Composition, adhesive, adhesive-based laminate, laminate production method, and laminate dismantling method
A Diels-Alder reaction-based adhesive composition with a maleimide dienophile and photopolymerization initiator addresses the limitations of conventional adhesives by offering strong bonding and easy dismantling at high temperatures, ensuring heat resistance and ease of handling.
Patent Information
- Application Number
- JP2024031676
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-01
- Publication Date
- 2024-10-07
AI Technical Summary
Conventional dismantling adhesives suffer from inferior adhesive strength, moisture resistance, durability, and heat resistance due to the addition of microcapsules and gas-generating agents, which also complicate handling and limit their applications.
A composition utilizing the Diels-Alder reaction with a maleimide-structured dienophile and a photopolymerization initiator, allowing for reversible bonding and easy dismantling at high temperatures, enhancing heat resistance and handling characteristics.
The composition provides excellent adhesive strength, heat resistance, and easy dismantling capabilities, suitable for applications requiring recyclability and durability.
Smart Images

Figure 2024137771000027 
Figure 2024137771000001 
Figure 2024137771000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition suitable for an adhesive that can easily perform bonding and disassembly, an adhesive, a laminate using the adhesive, a method for producing the laminate, and a method for disassembling the laminate, and also to a method for joining two members and a method for disassembling the joined members. [Background technology]
[0002] Dismantlable adhesives are adhesives whose adhesive strength is reduced by a specific stimulus after use, making it possible to easily dismantle the bonded (jointed) parts. From the perspective of efficient resource utilization and recycling, such as for separating and collecting different materials and replacing defective parts, dismantlable adhesives are becoming increasingly important in various technical fields.
[0003] A typical example of a dismantling adhesive is an adhesive that contains a foaming agent such as a thermally expandable microcapsule. When these adhesives are heated or immersed in warm water, the foaming agent in the adhesive expands, reducing the adhesive strength, allowing the bonded (jointed) parts to be dismantled and separated (Non-Patent Documents 1 and 2). Patent Document 1 discloses a photocurable, stimuli-release adhesive composition that contains a gas generating agent and generates gas in response to a stimulus. Patent Document 2 discloses a thermoreversible hot melt adhesive composition that has thermoreversible bonds and acrylate polymerization reactive groups, forms a polymer crosslinked body synthesized by free radical polymerization using an azo or peroxide as an initiator, and can be dismantled by heating to a threshold value or higher. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Materials Science and Engineering, 2004, Vol. 41, No. 2, 17-21 [Non-Patent Document 2] Journal of the Adhesion Society of Japan, 2008, Issue 44, No. 4, Paragraphs 19-24 [Patent documents]
[0005] [Patent Document 1] JP 2006-188586 A [Patent Document 2] Special Publication No. 2012-530150 Summary of the Invention [Problem to be solved by the invention]
[0006] The dismantlable adhesives disclosed in Non-Patent Documents 1 and 2 require the addition of a large amount of microcapsules, 30 to 50% by mass, and are considered to be inferior in adhesive strength, moisture resistance, durability, etc. of the adhesive itself. In particular, since the expansion start temperature of the thermal expansion material is low, if the bonded body is exposed to high temperatures during use, sufficient adhesive strength cannot be secured, and there is a possibility that there will be a problem with the heat resistance of the bonded body. The adhesive composition disclosed in Patent Document 1 may disintegrate at low temperatures due to the low thermal stability of the gas generating agent contained in the adhesive. Also, the adhesive composition disclosed in Patent Document 2 contains a polymer, which has a thickening effect that results in poor handling characteristics as an adhesive, and may limit the areas where it can be applied. As described above, all of the above-mentioned conventional technologies have had the problem that the heat resistance is reduced and the handling characteristics of the adhesive are deteriorated due to the additives that impart dismantling properties to the adhesive or the increase in molecular weight of the materials that make up the composition. In view of the above-mentioned circumstances, the present invention aims to provide a composition suitable for an adhesive that can easily perform bonding and disassembly, in particular a composition that has excellent heat resistance, good handling properties, and on-demand disassembly. It is also an object of the present invention to provide an adhesive made of the composition, a laminate using the adhesive, a method for producing the laminate, a method for disassembling the laminate, a method for joining two members, and a method for disassembling the joined members. [Means for solving the problem]
[0007] In developing a composition suitable for an adhesive that can easily perform bonding and disassembly, the present inventors focused on techniques that utilize reversible chemical bonds, and in particular conducted extensive research into the use of the Diels-Alder reaction. In the Diels-Alder (hereinafter sometimes referred to as "DA") reaction, a conjugated diene reacts with a dienophile to form a ring structure. This reaction is a thermoreversible equilibrium reaction, and it is known that at relatively high temperatures, a retro-Diels-Alder (hereinafter sometimes referred to as "rDA") reaction occurs, resulting in decomposition into the original conjugated diene and dienophile. The present inventors have found that the above-mentioned problems can be solved by using a dienophile having a maleimide structure instead of a chain-like unsaturated bond, and have thus completed the present invention. That is, the present invention relates to the following [1] to
[14] .
[0008] [1] A composition comprising a compound represented by the following formula (1) and a photopolymerization initiator:
[0009] [ka]
[0010] (In formula (1), X1 represents a divalent group. Y1 to Y4 each independently represent a hydrogen atom or a substituted or unsubstituted monovalent organic group, and at least one of the groups Y1 to Y4 is a group represented by the following formula (2) and formula (3). Z represents a substituted or unsubstituted trivalent to pentavalent organic group having 3 to 100 carbon atoms. n represents an integer of 3 to 5. The n structural units bonded to Z may be the same or different.)
[0011] [ka]
[0012] [ka]
[0013] (In formula (2), R 1 is an oxygen atom, a methylene group, or an alkylene group having 2 to 10 carbon atoms and which may have a branched structure, R 2 is a substituent of formula (3), R 3 , R 4 The bond is at one of the positions. * indicates a bond. 3 is an alkylene group consisting of 0 to 10 methylene groups, and R 4 is an alkylene group consisting of 1 to 5 methylene groups. 3 There are 0 methylene groups in R 4 When there is one methylene group in formula (3), the structure is not cyclic, and R 2 is R 4 ) [2] The composition according to the above [1], wherein in the formula (1), Z has an aromatic hydrocarbon group. [3] The composition according to [2] above, wherein Z contains a plurality of aromatic hydrocarbon groups, and the aromatic hydrocarbon groups are linked to each other by a linking group. [4] The composition according to any one of the above [1] to [3], wherein Z has at least one substituent selected from the group consisting of a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an aryl group, an alkenyl group, an alkynyl group, an alkoxy group, an alkylcarbonyl group, an ester group, a silyl group, and an amino group. [5] The composition according to any one of the above [1] to [4], wherein the compound represented by the formula (1) is thermally dissociable. [6] The composition according to any one of the above [1] to [5], wherein the content of the compound represented by the formula (1) in the total solid content is 30 mass % or more. [7] The composition according to any one of the above [1] to [6], further comprising an epoxy monomer. [8] An adhesive comprising the composition according to any one of [1] to [7] above. [9] A laminate having a substrate A, an adhesive layer, and a substrate B in this order, wherein the adhesive layer is a resin layer obtained by curing the composition according to any one of the above [1] to [7].
[10] The laminate according to the above [9], wherein at least one of the substrate A and the substrate B has a total light transmittance of 80% or more.
[11] A method for producing a laminate having a substrate A, an adhesive layer, and a substrate B in this order, comprising: a step (a) of applying the composition according to any one of the above [1] to [7] to the substrate A or the substrate B; a step (b) of bonding the substrate A and the substrate B together via the composition; and a step (c) of irradiating the composition with light to form an adhesive layer.
[12] A method for dismantling a laminate having a substrate A, an adhesive layer, and a substrate B in this order, wherein the adhesive layer is a resin layer obtained by curing the composition described in any one of [1] to [7] above, the method comprising the step of heating the adhesive layer to 100°C or higher.
[13] A method for joining two members, comprising: a step (d) of applying the composition according to any one of the above items [1] to [7] to at least one of the members; a step (e) of placing the other member on the applied composition; and a step (f) of curing the composition by irradiating the composition with light.
[14] A method for dismantling members joined by the method according to
[13] above, comprising the step of heating the cured adhesive layer to 100°C or higher. Effect of the Invention
[0014] According to the present invention, it is possible to provide a composition suitable for an adhesive which allows easy bonding and disassembly and has excellent heat resistance. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a conceptual diagram showing a method for producing a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] [Composition] <Compound represented by formula (1)> The composition of the present invention is characterized by containing a compound represented by the following formula (1) (hereinafter, may be referred to as "the compound of the present invention") and a photopolymerization initiator.
[0017] [ka]
[0018] (In formula (1), X1 represents a divalent group. Y1 to Y4 each independently represent a hydrogen atom or a substituted or unsubstituted monovalent organic group, and at least one of the groups Y1 to Y4 is a group represented by the following formula (2) and formula (3). Z represents a substituted or unsubstituted trivalent to pentavalent organic group having 3 to 100 carbon atoms. n represents an integer of 3 to 5. The n structural units bonded to Z may be the same or different.)
[0019] [ka]
[0020] [ka]
[0021] In formula (2), R 1 is an oxygen atom, a methylene group, or an alkylene group having 2 to 10 carbon atoms and which may have a branched structure, R 2 is a substituent of formula (3), R 3 , R 4 The bond is at one of the positions. * indicates a bond. 3 is an alkylene group consisting of 0 to 10 methylene groups, and R 4 is an alkylene group consisting of 1 to 5 methylene groups. 3 There are 0 methylene groups in R 4 When there is one methylene group in formula (3), the structure is not cyclic, and R 2 is R 4 is bound to.
[0022] X1 is not particularly limited as long as it is a divalent group that can stably maintain the structure of the compound of the present invention represented by formula (1). Specifically, it is preferably -O-, -S-, -NH-, -NR- (R is a hydrocarbon group having 1 to 20 carbon atoms), a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms, a substituted or unsubstituted phenylene group having 6 to 20 carbon atoms, and a substituted or unsubstituted silylene group having 2 to 20 carbon atoms (-Si(R 11 )R 12 -;R 11 and R 12 each independently represents an alkyl group having 1 to 20 carbon atoms.) Among these, X1 is preferably -O- from the viewpoints of small steric hindrance, stability of the compound according to the present invention, heat resistance, and ease of procurement of raw materials. When X1 is an alkylene group, a phenylene group, or a silylene group (hereinafter sometimes referred to as "alkylene group, etc.") having a substituent, the substituent is not particularly limited. Specific examples include a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, an alkylcarbonyl group, an ester group, etc. When X1 has a plurality of these substituents, adjacent substituents may be linked to each other to form a ring. From the viewpoint of making it easier to obtain a composition with strong adhesive strength without steric hindrance, when X1 has a carbon atom, the number of carbon atoms is preferably small. Specifically, when X1 has a carbon atom, the number of carbon atoms is preferably 1 to 20, and more preferably 1 to 10. For the same reason, when X1 is a divalent group having a substituent, the number of the substituents is preferably small.
[0023] As described above, Y1 to Y4 each independently represent a hydrogen atom or a substituted or unsubstituted monovalent organic group, and at least one of Y1 to Y4 is a group represented by the above formula (2) and formula (3). Y1 to Y4 other than the groups represented by formula (2) and formula (3) (hereinafter, sometimes referred to as "other Y1 to Y4") are preferably hydrogen atoms or organic groups having a small number of carbon atoms in terms of the stability, heat resistance, and ease of procurement of raw materials of the compound represented by formula (1). Specifically, when other Y1 to Y4 are organic groups, the number of carbon atoms of other Y1 to Y4 is preferably 1 to 50, more preferably 1 to 30, further preferably 1 to 20, and particularly preferably 1 to 10. Examples of the organic groups of other Y1 to Y4 include substituted or unsubstituted phenylene groups and substituted or unsubstituted silylene groups. Most preferably, other Y1 to Y4 are hydrogen atoms. Other Y1 to Y4 may be linked to each other to form a ring. When the other Y1 to Y4 are organic groups having a substituent, the substituent is not particularly limited, and examples thereof include a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an aryl group, an alkenyl group, an alkynyl group, an alkoxy group, an alkylcarbonyl group, an ester group, a silyl group, and an amino group.
[0024] As mentioned above, R 1 is an oxygen atom, a methylene group, or an alkylene group having 2 to 10 carbon atoms which may have a branched structure.
[0025] As mentioned above, R 2 is a substituent of formula (3), R 3 , R 4 It is bound to one of the positions.
[0026] As mentioned above, R 3 is an alkylene group having 0 to 10 linked methylene groups. From the viewpoints of the stability of the compound according to the present invention and the curability of the composition according to the present invention, the number of carbon atoms is preferably 0 to 7, and more preferably 0 to 5.
[0027] As mentioned above, R 4is an alkylene group having 1 to 5 linked methylene groups. From the viewpoints of the stability of the compound according to the present invention and the curability of the composition according to the present invention, the number of carbon atoms is preferably 1 to 3, and more preferably 1 or 2.
[0028] As mentioned above, R 3 There are 0 methylene groups in R 4 When there is one methylene group in formula (3), the structure is not cyclic, and R 2 is R 4 is bound to.
[0029] As described above, Z represents a substituted or unsubstituted trivalent or more and pentavalent or less organic group having 3 to 100 carbon atoms. When Z is a trivalent or more and pentavalent or less organic group, a multi-branched crosslinked structure is likely to be formed. The number of carbon atoms in Z is preferably large in terms of ease of synthesis of the compound according to the present invention and the difficulty of steric hindrance, and is preferably small in terms of the viscosity of the composition containing the compound according to the present invention that is easy to handle. Therefore, Z is preferably 3 or more, more preferably 4 or more, even more preferably 5 or more, and particularly preferably 6 or more, and is preferably 80 or less, and more preferably 60 or less.
[0030] Z is -O- (ether bond), -CO- (carbonyl bond), -COO- (ester bond), -Si(R 11 )R 12 - (silylene bond), -NHCO- (amide bond), -SO2- (sulfonyl bond), -NR 13 It may be an organic group having a bond such as an -(amino bond), etc. Furthermore, when Z is an aromatic group, it may be a single ring or a condensed ring, or it may be a heterocyclic aromatic group having a hetero atom.
[0031] Z is preferably a substituted or unsubstituted hydrocarbon group in terms of increasing solubility in low polarity solvents. When Z is a substituted or unsubstituted hydrocarbon group, the hydrocarbon group may be linear or cyclic, saturated or unsaturated. It may also be a group in which two or more types of hydrocarbon groups are bonded.
[0032] More specifically, the number of carbon atoms in the hydrocarbon group is preferably 1 to 20 when the hydrocarbon group is a chain hydrocarbon group, preferably 5 to 20 when the hydrocarbon group is an alicyclic hydrocarbon group, and preferably 4 to 60 when the hydrocarbon group is an aromatic hydrocarbon group (including the case where the hydrocarbon group is a heterocyclic aromatic hydrocarbon group), more preferably 4 to 30, and even more preferably 6 to 30.
[0033] In view of increasing the solubility of the compound according to the present invention in low polarity solvents, Z preferably has a substituted or unsubstituted aromatic hydrocarbon group, more preferably has a substituted aromatic hydrocarbon group. In addition, Z preferably has a plurality of aromatic hydrocarbon groups, more preferably the aromatic hydrocarbon groups are linked together by a linking group. Examples of this linking group include a linear alkylene group having 1 to 5 carbon atoms.
[0034] When the organic group of Z has a substituent, the substituent is not particularly limited. For example, a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an aryl group, an alkenyl group, an alkynyl group, an alkoxy group, an alkylcarbonyl group, an ester group, a silyl group, and an amino group can be mentioned. Here, these substituents may be bonded to each other to form a ring.
[0035] Specific examples of Z include the following organic groups. [ka] [ka]
[0036] [ka]
[0037] [ka]
[0038] [ka]
[0039] [ka]
[0040] [ka]
[0041] In the above structural formula, * represents a bond, and p, q, and r each independently represent an integer of 1 or more. As described above, in formula (1), the n structural units bonded to Z may be the same or different. From the viewpoint of facilitating desorption (dismantling) of the substrate or member at a constant temperature, it is preferable that the n structural units are identical. On the other hand, from the viewpoint of facilitating desorption (dismantling) of the substrate or member in stages, it is preferable that at least one of the n structural units is different from the other structural units. In other words, by binding a structural unit having a different structure to Z, it is possible to adjust the desorption temperature (dismantling temperature) of the substrate or member.
[0042] The molecular weight of the compound according to the present invention is not particularly limited. However, it is preferable that the molecular weight is low in terms of the viscosity of the compound according to the present invention being low and easy to handle, and on the other hand, it is preferable that the molecular weight is high in terms of forming a multi-branched structure. Therefore, it is preferably 100 or more, more preferably 150 or more, and on the other hand, it is preferably 10,000 or less, more preferably 3,000 or less, and even more preferably 1,000 or less. Here, when Z of the compound according to the present invention is an addition reactant or a polymer, the molecular weight is the number average molecular weight measured by GPC.
[0043] The compounds according to the present invention have a DA reactive site (bicyclo[2.2.1]hept-2-ene structure), and therefore can be synthesized from a dienophile and a diene. Specifically, the compound according to the present invention can be synthesized from a dienophile (A) and a diene (B) as shown in the following reaction formula. The DA reaction site (bicyclo[2.2.1]hept-2-ene structure) in formula (1) dissociates into a diene and a dienophile by the rDA reaction under heating. Therefore, the compound according to the present invention that is crosslinked by this structure also has thermal dissociation properties.
[0044] [ka]
[0045] The diene (B) has at least one polymerizable group represented by the following formula (2) or (3).
[0046] [ka]
[0047] [ka]
[0048] R in Equation (2) 1 , R 2and R in formula (3) 3 , R 4 is as described above. * represents a bond. R 1 , R 2 , R 3 and R 4 The preferred embodiments of are also as described above. That is, at least one of Y1 to Y4 is a group represented by the above formula (2) and formula (3), and the compound according to the present invention can be photopolymerized by the polymerizable group, and has photocurability.
[0049] Examples of the diene compound used as the diene (B) include furan, thiophene, pyrrole, cyclopentadiene, silacyclopentadiene (silole), etc. From the viewpoints of stability and reactivity of the diene compound, ease of handling, and ease of availability of raw materials, furan is preferred.
[0050] The dienophile (A) used in the synthesis of the compound according to the present invention is characterized by having a polyfunctional maleimide structure. By making the maleimide structure a polyfunctional maleimide structure instead of a chain-like unsaturated bond, the stability and heat resistance of the compound according to the present invention are increased. As the dienophile (A), various known polyfunctional maleimide compounds can be used.
[0051] From the viewpoints of solubility, stability of the compound according to the present invention, heat resistance, and ease of procurement of raw materials, the dienophile (A) preferably has the following structure.
[0052] [ka]
[0053] (In the formula, q is an integer equal to p-2.) As the dienophile (A), for example, a polyfunctional maleimide compound manufactured by Dainippon Ink and Chemicals, Inc. can be used.
[0054] When synthesizing the compound according to the present invention, the molar equivalent ratio of dienophile (A) to diene (B) (diene (B) / dienophile (A) ratio) is preferably 2.0 times or more, since almost all bismaleimide groups in the dienophile (A) react with the diene (B), and the adhesive strength is unlikely to decrease due to unreacted dienophile (A). There is no particular limit to the upper limit of the ratio, but it is preferably 5.0 or less from the viewpoint of the stability (adhesiveness, dismantling ability) of the compound according to the present invention.
[0055] As one example of the synthesis of the compound represented by formula (1), the reaction of furfuryl glycidyl ether with a polyfunctional maleimide (where q=1 in the above formula) is shown below.
[0056] [ka]
[0057] The content of the compound according to the present invention in the composition of the present invention is preferably high in terms of excellent adhesive strength and dismantling property when heated. Specifically, it is preferably 30% by mass or more. In addition, taking into consideration the amount of components other than the compound according to the present invention, such as a photopolymerization initiator described later, the content of the compound according to the present invention is more preferably 40% by mass or more, and on the other hand, it is preferably 98% by mass or less, and more preferably 95% by mass or less. However, when adhesives other than the compound according to the present invention (hereinafter sometimes referred to as "other adhesives") are used in combination, it is preferable that the total amount of the compound according to the present invention and the other adhesives is within the above-mentioned range.
[0058] The content of the compound according to the present invention in the composition of the present invention is 1 It can be confirmed by H-NMR measurement. More specifically, the content of the compound according to the present invention is 1 This can be confirmed by absolute quantification (internal standard method) of H-NMR. 1 The absolute amount of the compound according to the present invention can be quantified by adding a known amount of a standard substance to the H-NMR measurement solution.
[0059] <Photopolymerization initiator> The photopolymerization initiator is a component that polymerizes and cures the photocurable resin composition of the present invention when irradiated with active energy rays such as ultraviolet rays. In the present invention, both cationic initiators and radical initiators can be used as the photopolymerization initiator. However, cationic initiators are preferred because they can efficiently promote the polymerization of epoxy groups.
[0060] Specific examples of the photopolymerization initiator include triarylsulfonium salts (commercially available products; CPI-100, 200, 300, 400 series), diaryliodonium salts (commercially available products; IK-1 series), diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2- Hydroxy-2-methyl-1-propan-1-one, benzyl dimethyl ketal, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone (commercially available; Omnirad 184), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone Acetophenones such as Panone oligomer; benzoins such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether; benzophenone, o-benzoyl methyl benzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyl-diphenyl sulfide, 3,3',4,4'-tetra(t-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzophenone, 4-benzoyl-N,N-dimethyl-N -Benzophenones such as [2-(1-oxo-2-propenyloxy)ethyl]benzenemethanaminium bromide and (4-benzoylbenzyl)trimethylammonium chloride; thioxanthones such as 2-isopropylthioxanthone, 4-isopropylthioxanthone, 2,4-diethylthioxanthone, 2,4-dichlorothioxanthone, 1-chloro-4-propoxythioxanthone, and 2-(3-dimethylamino-2-hydroxy)-3,4-dimethyl-9H-thioxanthone-9-one mesochloride;Acylphosphine oxides such as 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethyl-pentylphosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)phenyl-, 2-(O-benzoyloxime)], ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime); The photopolymerization initiator may be used alone or in combination of two or more kinds.
[0061] The content of the photopolymerization initiator in the composition of the present invention is not particularly limited. However, it is preferable that the content is high in terms of being easily cured sufficiently and exhibiting strong adhesive strength, and on the other hand, it is preferable that the content is low in terms of being excellent in heat resistance. Therefore, specifically, the content of the photopolymerization initiator is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, particularly preferably 1% by mass or more, and especially preferably 1.5% by mass or more, and on the other hand, it is preferably 20% by mass or less, more preferably 18% by mass or less, even more preferably 16% by mass or less, particularly preferably 14% by mass or less, and especially preferably 12% by mass or less.
[0062] <Other ingredients> In addition to the compound represented by the above formula (1), the photocurable resin composition of the present invention may contain, if necessary, a known photosensitizer such as ethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, amyl 4-dimethylaminobenzoate, or 4-dimethylaminoacetophenone.
[0063] <Epoxy monomer> From the viewpoint of curing speed and coatability (adjustment of viscosity), the composition of the present invention preferably further contains at least one monomer selected from the epoxy group. Any epoxy resin can be used as the epoxy resin, and specific examples thereof include bisphenol A type epoxy resin, bisphenol F type epoxy resin, epoxy resin having an oxazolidone ring skeleton, novolac type epoxy resin, triglycidylaminophenol, tetraglycidyldiaminodiphenylmethane, hydrophthalic acid type epoxy resin, bisphenol S type epoxy resin, resorcin type epoxy resin, hydroquinone type epoxy resin, bisphenoxyethanolfluorene type epoxy resin, bisphenolfluorene type epoxy resin, biscresolfluorene type epoxy resin, etc. Among these, one or more epoxy resins selected from bisphenol A type epoxy resin, bisphenol F type epoxy resin, epoxy resin having an oxazolidone ring skeleton, novolac type epoxy resin, triglycidylaminophenol, and tetraglycidyldiaminodiphenylmethane are preferred. It is preferable to use a liquid epoxy resin and a solid epoxy resin in combination, which will be described later. In particular, by combining a plurality of these epoxy resins, excellent handleability can be achieved.
[0064] <Liquid epoxy resin> The liquid epoxy resin is an epoxy resin that is liquid at 25°C. The liquid epoxy resin mainly contributes to improving the solubility of the thermoplastic resin and improving the strength, elastic modulus, and heat resistance of the resin cured product of the resin composition. The term "liquid" here means that the epoxy resin exhibits fluidity. The viscosity of the epoxy resin that is liquid at 25°C is preferably 500 mPa·s or less at 25°C, more preferably 300 mPa·s or less. It is also preferably 0.1 mPa·s or more. When the viscosity is within this range, the workability of the resin composition can be improved. The viscosity can be measured by applying periodic deformation (strain) to the sample with a rotational rheometer and detecting the resulting stress and phase difference.
[0065] The liquid epoxy resin may be a commercially available product. Examples of commercially available bisphenol A type epoxy resins (liquid epoxy resins) that are liquid at 25°C include, but are not limited to, jER827 (epoxy equivalent 185g / eq), jER828 (epoxy equivalent 189g / eq) (all manufactured by Mitsubishi Chemical Corporation), YD-127 (epoxy equivalent 185g / eq), YD-128 (epoxy equivalent 189g / eq) (all manufactured by Nippon Steel Chemical & Material Co., Ltd.), EPICLON840 (epoxy equivalent 185g / eq), EPICLON850 (epoxy equivalent 189g / eq) (all manufactured by DIC Corporation), DER331 (epoxy equivalent 187 / eq), DER332 (epoxy equivalent 173g / eq) (manufactured by The Dow Chemical Company). Commercially available bisphenol F type epoxy resins (liquid epoxy resins) that are liquid at 25°C include, but are not limited to, jER806 (epoxy equivalent 165g / eq), jER807 (epoxy equivalent 170g / eq) (manufactured by Mitsubishi Chemical Corporation), YDF-170 (epoxy equivalent 170g / eq) (manufactured by Nippon Steel Chemical & Material Co., Ltd.), EPICLON830 (epoxy equivalent 170g / eq), EPICLON835 (epoxy equivalent 172g / eq) (manufactured by DIC Corporation), DER354 (epoxy equivalent 170g / eq) (manufactured by The Dow Chemical Company), etc. One of these may be used alone, or two or more may be used in combination.
[0066] <Solid epoxy resin> The solid epoxy resin is preferably a bisphenol type epoxy resin having a softening point of 70° C. or more. The softening point is preferably 72° C. or more, more preferably 75° C. or more, so that the cured resin has excellent toughness. On the other hand, the softening point is preferably 100° C. or less, more preferably 95° C. or less, so that the heat resistance of the cured resin is appropriately maintained.
[0067] Commercially available solid epoxy resins may be used. Commercially available bisphenol A type epoxy resins having a softening point of 70° C. or higher include, but are not limited to, jER1055, jER1004, jER1007, and jER1009 (all trade names, manufactured by Mitsubishi Chemical Corporation), EPICLON2050, EPICLON3050, EPICLON4050, EPICLON7050, EPICLON HM-091, and EPICLON HM-101 (all trade names, manufactured by DIC Corporation), and YD-902, YD-903N, YD-904, YD-907, YD-7910, and YD-6020 (all trade names, manufactured by Nippon Steel Chemical & Material Co., Ltd.). In addition, examples of commercially available bisphenol F type epoxy resins having a softening point of 70°C or higher include, but are not limited to, jER4004P, jER4005P, jER4007P, jER4010P (all trade names, manufactured by Mitsubishi Chemical Corporation), YDF2004, YDF-2005RD (all trade names, manufactured by Nippon Steel Chemical & Material Co., Ltd.), and the like. Examples of epoxy resins having an oxazolidone ring structure and a softening point of 70° C. or higher that are commercially available include AER4152, AER4151, LSA3301, LSA2102 (all trade names, manufactured by Asahi Kasei E-Materials Corporation), ACR1348 (trade name, manufactured by ADEKA Corporation), DER852, DER858 (trade names, manufactured by The Dow Chemical Company), and TSR-400 (trade name, manufactured by DIC Corporation), and all of these are preferably used in the present invention, with AER4152 and TSR-400 being particularly preferred. As the solid epoxy resin, one of these may be used alone, or two or more may be used in combination.
[0068] When these monomers are used, one type may be used alone, or two or more types may be used in combination.
[0069] <Solvent> The composition of the present invention may further contain a solvent. By containing a solvent, the viscosity of the composition can be adjusted.
[0070] Examples of the solvent include alcohols such as methanol, ethanol, propanol, n-butanol, and i-butanol; ketones such as acetone, methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone; cellosolves such as ethyl cellosolve; aromatics such as toluene and xylene; glycol ethers such as propylene glycol monomethyl ether; acetates such as methyl acetate, ethyl acetate, and butyl acetate; tetrahydrofuran, diacetone alcohol, etc. When a solvent is used, one type of solvent may be used alone, or two or more types may be used in combination. When a solvent is used, from the viewpoints of evaporation rate and coating property (adjustment of viscosity), a low polarity solvent such as acetone, methyl isobutyl ketone, methyl ethyl ketone, etc. is preferable. The compound according to the present invention has high solubility in low polarity solvents, and is therefore suitable for compositions containing low polarity solvents. When a solvent is used, the content in the composition is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less. When the composition of the present invention is used as an adhesive or the like, after the composition of the present invention is applied, the solvent is usually removed by drying.
[0071] <Other ingredients> The composition of the present invention may contain components other than those described above, within the scope of not significantly impairing the effects of the present invention. Specifically, conventionally known additives such as antistatic agents, antioxidants, leveling agents, rheology control agents, colorants, fillers, antioxidants, ultraviolet absorbers, and functional dyes can be used. The content of these components is preferably 30% by mass or less, more preferably 20% by mass or less, of the solid content of the composition of the present invention (when the composition of the present invention contains a solvent, the components other than the solvent). In addition to these additives, the composition may contain small amounts of impurities such as unreacted raw materials used in the production of the composition.
[0072] [Composition] The composition of the present invention can be obtained by mixing the above-mentioned components. In addition, by polymerizing the composition of the present invention, the composition of the present invention becomes a cured resin and exhibits an adhesive function. Therefore, the composition of the present invention can be suitably used as an adhesive (hereinafter, sometimes referred to as the "adhesive of the present invention"). The polymerization can be carried out by irradiation with light.
[0073] The viscosity of the composition of the present invention at 25° C. is usually 1 to 100,000 mPa·s, preferably 1 to 50,000 mPa·s, and particularly preferably 2 to 30,000 mPa·s. Therefore, the composition of the present invention is suitable for use as an adhesive, etc., in that it has excellent coatability (even and easy to apply).
[0074] The glass transition temperature (Tg) of the compound according to the present invention is preferably high in terms of excellent heat resistance, and is preferably low in terms of ease of dismantling when the composition of the present invention is used as an easily dismantled adhesive. Specifically, the glass transition temperature is preferably 20°C or higher, more preferably 50°C or higher, and is preferably 250°C or lower, more preferably 200°C or lower. The glass transition temperature can be measured by a method such as dynamic viscosity measurement (DMA measurement).
[0075] [Laminate] When the composition of the present invention is used as an adhesive, two substrates can be bonded by the adhesive of the present invention. That is, by using the composition of the present invention as an adhesive, a laminate having, in this order, a substrate A, a resin layer obtained by curing the composition of the present invention, and a substrate B (hereinafter, sometimes referred to as the "laminate of the present invention") can be obtained. The laminate of the present invention may have layers other than the substrate A, the substrate B, and the adhesive layer.
[0076] <Base material> Examples of the material of the substrate A and the substrate B include plastic, glass, and metal. Examples of plastics include polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyolefins such as polypropylene and polyethylene; polyamides; polycarbonates; and poly(meth)acrylic resins. Examples of the glass include alkali glass, non-alkali glass, and quartz glass.
[0077] The shape of the substrate is not particularly limited, and examples thereof include a film, a sheet, a plate, and various three-dimensional shapes. The thickness of the substrate is not particularly limited as long as light and heat can be sufficiently applied to the adhesive sandwiched between the substrate A and the substrate B. From this viewpoint, for example, the thickness of each of the substrate A and the substrate B may be as thin as several μm. In order to improve adhesion, the substrate may be subjected to a surface treatment. Specific examples include corona treatment, surface abrasion treatment, etc. Alternatively, a primer layer or a surface modification layer may be provided, and these surface treatments may be performed on the surface. When substrate A and substrate B are bonded with the composition of the present invention, at least one of substrate A and substrate B preferably has a total light transmittance of 80% or more.
[0078] <Adhesive layer> The laminate of the present invention has a resin layer formed by curing the composition of the present invention as an adhesive layer. The thickness of the adhesive layer is appropriately set according to the application, but it is preferable that it is thick to some extent in terms of easy adhesion strength, and on the other hand, when laminating a minute substrate or a thin substrate, it is preferable to make it thin. Therefore, specifically, it is preferable to make it 1 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, and on the other hand, it is preferable to make it 10 mm or less, more preferably 5 mm or less, even more preferably 2 mm or less, and particularly preferably 1 mm or less.
[0079] [Method of manufacturing laminate] The laminate of the present invention can be produced by applying a composition that is cured by irradiation with light to one substrate, laminating the other substrate via the composition, and then irradiating the composition with light to form an adhesive layer. That is, the method for producing the laminate of the present invention includes a step (a) of applying the composition of the present invention to substrate A or substrate B, a step (b) of laminating substrate A and substrate B via the composition, and a step (c) of irradiating the composition with light to form an adhesive layer.
[0080] The method of applying the composition in step (a) is not particularly limited and can be performed by a known method.Specific examples of the method include bar coating, applicator, curtain flow coating, roll coating, spray, gravure coating, comma coating, reverse roll coating, lip coating, die coating, slot die coating, air knife coating, and dip coating.In addition, in step (a), the composition may be applied to both substrates.
[0081] In step (b), the two substrates may be pressed together. The pressing may be performed using a machine. In step (c), the composition of the present invention is cured by irradiating it with light having a wavelength capable of curing the composition of the present invention, such as ultraviolet light, to form an adhesive layer.
[0082] The light source used in step (c) is not particularly limited as long as it can cure the composition of the present invention. For example, a high pressure mercury lamp, an electrodeless lamp, an ultra-high pressure mercury lamp, a carbon arc lamp, a xenon lamp, a metal halide lamp, a chemical lamp, a black light, an LED lamp, and the like can be used as the light source.
[0083] The amount of light irradiation in step (c) is not particularly limited as long as it can cure the composition of the present invention. However, a high amount is preferable in terms of sufficient curing and high adhesive strength, while a low amount is preferable in terms of easy and quick operation. Specifically, for example, when ultraviolet light is used as the light source, the cumulative light amount is 2 to 20,000 mJ / cm. 2 It is preferable to set the range to 10 to 10,000 mJ / cm 2 More preferably, it is 100 to 10,000 mJ / cm 2 It is even more preferable to set the range to 1,000 to 8,000 mJ / cm 2 It is more preferable that: When the composition of the present invention contains a solvent, it is preferable to provide a drying step prior to the step (c) and remove the solvent by heating or the like.
[0084] [Method of joining components] When the composition of the present invention is used as an adhesive, two members can be bonded together via the adhesive. The materials, shapes, etc. of the members to be bonded together are the same as those of the substrate of the laminate described above. The bonding of the two members can be carried out in the same manner as in the case of producing the laminate described above. Specifically, the two members can be bonded by applying a composition that is cured by irradiation with light to one member, laminating the other member via the composition, and then irradiating the composition with light to form an adhesive layer. That is, the method for bonding members of the present invention includes a step (d) of applying the composition of the present invention to at least one member, a step (e) of placing the other member on the composition, and a step (f) of curing the composition by irradiating the composition with light. Here, the steps (d) to (f) can be carried out in the same manner as the above-mentioned steps (a) to (c), respectively.
[0085] [How to disassemble the laminate] As described above, the compound according to the present invention undergoes an rDA reaction by heating, and dissociates into a diene and a dienophile. Thus, a laminate bonded with the adhesive of the present invention can be disassembled by heating. Specifically, a laminate having a substrate A, a resin layer (adhesive layer) formed by curing the composition of the present invention, and a substrate B in this order can be disassembled by heating the adhesive layer. That is, a method for disassembling a laminate having a substrate A, a resin layer (adhesive layer) formed by curing the composition of the present invention, and a substrate B in this order includes a step of heating the adhesive layer.
[0086] The heating conditions may be a temperature at which the rDA reaction proceeds or higher, and appropriate depending on the time required for dismantling and the heat resistance of the substrate, member, etc. Specifically, for example, the heating is preferably performed at 100°C or higher, more preferably at 120°C or higher, and even more preferably at 140°C or higher, while on the other hand, the heating is preferably performed at 300°C or lower, and more preferably at 250°C or lower. The heating time may be set appropriately depending on the heating method and heating temperature, but is preferably 5 seconds or more, more preferably 10 seconds or more, even more preferably 20 seconds or more, and particularly preferably 1 minute or more, and is preferably 2 hours or less, more preferably 1 hour or less, and even more preferably 50 minutes or less.
[0087] The heating method is not particularly limited as long as it can sufficiently transmit heat to the adhesive layer. For example, a method of heating the entire laminate by thermal conduction, a method of locally heating using electromagnetic waves such as infrared rays, microwaves, and white light, etc. can be mentioned. The heating device is not particularly limited, and any known heating device can be used, specifically, a hot plate, a hot air dryer, a heat gun, a dryer, etc. It is also possible to mix a conductive filler into the adhesive and heat the adhesive layer using an electromagnetic induction heating device. It is also possible to fill the adhesive with microwave-responsive particles (e.g., iron nanoparticles) and heat the adhesive layer using a microwave heating device.
[0088] [How to dismantle joint components] The bonded members bonded via the adhesive of the present invention can be dismantled in the same manner as the above-mentioned method for dismantling a laminate. That is, the method for dismantling members bonded by the above-mentioned method for bonding members of the present invention includes a step of heating the cured adhesive layer. Here, the heating conditions, heating method, heating device, etc. can each be performed in the same manner as in the above-mentioned method for dismantling a laminate of the present invention. In this way, by utilizing the adhesive function and thermal dissociation properties of the adhesive of the present invention, bonding, joining, and disassembly can be easily performed, and as an easily dismantlable adhesive, the bonding and disassembly of two substrates or two components can be easily performed.
[0089] <Applications of laminates> The laminate of the present invention has excellent heat resistance and is therefore useful as various optical parts and devices, electronic parts, precision instruments, and packaging materials that are placed in high-temperature environments. EXAMPLES
[0090] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0091] <Raw materials> The abbreviations of the raw materials and solvents used in the examples and comparative examples are as follows. (Photopolymerization initiator) CPI-400S: Photoresponsive cationic polymerization initiator (San-Apro Co., Ltd., triarylsulfonium salt) has the following structure:
[0092] [ka]
[0093] (solvent) Acetone (Wako Pure Chemical Industries, special grade reagent, boiling point 56°C)
[0094] <Base material (I), base material (II)> Slide glass (material: high-grade soda glass): width 26 mm x length 76 mm x thickness 1.3 mm Aluminum plate: Width 45mm x Length 120mm x Thickness 0.5mm -Iron plate: Width 45mm x Length 120mm x Thickness 0.5mm Copper plate: Width 45mm x Length 120mm x Thickness 0.5mm Polymethyl methacrylate (PMMA) plate: width 45 mm x length 120 mm x thickness 0.5 mm The substrate was rinsed with acetone and dried before use.
[0095] (Synthesis Example 1) [Preparation of thermally dissociable crosslinking monomer (M1)] 2.1 g of furfuryl glycidyl ether (Sigma-Aldrich, purity 95%) was added to 2.2 g of polyfunctional phenylmethanemaleimide (BMI-2300, Daiwa Chemical Industry Co., Ltd.), and the mixture was reacted at 60° C. for 1 day. 1 The progress of the reaction was confirmed from the disappearance of the peak at δ 6.86 ppm derived from the maleimide structure in the results of H-NMR measurement, and a thermally dissociable crosslinking monomer (M1) was obtained.
[0096] [ka]
[0097] < 1 H-NMR measurement> 1 H-NMR measurements were performed using a nuclear magnetic resonance apparatus (ADVANCE NEO400 (400 MHz) manufactured by Bruker Japan). Deuterated chloroform was used as the solvent. Measurements were performed at a solid content concentration of 1.0 mass% and an accumulation count of 16, and peaks were assigned based on chemical shifts and integral values.
[0098] (Synthesis Example 2) [Preparation of thermally dissociable crosslinking monomer (M2)] 51.25g of 2,5-bis(hydroxymethyl)furan and 2.57g of tetrabutylammonium bromide as a catalyst were added to 313ml of epichlorohydrin, heated at 65℃ for 5 hours, and then cooled to 30℃. Then, 200ml of 50% aqueous sodium hydroxide solution was gradually added under stirring to react, and the mixture was left to stand for 1 day. The reactant was extracted three times into dichloromethane, and the remaining solvent was washed with deionized water, and then MgSO4 was added and dehydrated several times. After the solvent was completely separated using a rotary evaporator, the mixture was purified by chromatography through a silica gel column using a mixed solvent of ethyl acetate and hexane (volume ratio 2:1) as the developing solvent, and 2,5-furfuryl diglycidyl ether was obtained. Next, in the same manner as in Synthesis Example 1, 3.3 g of the 2,5-furfuryl diglycidyl ether obtained above was added to 2.2 g of polyfunctional phenylmethanemaleimide (BMI-2300, manufactured by Daiwa Chemical Industry Co., Ltd.), and the mixture was dissolved by heating and stirring at 60°C for 1 hour, followed by reaction at 50°C for 3 days. 1 The progress of the reaction was confirmed from the disappearance of the peak at δ 6.47 ppm derived from the maleimide structure in the results of H-NMR measurement, and a thermally dissociable crosslinking monomer (M2) was obtained.
[0099] [ka]
[0100] [Production Example 1] (Preparation of Adhesive Composition) 1.0 g of the thermally dissociable crosslinking monomer (M1) prepared in Synthesis Example 1 was weighed out. 10 parts by mass of a photopolymerization initiator was added to 100 parts by mass of the monomer, and the mixture was stirred and mixed at room temperature (20° C.) for 2 hours to produce an adhesive composition (MA1).
[0101] [Production Example 2] 0.75 g of the thermally dissociable crosslinking monomer (M1) prepared in Synthesis Example 1 was dissolved in 0.25 g of acetone. 10 parts by mass of a photopolymerization initiator was added per 100 parts by mass of the resulting solution, and the mixture was stirred and mixed at room temperature (20° C.) for 2 hours to produce an adhesive composition (MA2).
[0102] [Example 1] Slide glasses were used as the substrates (I) and (II). As shown in FIG. 1, 61 mg (1 in FIG. 1) of adhesive composition (MA1) containing photopolymerization initiator CPI-400S produced in Production Example 1 was applied to an area of 26 mm×26 mm at the edge of substrate (II) (2 in FIG. 1), and substrate (I) (3 in FIG. 1) was placed on top and pressed. Next, an electrodeless ultraviolet irradiation device, Heraeus "FUSION LightHammer 6" (using D bulb, main wavelength 385 nm), was used to apply an accumulated light amount of 5000 mJ / cm. 2 The adhesive composition was cured by irradiating with ultraviolet light under the above conditions to produce a laminate composed of the substrate (I), the adhesive layer (1' in FIG. 1) and the substrate (II).
[0103] [Example 2] In Example 1, a laminate consisting of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that a slide glass was used as the substrate [I] and an iron plate was used as the substrate [II], and the amount of adhesive composition (MA1) applied was 62 mg.
[0104] [Example 3] In Example 1, a laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that a slide glass was used as the substrate [I] and an aluminum plate was used as the substrate [II], and the amount of adhesive composition (MA1) applied was 61 mg.
[0105] [Example 4] In Example 1, a laminate consisting of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that a slide glass was used as the substrate [I] and a copper plate was used as the substrate [II], and the amount of adhesive composition (MA1) applied was 61 mg.
[0106] [Example 5] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that PMMA plates were used as the substrates [I] and [II] and the amount of adhesive composition (MA1) applied was 64 mg.
[0107] [Example 6] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that 65 mg of the adhesive composition (MA2) produced in Production Example 2 was applied instead of the adhesive composition (MA1) in Example 1.
[0108] [Example 7] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 2, except that 55 mg of the adhesive composition (MA2) produced in Production Example 2 was applied instead of the adhesive composition (MA1).
[0109] [Production Example 3] (Preparation of Adhesive Composition) 1.0 g of the thermally dissociable crosslinking monomer (M2) prepared in Synthesis Example 2 was weighed out. 10 parts by mass of a photopolymerization initiator was added to 100 parts by mass of the monomer, and the mixture was stirred and mixed at 50° C. for 8 hours to produce an adhesive composition (MA3).
[0110] [Example 8] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that 51 mg of the adhesive composition (MA3) produced in Production Example 3 was applied instead of the adhesive composition (MA1) in Example 1.
[0111] [Example 9] In Example 8, a laminate consisting of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 8, except that a slide glass was used as the substrate [I] and an iron plate was used as the substrate [II], and the amount of adhesive composition (MA3) applied was 52 mg.
[0112] [Example 10] In Example 8, a laminate consisting of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 8, except that a slide glass was used as the substrate [I] and an aluminum plate was used as the substrate [II], and the amount of adhesive composition (MA3) applied was 55 mg.
[0113] [Example 11] In Example 8, a laminate consisting of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 8, except that a slide glass was used as the substrate [I] and a copper plate was used as the substrate [II], and the amount of adhesive composition (MA3) applied was 53 mg.
[0114] [Comparative Manufacturing Example 1] 100 parts by mass of (3',4'-Epoxycyclohexene)methyl 3,4-epoxycyclohexenecarboxylate (alicyclic epoxy C2021P, manufactured by Daicel Corporation) and 10 parts by mass of photopolymerization initiator CPI-400S were prepared and mixed with stirring at room temperature (20°C) for 2 hours to produce an adhesive composition (C1).
[0115] [Comparative Manufacturing Example 2] 0.75 g of (3',4'-epoxycyclohexene)methyl 3,4-epoxycyclohexenecarboxylate (alicyclic epoxy C2021P, manufactured by Daicel Corporation) was dissolved in 0.25 g of acetone. 10 parts by mass of a photopolymerization initiator was added per 100 parts by mass of the solution, and the mixture was stirred and mixed at room temperature (20°C) for 2 hours to produce an adhesive composition (C2).
[0116] [Comparative Example 1] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that 56 mg of the adhesive composition (C1) produced in Comparative Production Example 1 was applied instead of the adhesive composition (MA1).
[0117] [Comparative Example 2] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 2, except that 59 mg of the adhesive composition (C1) produced in Comparative Production Example 1 was applied instead of the adhesive composition (MA1).
[0118] [Comparative Example 3] A laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 1, except that 58 mg of the adhesive composition (C2) produced in Comparative Production Example 2 was applied instead of the adhesive composition (MA1).
[0119] [Comparative Example 4] In Example 2, a laminate composed of a substrate (I), an adhesive layer (1' in Figure 1) and a substrate (II) was produced in the same manner as in Example 2, except that 63 mg of the adhesive composition (C2) produced in Comparative Production Example 2 was applied instead of the adhesive composition (MA1).
[0120] <Evaluation of adhesiveness of laminate> Either the substrate [I] or the substrate [II] of the laminate was pinched with the fingers and evaluated for adhesion. As a result, the substrate [I] and the substrate [II] could not be separated in either laminate, and the adhesion was good.
[0121] <Evaluation of dismantling ability of laminated body at room temperature (20℃)> At room temperature (20°C), the substrates [I] and [II] in the laminate were pulled by hand in the tensile shear test direction to evaluate whether the substrates [I] and [II] could be disassembled. As a result, none of the laminates disassembled.
[0122] <Evaluation of dismantling property of laminate at 150℃> The laminate was heated on a hot plate set at 150°C for 20 minutes, and the substrate [II] was held down with tweezers while the substrate [I] was pulled with tweezers in the tensile shear direction to evaluate whether it could be disassembled. The evaluation results are shown in Table 1. In Table 1, if the substrate could be disassembled, the time required to disassemble it is recorded. If it could not be disassembled, it was recorded as "impossible to disassemble."
[0123] [Table 1]
[0124] The results of evaluating the adhesion and dismantling properties of the laminates of Examples 1 to 7 produced by bonding two substrates together using the compositions of Production 1 and 2 as an adhesive, and the results of evaluating the adhesion and dismantling properties of the laminates of Examples 8 to 11 produced by bonding two substrates together using the composition of Production Example 3 as an adhesive, support the fact that the composition of the present invention allows the two substrates to be easily bonded and dismantled by heating. In addition, the results of the evaluation at different heating temperatures support the fact that the composition did not dismantle below 100°C, but dismantled at 150°C, which supports its high heat resistance. It was demonstrated that by bonding substrates using the composition of the present invention, the produced laminate could be dismantled by the very simple method of heating, making it possible to recycle the substrates. [Explanation of symbols]
[0125] 1. Adhesive 1' Adhesive layer (cured product of adhesive composition) 2...Base material (II) 3...Base material (I)
Claims
1. A composition comprising a compound represented by the following formula (1) and a photopolymerization initiator: 【Chemistry 1】 (In formula (1), X 1 represents a divalent group. 1 ~Y 4 each independently represents a hydrogen atom or a substituted or unsubstituted monovalent organic group; Y 1 ~Y 4 At least one of the groups is a group represented by the following formula (2) and formula (3). Z represents a substituted or unsubstituted organic group having 3 to 100 carbon atoms and a valence of 3 to 5. n represents an integer of 3 to 5. The n structural units bonded to Z may be the same or different. 【Chemistry 2】 【Chemistry 3】 (In formula (2), R 1 is an oxygen atom, a methylene group, or an alkylene group having 2 to 10 carbon atoms and which may have a branched structure, R 2 is a substituent of formula (3), R 3 , R 4 The bond is at one of the positions. * represents a bond. 3 is an alkylene group having 0 to 10 methylene groups linked together, and R 4 is an alkylene group having 1 to 5 methylene groups linked together. 3 There are 0 methylene groups in R 4 When there is one methylene group in formula (3), the structure does not become a ring structure, and R 2 is R 4 is bonded to.)
2. The composition according to claim 1 , wherein in formula (1), Z has an aromatic hydrocarbon group.
3. The composition according to claim 2 , wherein Z comprises a plurality of aromatic hydrocarbon groups, the aromatic hydrocarbon groups being linked together by a linking group.
4. The composition according to any one of claims 1 to 3, wherein Z has at least one substituent selected from the group consisting of a halogen atom, a hydroxyl group, a nitro group, a cyano group, an alkyl group, an aryl group, an alkenyl group, an alkynyl group, an alkoxy group, an alkylcarbonyl group, an ester group, a silyl group, and an amino group.
5. The composition according to any one of claims 1 to 3, wherein the compound represented by formula (1) has thermal dissociation properties.
6. The composition according to any one of claims 1 to 3, wherein the content of the compound represented by formula (1) in the total solid content is 30 mass% or more.
7. The composition of any one of claims 1 to 3, further comprising an epoxy monomer.
8. An adhesive comprising the composition according to any one of claims 1 to 3.
9. A laminate having a substrate A, an adhesive layer, and a substrate B in this order, wherein the adhesive layer is a resin layer obtained by curing the composition according to any one of claims 1 to 3.
10. 10. The laminate according to claim 9, wherein at least one of the substrate A and the substrate B has a total light transmittance of 80% or more.
11. A method for producing a laminate having a substrate A, an adhesive layer, and a substrate B in this order, the method comprising the steps of: (a) applying the composition according to any one of claims 1 to 3 to the substrate A or the substrate B; (b) bonding the substrate A and the substrate B together via the composition; and (c) irradiating the composition with light to form an adhesive layer.
12. A method for dismantling a laminate having a substrate A, an adhesive layer, and a substrate B in this order, the adhesive layer being a resin layer obtained by curing the composition according to any one of claims 1 to 3, the method comprising the step of heating the adhesive layer to 100°C or higher.
13. A method for joining two members, comprising: a step (d) of applying the composition according to any one of claims 1 to 3 to at least one of the members; a step (e) of placing the other member on the applied composition; and a step (f) of curing the composition by irradiating the composition with light.
14. A method for dismantling members joined by the method according to claim 13, comprising the step of heating the cured adhesive layer to 100° C. or higher.
Citation Information
Patent Citations
JP,2008,44,
Stimulation-peelable adhesive composition, method for bonding and peeling member using stimulation-peelable adhesive composition, surface protection film, method for protecting surface of object to be protected and surface protection layer
JP2006188586A
A thermoreversible hot-melt adhesive composition containing polyfunctional dienes and dienophile compounds.
JP2012530150A