Electrode of non-aqueous electrolyte secondary battery and method for manufacturing the same

The use of controlled application of silicate or phosphate inorganic binders addresses adhesion issues in non-aqueous electrolyte secondary batteries, enhancing cycle characteristics and energy density by integrating the active material and inorganic binder for improved mechanical strength.

JP2024139287AActive Publication Date: 2024-10-09OSAKA RES INST OF IND SCI & TECH +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023050161
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries face challenges in maintaining sufficient adhesion between the inorganic binder and the active material, particularly in electrodes with thicker or higher density active material layers, leading to issues such as swelling, peeling, or cracking, which affect cycle characteristics and energy density.

Method used

A manufacturing method involving the use of an inorganic binder solution composed of specific silicates or phosphates, applied under controlled conditions of temperature, pressure, and time, to enhance adhesion and distribution within the active material layer, forming a modified material that integrates the active material and inorganic binder for improved mechanical strength and cycle characteristics.

Benefits of technology

The method significantly improves cycle characteristics and energy density by ensuring strong bonding between the inorganic binder and active material, even in thicker or denser electrodes, resulting in electrodes with high strength and stable performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139287000001
    Figure 2024139287000001
  • Figure 2024139287000002
    Figure 2024139287000002
  • Figure 2024139287000003
    Figure 2024139287000003
Patent Text Reader

Abstract

To propose a method for manufacturing an electrode which can greatly improve cycle characteristics even if the electrode is hard to sufficiently secure adhesion between an inorganic binder composed of a silicate and a phosphate and an active substance, or the electrode has an active substance layer having large film thickness and high density.SOLUTION: A method for manufacturing an electrode of a non-aqueous electrolyte secondary battery includes a step A of coating a current collector with a slurry containing an active substance and a resin binder or filling the current collector with the slurry, drying it, and manufacturing an active substance layer, and a step B of immersing the active substance layer in an inorganic binder aqueous solution having a temperature of 30°C or higher and 120°C or lower or coating the active substance layer with the inorganic binder aqueous solution, drying it, and manufacturing an electrode. The inorganic binder aqueous solution is a silicate aqueous solution or a phosphate aqueous solution. The silicate aqueous solution is a liquid in which silicate represented by A2O nSiO2 is dissolved in water; A is at least one kind of Li, Na and K; n is 1.7 or more and 5 or less. The phosphate aqueous solution is a liquid in which phosphate represented by Al2O3 nP2O5 is dissolved in water, and n is 1.7 or more and 5 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode for a non-aqueous electrolyte secondary battery and a method for producing the same. [Background technology]

[0002] Secondary batteries are being used in a wide range of applications, from electronic devices to automobiles and large-scale power storage systems, and the market is expected to grow to a scale of over 10 trillion yen. They have already become extremely popular in information and communication devices such as smartphones and tablet terminals.

[0003] In addition, the range of applications of secondary batteries is expanding to include power sources for next-generation automobiles, such as electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs). Secondary batteries are also being used for home backup power sources, natural energy storage, load leveling, etc. In this way, secondary batteries are also indispensable in the introduction of energy-saving and new energy technologies.

[0004] Conventional secondary batteries have mainly been storage batteries that contain water in the electrolyte, such as lead-acid batteries, nickel-cadmium batteries, and nickel-hydrogen batteries, but in recent years, the use of non-aqueous electrolyte secondary batteries has increased due to their characteristics of small size, light weight, high voltage, and no memory effect. A non-aqueous electrolyte secondary battery is a general term for a battery system that uses an electrolyte that does not contain water as a main component and is also a chargeable and dischargeable electricity storage device.

[0005] For example, known non-aqueous electrolyte secondary batteries include lithium ion batteries, lithium polymer batteries, all-solid-state lithium batteries, lithium air batteries, lithium sulfur batteries, sodium ion batteries, sodium sulfur batteries, potassium ion batteries, multivalent ion batteries, and fluoride ion batteries. The non-aqueous electrolyte secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, a battery case (storage case), etc. In addition, when the electrolyte has fluidity, a separator is further interposed between the positive electrode and the negative electrode.

[0006] Electrodes such as positive and negative electrodes are composed of an active material, a conductive assistant, a resin-based binder, and a current collector. In general, electrodes are manufactured by mixing the active material, the conductive assistant, and the resin-based binder in a solvent to form a slurry, applying this to a current collector and drying it to form an active material layer, and then adjusting the pressure with a roll press or the like.

[0007] However, in the non-aqueous electrolyte secondary battery, there is a demand for improving the battery life (cycle characteristics). In view of this, Patent Documents 1 to 3 and Non-Patent Document 1 disclose a technique in which a skeleton-forming agent containing a silicate having a siloxane bond is present at least on the surface of the active material layer, and the skeleton-forming agent is allowed to penetrate from the surface to the inside. According to these techniques, a strong inorganic skeleton can be formed in the active material layer, which is said to improve the cycle characteristics.

[0008] The degree of the effect of the skeletal former on improving cycle characteristics varies depending on the type of active material, and the skeletal former and the active material have compatibility. For example, Non-Patent Document 1 shows the results of comparing the cycle characteristics of a silicon (Si) electrode and a silicon oxide (SiO) electrode coated with the skeletal former (described as an inorganic binder in the document) with an electrode not coated with the skeletal former. It is shown that the Si electrode has a significant improvement in cycle characteristics due to the provision of the skeletal former, whereas the SiO electrode has an improvement in cycle characteristics due to the provision of the skeletal former, but the improvement effect is smaller than that of the Si electrode.

[0009] Furthermore, there is a demand for improving the energy density of the non-aqueous electrolyte secondary battery, and it is believed that increasing the thickness of the active material layer or increasing the density of the active material layer is effective in improving the energy density.

[0010] Therefore, the present inventors have investigated an electrode and a manufacturing method thereof that further improves cycle characteristics and energy density by using an inorganic binder aqueous solution containing silicate or phosphate, and have completed the present invention. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Japanese Patent No. 6369818 [Patent Document 2] Japanese Patent No. 6149147 [Patent Document 3] Japanese Patent Application Publication No. 2021-144922 [Patent Document 4] Japanese Patent Application Publication No. 2021-144923 [Non-patent literature]

[0012] [Non-Patent Document 1] Makiko Takahashi, Tomohiro Kinoshita, Kiyoshi Tanaami, Shintaro Aoyagi, Takashi Mukai, Yuta Ikeuchi, Taichi Sakamoto, Naoto Yamashita: Abstracts of the 61st Battery Symposium, 1C15 (2020) Summary of the Invention [Problem to be solved by the invention]

[0013] In the techniques of Patent Documents 1 to 3 and Non-Patent Document 1, the adhesion between the skeletal former and the active material may be insufficient. In particular, in the case of an electrode containing an active material made of an oxide, the binding strength between the skeletal former and the active material is not sufficient, and swelling, peeling, and cracking of the active material layer occur, making it difficult to maintain a stable capacity. Therefore, even in the case of a battery using such an electrode, it is desired to realize a battery with excellent cycle characteristics.

[0014] Furthermore, in an electrode with a thicker active material layer or an electrode having a high-density active material layer, the aqueous inorganic binder solution is less likely to penetrate into the active material layer, which poses the problem of non-uniform distribution of the framework-forming agent in the active material layer.

[0015] The present invention has been made in view of the above, and an object of the present invention is to provide an electrode for a non-aqueous electrolyte secondary battery that can improve the cycle characteristics and energy density of the battery compared to conventional ones, and a method for manufacturing the same.

[0016] In other words, according to the method for manufacturing an electrode according to one embodiment of the present invention, it is possible to significantly improve the cycle characteristics even in an electrode in which it is difficult to ensure sufficient adhesion between the active material and an inorganic binder made of silicate or phosphate, or in an electrode in which the active material layer is thickened or densified.

[0017] There are many types of silicates, including polysilicates such as orthosilicate (A4SiO4), metasilicate (A2SiO3), pyrosilicate (A6Si2O7), disilicate (A2Si2O5), and tetrasilicate (A2Si4O9), as well as A2Si2O5, A2Si3O7, and A2Si4O9, and these are known to exist as hydrates.

[0018] However, not all silicates are applicable to the present invention. The inventors have examined various silicates and found that the present invention is highly effective when the silicate represented by the general formula A2O·nSiO2 satisfies the conditions that A is at least one of Li, Na, or K, and n is 1.7 to 5. The silicate represented by the general formula A2O·nSiO2 may be a hydrate, but it is preferable to remove as much water as possible when assembling a battery.

[0019] There are a wide variety of phosphates, including aluminum monophosphate (Al(H2PO4)3), aluminum hydrogen phosphate (Al2(H2PO2)3), aluminum metaphosphate (Al(PO3)3), magnesium monophosphate (Mg(H2PO4)3), magnesium hydrogen phosphate (MgHPO4), magnesium metaphosphate (Mg(PO3)2), calcium monophosphate (Ca(H2PO4)3), calcium hydrogen phosphate (CaHPO4), tricalcium phosphate (Ca3(H2PO4)2), and calcium metaphosphate (Ca(PO3)2), and these are known to exist as hydrates.

[0020] However, not all phosphates are applicable to the present invention. The inventors have examined various phosphates and found that the present invention is highly effective when the phosphate represented by the general formula Al2O3·nP2O5 satisfies the condition that n is 1.7 or more and 5 or less. The phosphate represented by the general formula Al2O3·nP2O5 may be a hydrate, but it is preferable to remove as much water as possible when assembling a battery.

[0021] The electrode is composed of at least an active material layer and a current collector. The active material layer can be produced by applying or filling a slurry containing an active material and a resin binder to a current collector and drying it. The active material layer thus obtained is preferably immersed in or applied to an aqueous inorganic binder solution obtained by dissolving a silicate or a phosphate in water, and then dried.

[0022] Here, in the case where the resin binder described later has a property of precipitating the binder components when it comes into contact with an acidic or alkaline aqueous solution, it is not necessary to provide a drying step after applying or filling the current collector with the slurry. However, since binder migration (resin segregation) is likely to occur when the binder components precipitate, it is preferable to dry the active material layer after applying or filling the current collector with the slurry, regardless of the resin binder used.

[0023] Here, drying means removing vaporized components (such as water and organic solvents) contained in the slurry by heating or reducing pressure to dry it. There are no particular limitations on the means for drying, and examples include drying using a heat source (heat drying, hot air drying, far-infrared drying, etc.) and drying under reduced pressure. When drying using a heat source, the temperature is preferably 50°C or higher and 400°C or lower. When drying under reduced pressure, it is preferable to reduce the pressure to an absolute pressure of 0.05 MPa or lower. Note that drying using a heat source and drying under reduced pressure may be combined.

[0024] The concentration of the inorganic binder aqueous solution is preferably 0.1% by mass or more and 35% by mass or less. If it is less than 0.1% by mass, the amount of inorganic binder that functions as a skeleton forming agent is reduced, and the effect of improving cycle characteristics is difficult to be achieved. Although it varies depending on the type of active material, it is preferable that the concentration is 0.1% by mass or more for the positive electrode and 3% by mass or more for the negative electrode. In any electrode, if the concentration exceeds 35% by mass, the viscosity is high, so the penetration speed is slow and the electrode is likely to be non-uniformly permeated with the inorganic binder. In addition, the concentration is more preferably 30% by mass or less, and desirably 25% by mass or less.

[0025] Furthermore, by setting the concentration of the inorganic binder aqueous solution to 0.1% by mass or more and 35% by mass or less, the inorganic binder can be easily adjusted to a range of 0.1% by mass or more and 30% by mass or less, assuming that the total amount of the active material layer is 100%. If the inorganic binder is less than 0.1% by mass, it is difficult to obtain the desired effect, and if it exceeds 35% by mass, the internal resistance becomes large.

[0026] The temperature of the inorganic binder aqueous solution is preferably 30° C. or higher and 120° C. or lower, and more preferably 40° C. or higher and 95° C. or lower. By setting the temperature at 30° C. or higher, even in an electrode containing an active material made of an oxide, sufficient binding strength between the inorganic binder and the active material can be obtained, and an electrode with excellent cycle characteristics can be obtained. However, if the temperature exceeds 120° C., the active material may be altered to the inside of the active material, which may lead to an increase in irreversible capacity, a decrease in reversible capacity, a decrease in cycle characteristics, an increase in internal resistance, and the like.

[0027] When contacting with the inorganic binder, the active material layer is preferably contacted with the inorganic binder aqueous solution for a period of 10 seconds to 5 hours, more preferably 30 seconds to 3 hours, and even more preferably 1 minute to 1 hour. The contact between the active material layer and the inorganic binder aqueous solution can be achieved by immersing the active material layer in the inorganic binder aqueous solution or by applying the inorganic binder aqueous solution to the active material layer.

[0028] When an active material layer is brought into contact with an inorganic binder aqueous solution at a temperature of less than 30°C and then heated and dried, the inorganic binder aqueous solution in the specified temperature range does not come into contact for 10 seconds or more, and drying is completed immediately, so that the contact time between the active material layer and the inorganic binder aqueous solution cannot be sufficiently secured.

[0029] By contacting for 10 seconds or more, the oxides on the surface of the active material are etched, and the exposed surface of the active material can be firmly bonded to the inorganic binder. However, if the contact time exceeds 5 hours, the active material may be altered, leading to an increase in irreversible capacity and a decrease in life characteristics, and some active materials may lose their functions.

[0030] In addition, it is preferable to reduce the pressure to an absolute pressure of 0.03 MPa (30 kPa) or less before contacting with the inorganic binder, and remove air and volatile components from within the active material layer. By releasing the reduced pressure while the active material layer is in contact with the aqueous inorganic binder solution, the aqueous inorganic binder solution can be uniformly filled into the voids in the active material layer. Even in an electrode with a thick active material layer or an electrode with a dense active material layer, the inorganic binder can be uniformly permeated to the surface of the current collector by reducing the pressure in advance.

[0031] For example, Patent Document 1 describes that it is preferable to contain a surfactant in order to uniformly penetrate the framework-forming agent from the surface to the inside of the active material layer, but this method can also make it unnecessary to add a surfactant or antifoaming agent.

[0032] In addition, after filling the inorganic binder solution, the filling speed can be increased by applying an absolute pressure of 0.12 MPa or more, which allows the active material surface and the inorganic binder to be firmly bonded. As the pressure is increased, the filling speed tends to increase, but if the pressure exceeds 10 MPa, valuable metals will be eluted from the active material and current collector, causing material deterioration. In addition, a pressure-resistant container will be required, making the equipment larger.

[0033] The electrodes used in secondary batteries include positive and negative electrodes. When an active material with a high equilibrium potential (nobler) is used, it becomes a positive electrode, and when an active material with a low equilibrium potential (baser) is used, it becomes a negative electrode.

[0034] In the case of the positive electrode, there is no particular limitation as long as the positive electrode active material is used in a non-aqueous electrolyte secondary battery. Known positive electrode active materials including transition metal oxide materials, vanadium materials, sulfur materials, solid solution materials (lithium excess, sodium excess, potassium excess) materials, carbon materials, organic materials, polyanion materials, etc. may be used.

[0035] For example, ANiO2, ANi 0.6 Co 0.2 Mn 0.2 O2, ANi 0.8 Co 0.1 Mn 0.1 O2, ANi 0.8 Co 0.15 Al 0.05 O2, ANi 0.88 Co 0.1 Al 0.02 O2 and other transition metal oxide-based materials, AV2O5, AVO2, A3VO4 and other vanadium-based materials, sulfur-based materials such as sulfur, carbon sulfide, polysulfide, polycarbon sulfide, sulfur-modified polyacrylonitrile, disulfide compounds, and metal sulfides, solid solution-based materials such as A2MnO3-ANiO2, A2MnO3-AMnO2, A2MnO3-ACoO2, A2MnO3-A(Ni,Mn)O2, A2MnO3-A(Ni,Co)O2, A2MnO3-A(Mn,Co)O2, A2MnO3-A(Ni,Mn,Co)O2, and other carbon-based materials such as graphite, soft carbon, hard carbon, and glassy carbon, quinone compounds, radialene compounds, tetracyaquinodimethane, and phenazine oxide, and other organic materials, AFePO4, AMnPO4, AFe 0.2 Mn 0.8 PO4, ANiPO4, ACoPO4, AVPO4, A3V2(PO4)3, A2FeSiO4, A2Fe 0.5 Mn 0.5 These are polyanionic materials such as SiO4, A2MnSiO4, A2CoSiO4, and A2NiSiO4.

[0036] Among these, a positive electrode active material containing at least an alkali metal and oxygen is preferable. Among these, a silicate-based material is preferable from the viewpoint of high capacity and stable cycle characteristics. The silicate-based material is represented by the general formula A 2-a M b S c O 4-d Here, A is at least one of Li, Na, and K, M is at least one of Fe, Ni, Mn, and Co, a is 0 to 2, b is 0.8 to 1, c is 0.8 to 1, and d is 0 to 0.2.

[0037] In order to stabilize the crystal structure of the silicate-based material or to increase the potential of the battery, the silicate-based material may be, for example, a compound in which a part of a transition metal element is replaced by another transition metal element, a compound in which a part of a silicon element is replaced by a phosphorus element or a boron element, or a compound in which a part of a chalcogen element is replaced by another chalcogen element. In this case, the substitution rate is preferably 20% or less in terms of element ratio.

[0038] A 2-a M b S c O 4-d Although the volume change caused by charge and discharge is smaller than that of Si or SiO, the conventional method of applying an inorganic binder tends to result in insufficient adhesion between the active material and the inorganic binder. However, the method of the present invention can improve the bonding between the inorganic binder and the active material even in the case of an oxide, and suppress deterioration of cycle characteristics.

[0039] In the case of a negative electrode, the material is not particularly limited as long as it is capable of reversibly absorbing and releasing alkali metal ions (lithium ions, sodium ions, potassium ions, etc.), for example, at least one element selected from the group consisting of C, Mg, Al, Si, P, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Nb, Mo, Pd, Ag, Cd, In, Sn, Sb, W, Pb, and Bi, or an alloy, composite, oxide, chalcogenide, or halide using these elements.

[0040] From the viewpoint of high capacity and stable cycle characteristics, silicon oxide is preferred. Silicon oxide is represented by the general formula SiO x The negative electrode active material is represented by the formula: It is believed that the bonding strength between the active material and the inorganic binder decreases as x increases (see, for example, Patent Document 4 and Non-Patent Document 1).

[0041] However, according to the method of the present invention, x is preferably 0.2 to 1.8, more preferably 0.22 to 1.2, and even more preferably 0.25 to 0.85. As x becomes smaller, the electrode has a higher capacity and a smaller irreversible capacity, but the volume change due to charging and discharging becomes larger. On the other hand, as x becomes larger, the electrode has excellent cycle characteristics, but when x exceeds 1.8, the binding between the inorganic binder and the active material becomes poor, the cycle characteristics deteriorate, and the electrode has a small capacity, a large resistance, and a large irreversible capacity.

[0042] Regardless of whether it is a positive electrode or a negative electrode, the active material has a median diameter (D 50 The particle size is preferably 0.01 μm or more and 50 μm or less. The shape of the active material particles is not particularly limited, and may be spherical, elliptical, faceted, strip-like, fibrous, flake-like, doughnut-like, or hollow.

[0043] The resin binder may be any binder that can be dissolved or dispersed in water or an organic solvent, and examples of such binders include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide, polyamideimide, polyacrylic, styrene butadiene rubber (SBR), ethylene-vinyl acetate copolymer (EVA), styrene-ethylene-butylene-styrene copolymer (SEBS), carboxymethyl cellulose (CMC), xanthan gum, polyvinyl alcohol (PVA), polyvinyl butyral (PVB), ethylene vinyl alcohol (EVOH), polyethylene (PE), polypropylene (PP), polyacrylic acid, lithium polyacrylate, sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, methyl polyacrylate, ethyl polyacrylate, amine polyacrylate, polya, etc. Organic materials such as acrylic acid esters, epoxy resins, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), nylon, vinyl chloride, silicone rubber, nitrile rubber, cyanoacrylate, urea resin, melamine resin, phenolic resin, latex, polyurethane, silylated urethane, nitrocellulose, dextrin, polyvinylpyrrolidone, vinyl acetate, polystyrene, chloropropylene, resorcinol resin, polyaromatic, modified silicone, methacrylic resin, polybutene, butyl rubber, 2-propenoic acid, cyanoacrylic acid, methyl methacrylate, glycidyl methacrylate, acrylic oligomer, 2-hydroxyethyl acrylate, polyacetal, alginic acid, starch, sucrose, lacquer, glue, casein, and cellulose nanofibers may be used alone or in combination of two or more kinds. Examples of the resin binder that has the property of precipitating the binder components when it comes into contact with the above-mentioned acidic or alkaline aqueous solution include PVdF, polyacrylic, SEBS, EVA, CMC, xanthan gum, PVA, EVOH, polyacrylic acid, and polyacrylic acid salts.

[0044] When the total amount of solids contained in the slurry is taken as 100%, the resin binder is preferably contained in an amount of 0.1% by mass to 30% by mass. A strong active material layer is obtained by permeating the active material layer with the inorganic binder aqueous solution and then removing the moisture by heating, but the active material layer before the moisture removal is more brittle than the active material layer after the moisture removal.

[0045] If the active material layer peels off or collapses when immersed in an aqueous solution of an inorganic binder, an electrode with a long life cannot be obtained, so the active material layer must have a minimum strength to maintain its shape even when immersed in an aqueous solution of an inorganic binder. For this reason, the inclusion of a resin binder is essential. However, if the content exceeds 30% by mass, not only will the inorganic binder be less likely to penetrate, but the energy density of the electrode will decrease.

[0046] As another method for forming an active material layer on a current collector, a gas phase method such as sputtering or vapor deposition is known. In the case of the gas phase method, even if a resin binder is not used, the active material layer is characterized in that it is difficult to peel off from the current collector. However, the active material layer is dense, and even if it is immersed in an inorganic binder aqueous solution using the manufacturing method of the present invention, the components do not penetrate to the vicinity of the current collector, and it is difficult to improve the cycle characteristics in a thick electrode. In order to realize a battery with high capacity and long life by immersing in an inorganic binder aqueous solution, it is preferable to form a porous active material layer consisting of an active material and a resin binder.

[0047] From the viewpoint of increasing the conductivity of the active material layer, it is preferable that the slurry further contains a conductive assistant. When the total amount of solids contained in the slurry is taken as 100%, it is preferable that the conductive assistant is contained in an amount of 0 mass% or more and 20 mass% or less. In other words, the conductive assistant is contained as necessary.

[0048] The conductive assistant is not particularly limited as long as it has electronic conductivity, and examples thereof include metals, carbon materials, conductive polymers, conductive glass, etc., but carbon materials are preferred from the viewpoint of high electronic conductivity and oxidation / reduction resistance. Specific examples include acetylene black (AB), Ketjen black (KB), furnace black (FB), thermal black, lamp black, channel black, roller black, disc black, carbon black (CB), carbon fiber (for example, vapor-grown carbon fiber named VGCF, a registered trademark), carbon nanotubes (CNT), carbon nanohorns, graphite, graphene, glassy carbon (for example, non-graphitized carbon named Glassy Carbon, a registered trademark), and amorphous carbon, and one or more of these may be used. It is preferable to use a combination of AB and VGCF, AB and CNT, AB and graphene, or CNT and graphene, because they have excellent electronic conductivity and further increase the mechanical strength of the active material layer.

[0049] The current collector used in the electrode may be any material that has electronic conductivity and can pass current through the active material it holds. In cases where the current collector does not collapse upon charging and discharging, aluminum or an aluminum alloy is preferred from the viewpoint of reducing the weight and cost of the electrode.

[0050] Here, aluminum means aluminum with an aluminum purity of 99% or more. Aluminum alloys include Al-Cu alloys, Al-Cu-Mg alloys, Al-Mn alloys, Al-Si alloys, Al-Mg alloys, Al-Mg-Si alloys, Al-Zn alloys, Al-Zn-Mg alloys, Al-Zn-Mg-Cu alloys, Al-Fe alloys, Al-Fe-Si alloys, Al-Fe-Mn alloys, and Al-Mg-Si-Fe alloys.

[0051] However, when lithium ions are used as the carrier and as the negative electrode, the material of the current collector is preferably copper, nickel, stainless steel, or carbon.

[0052] However, aluminum, being an amphoteric metal, will corrode or dissolve when it comes into contact with acid or alkali. However, there are exceptions where it will not react with certain silicate or phosphate solutions. In other words, in silicates with the general formula A2O·nSiO2, where A is at least one of Li, Na, or K, and n is 1.7 to 5, or in phosphates with the general formula Al2O3·nP2O5, where n is 1.7 to 5, the corrosion reaction will not proceed.

[0053] In the case of silicates, if n is less than 1.7, the pH value is 10 or more, and the corrosion inhibition effect on aluminum and aluminum alloys is not exhibited, but rather corrosion is promoted. If n exceeds 5, a gel-like film is likely to form in the drying process after slurry application, which is a factor in increasing the electrode resistance. In addition, if n exceeds 5, there are drawbacks in that the pot life is short, and if the silicate aqueous solution is left in the air, it becomes cloudy and precipitates, and is easily deteriorated. In addition, if n exceeds 5, the pH value is less than 10, and the reversible capacity of the active material decreases.

[0054] The shape of the current collector can be linear, rod-like, plate-like, foil-like, porous, or fibrous, among which porous or fibrous is preferable because it can increase the packing density and can suppress peeling of the active material layer in the process of permeating the active material layer with the inorganic binder. In addition, if the current collector is porous or fibrous, the amount of resin binder used can be reduced, and even if a resin binder with poor binding strength is used, peeling is difficult even when it comes into contact with an inorganic binder aqueous solution. In addition, there is also an effect that the inorganic binder aqueous solution can easily permeate the active material layer, and the distribution of the inorganic binder in the active material layer is likely to be uniform.

[0055] Examples of the porous form include mesh, woven fabric, nonwoven fabric, embossed body, punched body, expanded body, and foamed body, and among these, the shape of the current collector is preferably embossed or foamed body because of its good output characteristics. Furthermore, it is preferable that the current collector has through holes. The fibrous form may be a single fiber, or a bundle of multiple single fibers is also effective. Specifically, a bundle of 10 to 1000 single fibers having a diameter of 3 to 50 μm is preferable, and this may be used to form a woven fabric or nonwoven fabric.

[0056] The electrode thus obtained contains a modified material resulting from the reaction of the active material with a silicate or phosphate. This modified material exists at least between the active material and the inorganic binder, and has an intermediate function of firmly binding the active material and the inorganic binder. The presence of this modified material makes it possible to obtain an electrode in which the mechanical strength of the active material layer is high and peeling between the current collector and the active material layer is unlikely to occur.

[0057] The above-mentioned modified materials are produced by the reaction of the active material with a silicate or phosphate, and therefore if they are produced in excess, the active material loses its function and the electrode capacity decreases, whereas if the amount produced is insufficient, the mechanical strength of the active material layer decreases and peeling between the current collector and the active material layer is likely to occur.

[0058] The above modified materials differ between silicates and phosphates. When silicates are used, A2SiO3, A4SiO4, Na2Si2O5, Na2Si4O9, H2SiO3, SiO2, etc. are used, and when phosphates are used, AlPO4, Al(PO3)3, Al2P4O 13 , Al(H2PO4)3, H3PO4, PO 10 , Al2O3, etc., which may also include hydrates and low crystallinity states.

[0059] The specific gravity of the modified material is preferably in the range of 1.5 to 3.5, more preferably 1.8 to 3.2. If the specific gravity is less than 1.5, the material contains a large amount of water, which may cause early cycle deterioration of the battery and battery swelling. If the specific gravity is more than 3.5, it becomes difficult to improve the energy density per unit weight of the battery.

[0060] The thickness of the above-mentioned modifying material is preferably 1 nm or more and 500 nm or less. By keeping the thickness of the modifying material within this range, the binding property between the active material and the inorganic binder is improved. If the thickness is less than 1 nm, the mechanical strength of the active material layer is reduced and the active material layer is easily peeled off from the current collector, while if the thickness exceeds 500 nm, the function of the active material is lost, resulting in a decrease in the electrode capacity.

[0061] The electrode obtained by this manufacturing method can be used as a positive electrode or a negative electrode of a non-aqueous electrolyte secondary battery. A non-aqueous electrolyte secondary battery includes a positive electrode, a negative electrode, and a non-aqueous electrolyte interposed between the positive electrode and the negative electrode, and includes, for example, a lithium ion battery, a sodium ion battery, a potassium ion battery, a lithium ion capacitor, a sodium ion capacitor, and a potassium ion capacitor.

[0062] When this electrode is used as the positive electrode of a secondary battery, it can be combined with an electrode having a lower charge / discharge potential than the electrode to produce a secondary battery. On the other hand, when this electrode is used as the negative electrode of a secondary battery, it can be combined with an electrode having a higher charge / discharge potential than the electrode to produce a secondary battery.

[0063] For example, when the electrode of the present disclosure is used as a positive electrode, the counter electrode (negative electrode) is not particularly limited as long as it is an electrode that can be used as a negative electrode in a secondary battery.

[0064] The electrolyte used in the secondary battery may be a liquid or solid that can move alkali metal ions or fluorine compound anions from the positive electrode to the negative electrode or from the negative electrode to the positive electrode. That is, the same electrolyte as that used in a secondary battery using a known non-aqueous electrolyte can be used. Examples include an electrolyte solution, a gel electrolyte, a solid electrolyte, an ionic liquid, and a molten salt. Here, the electrolyte solution refers to an electrolyte dissolved in a solvent.

[0065] The structure of the secondary battery is not particularly limited, and existing forms and structures such as a stacked type and a wound type can be adopted. That is, an electrode group in which a positive electrode and a negative electrode are stacked or wound facing each other with a separator interposed therebetween is immersed in an electrolyte and sealed to form a secondary battery. Alternatively, an electrode group in which a positive electrode and a negative electrode are stacked or wound facing each other with a solid electrolyte interposed therebetween is sealed to form a secondary battery. Effect of the Invention

[0066] According to the manufacturing method of the present invention, it is possible to significantly improve the cycle characteristics even in an electrode in which it is difficult to ensure sufficient adhesion between the inorganic binder made of silicate or phosphate and the active material, or in an electrode having an active material layer with a high thickness or density. In addition, the electrode obtained by this manufacturing method contains a material in which the surface of the active material is modified with silicate or phosphate. The inorganic binder and the active material are integrated via this modified material, resulting in an electrode with high strength and excellent cycle characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0067] Hereinafter, an embodiment and an example according to one aspect of the present invention will be described, but the present invention is not limited to these embodiments and examples.

[0068] As an example of a method for producing a nonaqueous electrolyte secondary battery according to this embodiment, a slurry consisting of an active material, a resin binder, a conductive assistant, etc. is applied to or filled into a current collector, which is then brought into contact with an aqueous solution of an inorganic binder containing a silicate or a phosphate at a predetermined temperature and dried to produce an electrode. Specific electrode materials will be described later.

[0069] As described below, a lithium ion battery was fabricated using the electrode obtained by this manufacturing method and tested. The lithium ion capacitor can be fabricated in the same manner as the lithium ion battery, except that the operation of the counter electrode is different.

[0070] Specifically, for example, the battery can be produced in the same manner as the battery described below, except that the electrode of the present embodiment is used as the positive electrode and a conventional negative electrode for lithium ion capacitors is used as the negative electrode. Alkali metal ion batteries other than lithium ion batteries can be produced in the same manner as lithium ion batteries, except that Li, which is the charge carrier of lithium ion batteries, is replaced with Na or K.

[0071] Specifically, a sodium ion battery can be fabricated in the same manner as the battery described later, except that the electrode of this embodiment is used as the positive electrode, a conventional negative electrode for sodium ion batteries is used as the negative electrode, and a sodium supporting salt is used as the electrolyte. A potassium ion battery can be fabricated in the same manner as the battery described later, except that the electrode of this embodiment is used as the positive electrode, a conventional negative electrode for potassium ion batteries is used as the negative electrode, and a potassium supporting salt is used as the electrolyte. EXAMPLES

[0072] [SiO electrode] (Example 1 and Example 2) SiO x (x=0.75, median diameter D 50 An aqueous slurry (solid ratio 92:3:1:3:1 mass%) consisting of cellulose acetate (C100, 100% N, 100% cellulose) was filled into a 130-μm thick foamed nickel (Celmet #8, Sumitomo Electric Industries, Ltd.) and dried at 80°C for 30 minutes, resulting in an electrode capacity per unit area of ​​6 mAh / cm. 2 A SiO electrode was fabricated.

[0073] Under the conditions shown in Table 1, a test electrode was prepared by immersing a SiO electrode in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10% by mass) at 40°C, pre-drying (80°C, 1 hour), and then vacuum drying (150°C, 10 hours). The weight of the electrode after impregnation (excluding the current collector) was increased by 15% compared to the electrode before impregnation (excluding the current collector). After the SiO electrode was completely immersed in the sodium silicate aqueous solution, the excess sodium silicate aqueous solution remaining on the electrode surface was removed by blotting with a paper sheet (Kimberly-Clark, Kimwipe).

[0074] (Examples 3 to 7) Under the conditions shown in Table 1, the SiO electrode was immersed in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10 mass%) at a temperature of 60°C, and the rest was the same as in Example 1.

[0075] (Examples 8 to 11) Under the conditions shown in Table 1, the SiO electrode was immersed in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10 mass%) at a temperature of 80°C, and the rest was the same as in Example 1.

[0076] (Example 12 and Example 13) Under the conditions shown in Table 1, the SiO electrode was immersed in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10 mass%) at a temperature of 95°C, and the rest was the same as in Example 1.

[0077] Example 14 The SiO electrode was placed in a stainless steel sealed container, and the pressure in the container was reduced to an absolute pressure of 10 kPa using a vacuum pump. After the pressure in the container reached 10 kPa, a sodium silicate aqueous solution (Na2O 3.0SiO2 aq., concentration 10 mass%) at 60°C was poured into the container while maintaining the reduced pressure until the electrode was completely immersed. After 1 minute, the reduced pressure was released by air purging, and the electrode was immersed in the same manner as in Example 3.

[0078] Example 15 After the pressure inside the container reached 10 kPa, a sodium silicate aqueous solution (Na2O 3.0SiO2 aq., concentration 10 mass%) at 60°C was poured into the container while maintaining the reduced pressure until the electrodes were completely immersed. After one minute had elapsed, compressed air was poured into the container using a pressure pump to increase the pressure to an absolute pressure of 0.3 MPa, and the pressurized state was released by air purging. The rest of the procedure was the same as in Example 14.

[0079] (Comparative Example 1 and Comparative Example 2) Under the conditions shown in Table 1, the SiO electrode was immersed in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10 mass%) at a temperature of 25°C, and the rest was the same as in Example 1.

[0080] Comparative Example 3 Under the conditions shown in Table 1, the SiO electrode was immersed in a sodium silicate aqueous solution (Na2O·3.0SiO2aq., concentration 10 mass%) at a temperature of 0°C, and the rest was the same as in Example 1.

[0081] Comparative Example 4 This is a SiO electrode that is not immersed in a sodium silicate aqueous solution.

[0082] (Battery characteristics) Batteries were fabricated using the test electrodes obtained in Examples 1 to 13 and Comparative Examples 1 to 4, a metallic lithium counter electrode (500 μm-thick lithium foil made by Honjo Metal), a three-layer microporous membrane of polypropylene (PP) / polyethylene (PE) / polypropylene (PP) (Celgard, 2325), a glass filter (Advantech, GA100), and 1 mol / L LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 1:1 vol., + 1 mass % vinylene carbonate (VC).

[0083] The charge-discharge cycle test was performed in a 30°C environment with a cut-off voltage of 0.01 to 0.9 V and a charge current of 0.05 mA / cm 2 , discharge current 0.1mA / cm 2 The test was performed under the condition of repeated charging and discharging at 1000 rpm.

[0084] Table 2 shows the cycle characteristics of the SiO electrode (discharge capacity, capacity retention rate, and coulombic efficiency in the first to third cycles).

[0085] In the case of the electrodes immersed in the sodium silicate aqueous solution at 40° C. or higher in Examples 1 to 15, the discharge capacity is larger than that of the untreated electrode in Comparative Example 4, and the capacity retention rate is higher than that of the electrodes immersed in the sodium silicate aqueous solution container at 25° C. or lower in Comparative Examples 1 to 3. In addition, in each Example, the coulombic efficiency is higher than that of Comparative Examples 1 to 4. Among them, the electrodes immersed at 40° C. for 10 minutes in Example 2, the electrodes immersed at 60° C. for 5 to 60 minutes in Examples 4 to 7, and the electrodes immersed at 80° C. for 1 to 10 minutes in Examples 8 and 9 show an initial discharge capacity of 85% or more, and the capacity retention rate at the third cycle is also large at 90% or more.

[0086] Thus, when the temperature of the sodium silicate aqueous solution is high, the immersion time tends to be short, and when the temperature is low, the immersion time tends to be long. It is also suggested that the immersion time can be shortened by reducing the pressure and removing the air from the active material layer before the impregnation process of the sodium silicate aqueous solution. It is also suggested that the immersion time can be shortened by performing the impregnation process in a high-pressure environment rather than atmospheric pressure. However, when the temperature of the sodium silicate aqueous solution is 25°C or less, the effect of the present invention cannot be obtained even if the treatment time is extended.

[0087] [Table 1]

[0088] [Table 2]

[0089] [Li2FeSiO4 electrode] Li2FeSiO4 (median diameter D 50An aqueous slurry (solid ratio 94:3:3 by mass%) consisting of ethylenediaminetetraacetate (Pb = 12 μm), acetylene black (Denka, Denka Black), and an acrylic binder (JSR, TRD202A) was filled into an aluminum foam (Sumitomo Electric, Al Celmet) whose thickness had been adjusted to 100 μm. The foam was then dried at 80°C for 30 minutes and then adjusted with a roll press to obtain an electrode capacity per unit area of ​​0.5 mAh / cm. 2 The Li2FeSiO4 electrode was fabricated. The Li2FeSiO4 was coated with 10 mass% carbon by rotary kiln treatment (700℃).

[0090] Example 16 A Li2FeSiO4 electrode was immersed in a lithium silicate aqueous solution (Li2O·3.5SiO2aq., concentration 1% by mass) at 40°C for 1 minute, pre-dried (80°C, 1 hour), and then vacuum-dried (140°C, 10 hours) to prepare a test electrode. The weight of the electrode after impregnation (excluding the current collector) was increased by 1-3% compared to the electrode before impregnation (excluding the current collector). After the SiO electrode was completely immersed in the lithium silicate aqueous solution, the excess sodium silicate aqueous solution remaining on the electrode surface was removed by blotting with a paper sheet (Kimberly-Clark, Kimwipe).

[0091] Comparative Example 5 The Li2FeSiO4 electrode was created by placing the Li2FeSiO4 electrode on a hot plate at 120°C and spraying the lithium silicate aqueous solution with a spray gun. Note that the lithium silicate aqueous solution dried immediately upon contact with the electrode, so the time that the lithium silicate aqueous solution was in liquid form and in contact with the active material layer was less than one second.

[0092] Comparative Example 6 This is a Li2FeSiO4 electrode that is not immersed in a lithium silicate aqueous solution.

[0093] (Battery characteristics) The electrodes obtained in Example 16, Comparative Example 5, and Comparative Example 6 were used as test electrodes, and a coin-type battery (R2032) was produced using a metallic lithium counter electrode (Honjo Metal, lithium foil with a thickness of 500 μm), a three-layer microporous membrane of PP / PE / PP (Celgard, 2325), a glass filter (Advantech, GA100), and 1 mol / L LiPF6 / ethylene carbonate (EC):diethyl carbonate (DEC) = 1:1 vol., + vinylene carbonate (VC) 1 wt.%.

[0094] The charge-discharge cycle test was carried out in a 30° C. environment under the conditions of one cycle of 0.1C charge-discharge with a cutoff voltage of 4.8 to 1.5 V, and repeated cycles of 0.2C charge-discharge with a cutoff voltage of 4.5 to 1.5 V.

[0095] Table 3 shows the cycle characteristics of the LiFe2SiO4 electrode (discharge capacity, capacity retention rate, and coulombic efficiency at the 1st, 2nd, and 50th cycles).

[0096] In the case of Example 16, when immersed in a 40° C. aqueous lithium silicate solution for 1 minute, the discharge capacity was about 100 mAh / g even after 50 cycles at a 0.2 C rate, indicating stable cycle characteristics.

[0097] On the other hand, in Comparative Example 5, where the lithium silicate aqueous solution was in liquid state and in contact with the active material layer for less than 1 second, and in Comparative Example 6, where the active material layer was not immersed in the lithium silicate aqueous solution, the discharge capacity was low from the first discharge. Comparing Comparative Example 5 and Comparative Example 6, Comparative Example 5 has a slightly higher capacity. However, comparing Comparative Example 5 and Example 16, it can be seen that there is a clear difference in capacity.

[0098] [Table 3]

[0099] As described above, the preferred embodiments and examples of the present invention have been described, but various additions, modifications, or deletions are possible without departing from the spirit of the present invention. Therefore, such additions, modifications, or deletions are also included in the scope of the present invention. In addition, although the numbers described in the general formula of the compound in this specification may be expressed as integers simply for the sake of expression, if the numbers satisfy electrical neutrality and are substantially the same, they are included in the scope of the present invention.

Claims

1. A method for manufacturing an electrode for a non-aqueous electrolyte secondary battery, comprising the steps of: A step A of coating or filling a current collector with a slurry containing an active material and a first binder, and then drying the slurry to produce an active material layer; A step B of preparing a second binder aqueous solution at a temperature higher than the room temperature of water; and a step C of immersing the active material layer in the second binder aqueous solution or applying the second binder aqueous solution to the active material layer, drying the active material layer, and then manufacturing an electrode. A method for manufacturing an electrode.

2. The first binder is a resin binder, and the second binder aqueous solution is an inorganic binder aqueous solution. A method for producing the electrode according to claim 1.

3. the second binder aqueous solution is a silicate aqueous solution or a phosphate aqueous solution, The silicate aqueous solution is 2 O.nSiO 2 A is at least one of Li, Na, and K, and n is 1.7 or more and 5 or less, The phosphate aqueous solution contains Al 2 O 3 ・nP 2 O 5 A liquid in which a phosphate represented by the formula (I) is dissolved in water, and n is 1.7 or more and 5 or less. A method for producing the electrode according to claim 2.

4. The step C is a step of immersing the active material layer in a second aqueous binder solution having a temperature of 30° C. or more and 120° C. or less, or applying the second aqueous binder solution to the active material layer, drying the active material layer, and then manufacturing an electrode; A method for producing the electrode according to any one of claims 1 to 3.

5. The step C includes immersing or applying for a period of 10 seconds or more and 5 hours or less. A method for producing the electrode according to claim 3.

6. The step C comprises: The pressure is reduced to an absolute pressure of 30 kPa or less in advance to remove air from within the active material layer, a step of immersing the active material layer from which air has been removed in the second binder aqueous solution, or applying the second binder aqueous solution to the active material layer from which air has been removed, and then drying the active material layer to produce an electrode; A method for producing the electrode according to claim 1 .

7. The step C comprises: In the step of immersing the active material layer in the second binder aqueous solution or applying the second binder aqueous solution to the active material layer, an absolute pressure is applied to the active material layer from 0.12 MPa to 10 MPa. A method for producing the electrode according to claim 1 .

8. The step C comprises: a step of reducing the pressure to an absolute pressure of 30 kPa or less in advance to remove air from within the active material layer; and a step of immersing the active material layer from which air has been removed in the second aqueous binder solution under a reduced pressure, or applying the second aqueous binder solution to the active material layer from which air has been removed, and pressurizing the active material layer from the reduced pressure state to an absolute pressure of 0.12 MPa or more and 10 MPa or less. A method for producing the electrode according to claim 1 .

9. The electrode after the step C contains an inorganic binder in an amount of 0.1 mass% or more and 30 mass% or less, when the total amount of the active material layer is taken as 100%. A method for producing the electrode according to claim 1 .

10. The active material is represented by the general formula A 2-a M b S c O 4-d Or the general formula SiO x The material includes a material represented by A is at least one of Li, Na, and K, M is at least one of Fe, Ni, Mn, and Co, a is 0 to 2, b is 0.8 to 1, c is 0.8 to 1, d is 0 to 0.2, and x is 0.2 to 1.

8. A method for producing the electrode according to claim 1 .

11. The current collector is a conductor made of a porous body or a fiber group. A method for producing the electrode according to claim 1 .

12. The material of the current collector is aluminum or an aluminum alloy. A method for producing the electrode according to claim 1 .

13. An electrode for a non-aqueous electrolyte secondary battery, An active material layer including an active material and a first binder, a current collector, and a second binder; the second binder is present on the surface and within the active material layer; the active material layer contains the second binder in an amount of 0.1% by mass or more and 30% by mass or less, when the total amount of the active material layer is taken as 100%, The second binder is an inorganic binder, 2 O.nSiO 2 A is at least one of Li, Na, and K, and n is 1.7 to 5; or Al 2 O 3 ・nP 2 O 5 The phosphate having n of 1.7 or more and 5 or less includes a silicate or a phosphate that is dissolved and modified in water having a temperature higher than room temperature, An electrode in which the second binder and the active material layer are bonded together.

14. The second binder contains a silicate or a phosphate that is dissolved and modified in water at a temperature of 30° C. or more and 120° C. or less.

14. The electrode of claim 13.

Citation Information

Patent Citations

  • Lithium ion battery and manufacturing method thereof

    JP2001508916A

  • Negative electrode and its manufacturing method, and secondary cell

    JP2008135382A

  • Electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

    WO2021131313A1

  • Negative electrode for nonaqueous electrolyte secondary batteries, nonaqueous electrolyte secondary battery, and method for producing negative electrode for nonaqueous electrolyte secondary batteries

    WO2021153526A1

  • Control method of idle speed

    JP1986049147A