Silicone rubber-based curable composition, blade member, and wiper blade

By integrating silica particles treated with a silane coupling agent into a silicone rubber-based curable composition, the wear resistance of wiper blades is significantly improved, addressing the wear resistance issues of existing wiper blades.

JP2024138330APending Publication Date: 2024-10-08SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024106744
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The wiper blades described in Patent Document 1 lack sufficient wear resistance.

Method used

Incorporating silica particles surface-treated with a silane coupling agent into a silicone rubber-based curable composition for blade members, which improves the abrasion resistance of the cured product.

Benefits of technology

The composition enhances the wear resistance of the wiper blades, reducing wear loss and improving tear strength and elongation at break, making it suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138330000001
    Figure 2024138330000001
  • Figure 2024138330000002
    Figure 2024138330000002
  • Figure 2024138330000003
    Figure 2024138330000003
Patent Text Reader

Abstract

To provide a silicone rubber-based curable composition excellent in abrasion resistance.SOLUTION: The silicone rubber-based curable composition of the present invention is used for forming a blade member and contains a vinyl group-containing polyorganosiloxane (A) and silica particles (C) surface-treated with a silane coupling agent (D).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicone rubber-based curable composition, a blade member, and a wiper blade. [Background technology]

[0002] Various developments have been made so far regarding sliding members such as wiper blades. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a wiper blade made of silicone rubber (claim 1 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-046734 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of studies by the present inventors, it has become clear that the wiper blade described in Patent Document 1 above has room for improvement in terms of wear resistance. [Means for solving the problem]

[0005] After further investigation, the inventors discovered that for silicone rubber used in blade members such as wiper blades, the abrasion resistance of the cured product (silicone rubber) of the silicone rubber-based curable composition can be improved by adding silica particles surface-treated with a silane coupling agent, and thus completed the present invention.

[0006] According to the present invention, A silicone rubber-based hardening composition used to form a blade member, comprising: A vinyl group-containing polyorganosiloxane (A), Silica particles (C) surface-treated with a silane coupling agent (D); A silicone rubber-based curable composition is provided, comprising:

[0007] Further, according to the present invention, There is provided a blade member comprising a cured product of the above silicone rubber-based curable composition.

[0008] Further, according to the present invention, There is provided a wiper blade comprising a cured product of the above silicone rubber-based curable composition. Effect of the Invention

[0009] According to the present invention, there are provided a silicone rubber-based curable composition having excellent abrasion resistance, and a blade member and a wiper blade each using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The silicone rubber-based hardening composition of this embodiment will now be described.

[0011] The silicone rubber-based hardenable composition of the present embodiment is used to form a part of the blade member. This silicone rubber-based hardenable composition contains a vinyl group-containing polyorganosiloxane (A) and silica particles (C) that have been surface-treated with a silane coupling agent (D).

[0012] According to the findings of the present inventors, it has been found that by using a vinyl group-containing polyorganosiloxane (A) and silica particles (C) surface-treated with a silane coupling agent (D), the abrasion loss in a Taber abrasion test can be reduced, thereby improving abrasion resistance.

[0013] Although the detailed mechanism is unclear, it is believed that by appropriately selecting the compositional components of a silicone rubber-based curable composition, it is possible to appropriately control the rubber properties of silicone rubber, such as tear strength and breaking elongation, and therefore reduce abrasion loss in the Taber abrasion test.

[0014] The silicone rubber-based hardening composition of the present embodiment has excellent abrasion resistance, and can realize a silicone rubber suitable for blade members such as wiper blades and general sliding members.

[0015] The blade member and wiper blade of the present embodiment are provided with a cured product of a silicone rubber-based curable composition.

[0016] In this embodiment, the blade member can be used, for example, as a component part of a vehicle, electronic device, machine tool, building, etc., and examples thereof include wiper blades used in vehicles such as automobiles and trains, ships, and aircraft.

[0017] The silicone rubber-based hardenable composition will now be described in detail.

[0018] The tear strength of the cured product of the silicone rubber-based curable composition, measured by the following procedure, is designated as TS (N / mm) and the breaking elongation is designated as BE (%).

[0019] (Measuring procedure for tear strength) A crescent-shaped test piece is prepared from the cured product of the silicone rubber-based curable composition in accordance with JIS K6252 (2001), and the tear strength of the obtained crescent-shaped test piece at 25° C. is measured (unit: N / mm).

[0020] (Procedure for measuring breaking elongation) Using the cured product of the silicone rubber-based curable composition, a dumbbell-shaped No. 3 test piece is prepared in accordance with JIS K6251 (2004), and the breaking elongation of the obtained dumbbell-shaped No. 3 test piece is measured at 25°C. The breaking elongation is calculated by [gage line movement distance (mm)] ÷ [initial gage line distance (20 mm)] × 100. The unit is %.

[0021] The silicone rubber-based hardening composition of the present embodiment has a TS and BE of 2.3×10 4 It may be configured to satisfy ≦TS×BE.

[0022] The lower limit of TS×BE is 2.3×10 4 More than 2.4×10 4 More preferably, 2.8×10 4 This makes it possible to realize a silicone rubber with excellent abrasion resistance. On the other hand, the upper limit of TS×BE is not particularly limited, but is, for example, 5.0×10 5 Less than 1.0×10 is acceptable. 5 Less than 9.0×10 is also acceptable. 4 This makes it possible to obtain a silicone rubber with an excellent balance of properties.

[0023] According to the findings of the present inventors, it has been discovered that the abrasion resistance of silicone rubber can be stably evaluated by using the integrated value of tear strength and breaking elongation as an index, and that by setting this integrated value to be equal to or above the above-mentioned lower limit value, it is possible to reduce the abrasion loss in the Taber abrasion test.

[0024] Although the detailed mechanism is unclear, it is believed that by increasing the product of tear strength and breaking elongation, resistance to friction with other materials is improved, making the material less susceptible to destruction, and thus improving abrasion resistance.

[0025] The lower limit of the tear strength is, for example, 25 N / mm or more, preferably 28 N / mm or more, more preferably 30 N / mm or more, even more preferably 33 N / mm or more, and even more preferably 35 N / mm or more. This can improve the durability of the silicone rubber during repeated use. Also, the scratch resistance and mechanical strength of the silicone rubber can be improved. On the other hand, the upper limit of the tear strength is not particularly limited, but may be, for example, 80 N / mm or less, or 70 N / mm or less. This can balance the various properties of the silicone rubber.

[0026] The durometer hardness A of the cured product of the silicone rubber-based curable composition is measured by the following procedure. The upper limit of the durometer hardness A is not particularly limited, but may be, for example, 90 or less, preferably 85 or less, and more preferably 80 or less. This allows the cured physical properties of the silicone rubber to be well balanced. This allows the silicone rubber to be adjusted in terms of its deformability, which allows it to be easily deformed, such as by bending or stretching. On the other hand, the lower limit of the durometer hardness A is not particularly limited, but is, for example, not less than 30, preferably not less than 33, and more preferably not less than 35. This can increase the mechanical strength of the silicone rubber.

[0027] (Durometer hardness A measurement procedure) A sheet-like test piece is prepared using the cured product of the silicone rubber-based curable composition, and the durometer hardness A of the obtained sheet-like test piece at 25° C. is measured in accordance with JIS K6253 (1997).

[0028] In this embodiment, it is possible to control the hardness, breaking elongation, and tear strength by appropriately selecting, for example, the type and blending amount of each component contained in the silicone rubber-based hardening composition, the preparation method of the silicone rubber-based hardening composition, etc. Among these, for example, appropriately controlling the type and blending ratio of the resin constituting the silicone rubber, the crosslinking density and crosslinking structure of the resin, the blending ratio of the inorganic filler, and improving the dispersibility of the inorganic filler by a silane coupling agent are listed as elements for setting the hardness, breaking elongation, and tear strength in the desired numerical range.

[0029] Next, the components of the silicone rubber-based hardening composition will be described.

[0030] The silicone rubber-based hardening composition of the present embodiment may contain a vinyl group-containing organopolysiloxane (A). The vinyl group-containing organopolysiloxane (A) is a polymer that is the main component of the silicone rubber-based hardening composition.

[0031] The vinyl group-containing organopolysiloxane (A) can contain a vinyl group-containing linear organopolysiloxane (A1) having a linear structure.

[0032] The vinyl group-containing linear organopolysiloxane (A1) has a linear structure and contains vinyl groups, and these vinyl groups become crosslinking points during curing.

[0033] The vinyl group content of the vinyl group-containing linear organopolysiloxane (A1) is not particularly limited, but for example, it is preferable that the vinyl group content is 15 mol% or less and that the vinyl group content is 2 or more in the molecule. This optimizes the amount of vinyl groups in the vinyl group-containing linear organopolysiloxane (A1), and ensures the formation of a network with each component described below. In this specification, the symbol "to" indicates that the upper and lower limits are included, unless otherwise specified.

[0034] In this specification, the vinyl group content refers to the mol % of vinyl group-containing siloxane units when all units constituting the vinyl group-containing linear organopolysiloxane (A1) are taken as 100 mol %, where it is considered that there is one vinyl group per vinyl group-containing siloxane unit.

[0035] The degree of polymerization of the vinyl group-containing linear organopolysiloxane (A1) is not particularly limited, but is, for example, preferably within the range of about 1000 to 10000, and more preferably about 2000 to 5000. The degree of polymerization can be determined, for example, as the polystyrene-equivalent number average degree of polymerization (or number average molecular weight) measured by GPC (gel permeation chromatography) using chloroform as a developing solvent.

[0036] Furthermore, the specific gravity of the vinyl group-containing linear organopolysiloxane (A1) is not particularly limited, but is preferably in the range of about 0.9 to 1.1.

[0037] By using a vinyl group-containing linear organopolysiloxane (A1) having a degree of polymerization and specific gravity within the above ranges, it is possible to improve the heat resistance, flame retardancy, chemical stability, etc. of the resulting silicone rubber.

[0038] As the vinyl group-containing linear organopolysiloxane (A1), those having a structure represented by the following formula (1) are particularly preferred.

[0039] [ka]

[0040] In formula (1), R 1 is a substituted or unsubstituted alkyl group, alkenyl group, aryl group, or a hydrocarbon group consisting of a combination thereof, each having 1 to 10 carbon atoms. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, and a propyl group, with a methyl group being preferred. Examples of the alkenyl group having 1 to 10 carbon atoms include a vinyl group, an allyl group, and a butenyl group, with a vinyl group being preferred. Examples of the aryl group having 1 to 10 carbon atoms include a phenyl group.

[0041] Also, R 2 is a substituted or unsubstituted alkyl group, alkenyl group, aryl group, or a hydrocarbon group consisting of a combination thereof, each having 1 to 10 carbon atoms. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferable. Examples of the alkenyl group having 1 to 10 carbon atoms include a vinyl group, an allyl group, and a butenyl group. Examples of the aryl group having 1 to 10 carbon atoms include a phenyl group.

[0042] Also, R 3is a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms, an aryl group, or a hydrocarbon group consisting of a combination thereof. Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferable. Examples of the aryl group having 1 to 8 carbon atoms include a phenyl group.

[0043] Furthermore, R in formula (1) 1 and R 2 Examples of the substituent of R include a methyl group and a vinyl group. 3 Examples of the substituent include a methyl group.

[0044] In addition, in formula (1), multiple R 1 are independent of each other and may be different or the same. 2 , and R 3 The same applies to.

[0045] Furthermore, m and n are the numbers of repeating units constituting the vinyl group-containing linear organopolysiloxane (A1) represented by formula (1), where m is an integer of 0 to 2000 and n is an integer of 1000 to 10000. m is preferably 0 to 1000 and n is preferably 2000 to 5000.

[0046] A specific example of the structure of the vinyl-containing linear organopolysiloxane (A1) represented by formula (1) is that represented by the following formula (1-1).

[0047] [ka]

[0048] In formula (1-1), R 1 and R 2 are each independently a methyl group or a vinyl group, and at least one of them is a vinyl group.

[0049] The vinyl group-containing linear organopolysiloxane (A1) may contain a first vinyl group-containing linear organopolysiloxane (A1-1) having two or more vinyl groups in the molecule and having a vinyl group content of 0.4 mol% or less. The vinyl group content of the first vinyl group-containing linear organopolysiloxane (A1-1) may be 0.1 mol% or less.

[0050] The vinyl group-containing linear organopolysiloxane (A1) may contain a first vinyl group-containing linear organopolysiloxane (A1-1) and a second vinyl group-containing linear organopolysiloxane (A1-2) having a vinyl group content of 0.5 to 15 mol %.

[0051] By combining the first vinyl group-containing linear organopolysiloxane (A1-1) and the second vinyl group-containing linear organopolysiloxane (A1-2) having a high vinyl group content as the raw rubber, which is the raw material of the silicone rubber, the vinyl groups can be unevenly distributed, and the crosslinking density can be more effectively formed in the crosslinked network of the silicone rubber. As a result, the tear strength of the silicone rubber can be more effectively increased.

[0052] Specifically, the vinyl group-containing linear organopolysiloxane (A1) may be, for example, a vinyl group-containing linear organopolysiloxane represented by the above formula (1-1), 1 is a vinyl group and / or R 2 a first vinyl group-containing linear organopolysiloxane (A1-1) having two or more units in the molecule each of which is a vinyl group and containing 0.4 mol % or less of a unit represented by R 1 is a vinyl group and / or R 2 It is preferable to use a second vinyl group-containing linear organopolysiloxane (A1-2) containing 0.5 to 15 mol % of units in which the vinyl group is present.

[0053] The first vinyl group-containing linear organopolysiloxane (A1-1) preferably has a vinyl group content of 0.01 to 0.2 mol %, and the second vinyl group-containing linear organopolysiloxane (A1-2) preferably has a vinyl group content of 0.8 to 12 mol %.

[0054] Furthermore, when the first vinyl group-containing linear organopolysiloxane (A1-1) and the second vinyl group-containing linear organopolysiloxane (A1-2) are combined and blended, the ratio of (A1-1) to (A1-2) is not particularly limited, but for example, the weight ratio of (A1-1):(A1-2) is preferably 50:50 to 95:5, and more preferably 80:20 to 90:10.

[0055] The first and second vinyl group-containing linear organopolysiloxanes (A1-1) and (A1-2) may each be used alone or in combination of two or more.

[0056] The vinyl group-containing organopolysiloxane (A) may also contain a vinyl group-containing branched organopolysiloxane (A2) having a branched structure.

[0057] <<Organohydrogenpolysiloxane (B)>> The silicone rubber-based hardenable composition of this embodiment can contain an organohydrogenpolysiloxane (B). The organohydrogenpolysiloxane (B) is classified into a linear organohydrogenpolysiloxane (B1) having a linear structure and a branched organohydrogenpolysiloxane (B2) having a branched structure, and may contain either one or both of these.

[0058] The linear organohydrogenpolysiloxane (B1) has a linear structure and a structure in which hydrogen is directly bonded to Si (≡Si-H), and is a polymer that undergoes a hydrosilylation reaction with the vinyl groups of the vinyl group-containing organopolysiloxane (A) and with vinyl groups of components blended into the silicone rubber-based curable composition, thereby crosslinking these components.

[0059] The molecular weight of the linear organohydrogenpolysiloxane (B1) is not particularly limited, but for example, the weight average molecular weight is preferably 20,000 or less, and more preferably 1,000 or more and 10,000 or less.

[0060] The weight average molecular weight of the linear organohydrogenpolysiloxane (B1) can be measured, for example, by polystyrene conversion in gel permeation chromatography (GPC) using chloroform as a developing solvent.

[0061] Furthermore, it is usually preferred that the linear organohydrogenpolysiloxane (B1) does not have a vinyl group, which can reliably prevent the crosslinking reaction from proceeding within the molecule of the linear organohydrogenpolysiloxane (B1).

[0062] As the linear organohydrogenpolysiloxane (B1) as described above, for example, one having a structure represented by the following formula (2) is preferably used.

[0063] [ka]

[0064] In formula (2), R 4is a substituted or unsubstituted alkyl group, alkenyl group, aryl group, a hydrocarbon group combining these groups, or a hydride group having 1 to 10 carbon atoms. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, a propyl group, etc., and among these, a methyl group is preferable. Examples of the alkenyl group having 1 to 10 carbon atoms include a vinyl group, an allyl group, a butenyl group, etc. Examples of the aryl group having 1 to 10 carbon atoms include a phenyl group.

[0065] Also, R 5 is a substituted or unsubstituted alkyl group, alkenyl group, aryl group, a hydrocarbon group combining these groups, or a hydride group having 1 to 10 carbon atoms. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferable. Examples of the alkenyl group having 1 to 10 carbon atoms include a vinyl group, an allyl group, and a butenyl group. Examples of the aryl group having 1 to 10 carbon atoms include a phenyl group.

[0066] In addition, in formula (2), multiple R 4 are independent of each other and may be different or the same. 5 The same applies to R. 4 and R 5 At least two of these are hydride groups.

[0067] Also, R 6 is a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms, an aryl group, or a hydrocarbon group combining these. Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferable. Examples of the aryl group having 1 to 8 carbon atoms include a phenyl group. 6 are independent of each other and may be different from each other or may be the same.

[0068] In addition, R in formula (2) 4 ,R 5 ,R 6Examples of the substituent include a methyl group and a vinyl group, and from the viewpoint of preventing an intramolecular crosslinking reaction, a methyl group is preferred.

[0069] Furthermore, m and n are the numbers of repeating units constituting the linear organohydrogenpolysiloxane (B1) represented by formula (2), where m is an integer of 2 to 150 and n is an integer of 2 to 150. Preferably, m is an integer of 2 to 100 and n is an integer of 2 to 100.

[0070] The linear organohydrogenpolysiloxane (B1) may be used alone or in combination of two or more kinds.

[0071] Since the branched organohydrogenpolysiloxane (B2) has a branched structure, it forms regions with high crosslink density, and is a component that greatly contributes to the formation of a sparsely-dense structure of crosslink density in the silicone rubber system. Also, like the linear organohydrogenpolysiloxane (B1), it has a structure in which hydrogen is directly bonded to Si (≡Si-H), and undergoes a hydrosilylation reaction with the vinyl groups of the vinyl group-containing organopolysiloxane (A) and with the vinyl groups of the components blended in the silicone rubber-based hardening composition, forming a polymer that crosslinks these components.

[0072] The specific gravity of the branched organohydrogenpolysiloxane (B2) is in the range of 0.9 to 0.95.

[0073] Furthermore, it is usually preferred that the branched organohydrogenpolysiloxane (B2) does not have a vinyl group, which can reliably prevent the crosslinking reaction from proceeding within the molecule of the branched organohydrogenpolysiloxane (B2).

[0074] As the branched organohydrogenpolysiloxane (B2), one represented by the following average composition formula (c) is preferred.

[0075] Average composition formula (c) (H a (R7 ) 3-a SiO 1 / 2 ) m (SiO 4 / 2 ) n (In formula (c), R 7 is a monovalent organic group, a is an integer ranging from 1 to 3, and m is H a (R 7 ) 3-a SiO 1 / 2 The number of units, n, is SiO 4 / 2 (the number of units)

[0076] In formula (c), R 7 is a monovalent organic group, preferably a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, an aryl group, or a hydrocarbon group consisting of a combination thereof. Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferred. Examples of the aryl group having 1 to 10 carbon atoms include a phenyl group.

[0077] In formula (c), a is the number of hydride groups (hydrogen atoms directly bonded to Si) and is an integer ranging from 1 to 3, and preferably 1.

[0078] In addition, in formula (c), m is H a (R 7 ) 3-a SiO 1 / 2 The number of units, n, is SiO 4 / 2 It is the number of units.

[0079] The branched organohydrogenpolysiloxane (B2) has a branched structure. The linear organohydrogenpolysiloxane (B1) and the branched organohydrogenpolysiloxane (B2) differ in that their structures are linear or branched, and the number of alkyl groups R bonded to Si (R / Si) when the number of Si is 1 is in the range of 1.8 to 2.1 for the linear organohydrogenpolysiloxane (B1) and 0.8 to 1.7 for the branched organohydrogenpolysiloxane (B2).

[0080] Since the branched organohydrogenpolysiloxane (B2) has a branched structure, for example, when heated in a nitrogen atmosphere to 1000° C. at a heating rate of 10° C. / min, the amount of residue is 5% or more. In contrast, since the linear organohydrogenpolysiloxane (B1) is linear, the amount of residue after heating under the above conditions is almost zero.

[0081] Specific examples of the branched organohydrogenpolysiloxane (B2) include those having a structure represented by the following formula (3).

[0082] [ka]

[0083] In formula (3), R 7 R is a substituted or unsubstituted alkyl group having 1 to 8 carbon atoms, an aryl group, or a hydrocarbon group combining these, or a hydrogen atom. Examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, and a propyl group, and among these, a methyl group is preferable. Examples of the aryl group having 1 to 8 carbon atoms include a phenyl group. 7 Examples of the substituent include a methyl group.

[0084] In addition, in formula (3), multiple R 7 are independent of each other and may be different from each other or may be the same.

[0085] In addition, in formula (3), "-O-Si≡" indicates that Si has a branched structure extending three-dimensionally.

[0086] The branched organohydrogenpolysiloxane (B2) may be used alone or in combination of two or more kinds.

[0087] In addition, the amount of hydrogen atoms (hydride groups) directly bonded to Si in the linear organohydrogenpolysiloxane (B1) and the branched organohydrogenpolysiloxane (B2) is not particularly limited. However, in the silicone rubber-based curable composition, the total amount of hydride groups in the linear organohydrogenpolysiloxane (B1) and the branched organohydrogenpolysiloxane (B2) is preferably 0.5 to 5 moles, more preferably 1 to 3.5 moles, per mole of vinyl group in the vinyl group-containing linear organopolysiloxane (A1). This ensures that a crosslinked network is formed between the linear organohydrogenpolysiloxane (B1) and the branched organohydrogenpolysiloxane (B2) and the vinyl group-containing linear organopolysiloxane (A1).

[0088] <<Silica particles (C)>> The silicone rubber-based hardenable composition of this embodiment may contain silica particles (C) in addition to the vinyl group-containing polyorganosiloxane (A).

[0089] The silica particles (C) are not particularly limited, but for example, fumed silica, calcined silica, precipitated silica, etc. These may be used alone or in combination of two or more kinds.

[0090] The silica particles (C) have a specific surface area, as measured by the BET method, of, for example, 50 to 400 m 2 / g, and 100 to 400m 2 / g is more preferable. The average primary particle size of the silica particles (C) is, for example, preferably from 1 to 100 nm, and more preferably from about 5 to 20 nm.

[0091] By using silica particles (C) having a specific surface area and average particle size within this range, it is possible to improve the hardness and mechanical strength, particularly the tensile strength, of the silicone rubber that is formed.

[0092] <<Silane coupling agent (D)>> The silicone rubber-based hardenable composition of this embodiment may contain a silane coupling agent (D). The silane coupling agent (D) may have a hydrolyzable group. The hydrolyzable group is hydrolyzed by water to become a hydroxyl group, and the hydroxyl group undergoes a dehydration condensation reaction with the hydroxyl group on the surface of the silica particles (C), thereby modifying the surface of the silica particles (C).

[0093] In addition, the silane coupling agent (D) may contain a silane coupling agent having a hydrophobic group. This provides the surface of the silica particles (C) with this hydrophobic group, so that the cohesive force of the silica particles (C) in the silicone rubber-based curable composition and in the silicone rubber is reduced (there is less cohesion due to hydrogen bonds caused by silanol groups), and as a result, it is presumed that the dispersibility of the silica particles in the silicone rubber-based curable composition is improved. This increases the interface between the silica particles and the rubber matrix, and enhances the reinforcing effect of the silica particles. Furthermore, it is presumed that the slipperiness of the silica particles in the matrix is ​​improved during deformation of the rubber matrix. And, due to the improvement in the dispersibility and slipperiness of the silica particles (C), the mechanical strength (for example, tensile strength, tear strength, etc.) of the silicone rubber due to the silica particles (C) is improved.

[0094] Furthermore, the silane coupling agent (D) may contain a silane coupling agent having a vinyl group. This allows the vinyl group to be introduced onto the surface of the silica particles (C). Therefore, when the silicone rubber-based curable composition is cured, that is, when the vinyl group of the vinyl group-containing organopolysiloxane (A) and the hydride group of the organohydrogenpolysiloxane (B) undergo a hydrosilylation reaction to form a network (crosslinked structure), the vinyl group of the silica particles (C) also participates in the hydrosilylation reaction with the hydride group of the organohydrogenpolysiloxane (B), so that the silica particles (C) are also incorporated into the network. This allows the formed silicone rubber to have a low hardness and a high modulus.

[0095] As the silane coupling agent (D), a silane coupling agent having a hydrophobic group and a silane coupling agent having a vinyl group can be used in combination.

[0096] An example of the silane coupling agent (D) is one represented by the following formula (4).

[0097] Y n -Si-(X) 4-n (4) In the above formula (4), n represents an integer of 1 to 3. Y represents any functional group having a hydrophobic group, a hydrophilic group, or a vinyl group, and when n is 1, it is a hydrophobic group, and when n is 2 or 3, at least one of them is a hydrophobic group. X represents a hydrolyzable group.

[0098] The hydrophobic group is an alkyl group having 1 to 6 carbon atoms, an aryl group, or a hydrocarbon group formed by combining these groups, and examples thereof include a methyl group, an ethyl group, a propyl group, and a phenyl group, with a methyl group being particularly preferred.

[0099] In addition, the hydrophilic group may be, for example, a hydroxyl group, a sulfonic acid group, a carboxyl group, or a carbonyl group, and among these, a hydroxyl group is particularly preferred. Note that, although a hydrophilic group may be included as a functional group, it is preferable that the hydrophilic group is not included from the viewpoint of imparting hydrophobicity to the silane coupling agent (D).

[0100] Further, examples of the hydrolyzable group include alkoxy groups such as methoxy and ethoxy groups, chloro groups, and silazane groups. Among these, silazane groups are preferred because of their high reactivity with the silica particles (C). In addition, those having a silazane group as a hydrolyzable group can be easily obtained by adding (Y n -Si-) structures.

[0101] Specific examples of the silane coupling agent (D) represented by the above formula (4) include, for example, alkoxysilanes such as methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, and decyltrimethoxysilane; chlorosilanes such as methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, and phenyltrichlorosilane; and hexamethyldisilazane, which have a hydrophobic group as a functional group. Examples of the silane having a vinyl group include alkoxysilanes such as methacryloxypropyltriethoxysilane, methacryloxypropyltrimethoxysilane, methacryloxypropylmethyldiethoxysilane, methacryloxypropylmethyldimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, and vinylmethyldimethoxysilane; chlorosilanes such as vinyltrichlorosilane and vinylmethyldichlorosilane; and divinyltetramethyldisilazane. Among these, taking into consideration the above description, it is particularly preferable that the silane having a hydrophobic group is hexamethyldisilazane, and the silane having a vinyl group is divinyltetramethyldisilazane.

[0102] <<Platinum or platinum compounds (E)>> The silicone rubber-based hardenable composition of this embodiment may contain platinum or a platinum compound (E). Platinum or a platinum compound (E) is a catalytic component that acts as a catalyst during curing. The amount of platinum or a platinum compound (E) added is a catalytic amount.

[0103] As the platinum or platinum compound (E), known substances can be used, such as platinum black, platinum supported on silica or carbon black, chloroplatinic acid or an alcohol solution of chloroplatinic acid, a complex salt of chloroplatinic acid and an olefin, and a complex salt of chloroplatinic acid and a vinylsiloxane.

[0104] The platinum or platinum compound (E) may be used alone or in combination of two or more kinds.

[0105] <<Water(F)>> Furthermore, the silicone rubber-based hardening composition of this embodiment may contain water (F) in addition to the above components (A) to (E).

[0106] Water (F) functions as a dispersion medium for dispersing each component contained in the silicone rubber-based hardening composition, and is also a component that contributes to the reaction between the silica particles (C) and the silane coupling agent (D). Therefore, the silica particles (C) and the silane coupling agent (D) can be more reliably linked to each other in the silicone rubber, and uniform properties can be exhibited overall.

[0107] Furthermore, the silicone rubber-based hardening composition of this embodiment may contain, in addition to the above components (A) to (F), known additive components that are blended into silicone rubber-based hardening compositions. Examples include diatomaceous earth, iron oxide, zinc oxide, titanium oxide, barium oxide, magnesium oxide, cerium oxide, calcium carbonate, magnesium carbonate, zinc carbonate, glass wool, mica, etc. In addition, dispersants, pigments, dyes, antistatic agents, antioxidants, flame retardants, thermal conductivity improvers, etc. may be blended as appropriate.

[0108] In the silicone rubber-based hardening composition, the content ratio of each component is not particularly limited, but is set, for example, as follows.

[0109] In this embodiment, the upper limit of the content of the silica particles (C) may be, for example, 80 parts by weight or less, preferably 75 parts by weight or less, and more preferably 70 parts by weight or less, based on 100 parts by weight of the total amount of the vinyl group-containing organopolysiloxane (A). This allows for a balance between mechanical strength such as hardness and tensile strength. The lower limit of the content of the silica particles (C) is, for example, 20 parts by weight or more, preferably 25 parts by weight or more, based on 100 parts by weight of the total amount of the vinyl group-containing organopolysiloxane (A). This allows for a balance between tear strength and breaking elongation.

[0110] The silane coupling agent (D) is preferably contained in an amount of 5 parts by weight or more and 100 parts by weight or less, more preferably 5 parts by weight or more and 40 parts by weight or less, per 100 parts by weight of the vinyl group-containing organopolysiloxane (A), which can reliably improve the dispersibility of the silica particles (C) in the silicone rubber-based curable composition.

[0111] The content of the organohydrogenpolysiloxane (B) is preferably, for example, 0.5 parts by weight or more and 20 parts by weight or less, and more preferably 0.8 parts by weight or more and 15 parts by weight or less, based on 100 parts by weight of the total amount of the vinyl group-containing organopolysiloxane (A), the silica particles (C), and the silane coupling agent (D). By keeping the content of (B) within the above range, a more effective curing reaction may be achieved.

[0112] The content of platinum or platinum compound (E) means the amount of catalyst, and can be set appropriately, but specifically, the amount of platinum group metal in this component is 0.01 to 1000 ppm by weight, preferably 0.1 to 500 ppm, relative to the total amount of vinyl group-containing organopolysiloxane (A), silica particles (C), and silane coupling agent (D). By making the content of platinum or platinum compound (E) equal to or greater than the lower limit, the obtained silicone rubber composition can be sufficiently cured. By making the content of platinum or platinum compound (E) equal to or less than the upper limit, the curing speed of the obtained silicone rubber composition can be improved.

[0113] Furthermore, when water (F) is contained, its content can be appropriately set, but specifically, for example, it is preferably in the range of 10 to 100 parts by weight, more preferably in the range of 30 to 70 parts by weight, relative to 100 parts by weight of the silane coupling agent (D). This makes it possible to more reliably proceed with the reaction between the silane coupling agent (D) and the silica particles (C).

[0114] <Silicone rubber manufacturing method> Next, a method for producing the silicone rubber of this embodiment will be described. In the method for producing the silicone rubber of this embodiment, a silicone rubber-based hardening composition is prepared, and the silicone rubber can be obtained by hardening the silicone rubber-based hardening composition. Details are provided below.

[0115] First, the components of the silicone rubber-based hardening composition are mixed uniformly using any kneading device to prepare the silicone rubber-based hardening composition.

[0116] [1] For example, a predetermined amount of vinyl group-containing organopolysiloxane (A), silica particles (C), and a silane coupling agent (D) are weighed out, and then kneaded using any kneading device to obtain a kneaded product containing these components (A), (C), and (D).

[0117] It is preferable to prepare this mixture by first kneading the vinyl-containing organopolysiloxane (A) with the silane coupling agent (D) and then kneading (mixing) the silica particles (C), which improves the dispersibility of the silica particles (C) in the vinyl-containing organopolysiloxane (A).

[0118] In addition, when obtaining this kneaded product, water (F) may be added to the kneaded product of the components (A), (C), and (D) as necessary, which allows the reaction between the silane coupling agent (D) and the silica particles (C) to proceed more reliably.

[0119] Furthermore, it is preferable that the kneading of each of the components (A), (C), and (D) is carried out through a first step of heating at a first temperature and a second step of heating at a second temperature. This allows the surface of the silica particles (C) to be surface-treated with the coupling agent (D) in the first step, and allows the by-products generated by the reaction between the silica particles (C) and the coupling agent (D) to be reliably removed from the kneaded product in the second step. After that, the component (A) may be added to the obtained kneaded product as necessary, and further kneaded. This allows the compatibility of the components in the kneaded product to be improved.

[0120] The first temperature is preferably, for example, about 40 to 120° C., and more preferably, for example, about 60 to 90° C. The second temperature is preferably, for example, about 130 to 210° C., and more preferably, for example, about 160 to 180° C.

[0121] Moreover, the atmosphere in the first step is preferably an inert atmosphere such as a nitrogen atmosphere, and the atmosphere in the second step is preferably a reduced pressure atmosphere.

[0122] Furthermore, the time for the first step is, for example, preferably about 0.3 to 1.5 hours, and more preferably about 0.5 to 1.2 hours, and the time for the second step is, for example, preferably about 0.7 to 3.0 hours, and more preferably about 1.0 to 2.0 hours.

[0123] By setting the above conditions for the first and second steps, the above effects can be obtained more significantly.

[0124] [2] Next, the organohydrogenpolysiloxane (B) and platinum or a platinum compound (E) are weighed out in predetermined amounts, and then the components (B) and (E) are kneaded into the mixture prepared in the above step [1] using any kneading device to obtain a silicone rubber-based curable composition. The obtained silicone rubber-based curable composition may be a paste containing a solvent.

[0125] In addition, when mixing the components (B) and (E), it is preferable to mix the mixture prepared in the above step [1] with the organohydrogenpolysiloxane (B) and the mixture prepared in the above step [1] with platinum or a platinum compound (E), and then mix the mixtures together. This allows the components (A) to (E) to be reliably dispersed in the silicone rubber-based curable composition without allowing the reaction between the vinyl group-containing organopolysiloxane (A) and the organohydrogenpolysiloxane (B) to proceed.

[0126] The temperature at which the components (B) and (E) are kneaded is, for example, preferably about 10 to 70°C, and more preferably about 25 to 30°C, as roll setting temperature.

[0127] Furthermore, the kneading time is, for example, preferably about 5 minutes to 1 hour, and more preferably about 10 to 40 minutes.

[0128] In the above steps [1] and [2], by setting the temperature within the above range, the progress of the reaction between the vinyl group-containing organopolysiloxane (A) and the organohydrogenpolysiloxane (B) can be more reliably prevented or inhibited. In addition, in the above steps [1] and [2], by setting the kneading time within the above range, the components (A) to (E) can be more reliably dispersed in the silicone rubber-based curable composition.

[0129] The kneading device used in each of steps [1] and [2] is not particularly limited, but for example, a kneader, a two-roll mill, a Banbury mixer (continuous kneader), a pressure kneader, etc. can be used.

[0130] In addition, a reaction inhibitor such as 1-ethynylcyclohexanol may be added to the kneaded mixture in step [2], which makes it possible to more effectively prevent or inhibit the progress of the reaction between the vinyl group-containing organopolysiloxane (A) and the organohydrogenpolysiloxane (B) even if the temperature of the kneaded mixture is set to a relatively high temperature.

[0131] [3] Next, the silicone rubber-based hardenable composition is hardened to form a silicone rubber.

[0132] In this embodiment, the curing step of the silicone rubber-based curable composition is carried out, for example, by heating at 100 to 250° C. for 1 to 30 minutes (first curing) and then post-baking at 200° C. for 1 to 4 hours (second curing). Through the steps described above, a silicone rubber can be obtained using the silicone rubber-based hardening composition of this embodiment.

[0133] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0134] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0135] The raw material components used in the examples and comparative examples shown in Table 1 are shown below. (Vinyl-containing organopolysiloxane (A)) Low vinyl group-containing linear organopolysiloxane (A1-1): Vinyl group-containing dimethylpolysiloxane (structure represented by formula (1-1) and R 1 (Structure in which only the terminal is vinyl) High vinyl-containing linear organopolysiloxane (A1-2): Vinyl-containing dimethylpolysiloxane (having the structure represented by formula (1-1) and R 1 and R 2 is a vinyl group) Low vinyl group-containing linear organopolysiloxane (A1-3): Vinyl group-containing dimethylpolysiloxane (structure represented by formula (1-1) and R 1 and R 2 is a vinyl group)

[0136] (Organohydrogenpolysiloxane (B)) Momentive: "TC-25D"

[0137] (Silica particles (C)) Silica particles (C-1): Silica particles (particle size 7 nm, specific surface area 300 m 2 / g), manufactured by Nippon Aerosil Co., Ltd., "AEROSIL300" Silica particles (C-2): Silica particles (particle size 7 nm, specific surface area 240 m 2 / g), Nippon Aerosil Co., Ltd., "AEROSIL R976"

[0138] (Silane coupling agent (D)) Silane coupling agent (D-1): Hexamethyldisilazane (HMDZ), manufactured by Gelest, "HEXAMETHYLDISILAZANE (SIH6110.1)" Silane coupling agent (D-2): Divinyltetramethyldisilazane, manufactured by Gelest, "1,3-DIVINYLTETRAMETHYLDISILAZANE (SID4612.0)"

[0139] (Platinum or platinum compounds (E)) Momentive: "TC-25A"

[0140] (Synthesis of vinyl group-containing organopolysiloxane (A)) [Synthesis Scheme 1: Synthesis of low vinyl group-containing linear organopolysiloxane (A1-1)] A low-vinyl-group-containing linear organopolysiloxane (A1-1) was synthesized according to the following formula (5). That is, 74.7 g (252 mmol) of octamethylcyclotetrasiloxane and 0.1 g of potassium siliconate were placed in a 300 mL separable flask equipped with a cooling tube and stirring blade and replaced with Ar gas, and the temperature was raised and the mixture was stirred at 120° C. for 30 minutes. At this time, an increase in viscosity was confirmed. The mixture was then heated to 155° C. and stirred for 3 hours, after which 0.1 g (0.6 mmol) of 1,3-divinyltetramethyldisiloxane was added and the mixture was stirred at 155° C. for an additional 4 hours. After four hours, the mixture was diluted with 250 mL of toluene and then washed three times with water. The washed organic layer was washed several times with 1.5 L of methanol for reprecipitation purification, and the oligomer and polymer were separated. The resulting polymer was dried overnight at 60°C under reduced pressure to obtain a low-vinyl-group-containing linear organopolysiloxane (A1-1) (Mn = 2.2 × 10 5 , Mw=4.8×10 5 The vinyl group content calculated from H-NMR spectrum measurement was 0.04 mol %.

[0141] [ka]

[0142] [Synthesis Scheme 2: Synthesis of high vinyl group-containing linear organopolysiloxane (A1-2)] A highly vinyl-containing linear organopolysiloxane (A1-2) was synthesized as shown in formula (6) below by the same synthesis process as for (A1-1), except that 0.86 g (2.5 mmol) of 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane was used in addition to 74.7 g (252 mmol) of octamethylcyclotetrasiloxane in the synthesis process for (A1-1) above. (Mn=2.3×10 5 , Mw=5.0×10 5 The vinyl group content calculated from H-NMR spectrum measurement was 0.93 mol %. [ka]

[0143] [Synthesis Scheme 3: Synthesis of low vinyl group-containing linear organopolysiloxane (A1-3)] In the synthesis process of (A1-2) above, 75.3 g (254 mmol) of octamethylcyclotetrasiloxane and 0.12 g (0.35 mmol) of 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane were used, and the stirring time after heating to 155°C was changed to 3 hours. The same synthesis process as that of (A1-2) was repeated to synthesize a low vinyl group-containing linear organopolysiloxane (A1-3) as shown in the above formula (6). (Mn=2.5×10 5 , Mw=5.0×10 5 The vinyl group content calculated from H-NMR spectrum measurement was 0.13 mol %.

[0144] (Examples 1 to 3: Preparation of silicone rubber-based curable compositions) A silicone rubber-based hardenable composition was prepared as follows. First, a mixture of 90% vinyl group-containing organopolysiloxane (A), silane coupling agent (D), and water (F) was pre-kneaded in the proportions shown in Table 1 below, and then silica particles (C) were added to the mixture and further kneaded to obtain a kneaded product (silicone rubber compound). Here, the kneading after the addition of the silica particles (C) was carried out through a first step of kneading for 1 hour under conditions of 60 to 90°C in a nitrogen atmosphere for the coupling reaction, and a second step of kneading for 2 hours under conditions of 160 to 180°C in a reduced pressure atmosphere for the removal of the by-product (ammonia). Thereafter, the mixture was cooled, and the remaining 10% of the vinyl group-containing organopolysiloxane (A) was added in two portions and kneaded for 20 minutes. Next, organohydrogenpolysiloxane (B) (TC-25D) and platinum or platinum compound (E) (TC-25A) were added to 100 parts by weight of the obtained kneaded product (silicone rubber compound) in the ratios shown in Table 1 below, and the mixture was kneaded with a roll to obtain a silicone rubber-based curable composition.

[0145] Comparative Example 1: Preparation of Silicone Rubber-Based Curable Composition In the ratio shown in Table 1 below, vinyl-containing organopolysiloxane (A) was kneaded alone for 5 minutes, and then silica particles (C) were added to the mixture and kneaded for an additional 2 hours to obtain a kneaded product (silicone rubber compound). Next, organohydrogenpolysiloxane (B) (TC-25D) and platinum or platinum compound (E) (TC-25A) were added to 100 parts by weight of the obtained kneaded product (silicone rubber compound) in the ratios shown in Table 1 below, and the mixture was kneaded with a roll to obtain a silicone rubber-based curable composition.

[0146] (Comparison 2: Preparation of silicone rubber-based curable composition) The vinyl-containing organopolysiloxane (A) was kneaded for 2 hours in the ratio shown in Table 1 below to obtain a kneaded product (silicone rubber compound). Next, organohydrogenpolysiloxane (B) (TC-25D) and platinum or platinum compound (E) (TC-25A) were added to 100 parts by weight of the obtained kneaded product (silicone rubber compound) in the ratios shown in Table 1 below, and the mixture was kneaded with a roll to obtain a silicone rubber-based curable composition.

[0147] [Table 1]

[0148] (Preparation of silicone rubber for evaluation) In Examples 1 to 3 and Comparative Examples 1 and 2, the obtained silicone rubber-based hardening composition was pressed at 170°C and 10 MPa for 10 minutes to form a sheet having a thickness of 1 mm and was subjected to a primary hardening. Subsequently, the sheet was heated at 200°C for 4 hours to be subjected to a secondary hardening. As a result, a sheet-shaped silicone rubber (a hardened product of the silicone rubber-based hardening composition) was obtained.

[0149] The obtained silicone rubber sheet (elastomer sheet) was evaluated based on the following evaluation items. The tensile strength and breaking elongation were measured on three samples, and the average of the three values ​​was used as the measured value. The tear strength was measured on five samples, and the average value of the five was recorded as the measured value. The hardness was measured using two samples, n=5 for each sample, and the average value of the total 10 measurements was taken as the measured value. The average values ​​are shown in Table 2.

[0150] [Table 2]

[0151] <Hardness: Durometer hardness> Six of the obtained 1 mm thick sheet-like silicone rubbers were laminated to prepare a 6 mm test piece. The type A durometer hardness of the obtained test piece was measured at 25°C in accordance with JIS K6253 (1997).

[0152] <Tear strength> A crescent-shaped test piece was prepared in accordance with JIS K6252 (2001) using the obtained 1 mm thick sheet-like silicone rubber, and the tear strength (TS) of the obtained crescent-shaped test piece at 25°C was measured, with the unit being N / mm.

[0153] <Elongation at break> Using the obtained 1 mm thick sheet-like silicone rubber, dumbbell-shaped No. 3 test pieces were prepared in accordance with JIS K6251 (2004), and the breaking elongation (BE) of the obtained dumbbell-shaped No. 3 test pieces was measured at 25°C. The breaking elongation was calculated by [gauge line movement distance (mm)] ÷ [initial gauge line distance (20 mm)] × 100. The unit is %.

[0154] <Wear loss> A sheet sample having a thickness of 2 mm was prepared in the same manner as described above (preparation of silicone rubber for evaluation). The obtained samples were subjected to a Taber abrasion test in accordance with JIS K7204. The abrasion wheel used was "CS-0+S42 Sandpaper Strip." The weight (g) of the sheet sample before the Taber abrasion test was A, and the weight (g) of the sheet sample after the Taber abrasion test was B. The abrasion loss (g) was calculated from the formula: AB. Two samples were evaluated, and the average calculated abrasion loss is shown in Table 2. In Table 2, "1>" means that the abrasion loss is more than 1 g.

[0155] The silicone rubber-based curable compositions of Examples 1 to 3 showed superior abrasion resistance compared to Comparative Examples 1 and 2. Among the Examples, Examples 1 and 2 showed a larger TS×BE than Example 3, and showed superior abrasion resistance. The silicone rubber-based curable compositions of such Examples can be suitably used for blade members, specifically wiper blades.

Claims

1. A silicone rubber-based hardening composition used to form a blade member, comprising: A vinyl group-containing polyorganosiloxane (A), Silica particles (C) surface-treated with a silane coupling agent (D); 1. A silicone rubber-based curable composition comprising:

2. The silicone rubber-based hardening composition according to claim 1, A silicone rubber-based curable composition, wherein the content of the silica particles (C) is 20 parts by weight or more and 80 parts by weight or less based on 100 parts by weight of the vinyl group-containing polyorganosiloxane (A).

3. The silicone rubber-based hardening composition according to claim 1 or 2, When the tear strength is TS (N / mm) and the breaking elongation is BE (%), When the tear strength of the cured product of the silicone rubber-based curable composition is TS (N / mm) and the breaking elongation is BE (%), the following properties are obtained: TS, BE is 2.3 x 10 4 A silicone rubber-based curable composition that satisfies ≦TS×BE. (Procedure for measuring tear strength) A crescent-shaped test piece is prepared from the cured product of the silicone rubber-based curable composition in accordance with JIS K6252 (2001), and the tear strength of the resulting crescent-shaped test piece at 25° C. is measured in units of N / mm. (Procedure for measuring elongation at break) A dumbbell-shaped No. 3 test piece is prepared using the cured product of the silicone rubber-based curable composition in accordance with JIS K6251 (2004), and the breaking elongation of the resulting dumbbell-shaped No. 3 test piece is measured at 25° C. The breaking elongation is calculated by [gauge line movement distance (mm)]÷[initial gauge line distance (20 mm)]×100, and is expressed in %.

4. The silicone rubber-based hardening composition according to claim 3, The silicone rubber-based curable composition has a tear strength of 25 N / mm or more.

5. The silicone rubber-based hardening composition according to any one of claims 1 to 4, A silicone rubber-based hardening composition, wherein a durometer hardness A of a cured product of the silicone rubber-based hardening composition is 30 or more and 90 or less, as measured by the following procedure. (Procedure for measuring durometer hardness A) A sheet-like test specimen is prepared using the cured product of the silicone rubber-based curable composition, and the durometer hardness A of the obtained sheet-like test specimen at 25° C. is measured in accordance with JIS K6253 (1997).

6. The silicone rubber-based hardening composition according to any one of claims 1 to 5, The vinyl group-containing polyorganosiloxane (A) has two vinyl groups only at the terminals of the molecule and contains a first vinyl group-containing linear organopolysiloxane (A1-1) having a vinyl group content of 0.4 mol% or less.

7. The silicone rubber-based hardening composition according to any one of claims 1 to 6, A silicone rubber-based hardening composition comprising the silica particles (C) that have been surface-treated with a silane coupling agent having a vinyl group.

8. A blade member comprising a cured product of the silicone rubber-based curable composition according to any one of claims 1 to 7.

9. A wiper blade comprising a cured product of the silicone rubber-based curable composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Wiper blade, and method for manufacturing the same

    JP2014046734A