Manufacturing method of sintered body
The method of cross-sectional imaging and binarization in sintered body production allows for accurate defect prediction and recycling of metal powder, addressing the limitations of existing technologies by enhancing defect detection and resource recovery.
Patent Information
- Application Number
- JP2023050200
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for manufacturing sintered bodies fail to accurately predict defects until after sintering, leading to wasted resources and difficulty in recycling defective metal powder.
A method involving injection molding a composition containing sinterable inorganic powder and an organic binder, followed by cross-sectional imaging and binarization to distinguish between the inorganic powder and organic binder, allowing for the calculation of a ratio (A/B) to determine sintered body quality without sintering, and enabling recycling of defective metal powder.
Enables early detection of defects in sintered bodies and facilitates the recycling of metal powder, reducing waste and improving manufacturing efficiency.
Smart Images

Figure 2024139317000004 
Figure 2024139317000005 
Figure 2024139317000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a sintered body. [Background technology]
[0002] Among sintered bodies using sinterable inorganic powder such as metal, ceramic, cermet, etc. as a material, for precise sintered bodies or sintered bodies with complex shapes, a technique is known which uses a composition for manufacturing sintered compacts containing a sinterable inorganic powder and a binder as a material. The composition for producing sintered compacts is heated and kneaded as a raw material for the sintered compact, which is then injection molded to produce a compact, which is then subjected to a degreasing process and then sintered.
[0003] In the production of sintered bodies using the above-mentioned composition for producing sintered bodies, the debinding step is the most important step in order to obtain a sintered body of good quality without defects such as cracks, swelling, deformation, etc. This debinding step is a step in which the binder is removed from the compact, which is a compact of the composition for producing sintered bodies, and known methods for this step include a method in which the compact is heated to pyrolyze and gasify the binder, and a method in which the compact is treated with a solvent to elute and remove the soluble binder components in the compact, and then the remaining binder is pyrolyzed and gasified.
[0004] In order to prevent the cracking and swelling of the molded body during the above-mentioned debinding step, various means have been devised. For example, Patent Document 1 discloses a technique related to an injection molding composition having increased strength by blending a component containing a glycidyl group from the viewpoint of shape retention during debinding, and Patent Document 2 proposes a technique related to an injection molding composition having an increased Vicat softening point. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5970794 [Patent Document 2] Patent No. 4317916 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the techniques disclosed in Patent Documents 1 and 2, it is not possible to determine whether or not a defect has occurred until sintering is actually performed and the state of the sintered body is confirmed, and a long process and costs are required to determine whether or not a defect has occurred. Furthermore, when judging defects based on the sintered body, since it is difficult to recover the metal powder used, the only option is to discard the defective product, and further improvement is desired from the viewpoint of recyclability.
[0007] Therefore, an object of the present invention is to provide a method for producing a sintered body that can accurately predict defects in the sintered body without sintering, and that enables recycling of defective metal powder. [Means for solving the problem]
[0008] The present inventors have conducted intensive research into the manufacturing method of a sintered molded body to solve the above-mentioned problems, and as a result, have found that it is possible to automatically determine whether a sintered body is good or bad by injection molding a composition for a sintered molded body containing a sinterable inorganic powder and an organic binder, observing the cross section of the molded body, obtaining a cross-sectional image, and performing a binarization process on the cross-sectional image to distinguish the sinterable inorganic powder from the organic binder, and judging whether the sintered body is good or bad based on the calculation result of the ratio (A / B) of the maximum area (A) of the discontinuous organic binder part in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one visual field of the binarized cross-sectional image. This makes it possible to detect defects occurring in the sintered body early, and also makes it possible to recycle metal powder from the molded body or the composition for a sintered molded body.
[0009] The present invention has been made based on the above findings, and the gist of the present invention is as follows. (1) A step of obtaining a molded body by injection molding a composition for sintered molded body, the composition including a sinterable inorganic powder and an organic binder; preparing a cross section of the molded body, observing the cross section, and obtaining a cross section image; performing a binarization process on the cross-sectional image to distinguish the sinterable inorganic powder from the organic binder; a step of calculating a ratio (A / B) of a maximum area (A) of a discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to a total area (B) of the organic binder in one visual field of the binarized cross-sectional image, and judging whether the sintered body is good or bad based on the calculation result; A method for producing a sintered body, comprising:
[0010] (2) The method for producing a sintered body according to (1), characterized in that the cross section of the compact is prepared by ion milling.
[0011] (3) The method for producing a sintered body according to (1) or (2), characterized in that the binarization process of the cross-sectional image is Otsu's adaptive binarization process.
[0012] (4) The method for producing a sintered body described in (3) is characterized in that the length of one side of the minimum range of the adaptive range used in the Otsu's adaptive binarization process is equal to or greater than the maximum particle size of the sinterable inorganic powder.
[0013] (5) The method for producing a sintered body according to (1) or (2), characterized in that the quality of the sintered body is judged based on whether the ratio (A / B) of the maximum area (A) of the discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one visual field of the binarized cross-sectional image is 0.5 or less.
[0014] (6) In the judgment of whether the sintered body is good or bad, after it is judged to be bad, The method for producing a sintered body according to (1) or (2), further comprising a step of changing the conditions of the injection molding so as to suppress the occurrence of defects. Effect of the Invention
[0015] According to the present invention, it is possible to provide a method for producing a sintered body, which can accurately predict defects in a sintered body without sintering, and enables the recycling of defective metal powder. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is an enlarged view of a part of a cross section of a molded body, showing a schematic diagram of the state of a sinterable inorganic powder and an organic binder. [Diagram 2] The cross-section of a molded test piece obtained in the example was observed by SEM and photographed at a magnification of 500x, where (a) shows the cross-sectional state before binarization processing, and (b) shows the cross-sectional state after binarization processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention (hereinafter simply referred to as "the present embodiment") will be described in detail. The following embodiments are merely illustrative for explaining the present invention, and are not intended to limit the present invention to the following contents. The present invention can be modified appropriately within the scope of the gist thereof.
[0018] <Composition for sintered compact> First, a composition for sintered compacts used as a material for the compact in the method for producing a sintered compact of this embodiment will be described. The composition for sintered compacts includes a sinterable inorganic powder and an organic binder. In addition to the inorganic powder and the organic binder, the composition for sintered compacts may include other additives as described below.
[0019] (Sinterable inorganic powder) The composition for sintered compacts contains a sinterable inorganic powder. The sinterable inorganic powder may be used alone or in combination of two or more kinds.
[0020] In this embodiment, the sinterable inorganic powder can be appropriately selected from known inorganic powders depending on the application. For example, the sinterable inorganic powder may be selected from metal powders, alloy powders, metal carbonyl powders, and mixtures thereof. Among these inorganic powders, it is preferable to use metal powders and ceramic powders in order to impart functionality.
[0021] Examples of the metal powder include powders of aluminum, magnesium, barium, calcium, cobalt, zinc, copper, nickel, iron, silicon, titanium, tungsten, and metal compounds and metal alloys based on these metals, etc. Here, the metal powder may be not only a completed alloy, but also a mixture of individual alloy components.
[0022] Examples of the ceramic powder include oxides such as zinc oxide, aluminum oxide, and zirconia; hydroxides such as hydroxyapatite; carbides such as silicon carbide; nitrides such as silicon nitride and boron nitride; halides such as fluorite; silicates such as stearite; titanates such as barium titanate and lead zirconate titanate; carbonates; phosphates; ferrite; high-temperature superconducting materials; and the like.
[0023] The sinterable inorganic powder may be used alone, or a combination of a plurality of inorganic substances such as various metals, metal alloys, or ceramics may be used. Particularly preferred metals and alloy metals include titanium alloys and stainless steels, and ceramics include Al2O3 and ZrO2. As the titanium alloy, for example, titanium-6 aluminum-4 vanadium alloy can be preferably used, and as the stainless steel, for example, SUS316L and SUS630 can be preferably used.
[0024] The method for producing the sinterable inorganic powder is not particularly limited, but the inorganic powder may be used after separating only the organic binder from a molding that is predicted to be defective by using an acid or heat, washing, etc. However, since there is a possibility that residues may adhere to the inorganic powder depending on the binder component, it is preferable to use a polyacetal resin that leaves little residue after depolymerization.
[0025] (organic binder) The composition for sintered compacts according to the embodiment contains an organic binder in addition to the above-mentioned sinterable inorganic powder.
[0026] The resin components constituting the organic binder are sometimes collectively called aggregate resin (P). The aggregate resin (P) is crushed and then mixed with the sinterable inorganic powder, and then used, thereby making it possible to reduce voids (air gaps) that occur in the sintered body. Therefore, the particle size of the powder of the aggregate resin (P) is preferably such that the passing rate through a 50 Mesh (300 μm) sieve in accordance with JIS Z 8801 is 40% or more, and more preferably 50% or more.
[0027] The organic binder may contain any resin component depending on the application, but preferably contains at least a polyacetal resin, a polyolefin resin, and an epoxy resin.
[0028] The polyacetal resin generates very little residue upon volatilization, and can improve the quality of the sintered body. The polyolefin resin can increase the strength of the molded body. The epoxy resin can increase the compatibility between the polyacetal resin and the polyolefin resin.
[0029] The volume proportion of the organic binder in the composition for sintered compacts is not particularly limited, but is preferably 25 to 60 volume %, more preferably 30 to 55 volume %, and particularly preferably 35 to 50 volume %, relative to 100 volume % of the composition for sintered compacts. By containing the organic binder within the above-mentioned range, a composition for sintered molded bodies having a melt viscosity suitable for injection molding can be obtained, and a sintered product with reduced shrinkage and good dimensional accuracy can be obtained.
[0030] Polyacetal resin The polyacetal resin may be a polyacetal homopolymer, a polyacetal copolymer, or a mixture thereof. Among these, it is preferable to use a polyacetal copolymer as the polyacetal resin from the viewpoint of thermal stability. The polyacetal resins may be used alone or in combination of two or more.
[0031] The polyacetal may be used in the form of powder other than pellets, which are usually provided. The particle size of the powder is preferably D50=500 μm or less, and more preferably D50=300 μm or less.
[0032] The polyacetal homopolymer may be a polymer having an oxymethylene unit in the main chain, and both ends of the polymer may be blocked with an ester group or an ether group. The polyacetal homopolymer may be obtained from formaldehyde and a known molecular weight regulator as raw materials, and may be obtained from these raw materials by a known slurry method using a known onium salt polymerization catalyst and a hydrocarbon as a solvent, for example, the polymerization method described in JP-B-47-6420 and JP-B-47-10059.
[0033] The polyacetal homopolymer is preferably one in which 99.8 mol % or more of the main chain excluding both ends is composed of oxymethylene units, and more preferably the main chain excluding both ends is composed only of oxymethylene units.
[0034] The polyacetal copolymer includes a polymer having an oxymethylene unit and an oxyethylene unit in the main chain, and can be obtained, for example, by copolymerizing trioxane with a cyclic ether and / or a cyclic formal in the presence of a polymerization catalyst.
[0035] The trioxane is a cyclic trimer of formaldehyde, and is generally obtained by reacting an aqueous solution of formalin in the presence of an acid catalyst.
[0036] The cyclic ether and / or cyclic formal are components that can be copolymerized with the trioxane, and examples thereof include ethylene oxide, propylene oxide, butylene oxide, epichlorohydrin, epibromohydrin, styrene oxide, oxatane, 1,3-dioxolane, ethylene glycol formal, propylene glycol formal, diethylene glycol formal, triethylene glycol formal, 1,4-butanediol formal, 1,5-pentanediol formal, and 1,6-hexanediol formal. In particular, ethylene oxide and 1,3-dioxolane are preferred. These may be used alone or in combination of two or more.
[0037] The polymerization catalyst used in the production of the polyacetal copolymer is not particularly limited, and examples thereof include boric acid, tin, titanium, phosphorus, arsenic, and antimonides, which are typified by Lewis acids. Among these, it is preferable to use at least one of boron trifluoride, boron trifluoride hydrates, and coordination complex compounds of boron trifluoride and an organic compound containing an oxygen atom or a sulfur atom. More specifically, for example, boron trifluoride, boron trifluoride diethyl etherate, and boron trifluoride-di-n-butyl etherate are suitable examples. These may be used alone or in combination of two or more.
[0038] The deactivation of the polymerization catalyst in the production of the polyacetal copolymer can be carried out by introducing the polyacetal resin obtained by the polymerization reaction into an aqueous solution containing at least one catalyst neutralizing deactivator, such as amines, such as ammonia, triethylamine, or tri-n-butylamine, or hydroxides, inorganic acid salts, or organic acid salts of alkali metals or alkaline earth metals, or into an organic solvent liquid, and stirring the resulting slurry for generally several minutes to several hours.
[0039] The slurry after the catalyst neutralization and deactivation is filtered and washed to remove unreacted monomers, catalyst neutralization deactivator, and catalyst neutralization salt, and then dried.
[0040] Further, the polymerization catalyst can be deactivated by a method in which the polyacetal copolymer is brought into contact with vapor of ammonia, triethylamine, or the like, or by a method in which the polyacetal resin is brought into contact with at least one of hindered amines, triphenylphosphine, calcium hydroxide, or the like, in a mixer.
[0041] Furthermore, without deactivating the polymerization catalyst, the polyacetal copolymer can be heated in an inert gas atmosphere at a temperature below the melting point of the polyacetal copolymer, thereby reducing the volatilization of the polymerization catalyst, and the terminal stabilization treatment described below can be performed using the polyacetal copolymer.
[0042] The above-mentioned operation for deactivating the polymerization catalyst and the operation for reducing the volatilization of the polymerization catalyst can be carried out, if necessary, after pulverizing the polyacetal resin obtained by the polymerization reaction.
[0043] The aromatic dicarboxylic acids constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more kinds.
[0044] The terminal stabilization treatment of the obtained polyacetal resin can be carried out by decomposing and removing the unstable terminal moiety as follows: For example, the polyacetal resin can be melted using a vented single screw extruder or a vented twin screw extruder in the presence of a known basic substance capable of decomposing unstable terminal moieties, such as ammonia, fatty acid amines such as triethylamine and tributylamine, hydroxides of alkali metals or alkaline earth metals typified by calcium hydroxide, inorganic weak acid salts, and organic weak acid salts, as a notching agent, to decompose and remove the unstable terminal moiety.
[0045] The polyacetal resin may be recycled. In the material recycling, polyacetal resin used as a product is collected, and after removing impurities such as grease, the pulverized polyacetal resin may be used. In addition to material recycling, polyacetal resin used as a product in chemical recycling or the like may be recycled into monomers, and the polyacetal resin produced from the monomers may be used. The recycled polyacetal resin may be used alone or in combination with a non-recycled polyacetal resin.
[0046] The polyacetal resin may be a modified polyacetal. In general, a modified polyacetal is a block copolymer having a modified segment in a polyacetal. The polyacetal segment may be a homopolymer residue consisting of only oxymethylene units, or a copolymer residue in which oxymethylene units and oxyalkylene units are randomly copolymerized. The modified segment is a component that does not fall under the category of a polyacetal segment, and examples of the modified segment include polyolefin, polyurethane, polyester, polyamide, polystyrene, and polyalkyl acrylate.
[0047] The polyacetal segment is preferably a polyacetal copolymer residue in which oxymethylene units and oxyalkylene units are randomly copolymerized, and the modified segment is preferably a polyolefin or polyurethane.
[0048] The modified segment of the modified polyacetal is preferably a polyolefin from the viewpoint of reducing residues derived from the organic binder in the degreasing step, specifically, polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, polybutadiene, hydrogenated polybutadiene, etc.
[0049] From a similar viewpoint, the modified segment of the modified polyacetal is more preferably polyethylene, polypropylene, or hydrogenated polybutadiene, and is particularly preferably hydrogenated polybutadiene from the viewpoints of shape retention in the degreasing step and suppression of cracking and swelling in the degreasing step.
[0050] The modified polyacetal resin may be used alone, or two or more kinds of modified polyacetal resins may be used together. Furthermore, the modified polyacetal resin may be used in combination with an unmodified polyacetal resin.
[0051] Polyolefin resin The organic binder further contains a polyolefin resin in addition to the polyacetal resin described above. Here, the polyolefin resin is a homopolymer or copolymer having a structural unit derived from an alkene having 2 to 8 carbon atoms, preferably 2 to 4 carbon atoms.
[0052] Specific examples of the polyolefin resin include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyisoprene, polybutadiene, etc. Polyethylene, polypropylene, and mixtures thereof are preferred, and polyethylene or polypropylene is more preferred from the viewpoint of shape retention in the degreasing step and suppression of cracking and swelling in the degreasing step. Examples of commercially available polyethylene that can be suitably used include Santech HD series (manufactured by Asahi Kasei), Santech LD series (manufactured by Asahi Kasei), Santech EVA series (manufactured by Asahi Kasei), Neozex, Ultzex, and Evolue (all manufactured by Prime Polymer), and examples of polypropylene include Sumitomo Noblen (manufactured by Sumitomo Chemical), Novatec PP (manufactured by Japan Polypropylene), Sanallomer PP series (manufactured by Sanallomer), and Prime Polypro (manufactured by Prime Polymer).
[0053] From the viewpoints of kneadability with sinterable inorganic powders and injection moldability, the polyolefin resin preferably has a melt flow index of 40 g / 10 min or more. The melt flow index of the polyolefin resin can be measured under conditions of 230° C. and 2.16 kg.
[0054] Epoxy resin The organic binder further contains an epoxy resin in addition to the polyacetal resin and polyolefin resin described above. The inclusion of the epoxy resin increases the compatibility with the polyacetal resin and the polyolefin resin, and at the same time increases the interaction (adhesiveness) with the metal powder, thereby improving the dispersibility and sintering density of the metal powder.
[0055] The epoxy resin means a resin composed of an aggregate of a plurality of epoxy compounds, and the epoxy compound means a compound having an epoxy group in the molecule. Here, the plurality of epoxy compounds constituting the epoxy resin may have the same or different molecular structures. From the viewpoints of kneadability with sinterable inorganic powders and injection moldability, the epoxy resin preferably has a melt flow index of 40 g / 10 min or more. The melt flow index of the polyolefin resin can be measured under conditions of 190° C. and 2.16 kg with reference to ASTM-D-1238-57T.
[0056] Here, the type of the epoxy resin is not particularly limited, but bisphenol A type epoxy, bisphenol F type epoxy, novolac type epoxy, aliphatic type epoxy, and epoxy resins having glycidyl, which will be described later, can be used.
[0057] The preferred epoxy resin is a copolymer of a glycidyl ester of an unsaturated acid and an olefin, and particularly preferably an ethylene-glycidyl methacrylate copolymer (EGMA).
[0058] Here, the saturated acid glycidyl ester is represented by the general formula (1): [ka] (In the formula, R represents an alkenyl group having 2 to 18 carbon atoms, and X represents a carbonyloxy group.) It is a compound represented by the formula: and has a structure formed by esterification of an unsaturated acid with an alcohol compound having a glycidyl group. Specific examples of the compound include glycidyl acrylate, glycidyl methacrylate, glycidyl ethacrylate, and glycidyl itaconate. Among these, glycidyl methacrylate is preferably used.
[0059] In addition, the unsaturated acid and / or its derivative, which is an optional component, can include, in addition to the glycidyl ester, an unsaturated compound having one or more carboxylic acid groups, an unsaturated compound having one or more carboxylic acid anhydride groups, an ester of a compound having a carboxylic acid group and an alkyl alcohol, etc. Specific compounds include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, citraconic acid, and mesaconic acid, unsaturated carboxylic anhydrides such as maleic anhydride, vinyl esters of saturated carboxylic acids such as vinyl acetate, vinyl propionate, and vinyl butyrate, and alkyl esters of unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, and butyl methacrylate. Among these, vinyl acetate, methyl acrylate, ethyl acrylate, and methyl methacrylate are preferred.
[0060] Further, the olefin to be copolymerized with the glycidyl ester of unsaturated acid may be an α-olefin having 2 to 10 carbon atoms, and among these, ethylene, propylene and 1-butene are particularly preferred. Furthermore, the method for copolymerizing the glycidyl ester of unsaturated acid with the olefin is not particularly limited, and may be a conventionally known method.
[0061] Among the copolymers of the glycidyl ester of an unsaturated acid and an olefin, ethylene-glycidyl methacrylate copolymer (EGMA) is preferred. Commercially available EGMA can be used, and suitable examples include Celloxide manufactured by Daicel Chemical Industries, Ltd. and Bondfast manufactured by Sumitomo Chemical Industries, Ltd.
[0062] Furthermore, the EGMA can be synthesized by various methods. For example, it can be produced by bulk polymerization, emulsion polymerization, solution polymerization, etc. using a free radical initiator. Representative polymerization methods include those described in JP-B-46-45085 and JP-A-61-127709, and can be produced under conditions of a pressure of 500 kg / cm2 or more and a temperature of 40 to 300°C in the presence of a polymerization initiator that generates free radicals. Other examples include a method in which an unsaturated epoxy compound and a radical generator are mixed with a resin consisting of at least one monomer selected from ethylene and olefin-based unsaturated compounds other than ethylene, and melt-graft copolymerized in an extruder, or a method in which an unsaturated epoxy compound and an olefin-based unsaturated compound are copolymerized in an inert medium such as water or an organic solvent in the presence of a radical generator.
[0063] The copolymer of the unsaturated acid glycidyl ester and the olefin resin has an unsaturated acid glycidyl ester unit content of 1 to 25% by weight, preferably 3 to 20% by weight, and more preferably 13 to 20% by weight. When the unsaturated acid glycidyl ester unit content is 1% or more, the interaction with other resin components and metal powder is strengthened, and dispersibility is improved. In addition, when the unsaturated acid glycidyl ester unit content is 25% or less, the thermal stability during kneading and injection molding is excellent.
[0064] The content of the unsaturated acid glycidyl ester can be measured by measuring the infrared absorption spectrum of the press sheet of the epoxy group-containing ethylene polymer. The absorbance of the characteristic absorption of the infrared absorption spectrum is corrected by the thickness of the sheet used for the measurement, and the content of the unsaturated compound having a glycidyl group is determined by a calibration curve method based on the corrected absorbance. The characteristic absorption peak is at 910 cm -1 Since it often appears near the
[0065] When EGMA is used as the epoxy resin, the melt flow index of EGMA is preferably 3 g / 10 min or more and 400 g / 10 min or less, more preferably 10 g / 10 min or more and less than 400 g / 10 min, and even more preferably 50 g / 10 min or more and less than 400 g / 10 min. When the melt flow index of EGMA is within the above range, separation from other resins during injection molding tends to be suppressed, and degreasing time tends to be shortened. The melt flow index of EGMA can be measured under conditions of 190° C. and 2.16 kg with reference to ASTM-D-1238.
[0066] (Compatibilizer) The composition for sintered compact may further contain a compatibilizer. By containing the compatibilizer, the quality of the composition for sintered compact can be further improved. The compatibilizer has properties different from those of the resin described above and the wax described below, and has an effect of further increasing the compatibility between the metal and the resin and wax, for example, due to an effect similar to that of a surfactant.
[0067] Examples of the compatibilizer include Sannix (Sanyo Chemicals), Sunflex (Sanyo Chemicals), Tafmer DF&A (Mitsui Chemicals), Tafmer XM (Mitsui Chemicals), Tafmer BL (Mitsui Chemicals), Tafmer M (Mitsui Chemicals), Tafmer PN (Mitsui Chemicals), and Maricon (Osaka Gas Chemicals).
[0068] (Fluidity imparting material) The composition for sintered compacts preferably further contains a fluidity imparting agent in addition to the above-mentioned sinterable inorganic powder and organic binder. By containing the fluidity imparting agent, the fluidity of the composition for sintered compacts can be further improved.
[0069] The fluidity imparting agent is a compound other than the resin components such as the polyacetal resin, polyolefin resin, and epoxy resin, and examples thereof include waxes. For the sake of convenience, the present specification distinguishes between those with a melting point of 100°C or less as "wax" and those with a melting point of more than 100°C as "resin." Such fluidity imparting materials are collectively referred to as the wax component (W).
[0070] Examples of the waxes include paraffin wax, polyethylene wax, polypropylene wax, carnauba wax, polyethylene glycol, polytetramethylene glycol, polytetraethylene glycol, polyisobutylene, microcrystalline wax, montan wax, beeswax, Japan wax, synthetic wax, poly-1,3-dioxolane, poly-1,3-dioxepane, etc. Among these, it is preferable to use paraffin wax, polyethylene glycol, and polytetramethylene glycol from the viewpoint of further improving the fluidity of the composition for sintered molded body in injection molding. Moreover, the waxes may be used alone or in combination of multiple types.
[0071] (Mixing method) The method for producing the composition for sintered compacts is not particularly limited, and the composition can be produced by a known method. For example, the sinterable inorganic powder and organic binder described above, as well as other optional components, can be mixed in, for example, a Henschel mixer, a tumbler, a V-shaped blender, or the like, and then melt-kneaded in a semi-molten state using a kneading machine such as a single-screw extruder, a twin-screw extruder, a heating roll, a kneader, or a Banbury mixer, to produce the composite material. The resulting composition for sintered compacts can be in various forms such as strands or pellets.
[0072] When kneading is performed using a pressure kneader, the kneading temperature is preferably set to 160°C to 210°C, and more preferably 170°C to 190°C. The rotation speed of the blade is preferably 10 rpm to 50 rpm, more preferably 15 rpm to 40 rpm. Furthermore, the kneading time is preferably 45 minutes or more and 2 hours or less. By kneading within the above range of conditions, it is possible to improve the compatibility between the resins and suppress the organic binder phenomenon caused by thermal decomposition.
[0073] (Pre-mixing) Furthermore, the organic binder can be pre-mixed (pre-mixed) before being mixed with the sinterable inorganic powder. Specifically, the aggregate resin (P) is kneaded using a kneader such as a pressure kneader, a twin-screw extruder, a heating roll, a kneader, a Banbury mixer, etc., and then the aggregate resin (P) and the wax component (W) are kneaded using a kneader such as a Henschel mixer, a tumbler, a V-shaped blender, a mixer stirrer, etc. It is also possible to carry out only one of these pre-kneading methods. Then, by kneading the sinterable inorganic powder with the pre-kneaded organic binder, the yield rate of the sintered body can be improved.
[0074] <Method of manufacturing sintered body> The method for producing a sintered body according to the present embodiment includes the steps of: A step of obtaining a molded body by injection molding a composition for sintered molded body, the composition including a sinterable inorganic powder and an organic binder; preparing a cross section of the molded body, observing the cross section, and obtaining a cross section image; performing a binarization process on the cross-sectional image to distinguish the sinterable inorganic powder from the organic binder; and calculating a ratio (A / B) of a maximum area (A) of a discontinuous organic binder portion where the organic binder is surrounded by the inorganic powder to a total area (B) of the organic binder in one field of view of the binarized cross-sectional image, and judging whether the sintered body is good or bad based on the calculation result.
[0075] (Production process of molded body) The method for producing a sintered body of the present embodiment includes a step of injection molding a composition for sintered compacts, which contains a sinterable inorganic powder and an organic binder, to obtain a compact. The green compact is also called a green compact before sintering. The green compact can be obtained by using a screw or piston type injection molding machine to mold the composition for sintered compact.
[0076] In the injection molding, the cylinder temperature is preferably set to 160 to 210° C., and more preferably 170 to 190° C. By setting the temperature to 160° C. or higher, the fluidity of the resin can be improved, and by setting the temperature to 200° C. or lower, the contamination of the mold due to the decomposition of the resin can be reduced.
[0077] The mold temperature is preferably 30 to 90° C., and more preferably 50 to 70° C. By setting the mold temperature at 30° C. or higher, dimensional stability during molding is improved, and by setting the mold temperature at 90° C. or lower, defects in the appearance of the green molded body caused by waxes having a melting point of 100° C. or lower can be suppressed.
[0078] The composition for sintered compacts, which is the material for the compacts, contains a sinterable inorganic powder and an organic binder, and the details are as described above.
[0079] (Cross-sectional image acquisition process) The method for producing a sintered body of the present embodiment includes, in addition to the step of producing the molded body, the steps of preparing a cross section of the molded body, observing the cross section, and obtaining an image of the cross section. This allows the binarization process described below to be performed.
[0080] The cross section of the molded body can be prepared using a microtome, polishing, ion milling, etc. Among these, it is preferable to use ion milling, and more preferably Ar ion milling, from the viewpoint of obtaining a smoother cross section suitable for cross section observation described later. This makes the cross section of the molded body smooth and minimizes processing marks, thereby minimizing noise generated during the binarization process described later and enabling clear binarization.
[0081] The conditions for the Ar ion milling are not particularly limited, but for example, the acceleration voltage is preferably set to 4 kV. If the acceleration voltage is lowered below this, the processing time will be longer, resulting in a decrease in work efficiency, whereas if the acceleration voltage is higher than this, the sample will be thermally damaged and may be denatured, so it is preferable to carry out ion milling under these conditions.
[0082] Furthermore, the conditions for observing the cross section of the molded body and obtaining a cross section image are not particularly limited as long as the conditions allow for accurate confirmation of the states of the sinterable inorganic powder and the organic binder. For example, the cross section of the molded body can be observed by a scanning electron microscope (SEM) to obtain a cross section image. Although the optimal magnification varies depending on the particle size of the inorganic powder, it is desirable to select an observation method with as wide a field of view as possible at a magnification that allows the organic binder to be clearly distinguished. For example, if the average particle size of the inorganic powder is about 10 μm, the magnification is preferably about 500 times, and if the average particle size of the inorganic powder is about 0.1 μm, the magnification is preferably about 2500 times.
[0083] (Binarization process of cross-sectional images) The method for producing a sintered body of this embodiment includes, in addition to the steps of producing the molded body and obtaining a cross-sectional image, a step of performing a binarization process on the cross-sectional image to distinguish between the sinterable inorganic powder and the organic binder.
[0084] A cross-sectional image of the composition for sintered compacts is obtained by SEM, and then the cross-sectional image is subjected to a binarization process, whereby the sinterable inorganic powder and the organic binder can be distinguished. When performing the binarization process, it is preferable to distinguish noise such as processing marks from sinterable inorganic powders and binders, and it is necessary to control the threshold value in the binarization and set it to a value that can distinguish between the inorganic powder and the organic binder.
[0085] Here, although there are various types of binarization processing, Otsu's adaptive binarization processing is preferable, because it allows for more accurate discrimination between the inorganic powder and the organic binder.
[0086] In Otsu's binarization process, the entire image is displayed in black and white, and a threshold is determined for the brightness to perform binarization, so depending on how the threshold is set, the binarization may be inaccurate. For example, when noise occurs due to the above-mentioned processing marks, brightness that is not due to the inorganic powder or organic binder but originates from the processing marks is generated, so the noise part may be mistakenly classified as inorganic powder or organic binder. Therefore, by adopting a method called Otsu's adaptive binarization process, in which an image is divided into small sections and binarized for each divided image, it is possible to distinguish the inorganic powder from the organic binder with higher accuracy. By attributing the brightness existing around the threshold to each image, not only is it possible to reduce the brightness gradient, but it is also possible to set the threshold in more detail, and it is possible to distinguish with high accuracy even in distinguishing noises derived from processing marks. What is important here is the setting of the adaptation range. If the image is divided into larger sections, the effect of adaptive Otsu's binarization will be weakened, but if the image is divided into finer sections, it is possible to reduce noise. This minimum range should preferably be set to a range that can enclose the largest inorganic powder particle, and the minimum range on one side should preferably be set to be equal to or greater than the diameter of the largest inorganic powder particle. Setting it in this way ensures that each image contains inorganic powder and organic binder, enabling more accurate binarization.
[0087] (Process for determining whether sintered body is good or bad) The method for producing a sintered body of the present embodiment includes, in addition to the steps of producing the molded body, acquiring a cross-sectional image, and binarizing the cross-sectional image, a step of calculating a ratio (A / B) of a maximum area (A) of a discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to a total area (B) of the organic binder in one field of view of the binarized cross-sectional image, and judging whether the sintered body is good or bad based on the calculation result. This makes it possible to accurately determine whether the resulting sintered body is good or bad.
[0088] The discontinuous organic binder portion is a region of the organic binder that is surrounded by inorganic powder, and since the evaporation path when the binder volatilizes during degreasing is blocked, if the resin volatilizes within this region, the volatilized binder that cannot be completely released to the outside may cause swelling or cracks. Therefore, in the resin composition for sintered bodies, the ratio (A / B) of the maximum area (A) of the discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view of the binarized cross-sectional image is calculated, and by using this calculated ratio (A / B), it is possible to judge whether the sintered body obtained later is good or bad, and it is also possible to recycle the defective metal powder.
[0089] FIG. 1 is an enlarged view of a part of a cross section of the composition for sintered compact, which diagrammatically illustrates a sinterable inorganic powder and an organic binder. As shown in Fig. 1, the discontinuous organic binder portion is a portion surrounded by a sinterable inorganic powder. When the cross section of the composition for sintered compact is observed, a plurality of such discontinuous organic binder portions are confirmed, and the area of the largest discontinuous organic binder portion among the discontinuous organic binder portions confirmed in one field of view is defined as the maximum area (A). The total area (B) of the organic binder is the total area of the organic binder portion observed in one field of view.
[0090] Furthermore, the threshold for determining whether the sintered body is good or bad is not particularly limited, but it is preferable that the ratio (A / B) of the maximum area (A) of the discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one visual field of the binarized cross-sectional image is 0.5 or less. By setting the ratio (A / B) of the maximum area (A) of the discontinuous organic binder portion where the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view of the binarized cross-sectional image to 0.5 or less (A / B≦0.5), it is possible to reduce the occurrence of swelling and cracks caused by the volatilized binder and increase the yield of the sintered body. From the same viewpoint, it is preferable that the ratio (A / B) is 0.3.
[0091] It is expected that a molding determined to be defective in the pass / fail judgment of the sintered body will cause a decrease in density and strength if it is subsequently sintered. The above ratio is found when the composition of the organic binder, the properties of the sinterable inorganic powder, or processing conditions such as kneading and molding conditions are not within the preferred range, and it can be said to be correlated with the dispersibility of the organic binder or the sinterable inorganic powder.
[0092] Further, the method for determining whether the sintered body is good or bad is not particularly limited, but it is preferable to make the determination by referring to an appropriate threshold value for the ratio (A / B) from a storage unit and checking the value. This is because the quality of the sintered body can be automatically determined by a computing device, allowing for more efficient production. The storage unit stores the ratio of the largest discontinuous organic binder portion (A) to the total binder area (B) that has been calculated up to that point. This storage unit can also use the stored data as training data to learn the detailed appropriate ratio for each portion. For example, if the allowable ratio differs between the thin and thick portions of a molded body, the appropriate ratio can be used to determine whether the molded body is good or bad.
[0093] Furthermore, the memory unit can also store the ratio of the maximum discontinuous organic binder portion (A) calculated up to that point to the total binder area (B), and information on the molding conditions at that time, such as the mold temperature, injection speed, dwell pressure, and cycle time. Therefore, by using the stored data as training data, it is possible to learn the correlation between the ratio and the molding conditions, which can be used to appropriately change the molding conditions.
[0094] (Injection molding condition change process) In addition, it is preferable that the manufacturing method of the sintered body of this embodiment further includes a step of changing the conditions of the injection molding so as to suppress the occurrence of defects after the sintered body is judged to be defective in the judgment of whether it is good or bad. This makes it possible to increase the number of good sintered bodies, leading to a higher yield.
[0095] As described above, by using the data stored in the storage unit as teacher data, it is possible to learn the correlation between the ratio (A / B) of the discontinuous organic binder part (A) to the total binder area (B) and the molding conditions, so that the molding conditions can be changed to appropriate ones. The change to appropriate molding conditions can be made by a system in which the device automatically inputs the molding conditions into the injection molding machine, or an operator can change the molding conditions based on the displayed molding conditions.
[0096] (Other processes) In addition, in the manufacturing method of the sintered body of this embodiment, in addition to the above-mentioned process of producing a molded body, the process of acquiring a cross-sectional image, the process of binarizing the cross-sectional image, and the process of changing the injection molding conditions, the process necessary for manufacturing a sintered body can be appropriately carried out. For example, there may be mentioned a degreasing step for degreasing the green body, and a sintering step for sintering the green body after degreasing. The conditions for the debinding step and the sintering step are not particularly limited, and known conditions can be appropriately adopted depending on the required performance.
[0097] In addition, the method for detecting defects in sintered bodies according to the present embodiment may further include a recycling step in which, when a sample (a composition for sintered body or a green body) in which defects are predicted is found, the organic binder is separated and removed from the sample by acid, heating, washing, etc., to recycle the sinterable inorganic powder. This can further reduce the cost of producing sintered bodies. The recycling step can be performed automatically by a device, or an operator can collect defective samples and perform recycling.
[0098] <Sintered body manufacturing system> The manufacturing system for a sintered body according to the present embodiment includes: A composition for sintered compacts, which contains a sinterable inorganic powder and an organic binder, is injection molded to obtain a compact, and then, A cross section of the molded body is prepared, and the cross section is observed to obtain a cross section image; performing a binarization process on the cross-sectional image to distinguish the sinterable inorganic powder from the organic binder; Then, the ratio (A / B) of the maximum area (A) of the discontinuous organic binder portion where the organic binder is surrounded by the inorganic powder to the total area (B) of the organic binder in one field of view of the binarized cross-sectional image is calculated, and the quality of the sintered body is judged based on the calculation result. By employing the system of this embodiment, defects in sintered bodies can be predicted with high accuracy without sintering, and defective metal powder can be recycled.
[0099] Each configuration of the system for producing a sintered body according to this embodiment is similar to that described in the method for producing a sintered body according to this embodiment described above. EXAMPLES
[0100] The present invention will be described in detail below with reference to specific examples and comparative examples, but the present invention is not limited to the following examples.
[0101] <Components> The components contained in each sample of the examples and comparative examples are shown below. (A) Polyacetal resin Tenac (registered trademark)-C FF520 manufactured by Asahi Kasei Corporation
[0102] (B) Epoxy resin (B-1) Bondfast CG5001 manufactured by Sumitomo Chemical Co., Ltd. (B-2) Bondfast BF-7B manufactured by Sumitomo Chemical (B-3) Bondfast BF-7M manufactured by Sumitomo Chemical
[0103] (C) Polyolefin resin (C-1) Polypropylene: SunAllomer PP PMB60A manufactured by SunAllomer Co., Ltd. (C-2) Polyethylene: Suntech (registered trademark) HDPE J300 manufactured by Asahi Kasei Corporation
[0104] (D) Fluidity imparting agent (D-1) Paraffin wax: Paraffin wax SP-0145 manufactured by Nippon Seiro Co., Ltd. (D-2) Carnauba wax: Refined Carnauba Wax No. 1 manufactured by Nippon Wax Co., Ltd. (D-3) Montan wax: Clariant Japan LicoWax E
[0105] (E) Compatibilizer (E-1) Mitsui Chemicals Toughmer PN-2070 (E-2) Sanyo Chemical Sannix GL-3000 (E-3) Mitsui Chemicals Toughmer XM-7070S (E-4) Mitsubishi Chemical PTMG3000
[0106] Aggregate resin (P) The above components (A), (B), (C), and (E) are collectively referred to as aggregate resin (P). Wax (W) In the following description, the (D) fluidity imparting agent will be referred to as a wax (W).
[0107] [Examples 1 to 6 and Comparative Examples 1 to 2] Each material was weighed out so as to obtain the blend ratio shown in Tables 1 and 2. Then, for samples with a check mark for "Crushing" of the aggregate resin (P), the aggregate resin (P) was kneaded at 180°C using a twin-screw extruder, and then freeze-crushed (-196°C) to obtain a powder with a sieve passing rate of 55% at 50 Mesh (300 μm). For samples marked with a circle in the "pre-mixing" of aggregate resin (P) and wax (W), the aggregate resin (P) was mixed at 180°C using a twin-screw extruder, and then the wax (W) and aggregate resin (P) were mixed at 300 rpm for approximately 5 minutes using a Henschel mixer. Furthermore, for samples with a check mark for both "Crushing" and "Pre-mixing" of the aggregate resin (P), the aggregate resin (P) was kneaded at 180°C using a twin-screw extruder, then freeze-pulverized (-196°C) to obtain a powder with a sieve passing rate of 55% at 50 Mesh (300 μm). The wax (W) and aggregate resin (P) were then kneaded using a Henschel mixer at 300 rpm for approximately 5 minutes. For each of the kneaded products obtained by the above-mentioned method, SUS316L (average particle size 10 μm) was used as the sinterable inorganic powder, and the sinterable inorganic powder and organic binder were weighed out in a ratio of 65 volume % and 35 volume %. Each sample of the composition for sintered compacts was produced in a pressure kneader under the conditions of temperature, blade rotation speed, and kneading time shown in Tables 1 and 2. Thereafter, each sample of the obtained composition for sintered compacts was cooled, crushed, and pelletized to prepare a raw material for injection molding, and then a plurality of molded specimens were produced using an injection molding machine (ROBOSHOT α-50iA manufactured by Fanuc Corporation) under the conditions of molding temperature, mold temperature, injection pressure, and injection speed shown in Tables 1 and 2. The produced molded specimens were all tensile dumbbell specimens of type 2 conforming to JIS K 6251, with a total length of 100 mm and a thickness of 3 mm.
[0108] Each of the produced molded test pieces was degreased by heating or with an acid. The produced compact test pieces were set in a degreasing furnace at intervals of 50 mm, and then the following degreasing treatment and sintering were carried out to obtain sintered body samples. (heat degreasing) The inside of the degreasing furnace was purged with nitrogen gas, and the temperature was raised to 150°C at 50°C / hr. Thereafter, the temperature was raised from 150 to 200°C at a rate of 30°C / hr and held for 1 hour, then the temperature was raised from 200 to 400°C at 30°C / hr, and then the temperature was raised from 400 to 600°C at 120°C / hr, and the furnace was cooled to obtain each degreasing sample. (Acid degreasing) The inside of the degreasing furnace was first heated to 110°C and purged with 500 L / h of nitrogen for 30 minutes. Then, 30 mL / h of 98% nitric acid was fed while maintaining the nitrogen purge. The acid feed was maintained for 2.5 hours, followed by purging the furnace with 500 L / h of nitrogen for 45 minutes and cooling to room temperature to obtain each sample of the degreased body. (Sintering) The degreased bodies of each sample were sintered in an argon atmosphere by gradually increasing the temperature from room temperature at 200°C / hr and holding the temperature at a maximum of 1350°C for 2 hours to obtain sintered samples.
[0109] <Evaluation> (1) Section preparation Cross sections were prepared from each of the produced green body test pieces by Ar ion milling (X) or a microtome (Y). (Ar ion milling X) The center of the parallel part of each compact test piece was cut in the direction perpendicular to the flow using a diamond disc cutter, and then the cross section was prepared by Ar ion milling. The Ar ion milling device used was an IM-4000 (Hitachi High-Technologies Corporation). (Microtome Y) The center of the parallel part of each molded specimen was cut in the direction perpendicular to the flow direction with a diamond disc cutter, and then the cross section was prepared with a microtome. A rotary microtome (manufactured by Leica) was used as the microtome device.
[0110] (2) Cross-sectional observation The cross section thus obtained was observed by SEM, and 10 images were taken at a magnification of 500. The SEM device used was a JSM IT-800 (manufactured by JEOL Ltd.).
[0111] (3) Binarization (3-1) Whether or not binarization is performed If Otsu's adaptive binarization was used on the obtained image, it was marked as "O", and if it was not used, it was marked as "X". When Otsu's adaptive binarization was applied to the obtained image, the sinterable inorganic powder part and the organic binder part were separated. Figure 2 (a) shows an example of a cross section of a molded test piece before binarization, and (b) shows an example of a cross section of a molded test piece after binarization. (3-2) Scope of binarization processing When Otsu's adaptive binarization was used on the obtained images, the minimum range of adaptation was set as the ratio of the length of one side to the diameter of the largest inorganic powder particle appearing in one field of view (length of one side / diameter of largest inorganic powder particle × 100%). (3-3) Ratio (A / B) After applying Otsu's adaptive binarization to the obtained images, the organic binder area was divided into discontinuous organic binder areas (A) and the total binder area (B), and the ratio (A / B) of the largest discontinuous organic binder area (A) in the image to the total binder area (B) was calculated. Then, the average value (number of samples = 10) and standard deviation (number of samples = 10) of the calculated ratio (A / B) were calculated.
[0112] (4) Density of sintered body The density (g / cm3) of the obtained sintered body was measured in accordance with JIS Z 8807 using an electronic specific gravity meter (manufactured by Alpha Mirage) at a water temperature of 25°C. 3 The number of samples was 30, and the average relative density of the SUS316L powder used is shown in Tables 1 and 2.
[0113] (5) Tensile strength of sintered body The sintered body thus obtained was subjected to a tensile test to measure the tensile strength. The measurement was performed using a universal testing machine, 5900R 5582 model (manufactured by Instron Corporation), at a test speed of 3.0 mm / min and a chuck distance of 30 mm. Thirty samples were used.
[0114] (6) Yield rate of sintered body Based on the results of (4) density of sintered body and (5) tensile strength of sintered body mentioned above, samples with a relative density of 95% or more and a tensile strength of 480 MPa or more were defined as non-defective products, and the percentage of non-defective products out of 30 samples was calculated as the yield rate. The results are shown in Tables 1 and 2.
[0115] (7) Recyclability of metal powder In the cross-sectional observation in the above evaluation (2), for those in which the ratio (A / B) of the maximum discontinuous organic binder portion (A) to the total binder area (B) in the image was 0.5 or more, the molded bodies were heated at 500°C for 5 hours to remove the binder, and then immersed in o-dichlorobenzene at 150°C for cleaning to obtain inorganic powder. Using the obtained inorganic powder, sintered bodies were produced under the conditions of Example 1, and samples with equivalent yield rates were obtained in all cases. In addition, for those in which the ratio (A / B) of the maximum discontinuous organic binder portion (A) to the total binder area (B) in the image was 0.5 or more, inorganic powder was extracted from some of the molded bodies by the above-mentioned method. When a sintered body was produced using the obtained inorganic powder under the same conditions as in Example 1, a sample with a comparable yield rate was obtained. [Table 1] [Table 2] [Industrial Applicability]
[0116] According to the present invention, it is possible to provide a method for producing a sintered body, which can accurately predict defects in a sintered body without sintering, and enables recycling of defective metal powder.
Claims
1. A step of obtaining a molded body by injection molding a composition for sintered molded body, the composition including a sinterable inorganic powder and an organic binder; preparing a cross section of the molded body, observing the cross section, and obtaining a cross section image; performing a binarization process on the cross-sectional image to distinguish the sinterable inorganic powder from the organic binder; a step of calculating a ratio (A / B) of a maximum area (A) of a discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to a total area (B) of the organic binder in one visual field of the binarized cross-sectional image, and judging whether the sintered body is good or bad based on the calculation result; A method for producing a sintered body, comprising:
2. 2. The method for producing a sintered body according to claim 1, wherein the cross section of the compact is prepared by ion milling.
3. 3. The method for producing a sintered body according to claim 1, wherein the binarization process of the cross-sectional image is Otsu's adaptive binarization process.
4. 4. The method for producing a sintered body according to claim 3, wherein the length of one side of the minimum range of the adaptive range used in the Otsu's adaptive binarization process is equal to or greater than the maximum particle size of the sinterable inorganic powder.
5. 3. The method for producing a sintered body according to claim 1, wherein the quality of the sintered body is judged based on whether a ratio (A / B) of a maximum area (A) of a discontinuous organic binder portion in which the organic binder is surrounded by the inorganic powder to a total area (B) of the organic binder in one visual field of the binarized cross-sectional image is 0.5 or less.
6. In the judgment of whether the sintered body is good or bad, after it is judged to be bad, 3. The method for producing a sintered body according to claim 1, further comprising the step of changing the conditions of the injection molding so as to suppress the occurrence of defects.
Citation Information
Patent Citations
Metallizing method on surface of formed plastic article
JP1984070794A
Injection molding composition
JP4317916B1