Catalyst group for producing p-xylene, method for producing catalyst group for producing p-xylene, and method for producing p-xylene

A catalyst system combining chromium-zinc, silicon-coated H-ZSM-5, and iron-manganese oxides efficiently produces para-xylene from carbon monoxide and hydrogen, addressing inefficiencies in existing methods and enhancing productivity.

JP2024137459APending Publication Date: 2024-10-07NIPPON STEEL CORPORATION +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023048987
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Existing catalysts and production methods for producing para-xylene from carbon monoxide and hydrogen are inefficient, and there is a need for improved catalysts that can enhance the productivity of para-xylene while reducing carbon dioxide emissions.

Method used

A catalyst system comprising a binary composite oxide of chromium and zinc, H-ZSM-5 zeolite coated with amorphous silicon, and a binary composite oxide of iron and manganese is used, with the third catalyst placed upstream to promote carbon-carbon bond formation, and the first and second catalysts mixed and granulated for efficient para-xylene synthesis.

Benefits of technology

The catalyst system significantly enhances para-xylene productivity by promoting alkenes formation and selective conversion to para-xylene, achieving high yields and reducing unwanted side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137459000002
    Figure 2024137459000002
  • Figure 2024137459000003
    Figure 2024137459000003
  • Figure 2024137459000004
    Figure 2024137459000004
Patent Text Reader

Abstract

To provide a catalyst group for producing p-xylene capable of efficiently producing p-xylene with carbon mono-oxide and hydrogen as a raw material, a method for producing a catalyst group for producing the p-xylene and a method for producing the p-xylene.SOLUTION: The present invention relates to a catalyst group for producing p-xylene, the catalyst group comprising a first catalyst containing a binary composite oxide of chromium and zinc, a second catalyst containing H-ZSM-5 zeolite the surface of which is coated with an oxide containing amorphous silicon, and a third catalyst containing a binary composite oxide of iron and manganese, wherein at least the first catalyst and the second catalyst among the first catalyst, the second catalyst, and the third catalyst are present as a granulated mixture, and a method for producing the catalyst group and a method for producing p-xylene using the catalyst group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a catalyst group for producing paraxylene, a method for producing the catalyst group for producing paraxylene, and a method for producing paraxylene. [Background technology]

[0002] In recent years, interest in global warming has been growing. The Conference of the Parties (COP), which discusses an international framework for reducing greenhouse gas emissions, aims to keep the increase in average temperature from pre-industrial levels well below 2°C as a global long-term common goal, with the goal of suppressing the peak of emissions as soon as possible and rapidly reducing emissions in accordance with the latest science. The COP21 Paris Agreement states that all countries should strive to formulate and submit long-term low greenhouse gas emission development strategies, and Japan has formulated a long-term goal of reducing greenhouse gas emissions by 80% by 2050. Carbon dioxide is estimated to have the greatest impact among greenhouse gases emitted artificially, and countermeasures to reduce carbon dioxide emissions are being vigorously developed in various places. As one of the countermeasures, several attempts have been proposed to convert emitted carbon dioxide into useful substances, but a large amount of energy is required to convert carbon dioxide into other substances, and there is a need to develop effective catalysts to promote the reaction.

[0003] Furthermore, to make this technology useful for reducing carbon dioxide emissions, it is necessary to produce useful substances that are in high demand. Paraxylene is a compound that is useful as a raw material for the general-purpose resin polyethylene terephthalate (PET). If it were possible to efficiently produce such a compound from carbon dioxide and hydrogen, this could be a useful measure for reducing carbon dioxide emissions.

[0004] Conventionally, paraxylene has been produced by reforming crude oil and naphtha. However, the conventional production method had a problem of emitting large amounts of carbon dioxide. Therefore, a technology for producing paraxylene using a mixed gas of carbon monoxide and hydrogen, so-called synthesis gas, as a raw material has been proposed (for example, Non-Patent Document 1). If this technology is established, in addition to suppressing carbon dioxide emissions, it will also be possible to use synthesis gas derived from biomass, etc., and will become a method for synthesizing useful chemical products with less environmental impact. The technology disclosed in Non-Patent Document 1 uses a catalyst with a ZnCr2O4 spinel structure as a catalyst for synthesizing methanol from synthesis gas, and uses a catalyst in which zinc-doped H-ZSM-5 zeolite is coated with silicalite-1 as a catalyst for synthesizing paraxylene from methanol. It is disclosed that by introducing synthesis gas into a system in which these catalysts are present, it is possible to synthesize paraxylene in one stage. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Peipei Zhang et al., Chemical Science, The Royal Society of Chemistry, October 2017, Volume 8, Pages 7941-7946 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in order to efficiently produce para-xylene using carbon monoxide and hydrogen as raw materials, there is room for improvement in the catalyst and the production method.

[0007] Therefore, the present disclosure has been made in consideration of the above problems, and an object of the present disclosure is to provide a catalyst group for producing paraxylene that can efficiently produce paraxylene using carbon monoxide and hydrogen as raw materials, a method for producing the catalyst group for producing paraxylene, and a method for producing paraxylene. [Means for solving the problem]

[0008] The gist of the present disclosure is as follows.

[0009] <1> A first catalyst including a binary composite oxide of chromium and zinc; a second catalyst comprising an H-ZSM-5 zeolite having a surface coated with an amorphous silicon-containing oxide; a third catalyst comprising a binary composite oxide of iron and manganese; A catalyst group for producing paraxylene, comprising the first catalyst, the second catalyst, and the third catalyst, wherein at least the first catalyst and the second catalyst are present as a mixed granule. <2> The first catalyst contains 30% by mass or more and 70% by mass or less of chromium and 30% by mass or more and 70% by mass or less of zinc relative to the total amount of metals contained in the first catalyst, and The third catalyst contains 90% by mass or more and 99% by mass or less of iron and 1% by mass or more and 10% by mass or less of manganese based on the total amount of metals contained in the third catalyst. <1> The catalyst group for producing paraxylene according to claim 1. <3> The second catalyst is contained in an amount of 10% by mass or more and 1000% by mass or less relative to the first catalyst, and The third catalyst is contained in an amount of 0.1 mass% or more based on the total amount of the first catalyst, the second catalyst, and the third catalyst. <1> or <2> The catalyst group for producing paraxylene according to claim 1. <4> Carbon monoxide and hydrogen <1> ~ <3> 2. A method for producing paraxylene, comprising: a step of synthesizing paraxylene by contacting a catalyst for producing paraxylene according to any one of the above items 1 to 11 with the catalyst for producing paraxylene. <5> The third catalyst is disposed on the upstream side with respect to a flow direction of the carbon monoxide and the hydrogen, and the granules obtained by mixing the first catalyst and the second catalyst are disposed on the downstream side, and the carbon monoxide and the hydrogen are contacted with the third catalyst, and the resulting gas is contacted with the granules to synthesize the paraxylene. <4> The method for producing paraxylene according to claim 1 . <6> <1> ~ <3> A method for producing a catalyst group for producing paraxylene according to any one of the above, obtaining a composite hydroxide containing chromium and zinc by a coprecipitation method, and drying and / or calcining the composite hydroxide containing chromium and zinc to obtain the first catalyst; performing hydrothermal synthesis or heating in the presence of a silicon compound and an H-ZSM-5 zeolite to obtain the second catalyst comprising an H-ZSM-5 zeolite the surface of which is coated with an amorphous silicon-containing oxide; obtaining a composite hydroxide containing iron and manganese by a coprecipitation method, and drying and / or calcining the composite hydroxide containing iron and manganese to obtain the third catalyst; A step of mixing at least the first catalyst and the second catalyst among the first catalyst, the second catalyst, and the third catalyst, and granulating the mixture to obtain the granules; The present invention relates to a method for producing a catalyst group for producing paraxylene, comprising the steps of: Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a catalyst group for producing paraxylene that can efficiently produce paraxylene using carbon monoxide and hydrogen as raw materials, a method for producing the catalyst group for producing paraxylene, and a method for producing paraxylene. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a diagram illustrating an example of the configuration of a catalyst group for producing paraxylene according to the present disclosure. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a catalyst group for producing paraxylene in an example. [Diagram 3] FIG. 2 is a diagram showing a schematic configuration of a catalyst group for producing paraxylene in a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment that is an example of the present disclosure will be described. In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. With respect to the contents of elements contained in the catalyst, "%" means "mass %" unless otherwise specified. In the numerical ranges described in stages in the present disclosure, the upper limit of a certain numerical range may be replaced with the upper limit of another numerical range described in stages or with a value shown in an example. Also, in the numerical ranges described in stages in the present disclosure, the lower limit of a certain numerical range may be replaced with the lower limit of another numerical range described in stages or with a value shown in an example. The term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.

[0013] In the course of intensive research to solve the above problems, the inventors of the present disclosure have concluded that adding a new FeMn composite oxide as a third catalyst to the conventionally used first catalyst having a ZnCr2O4 spinel structure and the second catalyst consisting of H-ZSM-5 zeolite coated with an oxide containing amorphous silicon might increase the productivity of alkenes, which are precursors of paraxylene, and also increase the final productivity of paraxylene production. As a result of intensive research, they have found that high productivity of paraxylene can be achieved by mixing the first catalyst and the second catalyst into a granule and then adding the third catalyst.

[0014] Specifically, for example, a reactor is filled with a mixture of a granulated product of a first catalyst having a ZnCr2O4 spinel structure, a second catalyst in which H-ZSM-5 zeolite is coated with an oxide containing amorphous silicon, and a third catalyst in which FeMn composite oxide is used to produce paraxylene from carbon monoxide and hydrogen. Conventionally, only the first catalyst having a ZnCr2O4 spinel structure and the second catalyst in which H-ZSM-5 zeolite is coated with an oxide containing amorphous silicon have been used, but the inventors of the present disclosure have found that the addition of an FeMn composite oxide promotes the carbon-carbon bond formation reaction, promotes the production of alkenes, which are precursors of paraxylene, and ultimately increases the productivity of paraxylene, leading to the invention of the present disclosure.

[0015] As a result of further investigation based on the knowledge obtained from the above investigation, the inventors of the present disclosure have also found that paraxylene productivity can be further improved by using a reactor in which an FeMn composite oxide as a third catalyst is packed in an upper layer (upstream side) with respect to the flow of carbon monoxide and hydrogen, and a catalyst in which the first catalyst and the second catalyst are physically mixed is packed in a lower layer (downstream side). In this specification, with regard to the arrangement of each catalyst, the upstream side may be referred to as the "upper layer" or "upper stage" and the downstream side may be referred to as the "lower layer" or "lower stage" with respect to the flow direction of the gases (carbon monoxide and hydrogen) that are the raw materials for the synthesis of para-xylene.

[0016] Preferred embodiments of the present disclosure will be described in detail below.

[0017] <1. Catalysts for paraxylene production> First, preferred embodiments of the catalyst group for producing para-xylene according to the present disclosure will be described. The catalyst group for producing paraxylene according to the present disclosure catalyzes a synthesis reaction of a hydrocarbon compound, particularly paraxylene, using carbon monoxide and hydrogen as raw materials. The catalyst group for producing paraxylene according to the present disclosure includes a first catalyst containing a binary composite oxide of chromium and zinc, a second catalyst containing H-ZSM-5 zeolite whose surface is coated with an oxide containing amorphous silicon, and a third catalyst containing a binary composite oxide of iron and manganese. Among the first catalyst, the second catalyst, and the third catalyst, at least the first catalyst and the second catalyst exist as a mixed granule.

[0018] The first catalyst, containing a binary oxide of chromium and zinc, catalyzes the conversion of carbon monoxide and hydrogen to methanol, while the second catalyst, containing an H-ZSM-5 zeolite coated with an amorphous silicon-containing oxide, catalyzes the conversion of methanol to paraxylene, and the third catalyst, containing a binary oxide of iron and manganese, catalyzes the carbon-carbon formation reaction from carbon monoxide and hydrogen to produce alkenes, which are precursors to methanol as well as paraxylene.

[0019] In this specification, the term "catalyst group" means a combination of three catalysts with different functions, i.e., the first catalyst, the second catalyst, and the third catalyst, and the catalyst group for producing paraxylene according to the present disclosure exists as a granule in which the first catalyst and the second catalyst are mixed, but the third catalyst may exist as a granule mixed with the first catalyst and the second catalyst, or may exist separately from the granule in which the first catalyst and the second catalyst are mixed. In addition, "granule", for example, "granule in which the first catalyst and the second catalyst are mixed" means that the first catalyst and the second catalyst are mixed and present in one particle.

[0020] FIG. 1 is a schematic diagram showing an example of the form of the catalyst group for producing paraxylene according to the present disclosure, in which a first catalyst 10, a second catalyst 20, and a third catalyst 30 are present as a mixed granule. FIG. 2 is a schematic diagram showing three forms of the catalyst group for producing paraxylene. In form (a) of FIG. 2, a granule in which the first catalyst 10, the second catalyst 20, and the third catalyst 30 are mixed is disposed in a reactor 40. In forms (b) and (c) of FIG. 2, the third catalyst is present as a separate entity from the granule in which the first catalyst and the second catalyst are mixed. As shown in FIG. 2(b), the third catalyst 30 may be present mixed with the granules in which the first catalyst 10 and the second catalyst 20 are mixed, or as shown in FIG. 2(c), the third catalyst may be present physically separated from the granules in which the first catalyst 10 and the second catalyst 20 are mixed without being mixed.

[0021] 3(d) and (e), the first catalyst 10 and the second catalyst 20 are not present as a mixed granule. In these forms, the yield of paraxylene is not improved, and they are not included in the group of catalysts for producing paraxylene according to the present disclosure.

[0022] (1.1. First Catalyst) As described above, the first catalyst is a binary composite oxide of chromium and zinc, which catalyzes the conversion of carbon monoxide and hydrogen to methanol. Here, since the binary composite oxide of chromium and zinc has oxygen vacancies, carbon monoxide is easily adsorbed onto the surface of the binary composite oxide of chromium and zinc, and the carbon monoxide adsorbed on the binary composite oxide reacts with hydrogen efficiently to produce methanol efficiently.

[0023] The binary composite oxide of chromium and zinc contained in the first catalyst is exemplified by ZnCr2O4, which is preferred because it has good catalytic activity and is stable in the environment in which the catalytic reaction occurs.

[0024] The first catalyst is mainly composed of a binary composite oxide of chromium and zinc, but may also contain other compounds resulting from the production of the first catalyst or compounds derived from the support used to support the first catalyst. The first catalyst preferably contains 30% to 70% by mass of chromium, more preferably 40% to 60% by mass of chromium, and more preferably 30% to 70% by mass of zinc, more preferably 50% to 60% by mass of zinc.

[0025] The metal mass concentration in the first catalyst can be quantified by a scanning high-frequency inductively coupled plasma spectrometry (ICP-AES method). Specifically, after crushing the sample, an alkali melting agent (e.g., sodium carbonate, sodium borate, etc.) is added and the sample is heated and melted in a platinum crucible, and after cooling, the entire amount is dissolved in a hydrochloric acid solution under heating. When the solution is injected into an ICP analyzer, the sample solution is atomized and thermally excited in the high-temperature plasma state inside the device, and when this returns to the ground state, an emission spectrum with wavelengths specific to the elements is generated, and the type and amount of contained elements can be qualitatively and quantitatively determined from the emission wavelength and intensity. The mass concentration of each metal can be calculated from the following formula. Chromium concentration [%] = (amount of chromium in the first catalyst) / (amount of chromium in the first catalyst + amount of zinc in the first catalyst) x 100 [%] Zinc concentration [%] = (amount of zinc in the first catalyst) / (amount of chromium in the first catalyst + amount of zinc in the first catalyst) × 100 [%]

[0026] The form of the first catalyst is not particularly limited, and may be, for example, granular or layered (membrane). The first catalyst is usually porous, and therefore has pores for carrying out the reaction, and has a relatively large specific surface area. The specific surface area and other properties of the first catalyst when it is porous will be described below.

[0027] The specific surface area of ​​the first catalyst can be increased by decreasing the pore size or increasing the pore volume. In other words, the pore size and pore volume are related to the specific surface area of ​​the first catalyst. Generally, a larger specific surface area is preferable, but if one tries to maintain the pore size and pore volume within an appropriate range, an extremely large specific surface area cannot be obtained.

[0028] The specific surface area of ​​the first catalyst is not particularly limited, but is, for example, 3 m 2 / g or more 500m 2 / g or less, preferably 10m 2 / g or more 100m 2 / g or less. This allows sufficient supply of active sites for the reaction of hydrogen and carbon monoxide. In addition, by having a specific surface area of ​​less than the above upper limit, the pore size becomes excessively small, which can prevent a difference in the gas diffusion speed between carbon monoxide and hydrogen in the pores and a difference in the partial pressure of carbon monoxide and that of hydrogen in the first catalyst. As a result, hydrogen and carbon monoxide are efficiently converted to methanol. The specific surface area can be measured by the BET method.

[0029] The average pore size of the first catalyst is not particularly limited, but is, for example, 0.5 nm to 100 nm, preferably 2 nm to 30 nm. This prevents the difference in gas diffusion speed between carbon monoxide and hydrogen in the pores, and allows the specific surface area of ​​the first catalyst to be increased, making it possible to supply a sufficient number of active sites. As a result, hydrogen and carbon monoxide are efficiently converted into methanol.

[0030] The pore size can be determined by analyzing data obtained from the gas adsorption method (BET specific surface area measurement) using the BJH (Barrett-Joyner-Halenda) method. For example, N2 molecules can be used as the adsorption gas used in the measurement, and the specific surface area can be measured from the amount of gas molecules adsorbed and the weight of the measurement sample. Furthermore, by performing this measurement at a temperature at which the adsorbed molecules are liquefied, the pore volume and pore size can be measured by measuring the liquid adsorbed molecules filled in the pores.

[0031] The pore volume of the first catalyst is not particularly limited and is, for example, 0.1 cc / g or more and 5 cc / g or less, preferably 0.5 cc / g or more and 2 cc / g or less.

[0032] The pore volume can be determined by mercury intrusion porosimetry. If mercury intrusion porosimetry is not available, it can be measured by water titration. The average pore size can be measured by mercury intrusion porosimetry using a mercury porosimeter. If mercury intrusion porosimetry is not available, it can be measured by gas adsorption.

[0033] In addition, when the first catalyst is granular, the average particle size of the first catalyst is, for example, 1 μm to 800 μm, preferably 10 μm to 200 μm. This accelerates the mass transfer between the first catalyst and the second catalyst, and reduces the flow resistance of the raw material gas (reduced pressure loss). In this specification, the term "average particle size" refers to the volume-based 50% particle size (D50) measured by a wet laser diffraction / scattering method. In addition, when it is difficult to measure by the laser diffraction / scattering method due to poor dispersibility or other reasons, a method such as an image imaging method can be applied.

[0034] (1.2. Second Catalyst) As described above, the second catalyst includes H-ZSM-5 zeolite whose surface is coated with an amorphous silicon-containing oxide. The second catalyst catalyzes the conversion of methanol produced through the first catalyst to para-xylene. Here, in the second catalyst, the H-ZSM-5 zeolite catalyzes the selective conversion of mainly methanol to para-xylene, while the amorphous silicon-containing oxide coated on the surface of the H-ZSM-5 zeolite prevents the isomerization of para-xylene.

[0035] The second catalyst is mainly composed of H-ZSM-5 zeolite whose surface is covered with an oxide containing amorphous silicon. Meanwhile, the oxide containing amorphous silicon in the second catalyst may contain trace amounts (e.g., 5% or less) of other elements resulting from the production of the second catalyst or elements derived from the carrier used to support the second catalyst. Examples of other elements include aluminum and magnesium.

[0036] The amorphous nature of oxides containing silicon is determined by observing a broad X-ray diffraction image. If the oxide contains crystalline silicon, the SiO2 peak intensity appears high, but if it is amorphous, it appears as a weak peak, making it possible to distinguish between them. Furthermore, the crystallinity and non-crystallinity can also be determined by the electron diffraction pattern obtained by a transmission electron microscope. In the case of crystalline oxides, the structure is periodic, so strong diffraction is obtained and a clear electron diffraction pattern is obtained, but in the case of amorphous oxides, the structure is not periodic, so the diffraction is weak and a halo image is obtained. Hereinafter, amorphous SiO2 may be simply referred to as "SiO2".

[0037] H-ZSM-5 is synthesized from a silicon compound and an aluminum compound. Meanwhile, the silicon compound and the aluminum compound may contain trace amounts (e.g., 5% or less) of other elements due to the production process. Potential other elements include magnesium.

[0038] Specifically, there are many acid sites in the pores of H-ZSM-5 zeolite, and these acid sites are used as active sites to form aromatic rings (benzene rings) from methanol via dimethyl ether and light olefins. Furthermore, the benzene rings are methylated at their 1,4 positions by further methanol in the pores of H-ZSM-5 zeolite through the Friedel-Crafts reaction. Here, the pores of H-ZSM-5 zeolite have a pore size that allows paraxylene to pass through, while ortho-xylene and meta-xylene cannot. Therefore, paraxylene is preferentially produced due to the so-called spatial confinement effect. The spatial confinement effect refers to the phenomenon and effect in which a reaction proceeds in a certain space, and the reaction is controlled or confined (restricted) depending on the shape and size of the space, and a specific reaction or a reaction at a specific site proceeds preferentially.

[0039] Furthermore, the generated paraxylene can remain stable within the pores of the H-ZSM-5 zeolite, which prevents the generated paraxylene from being isomerized into meta-xylene and ortho-xylene.

[0040] On the other hand, on the outer surface of H-ZSM-5 zeolite excluding the pores, there is no spatial restriction, so the spatial confinement effect does not occur. Therefore, there is a risk of ortho-xylene and meta-xylene being generated at the acid points on the outer surface. In contrast, in the present disclosure, the surface (outer surface) of H-ZSM-5 zeolite is covered with an oxide containing amorphous silicon.

[0041] The oxide containing amorphous silicon is an oxide whose main component is silica (preferably 50% or more), and corresponds to SiO2. SiO2 has low acidity and does not basically have the function of catalyzing the reaction of methanol or compounds derived from methanol. By covering the outer surface of H-ZSM-5 zeolite with an oxide containing amorphous silicon that does not contribute to such reactions, the acid sites, which are the active sites on the outer surface of the H-ZSM-5 zeolite, can be eliminated, and the isomerization of paraxylene to meta-xylene and ortho-xylene can be prevented. On the other hand, paraxylene generated in the pores of the H-ZSM-5 zeolite is released to the outside of the second catalyst through the pores of SiO2.

[0042] In the second catalyst, SiO2 and H-ZSM-5 zeolite may be in any positional relationship as long as the surface of the H-ZSM-5 zeolite is coated with SiO2. For example, the second catalyst may have a so-called core-shell structure in which the H-ZSM-5 zeolite particle forms a core, and the SiO2 is coated around the core as a shell. Furthermore, the SiO2 may be coated in a composite state.

[0043] In the second catalyst, the thickness of the SiO2 film covering the surface of the H-ZSM-5 zeolite is not particularly limited, but is, for example, 0.01 μm to 200 μm, preferably 0.05 μm to 50 μm. This makes it possible to more reliably prevent isomerization of para-xylene to meta-xylene and ortho-xylene, and also to prevent a decrease in reaction efficiency due to an insufficient supply of methanol to the H-ZSM-5 zeolite caused by an excessively large SiO2 film thickness.

[0044] The thickness of the SiO2 film formed on the outer surface of the H-ZSM-5 zeolite can be measured by observing the cross section of the catalyst using a scanning electron microscope (SEM). As a sample preparation method for observing the catalyst cross section, there is a method of embedding catalyst particles in resin and polishing them. Note that the above film thickness is an average value, and when measuring by observing the catalyst cross section with an SEM, if the film thickness is uniform, several measurement points are sufficient, but if it is not uniform, measurement points are set to a number that allows the average value to be calculated (for example, 16 points at approximately equal intervals in the circumferential direction). In addition, when the film thickness differs for each particle, multiple particles (for example, 10 particles) are observed as representatives and averaged. When selecting multiple representative particles, particles with an average film thickness are selected after observing more particles than the representative particle, excluding particles with extremely different film thicknesses. When catalysts with different particle sizes are mixed, a particle with a particle diameter of about the average particle diameter is selected when observing as a representative as described above. To measure the average particle diameter, a laser diffraction particle size distribution measuring device is used, which irradiates dispersed catalyst particles with laser light and measures the angular dependency of the scattered light intensity from the particles to determine the particle size distribution. Note that there may be defective parts where the SiO2 film is not formed, but in such cases, the defective parts are not measured, and the average value of the parts where SiO2 is formed is used.

[0045] In the second catalyst, the mass ratio of SiO2 is not particularly limited, but is, for example, 5% by mass to 100% by mass, preferably 10% by mass to 40% by mass, based on the mass of H-ZSM-5 zeolite. Here, "5% by mass to 100% by mass, based on the mass of H-ZSM-5 zeolite" means "5 parts by mass to 100 parts by mass, based on 100 parts by mass of H-ZSM-5 zeolite". This makes it possible to more reliably prevent isomerization of paraxylene to meta-xylene and ortho-xylene, and also to prevent a decrease in reaction efficiency due to an insufficient supply of methanol to the H-ZSM-5 zeolite caused by an excessively large SiO2 film thickness.

[0046] The mass ratio of SiO2 in the second catalyst is obtained by the following method. First, the silica (SiO2+H-ZSM-5) and alumina of the second catalyst are quantitatively analyzed by ICP-AES. Next, the silica / alumina ratio of H-ZSM-5 is obtained by cross-sectional analysis using scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDS). Then, taking into account the silica / alumina ratio of H-ZSM-5, the entire silica quantified by ICP-AES is divided into SiO2 and H-ZSM-5, and the mass ratio of SiO2 is calculated.

[0047] The average pore size of the second catalyst is not particularly limited, but is, for example, 0.1 nm to 2.5 nm, preferably 0.4 nm to 0.6 nm, which can more reliably obtain the above-mentioned spatial confinement effect in the pores and provides a pore size large enough to allow paraxylene synthesized by H-ZSM-5 in the second catalyst to pass through.

[0048] The specific surface area of ​​the second catalyst is not particularly limited, but is, for example, 20 m 2 / g or more 1000m 2 / g or less, preferably 100m 2 / g or more 400m 2 This makes it possible to sufficiently supply active sites for the reaction of methanol and the synthesis of para-xylene, and also makes it possible to easily set the pore size of the second catalyst within the above-mentioned range.

[0049] The pore volume of the second catalyst is not particularly limited and is, for example, 0.1 cc / g or more and 5 cc / g or less, preferably 0.5 cc / g or more and 2 cc / g or less.

[0050] When the second catalyst is granular, the average particle size of the second catalyst is, for example, 0.1 μm to 10 μm, preferably 0.5 μm to 5 μm, which accelerates the mass transfer between the first catalyst and the second catalyst and reduces the flow resistance of the raw material gas (reducing pressure loss).

[0051] (1.3. The third catalyst) As mentioned above, the third catalyst catalyzes the carbon-carbon formation reaction from carbon monoxide and hydrogen, promoting the production of alkenes, which are precursors of paraxylene, just like methanol. Here, the iron and manganese composite oxide promotes the production of carbenes, so the carbon-carbon bond formation reaction proceeds efficiently.

[0052] The third catalyst is mainly composed of a binary composite oxide of iron and manganese, but may also contain other compounds resulting from the production of the third catalyst or compounds originating from the support used to support the third catalyst. The third catalyst preferably contains 90% by mass or more and 99% by mass or less of iron, more preferably 95% by mass or more and 97% by mass or less of iron, based on the total amount of metals, and further preferably contains 1% by mass or more and 10% by mass or less of manganese, more preferably 1% by mass or more and 5% by mass or less of manganese, based on the total amount of metals.

[0053] The metal mass concentration in the third catalyst can be quantified by a scanning high-frequency inductively coupled plasma spectrometry (ICP-AES method). Specifically, after crushing the sample, an alkali melting agent (e.g., sodium carbonate, sodium borate, etc.) is added and the sample is heated and melted in a platinum crucible, and after cooling, the entire amount is dissolved in a hydrochloric acid solution under heating. When the solution is injected into an ICP analyzer, the sample solution is atomized and thermally excited in the high-temperature plasma state inside the device, and when this returns to the ground state, an emission spectrum with wavelengths specific to the elements is generated, and the type and amount of contained elements can be qualitatively and quantitatively determined from the emission wavelength and intensity. The mass concentration of each metal can be calculated from the following formula. Iron concentration [%] = (amount of iron in the third catalyst) / (amount of iron in the third catalyst + amount of manganese in the third catalyst) x 100 [%] Manganese concentration [%] = (amount of manganese in the third catalyst) / (amount of iron in the third catalyst + amount of manganese in the third catalyst) x 100 [%]

[0054] The form of the third catalyst is not particularly limited, and may be, for example, granular or layered (membrane). The third catalyst is usually porous, and therefore has pores for carrying out the reaction, and has a relatively large specific surface area.

[0055] The specific surface area of ​​the third catalyst can be increased by decreasing the pore size or increasing the pore volume. In other words, the pore size and pore volume are related to the specific surface area of ​​the third catalyst. Generally, a larger specific surface area is preferable, but if one tries to maintain the pore size and pore volume within an appropriate range, an extremely large specific surface area cannot be obtained.

[0056] The specific surface area of ​​the third catalyst is not particularly limited, but is, for example, 3 m 2 / g or more 500m 2 / g or less, preferably 10m 2 / g or more 100m 2 / g or less. This allows a sufficient supply of active sites for the carbon-carbon bond forming reaction. In addition, by having a specific surface area of ​​less than the above-mentioned upper limit, it is possible to prevent the pore size from becoming excessively small, which would cause a difference in the gas diffusion speed between carbon monoxide and hydrogen in the pores, and thus prevent a difference in the partial pressure of carbon monoxide and that of hydrogen in the third catalyst. As a result, hydrogen and carbon monoxide are efficiently converted to alkenes. The specific surface area can be measured by the BET method.

[0057] The average pore size of the third catalyst is not particularly limited, but is, for example, 0.5 nm to 100 nm, preferably 2 nm to 30 nm. This prevents the difference in gas diffusion speed between carbon monoxide and hydrogen in the pores, and allows the specific surface area of ​​the third catalyst to be increased, making it possible to supply sufficient active sites. As a result, the conversion of hydrogen and carbon monoxide to alkenes is efficiently performed.

[0058] The pore volume of the third catalyst is not particularly limited and is, for example, 0.1 cc / g or more and 5 cc / g or less, preferably 0.5 cc / g or more and 2 cc / g or less.

[0059] The pore volume can be determined by mercury intrusion porosimetry. If mercury intrusion porosimetry is not available, it can be measured by water titration. The average pore diameter can be measured by mercury intrusion porosimetry using a mercury porosimeter. If mercury intrusion porosimetry is not available, it can be measured by gas adsorption.

[0060] When the third catalyst is granular, the average particle size of the third catalyst is, for example, 1 μm to 800 μm, preferably 10 μm to 200 μm, which accelerates the mass transfer between the third catalyst and the second catalyst and reduces the flow resistance of the raw material gas (reducing pressure loss).

[0061] (1.4. Positional relationship of the three catalysts) As described above, the catalyst group for producing paraxylene according to the present disclosure includes a first catalyst, a second catalyst, and a third catalyst. The positional relationship of the first catalyst, the second catalyst, and the third catalyst is preferably such that the first catalyst and the second catalyst are physically mixed and then granulated, and the granulated material and the third catalyst are physically mixed, or the third catalyst is granulated after physical mixing. The third catalyst may be disposed at a position different from the granulated material of the first catalyst and the second catalyst. That is, the third catalyst may be used by mixing with the granulated material of the first catalyst and the second catalyst, or the third catalyst may be disposed in the upper layer (upstream side) of the reactor, and the granulated material obtained by physically mixing the first catalyst and the second catalyst and then granulating the granulated material may be filled in the lower layer (downstream side).

[0062] It is more preferable that the first catalyst and the second catalyst are in close proximity to each other. The reason is that if the first catalyst and the second catalyst are not in close proximity, other side reactions will proceed from the intermediate methanol, and the selectivity of paraxylene will decrease. If the first catalyst and the second catalyst are present as a granule in which they are mixed, the two will be in close proximity. Therefore, the catalyst group for producing paraxylene according to the present disclosure is present as a granule in which at least the first catalyst and the second catalyst are mixed with each other. In the present disclosure, the particle size of the granulated material is not particularly limited, and the particle size differs depending on whether the granulated material contains a third catalyst, but for example, the average particle size is 200 μm or more and 1000 μm or less. The particle size refers to the volume-based 50% particle size (D50) measured by a wet laser diffraction / scattering method. In addition, when measurement by the laser diffraction / scattering method is difficult due to poor dispersibility or the like, a method such as an image imaging method can be applied.

[0063] In the group of catalysts for producing paraxylene according to the present disclosure, the second catalyst is contained in an amount of, for example, 10% by mass or more and 1000% by mass or less relative to the first catalyst (i.e., 100 parts by mass of the first catalyst and 10 parts by mass or more and 1000 parts by mass or less of the second catalyst), and preferably 80% by mass or more and 120% by mass or less. This allows the methanol synthesis rate in the first catalyst and the methanol consumption rate in the second catalyst to be relatively close to each other, and prevents unintended side reactions caused by excess compounds.

[0064] In the production of the catalyst group for producing paraxylene according to the present disclosure, the ratio of the second catalyst to the first catalyst can be optimized by adjusting the mass (mixture) of each of the first catalyst and the second catalyst when they are mixed. In the catalyst after the first catalyst and the second catalyst are mixed (including the case where the catalyst is subsequently molded or granulated), the ratio can be determined, for example, by using a scanning high-frequency inductively coupled plasma method (ICP). Specifically, after crushing the sample, an alkali melting agent (e.g., sodium carbonate, sodium borate, etc.) is added and the sample is heated and melted in a platinum crucible, and after cooling, the entire amount is dissolved in a hydrochloric acid solution under heating. When the solution is injected into an ICP analyzer, the sample solution is atomized and thermally excited in the high-temperature plasma state in the device, and when this returns to the ground state, an emission spectrum of an element-specific wavelength is generated, so that the contained element type and amount can be qualitatively and quantitatively determined from the emission wavelength and intensity. Then, the ratio of the first catalyst to the second catalyst can be calculated taking into account the ratio of the contained element types quantified.

[0065] In the catalyst group for producing paraxylene, the third catalyst is contained in a mixture of the first catalyst and the second catalyst in an amount of, for example, 0.1 mass% to 1.5 mass%, preferably 0.1 mass% to 1.0 mass%. This promotes the production of alkenes that are precursors of paraxylene. On the other hand, if the amount of the third catalyst added is too large, the reaction to alkenes becomes the main reaction, and the selectivity of paraxylene decreases. Therefore, the amount of the third catalyst added in the mixture of the first catalyst and the second catalyst is preferably 0.1 mass% to 1.5 mass%.

[0066] The fact that the mixture of the granulated product of the first catalyst and the second catalyst and the third catalyst is mixed in the above ratio can be determined, for example, by using a scanning high-frequency inductively coupled plasma method (ICP). Specifically, after crushing the sample, an alkali melting agent (e.g., sodium carbonate, sodium borate, etc.) is added and the mixture is heated and melted in a platinum crucible, and after cooling, the entire amount is dissolved in a hydrochloric acid solution under heating. When the solution is injected into an ICP analyzer, the sample solution is atomized and thermally excited in the high-temperature plasma state inside the device, and when this returns to the ground state, an emission spectrum of an element-specific wavelength is generated, so that the contained element type and amount can be qualitatively and quantitatively determined from the emission wavelength and intensity. Then, the ratio of the contained element types determined can be calculated by considering the ratio of the contained element types.

[0067] The catalyst group for producing paraxylene according to the present disclosure has been described above. According to the present disclosure, paraxylene can be efficiently produced using carbon monoxide and hydrogen as raw materials. That is, paraxylene can be efficiently synthesized in a large yield by using a binary composite oxide of chromium and zinc, which easily adsorbs carbon monoxide and efficiently reacts with carbon monoxide and hydrogen, as the first catalyst, a H-ZSM-5 zeolite, which has a spatial confinement effect and is coated with an amorphous silicon-containing oxide on the surface and can selectively and efficiently synthesize paraxylene, as the second catalyst, and a binary composite oxide of iron and manganese, which promotes the production of alkenes that are precursors of paraxylene like methanol, as the third catalyst.

[0068] <2. Method for producing catalyst group for producing paraxylene> Next, a method for producing a catalyst group for producing paraxylene according to the present disclosure will be described. The method for producing a catalyst group for producing paraxylene according to the present disclosure includes a step (first step) of obtaining a first catalyst which is a binary oxide of at least chromium and zinc, a step (second step) of obtaining a second catalyst in which the surface of H-ZSM-5 zeolite is coated with an oxide containing amorphous silicon by performing hydrothermal synthesis or heating in the presence of a silicon compound and H-ZSM-5 zeolite, a step (third step) of obtaining a third catalyst which is a binary oxide of iron and manganese, and a step (fourth step) of mixing and / or disposing the first catalyst, the second catalyst, and the third catalyst. The method for producing a catalyst group for producing paraxylene according to the present disclosure may optionally include a step (fifth step) of synthesizing H-ZSM-5 zeolite from a silicon compound and an aluminum compound by hydrothermal synthesis prior to the third step.

[0069] For example, the first step is a step of obtaining a composite hydroxide containing chromium and zinc by a coprecipitation method, and obtaining a first catalyst by either or both of drying and calcining the composite hydroxide containing chromium and zinc; The second step is a step of obtaining a second catalyst comprising H-ZSM-5 zeolite, the surface of which is coated with an amorphous silicon-containing oxide, from a silicon compound and H-ZSM-5 zeolite by hydrothermal synthesis or heating; The third step is a step of obtaining a composite hydroxide containing iron and manganese by a coprecipitation method, and obtaining a third catalyst by either or both of drying and calcining the composite hydroxide containing iron and manganese; The fourth step is a step of mixing at least the first catalyst and the second catalyst out of the first catalyst, the second catalyst, and the third catalyst, and granulating the mixture to obtain a granulated product. Each step will now be described in detail.

[0070] (2.1. First step) First, in the first step, a composite hydroxide of chromium and zinc is obtained by, for example, a wet precipitation method (coprecipitation method), and the composite hydroxide of chromium and zinc is dried and / or calcined to obtain a first catalyst.

[0071] Specifically, first, a chromium compound and a zinc compound are dissolved in an aqueous solution, and a precipitating agent is added to the solution to precipitate a composite hydroxide of chromium and zinc. The chromium compound (chromium source) is not particularly limited as long as it is soluble in an aqueous solution, and for example, chromium nitrate, chromium acetate, chromium chloride, chromium bromide, ammonium dichromate, etc. can be used. The zinc compound (zinc source) is not particularly limited as long as it is soluble in an aqueous solution, and examples of the zinc compound that can be used include zinc nitrate, zinc acetate, zinc chloride, and zinc bromide.

[0072] The precipitating agent is not particularly limited as long as it is capable of precipitating (depositing) a composite hydroxide of chromium and zinc, and for example, ammonium carbonate, sodium carbonate, sodium hydrogen carbonate, urea, potassium carbonate, etc. can be used.

[0073] In addition, for the purpose of controlling the particle size and shape of the chromium and zinc composite hydroxide, an aging treatment may be performed in a settled state of the chromium and zinc composite hydroxide. The aging treatment can be performed, for example, by stirring for 30 minutes to 12 hours.

[0074] In the above treatment, the temperature of the aqueous solution is not particularly limited, but is, for example, 30°C or higher and 100°C or lower.

[0075] Next, the obtained chromium and zinc composite hydroxide is dried and / or calcined to obtain a first catalyst containing a chromium and zinc composite hydroxide. Note that, prior to the drying and / or calcination, the chromium and zinc composite hydroxide may be appropriately washed.

[0076] The drying can be carried out for example in an air atmosphere at 60° C. to 200° C. for 30 minutes to 12 hours, while the firing can be carried out for example in an air atmosphere at 400° C. to 600° C. for 30 minutes to 10 hours. In this manner, the first catalyst containing a composite oxide of chromium and zinc is obtained.

[0077] If the composite hydroxide of chromium and zinc is separately available, this step may be omitted. Furthermore, regardless of the above description, the composite oxide of chromium and zinc does not have to be produced by a wet precipitation method.

[0078] (2.2. Second step) In this step, hydrothermal synthesis is carried out in the presence of at least a silicon compound and H-ZSM-5 zeolite, or heating is carried out in the presence of a silicon compound and H-ZSM-5 zeolite to obtain a second catalyst in which the surface of H-ZSM-5 zeolite is coated with amorphous SiO2. SiO2 is formed, for example, by dropping tetraethoxysilane (TEOS) into an organic solvent in which H-ZSM-5 zeolite is dispersed, followed by heating.

[0079] Hexane, etc., is used as the organic solvent in which H-ZSM-5 is dispersed when covering with SiO2. Other organic solvents, alcohol, etc. may also be included.

[0080] Furthermore, stirring is performed to disperse H-ZSM-5 in the organic solvent. The stirring speed is not particularly limited, but can be, for example, 200 to 1000 rpm, and preferably 300 to 800 rpm.

[0081] The heating temperature after dropping TEOS into the organic solvent dispersing H-ZSM-5 is not particularly limited, but may be, for example, 50 to 150°C, preferably 50 to 80°C.

[0082] After dropping TEOS into the H-ZSM-5 dispersed organic solvent, the organic solvent is removed by heating. The heating time is not particularly limited, but may be, for example, 50 to 150°C, preferably 50 to 80°C.

[0083] The H-ZSM-5 zeolite coated with SiO2 as described above is dried and calcined as necessary after the heating is completed. The drying time is not particularly limited, but may be, for example, 0.5 to 20 hours. The drying temperature is not particularly limited, but may be, for example, 50 to 150°C.

[0084] Next, the dried catalyst is calcined to remove organic matter present in the pores of the zeolite. This results in the production of H-ZSM-5 zeolite coated with SiO2. The calcination time is not particularly limited, but may be, for example, 0.5 to 15 hours. The calcination temperature is not particularly limited, but may be, for example, 400 to 600°C.

[0085] In this manner, a second catalyst containing H-ZSM-5 zeolite having a surface coated with amorphous SiO2 can be obtained.

[0086] (2.3. Third step) In the third step, a composite hydroxide of iron and manganese is obtained by a wet precipitation method, and the composite hydroxide of iron and manganese is dried and / or calcined to obtain a third catalyst.

[0087] Specifically, first, an iron compound and a manganese compound are dissolved in an aqueous solution, and a precipitating agent is added to precipitate a composite hydroxide of iron and manganese. The iron compound (iron source) is not particularly limited as long as it is soluble in an aqueous solution, and for example, iron nitrate, iron acetate, iron chloride, iron bromide, etc. can be used. The manganese compound (manganese source) is not particularly limited as long as it is soluble in an aqueous solution, and for example, manganese nitrate, manganese acetate, manganese chloride, manganese bromide, etc. can be used.

[0088] The precipitating agent is not particularly limited as long as it is capable of precipitating (depositing) a composite hydroxide of iron and manganese, and for example, ammonium carbonate, sodium carbonate, sodium hydrogen carbonate, urea, potassium carbonate, etc. can be used.

[0089] In addition, for the purpose of controlling the particle size and shape of the iron and manganese composite hydroxide, an aging treatment may be performed in a state in which the iron and manganese composite hydroxide has settled. The aging treatment can be performed, for example, by leaving the mixture to stand for 30 minutes to 12 hours.

[0090] In the above treatment, the temperature of the aqueous solution is not particularly limited, but is, for example, 30°C or higher and 100°C or lower.

[0091] Next, the obtained iron and manganese composite hydroxide is dried and / or calcined to obtain a third catalyst containing a chromium and zinc composite hydroxide. Note that, prior to the drying and / or calcination, the iron and manganese composite hydroxide may be appropriately washed.

[0092] The drying can be carried out for example in an air atmosphere at 60° C. to 200° C. for 30 minutes to 12 hours, while the firing can be carried out for example in an air atmosphere at 400° C. to 600° C. for 30 minutes to 10 hours. In this manner, the first catalyst containing a composite hydroxide of iron and manganese is obtained.

[0093] If the iron and manganese composite hydroxide is separately available, this step may be omitted. Furthermore, regardless of the above description, the iron and manganese composite oxide does not have to be produced by a wet precipitation method.

[0094] (2.4. Fourth step) In this step, at least the first catalyst and the second catalyst among the first catalyst, the second catalyst, and the third catalyst are mixed and granulated to obtain a granulated product. For example, when producing a granulated product containing three types of catalysts, the first catalyst, the second catalyst, and the third catalyst are physically mixed and granulated. This produces a catalyst group for producing paraxylene. Mixing can be performed, for example, using a mortar, a ball mill, an automatic kneader, or the like.

[0095] After mixing, in order to improve the adhesion between the first catalyst, the second catalyst, and the third catalyst, or between the first catalyst and the second catalyst, the catalyst group for producing paraxylene may be molded into pellets and the pellets may be crushed.

[0096] In order for the reaction from methanol to paraxylene to proceed efficiently, it is particularly preferable that the first catalyst and the second catalyst are close to each other. In the catalyst group for producing paraxylene according to the present disclosure, the first catalyst and the second catalyst are present as a granule in which the first catalyst and the second catalyst are mixed, so that the first catalyst and the second catalyst are close to each other, and it is possible to achieve high reaction efficiency of the reaction from methanol to paraxylene.

[0097] In order to further increase the productivity of paraxylene using the catalyst group for producing paraxylene according to the present disclosure, it is preferable to fill the upper layer with the third catalyst, fill the lower layer with a powder (granules) in which the first catalyst and the second catalyst are physically mixed, and sandwich glass wool between the upper and lower layers. With such a configuration, the synthesis reaction of paraxylene can be carried out with high productivity.

[0098] (2.5. Fifth step) This step is a step that is optionally performed prior to the second step, and H-ZSM-5 zeolite is synthesized from a silicon compound and an aluminum compound, for example, by hydrothermal synthesis. The formation of H-ZSM-5 zeolite is performed, for example, by heating an aqueous solution (precursor solution) containing a silicon compound (silica source) and an aluminum compound (alumina source).

[0099] Examples of the silicon compound that can be used include tetramethyl orthosilicate and tetraethyl orthosilicate, and examples of the aluminum compound that can be used include aluminum nitrate and aluminum acetate, but are not limited to these.

[0100] The precursor solution may also contain an amine compound as a template agent (organic structure directing agent), such as tetrapropylammonium hydroxide, tetraethylammonium hydroxide, etc. Furthermore, the solvent of the precursor solution is mainly composed of water, but may also contain an alcohol-based solvent such as ethanol or methanol for the purpose of controlling the hydrolysis rate of the silicon compound.

[0101] The temperature in the hydrothermal synthesis is not particularly limited, but can be, for example, 150 to 200°C, preferably 170 to 190°C.

[0102] The particle size of the H-ZSM-5 zeolite increases with an increase in the hydrothermal synthesis time. The hydrothermal synthesis time is, for example, from 1 hour to 168 hours, and preferably from 24 hours to 72 hours.

[0103] In the hydrothermal synthesis, the reaction solution may be stirred as necessary. Stirring conditions can be appropriately set. In addition, the particle size, pore size, specific surface area, and other physical properties of H-ZSM-5 zeolite can be controlled by the hydrothermal synthesis conditions, such as time.

[0104] The H-ZSM-5 zeolite produced by hydrothermal synthesis is washed and dried appropriately after completion of hydrothermal synthesis. The drying time is not particularly limited, but can be, for example, 0.5 to 20 hours. The drying temperature is not particularly limited, but can be, for example, 50 to 150°C.

[0105] Next, the dried catalyst is calcined to remove organic matter present in the pores of the zeolite. This results in the production of H-ZSM-5 zeolite. The calcination time is not particularly limited, but may be, for example, 0.5 to 15 hours. The calcination temperature is not particularly limited, but may be, for example, 400 to 600°C.

[0106] If the H-ZSM-5 zeolite is available separately, this step may be omitted. Furthermore, regardless of the above description, the H-ZSM-5 zeolite does not have to be produced by a hydrothermal synthesis method.

[0107] <3. Method for producing paraxylene> Next, a method for producing paraxylene using the above-mentioned group of catalysts for producing paraxylene will be described based on a preferred embodiment.

[0108] Paraxylene can be produced by contacting carbon monoxide and hydrogen with the catalyst group for producing paraxylene according to the present disclosure. Carbon monoxide and hydrogen may be supplied separately, but are usually supplied as a mixed gas.

[0109] From the viewpoint of paraxylene productivity, the mixed gas of carbon monoxide and hydrogen used in the method according to the present disclosure is preferably a gas in which the total of carbon monoxide and hydrogen is 50 volume % or more of the total, and in particular, it is desirable that the molar ratio of hydrogen to carbon monoxide (hydrogen / carbon monoxide) is in the range of 0.5 to 4.0. This is because, when the molar ratio of hydrogen to carbon monoxide is less than 0.5, the amount of hydrogen present in the feed gas is too small, making it difficult for the hydrogenation reaction of carbon monoxide to proceed and productivity does not increase, while, when the molar ratio of hydrogen to carbon monoxide exceeds 4.0, the amount of carbon monoxide present in the feed gas is too small, so productivity of liquid hydrocarbons does not increase regardless of catalytic activity.

[0110] The reactor used for contacting the mixed gas with the catalyst according to the present disclosure is not particularly limited, and examples thereof include general reactors for gas phase synthesis processes such as fixed beds, entrained beds, and fluidized beds, reactors for liquid phase synthesis processes such as slurry beds, and microchannel reactors.

[0111] When carrying out the reaction for producing paraxylene, the binary composite oxide of chromium and zinc (first catalyst) needs to be in a reduced state. Therefore, before supplying the mixed gas to produce paraxylene, a reducing gas such as hydrogen gas is passed through to reduce the catalyst group for producing paraxylene. Although there is no particular limitation, such a reduction treatment can be carried out at a temperature of 300 to 500°C for 1 to 40 hours.

[0112] The catalyst group for producing paraxylene may be reduced after being packed into the reactor, or may be reduced before being packed into the reactor. For example, it is also possible to carry out a reduction treatment before the catalyst group for producing paraxylene is charged into the reactor, and then pack the catalyst group into the reactor.

[0113] To further increase productivity, the reaction can be carried out by filling the upper layer with a third catalyst, filling the lower layer with a powder of a physical mixture of the first and second catalysts, and sandwiching glass wool between the upper and lower layers.

[0114] The conditions for producing paraxylene are not particularly limited, and the conditions can be set depending on the type of reactor.

[0115] For example, the reaction temperature during the reaction for producing paraxylene is not particularly limited, but is 200 to 500° C., and preferably 300 to 400° C. The pressure in the system during the reaction is not particularly limited, but is, for example, 0.8 to 6.0 MPa, and preferably 2.5 to 5.0 MPa.

[0116] When activity is reduced due to factors such as an extremely high conversion rate or a long reaction time, the catalyst group for producing paraxylene can be regenerated by supplying a gas containing hydrogen (regeneration gas) instead of the mixed gas. The hydrogen content of the regeneration gas is preferably 5% or more. The hydrogen content of the regeneration gas may be 100%. The regeneration gas may contain an inert gas such as nitrogen or argon in addition to hydrogen.

[0117] The conditions for regenerating the catalyst group for producing paraxylene are not particularly limited as long as the catalyst regeneration proceeds. The catalyst regeneration mechanism by contacting the catalyst group for producing paraxylene with the regeneration gas containing hydrogen is presumed to involve re-reduction of the chromium oxide catalyst and the like oxidized by the by-product water and removal of the deposited carbon by hydrogen.

[0118] Specifically, the temperature during regeneration is, for example, 300 to 500°C. The pressure during regeneration is, for example, normal pressure to reaction pressure. In particular, when the regeneration pressure is set to the reaction pressure or lower, it becomes possible to use a compressor for increasing the pressure to the reaction pressure during the reaction, and it becomes unnecessary to install a new compressor for regeneration, which is advantageous in terms of equipment cost. In addition, the regeneration time can be, for example, 1 hour or more. EXAMPLES

[0119] Hereinafter, the catalyst group for producing paraxylene and the like according to the present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to these examples and comparative examples.

[0120] Example 1 (1. Production of catalysts for paraxylene production) 4.0 g of chromium nitrate and 3.0 g of zinc nitrate were precisely weighed and dissolved in 500 ml of pure water. This aqueous solution was heated to 70°C, and an aqueous ammonium carbonate solution was added to precipitate chromium and zinc as a binary composite hydroxide, and the mixture was thoroughly stirred with a stirrer. The mixture was then aged for 3 hours while being kept at 70°C, after which it was filtered and thoroughly washed with pure water at 80°C. The precipitate obtained after washing was dried at 100°C, coarsely crushed, and then calcined at 500°C in air. This resulted in the production of a binary composite oxide powder of chromium and zinc (ZnCr2O4) as the first catalyst.

[0121] On the other hand, to produce H-ZSM-5 zeolite, tetramethyl orthosilicate, aluminum nitrate, water, tetrapropylammonium hydroxide, and ethanol were precisely weighed and dissolved in a molar ratio of 1:1 / 40:50:0.24:4. The solution was introduced into a Teflon (registered trademark) sealed autoclave, stirred with a magnetic stirrer for 4 hours, and then reacted at 180 ° C for 24 hours. The product obtained was washed with distilled water, dried overnight at 120 ° C, and then calcined in air at 550 ° C for 5 hours to decompose and remove organic matter present in the zeolite pores, thereby obtaining a porous H-ZSM-5 zeolite powder. The obtained H-ZSM-5 zeolite powder had a BET specific surface area of ​​367.6 m2 by N2 adsorption and desorption. 2 / g and the average pore diameter was 2.0 nm.

[0122] 1 g of the zeolite (H-ZSM-5) thus obtained was added to 100 mL of normal hexane containing 7 g, and the mixture was stirred at 500 rpm using a stirrer. Then, 3.4 g of TEOS was added dropwise to the solvent. After the TEOS was added dropwise, stirring was continued for 4 hours. Next, the solution was heated to 80°C while stirring, and normal hexane was removed by suction. The obtained sample was dried at 100°C for 12 hours, and then calcined at 550°C for 5 hours to obtain H-ZSM-5 zeolite, the surface of which was coated with amorphous SiO2, as the second catalyst (hereinafter, sometimes referred to as "SiO2-coated zeolite").

[0123] On the other hand, the iron and manganese binary composite oxide was prepared by the following method. 10.1 g of iron nitrate nonahydrate and 0.63 g of manganese nitrate tetrahydrate were precisely weighed and dissolved in 500 ml of pure water. This aqueous solution was heated to 70 ° C., and an aqueous sodium carbonate solution was added to precipitate iron and manganese as a binary composite hydroxide, and the mixture was thoroughly stirred with a stirrer. After that, the mixture was kept at 70 ° C. and stirred for 3 hours for aging, and then filtered and thoroughly washed with pure water at 80 ° C. The precipitate obtained after washing was dried at 100 ° C., coarsely crushed, and then calcined in air at 500 ° C. As a result, a binary composite oxide powder of iron and manganese was obtained as the third catalyst.

[0124] The binary composite oxide of chromium and zinc (first catalyst), SiO2-coated zeolite (second catalyst), and binary composite oxide of iron and manganese (third catalyst) obtained as described above were precisely weighed out to a mass ratio of 125:70:2, and physically mixed in a mortar for 10 minutes to obtain a mixed powder. The mixed powder was then press-molded into a tablet shape of 3 mmφ using a compression molding machine to obtain a tablet molded body, which was then crushed and sized to 20-40 mesh to obtain a catalyst group for producing paraxylene (granulated powder).

[0125] (Production of paraxylene) 0.125 g of the obtained granulated powder was used and fixed with quartz wool so as to be positioned at the center of a SUS reaction tube (reactor) with an inner diameter of 6 mm. A thermocouple was inserted at the center of the catalyst layer, and the fixed-bed reaction tube was set at a predetermined position.

[0126] Before starting the synthesis reaction, the reactor was heated to 400° C. in a nitrogen atmosphere, and then reduction treatment was carried out for 2 hours while flowing hydrogen gas at 60 mL / min. After that, the temperature was lowered to room temperature, and a gas containing hydrogen:CO=3:1 and 5% argon as an internal standard was introduced at 30mL / min, and synthesis was carried out for 6 hours at 5MPa and 375°C. After removing moisture, the reaction product was injected into two gas chromatographs (Shimadzu Corporation: GC-8A) and analyzed by a thermal conductivity detector (TCD: Thermal Conductivity Detector) and a hydrogen flame ionization detector (FID: Flame Ionization Detector).

[0127] The degree of reaction of the synthesis reaction (production rate of paraxylene) was calculated using the following formula from the concentration of each component: CO conversion, CO2 selectivity, methane selectivity, selectivity of C2-C4(O) from ethane, propane, and butane, selectivity of C2-C4(=) from ethylene, propylene, and butylene, selectivity of CH3OH+DME from methanol and dimethyl ether (DME), selectivity of long-chain aliphatic hydrocarbons (C5+) from pentane and onward, selectivity of aromatics, selectivity of benzene (B) in aromatic compounds, selectivity of toluene (T), selectivity of ortho-xylene (oX), selectivity of meta-xylene (mX), selectivity of para-xylene (pX), selectivity of aromatic hydrocarbons with carbon number 9 (A(C9)), selectivity of aromatic hydrocarbons with carbon number 10 or more (A(C10+)), and pX / X as the ratio of para-xylene to all xylenes (ortho-xylene, meta-xylene, and para-xylene). The results are shown in Table 1 under Example 1.

[0128] CO conversion rate (%) = (1-(amount of CO after reaction) / (amount of CO supplied)) x 100 CO2 selectivity (%) = (volume of CO2) / ((amount of CO supplied) - (amount of CO after reaction)) x 100 Hydrocarbon selectivity (%) = (volume of hydrocarbon) / ((amount of CO fed) - (amount of CO after reaction)) × 100 CH4 selectivity (%) = (volume of CH4) / (volume of hydrocarbon) x 100 Ethane selectivity (%) = (volume of ethane) / (volume of hydrocarbon) × 100 Propane selectivity (%) = (volume of propane) / (volume of hydrocarbon) x 100 Butane selectivity (%) = (volume of butane) / (volume of hydrocarbon) x 100 C2-C4(O) selectivity (%) = (ethane selectivity) + (propane selectivity) + (butane selectivity)

[0129] Ethylene selectivity (%) = (volume of ethylene) / (volume of hydrocarbon) x 100 Propylene selectivity (%) = (volume of propylene) / (volume of hydrocarbon) × 100 Butylene selectivity (%) = (volume of butylene) / (volume of hydrocarbon) x 100 C2-C4 (=) selectivity (%) = (ethylene selectivity) + (propylene selectivity) + (butylene selectivity)

[0130] CH3OH selectivity (%) = (volume of CH3OH) / (volume of hydrocarbon) × 100 DME selectivity (%) = (volume of DME) / (volume of hydrocarbon) x 100 CH3OH+DME selectivity(%)=(CH3OH selectivity)+(DME selectivity) Pentane selectivity (%) = (volume of pentane) / (volume of hydrocarbon) x 100 Pentane and longer chain aliphatic hydrocarbons (C5+) (%) = (pentane selectivity) + (C6 and longer chain aliphatic hydrocarbon selectivity)

[0131] B selectivity (%) = (volume of benzene) / (volume of hydrocarbon) × 100 T selectivity (%) = (volume of toluene) / (volume of hydrocarbon) × 100 E selectivity (%) = (volume of ethylbenzene) / (volume of hydrocarbon) × 100 oX selectivity (%) = (volume of ortho-xylene) / (volume of hydrocarbon) x 100 mX selectivity (%) = (volume of meta-xylene) / (volume of hydrocarbon) × 100 pX selectivity (%) = (volume of paraxylene) / (volume of hydrocarbon) × 100 A(C9) selectivity (%) = (volume of cumene) / (volume of hydrocarbon) × 100 Tetralin selectivity (%) = (volume of tetralin) / (volume of hydrocarbon) × 100 A(C10+) selectivity (%) = (tetralin selectivity) + (C11 or higher aromatic hydrocarbon selectivity) Aromatics selectivity (%) = (B selectivity) + (T selectivity) + (oX selectivity) + (mX selectivity) + (pX selectivity) + (A(C9) selectivity) + (A(C10+) selectivity) Percentage of paraxylene in total xylenes (%) = (pX selectivity) / ((oX selectivity)+(mX selectivity)+(pX selectivity))×100

[0132] The yield (%) of paraxylene can be calculated by CO conversion (%) ÷ 100 × (100-CO2 selectivity (%)) × pX selectivity (%) ÷ 100. Therefore, under these conditions, it was found that paraxylene was produced at a rate of 26.6 ÷ 100 × (100-45.7) × 8.53 ÷ 100 = 1.23%.

[0133] Example 2 In the production of the third catalyst, 20.2 g of iron nitrate nonahydrate and 0.63 g of manganese nitrate tetrahydrate were used to obtain a binary composite oxide of iron and manganese, and the binary composite oxide of chromium and zinc (first catalyst), SiO2-coated zeolite (second catalyst), and the binary composite oxide of iron and manganese (third catalyst) were precisely weighed out to a mass ratio of 100:56:1. The catalyst group for producing paraxylene was prepared in the same manner as in Example 1, and paraxylene was synthesized using the obtained catalyst group for producing paraxylene in the same manner as in Example 1. The results are shown in Table 1 and Example 2.

[0134] [Examples 3 to 5] A catalyst group for producing paraxylene was obtained by preparation in the same manner as in Example 1, except that the amount of the third catalyst added relative to the total catalyst amount was 1.5 mass%, 0.1 mass%, or 0.5 mass%, respectively. Paraxylene was synthesized using the obtained catalyst group for producing paraxylene in the same manner as in Example 1. The results are shown in Table 1 and Examples 3 to 5.

[0135] Example 6 The first catalyst and the second catalyst were physically mixed, and then granulated by compression molding into pellets, which were then physically mixed with a third catalyst (a binary composite oxide of iron and manganese) prepared with the same Fe / Mn molar ratio as in Example 1. Except for this, a catalyst group for producing paraxylene was prepared in the same manner as in Example 2. Paraxylene was synthesized in the same manner as in Example 1 using the obtained catalyst group for producing paraxylene. The results are shown in Table 1 and Example 6.

[0136] Example 7 The third catalyst was packed in the upper part of the reactor, the first catalyst and the second catalyst were physically mixed and then granulated by compression molding into pellets, which were then packed in the lower part of the reactor, and glass wool was sandwiched between the upper and lower parts. A catalyst group for producing paraxylene was obtained by preparing the catalyst group for producing paraxylene in the same manner as in Example 1, except that the content of the third catalyst was 0.6 mass%. The obtained catalyst group for producing paraxylene was used to synthesize paraxylene in the same manner as in Example 1. The results are shown in Table 1 and Example 7.

[0137] Comparative Example 1 The second catalyst and the third catalyst were physically mixed, and then granulated by compression molding into pellets, which were then physically mixed with the first catalyst. Except for the fact that the content of the third catalyst was 0.6 mass%, a catalyst group for producing paraxylene was prepared in the same manner as in Example 1. Paraxylene was synthesized in the same manner as in Example 1 using the obtained catalyst group for producing paraxylene. The results are shown in Table 1 and Comparative Example 1.

[0138] Comparative Example 2 A catalyst group for producing paraxylene was obtained by preparing in the same manner as in Example 1, except that the first catalyst, the second catalyst, and the third catalyst were physically mixed and the content of the third catalyst was set to 0.6 mass%. Paraxylene was synthesized in the same manner as in Example 1, using the obtained catalyst group for producing paraxylene. The results are shown in Table 1 and Comparative Example 2.

[0139] Comparative Example 3 A catalyst group for producing paraxylene was obtained by preparation in the same manner as in Example 1, except that the third catalyst was not added and only the first catalyst and the second catalyst were physically mixed and then pelletized by compression molding. Paraxylene was synthesized in the same manner as in Example 1 using the obtained catalyst group for producing paraxylene. The results are shown in Table 1 and Comparative Example 3.

[0140] Comparative Example 4 The obtained 1 g of zeolite (H-ZSM-5) was immersed in a solution of silica, tetrapropylammonium hydroxide, ethanol and water in a molar ratio of 1:0.06:16:240, then placed in a Teflon-sealed autoclave and reacted at 180°C for 24 hours while rotating at a speed of 3 revolutions per minute. This operation was repeated twice to obtain a zeolite coated with silicalite-1 as a second catalyst. Preparation was carried out in the same manner as in Example 1 except that this zeolite coated with silicalite-1 (H-ZSM-5@silicalite-1) was used, to obtain a catalyst group for producing paraxylene. The obtained catalyst group for producing paraxylene was used to synthesize paraxylene in the same manner as in Example 1. The results are shown in Table 1 and Comparative Example 4.

[0141] [Table 1]

[0142] From the examples and comparative examples in Table 1, it was found that the space-time yields of Examples 1 to 7 were higher than those of Comparative Examples 1 to 3, and that by using the first catalyst and the second catalyst in a state of being close to each other after physical mixing and granulation, and further adding a third catalyst, a higher paraxylene productivity was obtained than Comparative Examples 1 and 2 in which the first catalyst and the second catalyst were not mixed and granulated, and also than Comparative Example 3 in which the third catalyst was not included. In particular, it was found that a higher paraxylene productivity was obtained by filling the upper part of the reactor with the third catalyst, physically mixing the first catalyst and the second catalyst, granulating them by compression molding into pellets, filling the lower part of the reactor, and sandwiching glass wool between the upper and lower parts (Example 7).

[0143] Furthermore, from the examples and comparative example 4 in Table 1, it can be seen that the catalyst group for producing paraxylene of the present disclosure is preferable because it has higher paraxylene productivity when SiO2-coated H-ZSM-5 is used than when silicalite-1-coated H-ZSM-5 is used.

[0144] Although the preferred embodiment of the present disclosure has been described in detail above, the present disclosure is not limited to such examples. It is clear that a person having ordinary knowledge in the technical field to which the present disclosure belongs can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present disclosure.

Claims

1. A first catalyst including a binary composite oxide of chromium and zinc; a second catalyst comprising an H-ZSM-5 zeolite having a surface coated with an amorphous silicon-containing oxide; a third catalyst comprising a binary composite oxide of iron and manganese; A catalyst group for producing paraxylene, comprising the first catalyst, the second catalyst, and the third catalyst, wherein at least the first catalyst and the second catalyst are present as a mixed granule.

2. The first catalyst contains 30% by mass or more and 70% by mass or less of chromium and 30% by mass or more and 70% by mass or less of zinc relative to the total amount of metals contained in the first catalyst, and 2. The catalyst group for producing paraxylene according to claim 1, wherein the third catalyst contains 90% by mass or more and 99% by mass or less of iron and 1% by mass or more and 10% by mass or less of manganese relative to a total amount of metals contained in the third catalyst.

3. The second catalyst is contained in an amount of 10% by mass or more and 1000% by mass or less relative to the first catalyst, and 2. The catalyst group for producing paraxylene according to claim 1, wherein the third catalyst is contained in an amount of 0.1 mass% or more based on the total amount of the first catalyst, the second catalyst, and the third catalyst.

4. A method for producing paraxylene, comprising the step of contacting carbon monoxide and hydrogen with the catalyst group for producing paraxylene according to any one of claims 1 to 3 to synthesize paraxylene.

5. 5. The method for producing paraxylene according to claim 4, wherein the third catalyst is arranged upstream of a flow direction of the carbon monoxide and the hydrogen, and the granulated material containing the first catalyst and the second catalyst is arranged downstream of the flow direction of the carbon monoxide and the hydrogen, and the gas obtained after contacting the carbon monoxide and the hydrogen with the third catalyst is brought into contact with the granulated material to synthesize paraxylene.

6. A method for producing the catalyst group for producing paraxylene according to any one of claims 1 to 3, comprising the steps of: A step of obtaining a composite hydroxide containing chromium and zinc by a coprecipitation method, and drying and / or calcining the composite hydroxide containing chromium and zinc to obtain the first catalyst; A step of performing hydrothermal synthesis or heating in the presence of a silicon compound and an H-ZSM-5 zeolite to obtain the second catalyst comprising an H-ZSM-5 zeolite the surface of which is coated with an amorphous silicon-containing oxide; obtaining a composite hydroxide containing iron and manganese by a coprecipitation method, and drying and / or calcining the composite hydroxide containing iron and manganese to obtain the third catalyst; A step of mixing at least the first catalyst and the second catalyst among the first catalyst, the second catalyst, and the third catalyst, and granulating the mixture to obtain the granules; The present invention relates to a method for producing a catalyst group for producing paraxylene, comprising the steps of: