Soft magnetic alloy plate, method for manufacturing soft magnetic alloy plate, iron core and rotating electric machine each using soft magnetic alloy plate
A soft magnetic iron alloy plate with controlled Co and N phases, manufactured through sintering and nitriding, addresses the challenge of high material cost and iron loss in existing iron cores, enhancing magnetic properties and torque output.
Patent Information
- Application Number
- JP2023049839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing iron cores for rotating electric machines and transformers face challenges in achieving high magnetic flux density and saturation magnetization while minimizing material cost and iron loss, with materials like permendur being costly and Fe-Si electrical steel sheets having lower magnetic properties.
A soft magnetic iron alloy plate with a specific composition and microstructure, including phases with varying Co and N content, is produced through a controlled manufacturing process involving sintering, nitriding, and sub-zero treatment to enhance magnetic properties and reduce material cost.
The alloy plate achieves higher magnetic flux density and saturation magnetization with reduced iron loss, enabling lower-cost production of iron cores with improved torque and output performance.
Smart Images

Figure 2024139054000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a technology for soft magnetic materials, and in particular to a soft magnetic alloy plate having higher magnetic properties than electromagnetic pure iron plate, a manufacturing method for said soft magnetic alloy plate, and an iron core and a rotating electric machine using said soft magnetic alloy plate. [Background technology]
[0002] Laminated cores made by laminating multiple soft magnetic materials such as pure iron sheets or steel sheets (e.g., 0.01 to 3 mm thick) are widely used as cores for rotating electrical machines and transformers. In recent years, there has been a strong demand for miniaturization and higher output in these rotating electrical machines and transformers, and improving the magnetic properties of the cores is one of the urgent issues.
[0003] For iron cores, it is important that the conversion efficiency between electric energy and magnetic energy is high, and high magnetic flux density and high magnetization are important magnetic properties. To increase the magnetic flux density / magnetization of an iron core, it is desirable for the material to have a high saturation magnetic flux density Bs / saturation magnetization Ms. Known examples of iron-based materials with a high Bs / Ms include Fe-Co alloy materials and Fe-N martensitic materials.
[0004] Among Fe-Co alloy materials, permendur (49Fe-49Co-2V mass% = 50Fe-48Co-2V atomic%) has the highest Ms (239 emu / g) among the currently commercially available soft magnetic bulk materials. However, the material cost of Co, although it varies depending on the market, is 100 to 200 times higher than that of Fe, so permendur has the disadvantage of high material cost. Permendur also has some difficulty in processability, and the process cost tends to be high. Reducing the Co content reduces the material cost and improves processability, but the Ms, which is its greatest feature, decreases.
[0005] On the other hand, for Fe-N martensitic materials, for example, Patent Document 1 (JP 2020-132894) discloses a soft magnetic material in the form of a plate or foil having a high saturation magnetic flux density, which contains iron, carbon, and nitrogen, and includes martensite containing carbon and nitrogen and γ-Fe, in which a phase containing nitrogen is formed in the γ-Fe. According to Patent Document 1, a soft magnetic material having a saturation magnetic flux density exceeding that of pure iron and thermal stability can be manufactured at low cost, and the characteristics of the magnetic circuit of an electric motor or the like can be improved using this, thereby realizing miniaturization and high torque of the electric motor or the like. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2020-132894 Summary of the Invention [Problem to be solved by the invention]
[0007] In order to increase the electric / magnetic energy conversion efficiency in an iron core, in addition to high Bs / high Ms, it is also important to suppress iron loss Pi. Pi is the sum of hysteresis loss and eddy current loss, and to reduce hysteresis loss, it is desirable to have a small coercive force Hc. The magnetic properties of commercially available electromagnetic pure iron sheets are said to be Bs ≒ 2.1 T, Ms ≒ 215 emu / g, and Hc ≒ 80 A / m. Iron cores using electromagnetic pure iron sheets have the advantages of high Bs, high Ms, and low material costs, but have the disadvantage that Pi tends to become large due to a relatively high Hc.
[0008] The Fe-Si-based electromagnetic steel sheet, which is currently widely used, has the advantage of having a smaller Pi than the electromagnetic pure iron sheet, but has the disadvantage that the Bs / Ms of the Fe-Si-based electromagnetic steel sheet is smaller than that of the electromagnetic pure iron sheet. Also, the soft magnetic material of Patent Document 1 has the advantage of having a higher Bs than the electromagnetic pure iron sheet, but has the disadvantage that Hc is easily increased.
[0009] In recent years, there has been a strong demand for high torque / high output designs in rotating electrical machines and transformers, and there is a strong demand for improved Bs / Ms of the core. In other words, improving the Bs / Ms of the core is given priority, and if the improvement in Bs / Ms is large, a certain degree of increase in Pi tends to be tolerated.
[0010] On the other hand, reducing the cost of the iron core is naturally one of the important issues, and there is a demand for a soft magnetic material that can be manufactured stably and at a lower cost than permendur while still satisfying the expected and required magnetic properties.
[0011] Therefore, an object of the present invention is to provide a soft magnetic iron alloy plate that has higher magnetic properties than electromagnetic pure iron plate and can be manufactured at a lower cost than permendur, a method for manufacturing the soft magnetic alloy plate, and an iron core and a rotating electric machine using the soft magnetic iron alloy plate. [Means for solving the problem]
[0012] (I) One aspect of the present invention is a soft magnetic iron alloy plate, The average composition includes 5 atomic % or more and 25 atomic % or less of cobalt (Co), 0 atomic % or more and 1 atomic % or less of vanadium (V), 0.2 atomic % or more and 5 atomic % or less of nitrogen (N), 0 atomic % or more and 5 atomic % or less of carbon (C), and the remainder is iron (Fe) and impurities; The first phase and the second phase have different contents of Co and N, The first phase has a relatively higher Co content than the second phase, The second phase has a relatively higher N content than the first phase, The present invention provides a soft magnetic iron alloy plate, characterized in that the second phase has a region in which a plurality of crystal grains are connected in the thickness direction of the soft magnetic iron alloy plate, and the region is at least half the thickness of the soft magnetic iron alloy plate.
[0013] In the present invention, the following improvements and modifications can be freely combined in the above-mentioned soft magnetic iron alloy plate (I). (i) the first phase contains more than 5 atomic % and not more than 40 atomic % Co and 0 atomic % or more and less than 0.2 atomic % N, and the second phase contains 0 atomic % or more and 5 atomic % or less Co and 0.5 atomic % or more and 10 atomic % or less N. (ii) the first phase and the second phase each have an average particle size of 45 μm or less; (iii) the volume fraction of the first phase is 50 volume % or more and 95 volume % or less, and the volume fraction of the second phase is 50 volume % or less and 5 volume % or more. (iv) The saturation magnetization is 222 emu / g or more.
[0014] In the present invention, the average grain size in the soft magnetic iron alloy plate is the average diameter of the equivalent area circle of the crystal grains observed by microstructural observation (e.g., scanning electron microscope observation). The average grain size of the powder is the volume-based average grain size (D50) measured by a laser diffraction / scattering type particle size distribution measuring device or the like.
[0015] (II) Another aspect of the present invention is a method for producing the above-mentioned soft magnetic iron alloy sheet, a starting material preparation step of preparing a starting material by mixing a first powder made of an iron-cobalt alloy containing more than 5 atomic % and 40 atomic % or less of cobalt and 0 atomic % or more and 1.2 atomic % or less of vanadium with a second powder made of an iron-based metal containing 0 atomic % or more and 5 atomic % or less of cobalt in a predetermined ratio; a molding / sintering step of forming a sintered body by molding and sintering the starting material; a martensite phase generating step of subjecting the sintered body to a heat treatment for infiltrating and diffusing nitrogen atoms, and then quenching the sintered body to generate a martensite phase; A subzero treatment step of further cooling the sintered body quenched in the martensite phase generation step to 0°C or lower. The present invention provides a method for producing a soft magnetic iron alloy plate, comprising the steps of:
[0016] In the present invention, the following improvements and modifications can be freely combined in the above-mentioned manufacturing method (II) of a soft magnetic iron alloy sheet. (v) The predetermined ratio in the starting material preparing step is such that the second powder is 5% by mass or more and 50% by mass or less. (vi) The first powder and the second powder in the starting material preparation step each have an average particle size of 1 μm or more and 45 μm or less, and the ratio of the average particle size of the first powder to the average particle size of the second powder is 1 or more and 10 or less. (vii) The heat treatment in the martensite phase formation step includes a process of adjusting the atmosphere to one containing ammonia gas after the temperature reaches 500°C or higher, and then increasing the temperature to a temperature range for the formation of austenite phase, and alternately switching between an atmosphere containing ammonia gas and an atmosphere not containing ammonia gas.
[0017] (III) Another aspect of the present invention is an iron core made of a laminate of soft magnetic iron alloy plates, The present invention provides an iron core, wherein the soft magnetic iron alloy plate is the soft magnetic iron alloy plate according to the present invention.
[0018] (IV) Yet another aspect of the present invention is a rotating electric machine having an iron core, The present invention also provides a rotating electric machine, wherein the iron core is the iron core according to the present invention. Effect of the Invention
[0019] According to the present invention, it is possible to provide a soft magnetic iron alloy plate that has higher magnetic properties than electromagnetic pure iron plate and can be manufactured at a lower cost than permendur, a method for manufacturing the soft magnetic alloy plate, and an iron core and a rotating electric machine that use the soft magnetic iron alloy plate. [Brief description of the drawings]
[0020] [Figure 1] 1 is a process diagram showing an example of a method for producing a soft magnetic iron alloy plate according to the present invention. [Figure 2A] FIG. 2 is a schematic perspective view showing an example of a stator of a rotating electric machine. [Figure 2B] FIG. 2 is an enlarged schematic cross-sectional view of a slot region of the stator. [Diagram 3]1 is an example of a component plane analysis in cross-sectional observation in Example 1, showing (a) the result of Fe component mapping and (b) the result of Co component mapping. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] [Basic concept of the present invention] In order to achieve the above-mentioned object, the inventors considered reducing the Co content compared to permendur to reduce material costs, and compensating for the decrease in magnetic properties (Bs and / or Ms) due to the decrease in Co content by generating an Fe-N martensite phase. They also considered that by generating an Fe-C martensite phase, it would be possible to suppress the increase in Pi without decreasing Bs / Ms.
[0022] However, it is said that it is difficult for N atoms and C atoms to penetrate and diffuse into Fe-Co alloy materials, making it difficult to form Fe-N martensite phases or Fe-C martensite phases. In other words, it is not easy to simply penetrate and diffuse N atoms and C atoms into Fe-Co alloy materials.
[0023] On the other hand, if an element that promotes the penetration and diffusion of N and C atoms is simply added to an Fe-Co alloy material in order to generate an Fe-N martensite phase, it becomes easier to generate nonmagnetic nonmetallic particles, which act as pinning points that prevent domain wall movement during magnetization reversal. The generation of nonmagnetic particles leads to a decrease in Bs and / or Ms, and another problem occurs in that the pinning points of the domain walls lead to an increase in Pi.
[0024] Therefore, the inventors of the present invention have conducted extensive research into a method for effectively penetrating and diffusing N and C atoms into the interior of a soft magnetic iron alloy sheet while maintaining and inheriting the magnetic properties of the Fe-Co alloy material itself. As a result, they have devised a method of mixing and sintering a first phase powder made of an Fe-Co alloy with excellent magnetic properties with a second phase powder made of an Fe-based metal in which N and C atoms can penetrate and diffuse relatively easily, and then performing a nitriding heat treatment or a nitriding and carburizing heat treatment. The second phase serves as a penetration and diffusion path for N and C atoms, allowing N and C atoms to penetrate and diffuse into the interior of the soft magnetic iron alloy sheet, effectively generating an Fe-N martensite phase, or an Fe-N and Fe-C martensite phase. The present invention has been completed based on this knowledge.
[0025] Numerous experiments by the inventors have revealed that a clear improvement in characteristics / significant difference can be achieved if a Bs improvement of 0.03 T or more or an Ms improvement of 3 emu / g or more is achieved compared to a comparative soft magnetic material. For this reason, the soft magnetic iron alloy sheet of the present invention must exhibit at least a Bs of 2.17 T or more or an Ms of 218 emu / g or more. From the perspective of recent demands for higher torque / higher output in rotating electrical machines, a Bs of 2.21 T or more or an Ms of 222 emu / g or more is more desirable.
[0026] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the embodiments described herein, and can be appropriately combined with known techniques or improved based on known techniques without departing from the technical concept of the invention.
[0027] [Soft magnetic iron alloy plate] Fig. 1 is a process diagram showing an example of a method for producing a soft magnetic iron alloy sheet according to the present invention. As shown in Fig. 1, the method for producing a soft magnetic iron alloy sheet according to the present invention generally includes a starting material preparation step S1, a compacting and sintering step S2, a martensite phase generating step S3, and a sub-zero treatment step S4. In the present invention, in order to obtain a soft magnetic iron alloy sheet that achieves the objective, the structure of the sintered body obtained in the compacting and sintering step S2 is controlled, and the composition of the starting material prepared in the starting material preparation step S1 is controlled in order to control the structure of the sintered body.
[0028] Each step will now be described in more detail.
[0029] The starting material preparation step S1 is a step of preparing a starting material by mixing in a predetermined ratio a first powder made of an Fe-Co alloy containing more than 5 atomic % and 40 atomic % or less of Co and 0 atomic % or more and 1.2 atomic % or less of V, and a second powder made of an Fe-based metal containing 0 atomic % or more and 5 atomic % or less of Co. The V component is a component that contributes to improving moldability in the subsequent molding and sintering step S2, but is not an essential component (i.e., it may or may not be contained).
[0030] The first powder and / or the second powder may contain 0 atomic % or more and 5 atomic % or less of the C component (in other words, the C component is not an essential component either). Note that, after the subsequent compacting and sintering step S2, the C component can be added by performing a carburizing heat treatment to penetrate and diffuse the C component as necessary.
[0031] It is preferable to control the mixing ratio of the first powder and the second powder so that the average composition of the entire starting material contains 5 atomic % or more and 25 atomic % or less of Co, 0 atomic % or more and 1 atomic % or less of V, and 0 atomic % or more and 5 atomic % or less of C, with the remainder being Fe and impurities.
[0032] In the subsequent compacting and sintering step S2, it is preferable to control the length of the region (particularly the length in the thickness direction of the sintered body) to be at least half the thickness of the sintered body, so that in the subsequent compacting and sintering step S2, the second powder is preferably mixed in a range of 5% to 50% by mass (95% to 50% by mass of the first powder), and more preferably in a range of 10% to 50% by mass (90% to 50% by mass of the first powder).
[0033] There is no particular limitation on the average particle size of the first powder and the second powder, but from the viewpoint of shape controllability of the sintered body in the subsequent molding and sintering step S2, it is preferable that each of them is 1 μm or more and 45 μm or less. There is no particular limitation on the ratio of the average particle size of the first powder to the average particle size of the second powder, but it is preferable to control it in the range of, for example, 1 to 10.
[0034] When two types of powders with different average particle sizes are mixed and molded, the powder with the larger average particle size basically tends to form the skeleton of the molded body, and the powder with the smaller average particle size tends to be arranged so as to fill the gaps in the skeleton. This tendency becomes stronger as the ratio of average particle sizes increases (for example, when it becomes 5 or more). In other words, when the ratio of average particle sizes is large, the powder with the smaller average particle size tends to become islands in a sea-island structure.
[0035] As described above, it is preferable to control the sintered body obtained in the subsequent molding and sintering step S2 so that a region is formed in which multiple crystal grains based on the second powder are connected to each other, and the length of the region (length in the thickness direction of the sintered body) is at least half the thickness of the sintered body. There are several types of starting material configurations for obtaining this structure. For example, "the ratio of the average grain size of the two types of powders is made small (e.g., 2 or less)", "the average grain size of the second powder is made larger than the average grain size of the first powder, and the mixing ratio of the second powder is set low (e.g., 20 mass% or less)", "the average grain size of the second powder is made smaller than the average grain size of the first powder, and the mixing ratio of the second powder is set high (e.g., 30 mass% or more)", etc.
[0036] The molding / sintering step S2 is a step of forming a sintered body by molding and sintering using the starting material prepared in the previous step S1. In the step S2 of the present invention, the order of molding and sintering does not matter. That is, sintering may be performed after molding, or main molding may be performed after provisional molding and sintering, or molding and sintering may be performed simultaneously.
[0037] The molding method and sintering method are not particularly limited as long as a dense sintered body can be obtained, and conventional techniques in powder metallurgy methods for metal materials can be used as appropriate. For example, cold isostatic pressing (CIP), hot isostatic pressing (HIP), hot pressing (HP), gas pressure sintering, millimeter wave sintering, microwave sintering, electric field assisted sintering, flash sintering, spark plasma sintering (SPS), etc. can be suitably used. For a dense sintered body, when a cross-sectional observation is performed, the porosity is preferably 7 area % or less, more preferably 5 area % or less, and even more preferably 3 area % or less. As an example, when using spark plasma sintering, it is preferable to sinter at a heating temperature of 1100°C or less and a maximum surface pressure of 50 MPa.
[0038] The sintered body obtained by this process S2 has the structural characteristics of having a region of crystal grains based on the first powder and a region in which multiple crystal grains based on the second powder are connected to each other, and the length of the region based on the second powder (the length in the thickness direction of the sintered body) is at least half the thickness of the sintered body.
[0039] The martensite phase generation step S3 is a step in which the sintered body formed in the previous step S2 is subjected to a nitriding heat treatment to cause N atoms to penetrate and diffuse, and then quenched to generate a martensite phase. In the nitriding heat treatment, N atoms preferentially penetrate and diffuse into the crystal grains that are the basis of the second powder. After nitriding to the desired N content, the martensite phase is generated by quenching to cool the body to less than 100°C.
[0040] The nitriding heat treatment is carried out at a temperature of 500°C or higher (for example, in the austenite phase (γ phase) formation temperature range) in a specific ammonia (NH3) gas atmosphere, where N atoms penetrate and diffuse from the surface of the sintered body (particularly from the surface of the region where multiple crystal grains based on the second powder are connected to each other). As the NH3 gas atmosphere, in addition to NH3 gas alone, a mixed gas of NH3 gas and N2 gas, a mixed gas of NH3 gas and Ar gas, or a mixed gas of NH3 gas and H2 gas can be suitably used.
[0041] It is preferable to introduce NH3 gas after the temperature reaches 500°C or higher. This is because if NH3 gas is actively introduced in the stable temperature range of the ferrite phase (α phase), the desired tetragonal structure of Fe-N phase (Fe8N phase (α' phase) and / or Fe 16 This is because undesirable Fe-N phases (e.g., Fe4N phase (γ' phase) and Fe3N phase (ε phase)) are more likely to form than undesirable Fe-N phases (e.g., Fe4N phase (γ' phase) and Fe3N phase (ε phase)).
[0042] The N content in the sintered body (particularly in the region where multiple crystal grains based on the second powder are connected to each other) can be controlled by controlling the heat treatment temperature, the NH3 gas partial pressure, and / or the NH3 gas supply time. The N content distribution in the thickness direction of the sintered body can be controlled by alternately switching between an atmosphere containing NH3 gas and an atmosphere not containing NH3 gas.
[0043] By rapid cooling after nitriding, most of the austenite phase (γ phase) can be transformed into martensite, but some γ phase may remain (residual γ phase). Since the γ phase is non-magnetic, it is preferable to keep the volume fraction of the residual γ phase below 5% from the viewpoint of magnetic properties.
[0044] Although not an essential step, when performing carburizing heat treatment to add C component, carburizing heat treatment may be performed following the above nitriding heat treatment (for example, after nitriding heat treatment and before quenching). There is no particular limitation on the method of carburizing heat treatment, and conventional methods can be used as appropriate. For example, following nitriding heat treatment, the atmospheric gas can be changed to acetylene (C2H2) gas or carbon monoxide (CO) gas.
[0045] The carburizing heat treatment may be performed simultaneously with the nitriding heat treatment. In this case, after the temperature reaches 500°C or higher, C2H2 gas or CO gas is introduced in addition to NH3 gas, and the temperature is raised to the γ-phase formation temperature range in the gas environment, so that N atoms and C atoms penetrate and diffuse from the surface of the sintered body (especially from the surface of the region where multiple crystal grains based on the second powder are connected to each other).
[0046] The C content can be controlled by controlling the heat treatment temperature, gas partial pressure and / or gas supply time, similar to the N content. The C content distribution in the thickness direction of the sintered body can be controlled by alternately switching between an atmosphere containing C2H2 or CO gas and an atmosphere not containing the gas.
[0047] Following the martensite phase generation step S3, it is preferable to carry out a sub-zero treatment step S4 in order to transform the residual γ phase into a martensite structure. The sub-zero treatment is a treatment for cooling to below 0°C, and preferably uses normal sub-zero treatment using dry ice or ultra-sub-zero treatment using liquid nitrogen.
[0048] The N content of the Fe-N martensite phase (referred to as the second phase in this specification) in step S3 is preferably 0.5 atomic % or more and 10 atomic % or less. By setting the N content to 0.5 atomic % or more, a significant amount of the Fe-N martensite phase is generated, which contributes to improving Bs / Ms. By setting the N content to 10 atomic % or less, it is possible to suppress the generation of the undesired Fe-N phase. The lower limit of the N content of the second phase is more preferably 1 atomic % or more, and even more preferably 1.5 atomic % or more. Moreover, the upper limit of the N content is more preferably 8 atomic % or less, and even more preferably 6 atomic % or less. The region of the crystal grains based on the first powder becomes the first phase in this specification.
[0049] The average composition of the entire soft magnetic iron alloy sheet includes 5 atomic % or more and 25 atomic % or less of Co, 0 atomic % or more and 1 atomic % or less of V, 0.2 atomic % or more and 5 atomic % or less of N, and 0 atomic % or more and 5 atomic % or less of C, with the remainder being Fe and impurities.
[0050] Although not an essential step, a tempering step S5 at 100°C or higher and 210°C or lower may be further carried out in order to impart toughness to the sintered body (soft magnetic iron alloy plate) that has undergone the sub-zero treatment step S4 (not shown in FIG. 1).
[0051] By using the above process, it is possible to obtain a soft magnetic iron alloy sheet in which the Co content is reduced compared to permendur, thereby reducing material costs, while the loss of magnetic properties due to the reduced Co content is compensated for by the formation of an Fe-N martensite phase.
[0052] [Iron cores and rotating electrical machines] Fig. 2A is a schematic perspective view showing an example of a stator of a rotating electric machine, and Fig. 2B is an enlarged schematic cross-sectional view of a slot region of the stator. Note that the cross-sectional view means a cross section perpendicular to the rotation axis direction (a cross section whose normal line is parallel to the axial direction). In the rotating electric machine, a rotor (not shown) is disposed radially inside the stator of Figs. 2A and 2B.
[0053] 2A and 2B, the stator 20 has stator coils 21 wound in multiple stator slots 11 formed on the inner periphery of the laminated core 10. The stator slots 11 are spaces that are arranged at a predetermined circumferential pitch around the circumferential direction of the laminated core 10 and penetrate the laminated core 10 in the axial direction, with slits 12 opening in the innermost periphery and extending in the axial direction. The areas separating adjacent stator slots 11 are referred to as teeth 13 of the laminated core 10, and the parts of the inner periphery tip areas of the teeth 13 that define the slits 12 are referred to as tooth claw portions 14.
[0054] The stator coil 21 is usually composed of a plurality of segment conductors 22. For example, in Fig. 2A and Fig. 2B, the stator coil 21 is composed of three segment conductors 22 corresponding to the U-phase, V-phase, and W-phase of a three-phase AC. In order to prevent partial discharge between the segment conductors 22 and the laminated core 10 and partial discharge between the phases (U-phase, V-phase, W-phase), the outer periphery of each segment conductor 22 is usually covered with an electrical insulating material 23 (e.g., insulating paper, enamel coating).
[0055] The rotating electric machine according to the present invention is a rotating electric machine that uses the laminated core 10 according to the present invention. The laminated core 10 according to the present invention has a higher Bs / higher Ms than conventional laminated cores made of pure electromagnetic iron sheets or electromagnetic steel sheets, leading to higher torque / higher output of the rotating electric machine. In addition, the laminated core 10 according to the present invention can be manufactured at a lower cost than laminated cores made of permendur sheets, thereby preventing excessive cost increases in the rotating electric machine. EXAMPLES
[0056] The present invention will be explained in more detail below with reference to various experiments, however, the present invention is not limited to the configurations and structures described in these experiments.
[0057] [Experiment 1] (Preparation of starting materials 1 to 3 and reference material 1 by starting material preparation step) First, we prepared Fe-30 atomic % Co powder (raw material A) with an average particle size of approximately 30 μm, Fe-25 atomic % Co powder (raw material B) with an average particle size of approximately 30 μm, Fe-20 atomic % Co powder (raw material C) with an average particle size of approximately 30 μm, Fe-5 atomic % Co powder (raw material D) with an average particle size of approximately 30 μm, pure Fe powder (raw material E) with an average particle size of approximately 30 μm, and pure Fe powder (raw material F) with an average particle size of approximately 4 μm.
[0058] Starting material 1 was prepared by mixing raw material A as the first powder and raw material F as the second powder so that the ratio of raw material A to raw material F was 67% by mass and 33% by mass. Starting material 2 was prepared by mixing raw material A as the first powder and raw material E as the second powder so that the ratio of raw material A to raw material E was 67% by mass and 33% by mass. Starting material 3 was prepared by mixing raw material B as the first powder and raw material D as the second powder so that the ratio of raw material B to raw material D was 67% by mass and 33% by mass.
[0059] Starting materials 1 to 3 have an average Co content of about 20 atomic % throughout the starting materials, which means that the material cost can be significantly reduced compared to commercially available permendur.
[0060] In contrast, Reference Material 1 was prepared using only Raw Material C.
[0061] [Experiment 2] (Formation of inventive sintered bodies 1 to 3 and reference sintered body 1 by compacting and sintering process) Appropriate amounts were sampled from the starting materials 1-3 and reference material 1 prepared in experiment 1, and the invention sintered bodies 1-3 and reference sintered body 1 (each 20 mm in diameter × 0.1 mm in thickness) were formed using the spark plasma sintering (SPS) method. The sintering conditions were vacuum: 10 Pa, sintering temperature: 1000°C, and holding time: 5 minutes. Multiple pieces of each sintered body sample were produced.
[0062] [Experiment 3] (Preparation of Examples 1 to 3 and Reference Example 1 by Martensite Phase Formation Step and Subzero Treatment Step) Test pieces (10 mm×9.5 mm×0.1 mm) were cut out from each of the samples of the inventive sintered bodies 1 to 3 and the reference sintered body 1 formed in Experiment 2, and a martensite phase generation process was carried out.
[0063] The nitriding heat treatment was performed in a N2 gas atmosphere (0.8×10 5 After heating to 500°C under a pressure of 1×10 Pa, 5 The temperature was increased to 1000°C and then the NH3 gas atmosphere (0.5×10 Pa) was replaced with NH3 gas atmosphere (0.5×10 5 Pa) and N2 gas atmosphere (0.4×10 5 The method was to alternate between the nitrogen immersion and the pressure (MPa) to control the amount of N atoms penetrating (N content) and the distribution of N content in the thickness direction of the sintered body. After the desired amount of nitrogen immersion was completed, the material was oil quenched (60°C) to cause martensitic transformation.
[0064] Immediately after the oil quenching, an ultra-subzero treatment was carried out to transform the residual γ phase into martensite. In this manner, samples of Examples 1 to 3 and Reference Example 1, which are soft magnetic iron alloy sheets, were produced.
[0065] [Experiment 4] (Property Investigation of Examples 1 to 3 and Reference Example 1) The surface of each sample was subjected to wide-angle X-ray diffraction measurement (WAXD) using Cu-Kα radiation with an X-ray diffractometer (Rigaku Corporation, Rint-Ultima III) to identify the crystal phase.
[0066] As a result, in Examples 1 to 3, the α phase (ferrite phase) was the main phase, and the generation of α' phase and / or α" phase (Fe-N phase with a tetragonal structure) was confirmed, while the γ phase (austenite phase) and γ' phase (FeN phase) were not confirmed. On the other hand, in Reference Example 1, only the α phase was confirmed. The results of Reference Example 1 mean that the α' phase and / or α" phase were not generated at a level / amount that could be detected by WAXD measurement.
[0067] The cross section of each of the obtained samples was subjected to microstructural observation using an electron probe microanalyzer (EPMA, manufactured by JEOL Ltd., JXA-8530F) to investigate the porosity and perform a component analysis.
[0068] In the investigation of the porosity, the area ratio of pores was found by performing image analysis on microstructure photographs. It was confirmed that in all of Examples 1 to 3 and Reference Example 1, the porosity was 3 area % or less.
[0069] 3 is an example of a component plane analysis in a cross-sectional observation of Example 1, showing (a) the Fe component mapping result and (b) the Co component mapping result. Example 1 is a sample obtained by mixing and sintering raw material A (Fe-30 atomic % Co powder, average particle size about 30 μm) and raw material F (pure Fe powder, average particle size about 4 μm).
[0070] The Fe component is distributed uniformly across the entire observation field (see Fig. 3(a)). On the other hand, the Co component is clearly unevenly distributed (see Fig. 3(b)). From these results, it can be seen that raw material A forms the skeleton, and raw material B fills in the gaps in the skeleton and connects them in a network-like manner.
[0071] Quantitative analysis was performed by spot measuring the N concentration at 50 points each in the region based on raw material A and the region based on raw material B. As a result, the N concentration measured in the region based on raw material B was 1.2 to 1.5 atomic %, while the N concentration measured in the region based on raw material A was 0 to 0.1 atomic %.
[0072] These findings confirm that the region based on raw material B (Fe-based metal region) acts as a pathway for the penetration and diffusion of N atoms, generating an Fe-N martensite phase and constituting a second phase region, and that in the region based on raw material A (Fe-Co alloy region), it is difficult for N atoms to penetrate and diffuse, making it difficult to generate an Fe-N martensite phase.
[0073] In addition, although not shown in the figure, the results of observation of element distribution using EPMA confirmed that the soft magnetic iron alloy plate had a region in which multiple crystal grains of the second phase were connected in the thickness direction, and that this region was more than half the thickness of the soft magnetic iron alloy plate.
[0074] Furthermore, although not shown in the figures, it was confirmed that the same results as in Example 1 were obtained in Examples 2 and 3. It was confirmed that in Reference Example 1, the entire sample was in the region of an Fe-Co based alloy, and it was difficult for N atoms to penetrate and diffuse, making it difficult to form an Fe-N based martensite phase.
[0075] The magnetic properties of each sample were investigated using a vibrating sample magnetometer (Riken Denshi Co., Ltd., BHV-525H). The magnetization (unit: emu) of the sample was measured under conditions of a magnetic field of 1.6 MA / m and a temperature of 20°C, and the saturation magnetization Ms (unit: emu / g) was calculated from the sample mass. In addition, the iron loss Pi of the sample was measured under conditions of a magnetic flux density of 1.0 T, 400 Hz, and a temperature of 20°C using a BH loop analyzer (IFG Co., Ltd., IF-BH550) and the H coil method (compliant with JIS C 2556:2015) using a vertical yoke single sheet tester. -1.0 / 400 The results are shown in Table 1.
[0076] [Table 1]
[0077] As shown in Table 1, in Examples 1 to 3, the saturation magnetization Ms was confirmed to be improved by 5 to 7% compared to Reference Example 1 having the same Co content as the average composition. -1.0 / 400 = 25 W / kg is a sufficiently low iron loss comparable to the iron loss of electromagnetic steel sheets.
[0078] The above-mentioned embodiments and experiments are described to aid in understanding of the present invention, and the present invention is not limited to the specific configurations described. For example, it is possible to replace a part of the configuration of the embodiments with a configuration according to the technical common sense of a person skilled in the art, and it is also possible to add a configuration according to the technical common sense of a person skilled in the art to the configuration of the embodiments. In other words, it is possible to delete, replace, or add a part of the configuration of the embodiments or experiments in this specification without departing from the technical idea of the invention. [Explanation of symbols]
[0079] 10... laminated core, 11... stator slot, 12... slit, 13... teeth, 14... teeth claw portion, 20... stator, 21... stator coil, 22... segment conductor, 23... electrical insulation material.
Claims
1. A soft magnetic iron alloy plate, The average composition includes 5 atomic % or more and 25 atomic % or less of cobalt, 0 atomic % or more and 1 atomic % or less of vanadium, 0.2 atomic % or more and 5 atomic % or less of nitrogen, 0 atomic % or more and 5 atomic % or less of carbon, and the balance is iron and impurities; a first phase and a second phase having different contents of cobalt and nitrogen; the first phase has a relatively higher cobalt content than the second phase; The second phase has a relatively higher nitrogen content than the first phase, A soft magnetic iron alloy plate, characterized in that the second phase crystal grains have a region in which multiple crystal grains are connected in the thickness direction of the soft magnetic iron alloy plate, and the region is more than half the thickness of the soft magnetic iron alloy plate.
2. The soft magnetic iron alloy plate according to claim 1, The first phase contains greater than 5 atomic % and less than 40 atomic % cobalt and greater than 0 atomic % and less than 0.2 atomic % nitrogen; The second phase contains 0 atomic % or more and 5 atomic % or less of cobalt and 0.5 atomic % or more and 10 atomic % or less of nitrogen.
3. The soft magnetic iron alloy plate according to claim 1, A soft magnetic iron alloy plate, characterized in that the first phase and the second phase have an average grain size of 45 μm or less, respectively.
4. The soft magnetic iron alloy plate according to claim 2, A soft magnetic iron alloy plate, characterized in that the first phase and the second phase have an average grain size of 45 μm or less, respectively.
5. The soft magnetic iron alloy plate according to claim 1, The volume fraction of the first phase is 50% by volume or more and 95% by volume or less, A soft magnetic iron alloy plate, characterized in that the volume fraction of the second phase is 50 volume % or less and 5 volume % or more.
6. The soft magnetic iron alloy plate according to claim 2, The volume fraction of the first phase is 50% by volume or more and 95% by volume or less, A soft magnetic iron alloy plate, characterized in that the volume fraction of the second phase is 50 volume % or less and 5 volume % or more.
7. The soft magnetic iron alloy plate according to claim 3, The volume fraction of the first phase is 50% by volume or more and 95% by volume or less, A soft magnetic iron alloy plate, characterized in that the volume fraction of the second phase is 50 volume % or less and 5 volume % or more.
8. The soft magnetic iron alloy plate according to claim 4, The volume fraction of the first phase is 50% by volume or more and 95% by volume or less, A soft magnetic iron alloy plate, characterized in that the volume fraction of the second phase is 50 volume % or less and 5 volume % or more.
9. The soft magnetic iron alloy plate according to any one of claims 1 to 8, A soft magnetic iron alloy plate having a saturation magnetization of 222 emu / g or more.
10. A method for producing a soft magnetic iron alloy sheet according to any one of claims 1 to 8, a starting material preparation step of preparing a starting material by mixing a first powder made of an iron-cobalt alloy containing more than 5 atomic % and 40 atomic % or less of cobalt and 0 atomic % or more and 1.2 atomic % or less of vanadium with a second powder made of an iron-based metal containing 0 atomic % or more and 5 atomic % or less of cobalt in a predetermined ratio; a molding / sintering step of forming a sintered body by molding and sintering the starting material; a martensite phase generating step of performing a heat treatment for infiltrating and diffusing nitrogen atoms into the sintered body, and then quenching the sintered body to generate a martensite phase; A subzero treatment step of further cooling the sintered body quenched in the martensite phase generation step to 0°C or lower. A method for manufacturing a soft magnetic iron alloy plate.
11. The method for producing a soft magnetic iron alloy sheet according to claim 10, A method for producing a soft magnetic iron alloy plate, characterized in that the specified ratio in the starting material preparation process is 5 mass% or more and 50 mass% or less of the second powder.
12. In the method for producing a soft magnetic iron alloy sheet according to claim 11, The first powder and the second powder in the starting material preparation step each have an average particle size of 1 μm or more and 45 μm or less, A method for producing a soft magnetic iron alloy plate, wherein a ratio of an average particle size of the first powder to an average particle size of the second powder is 1 or more and 10 or less.
13. The method for producing a soft magnetic iron alloy sheet according to claim 12, The heat treatment in the martensite phase generation step includes a process of adjusting the atmosphere to one containing ammonia gas after the temperature reaches 500°C or higher, raising the temperature to a temperature range for generating austenite phase, and then alternately switching between the atmosphere containing ammonia gas and the atmosphere not containing ammonia gas.
14. An iron core made of a laminate of soft magnetic iron alloy plates, An iron core, wherein the soft magnetic iron alloy plate is the soft magnetic iron alloy plate according to any one of claims 1 to 8.
15. A rotating electric machine having an iron core, A rotating electric machine, wherein the iron core is the iron core according to claim 14.
Citation Information
Patent Citations
HIGH SATURATION MAGNETIZATION Fe-N MAGNETIC MATERIAL
JP2001176715A
High hardness high magnetic property steel and its production method
JP2005226116A
Soft-magnetic iron plate, manufacturing method of soft-magnetic iron plate, and iron core and rotary electric machine using the soft-magnetic iron plate
JP2022055869A
Soft magnetic material, method for manufacturing soft magnetic material and electric motor
JP2022056923A
Soft magnetic iron alloy plate and its manufacturing method
JP2022141180A
Cited By
Stator cores, electric motors, and generators
JP2026124809A