing cyclic olefin copolymer 1 (40 / 60), the SP value of fluorine-containing cyclic olefin copolymer 1 was calculated as follows. SP value of fluorine-containing cyclic olefin copolymer 1 = 14.8 (MPa) 1 / 2 ×0.4+13.7(MPa) 1 / 2 ×0.6=14.1(MPa) 1 / 2

[0054] [Weight average molecular weight (Mw), ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn), and content of components with a weight average molecular weight (Mw) of 10,000 or less] For the fluorine-containing cyclic olefin copolymer 1 obtained after precipitation in each example, the weight average molecular weight (Mw), number average molecular weight (Mn) and content of components with a weight average molecular weight (Mw) of 10,000 or less of the polymer dissolved in THF were measured using gel permeation chromatography (GPC) under the following conditions: weight average molecular weight (Mw) = 1.32 × 10 of a polystyrene standard (manufactured by Resonac Holdings, Inc., product name: Shodex STANDARD SM-105) 3, 2.78×10 3 , 1.07×10 4 , 2.20×10 4 , 6.60×10 4 , 1.56×10 5 , 4.60×10 5 The molecular weight was calibrated and measured using the seven samples. (Mw / Mn) was calculated from the obtained weight average molecular weight (Mw) and number average molecular weight (Mn). Using the obtained weight average molecular weight (Mw) result, the total amount of components having a weight average molecular weight (Mw) of 10,000 or less was divided by the mass of the fluorine-containing cyclic olefin copolymer used in the measurement to calculate the content (mass%) of components having a weight average molecular weight (Mw) of 10,000 or less. The results are shown in Table 1. Detector: JASCO 830-RI and 875-UV Column: Shodex k-806M, 804, 803, 802.5 (manufactured by Resonac Holdings, Inc.) Solvent: Tetrahydrofuran Flow rate: 1.0mL / min Column temperature: 40℃ Concentration: 7.5mg / mL Injection volume: 100μL

[0055] [Amount of hydrogen fluoride generated] 0.1 g of the fluorine-containing cyclic olefin copolymer sample obtained in each example after precipitation was placed in a platinum boat and inserted into a quartz tube heated to 250°C while passing nitrogen gas at a flow rate of 0.2 L / min using a thermal gas collector (horizontal heating furnace). The sample was heated at 250°C for 30 minutes in the heating furnace, and the hydrogen fluoride generated during this process was collected and dissolved in 5 mL of absorption liquid (ultrapure water) in an impinger. The hydrogen fluoride dissolved in the absorption liquid was converted to hydrogen ions (H + ) and fluorine ion (F - ), the amount of fluorine ions was measured using an ion chromatograph under the following conditions.

[0056] The measurement conditions for the ion chromatography are shown below. (Measurement conditions) Measurement equipment: Ion chromatograph ICS-5000 (Thermo Fisher Scientific Co., Ltd.) Detector: Electrical conductivity detector The absorbent obtained above was transferred to a measuring flask, and ultrapure water was added to prepare a sample solution for analysis. The solution was passed through a membrane filter to remove insoluble matter, and then subjected to measurement. The fluoride ion content in the absorbent was calculated using the above device. The amount of fluoride ion generated was calculated using a calibration curve created using a standard substance (fluorine compound).

[0057] The amount of hydrogen fluoride generated (ppm) was calculated from the obtained amount of fluoride ions according to the following formula (1). Amount of hydrogen fluoride generated (ppm) = (amount of fluoride ions generated (mg)) ÷ (total mass of copolymer (kg)) × (20 / 19) (1) Here, the number 19 represents the atomic weight of fluorine, and the number 20 represents the molecular weight of hydrogen fluoride.

[0058] [Table 1]

Claims

1. A fluorine-containing cyclic olefin copolymer, The fluorine-containing cyclic olefin copolymer has a content of a component having a weight average molecular weight (Mw) of 10,000 or less as measured by gel permeation chromatography, which is 10.0 mass% or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100 mass%.

2. 2. The fluorine-containing cyclic olefin copolymer according to claim 1, which has an amount of hydrogen fluoride generated of less than 60 ppm as measured by ion chromatography in accordance with the following <Amount of Hydrogen Fluoride Generated>. <Amount of hydrogen fluoride generated> (1) 0.1 g of the fluorine-containing cyclic olefin copolymer is placed in a platinum boat and inserted into a quartz tube in a heating furnace heated to 250° C. while passing nitrogen gas at a rate of 0.2 L / min. (2) The fluorine-containing cyclic olefin copolymer is heated in a heating furnace at 250° C. for 30 minutes, and the hydrogen fluoride generated during the heating is dissolved in 5 mL of ultrapure water in an impinger. (3) The hydrogen fluoride dissolved in the ultrapure water is converted into hydrogen ions (H + ) and fluorine ion (F - ) and the amount of fluorine ions generated is measured using an ion chromatograph. (4) The amount of hydrogen fluoride generated is calculated according to the following formula (1). Amount of hydrogen fluoride generated (ppm)=(amount of fluoride ions generated (mg))÷(total mass of copolymer (kg))×(20 / 19) (1) Here, the number 19 represents the atomic weight of fluorine, and the number 20 represents the molecular weight of hydrogen fluoride.

3. 3. The fluorine-containing cyclic olefin copolymer according to claim 1, which has a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of 50,000 or more and 100,000 or less.

4. 4. The fluorine-containing cyclic olefin copolymer according to claim 1, wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) in terms of polystyrene measured by gel permeation chromatography (GPC) is 2.8 or less.

5. A structural unit (x) derived from a compound (X) represented by the following general formula (A), The fluorine-containing cyclic olefin copolymer according to any one of claims 1 to 4, which contains a structural unit (y) derived from a compound (Y) represented by the following general formula (B): [Formula 1] (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a group that does not contain fluorine, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [Case 2] (In the above formula (B), R 5 ~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a group that does not contain fluorine, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

6. In the general formula (A), R 1 ~R 4 at least one of the groups is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms; In the general formula (B), R 5 ~R 8 6. The fluorine-containing cyclic olefin copolymer according to claim 5, wherein at least one of the above is fluorine or a fluorine-containing alkyl group having 1 to 4 carbon atoms.

7. 7. The fluorine-containing cyclic olefin copolymer according to claim 5 or 6, wherein the molar ratio (x / y) of the structural unit (x) to the structural unit (y) in the fluorine-containing cyclic olefin copolymer is 0.25 or more and 4.0 or less.

8. The fluorine-containing cyclic olefin copolymer according to any one of claims 5 to 7, wherein the total content of the structural unit (x) and the structural unit (y) in the fluorine-containing cyclic olefin copolymer is 50% by mass or more and 100% by mass or less, when the entire fluorine-containing cyclic olefin copolymer is taken as 100% by mass.

9. A fluorine-containing cyclic olefin resin composition comprising the fluorine-containing cyclic olefin copolymer according to any one of claims 1 to 8.

10. A molded article comprising the fluorine-containing cyclic olefin copolymer according to any one of claims 1 to 8 or the fluorine-containing cyclic olefin resin composition according to claim 9.

11. The molded article according to claim 10, which is an optical lens.

12. An optical component having two or more optical lenses, An optical component, wherein an optical lens in an outermost layer of the optical component is the molded article according to claim 11.

13. A method for producing a fluorine-containing cyclic olefin copolymer, comprising the steps of: Hildebrand solubility parameter δ (SP value) is 20 MPa 1/238MPa or more 1/2 A method for producing a fluorine-containing cyclic olefin copolymer, comprising the step of precipitating the fluorine-containing cyclic olefin copolymer using a solvent selected from the group consisting of:

14. The method for producing a fluorine-containing cyclic olefin copolymer according to claim 13, wherein the fluorine-containing cyclic olefin copolymer has a weight average molecular weight (Mw) of 50,000 or more and 100,000 or less in terms of polystyrene as measured by gel permeation chromatography (GPC).

15. The method for producing a fluorine-containing cyclic olefin copolymer according to claim 13 or 14, wherein the ratio (Mw / Mn) of the weight average molecular weight (Mw) and the number average molecular weight (Mn) of the fluorine-containing cyclic olefin copolymer in terms of polystyrene measured by gel permeation chromatography (GPC) is 2.8 or less.

16. The method for producing a fluorine-containing cyclic olefin copolymer according to any one of claims 13 to 15, wherein the fluorine-containing cyclic olefin copolymer comprises a structural unit (x) derived from a compound (X) represented by the following general formula (A) and a structural unit (y) derived from a compound (Y) represented by the following general formula (B): [C3] (In the above formula (A), R 1 ~R 4 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 1 ~R 4 When R is a group that does not contain fluorine, 1 ~R 4 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 1 ~R 4 may be bonded to each other to form a ring structure. [C4] (In the above formula (B), R 5~R 8 at least one of R is fluorine, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a fluorine-containing alkoxy group having 1 to 10 carbon atoms, or a fluorine-containing alkoxyalkyl group having 2 to 10 carbon atoms; 5 ~R 8 When R is a group that does not contain fluorine, 5 ~R 8 is selected from hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, or an alkoxyalkyl group having 2 to 10 carbon atoms; R 5 ~R 8 may be bonded to each other to form a ring structure.

17. The method for producing a fluorine-containing cyclic olefin copolymer according to any one of claims 13 to 16, wherein the fluorine-containing cyclic olefin copolymer contains a component having a weight average molecular weight (Mw) of 10,000 or less as measured by gel permeation chromatography, and the component accounts for 10.0 mass% or less of the fluorine-containing cyclic olefin copolymer as a whole, taken as 100 mass%.

18. A method for producing a lens molding, comprising a step of molding the fluorine-containing cyclic olefin copolymer according to any one of claims 1 to 8 or the fluorine-containing cyclic olefin resin composition according to claim 9 into a lens.

Citation Information