Method for producing biocompatible member
A biocompatible member with controlled water content and fiber bonding ensures high biocompatibility and ease of handling, supporting tissue integration and healing by maintaining structural integrity and flexibility.
Patent Information
- Application Number
- JP2024112166
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2040-02-06
AI Technical Summary
Existing biocompatible members lack high biocompatibility and ease of handling, as they often fail to maintain shape under stress while being soft enough to be cut or molded.
A biocompatible member composed of fibers bonded with water content between 40% to 90% by mass, manufactured through electrospinning, volatile liquid impregnation, and hydrous treatment, allowing for a soft yet strong and flexible structure.
The biocompatible member maintains shape under stress while being easily handled and promotes cell proliferation by aligning with tissue structures, facilitating wound healing and tissue reconstruction.
Smart Images

Figure 2024138475000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiments relate to a method for manufacturing a biocompatible component. [Background technology]
[0002] In the medical field, biocompatible materials have been developed as materials to be used in living bodies or as a base for cell growth. Biocompatible materials are required to have high biocompatibility and to be easy to handle. For example, biocompatible materials are required to be strong enough to maintain their shape even when held with tweezers, and soft enough to be cut with scissors or a scalpel. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 6450894 [Patent Document 2] Patent No. 6470327 Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the embodiments is to provide a method for producing a biocompatible component that is highly biocompatible and easy to handle. [Means for solving the problem]
[0005] A biocompatible component according to an embodiment includes an aggregate in which fibers containing a biocompatible material are bonded to each other, and water contained between the fibers. The water content in the biocompatible component is 40% by mass or more and 90% by mass or less.
[0006] A method for manufacturing a biocompatible component according to an embodiment includes the steps of forming a laminated sheet by depositing fibers containing a biocompatible material, permeating the laminated sheet with a volatile liquid, volatilizing the liquid that has permeated the laminated sheet, and subjecting the laminated sheet from which the liquid has been volatilized to a moisture-containing treatment. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a diagram showing a biocompatible component according to a first embodiment. [Diagram 2] 1(a) and 1(b) are diagrams showing a method for producing a biocompatible component according to a first embodiment. [Diagram 3] FIG. 2(a) to (c) are diagrams showing a method for producing a biocompatible component according to the first embodiment. [Figure 4] FIG. 11 is a diagram showing a hydrostatic pressure treatment in a method for producing a biocompatible component according to a second embodiment. [Diagram 5] FIG. 11 is a diagram showing a decompression process in a method for producing a biocompatible component according to a third embodiment. [Figure 6] (a) is an SEM photograph of the surface of a deposition layer formed by electrospinning, and (b) is an SEM photograph of the surface of a laminated sheet after ethanol treatment. [Figure 7] 13(a) and (b) are SEM photographs of the surface of a freeze-dried sample of a biocompatible component according to a test example. [Figure 8] 1 is a graph showing the results of differential scanning calorimetry of a laminate sheet and a biocompatible component according to a test example, with the horizontal axis representing temperature and the vertical axis representing heat flow. [Figure 9] 1 is a table showing the results of differential scanning calorimetry of a laminate sheet and a biocompatible component according to a test example. [Figure 10] 13 is a table showing the measurement results of the compressive elastic modulus of the biocompatible components according to the test examples. [Figure 11]Graph (a) shows the storage modulus-frequency curve of a biocompatible material according to a test example, with frequency on the horizontal axis and storage modulus on the vertical axis; graph (b) shows the loss modulus-frequency curve of a biocompatible material according to a test example, with frequency on the horizontal axis and loss modulus on the vertical axis. [Figure 12] 1 is a surface SEM photograph showing a cut surface of a biocompatible component according to a test example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <First embodiment> The first embodiment will be described below. FIG. 1 is a diagram showing a biocompatible component according to this embodiment.
[0009] 1, the biocompatible component 1 according to this embodiment includes an aggregate 12 in which a plurality of fibers 11 are bonded together, and water 13 contained between the fibers 11. The content of water 13 in the biocompatible component 1 is 40% by mass or more and 90% by mass or less.
[0010] The fiber 11 includes a biocompatible material. The biocompatible material is, for example, a bio-derived material. The bio-derived material is a material produced by life activities, or a material obtained by processing the material. The biocompatible material does not have to be a bio-derived material, and may be, for example, a synthetic polymer, a functional protein or a synthetic polypeptide obtained by artificial synthesis, or the like.
[0011] Examples of biocompatible materials include proteins such as collagen, laminin, and gelatin, nucleic acids such as deoxyribonucleic acid (DNA) and ribonucleic acid (RNA), and polysaccharides such as chitosan, chitin, hyaluronic acid, alginic acid, and heparin. Examples of synthetic polymers include polyethylene (PE), polypropylene (PP), polymethylmethacrylate (PMMA), poly(2-hydroxyethyl methacrylate) (PHEMA), poly(N-isopropylacrylamide) (PNIPAAm), polyvinyl alcohol (PVA), polycyanoacrylate, polyethylene terephthalate (PET), nylon 66, polyurethane (PU), polyethylene glycol (PEG), polyethylene oxide (PEO), polylactic acid (PLA), polyglycolic acid, polyhydroxy acids such as polycaprolactone, and silicones such as polydimethylsiloxane (PDMS) and polydimethylsiloxane (PDMS).
[0012] For example, the fibers 11 are made of collagen with a high-dimensional, i.e., three-dimensional structure. The original structure of a collagen molecule is a triple helix structure, and the collagen constituting the fibers 11 also maintains this structure. In the aggregate 12, the fibers 11 are bonded to each other by being partially fused, for example, by non-covalent interactions. Examples of non-covalent interactions include intermolecular forces, hydrophobic interactions, and hydrogen bonds. The diameter of the fibers 11 is, for example, about 60 nm to 3 μm.
[0013] The shape of the biocompatible component is, for example, a sheet. The biocompatible component 1 has a plurality of layers 10 laminated in the thickness direction. The layers 10 are laminated, for example, in a number of about 2 to 100 layers, and each layer 10 has a thickness of, for example, about 5 to 500 μm. The total thickness of the biocompatible component 1 is, for example, about 0.03 to 50 mm.
[0014] In each layer 10, the fibers 11 are oriented in, for example, one direction. The orientation directions of the fibers 11 in two adjacent layers 10 cross each other, for example, are approximately perpendicular to each other. As shown in FIG. 1, in an XYZ orthogonal coordinate system, when the thickness direction of the biocompatible component 1, i.e., the stacking direction of the layers 10, is the Z direction, layers 10 oriented in the X direction and layers 10 oriented in the Y direction are stacked alternately. In each layer 10, adjacent fibers 11 are bonded to each other in a linear manner. The bonding strength between the layers 10 is weaker than the bonding strength between the fibers 11 within the layers 10. Voids 15 having a diameter of 10 μm or more are present on the surface of the biocompatible component 1 at a density of 1 / mm. 2 It is formed with a density of more than 1000 nm.
[0015] FIG. 1 is a schematic diagram conceptually showing the configuration of the biocompatible component 1, and does not necessarily correspond to the actual configuration. For example, as described above, the diameter of the fiber 11 is about 1 / 1000 of the thickness of the layer 10, but in FIG. 1, the fiber 11 is drawn larger than it actually is to make the drawing easier to see. In addition, since the fibers 11 are bonded to each other, even if the biocompatible component 1 is observed under a microscope, it is not always possible to distinguish each fiber 11. Furthermore, the boundaries between the layers 10 are not always clearly observed. The same applies to other figures described later.
[0016] The compressive elastic modulus of the biocompatible component 1 is 5 kPa or more. The biocompatible component 1 is an elastic body, and when a viscoelasticity-frequency curve is measured by a dynamic viscoelastic method, the storage elastic modulus is higher than the loss elastic modulus. The biocompatible component 1 is a solid, soft elastic body as a whole, and has no fluidity. The biocompatible component 1 is also transparent or translucent.
[0017] Next, a method for producing the biocompatible component 1 according to this embodiment will be described. 2(a) and (b) and 3(a) to (c) are diagrams showing a manufacturing method of the biocompatible component 1 according to this embodiment.
[0018] 2(a), a fiber 11 is formed by an electrospinning method. A manufacturing apparatus 101 for the fiber 11 is provided with a nozzle 102, a roller 103, and a power source 104. The roller 103 rotates at high speed. The power source 104 applies a voltage to the nozzle 102.
[0019] In this state, the charged raw material liquid 110 is discharged from the nozzle 102. The raw material liquid 110 contains a biocompatible material, for example, collagen. Immediately after being discharged from the nozzle 102, the raw material liquid 110 is stretched by electrostatic repulsion, becomes fibers 11, reaches the outer circumferential surface of the roller 103, and is taken up at high speed by the roller 103. As a result, the fibers 11 are deposited in a state oriented in the outer circumferential direction of the roller 103, and a deposition layer 10a is formed. The deposition layer 10a is a layer in which the fibers 11 are deposited in a state in which they are oriented.
[0020] Next, as shown in Fig. 2(b), a plurality of deposition layers 10a are laminated on the substrate 112. At this time, the orientation directions of adjacent deposition layers 10a are crossed, for example, perpendicular to each other. A laminated sheet 10b is formed by the stacked deposition layers 10a.
[0021] The composition and shape of the substrate 112 are not particularly limited, but a composition and shape that provide as good adhesion as possible to the deposition layer 10a are preferable. The material of the substrate 112 may be, for example, synthetic polymers such as polystyrene (PS), polyethylene (PE), polypropylene (PP), polymethylmethacrylate (PMMA), polylactic acid (PLA), polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyacrylonitrile (PAN), polyethylene terephthalate (PET), polycarbonate (PC), polyurethane (PU), silicone, natural polymers such as collagen, gelatin, laminin, chitosan, chitin, decellularized tissue, human skin, organs, and other biological tissues. In addition, the substrate 112 may be a biocompatible member 1 that has already been manufactured, or a member such as a substrate, cloth, sphere, rod, or tube formed by molding the biocompatible member 1, or an artificial biological structure such as an artificial blood vessel, an artificial valve, an artificial joint, or an artificial tooth. Additionally, substrate 112 may include drugs, cells, blood, bodily fluids, and the like.
[0022] Next, as shown in Fig. 3(a), a volatile liquid is permeated into the laminate sheet 10b. The volatile liquid is not particularly limited, but it is preferable to use a liquid in which the fibers 11 are as insoluble as possible. For example, water, alcohols (ethanol, methanol, isopropyl alcohol, etc.), and alcohol aqueous solutions are used. For example, a cloth 113 soaked in ethanol is placed on the laminate sheet 10b placed on the substrate 112. This causes the ethanol in the cloth 113 to permeate into the laminate sheet 10b.
[0023] Next, as shown in FIG. 3(b), the volatile liquid that has permeated into the laminated sheet 10b is volatilized and removed from the laminated sheet 10b. As a result, the capillary force of the liquid causes some of the fibers 11 to weld together, and the fibers 11 are bonded together. As a result, an aggregate 12 is formed on the substrate 112. The aggregate 12 is a structure in which the fibers 11 are three-dimensionally accumulated. Furthermore, if spaces (air bubbles) that are not filled with the volatile liquid are formed in the laminated sheet 10b, voids 15 (see FIG. 1) are formed in the aggregate 12 after the volatile liquid is removed. The thickness of the aggregate 12 becomes about 1 / 3 to 1 / 5 times that of the laminated sheet 10b before the volatile liquid is permeated. Furthermore, the aggregate 12 becomes transparent or translucent.
[0024] The assembly 12 formed on the substrate 112 may be peeled off from the substrate 112 and used alone, or may be used integrally with the substrate 112 .
[0025] Next, as shown in FIG. 3(c), the assembly 12 is subjected to a hydration treatment. The hydration treatment may be performed by immersing the assembly 12 in water 116 in a container 115, pouring the water 116 into the assembly, contacting the assembly with a cloth soaked in the water 116, or spraying the assembly 12 with the water 116 in a mist form. The water 116 may be pure water or physiological saline. The water 116 may be serum such as fetal bovine serum (FBS), various liquid media, an aqueous solution containing protein, RNA, DNA, or a substrate, or may be a suspension of cells, body fluid, or blood. As a result, water penetrates between the fibers 11, and the fibers 11 absorb water and swell, thereby producing the biocompatible component 1. By these hydration treatments, the biocompatible component 1 swells 2 to 5 times in a room temperature environment.
[0026] Next, the effects of this embodiment will be described. The biocompatible member 1 according to this embodiment has high biocompatibility because the fibers 11 are made of a biocompatible material. For example, even if the biocompatible member 1 is placed in a living body, it does not show toxicity. In addition, rejection reactions such as inflammation caused by the living body can be suppressed. In particular, by forming the fibers 11 from high-dimensional collagen that has not deteriorated, the rejection reaction can be suppressed more effectively. In addition, when the fibers 11 are formed from a biomaterial and the biocompatible member 1 is placed in a living body, the biomaterial is consumed with the metabolism of the living body, and the fibers 11 are loosened. This makes it easier for cells to enter between the fibers 11.
[0027] Furthermore, the biocompatible component 1 contains water 13 at a content rate of 40% by mass to 90% by mass. This water content rate is close to the water content rate in a living body. This also makes the biocompatible component 1 highly biocompatible.
[0028] Furthermore, the surface of the biocompatible component 1 has voids 15 with a diameter of 10 μm or more at a rate of 1 void / mm 2 The voids 15 are formed with a density equal to or higher than this. As a result, when the biocompatible component 1 is placed inside a living body, living body cells can easily enter into the voids 15. The cells that have entered into the voids 15 use them as a scaffold to further enter into the biocompatible component 1.
[0029] Furthermore, the biocompatible component 1 is provided with a plurality of layers 10, and the bonding strength between the layers 10 is weaker than the bonding strength between the fibers 11 within the layers 10. For this reason, when the biocompatible component 1 is placed in a living body and pressure or heat is applied to the biocompatible component 1 from the surrounding living tissue, the layers 10 tend to peel off and gaps are likely to be formed. This allows cells to enter the gaps between the layers 10, further promoting the formation of cellular tissue.
[0030] Furthermore, since the fibers 11 of the biocompatible component 1 have orientation, the biocompatibility of the biocompatible component 1 can be further improved by aligning the orientation direction of the fibers 11 with the direction of biological tissue.
[0031] Thus, the biocompatible material 1 is highly compatible with the surrounding cell tissue. Therefore, for example, if the biocompatible material 1 is placed in the space after tissue damage or tumor resection, it is expected that the biocompatible material 1 will act as a scaffold for cell growth and promote wound healing and tissue reconstruction. In addition, if the biocompatible material 1 is used as a covering material when implanting artificial objects or drugs in the body, it is expected to have the effect of suppressing inflammation in the body. Furthermore, if the biocompatible material 1 is used as a scaffold when growing cells and tissues outside the body, it is expected that the cells and tissues can be grown and cultured efficiently or three-dimensionally.
[0032] Since the biocompatible component 1 is formed from fibers 11 made of biocompatible materials and water 13, when the biocompatible component 1 is placed in a living body, the biocompatible component 1 gradually disappears due to reactions within the body. As a result, the biocompatible component 1 that has completed its role does not remain in the living body, and does not interfere with cell proliferation or tissue regeneration.
[0033] Furthermore, in the biocompatible component 1, the fibers 11 are bonded to one another, for example, welded, to form an aggregate 12. Therefore, even if water 13 is contained in the fibers 11 in the aggregate 12, the strength of the entire biocompatible component 1 can be maintained. For example, the biocompatible component 1 has a compressive modulus of elasticity of 5 kPa or more, and a storage modulus higher than the loss modulus. Therefore, the biocompatible component 1 has a high enough rigidity to maintain its shape even when it is picked up with tweezers or the like.
[0034] On the other hand, the biocompatible member 1 is soft enough to be cut with scissors or a scalpel. Therefore, for example, in a medical setting, the biocompatible member 1 can be processed by holding it with tweezers, cutting it with scissors or a scalpel, or bending it to fit the shape of a wound. In this way, the biocompatible member 1 is easy to handle. In addition, since the biocompatible member 1 is transparent or semi-transparent, it is easy to position it according to the space in the tissue damage area or after tumor resection.
[0035] If the fibers 11 are not bonded to each other, the entire sheet will become weak when it is made to absorb water, and will not be able to maintain its shape. Therefore, if the water content is adjusted to a value close to that of living tissue, the sheet will become gel-like, making it difficult to handle. Even if the fibers 11 are bonded to each other, if an appropriate amount of water is not contained between the fibers 11, the flexibility of the entire sheet will be low, making it difficult to cut with scissors or a scalpel. Furthermore, if the flexibility of the biocompatible member 1 is low, there is a possibility that the surrounding cell tissue will be damaged when it is placed in a living body.
[0036] It is also possible to bond the fibers 11 together by heating or chemical cross-linking. In this case, however, there is a possibility that the biomaterial may be denatured or toxic due to heat, resulting in a decrease in biocompatibility.
[0037] <Second embodiment> Next, a second embodiment will be described. This embodiment is an example in which the moisture impregnation treatment in the first embodiment is replaced with hydrostatic pressure treatment. The method for producing a biocompatible component according to this embodiment will be described below. FIG. 4 is a diagram showing the hydrostatic pressure treatment in the method for producing a biocompatible component according to this embodiment.
[0038] First, the steps shown in FIG. 2(a) to FIG. 3(b) are carried out. 4, the assembly 12 from which the volatile liquid has been absorbed and then removed is sealed in a sealed bag 117 together with water 116. As described in the first embodiment, various forms of water can be used as the water 116, for example, physiological saline can be used. Then, the sealed bag 117 is placed in a chamber 119 connected to a pump 118. Air 120 is introduced outside the sealed bag 117 in the chamber 119.
[0039] Then, the water 116 and the aggregate 12 are pressurized by the pump 118 via the air 120 and the sealed bag 117. The pressure is higher than atmospheric pressure (1 atm), and is preferably 5 MPa to 1 GPa, more preferably 100 MPa to 1 GPa, for example, 500 MPa. This causes water to permeate between the fibers 11 and into the fibers 11 in the aggregate 12. Also, the air that was present in the voids 15 is removed from the aggregate 12. Air released from the voids 15 may accumulate in the sealed bag 117 after the hydrostatic pressure treatment. In this manner, the biocompatible component according to this embodiment is manufactured.
[0040] According to this embodiment, by carrying out hydrostatic pressure treatment as the water-containing treatment, water can be efficiently contained in the aggregate 12. In addition, the biocompatible component 1 can be sterilized by the hydrostatic pressure treatment. This also improves the biocompatibility of the biocompatible component 1. Other configurations, manufacturing methods, and effects of this embodiment are similar to those of the first embodiment.
[0041] <Third embodiment> Next, a third embodiment will be described. This embodiment is an example in which the moisture impregnation treatment in the first embodiment is replaced with a reduced pressure treatment. The method for producing a biocompatible component according to this embodiment will be described below. FIG. 5 is a diagram showing the decompression process in the method for producing a biocompatible component according to this embodiment.
[0042] First, the steps shown in FIG. 2(a) to FIG. 3(b) are carried out. Next, as shown in Fig. 5, the laminated sheet 10b is subjected to a decompression treatment. Specifically, the laminated sheet 10b is placed in a chamber 121 and immersed in water 122. In this state, the pressure inside the chamber 121 is reduced. The pressure inside the chamber 121 is set to less than 1 atmosphere. After the decompression treatment, a hydrostatic pressure treatment may be performed as described in the second embodiment.
[0043] This also makes it possible to contain water 13 between the fibers 11 of the assembly 12. Other configurations, manufacturing methods, and effects of this embodiment are similar to those of the first embodiment.
[0044] <Test Example> Next, a test example of the first embodiment will be described. In this test example, a biocompatible component 1 was actually manufactured by the manufacturing method according to the first embodiment. In this test example, collagen, which is a biomaterial, was used as the biocompatible material. Also, an ethanol solution was used as the volatile liquid.
[0045] That is, in this test example, a deposition layer 10a was formed by depositing fibers 11 by electrospinning, and a laminated sheet 10b was formed by stacking a plurality of deposition layers 10a so that the orientation directions crossed each other, and an ethanol treatment was performed in which an ethanol solution was permeated and evaporated to the extent that a few air bubbles remained, and then the sheet was immersed in physiological saline to perform a water impregnation treatment. In this way, a sheet-shaped biocompatible component 1 was produced. The properties of the biocompatible component 1 were evaluated by the following method.
[0046] (External Observation) Samples at each stage in the manufacturing process of the biocompatible component 1 were observed by a SEM (Scanning Electron Microscope).
[0047] FIG. 6(a) is an SEM photograph of the surface of a deposition layer 10a formed by electrospinning, and (b) is an SEM photograph of the surface of a laminate sheet 10b after an ethanol treatment.
[0048] As shown in Fig. 6(a), in the deposition layer 10a formed by the electrospinning method and before the ethanol treatment, many fibers 11 were extending in roughly one direction. This confirmed that the deposition layer 10a had orientation. In addition, as shown in Fig. 6(b), the treatment of permeating and volatilizing the ethanol caused some of the fibers 11 to fuse together and become integrated, making the surface smooth.
[0049] 7(a) and (b) are SEM photographs of the surface of a frozen sample of biocompatible component 1 according to this test example, in which collagen was crosslinked with glutaraldehyde and the ice was sublimated using a cooling SEM. As shown in Figs. 7(a) and (b), the surface of the biocompatible component 1 has voids 15 with a diameter of 10 µm or more at a rate of 1 void / mm 2 It was formed at a density of more than 1000m.
[0050] (Polarized FT-IR-ATR method) In a stretched polymeric material, the direction in which the long axes of the molecules extend (molecular axes) tends to be the direction in which the polymeric material (fibers) extends. Therefore, by examining the direction in which the long axes of the molecules extend on the surface of the biocompatible component 1, the direction in which the fibers 11 extend can be estimated, and therefore it can be determined whether the fibers 11 are oriented or not.
[0051] The direction in which the long axis of the molecule extends can be determined by a structure determination method that corresponds to the type of polymer material. For example, Raman spectroscopy can be used in the case of polystyrene, and polarized absorbance analysis can be used in the case of polyimide. In this test example, as an example, a case in which the polymer material is an organic compound having an amide group, such as collagen, is described. In the case of an organic compound having an amide group, for example, the direction in which the long axis of the molecule extends can be determined by using polarized FT-IR-ATR (Fourier Transform-Infrared Spectroscopy- Attenuated Total Reflectance), which is a type of infrared spectroscopy.
[0052] The analysis method using the polarized FT-IR-ATR method will be described below. Wave number: 1640cm -1 The absorption intensity of light with a wave number of 1540 cm is T1. -1Let the absorption intensity of this light be T2. Absorption intensity T1 is the absorption intensity in a direction perpendicular to the direction in which the long axis of the molecule extends. Absorption intensity T2 is the absorption intensity in the direction in which the long axis of the molecule extends. Therefore, if the absorbance ratio (T1 / T2) in a given polarization direction is small, it can be seen that there are many molecules extending in that polarization direction.
[0053] Then, for a sample obtained by freeze-drying the biocompatible material 1 after the hydration treatment, the absorbance ratio (T1 / T2) is measured while changing the angle with the polarization direction. The absorbance ratio with the maximum value is designated as R1, and the absorbance ratio with the minimum value is designated as R2. For example, the orientation of the biocompatible material 1 at which the absorbance ratio R2 is obtained is rotated by 90° from the orientation of the biocompatible material 1 at which the absorbance ratio R1 is obtained. The ratio (R1 / R2) is designated as the orientation parameter. The larger the orientation parameter (R1 / R2), the higher the degree of orientation.
[0054] In the sample obtained by freeze-drying the biocompatible material 1 after the hydration treatment, the value of the orientation parameter (R1 / R2) was about 1.10. In this manner, it was confirmed that the fibers 11 were oriented in the biocompatible material 1 after the hydration treatment.
[0055] (Differential Scanning Calorimetry) Differential scanning calorimetry (DSC) was performed on the laminate sheet 10b before the hydration treatment and on samples obtained by freeze-drying the biocompatible component 1 after the hydration treatment.
[0056] FIG. 8 is a graph showing the results of differential scanning calorimetry of the laminate sheet and biocompatible component according to this test example, with the horizontal axis representing temperature and the vertical axis representing heat flow. FIG. 9 is a table showing the differential scanning calorimetry results. For comparison, the measurement results of untreated collagen powder are also shown in Figure 9. Collagen powder has a triple helix structure, which is the original structure of collagen molecules.
[0057] As shown in Figures 8 and 9, in the laminate sheet 10b and the biocompatible component 1, a first endothermic peak P1 appeared in the temperature range of 20°C to 100°C, and a second endothermic peak P2 appeared in the temperature range of 200°C to 240°C. This is presumed to be due to an endothermic reaction that occurs when collagen molecules having a high-dimensional, i.e., three-dimensional, molecular structure are decomposed by heating. Therefore, the presence of endothermic peaks P1 and P2 suggests that the molecular structure of collagen molecules in the laminate sheet 10b and the biocompatible component 1 before heating is the original high-dimensional structure.
[0058] Furthermore, the heat quantity of the endothermic peak P1 of the biocompatible component 1 was greater than that of the laminate sheet 10b. Specifically, the endothermic peak P1 of the laminate sheet 10b was about 16 to 19 J / g, and the endothermic peak P1 of the sample 1s was about 27 J / g. This suggests that the triple helix structure of the collagen molecule was maintained.
[0059] (Compressive elastic modulus) The compressive modulus was measured for the biocompatible component 1. The thickness of the biocompatible component 1 was set to four levels, 0.3 mm, 0.9 mm, 1.3 mm, and 1.9 mm, and three samples were prepared for each level and measured.
[0060] FIG. 10 is a table showing the measurement results of the compressive elastic modulus of the biocompatible component according to this test example. As shown in FIG. 10, the compressive elastic modulus was 7.5 to 74.8 kPa in the measurement results for the 12 samples.
[0061] (Dynamic viscoelasticity measurement) The viscoelasticity-frequency curve of the biocompatible member 1 was measured by dynamic viscoelasticity. The thickness of the biocompatible member 1 was set to four levels, 0.3 mm, 0.9 mm, 1.3 mm, and 1.9 mm, and the temperature was room temperature. A sinusoidal wave force was applied to the biocompatible member 1, and the elastic modulus was measured. The frequency of the sinusoidal wave force was set to 1 to 100 Hz.
[0062] Figure 11(a) is a graph showing the storage modulus-frequency curve of the biocompatible material of this test example, with frequency on the horizontal axis and storage modulus on the vertical axis, and (b) is a graph showing the loss modulus-frequency curve of the biocompatible material of this test example, with frequency on the horizontal axis and loss modulus on the vertical axis.
[0063] 11(a) and (b), the storage modulus was higher than the loss modulus over the entire measured frequency range, which indicates that the biocompatible material 1 has strong elastic properties.
[0064] (Structural changes in vivo) When biocompatible component 1 is placed inside a living body, the structural changes of biocompatible component 1 due to stress from the living body were simulated. Specifically, collagen in biocompatible component 1 was cross-linked with glutaraldehyde, and the biocompatible component was cut with a razor while still unfrozen. The shear force from the razor simulates the stress that biocompatible component 1 would experience inside a living body. Next, the ice was sublimated using a cooling SEM, and the surface of the cut surface was observed using an SEM.
[0065] FIG. 12 is a surface SEM photograph showing a cut surface of the biocompatible component 1 after the above-mentioned treatment. 12, gaps 16 between the layers 10 were observed on the cut surface of the biocompatible component 1. This is thought to be because the layers 10 were misaligned due to the shear force applied to the biocompatible component 1 in the thickness direction (Z direction) when it was cut with a razor. On the other hand, no gaps 16 between the layers 10 were observed on the cross section formed by cutting with a knife in a frozen and high vacuum state.
[0066] Next, the sheet-like biocompatible material 1 was punched out into test pieces with a diameter of 5 mm. The test pieces were divided into four groups and placed in PS culture dishes and stored under the following four conditions. The changes in the test pieces before and after storage were observed.
[0067] Condition 1: The test specimen was immersed in saline and stored at 5°C. Condition 2: The test specimen was immersed in saline and stored at 37°C. Condition 3: The test specimen was immersed in FBS (Fetal bovine serum) and stored at 5°C. Condition 4: The test specimen was immersed in FBS and stored at 37°C.
[0068] As a result, peeling between layers 10 was observed in a high-temperature environment of 37° C. regardless of the type of immersion liquid. On the other hand, in a low-temperature environment of 5° C., no peeling between layers 10 was observed.
[0069] These results indicate that in the biocompatible component 1, the bonding strength between the layers 10 is weaker than the bonding strength between the fibers 11 within the layers 10. It was also estimated that when stress or heat is applied to the biocompatible component 1 in a living body, gaps 16 are formed between the layers 10. As described above, when cells enter the gaps 16, the fusion between the biocompatible component 1 and the living body is improved.
[0070] (Subcutaneous implantation in rats) Biocompatible material 1 was implanted subcutaneously into a rat, and the condition was then visually observed. As a result, 1-2 days after implantation, biocompatible material 1 became gel-like and lost its elasticity. 7 days after implantation, biocompatible material 1 had disappeared. During this time, no rejection reaction such as inflammation was observed.
[0071] According to the embodiment described above, a biocompatible material that is highly biocompatible and easy to handle, and a method for producing the same can be realized.
[0072] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These new embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0073] 1: Biocompatible materials 10: layer 10a: Sedimentary layer 10b: Laminated sheet 11: Fiber 12: Accumulation 13:Water 15: Void 16: Gap 101: Manufacturing equipment 102: Nozzle 103: Laura 104: Power supply 110: Raw material liquid 112: Base material 113: Wes 115: Container 116:Water 117: Airtight bag 118: Pump 119: Chamber 120: Air 121: Chamber 122:Water P1, P2: endothermic peak
Claims
1. forming a laminate sheet by depositing fibers including a biocompatible material; Permeating the laminated sheet with a volatile liquid; volatilizing the liquid that has permeated the laminated sheet; a step of subjecting the laminated sheet from which the liquid has been volatilized to a moisture impregnation treatment; A method for manufacturing a biocompatible component comprising the steps of:
2. The method for producing a biocompatible component according to claim 1 , wherein the step of forming a laminate sheet includes a step of forming the fibers by an electrospinning method.
3. The method for producing a biocompatible component according to claim 1 or 2, wherein in the step of forming the laminated sheet, the fibers are pulled in one direction to align the extending direction of the deposited fibers.
4. The method for producing a biocompatible component according to any one of claims 1 to 3, wherein in the step of permeating the volatile liquid, a space that is not filled with the volatile liquid is formed.
5. The method for producing a biocompatible component according to any one of claims 1 to 4, wherein the volatile liquid is an aqueous ethanol solution.
6. The method for producing a biocompatible component according to any one of claims 1 to 5, wherein the biocompatible material is collagen.
Citation Information
Patent Citations
Suturable tissue regeneration induction type adhesion preventive membrane
JP2000210376A
Collagen sponge manufacturing method, artificial skin manufacturing method, artificial skin and cell tissue culture substrate
JP2005000314A
Collagen film and method for producing the same
JP2012024250A
Collagen molded body and method for producing the same
JP2014218453A
Formed sheet and hemostatic material
JP2016073641A