Electret fiber sheet, production method thereof, and air filter medium
The electret fiber sheet, made of non-conductive polyolefin fibers with hindered amine compounds and chlorine/sulfur atoms, addresses the challenge of high collection efficiency and low pressure loss in air filters, achieving excellent performance.
Patent Information
- Application Number
- JP2024045028
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-07
AI Technical Summary
Existing air filters using nonwoven fabrics face challenges in achieving high collection efficiency while maintaining low pressure loss, despite previous methods to enhance electret properties.
An electret fiber sheet composed of non-conductive fibers, primarily polyolefin resin, with 0.1 to 5.0% by mass of a hindered amine compound and surface presence of chlorine and/or sulfur atoms, achieved through electret treatment using specific aqueous solutions.
The solution results in an electret fiber sheet with high collection efficiency and low pressure loss, exemplified by a QF value of 0.20Pa-1 or higher, suitable for air filter media.
Smart Images

Figure 2024137876000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric, and more particularly to an electret fiber sheet having excellent collection performance, a method for producing the same, and an air filter medium. [Background technology]
[0002] 2. Description of the Related Art Air filters have been used to remove pollen, dust, droplets, and the like from gas, and nonwoven fabrics are often used as the filtering material for these air filters.
[0003] In general, it is difficult to achieve high collection efficiency and low pressure loss in air filters using nonwoven fabric, so attempts have been made to simultaneously achieve high collection efficiency and low pressure loss by subjecting the nonwoven fabric to electret processing, thereby utilizing electrostatic action in addition to physical action.
[0004] For example, a method for producing an electret fiber sheet has been proposed in which a nonwoven fabric is brought into contact with an earth electrode, and a high voltage is applied by a non-contact type electrode while moving both the earth electrode and the nonwoven fabric to continuously convert the fabric into an electret fiber (see, for example, Patent Document 1). Other methods for charging the fabric by contacting the fabric with water include a method in which a jet or a flow of water droplets is sprayed onto the fabric sheet at a pressure sufficient to cause the water to penetrate into the fabric, converting the fabric into an electret fiber and uniformly mixing positive and negative charges (see, for example, Patent Document 2), a method in which the fabric sheet is passed over a slit-shaped nozzle, and the nozzle sucks the water to cause the water to penetrate the fabric sheet and mix positive and negative charges (see, for example, Patent Document 3), and a method in which an aqueous solution containing an organic or inorganic compound is sprayed at a pressure sufficient to pass through the fabric sheet to convert the fabric into an electret fiber (see, for example, Patent Document 4), which are so-called hydrocharging methods, have been proposed. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 61-289177 [Patent Document 2] U.S. Patent No. 6,119,691 [Patent Document 3] JP 2003-3367 A [Patent Document 4] JP 2004-66026 A Summary of the Invention [Problem to be solved by the invention]
[0006] As proposed in the above Patent Documents 1 to 4, the collection performance can be improved to some extent by converting the melt-blown nonwoven fabric into an electret. However, when used as an air filter, for example, a filter with a lower pressure loss without impairing the collection efficiency is required.
[0007] Therefore, an object of the present invention is to provide an electret fiber sheet having higher collection performance by focusing on the above-mentioned problems and achieving high collection efficiency while maintaining low pressure loss. [Means for solving the problem]
[0008] The electret fiber sheet and its manufacturing method, as well as the air filter medium, of the present invention, which solve the above problems, have the following configurations. [1] An electret fiber sheet mainly comprising non-conductive fibers, characterized in that the electret fiber sheet contains 0.1 to 5.0 mass% of a hindered amine compound, and at least one of chlorine atoms and sulfur atoms is present in an amount of 1 to 500 ppm on the fiber surface of the electret fiber sheet.
[0009] [2] The electret fiber sheet according to [1], wherein at least one of sodium atoms and potassium atoms is further present in an amount of 1 to 500 ppm on the surface of the electret fiber sheet. [3] The electret fiber sheet according to [1] or [2], wherein the non-conductive fibers are made of a polyolefin resin. [4] The QF value of the electret fiber sheet is 0.20 Pa -1 The electret fiber sheet according to any one of [1] to [3] above.
[0010] [5] An air filter medium comprising the electret fiber sheet according to any one of [1] to [4]. [5] A method for producing an electret fiber sheet according to any one of [1] to [4], comprising the steps of: preparing a polyolefin resin composition comprising a polyolefin resin and 0.1 to 5.0 mass% of a hindered amine compound; forming a fiber sheet from the polyolefin resin composition; and contacting the fiber sheet with an aqueous solution containing chlorine atoms and / or sulfur atoms. Effect of the Invention
[0011] According to the present invention, by introducing chlorine atoms and / or sulfur atoms into the fiber surface of a fiber sheet containing an electret hindered amine compound, it is possible to obtain an electret fiber sheet having both low pressure loss and high collection efficiency and excellent collection performance. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic side view showing a measuring device for collection efficiency and pressure loss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The electret fiber sheet of the present invention is an electret fiber sheet mainly comprising non-conductive fibers, characterized in that the electret fiber sheet contains 0.1 to 5.0 mass% of a hindered amine compound, and at least one of chlorine atoms and sulfur atoms is present in an amount of 1 to 500 ppm on the fiber surface of the electret fiber sheet. The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the present invention.
[0014] In the present invention, non-conductive means a material having a volume resistivity of 10 12 Ω cm or more, and 14 It is preferable that the resistivity is 1.5 Ω·cm or more. In the present invention, "mainly comprising non-conductive fibers" means that the electret fiber sheet contains 90% by mass or more of non-conductive fibers. The non-conductive fibers are preferably contained in an amount of 95% by mass or more, more preferably 97% by mass or more. If the non-conductive fibers are contained in the electret fiber sheet in an amount of less than 90% by mass, sufficient electret performance cannot be obtained, which is not preferable.
[0015] Examples of the resin raw material for the non-conductive fiber used in the present invention include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, and polylactic acid, polycarbonate resins, polystyrene resins, polyphenylene sulfide resins, fluorine resins, elastomers such as polystyrene elastomers, polyolefin elastomers, polyester elastomers, polyamide elastomers, and polyurethane elastomers, and copolymers or mixtures of these.
[0016] Among these, fibers made of polyolefin resin are preferably used as the non-conductive fibers. Since polyolefin resin has high volume resistivity and low water absorption, it is possible to enhance the chargeability and charge retention when a fiber sheet (nonwoven fabric) of polyolefin resin is subjected to electret processing, and these effects can achieve high collection efficiency.
[0017] In the present invention, examples of polyolefin resins include homopolymers such as polyethylene, polypropylene, polybutene, and polymethylpentene. In addition, resins such as copolymers in which a different olefin component is copolymerized with the olefin component of these homopolymers, and blends of two or more different polymers can also be used. Among these, polypropylene resins and polymethylpentene resins are preferably used from the viewpoint of charge retention. In particular, polypropylene resins are preferably used from the viewpoints of low cost use and easy reduction of fiber diameter. The polypropylene resins include resins such as polypropylene homopolymers, copolymers with other olefin components, and polymer blends with different resins. Among these, polypropylene homopolymers and polypropylene copolymers containing 90% or more by mass of propylene units are preferred. In addition, the fibers made of polyolefin resins may be composite fibers, and may take the form of composite fibers such as core-sheath type, eccentric core-sheath type, side-by-side type, split type, sea-island type, and alloy type.
[0018] The electret fiber sheet of the present invention contains 0.1% by mass or more and 5.0% by mass or less of a hindered amine compound in the fibers constituting the electret fiber sheet. By containing 0.1% by mass or more, preferably 0.7% by mass or more of a hindered amine compound, an electret fiber sheet having excellent chargeability and charge retention properties when subjected to electret processing can be obtained. On the other hand, by containing 5.0% by mass or less, preferably 3.0% by mass or less of a hindered amine compound, it is possible to develop the chargeability and charge retention properties at a lower cost.
[0019] The content of the hindered amine compound in the fibers constituting the electret fiber sheet can be determined, for example, as follows. That is, the electret fiber sheet is subjected to Soxhlet extraction with a methanol / chloroform mixed solution, and the extract is repeatedly fractionated by HPLC. Each fraction is subjected to IR measurement, GC measurement, GC / MS measurement, MALDI-MS measurement, 1 H-NMR measurement, and 13 The structure is confirmed by C-NMR measurement. The masses of the fractions containing the hindered amine compound are added up, and the ratio to the entire electret fiber sheet is calculated, and this is taken as the content of the hindered amine compound.
[0020] Examples of the hindered amine compound used in the present invention include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (manufactured by BASF Japan Ltd., "Chimassorb" (registered trademark) 944LD), dimethyl succinate-1-(2-hydroxyethyl)-4- Examples of such polycondensates include hydroxy-2,2,6,6-tetramethylpiperidine (manufactured by BASF Japan Ltd., "Tinuvin" (registered trademark) 622LD), 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonate bis(1,2,2,6,6-pentamethyl-4-piperidyl) (manufactured by BASF Japan Ltd., "Tinuvin" (registered trademark) 144), and "Chimasorb" (registered trademark) 2020FDL, manufactured by BASF Japan Ltd.
[0021] In addition, in addition to the above-mentioned hindered amine compound, additives such as a heat stabilizer, a crystal nucleating agent, a weathering agent, and a polymerization inhibitor can be added to the polyolefin resin composition used for the non-conductive fiber of the electret fiber sheet, as long as the effects of the present invention are not impaired.
[0022] The electret fiber sheet of the present invention contains at least one of chlorine atoms and sulfur atoms in an amount of 1 to 500 ppm on the fiber surface. When both chlorine atoms and sulfur atoms are contained, the total amount is 1 to 500 ppm. By containing 1 ppm or more, preferably 5 ppm or more, of chlorine atoms and / or sulfur atoms, an electret fiber sheet having excellent charging properties can be obtained. On the other hand, by containing 500 ppm or less, preferably 300 ppm or less, of chlorine atoms and / or sulfur atoms, it becomes possible to develop charging properties at a lower cost. The concentration of chlorine atoms and sulfur atoms present on the fiber surface of the electret fiber sheet can be adjusted by the concentration of chlorine atoms and sulfur atoms in the aqueous solution used in the electret treatment (charging treatment) described later, the type of compound containing chlorine atoms or sulfur atoms, the type of water, the fiber diameter of the fiber sheet, and the like.
[0023] The content of chlorine atoms and sulfur atoms can be obtained, for example, as follows. That is, the electret fiber sheet is burned in a combustion tube, the generated gas is absorbed in an absorption liquid, and then the chlorine atoms and sulfur atoms are measured and quantified by ion chromatography. Alternatively, the electret fiber sheet is immersed in pure water and thoroughly washed, and then the washed fiber sheet is burned in a combustion tube, the generated gas is absorbed in an absorption liquid, and then the chlorine atoms and sulfur atoms are measured and quantified by ion chromatography. The difference between the concentration of chlorine and sulfur atoms per mass of the electret fiber sheet in the fiber sheet before washing and the concentration of chlorine and sulfur atoms per mass of the electret fiber sheet in the fiber sheet after washing can be taken as the concentration of chlorine atoms and sulfur atoms on the surface of the electret fiber sheet.
[0024] Examples of the compound containing a chlorine atom or a sulfur atom for use in the present invention include lithium chloride, sodium chloride, potassium chloride, magnesium chloride, calcium chloride, sodium sulfate, potassium sulfate, magnesium sulfate, sodium thiosulfate, potassium thiosulfate, magnesium thiosulfate, calcium thiosulfate, sodium sulfite, potassium sulfite, magnesium sulfite, and calcium sulfite.
[0025] The electret fiber sheet of the present invention is a fiber sheet (nonwoven fabric) that has been subjected to an electret treatment (charging treatment). For example, the method of making the fiber sheet of the present invention into an electret can be a method of spraying a jet or a flow of water droplets onto the fiber sheet at a pressure sufficient to cause the water to penetrate into the fiber sheet, thereby making the fiber sheet into an electret, and making the positive and negative charges uniformly mixed, or a method (hydrocharge method) can be used in which the fiber sheet is passed over a slit-shaped nozzle, and the nozzle sucks the water to cause the water to penetrate into the fiber sheet, thereby making the positive and negative charges uniformly mixed.
[0026] In the present invention, by using an aqueous solution containing chlorine atoms and / or sulfur atoms as the aqueous solution used for electretization, chlorine atoms and / or sulfur atoms can be present on the fiber surface of the electret fiber sheet. For example, an aqueous solution in which the above-mentioned inorganic salt containing chlorine atoms and / or sulfur atoms is dissolved in water from which dirt has been removed using a liquid filter or the like can be used, or alkaline electrolytic water can be used. In particular, pure water such as ion-exchanged water, distilled water, and filtered water permeated through a reverse osmosis membrane is preferably used as the water solvent. In addition, the level of pure water is 10 in terms of conductivity. 2 It is pure water with a purity of less than μS / m.
[0027] In addition, the electret fiber sheet of the present invention preferably has at least one of sodium and potassium atoms present in an amount of 1 to 500 ppm on the fiber surface together with chlorine atoms and / or sulfur atoms. When both sodium and potassium atoms are present, the total amount is 1 to 500 ppm. By containing 1 ppm or more, preferably 5 ppm or more, of sodium and / or potassium atoms, an electret fiber sheet with excellent electrostatic chargeability can be obtained. On the other hand, by containing 500 ppm or less, preferably 300 ppm or less, of sodium and / or potassium atoms, it becomes possible to develop electrostatic chargeability at a lower cost.
[0028] The content of sodium and potassium atoms can be determined, for example, as follows. That is, sulfuric acid is added to an electret fiber sheet, which is heated and carbonized, and then heated and incinerated. The ash is thermally decomposed with sulfuric acid and hydrofluoric acid, and dissolved in dilute nitric acid to a constant volume. Sodium and potassium are measured using this solution by atomic absorption spectrometry. The electret fiber sheet is immersed in pure water, and the content of sodium and potassium atoms is quantified before and after thorough washing. The difference between the concentration of sodium and potassium atoms per mass of the electret fiber sheet in the fiber sheet before washing and the concentration of sodium and potassium atoms per mass of the electret fiber sheet in the fiber sheet after washing can be regarded as the concentration of sodium and potassium atoms on the surface of the electret fiber sheet.
[0029] Examples of compounds containing sodium or potassium atoms used in the present invention include sodium chloride, potassium chloride, sodium sulfate, potassium sulfate, sodium thiosulfate, potassium thiosulfate, sodium sulfite, and potassium sulfite. By using an aqueous solution containing these compounds in the electret treatment (charging treatment), sodium atoms and / or potassium atoms can be present on the fiber surface of the electret fiber sheet. In addition, the concentration of sodium atoms and potassium atoms present on the fiber surface of the electret fiber sheet can be adjusted by the concentration of sodium atoms and potassium atoms in the aqueous solution used in the electret treatment, the type of compound containing sodium atoms or potassium atoms, the type of water, the fiber diameter of the fiber sheet, and the like.
[0030] The electret fiber sheet of the present invention is preferably made of a melt-blown nonwoven fabric. By using the melt-blown nonwoven fabric, fine fibers of several μm can be easily obtained without requiring complicated processes, and high dust collection properties can be easily achieved.
[0031] The average single fiber diameter of the fibers constituting the electret fiber sheet of the present invention is preferably in the range of 0.1 μm to 8.0 μm. By setting the average single fiber diameter to preferably 0.1 μm to 8.0 μm, more preferably 0.3 μm to 7.0 μm, and even more preferably 0.5 μm to 5.0 μm, an electret fiber sheet having excellent breathability and dust collection properties can be easily obtained.
[0032] The average single fiber diameter of the fibers used in the electret fiber sheet of the present invention refers to a value obtained by taking 15 measurement samples of 3 mm × 3 mm from three points in the width direction of the fiber sheet (two points on the side ends and one point in the center) and five points every 5 cm in the longitudinal direction, for a total of 15 points, adjusting the magnification to 2000 times with a scanning electron microscope (for example, "VE-9800" manufactured by Keyence Corporation), taking one fiber surface photograph from each of the taken measurement samples, for a total of 15 photographs, measuring the single fiber diameter (unit: μm) of the fibers in which the fiber diameter (single fiber diameter) can be clearly confirmed in each photograph, and rounding off the average value to one decimal place.
[0033] The electret fiber sheet of the present invention has a basis weight of 5 g / m 2 More than 100g / m 2 The weight is preferably 5 g / m or less. 2 More preferably, 7 g / m 2 More preferably, 10 g / m 2 By setting the value at 100 g / m or more, the collection efficiency of the electret melt-blown nonwoven fabric can be improved. 2 Less than 80 g / m 2 Less than 60 g / m, more preferably 2 By setting the above as follows, the pressure loss of the electret fiber sheet can be reduced.
[0034] The basis weight of the electret fiber sheet in the present invention is determined by taking a sample of 15 cm x 15 cm length x width from the fiber sheet, measuring the mass of the sample, and calculating the mass per unit area per m 2Convert the value per unit area and round off to the nearest tenth to obtain the weight per unit area of the fiber sheet (g / m 2 ) will be calculated.
[0035] The electret fiber sheet of the present invention has the above-mentioned configuration, and thus achieves both high collection efficiency and low pressure loss. The QF value (Pa -1 The QF value indicates the relationship between collection efficiency and pressure loss, as expressed by the following formula: the higher the QF value, the higher the collection efficiency and the lower the pressure loss. QF value (Pa -1 ) = -[ln(1-collection efficiency (%) / 100)] / pressure loss (Pa) In the above formula, the collection efficiency (%) of the electret fiber sheet is the collection rate of 0.3 to 0.5 μm particles based on JIS K0901, and the pressure loss (Pa) of the electret fiber sheet is the static pressure difference between the upstream and downstream of the electret fiber sheet.
[0036] The QF value of the electret fiber sheet is preferably 0.20 Pa -1 More preferably, 0.22 Pa -1 The QF value is 0.20 Pa or more. -1 The above means that the electret fiber sheet achieves both high collection efficiency and low pressure loss.
[0037] Here, the collection efficiency and pressure loss of the electret fiber sheet in the present invention are measured and calculated according to the following procedure. (1) Take measurement samples M (total of five samples) measuring 15 cm x 15 cm (length x width) at five locations across the width of the electret fiber sheet. (2) Prepare a collection efficiency measuring device as shown in the schematic side view of Figure 1. In this collection efficiency measuring device, a dust inlet 2 is connected to the upstream side of a sample holder 1 in which a measurement sample M is set, and a flow meter 3, a flow control valve 4, and a blower 5 are connected to the downstream side. In addition, a particle counter 6 is used on the upstream side of sample M of the sample holder 1, and a particle counter 7 is used on the downstream side of sample M, so that the number of dust particles on the upstream side and the downstream side of the measurement sample M can be measured. (3) The dust inlet 2 is opened to introduce air. (4) The measurement sample M is set in the sample holder 1, and the airflow rate is adjusted with the flow control valve 4 so that the filter passing speed is 3.0 m / min. The atmospheric dust concentration is adjusted to 10,000 to 40,000 particles / 2.83×10 -4 m 3 Check that the above is stable. (5) The number of dust particles D upstream of the measurement sample M is measured with a particle counter 6 (for example, "KC-01E" manufactured by Rion Co., Ltd.) and the number of dust particles d downstream is measured with a particle counter 7 three times per measurement sample M, and the collection efficiency (%) of 0.3 to 0.5 μm particles is calculated using the following formula based on JIS K0901:1991 "Test method for shape, dimensions and performance of filter media for collecting dust samples in gas". Collection efficiency (%) = [1-(d / D)] x 100 (where d represents the total number of downstream dust particles measured three times, and D represents the total number of upstream dust particles measured three times.) (6) In addition, the static pressure difference between the upstream and downstream of the measurement sample M is read by the pressure gauge 8, and the pressure loss (Pa) of the measurement sample M is calculated. (7) The average collection efficiency (%) for the five measurement samples M is calculated, and the value obtained by rounding off to two decimal places is regarded as the collection efficiency (%) of the electret fiber sheet. (8) The average value of the pressure loss (Pa) for the five measurement samples M is calculated, and the value obtained by rounding off to one decimal place is regarded as the pressure loss (Pa) of the electret fiber sheet.
[0038] Next, a method for producing the electret fiber sheet of the present invention will be described. The method for producing an electret fiber sheet of the present invention is characterized in that a polyolefin resin composition containing a polyolefin resin and 0.1 to 5.0 mass % of a hindered amine compound is prepared, a fiber sheet (nonwoven fabric) is formed from the polyolefin resin composition, and the fiber sheet is brought into contact with an aqueous solution containing chlorine atoms and / or sulfur atoms.
[0039] <Resin composition> The polyolefin resin composition constituting the non-conductive fibers of the electret fiber sheet of the present invention can be prepared by mixing the polyolefin resin and the hindered amine compound at once, or by chip blending using a master batch of the polyolefin resin and the hindered amine described below.
[0040] A method for preparing a polyolefin resin composition by mixing at once includes a method in which the hindered amine compound is added to the polyolefin resin in an amount of 0.1% by mass or more and 5.0% by mass or less, and the mixture is extruded using a twin-screw extruder or the like.
[0041] In addition, as a method of preparing a chip blend using a master batch of a polyolefin resin and a hindered amine and then extruding, for example, there is a method of preparing a master batch in which a hindered amine compound is kneaded into a polyolefin resin, chip-blending the polyolefin resin with this, and kneading the mixture in an extruder to prepare a polyolefin resin composition.
[0042] <Fiber sheet> Next, a fiber sheet (nonwoven fabric) is formed from the obtained polyolefin resin composition. In the melt-blowing method, a molten polyolefin resin composition is discharged from a nozzle having a predetermined hole diameter to form threads. Hot air is sprayed from a certain angle onto the discharge section to reduce the diameter of the threads, and the threads are accumulated in a collection section to form a fiber sheet.
[0043] <Electret treatment> The fiber sheet thus obtained is then subjected to electret processing. 2 The method uses an aqueous solution of inorganic salts containing chlorine atoms and / or sulfur atoms dissolved in pure water of μS / m or less, or alkaline electrolyzed water, and sprays a jet or a stream of droplets of the aqueous solution onto a fiber sheet at a pressure sufficient to allow the aqueous solution to penetrate into the fiber sheet, thereby forming an electret and uniformly mixing positive and negative charges. Alternatively, the fiber sheet is passed over a slit-shaped nozzle, and the aqueous solution is sucked into the nozzle, thereby allowing the aqueous solution to penetrate into the nonwoven fabric, thereby uniformly mixing positive and negative charges (hydrocharging method).
[0044] <Air filter media> The electret fiber sheet of the present invention can be suitably used as an air filter medium. This air filter medium has high collection efficiency, low pressure loss, and excellent collection performance. EXAMPLES
[0045] Next, the present invention will be specifically described based on examples. However, the present invention is not limited to these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method. [Measurement method] (1) Average single fiber diameter of electret fiber sheet: The scanning electron microscope used was a "VE-9800" manufactured by Keyence Corporation, and the measurements were carried out according to the above method. (2) Electret fiber sheet basis weight: The measurements were carried out according to the method described above. (3) Collection efficiency, pressure loss, and QF value of electret fiber sheet: The measurements were carried out according to the above method. The particle counter used for the collection efficiency measurement device was the "KC-01E" manufactured by Rion Co., Ltd. (4) The amount of chlorine atoms and sulfur atoms present on the fiber surface of the electret fiber sheet The measurements were carried out according to the method described above. (5) The amount of sodium and potassium atoms on the fiber surface of the electret fiber sheet The measurements were carried out according to the method described above. (6) Electrical conductivity of water and treated aqueous solutions The electrical conductivity was measured using a CM-31P manufactured by DKK-TOA Corporation.
[0046] [Resin composition for producing electret fiber sheet] In the comparative examples below, the resins and compounds used as raw materials for the electret fiber sheets are as follows. Melt-blown nonwoven resin (PP): Polypropylene (MFR: 850g / 10min) Hindered amine compounds (HA1): Chimassorb 944 Hindered amine compounds (HA2): Chimassorb 2020
[0047] [Example 1] Using a melt-blown nonwoven fabric manufacturing device, a polyolefin resin composition containing 1.0 mass% of a hindered amine compound (HA1: Chimassorb 944) added to a homopolymer polypropylene resin (PP) having an MFR of 850 g / 10 min was melted in an extruder and extruded from a spinning nozzle with a die set temperature of 260°C and a hole diameter of 0.3 mm at a single hole discharge rate of 0.36 g / min. Air heated and compressed at a set temperature of 290°C was blown from both sides of the spinning nozzle at a pressure of 1200 Nm 3 / hr and collected in a collection drum, resulting in a basis weight of 40g / m 2A melt-blown nonwoven fabric was obtained. Next, NaCl was dissolved in pure water (electrical conductivity: 2 μS / m, pH 7.1), and the resulting melt-blown nonwoven fabric was run along the surface of a water tank supplied with an aqueous NaCl solution adjusted to 10 ppm. A slit-shaped suction nozzle was brought into contact with the surface of the fabric to suck in the aqueous NaCl solution for permeation treatment. After draining, the fabric was dried with hot air at 80° C. for 20 minutes to obtain an electret fiber sheet. The properties of the aqueous solution used in the electret treatment and the characteristic values of the resulting electret fiber sheet are shown in Table 1.
[0048] [Example 2] Except for changing the concentration of the NaCl aqueous solution during the electret treatment to 28 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 1.
[0049] [Example 3] An electret fiber sheet was obtained in the same manner as in Example 2, except that the hindered amine compound in the raw polypropylene resin was changed to a hindered amine compound (HA2: Chimassorb 2020). The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 1.
[0050] [Example 4] Except for changing the concentration of the NaCl aqueous solution during the electret treatment to 58 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 1.
[0051] [Example 5] Except for changing the concentration of the NaCl aqueous solution during the electret treatment to 80 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 1.
[0052] [Example 6] Except for changing the NaCl aqueous solution during the electret treatment to a KCl aqueous solution with a concentration of 4 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 1.
[0053] [Example 7] Except for changing the concentration of the KCl aqueous solution during the electret treatment to 13 ppm, an electret fiber sheet was obtained in the same manner as in Example 6. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 1.
[0054] [Example 8] Except for changing the concentration of the KCl aqueous solution during the electret treatment to 36 ppm, an electret fiber sheet was obtained in the same manner as in Example 6. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 1.
[0055] [Example 9] Except for changing the NaCl aqueous solution during the electret treatment to a Na2SO4 aqueous solution with a concentration of 10 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 2.
[0056] [Example 10] Except for changing the concentration of the Na2SO4 aqueous solution during the electret treatment to 26 ppm, an electret fiber sheet was obtained in the same manner as in Example 9. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 2.
[0057] [Example 11] Except for changing the concentration of the Na2SO4 aqueous solution during the electret treatment to 68 ppm, an electret fiber sheet was obtained in the same manner as in Example 9. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 2.
[0058] [Example 12] Except for using alkaline electrolyzed water (produced using Panasonic's alkaline ionized water purifier TK-AS47-H) instead of the NaCl aqueous solution during the electret treatment, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the alkaline electrolyzed water used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 2.
[0059] [Example 13] Except for changing the NaCl aqueous solution during the electret treatment to a K2SO4 aqueous solution with a concentration of 16 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 2.
[0060] [Example 14] An electret fiber sheet was obtained in the same manner as in Example 13, except that the concentration of the K2SO4 aqueous solution during the electret treatment was 31 ppm. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 2.
[0061] [Example 15] An electret fiber sheet was obtained in the same manner as in Example 13, except that the concentration of the K2SO4 aqueous solution during the electret treatment was 94 ppm. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 2.
[0062] [Comparative Example 1] Except for using pure water (electrical conductivity: 2 μS / m, pH 7.1) instead of the NaCl aqueous solution during the electret treatment, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 3.
[0063] [Comparative Example 2] Except for not containing a hindered amine compound in the raw polypropylene resin, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the property values of the obtained electret fiber sheet are shown in Table 3.
[0064] [Comparative Example 3] Except for changing the NaCl aqueous solution during the electret treatment to a Na2CO3 aqueous solution with a concentration of 40 ppm, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the aqueous solution used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 3.
[0065] [Comparative Example 4] Except for using acidic electrolyzed water (produced using Panasonic's alkaline ionized water purifier TK-AS47-H) instead of the NaCl aqueous solution during the electret treatment, an electret fiber sheet was obtained in the same manner as in Example 1. The properties of the acidic electrolyzed water used in the electret treatment and the characteristic values of the obtained electret fiber sheet are shown in Table 3.
[0066] [Table 1]
[0067] [Table 2]
[0068] [Table 3]
[0069] As is clear from Tables 1 and 2, the electret fiber sheets according to Examples 1 to 15 of the present invention achieve high collection efficiency while exhibiting low pressure loss, and are therefore excellent in collection performance.
[0070] In contrast, as is clear from Table 3, in Comparative Example 1 and Comparative Example 3, which do not contain either chlorine atoms or sulfur atoms on the electret fiber surface, the collection efficiency was lower than that of the electret fiber sheet described in Example 1.
[0071] Moreover, in Comparative Example 2 in which the fiber sheet did not contain a hindered amine compound, the result showed that the collection efficiency was lower than that of the electret fiber sheet described in Example 1.
[0072] In Comparative Example 4, in which acidic electrolyzed water was used during the electret treatment, the fiber surface did not contain chlorine atoms or sulfur atoms, and the result showed a lower collection efficiency than the laminated electret nonwoven fabric described in Example 1.
[0073] As described above, according to the present invention, by making chlorine atoms and / or sulfur atoms exist on the surface of a fiber sheet containing an electretized hindered amine compound, an electret fiber sheet having unprecedentedly high collection performance can be obtained. This electret fiber sheet can be suitably used for air filter media and air filters in general. [Explanation of symbols]
[0074] 1: Sample holder 2: Dust inlet 3:Flow meter 4: Flow control valve 5: Blower 6: Upstream particle counter 7: Downstream particle counter 8: Pressure gauge M: Measurement sample
Claims
1. An electret fiber sheet mainly comprising non-conductive fibers, the electret fiber sheet containing 0.1 to 5.0 mass % of a hindered amine compound, and at least one of chlorine atoms and sulfur atoms being present in an amount of 1 to 500 ppm on the fiber surface of the electret fiber sheet.
2. The electret fiber sheet according to claim 1, characterized in that at least one of sodium atoms and potassium atoms is further present in an amount of 1 to 500 ppm on the fiber surface of the electret fiber sheet.
3. 3. The electret fiber sheet according to claim 1, wherein the non-conductive fibers are made of a polyolefin resin.
4. The QF value of the electret fiber sheet is 0.20 Pa. -1 The electret fiber sheet according to claim 1 or 2.
5. 3. An air filter medium comprising the electret fiber sheet according to claim 1 or 2.
6. The method for producing the electret fiber sheet according to claim 1 or 2, comprising: preparing a polyolefin resin composition comprising a polyolefin resin and 0.1 to 5.0 mass% of a hindered amine compound; forming a fiber sheet from the polyolefin resin composition; and contacting the fiber sheet with an aqueous solution containing chlorine atoms and / or sulfur atoms.
Citation Information
Patent Citations
Production of electret fibrous sheet
JP1986289177A
Electret fiber sheet
JP2003003367A
Production method of electret filter medium
JP2004066026A
Electret filter media
US6119691A