Dimethyl acridine derivative, organic electroluminescence device, display device, and illumination device
Dimethylacridine derivatives with a low ionization potential are used in organic electroluminescent devices to form exciplexes with high electron affinity materials, addressing the challenge of high driving voltages and improving luminescent efficiency.
Patent Information
- Application Number
- JP2023050088
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing organic electroluminescent devices face challenges in achieving low driving voltages due to the limited availability of donor materials with low ionization potentials that can efficiently form exciplexes with acceptor materials.
The development of dimethylacridine derivatives with a methoxy group connected to the dimethylacridine skeleton, which have a low ionization potential of 4.5 eV or less, are used as donor materials in the hole transport layer, forming an exciplex with a second organic compound having high electron affinity in the light-emitting layer.
This configuration allows for organic electroluminescent devices to operate at significantly lower driving voltages, enhancing luminescent properties and reducing energy consumption.
Smart Images

Figure 2024139236000030 
Figure 2024139236000031 
Figure 2024139236000032
Abstract
Description
[Technical field]
[0001] The present invention relates to a dimethylacridine derivative, an organic electroluminescence (hereinafter, electroluminescence (field emission) may be abbreviated as "EL") element, a display device, and a lighting device. [Background technology]
[0002] In recent years, efforts have been actively made to make organic electroluminescence elements emit light at low applied voltages. For example, it has been reported that by using rubrene, a tetracene derivative, as a donor and fullerene, which has a large electron affinity, as an acceptor, the energy of an exciplex formed at the interface between them can be extracted as light emission from the singlet excited state of rubrene through triplet-triplet annihilation in an organic electroluminescence element (see, for example, Non-Patent Documents 1 and 2).
[0003] In addition, as compounds that can utilize triplet-triplet annihilation, compounds such as anthracene derivatives and tetracene derivatives have excellent electronic properties and exhibit high luminescence quantum yields, and are therefore used as light-emitting materials for organic electroluminescence devices that emit light at a low driving voltage (see, for example, Non-Patent Documents 1 to 5).
[0004] In an organic electroluminescence element combining rubrene and fullerene as described above, the energy difference between the ionization potential, which is the energy of the highest occupied molecular orbital (HOMO) of rubrene, and the lowest unoccupied molecular orbital (LUMO) of fullerene is small, and an excited state that contributes to light emission can be generated with a low applied voltage because an excited state can be formed with this small energy difference. In a typical organic electroluminescence element, charges are recombined in one molecule, so an applied voltage equivalent to the band gap energy is required to generate an excited state that contributes to light emission, but an organic electroluminescence element that uses an exciplex of a donor material with a small ionization potential and an acceptor material with a large electron affinity can emit light at a lower voltage.
[0005] However, there are only a limited number of donor materials that can form exciplexes and efficiently transfer energy to acceptor materials, and in order to obtain light emission at a further low voltage, a donor material with a small ionization potential is required. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] Sebastian Engmann and 5 others, "Nature Communications", Vol. 10, 2019, p. 227, doi.org / 10.1038 / s41467-018-08075-z [Non-Patent Document 2] Seiichiro Izawa, 3 others, DOI:10.26434 / chemrxiv.14685417.v1 [Non-Patent Document 3] Futong Liu, 8 others, "Journal of Materials Chemistry C", Volume 7, 2019, p14881, DOI:10.1039 / c9tc05040j [Non-Patent Document 4] Youn Jue Bae, 9 others, "Journal of the American chemical society", 2018, Volume 140, p15140, DOI:10.1021 / jacs.8b07498 [Non-Patent Document 5] Xiangyang Tang, 10 others, "Advanced Functional Materials", 2018, DOI:10.1002 / adfm.201705813 Summary of the Invention [Problem to be solved by the invention]
[0007] In the above Non-Patent Documents 1 and 2, light emission is obtained at a low applied voltage by using rubrene, which is a tetracene derivative, as a donor material. However, when rubrene is used as the donor material, it is difficult to reduce the energy gap, which is the difference between the ionization potential of the donor material and the electron affinity of the acceptor material, because the ionization potential of rubrene is 5.0 eV or more. In contrast, if a donor material with a smaller ionization potential could be created, it may be possible to realize an organic electroluminescence element that operates at a low voltage.
[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a donor material having a small ionization potential and excellent luminescence characteristics. Another object of the present invention is to provide an organic EL element, a display device and a lighting device which use such a donor material and have a low driving voltage. [Means for solving the problem]
[0009] The present inventors have conducted extensive research into donor materials with low ionization potential and have come to the conclusion that the above-mentioned problems can be solved by linking a methoxy group to a dimethylacridine skeleton as a donor material, thereby completing the present invention. That is, the essential configurations of the dimethylacridine derivative, organic electroluminescence element, display device, and lighting device of the present invention that solve the above problems are as follows.
[0010] [1] The following general formula (1): [ka] [In general formula (1), X 1 One of the X's is a methoxy group. 2 One of X is a methoxy group, and the other X 1 and X 2 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, A is C(CH3)2 or O; R' is hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and a group represented by the following general formula (1-1): [ka] (In general formula (1-1), X 3 One of the X's is a methoxy group. 4 One of X is a methoxy group, and the other X 3 and X 4are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be taken together to form a ring, and * represents a bond; In the general formulas (1) and (1-1), R each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. The dimethylacridine derivative of the present invention described in the above [1] has a small ionization potential (for example, a calculated value of the ionization potential is 4.5 eV or less) and is excellent in luminescence properties.
[0011] [2] The following general formula (2): [ka] [In general formula (2), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 5 One of the X's is a methoxy group. 6 One of X is a methoxy group, and the other X 1 , X 2 , X 5 and X 6each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently a hydrogen atom or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. The dimethylacridine derivative described in the above item [2] has a small ionization potential (for example, a calculated value of the ionization potential is 4.5 eV or less) and is excellent in luminescence properties.
[0012] [3] The following general formula (3): [ka] [In general formula (3), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 3 One of the X's is a methoxy group. 4 One of the X's is a methoxy group. 5 One of X is a methoxy group, and the other X 1 , X 2 , X 3 , X 4 and X 5each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently a hydrogen atom or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. The dimethylacridine derivative described in the above [3] has a small ionization potential (for example, a calculated value of the ionization potential is 4.5 eV or less) and is excellent in luminescence properties.
[0013] [4] The following general formula (4): [ka] [In general formula (4), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 3 One of the X's is a methoxy group. 4 One of X is a methoxy group, and the other X 1 , X 2 , X 3 and X 4each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently a hydrogen atom or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. The dimethylacridine derivative described in the above [4] has a small ionization potential (for example, a calculated value of the ionization potential is 4.5 eV or less) and is excellent in luminescence properties.
[0014] [5] An organic light-emitting device comprising, in this order, an anode, a hole transport layer, a light-emitting layer, and a cathode; the hole transport layer comprises a first organic compound which is a donor material having a small ionization potential; the light-emitting layer includes a second organic compound which is an acceptor material having a large electron affinity; An organic electroluminescence device, in which an exciplex is formed between the first organic compound and the second organic compound, An organic electroluminescence device, wherein the first organic compound is a dimethylacridine derivative according to any one of [1] to [4]. The organic electroluminescence device of the present invention described in [5] above has a low driving voltage.
[0015] [6] The organic electroluminescence device according to [5], wherein the first organic compound has a calculated ionization potential (IP) of 4.5 eV or less, calculated using a density functional theory method. The organic electroluminescence element described in [6] above has an even lower driving voltage.
[0016] [7] The organic electroluminescence element according to [5] or [6], wherein the second organic compound has a calculated electron affinity (EA) of 2.1 eV or more as calculated using density functional theory, or a measured electron affinity (EA) of 2.8 eV or more as measured by low-energy inverse photoelectron spectroscopy. The organic electroluminescence element described in [7] above has an even lower driving voltage.
[0017] [8] A display device comprising the organic electroluminescence element according to any one of [5] to [7]. The display device of the present invention described in [8] above emits light at a low applied voltage.
[0018] [9] A lighting device comprising the organic electroluminescence element according to any one of [5] to [7]. The lighting device of the present invention described in [9] above emits light at a low applied voltage. Effect of the Invention
[0019] According to the present invention, it is possible to provide a dimethylacridine derivative having a small ionization potential and excellent luminescence properties. Another object of the present invention is to provide an organic EL device, a display device and a lighting device which use the dimethylacridine derivative and have a low driving voltage. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a schematic diagram showing an example of the structure of an organic EL element of the present invention. [Diagram 2]FIG. 2 is a schematic diagram showing the energy levels in an example of an organic EL element of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing light emission from a singlet excited state of a material in an emitting layer, utilizing energy transfer from an exciplex and triplet-triplet annihilation, which is an example of the light-emitting mechanism of an organic EL device using an exciplex. [Figure 4] FIG. 2 is a schematic diagram showing another example of the structure of the organic EL element of the present invention. [Diagram 5] NMR spectrum of a dimethylacridine derivative represented by formula (2-1). [Figure 6] NMR spectrum of a dimethylacridine derivative represented by formula (3-1). [Figure 7] NMR spectrum of a dimethylacridine derivative represented by formula (4-1). [Figure 8] 1 is a graph showing the results of measuring (a) the current density-voltage characteristics and (b) the luminance-voltage characteristics of various organic EL elements produced in Example 1 and Comparative Example 1. [Figure 9] 1 is a graph showing the results of measuring (a) the current density-voltage characteristics and (b) the luminance-voltage characteristics of various organic EL elements produced in Example 2 and Comparative Example 1. [Figure 10] 1 is a graph showing the results of measuring (a) the current density-voltage characteristics and (b) the luminance-voltage characteristics of various organic EL elements produced in Example 3 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The dimethylacridine derivative, the organic electroluminescence element, the display device, and the lighting device of the present invention will be illustrated in detail below based on their embodiments. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.
[0022] <Dimethylacridine derivatives> The dimethylacridine derivative of the present invention is represented by the following general formula (1): [ka] [In general formula (1), X 1 One of the X's is a methoxy group. 2 One of X is a methoxy group, and the other X 1 and X 2 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, A is C(CH3)2 or O; R' is hydrogen, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and a group represented by the following general formula (1-1): [ka] (In general formula (1-1), X 3 One of the X's is a methoxy group. 4 One of X is a methoxy group, and the other X 3 and X 4are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be taken together to form a ring, and * represents a bond; In general formulas (1) and (1-1), R each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
[0023] The dimethylacridine derivative represented by the above general formula (1) has a structure in which a methoxy group is linked to a dimethylacridine skeleton, has a small ionization potential (for example, the calculated ionization potential calculated using density functional theory is 4.5 eV or less), and has excellent luminescence properties. The dimethylacridine derivative represented by the above general formula (1) contains a structure in which the two hydrogen atoms at the 9-position of 9,10-dihydroacridine are replaced by methyl groups and can also be called a "dimethyldihydroacridine derivative", but in this specification it will be simply called a "dimethylacridine derivative".
[0024] In the above general formula (1), X 1 One of the X's is a methoxy group. 2 One of X is a methoxy group, and the other X 1 and X 2are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. X 1 As one of the above, a methoxy group is linked to the dimethylacridine skeleton, and further, X 2 By connecting a substituted phenyl group having a methoxy group as one of the above to the nitrogen atom of the dimethylacridine skeleton, a dimethylacridine derivative with a small ionization potential and excellent luminescence properties can be obtained.
[0025] Also, four X 1 Any one of the X's may be a methoxy group, but the X's at the para position relative to the bonding position of the nitrogen atom 1 is preferably a methoxy group. 1 The other three of these are other than a methoxy group and may be the same or different.
[0026] Also, five X 2 Any one of the X's may be a methoxy group, but the X's at the para position relative to the bonding position of the nitrogen atom 2 is preferably a methoxy group. 2 The other four of are other than a methoxy group and may be the same or different.
[0027] In the above general formula (1), A is C(CH3)2 (i.e., 1,1-dimethylmethylene group) or O (oxygen). When A is C(CH3)2, the fused ring moiety containing A is also a dimethylacridine skeleton, whereas when A is O, the fused ring moiety containing A is a phenoxazine skeleton.
[0028] In the above general formula (1), R' is a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and a heterocyclic group represented by the above general formula (1-1), and adjacent substituents may be joined together to form a ring. R' corresponds to the para position with respect to the bonding position of the nitrogen atom, and a structure in which the heterocyclic group represented by the general formula (1-1) is bonded to this position is also included in the dimethyldihydroacridine derivative of the present invention. Here, * in general formula (1-1) represents a bond, and the heterocyclic group represented by general formula (1-1) can be bonded to the carbon atom to which R' in general formula (1) is bonded at the position of *.
[0029] In the above general formula (1-1), X 3 One of the X's is a methoxy group. 4 One of X is a methoxy group, and the other X 3 and X 4 are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
[0030] Also, four X 3 Any one of the X's may be a methoxy group, but the X's at the para position relative to the bonding position of the nitrogen atom 3 is preferably a methoxy group. 3 The other three of these are other than a methoxy group and may be the same or different.
[0031] Also, five X4 Any one of the X's may be a methoxy group, but the X's at the para position relative to the bonding position of the nitrogen atom 4 is preferably a methoxy group. 4 The other four of are other than a methoxy group and may be the same or different.
[0032] In the above general formulas (1) and (1-1), R each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
[0033] X in the above general formula (1) 1 , X 2 , R′ and R, and X in the above general formula (1-1) 3 , X 4Regarding R, examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, and a nonyl group, examples of the alkylthio group having 1 to 10 carbon atoms include a methylthio group, an ethylthio group, a propylthio group, a butylthio group, a pentylthio group, a hexylthio group, a heptylthio group, an octylthio group, and a nonylthio group, examples of the alkylamino group having 1 to 10 carbon atoms include a methylamino group, an ethylamino group, a propylamino group, a butylamino group, a pentylamino group, a hexylamino group, a heptylamino group, an octylamino group, and a nonylamino group, examples of the acyl group having 2 to 10 carbon atoms include an acetyl group, a propionyl group, and a butyryl group, Examples of the aralkyl group having 7 to 20 carbon atoms include a benzyl group, a phenethyl group, a phenylpropyl group, and a naphthylmethyl group. Examples of the substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms include a phenyl group, a 2,6-xylyl group, a mesityl group, a duryl group, a biphenyl group, a terphenyl group, a naphthyl group, an anthryl group, a pyrenyl group, a toluyl group, an anisyl group, a fluorophenyl group, a diphenylaminophenyl group, a dimethylaminophenyl group, a diethylaminophenyl group, a pyridylphenyl group, and a phenanthrenyl group. Examples of the substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms include a pyridyl group, a pyrazinyl group, a pyrimidinyl group, a pyridazinyl group, and a triazinyl group.
[0034] Regarding R′ and R in the above general formula (1), and R in the above general formula (1-1), examples of the alkoxy group having 1 to 10 carbon atoms include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, and an octyloxy group. 1 and X 2 and X in the above general formula (1-1) 3 and X 4With regard to the above, examples of the alkoxy group having 2 to 10 carbon atoms include an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, and an octyloxy group.
[0035] The dimethylacridine derivative represented by the above general formula (1) includes the following general formula (2): [ka] [In general formula (2), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 5 One of the X's is a methoxy group. 6 One of X is a methoxy group, and the other X 1 , X 2 , X 5 and X 6 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. The dimethylacridine derivative represented by the above general formula (2) has a small ionization potential (for example, a calculated value of the ionization potential calculated using density functional theory is 4.5 eV or less) and has excellent luminescence properties.
[0036] The dimethylacridine derivative represented by the above general formula (2) is a compound in which A in the above general formula (1) is C(CH3)2 (i.e., 1,1-dimethylmethylene group), R' is R, and five Rs bonded to specific sites (i.e., phenyl sites bonded to nitrogen atoms of the dimethylacridine skeleton) are X. 5 The four Rs that bind to other specific sites (i.e., the sides of the dimethylacridine skeleton that are not bound to other dimethylacridine skeletons) are X. 6 This corresponds to a compound in which
[0037] X in the above general formula (2) 1 , X 2 and R is X in the above general formula (1). 1 , X 2 and R.
[0038] In addition, in the above general formula (2), X 5 One of the X's is a methoxy group. 6 One of X is a methoxy group, and the other X 5 and X 6 are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring. X 6 As one of the above, a methoxy group is linked to the dimethylacridine skeleton, and further, X 5 By connecting a substituted phenyl group having a methoxy group as one of the groups to the nitrogen atom of the dimethylacridine skeleton, the ionization potential is further reduced.
[0039] X in the above general formula (2) 5 and X 6 With regard to the above, examples of the alkyl group having 1 to 10 carbon atoms, the alkoxy group having 2 to 10 carbon atoms, the alkylthio group having 1 to 10 carbon atoms, the alkylamino group having 1 to 10 carbon atoms, the acyl group having 2 to 10 carbon atoms, the aralkyl group having 7 to 20 carbon atoms, the substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and the substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms include X in the above general formula (1). 1 and X 2 and X in general formula (1-1) 3 and X 4 The examples given with respect to can be similarly exemplified.
[0040] Specific examples of the dimethylacridine derivative represented by the above general formula (2) include compounds represented by the following structural formulas (2-1) to (2-3). [ka]
[0041] The dimethylacridine derivative represented by the above general formula (1) includes the following general formula (3): [ka] [In general formula (3), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 3 One of the X's is a methoxy group. 4 One of the X's is a methoxy group. 5 One of X is a methoxy group, and the other X 1 , X 2 , X 3 , X 4 and X 5each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.] is also preferred. The dimethylacridine derivative represented by the above general formula (3) has a small ionization potential (for example, a calculated value of the ionization potential calculated using density functional theory is 4.5 eV or less) and has excellent luminescence properties.
[0042] The dimethylacridine derivative represented by the above general formula (3) is a compound in which A in the above general formula (1) is C(CH3)2 (i.e., 1,1-dimethylmethylene group), R' is a heterocyclic group represented by the above general formula (1-1), and five Rs bonded to specific sites (i.e., phenyl sites bonded to nitrogen atoms of the dimethylacridine skeleton) are X 5 This corresponds to a compound in which
[0043] X in the above general formula (3) 1 , X 2 and R is X in the above general formula (1). 1 , X 2 and R.
[0044] In addition, X in the above general formula (3) 3 and X 4 represents X in the above general formula (1-1).3 and X 4 X 3 As one of the above, a methoxy group is linked to the dimethylacridine skeleton, and further, X 4 By connecting a substituted phenyl group having a methoxy group as one of the groups to the nitrogen atom of the dimethylacridine skeleton, the ionization potential is further reduced.
[0045] In addition, X in the above general formula (3) 5 is X in the above general formula (2). 5 X 5 By connecting a substituted phenyl group having a methoxy group as one of the groups to the nitrogen atom of the dimethylacridine skeleton, the ionization potential is further reduced.
[0046] Specific examples of the dimethylacridine derivative represented by the above general formula (3) include compounds represented by the following structural formulas (3-1) to (3-3). [ka]
[0047] The dimethylacridine derivative represented by the above general formula (1) includes the following general formula (4): [ka] [In general formula (4), X 1 One of the X's is a methoxy group. 2 One of the X's is a methoxy group. 3 One of the X's is a methoxy group. 4 One of X is a methoxy group, and the other X 1 , X 2 , X 3 and X 4each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.] is also preferred. The dimethylacridine derivative represented by the above general formula (4) has a small ionization potential (for example, a calculated value of the ionization potential calculated using density functional theory is 4.5 eV or less) and has excellent luminescence properties.
[0048] The dimethylacridine derivative represented by the above general formula (4) corresponds to a compound in which A in the above general formula (1) is O (oxygen) and R' is a heterocyclic group represented by the general formula (1-1).
[0049] X in the above general formula (4) 1 , X 2 and R is X in the above general formula (1). 1 , X 2 and R.
[0050] In addition, X in the above general formula (4) 3 and X 4 represents X in the above general formula (1-1). 3 and X 4 X 3 As one of the above, a methoxy group is linked to the dimethylacridine skeleton, and further, X4 By connecting a substituted phenyl group having a methoxy group as one of the above to the nitrogen atom of the dimethylacridine skeleton, the ionization potential is reduced.
[0051] Specific examples of the dimethylacridine derivative represented by the above general formula (4) include compounds represented by the following structural formulas (4-1) to (4-3). [ka]
[0052] The dimethylacridine derivative represented by the above general formula (1) can be obtained by synthesis using a known method. The synthesis method for the dimethylacridine derivative represented by the general formula (1) is not particularly limited, but examples are shown below.
[0053] First, in one example, a compound having a dimethylacridine skeleton is prepared. An example of such a compound is 9,9'-dimethyl-9,10-dihydroacridine. Next, the hydrogen atoms bonded to the nitrogen atoms of the compound having the dimethylacridine skeleton are substituted with substituted or unsubstituted phenyl groups. Here, examples of the substituted phenyl group include a methoxyphenyl group, and by substituting a phenyl group having one methoxy group, five X 2 One of the bonds is a methoxy group, and the phenyl moiety can be prepared by using 4-iodoanisole or the like in the substitution reaction, and the reaction can be carried out in the presence of t-BuONa, Pd2(dba)3, t-Bu3P, or the like.
[0054] Next, the desired site of the compound having the phenyl-substituted dimethylacridine skeleton is halogenated. For the halogenation, benzyltrimethylammonium dichloroiodide (BTMA-ICl2) or the like can be used. The reaction can be carried out in the presence of calcium carbonate.
[0055] Next, the halogenated sites in the previous step are methoxylated. NaOCH3, copper(I) iodide, etc. can be used for the methoxylation. By the methoxylation, four X 1 A dimethylacridine skeleton can be prepared in which one of the groups is a methoxy group.
[0056] Next, the product obtained by methoxylation in the above step is halogenated again. For this halogenation, benzyltrimethylammonium dichloroiodide (BTMA-ICl2) or the like can be used. The reaction can also be carried out in the presence of calcium carbonate.
[0057] Next, a boryl group is introduced into the halogenated site in the previous step to obtain an organoboron compound. Isopropoxypinacolborane or the like can be used to introduce the boryl group. The reaction can be carried out in the presence of n-BuLi or the like.
[0058] The organoboron compound obtained as above can be subjected to Suzuki coupling with a phenyl-substituted, optionally methoxylated, and further halogenated dimethylacridine derivative to produce the dimethylacridine derivative represented by the above general formula (1).
[0059] Furthermore, in the case of a compound having three dimethylacridine skeletons, a dimethylacridine derivative which is phenyl-substituted and further has two halogen groups bonded thereto is prepared, and the dimethylacridine derivative having the two halogen groups bonded thereto is subjected to Suzuki coupling with the organoboron compound obtained as described above, thereby enabling synthesis.
[0060] Furthermore, when synthesizing a compound in which A in general formula (1) is O (oxygen), a phenoxazine derivative having two halogen groups bonded thereto, such as 3,7-dibromo-10-phenyl-10H-phenoxazine, can be used as a starting material, and the phenoxazine derivative can be subjected to Suzuki coupling with the organoboron compound obtained as described above to synthesize the compound.
[0061] The Suzuki coupling can be carried out in the presence of a ligand such as S-Phos{dicyclohexyl(2',6'-dimethoxy-[1,1'-biphenyl]-2-yl)phosphine}, a palladium catalyst such as palladium acetate [Pd(OAc)2], Pd2(dba)3, Pd(Ph3P)4, or Pd(dppf)Cl2, and a base such as tripotassium phosphate, sodium carbonate, or sodium bicarbonate.
[0062] <Organic electroluminescence element> The organic electroluminescence device of the present invention comprises an anode, a hole transport layer, a light emitting layer, and a cathode in this order, the hole transport layer containing a first organic compound which is a donor material having a small ionization potential, and the light emitting layer containing a second organic compound which is an acceptor material having a large electron affinity. The organic electroluminescence device of the present invention is characterized in that an exciplex is formed between the first organic compound and the second organic compound, and the first organic compound is a dimethylacridine derivative represented by the above general formula (1).
[0063] The donor material is a material that can donate electrons to adjacent molecules or atoms, and the smaller the ionization potential (IP) is, the easier it is to donate electrons. The acceptor material is a material that can attract electrons from adjacent molecules or atoms, and the larger the electron affinity (EA), the easier it is to attract electrons. In addition, a donor material has a small ionization potential and an acceptor material has a large electron affinity, meaning that the ionization potential is small, the electron affinity is large, and the energy difference between them is small to the extent that an exciplex is formed between the donor material (first organic compound) and the acceptor material (second organic compound).
[0064] In the organic electroluminescence element of the present invention, since the energy difference between the ionization potential (IP) of the first organic compound, which is the donor material, and the electron affinity (EA) of the second organic compound, which is the acceptor material, is small, the first organic compound, which is a donor material, is used in the hole transport layer, the second organic compound, which is an acceptor material, is used in the light-emitting layer, and the first organic compound, which is a donor material, and the second organic compound, which is an acceptor material, are adjacent to each other so as to form an exciplex between them, making it possible to obtain light emission at a low applied voltage.
[0065] Next, one embodiment of the organic electroluminescence (EL) element of the present invention will be described in detail with reference to the drawings. Fig. 1 is a schematic diagram showing an example of the structure of the organic EL element of the present invention. The organic EL element 1 shown in Fig. 1 has a laminated structure in which an anode 3, a hole injection layer 4, a hole transport layer 5, a light emitting layer 6, an electron injection layer 7, and a cathode 8 are formed in this order on a substrate 2.
[0066] The energy levels in the organic EL element 1 shown in Fig. 1 are shown in Fig. 2. In the organic EL element 1, electrons injected into the light-emitting layer 6 containing the second organic compound, which is an acceptor material with a large electron affinity, and holes injected into the hole-transporting layer 5 containing the first organic compound, which is a donor material with a small ionization potential, form an exciplex, which causes a current to flow and emits light. At this time, the voltage required for light emission is determined by the energy difference between the electron affinity (EA) of the material used in the light-emitting layer 6 and the ionization potential (IP) of the material used in the hole-transporting layer 5. However, if the material used in the light-emitting layer 6 has a large electron affinity and the material used in the hole-transporting layer 5 has a small ionization potential, this energy difference becomes small and the externally applied voltage required for light emission decreases.
[0067] Next, FIG. 3 shows the process of energy transfer from the formation of an exciplex to light emission. As shown in FIG. 3, the fact that the external voltage required for the formation of an exciplex is small means that the light energy of the obtained exciplex is not large. However, if the triplet energy of the material (e.g., anthracene derivatives, etc.) used in the light-emitting layer 6 involved in the formation of the exciplex is smaller than the excited state energy of this exciplex, the energy of the exciplex is transferred to the triplet excited state of the material used in the light-emitting layer 6. It is well known that anthracene derivatives, etc., generate a singlet excited state by utilizing triplet-triplet annihilation, and therefore, by utilizing this characteristic, a singlet excited state can be generated and light can be obtained from it.
[0068] The organic EL element 1 of this embodiment may be an organic EL element having an inverted structure in which a cathode 8 is provided on a substrate 2, as shown in Fig. 4. The organic EL element 1 shown in Fig. 4 has a laminated structure in which a cathode 8, an electron injection layer 7, an emitting layer 6, a hole transport layer 5, a hole injection layer 4, and an anode 3 are formed in this order on the substrate 2.
[0069] The organic EL element 1 of this embodiment may be an organic-inorganic hybrid organic electroluminescent element (HOILED element) in which some of the layers constituting the organic EL element are formed using inorganic compounds.
[0070] "substrate" The material of the substrate 2 may be a resin material, a glass material, or the like. Examples of the resin material used for the substrate 2 include polyethylene terephthalate, polyethylene naphthalate, polypropylene, cycloolefin polymer, polyamide, polyethersulfone, polymethyl methacrylate, polycarbonate, polyarylate, etc. When a resin material is used as the material for the substrate 2, it is preferable because an organic EL element 1 having excellent flexibility can be obtained. Examples of glass materials used for the substrate 2 include quartz glass and soda glass.
[0071] When the organic EL element 1 is of a bottom emission type, the material of the substrate 2 is a transparent substrate. When the organic EL element 1 is of a top emission type, not only a transparent substrate but also an opaque substrate may be used as the material of the substrate 2. Examples of opaque substrates include a substrate made of a ceramic material such as alumina, a substrate in which an oxide film (insulating film) is formed on the surface of a metal plate such as stainless steel, and a substrate made of a resin material.
[0072] The average thickness of the substrate 2 can be determined depending on the material of the substrate 2, and is preferably 0.1 to 30 mm, and more preferably 0.1 to 10 mm. The average thickness of the substrate 2 can be measured with a digital multimeter and a vernier caliper.
[0073] "anode" The anode 3 shown in FIG. 1 is formed on and in direct contact with the substrate 2, but in the case of an organic EL element having an inverted structure as shown in FIG. Examples of materials for the anode 3 include conductive oxide materials such as ITO (indium tin oxide), IZO (indium zinc oxide), FTO (fluorine tin oxide), In2O3, SnO2, Sb-containing SnO2, and Al-containing ZnO. Among these, it is preferable to use ITO, IZO, or FTO as the material for the anode 3. The average thickness of the anode 3 is not particularly limited, but is preferably from 10 to 500 nm, and more preferably from 100 to 200 nm. The average thickness of the anode 3 can be measured by a stylus step gauge or spectroscopic ellipsometry.
[0074] "Hole injection layer" The hole injection layer 4 may be made of an inorganic material or an organic material. Inorganic materials are more stable than organic materials, and therefore, it is easier to obtain high resistance to oxygen and water compared to the case where an organic material is used. The inorganic material is not particularly limited, but for example, one or more metal oxides such as vanadium oxide (V2O5), molybdenum oxide (MoO3), and ruthenium oxide (RuO2) can be used. Examples of organic materials that can be used include dipyrazino[2,3-f:2',3'-h]quinoxaline-2,3,6,7,10,11-hexacarbonitrile (HAT-CN) and 2,3,5,6-tetrafluoro-7,7,8,8-tetracyano-quinodimethane (F4-TCNQ). Polymer materials such as poly(3,4-ethylenedioxythiophene) (PEDOT) can also be used. The average thickness of the hole injection layer 4 is not particularly limited, but is preferably from 1 to 1000 nm, and more preferably from 5 to 50 nm. The average thickness of the hole injection layer 4 can be measured during deposition using a quartz crystal thickness gauge.
[0075] "Hole transport layer" As described above, the hole transport layer 5 contains the first organic compound, which is a donor material having a small ionization potential, and the first organic compound is the dimethylacridine derivative represented by the above general formula (1). The hole transport layer 5 is preferably formed mainly from the dimethylacridine derivative represented by the above general formula (1), and may be composed only of the dimethylacridine derivative represented by the above general formula (1), or may contain other components.
[0076] The first organic compound contained in the hole transport layer 5 has a calculated ionization potential (IP) of 4.5 eV or less, more preferably 4.3 eV or less, calculated using density functional theory [B3LPY / 6-31G(d,p)]. When the calculated ionization potential (IP) of the first organic compound contained in the hole transport layer 5 is 4.5 eV or less, the energy difference with the electron affinity (EA) of the second organic compound, which is an acceptor material described later, becomes smaller, and light emission can be obtained at a lower applied voltage.
[0077] For reference, calculated values of the ionization potentials (also referred to as "ionization energies") of common hole transport materials α-NPD and TPDI, the compound of the above structural formula (2-1), the compound of the above structural formula (3-1), and the compound of the above structural formula (4-1) are shown in Table 1. [ka]
[0078] [Table 1]
[0079] The average thickness of the hole transport layer 5 is not particularly limited, but is preferably from 10 to 150 nm, and more preferably from 20 to 100 nm. The average thickness of the hole transport layer 5 can be measured by, for example, a stylus step gauge or spectroscopic ellipsometry.
[0080] "Light-emitting layer" As described above, the light-emitting layer 6 contains a second organic compound that is an acceptor material with a large electron affinity, and the second organic compound can form an exciplex with the first organic compound. The light-emitting layer 6 may be composed of only the second organic compound, or may contain other components (e.g., dopants). The light-emitting layer 6 is mainly formed from a material that can generate a singlet excited state by triplet-triplet annihilation, and preferably contains a tetracene derivative such as a rubrene derivative, an anthracene derivative, or the like. In other words, the second organic compound is preferably a tetracene derivative such as a rubrene derivative, an anthracene derivative, or the like. Here, the rubrene derivative refers to a compound in which the hydrogen atoms in the molecular structure of rubrene are substituted with a substituent. The tetracene derivative refers to a compound having a tetracene skeleton (tetracene ring), and includes a compound in which the hydrogen atoms in the molecular structure of tetracene are substituted with a substituent. The anthracene derivative refers to a compound having an anthracene skeleton (anthracene ring), and includes a compound in which the hydrogen atoms in the molecular structure of anthracene are substituted with a substituent. Here, examples of the substituent include a cyano group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms.
[0081] The second organic compound preferably has a calculated electron affinity (EA) of 2.1 eV or more calculated using density functional theory [B3LPY / 6-31G(d,p)] or a measured electron affinity (EA) of 2.8 eV or more measured using low-energy inverse photoemission spectroscopy (LEIPS). When the calculated electron affinity (EA) of the second organic compound contained in the light-emitting layer 6 is 2.1 eV or more calculated using density functional theory or the measured electron affinity (EA) of the second organic compound is 2.8 eV or more, the energy difference with the ionization potential of the first organic compound, which is the donor material, becomes smaller, so that light emission can be obtained at a lower applied voltage.
[0082] In the light-emitting layer 6, it is also possible to extract light emission from another light-emitting dopant by using the second organic compound (exciplex) as a host of the light-emitting layer 6. In this case, a phosphorescent material such as an iridium complex or platinum complex, a fluorescent material, a thermally activated delayed fluorescent material, or the like may be mixed into the light-emitting layer 6 as a dopant for the host. The mixing ratio of the dopant is preferably 20% by mass or less, more preferably 10% by mass or less, relative to the second organic compound (exciplex).
[0083] In one embodiment, the light-emitting layer 6 further includes a phosphorescent material in addition to the second organic compound. As the phosphorescent material, a metal complex containing a metal such as Ir or Pt can be used. As an iridium complex, factris(2-phenylpyridine)iridium (Ir(ppy)3), fac-tris(3-methyl-2-phenylpyridinato-N,C2'-)iridium(III) (Ir(mppy)3), tris[1-phenylisoquinoline]iridium(III) (Ir(piq)3), etc. As an platinum complex, 2,3,7,8,12,13,17,18-octaethyl-21H,23H-porphine platinum(II), etc. can be used.
[0084] In another embodiment, the light-emitting layer 6 further contains a fluorescent material in addition to the second organic compound. Examples of the fluorescent material include various metal complexes such as 8-hydroxyquinoline aluminum (Alq3), tris(4-methyl-8-quinolinolato)aluminum(III) (Almq3), and 8-hydroxyquinoline zinc (Znq2); benzene-based compounds such as distyrylbenzene (DSB) and diaminodistyrylbenzene (DADSB); naphthalene-based compounds such as naphthalene and Nile Red; phenanthrene-based compounds such as phenanthrene; and chrysene-based compounds such as chrysene and 6-nitrochrysene. perylene, N,N'-bis(2,5-di-t-butylphenyl)-3,4,9,10-perylene-di-carboximide (BPPC), and other perylene-based compounds; coronene, and other coronene-based compounds; anthracene, bisstyrylanthracene, and other anthracene-based compounds; pyrene, BD-1, and other pyrene-based compounds; 4-(di-cyanomethylene)-2-methyl-6-(para-dimethylaminostyryl)-4H-pyran (DCM), and other pyran-based compounds; acridine, and other acridine-based compounds; styryl thiophene compounds such as 2,5-dibenzoxazolethiophene; benzoxazole compounds such as benzoxazole; benzimidazole compounds such as benzimidazole; benzothiazole compounds such as 2,2'-(para-phenylenedivinylene)-bisbenzothiazole; butadiene compounds such as bistyryl(1,4-diphenyl-1,3-butadiene) and tetraphenylbutadiene; naphthalimide compounds such as naphthalimide; coumarin perinone-based compounds such as perinone; oxadiazole-based compounds such as oxadiazole; aldazine-based compounds; cyclopentadiene-based compounds such as 1,2,3,4,5-pentaphenyl-1,3-cyclopentadiene (PPCP); quinacridone-based compounds such as quinacridone and quinacridone red; pyridine-based compounds such as pyrrolopyridine and thiadiazolopyridine; and spiro compounds such as 2,2',7,7'-tetraphenyl-9,9'-spirobifluorene.
[0085] In yet another embodiment, the light-emitting layer 6 further contains a thermally activated delayed fluorescent material in addition to the second organic compound. Examples of the thermally activated delayed fluorescent material include 2,4,5,6-tetra(9-carbazole)-isophthalonitrile (4CzIPN), 4,5-di(9-carbazole)-phthalonitrile (2CzPN), 3,4,5,6-tetra(9-carbazole)-phthalonitrile (4CzPN), 2,3,5,6-tetra(9-carbazole)-terephthalonitrile (4CzTPN), 2,3,5,6-tetra(3,6-dimethyl-9-carbazole)-terephthalonitrile (4CzTPN-Me), 2,3,5,6-tetra(3,6-diphenyl-9-carbazole)-terephthalonitrile (4CzTPN-Ph), and further include compounds described in JP2012-193352A and WO2011 / 070963A.
[0086] The average thickness of the light-emitting layer 6 is not particularly limited, but is preferably from 10 to 150 nm, and more preferably from 20 to 100 nm. The average thickness of the light-emitting layer 6 may be measured by a stylus-type step gauge, or may be measured by a quartz crystal thickness gauge during the deposition of the light-emitting layer 6.
[0087] "Electron injection layer" The electron injection layer 7 can be made of any of a variety of materials having a low work function, such as alkali metals and alkaline earth metals; compounds containing a metal having a low work function, such as lithium quinoline, lithium fluoride, cesium carbonate, and calcium carbonate; a hexahydropyrimidopyrimidine compound having a structure represented by the following general formula (5); or a compound having a structure represented by the following general formula (6).
[0088] [ka] (In general formula (5), R 1represents an aromatic hydrocarbon group, an aromatic heterocyclic group, an aryl alkylene group, a divalent to tetravalent linear or cyclic hydrocarbon group, which may have a substituent, a group formed by combining two or more of these groups, or a group formed by combining one or more of these groups with a nitrogen atom. 1 is an integer from 1 to 4.)
[0089] [ka] (In general formula (6), X 7 , X 8 are the same or different and each represents a nitrogen atom, an oxygen atom, a sulfur atom, or a divalent linking group which may have a substituent. L represents a direct bond or a p-valent linking group. 2 represents a number of 0 or 1, and p represents a number of 1 to 4. q represents a number of 0 or 1, and when p is 1, q is 0. R 2 ~R 4 m may be the same or different and represents a monovalent substituent. 1 ~m 3 R may be the same or different and represents a number from 0 to 3. 2 ~R 4 X 7 , X 8 may be bonded to form a ring structure, R 2 If there are multiple R 2 may be bonded to form a ring structure. 3 If there are multiple R 3 may be bonded to form a ring structure. 4 If there are multiple R 4 may be bonded to form a ring structure.
[0090] R in the above general formula (5) 1 represents an aromatic hydrocarbon group which may have a substituent, an aromatic heterocyclic group, an aryl alkylene group, a divalent to tetravalent chain or cyclic hydrocarbon group, a group formed by combining two or more of these groups, or a group formed by combining one or more of these groups with a nitrogen atom. The aromatic hydrocarbon group and aromatic heterocyclic group preferably have 3 to 30 carbon atoms, more preferably have 4 to 24 carbon atoms, and further preferably have 5 to 20 carbon atoms. Examples of aromatic hydrocarbon groups include compounds consisting of only one aromatic ring, such as benzene; compounds in which multiple aromatic rings, such as biphenyl and diphenylbenzene, are directly bonded to each other via one carbon atom; and groups formed by removing one to four hydrogen atoms from any of the aromatic rings of condensed ring aromatic hydrocarbon compounds, such as naphthalene, anthracene, phenanthrene, and pyrene. Examples of the aromatic heterocyclic group include compounds consisting of only one aromatic heterocycle, such as thiophene, furan, pyrrole, oxazole, oxadiazole, thiazole, thiadiazole, imidazole, pyridine, pyrimidine, pyrazine, and triazine; compounds in which a plurality of compounds consisting of only one aromatic heterocycle are directly bonded to each other via one carbon atom (such as bipyridine); and groups obtained by removing 1 to 4 hydrogen atoms from any of the aromatic heterocycles of condensed ring heteroaromatic hydrocarbon compounds, such as quinoline, quinoxaline, benzothiophene, benzothiazole, benzimidazole, benzoxazole, indole, carbazole, dibenzofuran, dibenzothiophene, acridine, and phenanthroline. The arylalkylene group includes a group formed by combining the above aromatic hydrocarbon group with an alkylene group having 1 to 3 carbon atoms. The divalent to tetravalent chain or cyclic hydrocarbon group preferably has 1 to 12 carbon atoms, more preferably has 1 to 6 carbon atoms, and further preferably has 1 to 4 carbon atoms. The chain hydrocarbon group may be either linear or branched. Also, R 1 may be a group formed by combining two or more of the above-mentioned aromatic hydrocarbon groups, aromatic heterocyclic groups, aryl alkylene groups, and divalent to tetravalent chain hydrocarbon groups. Furthermore, R 1may be a group formed by combining one or more of the above aromatic hydrocarbon groups, aromatic heterocyclic groups, aryl alkylene groups, and divalent to tetravalent chain hydrocarbon groups with a nitrogen atom. Examples of such groups include groups formed by removing 1 to 4 hydrogen atoms from trialkylamines such as trimethylamine or triphenylamine.
[0091] The aromatic hydrocarbon group, aromatic heterocyclic group, or arylalkylene group may have one or more monovalent substituents. Examples of the monovalent substituent include a fluorine atom; a haloalkyl group such as a fluoromethyl group, a difluoromethyl group, or a trifluoromethyl group; a linear or branched alkyl group having 1 to 20 carbon atoms such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a tert-butyl group; a cyclic alkyl group having 5 to 7 carbon atoms such as a cyclopentyl group, a cyclohexyl group, or a cycloheptyl group; a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, or a methyloxy group. linear or branched alkoxy groups having 1 to 20 carbon atoms, such as a silyl group or an octyloxy group; a nitro group; a cyano group; an alkylamino group having an alkyl group having 1 to 10 carbon atoms, such as a methylamino group, an ethylamino group, a dimethylamino group or a diethylamino group; a cyclic amino group, such as a pyrrolidino group, a piperidino group or a morpholino group; a diarylamino group, such as a diphenylamino group or a carbazolyl group; an acyl group, such as an acetyl group, a propionyl group or a butyryl group; an alkenyl group having 2 to 30 carbon atoms, such as a styryl group; a halogen atom, such as a fluorine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a cyclic amino group having 1 to 10 carbon atoms, such as ... an aryl group having 5 to 20 carbon atoms which may be substituted with a silyl group, an amino group, or the like (specific examples of the aryl group are the same as those of the aromatic hydrocarbon group described above); a heterocyclic group containing one or more of a nitrogen atom, a sulfur atom, and an oxygen atom which may be substituted with a halogen atom such as a fluorine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group, an amino group, or the like (the heterocyclic group may be one consisting of only one ring, or may be a compound in which a plurality of compounds consisting of only one aromatic heterocycle are directly bonded to each other at one carbon atom, or may be a condensed heterocyclic group. Specific examples of the heterocyclic group include Specific examples of aromatic heterocyclic groups include a thiophene ring, a furan ring, a pyrrole ring, a benzothiophene ring, a benzofuran ring, an indole ring, a dibenzothiophene ring, a dibenzofuran ring, a carbazole ring, a thiazole ring, a benzothiazole ring, an oxazole ring, a benzoxazole ring, an imidazole ring, a benzimidazole ring, a pyridine ring, a pyrimidine ring, a pyrazine ring, a pyridazine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, a benzothiadiazole ring, a phenanthridine ring, etc.); an ester group, a thioether group, etc.These groups may be substituted with a halogen atom, a hetero element, an alkyl group, an aromatic ring, or the like.
[0092] In the above general formula (5), n 1 is an integer of 1 to 4, preferably 2 or 3.
[0093] X in the above general formula (6) 7 , X 8 are the same or different and represent a nitrogen atom, an oxygen atom, a sulfur atom or a divalent linking group which may have a substituent. Examples of the divalent linking group include divalent hydrocarbon groups and groups in which some of the carbon atoms of a hydrocarbon group have been substituted with a heteroatom such as a nitrogen atom, an oxygen atom or a sulfur atom. The hydrocarbon group preferably has 1 to 6 carbon atoms, and more preferably has 1, 2 or 6 carbon atoms. The hydrocarbon group may be linear, branched, cyclic, or a combination thereof. The divalent hydrocarbon group may be an alkylene group, which is a saturated hydrocarbon group, or an unsaturated hydrocarbon group such as an alkenylene group or an alkynylene group.
[0094] In the above general formula (6), L represents a direct bond or a p-valent linking group. Note that L becomes a direct bond only when p is 2. Examples of the p-valent linking group include a nitrogen atom, an oxygen atom, a sulfur atom, a carbon atom, and also a group obtained by removing p hydrogen atoms from a hydrocarbon group or a group in which some of the carbon atoms of a hydrocarbon group have been substituted with a heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom. When the p-valent linking group has a carbon atom, it preferably has 1 to 30 carbon atoms, and more preferably has 1 to 20 carbon atoms. The hydrocarbon group may be linear, branched, cyclic, or a combination thereof. The hydrocarbon group may be any of a saturated hydrocarbon group, an unsaturated hydrocarbon group, and an aromatic hydrocarbon group. Examples of aromatic hydrocarbon groups include groups formed by removing a hydrogen atom from an aromatic compound such as a benzene ring, a naphthalene ring, an anthracene ring, a tetracene ring, a pentacene ring, a triphenylene ring, a pyrene ring, a fluorene ring, or an indene ring.
[0095] R in the above general formula (6) 2 ~R 4 are the same or different and each represents a monovalent substituent. 1 ~m 3 are the same or different and represent a number from 0 to 3. Examples of the monovalent substituent include a fluorine atom; a haloalkyl group such as a fluoromethyl group, a difluoromethyl group, or a trifluoromethyl group; a linear or branched alkyl group having 1 to 20 carbon atoms such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, or a tert-butyl group; a cyclic alkyl group having 5 to 7 carbon atoms such as a cyclopentyl group, a cyclohexyl group, or a cycloheptyl group; a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, a heptyloxy group, or a methyloxy group. linear or branched alkoxy groups having 1 to 20 carbon atoms, such as a silyl group or an octyloxy group; a nitro group; a cyano group; an alkylamino group having an alkyl group having 1 to 10 carbon atoms, such as a methylamino group, an ethylamino group, a dimethylamino group or a diethylamino group; a cyclic amino group, such as a pyrrolidino group, a piperidino group or a morpholino group; a diarylamino group, such as a diphenylamino group or a carbazolyl group; an acyl group, such as an acetyl group, a propionyl group or a butyryl group; an alkenyl group having 2 to 30 carbon atoms, such as a styryl group; a halogen atom, such as a fluorine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a cyclic amino group having 1 to 10 carbon atoms, such as ... an aryl group having 5 to 20 carbon atoms which may be substituted with a silyl group, an amino group, or the like (specific examples of the aryl group are the same as those of the aromatic hydrocarbon group described above); a heterocyclic group containing one or more of a nitrogen atom, a sulfur atom, and an oxygen atom which may be substituted with a halogen atom such as a fluorine atom, an alkyl group having 1 to 20 carbon atoms, an alkoxy group, an amino group, or the like (the heterocyclic group may be one consisting of only one ring, or may be a compound in which a plurality of compounds consisting of only one aromatic heterocycle are directly bonded to each other at one carbon atom, or may be a condensed heterocyclic group. Specific examples of the heterocyclic group include Specific examples of aromatic heterocyclic groups include a thiophene ring, a furan ring, a pyrrole ring, a benzothiophene ring, a benzofuran ring, an indole ring, a dibenzothiophene ring, a dibenzofuran ring, a carbazole ring, a thiazole ring, a benzothiazole ring, an oxazole ring, a benzoxazole ring, an imidazole ring, a benzimidazole ring, a pyridine ring, a pyrimidine ring, a pyrazine ring, a pyridazine ring, a triazine ring, a quinoline ring, an isoquinoline ring, a quinoxaline ring, a benzothiadiazole ring, a phenanthridine ring, etc.); an ester group, a thioether group, etc.These groups may be substituted with a halogen atom, a hetero element, an alkyl group, an aromatic ring, or the like.
[0096] In the above general formula (6), p represents a number of 1 to 4, and is preferably a number of 1 to 3. In addition, n in the above general formula (6) 2 represents the number 0 or 1, with 0 being preferred.
[0097] The average thickness of the electron injection layer 7 is preferably 0.5 to 100 nm, and more preferably 1 to 10 nm. The electron injection layer 7 can be formed by applying a coating composition or by co-deposition using a vacuum deposition method. The average thickness of the electron injection layer 7 can be measured by, for example, a stylus step gauge or spectroscopic ellipsometry.
[0098] "cathode" Examples of materials used for the cathode 8 include ITO, IZO, Au, Pt, Ag, Cu, Al, and alloys containing these. Among these, it is preferable to use ITO, IZO, Au, Ag, or Al as the material for the cathode 8. The average thickness of the cathode 8 is not particularly limited, but is preferably 10 to 1000 nm, and more preferably 30 to 150 nm. Even when an opaque material is used as the material for the cathode 8, by setting the average thickness to, for example, about 10 to 30 nm, it can be used as a transparent cathode in a top-emission organic EL element. The average thickness of the cathode 8 can be measured by a quartz crystal film thickness meter during the deposition of the cathode 8.
[0099] In particular, in the organic EL element having an inverted structure shown in FIG. 4, the layer made of an inorganic oxide formed on the cathode 8 is also treated as a part of the cathode. The oxide used in this case is a semiconductor or insulator laminated thin film layer. Specifically, it may be any of a layer made of a single metal oxide, a layer made of a mixture of two or more metal oxides and a layer made of a single metal oxide, or a layer made of a mixture of two or more metal oxides.
[0100] Metal elements constituting metal oxides that form inorganic oxides include magnesium, calcium, strontium, barium, titanium, zirconium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, indium, gallium, iron, cobalt, nickel, copper, zinc, cadmium, aluminum, and silicon.
[0101] When the layer made of an inorganic oxide includes a layer containing a mixture of two or more kinds of metal oxides, it is preferable that at least one of the metal elements constituting the metal oxide is a layer made of magnesium, aluminum, calcium, zirconium, hafnium, silicon, titanium, or zinc. When the layer made of an inorganic oxide is a layer made of a simple metal oxide, it is preferable that the layer is made of a metal oxide selected from the group consisting of magnesium oxide, aluminum oxide, zirconium oxide, hafnium oxide, silicon oxide, titanium oxide, and zinc oxide.
[0102] When the layer made of an inorganic oxide is a layer obtained by laminating either or both of a layer made of a mixture of two or more kinds of metal oxides and a layer made of a single metal oxide, or a layer obtained by mixing two or more kinds of metal oxides, examples of the layer made of an inorganic oxide include a layer made of a mixture of two kinds of metal oxides selected from titanium oxide / zinc oxide, titanium oxide / magnesium oxide, titanium oxide / zirconium oxide, titanium oxide / aluminum oxide, titanium oxide / hafnium oxide, titanium oxide / silicon oxide, zinc oxide / magnesium oxide, zinc oxide / zirconium oxide, zinc oxide / hafnium oxide, zinc oxide / silicon oxide, and calcium oxide / aluminum oxide, a layer made of a mixture of three kinds of metal oxides selected from titanium oxide / zinc oxide / magnesium oxide, titanium oxide / zinc oxide / zirconium oxide, titanium oxide / zinc oxide / aluminum oxide, titanium oxide / zinc oxide / hafnium oxide, titanium oxide / zinc oxide / silicon oxide, and indium oxide / gallium oxide / zinc oxide.
[0103] The inorganic oxide may include IGZO (indium gallium zinc oxide), which is an oxide semiconductor that exhibits favorable characteristics as a special composition, and / or 12CaO·7Al2O3, which is an electride. When an inorganic oxide film is formed, the average thickness is not particularly limited, but is preferably 1 to 1000 nm, and more preferably 2 to 100 nm. The average thickness of the layer made of an inorganic oxide can be measured by a stylus step gauge or spectroscopic ellipsometry.
[0104] "Sealing" The organic EL element 1 may be sealed, if necessary. For example, the organic EL element 1 may be sealed by a sealing container (not shown) having a concave space for accommodating the organic EL element 1, and an adhesive for bonding the edge of the sealing container to the substrate 2. Alternatively, the organic EL element 1 may be accommodated in a sealing container and sealed by filling it with a sealant made of an ultraviolet (UV) curable resin or the like.
[0105] When the organic EL element 1 is sealed using a sealing container or a sealing member, a desiccant that absorbs moisture may be placed inside the sealing container or the sealing member. A material that absorbs moisture may be used as the sealing container or the sealing member. A space may be formed inside the sealed sealing container or the sealing member.
[0106] Resin materials, glass materials, etc. can be used as the material of the sealing container or sealing member used to seal the organic EL element 1. Examples of the resin materials and glass materials used for the sealing container or sealing member include the same materials as those used for the substrate 2.
[0107] "Manufacturing method for organic EL elements" Next, a method for producing the organic EL element 1 will be described as an example of a method for producing the organic EL element of the present invention.
[0108] To manufacture the organic EL element 1, first, the anode 3 is formed on the substrate 2. The anode 3 can be formed by a sputtering method, a vacuum deposition method, a sol-gel method, a spray pyrolysis (SPD) method, an atomic layer deposition (ALD) method, a vapor phase deposition method, a liquid phase deposition method, etc. The anode 3 may be formed by bonding a metal foil.
[0109] Next, on the anode 3, a hole injection layer 4, a hole transport layer 5, a light emitting layer 6, and an electron injection layer 7 are formed in this order. The methods for forming the hole injection layer 4, the hole transport layer 5, the light emitting layer 6, and the electron injection layer 7 are not particularly limited, and various conventionally known formation methods can be used appropriately in accordance with the properties of the materials used for the hole injection layer 4, the hole transport layer 5, the light emitting layer 6, and the electron injection layer 7, respectively. Specifically, methods for forming the hole injection layer 4, the hole transport layer 5, the light emitting layer 6, and the electron injection layer 7 include a coating method in which an organic compound solution containing an organic compound that will become the hole injection layer 4, the hole transport layer 5, the light emitting layer 6, and the electron injection layer 7 is applied, a vacuum deposition method, an ESDUS (Evaporative Spray Deposition from Ultra-dilute Solution) method, and the like.
[0110] Next, the cathode 8 is formed on the electron injection layer 7. The cathode 8 can be formed in the same manner as the anode 3, for example.
[0111] The order is reversed when fabricating an organic EL element having an inverted structure as shown in Fig. 4. When forming a layer made of an inorganic oxide on the cathode 8 in the organic EL element having an inverted structure as shown in Fig. 4, the oxide is formed by using a method such as a spray pyrolysis method, a sol-gel method, a sputtering method, or a vacuum deposition method. Through the above steps, the organic EL element 1 is obtained.
[0112] "Sealing method" When sealing the organic EL element 1, it can be sealed by using a method commonly used for sealing an organic EL element.
[0113] <Display device, lighting device> The organic EL device 1 of the present embodiment emits light by utilizing an exciplex formed between a first organic compound, which is an organic material (donor material) of the present invention having a small ionization potential, and a second organic compound, which is an acceptor material having a large electron affinity, and therefore allows recombination of charges with small energy, resulting in an organic EL device 1 with a low driving voltage.
[0114] The organic EL element of the present invention can change the emission color by appropriately selecting the materials for the light-emitting layer, etc., and can also obtain a desired emission color by using a color filter, etc. Therefore, the organic EL element of the present invention can be suitably used as a light-emitting portion of a display device or a lighting device.
[0115] The display device of the present invention has an excellent productivity due to its simple element structure, and includes the organic EL element of the present invention, which has a low driving voltage, and is therefore preferable as a display device. The display device of the present invention emits light at a low applied voltage.
[0116] Furthermore, the lighting device of the present invention has excellent productivity due to its simple element structure, and includes the organic EL element of the present invention, which has a low driving voltage, and is therefore preferable as a lighting device. The lighting device of the present invention emits light at a low applied voltage. EXAMPLES
[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0118] <Synthesis of compound represented by formula (7-5)> The compound represented by formula (7-5) was synthesized according to the following reaction scheme. [ka]
[0119] "Synthesis process of the compound represented by formula (7-1)" In an argon atmosphere, 9,9'-dimethyl-9,10-dihydroacridine (5.1 g, 24.4 mmol, 1.0 eq.), 4-iodoanisole (11.4 g, 48.7 mmol, 2.0 eq.), t-BuONa (7.02 g, 73.1 mmol, 3.0 eq.), and degassed toluene (100 mL) were added to a 300 mL reactor. After degassing the suspension under reduced pressure, Pd2(dba)3 (440 mg, 0.487 mmol, 0.02 eq.) and a toluene solution (1.0 M) of t-Bu3P (1.46 mL, 1.46 mmol, 0.06 eq.) were added, and the suspension was degassed again under reduced pressure. This suspension was heated and stirred at a bath temperature of 100°C for 3 hours, then allowed to cool, and the precipitated solid was filtered through Celite, the filter bed was washed with toluene (50mL x 2), and the filtrate was concentrated to obtain a dark brown solid (10.1g). This was purified through a column (SiO2 = 200g, heptane / toluene = 2 / 1 → 1 / 1) to obtain compound 1 (7.75g, 24.6mmol, quant) represented by formula (7-1) as a colorless solid.
[0120] In an argon atmosphere, 9,9'-dimethyl-9,10-dihydroacridine (5.1 g, 24.4 mmol, 1.0 eq.), 4-iodoanisole (11.4 g, 48.7 mmol, 2.0 eq.), t-BuONa (7.02 g, 73.1 mmol, 3.0 eq.), and degassed toluene (100 mL) were added to a 300 mL reactor. After degassing the suspension under reduced pressure, Pd2(dba)3 (440 mg, 0.487 mmol, 0.02 eq.) and a toluene solution (1.0 M) of t-Bu3P (1.46 mL, 1.46 mmol, 0.06 eq.) were added, and the suspension was degassed again under reduced pressure. This suspension was heated and stirred at a bath temperature of 100°C for 3 hours, then allowed to cool, and the precipitated solid was filtered through Celite. The filter bed was washed with toluene (50mL x 2), and the filtrate was concentrated to obtain a dark brown solid (10.1g). This was purified through a column (SiO2 = 150g, heptane / toluene = 2 / 1 → 1 / 1) to obtain compound 2 (7.2g, 22.8mmol, 93%) represented by formula (7-1) as a colorless solid.
[0121] In an argon atmosphere, 9,9'-dimethyl-9,10-dihydroacridine (10.2 g, 48.8 mmol, 1.0 eq.), 4-iodoanisole (22.8 g, 97.5 mmol, 2.0 eq.), t-BuONa (14.0 g, 146 mmol, 3.0 eq.), and degassed toluene (250 mL) were added to a 500 mL reactor. After degassing the suspension under reduced pressure, Pd2(dba)3 (890 mg, 0.975 mmol, 0.02 eq.) and a toluene solution (1.0 M) of t-Bu3P (3.9 mL, 3.90 mmol, 0.08 eq.) were added, and the suspension was degassed again under reduced pressure. The suspension was heated and stirred at a bath temperature of 100°C for 3 hours, then allowed to cool, and the precipitated solid was filtered through Celite. The filter bed was washed with toluene (100mL x 2), and the filtrate was concentrated to obtain a dark brown solid (21.0g). This was purified through a column (SiO2 = 250g, heptane / toluene = 2 / 1 → 1 / 1) to obtain compound 3 (15.1g, 48.0mmol, 98%) represented by formula (7-1) as a colorless solid.
[0122] "Synthesis process of the compound represented by formula (7-2)" In an argon atmosphere, compound 1 (1.5 g, 4.75 mmol, 1.0 eq.) represented by formula (7-1), calcium carbonate (0.476 g, 4.75 mmol, 1.0 eq.), dehydrated dichloromethane (150 mL), and dehydrated methanol (40 mL) were added to a 300 mL reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (1.66 g, 4.75 mmol, 1.0 eq.) was added to this vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 6 hours. The reddish-brown suspension was concentrated, and an aqueous sodium hydrosulfide solution (3%) (100 mL) and ethyl acetate (100 mL) were added to the residue, and the mixture was stirred for 10 minutes and then separated into two layers. The aqueous layer was extracted with ethyl acetate (50 mL), and the organic layers were combined, washed with city water and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (3.1 g, wet). This was purified by column chromatography (NH-SiO2 = 30 g, heptane / toluene = 1 / 1 → toluene only) to obtain compound 1 (2.0 g, 4.53 mmol, 95%) represented by formula (7-2) as a colorless solid.
[0123] In an argon atmosphere, compound 1 (6.2 g, 19.6 mmol, 1.0 eq.) represented by formula (7-1), calcium carbonate (2.16 g, 21.6 mmol, 1.1 eq.), dehydrated dichloromethane (620 mL), and dehydrated methanol (248 mL) were added to a 2 L reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (7.52 g, 21.6 mmol, 1.0 eq.) was added to this vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 8 hours. The reddish brown suspension was concentrated, and an aqueous sodium hydrosulfide solution (3%) (700 mL) and ethyl acetate (500 mL) were added to the residue, and the mixture was stirred for 10 minutes and then separated into two layers. The aqueous layer was extracted with ethyl acetate (300 mL), and the organic layers were combined, washed with city water and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (9.4 g, wet). This was purified by column chromatography (NH-SiO2 = 150 g, heptane / toluene = 1 / 1 → toluene only) to obtain compound 2 (8.4 g, 19.0 mmol, 97%) represented by formula (7-2) as a colorless solid.
[0124] In an argon atmosphere, compound 2 (6.0 g, 19.0 mmol, 1.0 eq.) represented by formula (7-1), calcium carbonate (2.85 g, 28.5 mmol, 1.5 eq.), dehydrated dichloromethane (300 mL), and dehydrated methanol (120 mL) were added to a 2 L reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (8.6 g, 24.7 mmol, 1.0 eq.) was added to this vigorously stirred suspension at room temperature, and the mixture was stirred for 24 hours at the same temperature in an oxygen atmosphere. The reddish brown suspension was concentrated, and an aqueous sodium hydrosulfide solution (3%) (150 mL) and ethyl acetate (500 mL) were added to the residue, and the mixture was stirred for 10 minutes, after which the mixture was separated into two layers. The aqueous layer was extracted with ethyl acetate (300 mL), and the organic layers were combined and washed with saturated sodium bicarbonate water, tap water, and saturated saline, successively, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (9.4 g, wet.). This was purified by column purification (NH-SiO2 = 150 g, heptane / toluene = 1 / 1 → toluene only) to obtain compound 3 (10.5 g, 23.7 mmol, excess, including diiodo form) represented by formula (7-2) as a colorless solid.
[0125] "Synthesis process of the compound represented by formula (7-3)" In an argon atmosphere, anhydrous methanol and anhydrous DMF (30 mL) were added to a 100 mL reactor, and NaH (60%) (2.08 g, 90.6 mmol, 20 eq.) was added to this solution. After about 1 hour until the foaming of this suspension subsided, compound 1 (2.0 g, 4.53 mmol, 1.0 eq.) represented by formula (7-2) and copper (I) iodide (1.72 g, 9.06 mmol, 2.0 eq.) were added. The suspension was heated to 120°C and stirred at the same temperature for 3 hours. After cooling, the suspension was filtered through Celite, the filter bed was washed with ethyl acetate, and 5% aqueous ammonium chloride solution (120 mL) was added to the filtrate, and the mixture was separated into two layers. The aqueous layer was extracted with ethyl acetate (30 mL), and the organic layers were combined and washed with city water and saturated saline, dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a dark brown solid 1 (3.0 g).
[0126] Under an argon atmosphere, a 500 mL reactor was charged with a 28% solution of NaOCH3 in CH3OH (73.4 g, 381 mmol, 20 eq.) and anhydrous DMF (125 mL). To this suspension was added a mixture of compound 1 represented by formula (7-2) and compound 2 represented by formula (7-2) (8.4 g, 19.0 mmol, 1.0 eq.), and copper (I) iodide (7.2 g, 38.1 mmol, 2.0 eq.). The suspension was heated to 120°C and stirred at the same temperature for 5 hours. After cooling, the suspension was filtered through Celite, the filter bed was washed with ethyl acetate, and 5% aqueous ammonium chloride solution (480 mL) was added to the filtrate, and the mixture was separated into two layers. The aqueous layer was extracted with ethyl acetate (200 mL), and the organic layers were combined, washed with city water and saturated saline, dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a dark brown solid 2 (8.1 g). The obtained dark brown solid 2 was combined with the above dark brown solid 1 and purified by column chromatography (SiO2 = 240 g, heptane / toluene = 2 / 1 → 1 / 1 → 1 / 2) to obtain compound 1 (6.24 g, 18.1 mmol, 76%) represented by formula (7-3) as a colorless solid.
[0127] Under an argon atmosphere, a 500 mL reactor was charged with a 28% solution of NaOCH3 in CH3OH (73.4 g, 381 mmol, 20 eq.) and anhydrous DMF (125 mL). Compound 3 (10.4 g, 19.0 mmol, 1.0 eq. containing diiodo form) represented by formula (7-2) and copper (I) iodide (7.2 g, 38.1 mmol, 2.0 eq.) were added to this suspension. The temperature of this suspension was raised to 120°C and stirred at the same temperature for 5 hours. After cooling, the suspension was filtered through Celite, the filter bed was washed with ethyl acetate, and 5% aqueous ammonium chloride solution (480 mL) was added to the filtrate, and the mixture was separated into two layers. The aqueous layer was extracted with ethyl acetate (200 mL), and the organic layers were combined, washed with city water and saturated saline, dried over anhydrous sodium sulfate, filtered, and the filtrate was concentrated to obtain a dark brown solid 3 (8.1 g). The obtained dark brown solid 3 was combined with the above dark brown solid 1 and purified by column chromatography (SiO2 = 200 g, heptane / toluene = 2 / 1 → 1 / 1 → 1 / 2) to obtain compound 2 (5.92 g, 17.1 mmol, 90%) represented by formula (7-3) as a colorless solid.
[0128] "Synthesis process of the compound represented by formula (7-4)" In an argon atmosphere, compound 1 (1.0 g, 2.89 mmol, 1.0 eq.) represented by formula (7-3), calcium carbonate (0.289 g, 2.89 mmol, 1.0 eq.), dehydrated dichloromethane (50 mL), and dehydrated methanol (20 mL) were added to a 300 mL reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (1.2 g, 3.47 mmol, 1.2 eq.) was added to the vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 3 hours. The reddish-brown suspension was filtered through Celite, the filter bed was washed with ethyl acetate, the filtrate was concentrated, and an aqueous sodium hydrosulfide solution (5%) (20 mL) and ethyl acetate (50 mL) were added to the residue, and the mixture was stirred for 10 minutes, after which it was separated into two layers. The aqueous layer was extracted with ethyl acetate (25 mL), and the organic layers were combined, washed with tap water and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (1.69 g, wet.). This was purified by column purification (SiO2 = 30 g, heptane / toluene = 1 / 2 → toluene only) to obtain compound 1 (1.29 g, 2.74 mmol, 94%) represented by formula (7-4) as a colorless solid.
[0129] In an argon atmosphere, compound 1 (5.24 g, 15.2 mmol, 1.0 eq.) represented by formula (7-3), calcium carbonate (1.97 g, 19.7 mmol, 1.0 eq.), dehydrated dichloromethane (262 mL), and dehydrated methanol (105 mL) were added to a 1 L reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (6.34 g, 18.2 mmol, 1.2 eq.) was added to the vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 4.5 hours. The reddish brown suspension was filtered through Celite, the filter bed was washed with ethyl acetate, the filtrate was concentrated, and an aqueous sodium hydrosulfide solution (5%) (200 mL) and ethyl acetate (200 mL) were added to the residue, and the mixture was stirred for 10 minutes, after which it was separated into two layers. The aqueous layer was extracted with ethyl acetate (100 mL), and the organic layers were combined, washed with tap water and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (7.4 g, wet.), which was purified with a column (SiO2=225 g, heptane / toluene=1 / 1→1 / 2) to obtain compound 2 (6.35 g, 13.5 mmol, 88%) represented by formula (7-4) as a colorless solid.
[0130] In an argon atmosphere, a mixture of compound 1 represented by formula (7-3) and compound 2 represented by formula (7-3) (6.26 g, 18.1 mmol, 1.0 eq.), calcium carbonate (2.72 g, 27.2 mmol, 1.0 eq.), dehydrated dichloromethane (313 mL), and dehydrated methanol (125 mL) were added to a 1 L reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (6.94 g, 19.9 mmol, 1.1 eq.) was added to this vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 6 hours. The reddish brown suspension was filtered through Celite, the filter bed was washed with ethyl acetate, the filtrate was concentrated, and an aqueous sodium hydrosulfide solution (5%) (250 mL) and ethyl acetate (250 mL) were added to the residue, and the mixture was stirred for 10 minutes, after which it was separated into two layers. The aqueous layer was extracted with ethyl acetate (150 mL), and the organic layers were combined, washed with tap water and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (8.14 g, wet.). This was purified by column purification (SiO2 = 200 g, heptane / toluene = 1 / 1 → 1 / 2) to obtain compound 3 (7.51 g, 15.9 mmol, 87%) represented by formula (7-4) as a colorless solid.
[0131] "Synthesis process of the compound represented by formula (7-5)" In an argon atmosphere, compound 1 (1.2 g, 2.55 mmol, 1.0 eq.) represented by formula (7-4) and THF (15 mL) were added to a 50 mL reactor and cooled to -78°C. n-BuLi (1.59 mol / L hexane solution) (1.92 mL, 3.06 mmol, 1.2 eq.) was added to this solution and stirred at the same temperature for 30 minutes. Isopropoxypinacolborane (0.71 g, 3.82 mmol, 1.5 eq.) diluted with THF (1 mL) was added at once to this solution and stirred at the same temperature for 15 minutes, after which the cooling bath was removed and the temperature was raised to room temperature. City water was added to this solution, and the solution was separated into two layers. The aqueous layer was extracted with ethyl acetate (20 mL), and the organic layers were combined, washed with city water and saturated saline in that order, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (1.71 g). This was purified by column chromatography (SiO2 = 50 g, toluene only) to obtain compound 1 (0.67 g, 1.42 mmol, 55%) represented by formula (7-5) as a colorless solid.
[0132] In an argon atmosphere, compound 2 (4.35 g, 9.23 mmol, 1.0 eq.) represented by formula (7-4) and THF (50 mL) were added to a 200 mL reactor and cooled to -78°C. n-BuLi (1.59 mol / L hexane solution) (7.55 mL, 12.0 mmol, 1.3 eq.) was added to this solution and stirred at the same temperature for 30 minutes. Isopropoxypinacolborane (2.58 g, 13.8 mmol, 1.5 eq.) diluted with THF (3 mL) was added at once to this solution and stirred at the same temperature for 15 minutes, after which the cooling bath was removed and the temperature was raised to room temperature. City water was added to this solution, and the solution was separated into two layers. The aqueous layer was extracted with ethyl acetate (50 mL), and the organic layers were combined, washed with city water and saturated saline solution in that order, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (4.15 g). This was purified by column chromatography (SiO2 = 125 g, heptane / toluene = 1 / 1 → 1 / 2) to obtain compound 2 (3.0 g, 6.36 mmol, 68%) represented by formula (7-5) as a colorless solid.
[0133] In an argon atmosphere, compound 3 (6.0 g, 12.7 mmol, 1.0 eq.) represented by formula (7-4) and THF (70 mL) were added to a 200 mL reactor and cooled to -78°C. n-BuLi (1.59 mol / L hexane solution) (9.6 mL, 15.3 mmol, 1.2 eq.) was added to this solution and stirred at the same temperature for 30 minutes. Isopropoxypinacolborane (3.55 g, 19.1 mmol, 1.5 eq.) diluted with THF (7 mL) was added at once to this solution and stirred at the same temperature for 15 minutes, after which the cooling bath was removed and the temperature was raised to room temperature. City water was added to this solution, and the solution was separated into two layers. The aqueous layer was extracted with ethyl acetate (80 mL), and the organic layers were combined, washed with city water and saturated saline solution in that order, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (7.96 g). This was purified by column chromatography (SiO2 = 125 g, heptane / toluene = 1 / 1 → toluene only → toluene / ethyl acetate = 20 / 1) to obtain compound 3 (3.22 g, 6.83 mmol, 53%) represented by formula (7-5) as a colorless solid.
[0134] <Synthesis of dimethylacridine derivatives 1> According to the following reaction scheme, a dimethylacridine derivative represented by formula (2-1) was synthesized. [ka]
[0135] In an argon atmosphere, compound 2 (1.2 g, 2.54 mmol, 1.0 eq.) represented by formula (7-4), compound 1 (1.26 g, 2.67 mmol, 1.05 eq.) represented by formula (7-5), tripotassium phosphate (1.62 g, 7.64 mmol, 3.0 eq.), and degassed toluene (18 mL) were added to a 100 mL reactor. After degassing the suspension under reduced pressure, S-Phos (63 mg, 0.152 mmol, 0.06 eq.) and Pd2(dba)3 (35 mg, 0.0382 mmol, 0.015 eq.) were added, degassed again, and distilled water (0.1 mL) was added. The bath temperature was raised to 110°C and the mixture was heated and stirred for 24 hours. Toluene (40 mL) was added to this brown suspension, and after stirring at 50°C for 30 minutes, it was filtered through Celite, the filter bed was washed with toluene (50 mL), and the filtrate was concentrated to obtain a brown solid (3.15 g). This was purified through a column (SiO2 = 120 g, toluene / heptane = 1 / 1 → 1 / 2 → toluene only) to obtain a beige solid (1.2 g). Toluene (5 mL) was added to this and completely dissolved at 70°C, and then heptane (5 mL) and ethanol (3 mL) were slowly added in sequence, and the mixture was allowed to cool to room temperature. The precipitated solid was filtered, the filter bed was washed with ethanol, and the mixture was dried under high vacuum at 80°C to obtain the dimethylacridine derivative represented by formula (2-1) (0.83 g, 1.20 mmol, 47%, HPLC 99.3%). The product 1 The H-NMR spectrum is shown in Figure 5.
[0136] <Synthesis of dimethylacridine derivatives 2> According to the following reaction scheme, a dimethylacridine derivative represented by formula (3-1) was synthesized. [ka]
[0137] "Synthesis process of the compound represented by formula (7-6)" In an argon atmosphere, compound 3 (2.5 g, 7.92 mmol, 1.0 eq.) represented by formula (7-1), calcium carbonate (1.82 g, 18.2 mmol, 1.0 eq.), dehydrated dichloromethane (250 mL), and dehydrated methanol (100 mL) were added to a 300 mL reactor. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (6.34 g, 18.2 mmol, 2.3 eq.) was added to the vigorously stirred suspension at room temperature, and the mixture was stirred at the same temperature for 8 hours. The reddish-brown suspension was filtered through Celite, the filter bed was washed with dichloromethane, the filtrate was concentrated, and an aqueous solution of sodium hydrosulfide (3%) (100 mL) and toluene (100 mL) were added to the residue, and the mixture was stirred for 10 minutes, after which it was separated into two layers. The aqueous layer was extracted with ethyl acetate (50 mL), and the organic layers were combined and washed successively with saturated sodium bicarbonate water, tap water, and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (3.91 g, wet). This was completely dissolved in heated toluene, heptane was added, and the mixture was allowed to cool. The precipitated solid was filtered, the filter bed was washed with toluene, and dried under high vacuum at 80°C for 2 hours. 1 Analysis by H-NMR showed that it contained a large amount of monoiodide. This was added to a 200 mL reactor, and calcium carbonate (1.58 g, 15.8 mmol), dehydrated dichloromethane (200 mL), and dehydrated methanol (80 mL) were added. Benzyltrimethylammonium dichloroiodide (BTMA-ICl2) (4.13 g, 11.9 mmol) was added to this vigorously stirred suspension at room temperature, and the mixture was stirred at 40 °C for 4 hours. This reddish-brown suspension was filtered through Celite, the filter bed was washed with dichloromethane, the filtrate was concentrated, and an aqueous solution of sodium hydrosulfide (3%) (100 mL) and toluene (100 mL) were added to the residue, and the mixture was stirred for 10 minutes, and then separated into two layers. The aqueous layer was extracted with ethyl acetate (50 mL), and the organic layers were combined and washed successively with saturated sodium bicarbonate water, city water, and saturated saline, dried over anhydrous sodium sulfate, and concentrated to obtain a colorless solid (4.61 g, wet). This was recrystallized from heated toluene / heptane to obtain a colorless solid, the compound represented by formula (7-6) (4.28 g, 7.54 mmol, 95%, containing monoiodo form).
[0138] "Synthesis process of dimethylacridine derivative represented by formula (3-1)" In an argon atmosphere, a compound represented by formula (7-6) (1.0 g, 1.76 mmol, 1.0 eq.), compound 2 represented by formula (7-5) (1.99 g, 4.23 mmol, 2.4 eq.), tripotassium phosphate (2.24 g, 10.6 mmol, 6.0 eq.), and degassed toluene (20 mL) were added to a 100 mL reactor. After degassing the suspension under reduced pressure, S-Phos (87 mg, 0.212 mmol, 0.12 eq.) and Pd2(dba)3 (16 mg, 0.0705 mmol, 0.04 eq.) were added, degassed again, and distilled water (0.2 mL) was added. The bath temperature was raised to 110 °C and the mixture was heated and stirred for 12 hours. Toluene (40 mL) was added to this brown suspension, and the mixture was stirred at 50°C for 30 minutes. The mixture was then filtered through Celite, the filter bed was washed with toluene (20 mL), and the filtrate was concentrated to obtain a brown solid (3.71 g). This was purified through a column (SiO2 = 120 g, toluene / heptane = 1 / 1 → 1 / 2 → toluene only) to obtain a beige solid (0.81 g). This was purified again through a column (NH-SiO2 = 70 g, toluene / heptane = 1 / 1 → 1 / 2) to obtain a beige solid (0.56 g). Toluene (3 mL) was added to this, and the mixture was completely dissolved at 70°C, after which ethanol (1.5 mL) was slowly added and the mixture was allowed to cool to room temperature. The precipitated solid was filtered, the filter bed was washed with ethanol, and the mixture was dried under high vacuum at 80°C to obtain the dimethylacridine derivative represented by formula (3-1) (0.47 g, 0.469 mmol, 26%). The product 1 The H-NMR spectrum is shown in Figure 6.
[0139] <Synthesis of dimethylacridine derivatives 3> According to the following reaction scheme, a dimethylacridine derivative represented by formula (4-1) was synthesized. [ka]
[0140] In an argon atmosphere, 3,7-dibromo-10-phenyl-10H-phenoxazine (0.635 g, 1.52 mmol, 1.0 eq.), compound 3 represented by formula (7-5) (1.58 g, 3.35 mmol, 2.2 eq.), tripotassium phosphate (1.62 g, 7.62 mmol, 5.0 eq.), and degassed toluene (30 mL) were added to a 100 mL reactor. After degassing the suspension under reduced pressure, S-Phos (125 mg, 0.305 mmol, 0.20 eq.) and Pd2(dba)3 (98 mg, 0.107 mmol, 0.07 eq.) were added, degassed again, and distilled water (0.3 mL) was added. The bath temperature was raised to 110°C, and the mixture was heated and stirred for 12 hours. Toluene (30 mL) was added to this brown suspension, and after stirring at 50°C for 30 minutes, it was filtered through Celite, the filter bed was washed with toluene (20 mL), and the filtrate was concentrated to obtain a brown solid (2.41 g). This was purified through a column (SiO2 = 70 g, toluene / heptane = 1 / 2 → toluene only) to obtain a beige solid (1.05 g). Toluene (5 mL) was added to this and completely dissolved at 80°C, after which ethanol (5 mL) was slowly added and the mixture was allowed to cool to room temperature. The precipitated solid was filtered, the filter bed was washed with ethanol, and the mixture was dried under high vacuum at 60°C to obtain the dimethylacridine derivative represented by formula (4-1) (0.78 g, 0.824 mmol, 54%). The product 1 The H-NMR spectrum is shown in Figure 7.
[0141] "Example 1" (Fabrication of organic EL elements) An organic EL device 1 having the structure shown in FIG. 1 was produced by the method described below and evaluated.
[0142] [Process 1] As the substrate 2, a commercially available transparent glass substrate having an average thickness of 0.7 mm and having an electrode (anode 3) patterned with ITO to a width of 3 mm was prepared. Then, the surface of the substrate 2 having the anode 3 was thoroughly washed with an organic solvent, and then subjected to UV ozone cleaning for 20 minutes.
[0143] [Process 2] The substrate 2 on which the anode 3 cleaned in [Step 1] was formed was set on a spin coater, and a hole injection material "Clevios HIL 1.3N" manufactured by Heraeus was applied as a hole injection layer 4, followed by heat treatment in the atmosphere to form a hole injection layer 4 of 10 nm.
[0144] [Process 3] Next, the substrate 2 on which each layer up to the hole injection layer 4 had been formed was fixed to a substrate holder of a vacuum deposition apparatus. -5 The pressure was reduced to 100 Pa. First, a dimethylacridine derivative represented by the above formula (2-1) and NDP-9, a p-type dopant from Novaled, were deposited in a mass ratio of 9:1 to form a hole transport layer 5 on the hole injection layer 4 to a thickness of 30 nm, and then a dimethylacridine derivative represented by the above formula (2-1) was deposited to a thickness of 10 nm. The ionization potential (IP) of the dimethylacridine derivative represented by the above formula (2-1) used in the hole transport layer 5 was calculated to be 4.18 eV using a density functional theory method.
[0145] Furthermore, the light-emitting layer 6 may further comprise a compound represented by the following structural formula (8-1): [ka] A film was formed by depositing a 50 nm thick anthracene derivative represented by the structural formula (8-1) above in the light-emitting layer 6. The electron affinity (EA) of the anthracene derivative represented by the structural formula (8-1) above used in the light-emitting layer 6 was calculated to be 2.73 eV using density functional theory, and was actually measured to be 2.89 eV using low-energy inverse photoemission spectroscopy (LEIPS).
[0146] The anthracene derivative of the structural formula (8-1) was synthesized as follows. First, isophthalic acid is used as a starting material, and the isophthalic acid is brominated with N-bromosuccinimide (NBS) to synthesize 5-bromoisophthalic acid. Next, the carboxyl group of 5-bromoisophthalic acid is chlorinated with thionyl chloride to obtain a carboxylic acid chloride (acid chloride), which is amidated with t-butylamine to obtain an amide compound, and the amide compound is nitrified with thionyl chloride to synthesize 5-bromoisophthalonitrile. Next, bis(pinacolato)diboron is reacted with 5-bromoisophthalonitrile to introduce a pinacolatoboryl group, and 3,5-dicyanophenylboronic acid pinacol ester is obtained. On the other hand, 2,6-dichloro-4-iodopyridine is used as a starting material and subjected to Suzuki coupling with 9-anthraceneboronic acid to give 9-(2,6-dichloro-4-pyridyl)anthracene, which is then brominated at the 10-position with N-bromosuccinimide (NBS) to give 9-(2,6-dichloro-4-pyridyl)-10-bromoanthracene. The anthracene derivative of structural formula (8-1) was synthesized by Suzuki coupling of the 3,5-dicyanophenylboronic acid pinacol ester obtained as described above with 9-(2,6-dichloro-4-pyridyl)-10-bromoanthracene.
[0147] After the light-emitting layer 6 was formed, a compound represented by the following structural formula (5-1) was deposited to a thickness of 3 nm as the electron-injection layer 7. [ka] The compound represented by the above structural formula (5-1) was synthesized according to the method described in T. Sasaki, M. Hasegawa, K. Inagaki, H. Ito, K. Suzuki, T. Oono, K. Morii, T. Shimizu and H. Fukagawa, Nature Communications, 12, pp. 2706.1, DOI: 10.1038 / s41467-021-23067-2.
[0148] Next, a cathode 8 made of aluminum and having a thickness of 100 nm was formed by vacuum deposition on the substrate 2 on which the electron injection layer 7 had been formed. The cathode 8 was formed using a stainless steel deposition mask so that the deposition surface would be in the shape of a strip with a width of 3 mm, and the light-emitting area of the fabricated organic EL element was 9 mm 2 It was decided.
[0149] [Step 4] Next, the substrate 2 on which each layer up to the cathode 8 was formed was placed in a glass cap (sealing container) having a concave space, and sealed by filling it with a sealant made of an ultraviolet (UV) curable resin, thereby obtaining the organic EL element of Example 1.
[0150] "Comparative Example 1" The hole transport layer 5 is formed of a material having the following structural formula: [ka] TPDI (calculated ionization potential (IP) calculated using density functional theory = 4.66 eV) and NDP-9, a p-type dopant from Novaled, were evaporated to a thickness of 30 nm in a mass ratio of 9:1, and then TPDI was evaporated to a thickness of 10 nm.
[0151] As the light-emitting layer 6, the same anthracene derivative as in Example 1 was vapor-deposited to a thickness of 40 nm.
[0152] An organic EL element of Comparative Example 1 was produced in the same manner as in Example 1, except for the hole transport layer 5 and the light emitting layer 6 .
[0153] (Evaluation of organic EL element characteristics) Voltage was applied to the thus obtained elements of Example 1 and Comparative Example 1 using a Keithley 2400 Source Meter, and the luminance was measured using a Konica Minolta LS-100 to examine the relationship between the applied voltage and the luminance, and the relationship between the applied voltage and the current density. These results are shown in FIG.
[0154] FIG. 8(a) shows the applied voltage-current density characteristics of Example 1 and Comparative Example 1. A rise in current was observed at a lower applied voltage in Example 1 than in Comparative Example 1. This is because the ionization potential of the material used in the hole transport layer 5, the dimethylacridine derivative represented by the above formula (2-1), is smaller than that of TPDI.
[0155] FIG. 8(b) shows the applied voltage-luminance characteristics of Example 1 and Comparative Example 1. As shown in FIG. 8(b), in Example 1, light emission is obtained at a lower applied voltage than in Comparative Example 1. In particular, in Example 1, the rise of the applied voltage is excellent, and further improvements in brightness and efficiency can be expected by combining a highly efficient light-emitting dopant. These excellent characteristics are believed to be due to the fact that, as shown in FIGS. 2 and 3, an exciplex is formed between the dimethylacridine derivative of the present invention, which has a small ionization potential, and an acceptor material, which has a large electron affinity, and the energy of the exciplex can be extracted as light emission.
[0156] "Example 2" (Fabrication of organic EL elements) An organic EL device 1 having the structure shown in FIG. 1 was produced by the method described below and evaluated.
[0157] [Process 1] As the substrate 2, a commercially available transparent glass substrate having an average thickness of 0.7 mm and having an electrode (anode 3) patterned with ITO to a width of 3 mm was prepared. Then, the surface of the substrate 2 having the anode 3 was thoroughly washed with an organic solvent, and then subjected to UV ozone cleaning for 20 minutes.
[0158] [Process 2] The substrate 2 on which the anode 3 cleaned in [Step 1] was formed was set on a spin coater, and a hole injection material "Clevios HIL 1.3N" manufactured by Heraeus was applied as a hole injection layer 4, followed by heat treatment in the atmosphere to form a hole injection layer 4 of 10 nm.
[0159] [Process 3] Next, the substrate 2 on which each layer up to the hole injection layer 4 had been formed was fixed to a substrate holder of a vacuum deposition apparatus. -5 The pressure was reduced to 100 Pa. First, a dimethylacridine derivative represented by the above formula (3-1) and NDP-9, a p-type dopant from Novaled, were deposited in a mass ratio of 9:1 to form a hole transport layer 5 on the hole injection layer 4 to a thickness of 20 nm, and then a dimethylacridine derivative represented by the above formula (3-1) was deposited to a thickness of 10 nm. The ionization potential (IP) of the dimethylacridine derivative represented by the above formula (3-1) used in the hole transport layer 5, calculated using a density functional theory method, is 4.17 eV.
[0160] Furthermore, as the light-emitting layer 6, a film of the anthracene derivative represented by the above structural formula (8-1) was vapor-deposited to a thickness of 40 nm.
[0161] After the light-emitting layer 6 was formed, the compound represented by the above structural formula (5-1) was deposited to a thickness of 3 nm as the electron-injection layer 7.
[0162] Next, a cathode 8 made of aluminum and having a thickness of 100 nm was formed by vacuum deposition on the substrate 2 on which the electron injection layer 7 had been formed. The cathode 8 was formed using a stainless steel deposition mask so that the deposition surface would be in the shape of a strip with a width of 3 mm, and the light-emitting area of the fabricated organic EL element was 9 mm 2 It was decided.
[0163] [Step 4] Next, the substrate 2 on which each layer up to the cathode 8 was formed was placed in a glass cap (sealing container) having a concave space, and sealed by filling it with a sealant made of an ultraviolet (UV) curable resin, thereby obtaining the organic EL element of Example 2.
[0164] (Evaluation of organic EL element characteristics) Voltage was applied to the element of Example 2 thus obtained using a Keithley 2400 Source Meter, and the luminance was measured using a Konica Minolta LS-100 to examine the relationship between the applied voltage and the luminance, and the relationship between the applied voltage and the current density. These results are shown in FIG. 9. For comparison, the results of the element of Comparative Example 1 are also shown in FIG. 9.
[0165] FIG. 9(a) shows the applied voltage-current density characteristics of Example 2 and Comparative Example 1. A current rise was observed at a lower applied voltage in Example 2 than in Comparative Example 1. This is because the ionization potential of the material used in the hole transport layer 5, the dimethylacridine derivative represented by the above formula (3-1), is smaller than that of TPDI.
[0166] FIG. 9(b) shows the applied voltage-luminance characteristics of Example 2 and Comparative Example 1. As shown in Figure 9(b), in Example 2, the luminance at 1.9 V or higher was inferior to that of Comparative Example 1, but the applied voltage rise and ease of current flow were excellent, so it is believed that the luminance characteristics can be improved sufficiently by combining it with a highly efficient light-emitting dopant. These excellent characteristics can be attributed to the fact that, as shown in Figures 2 and 3, an exciplex is formed between the dimethylacridine derivative of the present invention, which has a small ionization potential, and an acceptor material, which has a large electron affinity, and the energy of the exciplex can be extracted as light emission.
[0167] "Example 3" (Fabrication of organic EL elements) An organic EL device 1 having the structure shown in FIG. 1 was produced by the method described below and evaluated.
[0168] [Process 1] As the substrate 2, a commercially available transparent glass substrate having an average thickness of 0.7 mm and having an electrode (anode 3) patterned with ITO to a width of 3 mm was prepared. Then, the surface of the substrate 2 having the anode 3 was thoroughly washed with an organic solvent, and then subjected to UV ozone cleaning for 20 minutes.
[0169] [Process 2] The substrate 2 on which the anode 3 cleaned in [Step 1] was formed was set on a spin coater, and a hole injection material "Clevios HIL 1.3N" manufactured by Heraeus was applied as a hole injection layer 4, followed by heat treatment in the atmosphere to form a hole injection layer 4 of 10 nm.
[0170] [Process 3] Next, the substrate 2 on which each layer up to the hole injection layer 4 had been formed was fixed to a substrate holder of a vacuum deposition apparatus. -5 The pressure was reduced to 100 Pa. First, a dimethylacridine derivative represented by the above formula (4-1) and NDP-9, a p-type dopant from Novaled, were deposited in a mass ratio of 9:1 to form a hole transport layer 5 on the hole injection layer 4 to a thickness of 30 nm, and then a dimethylacridine derivative represented by the above formula (4-1) was deposited to a thickness of 10 nm. The ionization potential (IP) of the dimethylacridine derivative represented by the above formula (4-1) used in the hole transport layer 5, calculated using a density functional theory method, is 4.11 eV.
[0171] Furthermore, as the light-emitting layer 6, a film of the anthracene derivative represented by the above structural formula (8-1) was vapor-deposited to a thickness of 40 nm.
[0172] After the light-emitting layer 6 was formed, the compound represented by the above structural formula (5-1) was deposited to a thickness of 3 nm as the electron-injection layer 7.
[0173] Next, a cathode 8 made of aluminum and having a thickness of 100 nm was formed by vacuum deposition on the substrate 2 on which the electron injection layer 7 had been formed. The cathode 8 was formed using a stainless steel deposition mask so that the deposition surface would be in the shape of a strip with a width of 3 mm, and the light-emitting area of the fabricated organic EL element was 9 mm 2 It was decided.
[0174] [Step 4] Next, the substrate 2 on which each layer up to the cathode 8 was formed was placed in a glass cap (sealing container) having a concave space, and sealed by filling it with a sealant made of an ultraviolet (UV) curable resin, thereby obtaining the organic EL element of Example 3.
[0175] (Evaluation of organic EL element characteristics) Voltage was applied to the element of Example 3 thus obtained using a Keithley 2400 Source Meter, and the luminance was measured using a Konica Minolta LS-100 to examine the relationship between the applied voltage and the luminance, and the relationship between the applied voltage and the current density. These results are shown in FIG. 10. For comparison, the results of the element of Comparative Example 1 are also shown in FIG. 10.
[0176] FIG. 10(a) shows the applied voltage-current density characteristics of Example 3 and Comparative Example 1. A current rise was observed at a lower applied voltage in Example 3 than in Comparative Example 1. This is because the ionization potential of the material used in the hole transport layer 5, the dimethylacridine derivative represented by the above formula (4-1), is smaller than that of TPDI.
[0177] FIG. 10(b) shows the applied voltage-luminance characteristics of Example 3 and Comparative Example 1. As shown in FIG. 10(b), in Example 3, light emission is obtained at a lower applied voltage than in Comparative Example 1. In particular, in Example 3, the rise of the applied voltage is excellent, and further improvements in brightness and efficiency can be expected by combining a highly efficient light-emitting dopant. These excellent characteristics are believed to be due to the fact that, as shown in FIGS. 2 and 3, an exciplex is formed between the dimethylacridine derivative of the present invention, which has a small ionization potential, and an acceptor material, which has a large electron affinity, and the energy of the exciplex can be extracted as light emission. [Industrial Applicability]
[0178] The dimethylacridine derivative of the present invention can be used to form a light-emitting device such as an organic EL device. [Explanation of symbols]
[0179] 1: Organic EL element 2: Substrate 3:Anode 4: Hole injection layer 5: Hole transport layer 6: Light-emitting layer 7:Electron injection layer 8: Cathode
Claims
1. The following general formula (1): 【Chemistry 1】 [In general formula (1), X 1 One of X is a methoxy group. 2 Any one of X is a methoxy group, and the other X 1 and X 2 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, A is C(CH 3 ) 2 or O, R' is hydrogen, or an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, or a group represented by the following general formula (1-1): 【Chemistry 2】 (In general formula (1-1), X 3 One of X is a methoxy group. 4 Any one of X is a methoxy group, and the other X 3 and X 4 are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, adjacent substituents may be taken together to form a ring, * represents a bond, In general formulas (1) and (1-1), R each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
2. The following general formula (2): 【Chemistry 3】 [In general formula (2), X 1 One of X is a methoxy group. 2 One of X is a methoxy group. 5 One of X is a methoxy group. 6 Any one of X is a methoxy group, and the other X 1 , X 2 , X 5 and X 6 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R's are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
3. The following general formula (3): 【Chemistry 4】 [In general formula (3), X 1 One of X is a methoxy group. 2 One of X is a methoxy group. 3 One of X is a methoxy group. 4 One of X is a methoxy group. 5 Any one of X is a methoxy group, and the other X 1 , X 2 , X 3 , X 4 and X 5 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R's are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
4. The following general formula (4): 【Chemistry 5】 [In general formula (4), X 1 One of X is a methoxy group. 2 One of X is a methoxy group. 3 One of X is a methoxy group. 4 Any one of X is a methoxy group, and the other X 1 , X 2 , X 3 and X 4 each independently represents hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 2 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, wherein adjacent substituents may be joined together to form a ring, R's are each independently hydrogen or a monovalent substituent selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, an acyl group having 2 to 10 carbon atoms, an aralkyl group having 7 to 20 carbon atoms, a substituted or unsubstituted aromatic hydrocarbon group having 6 to 30 carbon atoms, and a substituted or unsubstituted aromatic 6-membered heterocyclic group having 3 to 30 carbon atoms, and adjacent substituents may be joined together to form a ring.
5. The device comprises an anode, a hole transport layer, a light emitting layer, and a cathode, in this order; the hole transport layer comprises a first organic compound which is a donor material having a small ionization potential; the light-emitting layer includes a second organic compound which is an acceptor material having a large electron affinity; An organic electroluminescence device, in which an exciplex is formed between the first organic compound and the second organic compound, 2. An organic electroluminescence device, wherein the first organic compound is the dimethylacridine derivative according to claim 1.
6. 6. The organic electroluminescence device according to claim 5, wherein the first organic compound has an ionization potential (IP) calculated by density functional theory of 4.5 eV or less.
7. The organic electroluminescence device according to claim 5, wherein the second organic compound has a calculated electron affinity (EA) of 2.1 eV or more as calculated using a density functional theory method, or a measured electron affinity (EA) of 2.8 eV or more as measured by low-energy inverse photoelectron spectroscopy.
8. A display device comprising the organic electroluminescence element according to claim 5.