Resin molding
A resin molded article using a polymerizable composition with methyl methacrylate and a crosslinking agent controls high temperature tensile elongation to address webbing defects and maintain heat resistance, enhancing moldability and accuracy of complex shapes.
Patent Information
- Application Number
- JP2024032421
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-04
- Publication Date
- 2024-10-07
AI Technical Summary
Molded products containing (meth)acrylic resins often suffer from defects such as webbing during molding, particularly when forming complex shapes with curved parts, and there is a need to suppress these defects while maintaining heat resistance.
A resin molded article is produced using a polymerizable composition containing methyl methacrylate and a crosslinking agent, with controlled high temperature tensile elongation, to suppress webbing and maintain heat resistance.
The solution effectively suppresses webbing during molding and maintains the heat resistance inherent to methacrylic polymers, allowing for improved dimensional accuracy and moldability of complex shapes.
Smart Images

Figure 2024137773000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin molded product. More specifically, the present invention relates to a resin molded product containing a crosslinked (meth)acrylic polymer obtained by polymerizing a polymerizable composition (S2), the polymerizable composition (S2) containing a monomer composition (S1) containing methyl methacrylate and a crosslinking agent (A), and the resin molded product has a specific high-temperature tensile elongation. [Background technology]
[0002] (Meth)acrylic resins are excellent in transparency, heat resistance, and weather resistance, and also have well-balanced performance in terms of mechanical strength, thermal properties, moldability, etc. For this reason, they are used in many applications such as lighting materials, optical materials, signs, displays, decorative materials, and building materials, and in recent years, they are also used in sanitary products and kitchenware. Sanitary products and kitchen utensils tend to have complex shapes, including curved parts, unlike signs and the like which are constructed with flat surfaces. Therefore, sanitary products or kitchen utensils may require a high degree of moldability, such as bending or deep drawing. It is known that (meth)acrylic resins may have thickness unevenness at curved portions when they are subjected to bending or deep drawing by heating, etc. Also, it is known that (meth)acrylic resins are prone to necking during heat stretching, making deep drawing and other processes difficult. Patent Document 1 discloses that a resin molded product obtained by molding a resin composition containing a crosslinking agent, which uses a methacrylic resin having a storage modulus in a specific rubber-like flat region and a peak value of tan δ in the dynamic viscoelastic properties, can improve the dimensional accuracy of a curved portion obtained when the curved portion is formed by bending or deep drawing or the like. Patent Document 2 discloses that by using a methacrylic resin composition containing a crosslinker and a citric acid ester having a specific boiling point, it is possible to provide a cast plate that can be subjected to bending, deep drawing, and other processes with higher dimensional accuracy. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2015 / 122174 [Patent Document 2] International Publication No. 2018 / 168954 Summary of the Invention [Problem to be solved by the invention]
[0004] However, molded articles containing (meth)acrylic resins may still suffer from defects during molding, such as webbing, and there is a need to suppress such defects. An object of the present invention is to solve such problems. That is, one object of the present invention is to provide a resin molded article that suppresses defects such as the occurrence of webbing during molding. Another object of the present invention is to provide a resin molded article which suppresses defects such as the occurrence of webbing during molding and which maintains the heat resistance inherent to methacrylic polymers. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to achieve the above object, and have found that the resin molded product of the present invention can be obtained by polymerizing a polymerizable composition (S2) containing a monomer composition (S1) containing methyl methacrylate and a crosslinking agent (A) to obtain a resin molded product containing a crosslinked (meth)acrylic polymer, and that by controlling the high-temperature tensile elongation of the obtained resin molded product within a specific range, defects such as the occurrence of webbing during molding can be suppressed, thereby completing the present invention. Furthermore, the present inventors have found that the resin molded product generally maintains the heat resistance inherent to a methacrylic polymer.
[0006] That is, the present invention has the following aspects. (1) A resin molded product comprising a (meth)acrylic polymer obtained by polymerizing a polymerizable composition (S2), The polymerizable composition (S2) comprises a monomer composition (S1) containing methyl methacrylate and a crosslinking agent (A), a resin molded product, the resin molded product having a high-temperature tensile elongation at 160°C of 700% or less; (2) The resin molded article according to (1), wherein the high-temperature tensile elongation is 450% or less. (3) The resin molded product according to (1) or (2), which contains the crosslinking agent (A) in an amount of 0.2 to 6.0 parts by mass per 100 parts by mass of the total mass of the polymerizable composition (S2); (4) The resin molded article according to any one of (1) to (3), wherein the (meth)acrylic polymer contains 80 mass% or more of structural units derived from methyl methacrylate; (5) The resin molded article according to any one of (1) to (4), wherein the crosslinking agent (A) contains at least one selected from the group consisting of ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; (6) The resin molded article according to any one of (1) to (5), wherein the crosslinking agent (A) contains at least one member selected from the group consisting of ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, and polybutylene glycol di(meth)acrylate; (7) The (meth)acrylic polymer according to any one of (1) to (6) contains a non-crosslinked (meth)acrylic polymer, The resin molded article according to any one of (1) to (6), wherein the non-crosslinked (meth)acrylic polymer has a mass average molecular weight of 10,000 or more and 700,000 or less; or (8) The resin molded article according to any one of (1) to (7), which is a sanitary product or a kitchenware. Effect of the Invention
[0007] According to the present invention, it is possible to provide a resin molded article in which defects such as the generation of webbing during molding are suppressed. It is also possible to provide a resin molded article in which defects such as the generation of webbing during molding are suppressed and which maintains the heat resistance inherent to a methacrylic polymer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will be described in detail below. The following definitions of terms apply throughout the specification and claims, unless otherwise stated.
[0009] The term "(meth)acrylic polymer" is a concept including a polymer obtained by polymerizing the same (meth)acrylic monomer, a copolymer obtained by polymerizing different (meth)acrylic monomers, and a copolymer obtained by polymerizing the same or different (meth)acrylic monomers and a monomer other than the (meth)acrylic monomer. In other words, the term "(meth)acrylic polymer" may be any one of a polymer or copolymer selected from a polymer obtained by polymerizing the same (meth)acrylic monomer, a copolymer obtained by polymerizing different (meth)acrylic monomers, and a copolymer obtained by polymerizing the same or different (meth)acrylic monomers and a monomer other than the (meth)acrylic monomer, or a mixture of two or more of them. Therefore, a "(meth)acrylic polymer" is a polymer or copolymer that contains structural units derived from the same or different (meth)acrylic monomers and may further contain structural units derived from monomers other than (meth)acrylic monomers. Here, "derived from" means that the chemical structure has been changed due to polymerization.
[0010] Among "(meth)acrylic polymers", those that are crosslinked are referred to as "crosslinked (meth)acrylic polymers", and those that are not crosslinked are referred to as "non-crosslinked (meth)acrylic polymers". Here, "crosslinking" has the usual meaning in this technical field, and refers to chemically bonding polymer molecules together. The molecules that are crosslinked may themselves be crosslinked or non-crosslinked. The "(meth)acrylic polymer" includes a "crosslinked (meth)acrylic polymer" and may further include a "non-crosslinked (meth)acrylic polymer".
[0011] "(Meth)acrylate" is a general term for acrylate and methacrylate, "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, and "(meth)acryloyl group" is a general term for acryloyl group and methacryloyl group. The term "(meth)acrylic monomer" refers to a monomer having an acryloyl group or a methacryloyl group.
[0012] The term "structural unit" refers to a structural unit derived from a polymerizable monomer formed by polymerization of a polymerizable monomer, or a structural unit in which a portion of the structural unit is converted into a different structure by treating a polymer.
[0013] The term "resin molded product" refers to a product formed by molding a resin composition, and may be, for example, a planar shape, i.e., a sheet, or a three-dimensional shape, such as a cylindrical or granular primary molded product. The sheet may be a film or a plate. Here, the term "film" refers to a sheet with a thickness of less than 1 mm, and the term "plate" refers to a sheet with a thickness of 1 mm or more. The term also refers to the primary molded product and a secondary molded product formed from the primary molded product.
[0014] A "sanitary product" is a product that is applied to sanitary facilities other than kitchens or commercial kitchens, and may be, for example, a product that is applied to or used in a bathroom, washroom, or toilet booth. A "kitchen appliance" may be a product that is applied to equipment in a kitchen or a commercial kitchen, or that is used in a kitchen or a commercial kitchen. Here, the "kitchen" may be a kitchen in a private home, a commercial kitchen, or a kitchen in a place of business.
[0015] "Webbing" may typically refer to paddle-like projections that appear at the corners of a molded article during molding.
[0016] <Resin molded body> In one embodiment, the resin molded product is a resin molded product comprising a (meth)acrylic polymer obtained by polymerizing a polymerizable composition (S2) described later, and the resin molded product has a high-temperature tensile elongation at 160°C of 700% or less. When the resin molded article has a high-temperature tensile elongation at 160° C. of 700% or less, defects such as the occurrence of webbing during molding can be suppressed. Furthermore, when the resin molded article has a high-temperature tensile elongation at 160° C. of 700% or less, the inherent heat resistance of the methacrylic polymer can be maintained.
[0017] The resin molded article preferably has a high-temperature tensile elongation of 650% or less, more preferably 600% or less, and most preferably 450% or less at 160° C. When the high-temperature tensile elongation at 160° C. is 450% or less, the effect of suppressing the occurrence of webbing or the effect of maintaining heat resistance may be more significant. The resin molded article preferably has a high-temperature tensile elongation of 250% or more at 160° C., more preferably 270% or more, particularly preferably 290% or more, and most preferably 310% or more. When the high-temperature tensile elongation at 160° C. is 310% or more, the moldability of the resulting resin composition is favorable. Therefore, the high temperature tensile elongation of the resin molded product at 160° C. is, for example, preferably from 250 to 700%, more preferably from 270 to 650%, further preferably from 290 to 600%, and particularly preferably from 310 to 450%. In this specification, the high-temperature tensile elongation at 160° C. of the resin molded product can be measured by the method described later in <Method of measuring high-temperature tensile elongation (elongation at break (%))>.
[0018] <(Meth)acrylic polymer> The (meth)acrylic polymer of the present invention is a polymer obtained by polymerizing the polymerizable composition (S2). The definition of "(meth)acrylic polymer" has the above meaning, and may include the non-crosslinked (meth)acrylic polymer described below.
[0019] Among them, the (meth)acrylic polymer is preferably a copolymer containing a structural unit derived from methyl methacrylate and a structural unit derived from a vinyl monomer other than methyl methacrylate that is copolymerizable with methyl methacrylate (hereinafter, also simply referred to as a "vinyl monomer"). The vinyl monomer will be described later. In this specification, the term "structural unit" refers to a unit derived from a monomer formed by polymerization of the monomer. The structural unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by processing the polymer.
[0020] From the viewpoint of heat resistance and thermal stability of the resin composition and the resin molded body, the content ratio of the structural unit derived from methyl methacrylate is preferably 50 to 100% by mass, and the content ratio of the structural unit derived from vinyl monomer is preferably 0 to 50% by mass, based on the total mass of the (meth)acrylic polymer. The content ratio of the structural unit derived from methyl methacrylate is more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more, based on the total mass of the (meth)acrylic polymer. Moreover, the content ratio of the structural unit derived from vinyl monomer is more preferably 40% by mass or less, even more preferably 30% by mass or less, particularly preferably 20% by mass or less, and most preferably 10% by mass or less, based on the total mass of the (meth)acrylic polymer. Therefore, in the (meth)acrylic polymer, the content of the structural unit derived from methyl methacrylate is, for example, more preferably 60 to 100% by mass, further preferably 70 to 100% by mass, particularly preferably 80 to 100% by mass, and most preferably 90 to 100% by mass, relative to the total mass of the (meth)acrylic polymer. Also, the content of the structural unit derived from a vinyl monomer is, for example, more preferably 0 to 40% by mass, further preferably 0 to 30% by mass, and particularly preferably 0 to 20% by mass, relative to the total mass of the (meth)acrylic polymer.
[0021] When the (meth)acrylic polymer is a copolymer, the arrangement of the copolymer is not particularly limited and may be, for example, a random copolymer, a block copolymer, an alternating copolymer, or the like, with a random copolymer being preferred.
[0022] <Polymerizable composition (S2)> The polymerizable composition (S2) of the present invention contains, as essential components, a monomer composition (S1) containing methyl methacrylate and a crosslinking agent (A).
[0023] [Other additives] The polymerizable composition (S2) of the present invention may further contain, as necessary, additives selected from chain transfer agents, polymerization initiators, release agents, lubricants, plasticizers, antistatic agents, light stabilizers, UV absorbers, flame retardants, flame retardant assistants, polymerization inhibitors, antioxidants, fillers, pigments, dyes, silane coupling agents, leveling agents, defoamers and fluorescent agents. These may be used alone or in any combination of two or more kinds in any ratio.
[0024] As the polymerization initiator, a known one can be used, for example, azo compounds such as 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), etc.; organic peroxides such as benzoyl peroxide, cumene hydroperoxide, lauryl peroxide, di-t-butyl peroxide, t-butylperoxy-2-ethylhexanoate, t-hexylperoxypivalate, etc. The content of the polymerization initiator is not particularly limited and can be set appropriately.
[0025] In one embodiment, the amount of the polymerization initiator in the polymerizable composition (S2) may be 0.001 to 1.0 part by mass, more preferably 0.015 to 0.50 part by mass, and particularly preferably 0.030 to 0.40 part by mass, based on 100 parts by mass of the total mass of the polymerizable composition (S2). When the amount of the polymerization initiator is within the above range, the polymerization reaction between the (meth)acrylic monomer, the (meth)acrylic monomer and / or the monomer other than the (meth)acrylic monomer and the crosslinking agent (A) can be appropriately controlled.
[0026] The chain transfer agent may be a known one, for example, mercaptans such as n-dodecyl mercaptan (also called 1-dodecanethiol), thioglycolic acid esters such as octyl thioglycolate, α-methylstyrene dimer, terpinolene, etc. The content of the chain transfer agent is not particularly limited and may be appropriately set.
[0027] <Monomer composition (S1)> The monomer composition (S1) is a composition containing methyl methacrylate. Since the resin molded product of the present invention contains a (meth)acrylic polymer described below, the monomer composition (S1) is a composition containing a monomer that is a raw material of the (meth)acrylic polymer.
[0028] The content ratio of methyl methacrylate contained in the monomer composition (S1) is not particularly limited, but from the viewpoint of improving the heat resistance, transparency, and mechanical strength of the obtained resin molded body, it is preferable that the monomer composition (S1) contains methyl methacrylate as a main component, and the content of methyl methacrylate is preferably 50 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and may be 100 mass%, relative to the total mass of the monomer composition (S1) (100 mass%).
[0029] The monomer composition (S1) may contain methyl methacrylate and the vinyl monomer, that is, the monomer composition (S1) may be a monomer composition consisting of 50 to 100% by mass of methyl methacrylate and 0 to 50% by mass of a vinyl monomer, or a partial polymer thereof, or a mixture thereof.
[0030] The vinyl monomer constituting the monomer composition (S1) is not particularly limited as long as it is a monomer copolymerizable with methyl methacrylate, and examples thereof include methyl acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and (meth)acrylic acid. Hydrocarbon group-containing (meth)acrylic acid esters such as hexadecyl, nonyl (meth)acrylate, isononyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, isobornyl (meth)acrylate, 3,5,5-trimethylcyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, terpene acrylate and derivatives thereof, hydrogenated rosin acrylate and derivatives thereof, and docosyl (meth)acrylate;
[0031] hydroxyl group-containing (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate;
[0032] Examples of the (meth)acrylic monomer include (meth)acrylic acid, 2-(meth)acryloyloxyethyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxyethyl phthalic acid, 2-(meth)acryloyloxypropyl phthalic acid, 2-(meth)acryloyloxyethyl maleic acid, 2-(meth)acryloyloxypropyl maleic acid, 2-(meth)acryloyloxyethyl succinic acid, and 2-(meth)acryloyloxypropyl succinic acid, and at least one of the above (meth)acrylic monomers is selected.
[0033] Examples of the "monomer other than the (meth)acrylic monomer" constituting the (meth)acrylic polymer include vinyl monomers such as styrene, α-methylstyrene, vinyl toluene, (meth)acrylonitrile, vinyl chloride, vinyl acetate, and vinyl propionate; Cyano group-containing vinyl monomers such as acrylonitrile and methacrylonitrile;
[0034] Vinyl monomers containing an amide group, such as (meth)acrylamide, Nt-butyl(meth)acrylamide, N-methylol(meth)acrylamide, N-isopropylacrylamide, hydroxyethylacrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone acrylamide, maleic acid amide, and maleimide; Examples of the vinyl monomer include vinyl monomers containing an acid anhydride group such as maleic anhydride and itaconic anhydride.
[0035] Among them, the vinyl monomer is preferably an acrylic acid ester or styrene, which improves the thermal stability of the resulting resin molded article.
[0036] When the vinyl monomer is an acrylic acid ester, the monomer composition (S1) preferably contains 70 to 100 mass% of methyl methacrylate and 0 to 30 mass% of acrylic acid ester, based on the total mass of the monomer composition (S1).When the vinyl monomer is styrene, the monomer composition (S1) preferably contains 50 to 100 mass% of methyl methacrylate and 0 to 50 mass% of styrene.
[0037] The acrylic acid ester is preferably an acrylic acid ester having an alkyl group having 1 to 11 carbon atoms in the side chain, and examples thereof include methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, t-butyl acrylate, and 2-ethylhexyl acrylate. These may be used alone or in any ratio and combination of two or more. Among these, from the viewpoint of the thermal stability of the resin composition and the resin molded product, at least one selected from the group consisting of methyl acrylate, ethyl acrylate, and n-butyl acrylate is preferred, and methyl acrylate and ethyl acrylate are more preferred.
[0038] The vinyl monomers can be used alone or in any combination of two or more kinds in any ratio.
[0039] <Crosslinking agent (A)> The crosslinking agent (A) used in the present invention is not particularly limited, but for example, a monomer having at least two (meth)acryloyl groups in the molecule is preferable, and more specifically, ethylene glycol di(meth)acrylate, 1,3-propylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate (also called 1,3-butanediol di(meth)acrylate), 1,4-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dimethylolethane di(meth)acrylate, 1,1-dimethylolpropane di(meth)acrylate. , 2,2-dimethylolpropane di(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 2,2-bis[4-((meth)acryloxyethoxy)phenyl]propane, 2,2-bis[4-((meth)acryloxypentenoxy)phenyl]propane, 1,4-bis((meth)acryloyloxymethyl)cyclohexyl di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate.
[0040] In addition, in a resin molded article including a resin composition containing the crosslinking agent (A), from the viewpoint of suppressing defects (webbing) during molding, the crosslinking agent (A) is preferably ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate (also referred to as 1,3-butanediol di(meth)acrylate), neopentyl glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, or polyethylene glycol di(meth)acrylate, and more preferably ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate (also referred to as 1,3-butanediol di(meth)acrylate), or polybutylene glycol di(meth)acrylate.
[0041] One or more compounds may be selected from the above-mentioned crosslinking agents (A) and used in the production of a crosslinked (meth)acrylic polymer.
[0042] The crosslinking agent (A) can be obtained as a commercially available product or can be produced and obtained by a method known per se.
[0043] By appropriately selecting and polymerizing the one or more monomers and the crosslinking agent (A) by type and amount, etc., and adjusting the molecular weight, etc., of the (meth)acrylic polymer, it is possible to adjust the properties of the resin molded article molded from the resin composition, and the high-temperature tensile elongation at 160°C can be adjusted to 700% or less.
[0044] In one embodiment, the (meth)acrylic polymer can be produced by polymerizing a polymerizable composition (S2) including a monomer composition (S1) containing methyl methacrylate and, if desired, a monomer selected from monomers other than methyl methacrylate, and a crosslinking agent (A).
[0045] In one embodiment, the (meth)acrylic polymer may contain a non-crosslinked (meth)acrylic polymer.
[0046] "Non-crosslinked (meth)acrylic polymer" The (meth)acrylic polymer of the present invention may contain a non-crosslinked (meth)acrylic polymer. The non-crosslinked (meth)acrylic polymer is obtained by polymerizing the monomer composition (S1) of the polymerizable composition (S2) without crosslinking. In other words, if the monomer composition (S1) is one type, it may contain a homopolymer, and if it is two or more types, it may contain a copolymer.
[0047] A polymerization initiator may be added to the monomer composition (S1) in advance, separately from the polymerization initiator contained in the polymerizable composition (S2) of the present invention, and a composition containing the prepolymer (B) (hereinafter referred to as "syrup") may be contained in the polymerizable composition (S2) by polymerizing a part of the monomer composition (S1) with the polymerization initiator. In one embodiment of the present invention, the (meth)acrylic polymer can be produced by subjecting a polymerizable composition (S2) obtained by mixing the prepolymer (B), the monomer composition (S1) and the crosslinking agent (A) in the polymerizable composition (S2) to a polymerization reaction.
[0048] The polymerization method for polymerizing the part is not particularly limited, but examples thereof include bulk polymerization, suspension polymerization, emulsion polymerization, and dispersion polymerization. Among these, the bulk polymerization is preferably used from the viewpoint of productivity of the resin molded article of the present invention. In one embodiment, the bulk polymerization method is preferably carried out in an atmosphere of an inert gas such as nitrogen. For example, the bulk polymerization method can be carried out by heating the monomer or a monomer composition comprising a combination of two or more monomers to 50 to 120°C, preferably 60 to 100°C, and more preferably 65 to 80°C, and when the monomer or monomer composition reaches the above temperature, a radical polymerization initiator and a chain transfer agent are added, and then the temperature is further increased by 20 to 40°C from the above temperature and maintained for 5 to 40 minutes.
[0049] The mass average molecular weight of the prepolymer (B) is preferably from 10,000 to 700,000, more preferably from 50,000 to 550,000, further preferably from 70,000 to 300,000, particularly preferably from 80,000 to 150,000, and most preferably from 90,000 to 120,000. When the mass average molecular weight of the prepolymer (B) is not less than the above lower limit, the chemical resistance and heat resistance of the resulting resin molded article tend to be excellent, whereas when it is not more than the above upper limit, the adhesion and releasability of the resulting resin molded article tend to be excellent.
[0050] The mass average molecular weight of the prepolymer (B) can be measured by the method described later in <Method for measuring mass average molecular weight of prepolymer (B)>. In this specification, the mass average molecular weight is a value measured by gel permeation chromatography using standard polystyrene as a standard sample.
[0051] The content of the (meth)acrylic polymer in the resin molded body is preferably 80 to 99.999 mass%, more preferably 85 to 99.99 mass%, even more preferably 90 to 99.9 mass%, and particularly preferably 95 to 99.0 mass%, relative to the total mass of the resin molded body. When the content of the (meth)acrylic polymer in the resin molded body is within the above range, it is easy to suppress defects such as the occurrence of webbing during molding of the resin molded body, and it is also easy to maintain the heat resistance that the methacrylic polymer inherently has.
[0052] The polymerization method applied to the polymerization of the (meth)acrylic monomer, the (meth)acrylic monomer and / or the monomer other than the (meth)acrylic monomer with the crosslinking agent (A) is not particularly limited, and examples thereof include bulk polymerization, suspension polymerization, emulsion polymerization and dispersion polymerization. Among them, from the viewpoint of productivity of the resin molded article of the present invention, the bulk polymerization is preferably applied, and among the bulk polymerization methods, the cast polymerization (also called casting polymerization) is preferable.
[0053] When the cast polymerization method is applied, since it is necessary to inject the polymerizable composition (S2) into a mold, it is preferable that the viscosity of the polymerizable composition (S2) is within an appropriate range, and it is preferable that the polymerizable composition (S2) obtained by mixing the prepolymer (B), a syrup containing a monomer selected from a (meth)acrylic monomer and a monomer other than a (meth)acrylic monomer, the crosslinking agent (A), and a polymerization initiator is polymerized to obtain a resin composition.
[0054] The content of the prepolymer (B) in the syrup may be, for example, 5 to 50% by mass, preferably 10 to 35% by mass, based on the total mass of the syrup. When the content of the (meth)acrylic polymer is within the above range, the viscosity of the polymerizable composition (S2) becomes within a range suitable for injection into a mold, and the polymerization reaction of the crosslinking agent (A) also proceeds smoothly.
[0055] In one embodiment, the blending amount of the crosslinking agent (A) in the polymerizable composition (S2) may be 0.01 to 6.0 parts by mass, more preferably 0.05 to 5.0 parts by mass, more preferably 0.07 to 4.0 parts by mass, more preferably 0.1 to 3.0 parts by mass, even more preferably 0.3 to 1.5 parts by mass, and particularly preferably 0.4 to 0.6 parts by mass, based on 100 parts by mass of the total mass of the polymerizable composition (S2). In another embodiment, the blending amount of the crosslinking agent (A) in the polymerizable composition (S2) may be 0.2 to 6.0 parts by mass, based on 100 parts by mass of the total mass of the polymerizable composition (S2). By appropriately adjusting the amount of the crosslinking agent (A) and the composition ratio of the monomer composition (S1), the mass average molecular weight and the like of the preliminary polymer (B) can be adjusted to an appropriate range. Furthermore, by appropriately adjusting the amount and type of the crosslinking agent (A) and the type of the monomer composition (S1), the high-temperature tensile elongation at 160°C of the resin molded product containing the crosslinked (meth)acrylic polymer can be adjusted to 700% or less.
[0056] If desired, other additives may be added to the polymerizable composition (S2). Examples of other additives include plasticizers, colorants such as pigments or dyes, ultraviolet absorbers, antioxidants, dispersants, fillers, release agents, and other resins different from the above-mentioned resins, and one or more of these may be selected as desired. The other additives are preferably added to the polymerizable composition (S2) for cast polymerization, for example. The content of the other additives can be appropriately adjusted depending on the purpose.
[0057] In one embodiment, the cast polymerization method may be a cell casting method in which the polymerizable composition (S2) is injected into a mold composed of two inorganic glass plates or metal plates (e.g., SUS plates) facing each other with the periphery sealed with a gasket made of soft resin or the like, and heated. The heating can be carried out by heating the mold into which the polymerizable composition (S2) has been poured at 60 to 150°C, preferably 70 to 140°C, more preferably 80 to 130°C, for 30 minutes to 2 hours, preferably 45 to 75 minutes, more preferably 60 minutes. The heating can be carried out stepwise, for example, by heating the mold at 60 to 90°C, preferably 70 to 90°C, more preferably 80°C, for 15 to 45 minutes, preferably 20 to 40 minutes, more preferably 30 minutes, and then heating at 110 to 150°C, preferably 120 to 140°C, more preferably 130°C, for 15 to 45 minutes, preferably 20 to 40 minutes, more preferably 30 minutes. As a heating means, a water bath or an air oven, etc., in which the temperature is appropriately controlled, can be applied. The gap between the mold voids can be appropriately adjusted so as to obtain a resin molded product of the desired thickness, and is usually 1 to 30 mm, and preferably 1 to 15 mm.
[0058] In another embodiment, the cast polymerization method may be a continuous casting method in which the polymerizable composition (S2) is continuously injected from upstream using a space sealed by two stainless steel endless belts, each having a mirror finish on one side, traveling in the same direction at the same speed and sealed by a gasket as a mold, and heated to continuously polymerize the composition. In the continuous casting method, the traveling speed of the endless belt can be adjusted so that the polymerizable composition (S2) injected into a mold is heated to a heating temperature and for a heating time equivalent to those in the cell casting method. The gap between the mold voids can be appropriately adjusted so as to obtain a resin molded product of the desired thickness, and is usually 1 to 30 mm, and preferably 1 to 15 mm.
[0059] After the polymerization is completed, the plate-shaped resin molded body can be removed from the mold. In this specification, the plate-shaped resin molded body may be referred to as a primary molded product or a cast plate. The thickness of the plate-shaped resin molded body is determined according to the gap of the mold used in the cast polymerization method, and may usually be 1 to 30 mm. If desired, a secondary molded product having a curved portion can be produced by subjecting the plate-like resin molded product (primary molded product) to bending and / or deep drawing. The primary molded product may be processed by vacuum molding, pressure molding, heat press molding, etc. The vacuum molding, pressure molding, heat press molding, etc. may be processed under known molding conditions.
[0060] In one embodiment, the vacuum molding of the primary molded product is performed by placing the primary molded product heated to 150 to 250°C, preferably 160 to 230°C, more preferably substantially 220°C, on a mold, and creating a vacuum between the primary molded product and the mold, thereby sucking the primary molded product into the mold. Either a male mold (convex mold) or a female mold (concave mold) can be used as the mold, and thin-walled secondary molded products and relatively large secondary molded products such as bathtubs can be produced.
[0061] <Use of resin molded bodies> The primary molded product of the resin molded body provided by the present invention is useful as a material for forming various secondary molded products because the occurrence of defects such as webbing is suppressed when a molded product having a curved portion is manufactured by performing bending or deep drawing. In addition, by using the primary molded product of the resin molded body provided by the present invention, a secondary molded product having small thickness unevenness at the curved portion and high dimensional accuracy can be manufactured. This secondary molded product can be applied to the sanitary field, the kitchen field, signboards and building materials, small boat hulls, electrical appliance body parts, automobile body parts, etc., and can be preferably used in the sanitary field such as bathtubs, bathrooms, and washrooms, and in the kitchen field such as the top plate of a system kitchen, etc., and is therefore useful for manufacturing sanitary products including bathtubs, kitchenware, etc. That is, in one embodiment, the resin molded article of the present invention can be used as a molding material for sanitary products, kitchenware, etc. It is particularly preferably used as a molding material for bathtubs. In another embodiment, the resin molded article of the present invention is a sanitary product, a kitchen utensil, etc. It is particularly preferably used as a bathtub.
[0062] The present invention will be further described below with reference to examples, but the present invention is not limited to these. EXAMPLES
[0063] <Compound abbreviation> The abbreviations of the compounds used in the examples and comparative examples are shown below. MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation, product name: Acryester M) BA: n-Butyl acrylate (manufactured by Mitsubishi Chemical Corporation) EDMA: Ethylene glycol dimethacrylate (manufactured by Mitsubishi Chemical Corporation, product name: Acryester ED)
[0064] <Method for measuring mass average molecular weight of prepolymer> 3.0993 g of the syrup (X) was dissolved in 50 ml of acetone, and this was dropped into 500 ml or more of n-hexane to obtain a precipitate. The precipitate was filtered and dried in vacuum to obtain a polymer, and the mass average molecular weight was measured using a high-performance liquid chromatograph (type: 8020 series, manufactured by Tosoh Corporation).
[0065] <Method of measuring high temperature tensile elongation (breaking elongation (%))> Test pieces were prepared in accordance with JIS K7161-2 using the obtained resin molded body, and the length of the test piece at break was measured at a tensile speed of 500 mm / min and a temperature of 160°C using a tensile testing machine (Instron Japan Co., Ltd., model name: 5567), a high and low temperature thermostatic chamber (Mita Sangyo Co., Ltd., model: G00061-2), and dedicated software (Instron Japan Co., Ltd., Bluehill2, version 2.12). The breaking elongation was calculated using the following formula (1). Breaking elongation (%) = 100 × (L-Lo) / Lo (1) Lo: Length of the test piece before testing L: Length of the test piece at break
[0066] <Webbing evaluation> The obtained cast plate was heated to substantially 220°C by the heater of a vacuum forming machine (manufactured by Fuse Vacuum Co., Ltd., model: CSVF1015), and then placed on a box-shaped mold (pedestal outer dimensions: diameter 190 mm, box mold outer dimensions: length 90 mm, width 90 mm, height 80 mm), and the entire circumference of the cast plate was gripped with a clamp. After pushing up the mold in this state, the air in the space between the mold and the cast plate was removed using a vacuum pump, so that the cast plate was made to conform to the inner shape of the square-shaped mold and was secondary molded into a box shape. This was cooled to substantially room temperature using a blower, and the cooled and solidified secondary molded product was removed from the mold. In this manner, a box-shaped secondary molded product with outer dimensions: length 90 mm, width 90 mm, height 80 mm was obtained. The appearance of the secondary molded product due to webbing that may occur at the corners of the product was visually evaluated based on the following criteria. ◎: No webbing was observed. ○: Webbing was visible, but was minimal. ×: Web-like protrusions (webbing) were observed, and the degree of webbing was large.
[0067] <How to evaluate heat resistance> As an index of the heat resistance of the resin molded article, the deflection temperature under load (hereinafter referred to as "HDT") (°C) was measured for the test pieces of the resin molded articles obtained in the examples and comparative examples. The method for measuring the deflection temperature under load is shown below. The resin molded body was cut into a size of 80 mm in length and 10 mm in width (4 mm in thickness), and then annealed at 80° C. for 16 hours. The molded body (B) after annealing was used as a test piece for evaluating heat resistance. The deflection temperature under load (HDT, unit: °C) of the test piece was measured using a deflection temperature under load tester (HDT / VICAT tester; model name: No. 148-HD-PC3 Heat Distortion Tester, manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with ISO75-1.2 under a load of 1.8 MPa.
[0068] Example 1 (Production of resin molded body) (1) Manufacture of syrup (X) A monomer composition (S1) containing 98 parts by mass of MMA and 2 parts by mass of BA in a total amount of 100 parts by mass was supplied to a reactor (polymerization kettle) equipped with a cooling tube, a thermometer, and a stirrer, and after bubbling with nitrogen gas while stirring, the temperature of the monomer composition (S1) in the reactor was raised to 80 ° C. When the temperature of the monomer composition (S1) reached 80 ° C., 0.1 parts by mass of 2,2'-azobis-(2,4-dimethylvaleronitrile) as a radical polymerization initiator and 0.07 parts by mass of 1-dodecanethiol as a chain transfer agent were added to 100 parts by mass of the monomer composition (S1), and the temperature of the monomer composition (S1) in the reactor was further raised to 100 ° C. and then maintained for 10 minutes. Next, the reactor was cooled to room temperature to obtain a syrup (X) containing 25% by mass of a prepolymer. The mass average molecular weight (Mw) of the obtained prepolymer was about 100,000 to 110,000.
[0069] (2) Casting polymerization Two SUS plates were placed opposite each other and the periphery was sealed with a gasket made of soft resin to prepare a mold for cast polymerization. The polymerizable composition (S2) prepared by mixing the above-mentioned syrup (X), MMA, BA, and EDMA as a crosslinking agent (A) in the ratios shown in Table 1 and further adding 0.3 parts by mass of t-hexyl peroxypivalate as a polymerization initiator was poured into the mold, and the mixture in the mold was polymerized by heating in a water bath at 80°C for 30 minutes and in an air oven at 130°C for 30 minutes to obtain a resin composition. The mold was then cooled and the SUS plates were removed to obtain a sheet-shaped resin molded body having a thickness of 2.5 mm and made of a resin composition containing a (meth)acrylic polymer.
[0070] Examples 2, 3 and 4, Comparative Examples 1 and 2 A sheet-shaped resin molding was obtained under the same production conditions as in Example 1, except that the amounts of syrup (X), methyl methacrylate, acrylic ester, and crosslinking agent (A) added to the polymerizable composition (S2) were changed as shown in Table 1. Table 1 shows the evaluation results of the high-temperature tensile elongation (breaking elongation (%)), webbing, and heat resistance for the resin molded articles in the examples and comparative examples.
[0071] [Table 1]
[0072] As shown in Table 1, in Examples 1 to 4, in which the high-temperature tensile elongation at 160°C of the resin molded body was 700% or less, the occurrence of webbing during molding was suppressed, whereas in Comparative Examples 1 and 2, in which the high-temperature tensile elongation at 160°C of the resin molded body exceeded 700%, webbing occurred during molding. Furthermore, in Examples 1 to 3, in which the resin moldings had high-temperature tensile elongation of 700% or less at 160°C, the deflection temperatures under load were equivalent to those of the resin moldings of Comparative Examples 1 and 2. Therefore, it can be evaluated that the heat resistance conventionally possessed by methacrylic polymers is maintained. [Industrial Applicability]
[0073] INDUSTRIAL APPLICABILITY The resin molded product provided by the present invention can suppress defects during molding of webbing and the like, and can maintain the heat resistance inherent to methacrylic polymers, and is therefore useful in the fields of sanitary products, kitchens, signs and building materials, small boat hulls, electrical appliance body parts, automobile body parts, and the like.
Claims
1. A resin molded product comprising a (meth)acrylic polymer obtained by polymerizing a polymerizable composition (S2), The polymerizable composition (S2) contains a monomer composition (S1) containing methyl methacrylate and a crosslinking agent (A), The resin molded article has a high-temperature tensile elongation at 160°C of 700% or less.
2. The resin molded article according to claim 1 , wherein the high-temperature tensile elongation is 450% or less.
3. The resin molded product according to claim 1, wherein the crosslinking agent (A) is contained in an amount of 0.2 to 6.0 parts by mass per 100 parts by mass of the total mass of the polymerizable composition (S2).
4. The resin molded article according to claim 1 , wherein the (meth)acrylic polymer contains structural units derived from methyl methacrylate in an amount of 80% by mass or more.
5. The resin molded article according to claim 1, wherein the crosslinking agent (A) contains at least one selected from the group consisting of ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polybutylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate.
6. The resin molded article according to claim 1, wherein the crosslinking agent (A) contains at least one selected from the group consisting of ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, and polybutylene glycol di(meth)acrylate.
7. The (meth)acrylic polymer according to any one of claims 1 to 6 comprises a non-crosslinked (meth)acrylic polymer, The resin molded article according to claim 1, wherein the non-crosslinked (meth)acrylic polymer has a mass average molecular weight of 10,000 or more and 700,000 or less.
8. The resin molded article according to claim 1 , which is a sanitary product or a kitchen utensil.
Citation Information
Patent Citations
Methacrylic resin and molded article
WO2015122174A1
Cast sheet, method for manufacturing same, and secondary molded article
WO2018168954A1