COMPOSITION COMPRISING Ti COMPOUND, Si COMPOUND, AND SOLVENT
A composition of titania nanoparticles with organic chains and a Si compound improves adhesion and stability, addressing peeling and agglomeration issues in photocatalytic coatings, enhancing transparency and photocatalytic activity.
Patent Information
- Application Number
- JP2023050234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing photocatalytic titanium oxide compositions face issues with adhesion to substrates, transparency, and dispersion stability, leading to peeling and agglomeration, which affect their durability and effectiveness.
A composition comprising titania nanoparticles with organic chains like acetyl or acetoxy groups bonded to their surface, combined with a Si compound such as TEOS, and a solvent like alcohol, enhances dispersibility and stability, forming a titania particle composite binder through a hydrolysis reaction.
The composition improves adhesion, transparency, and solvent stability, reducing agglomeration and peeling, while maintaining high photocatalytic activity and antibacterial properties.
Smart Images

Figure 2024139342000001 
Figure 2024139342000002 
Figure 2024139342000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition containing a Ti compound, a Si compound, and a solvent. [Background technology]
[0002] Titanium oxide (TiO2) has photocatalytic activity and exhibits unique properties such as superhydrophilicity under ultraviolet light. Titanium oxide is expected to be applied in a variety of situations, including as an anti-fouling coating for wallpaper, a deodorizing coating for automobiles, and a hydrogen generation catalyst. In order to improve the weakness of titanium oxide, which is that it is only effective under ultraviolet light, visible light-responsive photocatalysts that are responsive to visible light have been developed.
[0003] Patent Document 1 discloses an antibacterial and antiviral agent that is composited with an inorganic metal. Patent Document 2 discloses a photocatalytic material that imparts a photocatalytic effect without impairing the design of the substrate by finely controlling the particle size of titanium oxide and improving transparency to visible light.
[0004] Photocatalytic titanium oxide is a material that is expected to be used in a variety of situations in the future.
[0005] However, there have been problems with fixing titanium oxide to a substrate. When titanium oxide is used for a long period of time, the titanium oxide wears off or peels off from the substrate due to external factors such as rain and wind, and the effect of titanium oxide does not last.
[0006] Therefore, it has been proposed to combine titanium oxide with a silica-based binder to improve the adhesion to the substrate.
[0007] Patent Documents 3 and 4 disclose photocatalysts in which titanium oxide, colloidal silica, a Si-based binder, and the like are combined to improve adhesion.
[0008] Conventionally, however, there is a problem that the dispersion stability of titanium oxide in the liquid decreases due to the difference in surface energy, and the transparency of the liquid decreases. As the titanium oxide aggregates in the liquid, the dispersion stability of the entire liquid decreases, and the titanium oxide precipitates and separates in the liquid during long-term storage, which causes problems in use. Although the titanium oxide composited with a binder has improved adhesion compared to titanium oxide that does not contain a binder, the titania sol aggregates, which causes peeling and cracking of the film containing titanium oxide, which is a durability problem.
[0009] Photocatalysts using titanium oxide are desired to exhibit transparency, durability, solvent stability, photocatalytic activity, and the like, all at the same time, in packaging. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Patent No. 6714530 [Patent Document 2] Patent No. 6607407 [Patent Document 3] Patent No. 7121356 [Patent Document 4] Patent Publication No. 09-075243 Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a composition which is excellent in adhesion to a substrate, transparency, and dispersion stability of the solution, and which has antibacterial and antiviral effects. [Means for solving the problem]
[0012] The present invention includes a composition containing the following Ti compound, Si compound, and solvent.
[0013] Section 1. A composition containing a Ti (titanium) compound (titania nanoparticles), a Si compound (silicon, Si binder), and a solvent, The Si compound is a hydrolyzate of an alkylsilane, The Ti compound has a mass loss of 0.1% by mass or more at 200°C or higher when the Ti compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomeasuring device; The average primary particle size of the Ti compound is 1 nm to 50 nm, The composition, wherein the solvent comprises water and alcohol.
[0014] Section 2. 2. The composition according to item 1, wherein the Ti compound exhibits a mass loss of 1% or more at 200° C. or higher when the Ti compound is heated to 600° C. using a simultaneous differential thermogravimetry and thermomechanical analysis apparatus.
[0015] Section 3. 2. The composition according to item 1, wherein the Ti compound exhibits a mass loss of 5% by mass or more at 200° C. or higher when the Ti compound is heated to 600° C. using a simultaneous differential thermogravimetry and thermomechanical analysis apparatus.
[0016] Section 4. 2. The composition according to item 1, wherein the Ti compound has an average primary particle size of 1 nm to 20 nm.
[0017] Section 5. 2. The composition according to item 1, wherein the Ti compound has an average primary particle size of 1 nm to 10 nm.
[0018] Section 6. Item 2. The composition according to item 1, wherein the Ti compound has an organic chain bonded to a surface thereof.
[0019] Section 7. 2. The composition according to item 1, wherein the Ti compound has at least one organic chain selected from the group consisting of an acetyl group and an acetoxy group bonded to a surface thereof.
[0020] Section 8. 2. The composition according to item 1, wherein the content of the Ti compound in the composition is 0.01% by mass to 5% by mass.
[0021] Section 9. 2. The composition according to item 1, wherein the content of the Si compound in the composition is 0.01% by mass to 20% by mass.
[0022] Section 10. 2. The composition according to item 1, wherein the Ti compound and the Si compound are contained in a ratio of 0.02 to 20 by mass relative to the Si compound in the composition.
[0023] Section 11. 2. The composition according to item 1, wherein the Ti compound and the Si compound are contained in the composition in a ratio of 0.1 to 1 in terms of mass ratio relative to the Si compound.
[0024] Section 12. Item 2. The composition according to item 1, wherein the Si compound is a hydrolysis product of TEOS.
[0025] Section 13. Item 2. The composition according to item 1, further comprising at least one metal selected from the group consisting of silver, copper, and platinum.
[0026] Section 14. 14. An antibacterial and antiviral coating film comprising the composition according to any one of items 1 to 13.
[0027] Section 15. A method for producing a composition containing a Ti compound, a Si compound, and a solvent, comprising the steps of: (1) bonding an organic chain to the surface of a Ti compound in a solvent; and (2) mixing the Ti compound having the organic chain bonded thereto obtained in step (1) with a Si compound in a solvent to hydrolyze the Si compound; A manufacturing method comprising: Effect of the Invention
[0028] In the past, titania particles and a binder, which is a hydrolyzate of alkoxysilane, were added separately to improve the adhesion to the substrate. In the conventional method, the stability of the titania particles decreases, causing aggregation, resulting in a decrease in transparency and precipitation of the liquid.
[0029] In the present invention, first, the dispersibility of titania particles is improved by adding an organic substance to the surface of fine titania particles, then, the titania particles are mixed with alkoxysilane, which is a raw material for a binder, and a hydrolysis reaction is carried out while maintaining high dispersibility in the coexistence of both, to produce a titania particle composite binder.
[0030] The present invention uses a new process to prepare a composition containing titania particles, thereby making it possible to improve the aggregation of titania, which has been a problem in the past, and to greatly improve solvent stability and adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention will be described in detail below.
[0032] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.
[0033] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."
[0034] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."
[0035] In this specification, the designations parts, % etc. are generally used.
[0036] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.
[0037] [1] A composition containing a Ti compound, a Si compound, and a solvent The composition of the present invention containing a Ti (titanium) compound, a Si (silicon) compound, and a solvent is The Si compound is a hydrolyzate of an alkylsilane, The Ti compound has a mass loss of 0.1% by mass or more at 200°C or higher when the Ti compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomeasuring device; The average primary particle size of the Ti compound is 1 nm to 50 nm, The solvent includes water and alcohol.
[0038] In the composition of the present invention, the Ti compound preferably exhibits a mass loss of 1% or more, more preferably 5% or more, at 200°C or higher when the Ti compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomechanical analyzer.
[0039] In the composition of the present invention, the average primary particle size of the Ti compound is preferably from 1 nm to 20 nm, and more preferably from 1 nm to 10 nm.
[0040] In the composition of the present invention, the Ti compound preferably has an organic chain bonded to its surface, and more preferably has at least one type of organic chain selected from the group consisting of an acetyl group and an acetoxy group bonded to its surface.
[0041] In the composition of the present invention, the content of the Ti compound in the composition is preferably 0.01% by mass to 5% by mass.
[0042] In the composition of the present invention, the content of the Si compound in the composition is preferably 0.01% by mass to 20% by mass.
[0043] In the composition of the present invention, the content ratio of the Ti compound and the Si compound in the composition is preferably such that, relative to the Si compound (1 part by mass), the Ti compound is contained in a mass ratio of 0.02 to 20 (0.02 parts by mass to 20 parts by mass), and more preferably, the Ti compound is contained in a mass ratio of 0.1 to 1 (0.1 parts by mass to 1 part by mass).
[0044] In the composition of the present invention, the Si compound is preferably a hydrolysis product of TEOS (Tetraethyl orthosilicate, Si(OC2H5)4, tetraethyl orthosilicate, tetraethoxysilane).
[0045] The composition of the present invention preferably further contains at least one metal selected from the group consisting of silver, copper, and platinum.
[0046] The present invention includes an antibacterial and antiviral coating film comprising the composition of the present invention.
[0047] [1-1] Composition containing a Ti compound, a Si compound, and a solvent The composition contains a Ti compound (titania nanoparticles), a Si compound, and a solvent, and the Si compound is a Si binder and is a hydrolysate of an alkylsilane (such as TEOS).
[0048] The Ti compound preferably has an organic chain bonded to the surface, and when the Ti compound is heated to 600°C using a differential thermogravimetry and thermomechanical simultaneous measurement device, the mass loss at 200°C or higher is 0.1% by mass or more.
[0049] The average primary particle size of the Ti compound is 1 nm to 50 nm.
[0050] Solvents include water and alcohols (1-propanol, 1-butanol, etc.).
[0051] A composition containing a Ti compound, a Si compound (Si binder), and a solvent can improve the cohesion of titania, and can greatly improve the solvent stability and adhesion.
[0052] [1-2] Ti compounds (titania nanoparticles) Water, inorganic acids, free organic acids, etc. generally evaporate at temperatures below 200°C.
[0053] The Ti compound (titania nanoparticles) contained in the composition of the present invention has acetyl groups (CH3-C(=O)-, Ac), acetoxy groups (acetyloxy group, CH3-C(=O)-O-, AcO) and the like bonded to at least some of the titanium atoms present on the surface, which are gradually eliminated in the range of 200°C to 600°C. For example, in the case of acetoxy groups, they are gradually eliminated in the range of 200°C to 600°C, reaching a peak at about 260°C.
[0054] The Ti compound contained in the composition of the present invention can improve the dispersibility of titania particles by imparting an organic substance to the surface of fine titania particles.
[0055] The Ti compound contained in the composition of the present invention preferably has an organic chain such as an acetyl group or an acetoxy group bonded to at least some of the titanium atoms present on the surface, which can suppress aggregation of titania nanoparticles during drying or firing, making it less likely to crack or peel off, and providing particularly excellent coatability and transparency.
[0056] The Ti compound contained in the composition of the present invention can suppress cracking, peeling, and the like, and can easily form a strong composite with metals, resulting in excellent visible light catalytic activity.
[0057] The Ti compound contained in the composition of the present invention is capable of suppressing aggregation of titania nanoparticles during drying or firing, and is therefore particularly effective in suppressing cracking, peeling, and the like.
[0058] In the Ti compound, preferably, an organic chain such as an acetyl group or an acetoxy group is bonded to the titanium atom present on the surface. When an organic chain such as an acetyl group or an acetoxy group is present on at least a part of the titanium atoms present on the surface, the organic chain is gradually released in the range of 200°C to 600°C, and therefore, when the temperature is increased by a thermogravimetric and differential thermal analyzer (TG-DTA), the mass loss is large at 200°C or higher.
[0059] When Ti compounds are heated using a thermogravimetry-differential thermal analyzer (TG-DTA), the mass loss at temperatures above 200°C is an index of the number of organic chains, such as acetyl groups and acetoxy groups, that are bonded to titanium atoms on the surface.
[0060] The mass loss of the Ti compound at 200° C. or higher when heated to 600° C. by a thermogravimetry-differential thermal analyzer (TG-DTA) is 0.1% by mass or more, preferably 1% by mass or more, and more preferably 5% by mass or more. The upper limit of the mass loss of the Ti compound is preferably 20% by mass.
[0061] The detailed conditions for the thermogravimetry-differential thermal analyzer (TG-DTA) were as follows: atmosphere: air, heating rate: 3° C. / min.
[0062] The Ti compound is preferably one in which an organic chain such as an acetyl group or an acetoxy group is bonded to at least some of the titanium atoms present on the surface.
[0063] The organic chain is an acetyl group (CH3-C(=O)-), an acetoxy group (CH3-C(=O)-O-), etc., from the viewpoints of water solubility, odor, volatility, harmfulness, decomposability, etc.
[0064] The organic chain may be at least one type of organic chain selected from the group consisting of the above organic chains, and one type of organic chain may be bonded alone, or two or more types of organic chains may be bonded depending on the purpose.
[0065] The average primary particle size of the Ti compound is 1 nm to 50 nm, more preferably 1 nm to 20 nm, and even more preferably 1 nm to 10 nm. By adjusting the average particle size of the Ti compound to this range, the Ti compound can be appropriately and more firmly composited with metals (silver and copper). The titania nanoparticles can form a film with higher visible light catalytic activity and higher transparency. The Ti compound has excellent coating properties.
[0066] The average particle size of the Ti compound (titania nanoparticles) is measured by observation with a transmission electron microscope (TEM).
[0067] The specific surface area of the Ti compound is preferably 150 m 2 / g~500m 2 / g, more preferably 200m 2 / g~400m 2 / g. By adjusting the specific surface area of the Ti compound to this range, the Ti compound can be appropriately and more firmly composited with metals (silver and copper). The Ti compound has high visible light catalytic activity.
[0068] The specific surface area of the Ti compound is measured by the BET method.
[0069] The Ti compound can have the N, Cl, and S element concentrations of 0 to 5,000 ppm, and more preferably 0 to 1,000 ppm. By adjusting the N, Cl, and S element concentrations of the Ti compound to within this range, corrosion of the substrate can be suppressed. The N, Cl, and S element concentrations of the Ti compound mean that there is no impurity derived from the acidic Ti compound precursor such as TiCl4 or TiOSO4, or there are only a very small amount of impurities.
[0070] The concentrations of N, Cl, and S elements in the Ti compound are measured by WDX (fluorescent X-ray).
[0071] The crystalline form of the Ti compound is preferably anatase type, and the titania nanoparticles preferably do not contain any crystalline form other than anatase type. By adopting anatase type, the Ti compound has improved visible light catalytic activity. The Ti compound preferably does not contain any crystalline form other than anatase type, and is 100% anatase type.
[0072] [1-3]Si (silicon) compounds (Si binders) The Ti compound (titania particles) contained in the composition of the present invention can improve the dispersibility of the titania particles by adding an organic substance to the fine titania surface.
[0073] By mixing Ti compounds (titania particles) with alkoxysilanes (Si compounds), which are the raw materials for the binder, and allowing the two to coexist while maintaining high dispersibility, a titania particle composite binder can be produced.
[0074] The composition of the present invention can improve the aggregation of titania, and can greatly improve the solvent stability and adhesion.
[0075] The Si compound is a hydrolysis product of alkylsilane (alkoxysilane).
[0076] As the alkylsilane (alkoxysilane), preferably, monoalkoxysilane, dialkoxysilane, trialkoxysilane, tetraethoxysilane, or the like is used.
[0077] As the monoalkoxysilane, trimethylmethoxysilane, trimethylethoxysilane, or the like is preferably used.
[0078] As the dialkoxysilane, preferably dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldiethoxysilane, diethyldiethoxysilane, diisobutyldimethoxysilane, dimethoxymethyl-n-octylsilane, or the like is used, and more preferably dimethyldimethoxysilane, dimethyldiethoxysilane, or the like is used.
[0079] The trialkoxysilane is preferably methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, ethyltriisopropoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-propyltrippropoxysilane, n-propyltriisopropoxysilane, isopropyltrimethoxysilane, isopropyltrimethoxysilane, isopropyltrimethoxysilane, isopropyl Tripropoxysilane, n-butyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-octyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, etc. are used, and more preferably methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, etc. are used.
[0080] The tetraalkoxysilane is preferably tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, or the like, and more preferably tetraethoxysilane (tetraethyl orthosilicate), tetramethoxysilane, or the like.
[0081] The alkylsilane may be at least one compound selected from the group consisting of the above alkylsilanes. These alkylsilanes may be used alone or in combination (blended) in two or more types depending on the purpose.
[0082] The Si compound is particularly preferably a hydrolysis product of TEOS (tetraethyl orthosilicate, tetraethoxysilane).
[0083] [1-4] Solvent Solvents include water and alcohols.
[0084] The alcohol is preferably an aliphatic alcohol having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, or isopropanol; a non-aliphatic alcohol, such as α-terpineol; a glycol solvent, such as butyl carbitol (diethylene glycol monobutyl ether), hexylene glycol (2-methyl-2,4-pentanediol), ethylene glycol-2-ethylhexyl ether, ethylene glycol monomethyl ether, or propylene glycol monomethyl ether; or a diol, such as 1,4-butanediol, 1,5-pentanediol, or 1,6-hexanediol.
[0085] The solvent of the composition may be changed. Water may be removed from the reaction solution by centrifugation, filtration membrane, etc., and replaced with an organic solvent.
[0086] The alcohol may be at least one compound selected from the group consisting of the above alcohols. These alcohols may be used alone or in combination (blend) of two or more depending on the purpose.
[0087] [1-5] Metal The composition of the present invention preferably further contains at least one metal selected from the group consisting of silver, copper, and platinum.
[0088] In the composition, by compounding a metal (silver, silver salt, etc.) with a Ti compound (titania nanoparticles), the coatability and transparency of the composition can be easily maintained, and the antibacterial activity, antiviral activity, and photocatalytic activity in a dark place can be particularly improved.
[0089] When a silver salt is used as the silver compound, the silver salt is preferably a silver salt whose aqueous solution is acidic or neutral. The silver salt preferably used is silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc.
[0090] The silver salt may be at least one compound selected from the group consisting of the above silver salts. These silver salts may be used alone or in combination (blend) of two or more depending on the purpose.
[0091] The amount of at least one metal selected from the group consisting of silver (silver salt), copper, and platinum used is preferably 50 mass % or less, more preferably 0.01 mass % to 40 mass %, and even more preferably 0.01 mass % to 25 mass %, relative to titanium oxide in the Ti compound (titania nanoparticles), calculated as the mass of silver element in the silver salt, from the viewpoints of facilitating the complexation of the metal (silver, silver salt, etc.) with the Ti compound (titania nanoparticles) and of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the Ti compound (titania nanoparticles), and the like.
[0092] By adjusting the amount of metal (silver, silver salt, etc.) used within this range, it becomes easy to combine the metal (silver, silver salt, etc.) with the Ti compound (titania nanoparticles), it becomes easier to maintain the coatability and transparency, and it is possible to particularly improve the antibacterial activity, antiviral activity, and photocatalytic activity in dark places.
[0093] [1-6] Dispersion containing Ti compound, Si compound, and solvent The Ti compound (titania particles) contained in the composition of the present invention can improve the dispersibility of the titania particles by adding an organic substance to the fine titania surface.
[0094] By mixing Ti compounds (titania particles) with alkoxysilanes (Si compounds), which are the raw materials for the binder, and allowing the two to coexist while maintaining high dispersibility, a titania particle composite binder can be produced.
[0095] The composition of the present invention can improve the aggregation of titania, and can greatly improve the solvent stability and adhesion.
[0096] The composition of the present invention has good dispersibility, and as a result, the coating has excellent crack resistance. The composition of the present invention enables a dense titania coating, and has excellent coatability and transparency, as well as excellent visible light catalytic activity.
[0097] In the composition, the content of the Ti compound is preferably 0.01% by mass to 5% by mass in the composition from the viewpoints of ease of coating, film properties of the coating, and the like.
[0098] In the composition, the content of the Si compound is preferably 0.01% by mass to 20% by mass in the composition from the viewpoints of ease of coating, film properties of the coating, and the like.
[0099] In the composition, from the viewpoints of ease of coating, coating film properties, and the like, the content ratio of the Ti compound to the Si compound is preferably 0.02 to 20 (0.02 parts by mass to 20 parts by mass) of the Ti compound relative to the Si compound (1 part by mass), and more preferably 0.1 to 1 (0.1 parts by mass to 1 part by mass) of the Ti compound.
[0100] The pH of the composition (dispersion) varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.
[0101] The dispersion containing the Ti compound, the Si compound, and the solvent is preferably adjusted in viscosity according to the application to prepare a coating material. When the coating material is applied by spin coating, dip coating, spraying, or the like, the viscosity is preferably adjusted to be low. When the coating material is applied by brush coating, squeegee method, or the like, the viscosity is preferably adjusted to be higher. When the coating material is applied by screen printing, the viscosity is preferably adjusted to be even higher to suppress the flowability.
[0102] The resulting coating film allows for a dense coating.
[0103] The present invention includes an antibacterial and antiviral coating film comprising the composition of the present invention.
[0104] The coated product having a coating film is not particularly limited, and examples thereof include building materials, building exteriors, building interiors, window frames, window glass, various lenses, structural members, building facilities such as housing, cooking utensils, textile products, furniture, displays, display protective films, plumbing members, vehicle lighting covers and window glass, mechanical equipment or exteriors of articles, dustproof covers and coatings, display devices, their covers, traffic signs, various display devices, display objects such as billboards, sound insulation walls for roads and railways, exteriors and coatings of bridges and guardrails, interiors and coatings of tunnels, insulators, solar cell covers, solar hot water heater heat collector covers, and other exterior parts of electronic and electrical devices used outside, particularly transparent members, exteriors of vinyl greenhouses, greenhouses, and the like.
[0105] [2] Method for producing a composition containing a Ti compound, a Si compound, and a solvent The method for producing a composition containing a Ti (titanium) compound, a Si (silicon) compound, and a solvent of the present invention includes the steps of: (1) bonding an organic chain to the surface of a Ti compound in a solvent; and (2) mixing the Ti compound having the organic chain bonded thereto obtained in the step (1) with a Si compound in a solvent to hydrolyze the Si compound.
[0106] In the production method of the present invention, first, an organic substance is applied to the surface of fine titania particles to improve the dispersibility of the titania particles.
[0107] In the manufacturing method of the present invention, the titania particles are then mixed with alkoxysilane, which is a raw material for the binder, and a hydrolysis reaction is carried out in the coexistence of the two while maintaining high dispersibility, to produce a titania particle composite binder.
[0108] The manufacturing method of the present invention uses a new process to prepare a composition containing titania particles, which can improve the aggregation of titania, which has been a problem in the past, and can greatly improve solvent stability and adhesion.
[0109] [2-1] (1) A step of bonding an organic chain to the surface of a Ti compound in a solvent (Preparation of Coating Composition) In the production method of the present invention, first, an organic substance is applied to the surface of fine titania particles to improve the dispersibility of the titania particles.
[0110] In step (1), an organic chain is bonded to the surface of a Ti compound in a solvent.
[0111] The Ti compound (substance containing titanium) is preferably a substance that becomes titanium oxide when heated. The substance containing titanium is preferably titanium oxide and / or a titanium oxide precursor, and more preferably titanium oxide; titanium hydroxide; titanium alkoxide; titanium halide such as titanium trichloride or titanium tetrachloride (particularly, those neutralized with a base); metallic titanium, etc. are used.
[0112] From the viewpoints of dispersibility, coatability, and visible light catalysis of the resulting titania, the titanium-containing substance is preferably titanium alkoxide, titanium hydroxide, or titanium halide (particularly, one neutralized with a base). From the viewpoints of purity, dispersibility, coatability, transparency, and visible light catalysis, the titanium-containing substance is more preferably titanium alkoxide.
[0113] The titanium alkoxide is preferably titanium tetraisopropoxide, titanium tetra n-butoxide, titanium tetra n-propoxide, titanium tetraethoxide, etc. From the viewpoints of cost, water solubility of by-products, coatability, and visible light catalytic property, the titanium alkoxide is more preferably titanium tetraisopropoxide.
[0114] The Ti compound may be at least one compound selected from the group consisting of the Ti compounds described above. These Ti compounds may be used alone or in combination (blend) of two or more types depending on the purpose.
[0115] The average particle size of the Ti compound is preferably 100 nm or less, more preferably 50 nm or less. The lower limit of the average particle size of the titanium-containing substance is not particularly set, and is preferably about 1 nm. When the particle size is large, it is preferable to use a planetary ball mill, a paint shaker, or the like, after grinding in a dry or wet manner.
[0116] The average particle size of Ti compounds (solids such as titanium oxide and metallic titanium) is measured by observation with a transmission electron microscope (TEM).
[0117] The concentration of the Ti compound in the dispersion is preferably 0.01 mol / L to 5 mol / L, and more preferably 0.05 mol / L to 3 mol / L, from the viewpoints of productivity, viscosity of the reaction liquid, coatability, transparency, and visible light catalytic properties.
[0118] The acid used in the reaction is an organic acid, and since it is preferable that it is a volatile acid, it is preferably an acid represented by the chemical formula C n H 2n+1 Monocarboxylic acids represented by COOH (n=0 to 3) (monocarboxylic acids having 1 to 4 carbon atoms), hydroxycarboxylic acids having 2 to 3 carbon atoms, etc. are used.
[0119] The monocarboxylic acid is preferably formic acid (n=0) or acetic acid (n=1) from the viewpoints of volatility, toxicity and decomposability.
[0120] The hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc., and from the viewpoints of water solubility and odor, more preferably acetic acid, glycolic acid, lactic acid, etc.
[0121] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.
[0122] From the viewpoints of dispersibility, coatability, transparency, visible light catalytic properties and cost, the amount of organic acid used is adjusted so that the number of moles of acyloxy groups is preferably 0.5 moles or more, more preferably 1 mole or more, per mole of titanium in the Ti compound. The upper limit of the amount of organic acid used is not particularly limited, and is preferably adjusted so that the number of moles of acyloxy groups is 10 moles or less, per mole of titanium in the Ti compound.
[0123] The concentration of the organic acid in the dispersion is preferably 0.02 mol / L to 10 mol / L, and more preferably 0.1 mol / L to 7 mol / L, from the viewpoints of dispersibility, coatability, transparency, visible light catalytic properties, and cost.
[0124] The reaction solvent is preferably an aqueous solvent such as water, the main component being preferably 50% by mass or more. The reaction solvent may contain an alcohol or an ester during the reaction.
[0125] When titanium tetraisopropoxide is used as a raw material, the reaction solvent generates isopropyl alcohol by reaction with an organic acid. Heating may generate an isopropyl ester of the organic acid. The alcohol or ester may be added to the dispersion liquid, or may be generated in the system. The alcohol or ester may be removed by heating in an open system below 100°C, may be removed by reducing pressure, or may remain in the reaction liquid.
[0126] When alcohol is contained in the dispersion liquid, the average particle size of the obtained Ti compound (titania nanoparticles) tends to become small, and therefore alcohol may be intentionally added in order to control the average particle size.
[0127] The pH of the dispersion is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of corrosion of the apparatus, safety in handling, dispersibility, and the like.
[0128] The method for preparing the dispersion is not particularly limited, and the Ti compound, organic acid, and water (solvent) may be mixed simultaneously or sequentially. In mass production scale, from the viewpoint of preventing aggregation and forming large lumps and facilitating continued stirring, it is preferable to mix the organic acid and water (solvent) and then add the titanium-containing substance while stirring. In laboratory scale, it is preferable to mix the titanium-containing substance and organic acid and then add water while stirring.
[0129] [2-2] (Additionally) a step of complexing with a metal ion In the manufacturing method of the present invention, the Ti compound and the metal ion can be additionally composited. The dispersion obtained by mixing the dispersion obtained in the step (1) with a silver salt is irradiated with ultraviolet light.
[0130] By using metal ions of at least one metal selected from the group consisting of silver (silver salts), copper, and platinum, a metal (silver, silver salts, etc.) is composited with a Ti compound (titania nanoparticles), which can improve the dispersibility, transparency, antimicrobial activity (antibacterial activity, and antiviral activity) of the composition, and the stability of the Ti compound (titania nanoparticles).
[0131] The silver salt is preferably a silver salt whose aqueous solution is acidic or neutral, and the silver salt preferably used is silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc.
[0132] The silver salt may be at least one compound selected from the group consisting of the above silver salts. These silver salts may be used alone or in combination (blend) of two or more depending on the purpose.
[0133] The amount of silver salt used is preferably 50% by mass or less, more preferably 0.01% by mass to 40% by mass, and even more preferably 0.1% by mass to 25% by mass, relative to titanium oxide in the Ti compound (titania nanoparticles) contained in the dispersion, in terms of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the Ti compound (titania nanoparticles), etc., converted into the mass of silver element in the silver salt. By adjusting the amount of silver salt used within this range, it is possible to composite silver with the Ti compound (titania nanoparticles), easily maintain the coating property and transparency, and particularly improve the antibacterial activity, antiviral activity, and photocatalytic activity in the dark.
[0134] The ultraviolet light irradiation is preferably performed at a temperature lower than room temperature (20° C.), more preferably at 15° C. or lower, from the viewpoints of facilitating the composite of silver to a Ti compound (titania nanoparticles), visible light catalytic activity, reaction rate, productivity, controllability of aspect ratio, resistance to discoloration when irradiated with low-intensity ultraviolet light, visibility when irradiated with high-intensity ultraviolet light, and re-transparency in an ultraviolet light-stopped environment, etc. The lower limit of the temperature for ultraviolet light irradiation is not particularly limited, and is preferably 0° C. when the reaction is performed at normal pressure.
[0135] During the irradiation with ultraviolet light, the dispersion is preferably stirred in order to sufficiently react with the silver salt. The stirring method is not particularly limited, and may be performed according to a conventional method.
[0136] The composite of the Ti compound and the metal ion may be carried out in an air atmosphere or an anaerobic atmosphere, preferably in an inert gas atmosphere such as a nitrogen atmosphere or an argon atmosphere.
[0137] The pH of the dispersion varies depending on the type of metal added and the amount of the metal added, but is preferably 1 to 5, and more preferably 2 to 4, from the viewpoint of coatability.
[0138] Thereafter, the silver composite Ti compound (silver composite titania nanoparticles) can be recovered by precipitating and centrifuging the compound in a conventional manner, etc. The organic chains are bonded to the titanium atoms present on the surface, and titania nanoparticles with silver composited on the surface can be obtained.
[0139] [2-3] (2) A step of mixing the Ti compound having the organic chain bonded thereto obtained in the step (1) with a Si compound in a solvent to hydrolyze the Si compound. (Preparation of coating liquid) In the manufacturing method of the present invention, the titania particles are then mixed with alkoxysilane, which is a raw material for the binder, and a hydrolysis reaction is carried out in the coexistence of the two while maintaining high dispersibility, to produce a titania particle composite binder.
[0140] The hydrolysis reaction of alkoxysilane is accelerated by carrying out the reaction under acidic conditions. From the viewpoints of reaction rate and dispersion stability, the pH of the dispersion is preferably 2 or more and less than 6, and more preferably 2.1 to 5.
[0141] The hydrolysis is preferably carried out by keeping the dispersion at about 60° C. for about 12 hours with a lid on to prevent the solvent from volatilizing.
[0142] The hydrolysis is preferably carried out under normal pressure or under pressure in a closed vessel.
[0143] By reacting the organic matter (acetyl groups, acetoxy groups, etc.) bonded to the surface of the Ti compound (titania) with the Si compound (alkylsilane such as TEOS), it is possible to suppress the aggregation of Ti compounds and the aggregation of Si compounds, resulting in a more uniform and transparent coating liquid.
[0144] The coating liquid is preferably subjected to a dispersion treatment using an ultrasonic homogenizer, whereby a transparent dispersion liquid can be obtained.
[0145] The manufacturing method of the present invention uses a new process to prepare a composition containing titania particles, which can improve the aggregation of titania, which has been a problem in the past, and can greatly improve solvent stability and adhesion. EXAMPLES
[0146] The present invention will be specifically described below with reference to examples.
[0147] The present invention is not limited to the following specific examples.
[0148] [1] Preparation of coating composition [Example 1] [Method for preparing photocatalytic titanium oxide] 30g of acetic acid was added to 70g of titanium tetraisopropoxide and stirred, then water was added to make the total amount 400g, and stirred for 90 minutes. After that, it was heated to 95℃ and stirred for 9 hours with a hot stirrer, and a uniform titania sol was obtained. The obtained sol was subjected to ultrasonic dispersion for 30 minutes to obtain a transparent titania sol.
[0149] The TG-DTA of the obtained titania sol was measured by heating it up to 600°C at a temperature increase rate of 3°C / min in an air atmosphere, and the mass loss rate at 200°C or higher was 10% by mass. This mass loss rate at 200°C or higher is due to organic matter derived from acetic acid bonded to the titania surface.
[0150] In order to adjust the concentration of the obtained titania sol, it was diluted with water (solvent) to obtain a titania sol with a TiO2 concentration of 2 mass%. The particle size of the obtained titania sol was observed by TEM observation, and the average particle size was 3 nm. [Complexation with metal ions] Silver nitrate (I) was added to the titania sol with a TiO2 concentration of 2% by mass so that the weight ratio of Ag / TiO2 was 0.01, and the mixture was thoroughly stirred until it became homogeneous. After that, the mixture was irradiated with an ultraviolet lamp for 24 hours to reduce the silver nitrate, and a silver composite titania sol was obtained.
[0151] [Preparation of coating liquid] To the prepared 2 mass % silver composite titania sol (Ti compound), 9 g, 0.45 g, and 369 g of tetraethyl orthosilicate (TEOS, Si compound) and 1-propanol (solvent, alcohol) were added, respectively.
[0152] Thereafter, the container was covered to prevent the solvent from evaporating and kept at 60° C. for 12 hours.
[0153] The organic matter bonded to the titania surface reacted with tetraethyl orthosilicate, and the hydrolysis of tetraethyl orthosilicate (hydrolyzate of alkylsilane) proceeded, resulting in a transparent coating liquid. The resulting liquid was dispersed for 10 minutes using an ultrasonic homogenizer, resulting in a transparent dispersion.
[0154] [Example 2] A coating liquid was prepared in the same manner as in Example 1, except that the stirring time in [Method for preparing photocatalytic titanium oxide] was changed to 1 hour and silver acetate (I) was used instead of silver nitrate.
[0155] [Example 3] A coating liquid was prepared in the same manner as in Example 1, except that the [composite formation with metal ions] in Example 1 was not carried out.
[0156] [Example 4] A coating liquid was prepared in the same manner as in Example 3, except that trimethoxysilane (methyltrimethoxysilane) was used instead of TEOS.
[0157] [Example 5] A coating liquid was prepared in the same manner as in Example 3, except that the amount of acetic acid added was changed to 0.6 g.
[0158] [Example 6] A coating liquid was prepared in the same manner as in Example 3, except that the amount of acetic acid added was changed to 3 g.
[0159] [Example 7] A coating liquid was prepared in the same manner as in Example 3, except that the amounts of TEOS and titania sol were adjusted and added so that the mass ratio of TiO2 in the total weight was 0.01 mass% and the amount of Si binder in the total weight was 0.02 mass%.
[0160] [Example 8] A coating liquid was prepared in the same manner as in Example 3, except that the amounts of TEOS and titania sol were adjusted and added so that the mass ratio of TiO2 in the total weight was 5 mass% and the amount of Si binder in the total weight was 10 mass%.
[0161] [Example 9] In Example 3, the coating liquid was prepared by the same process as in Example 3, except that the amount of TEOS and titania sol were adjusted and added so that the mass ratio of TiO2 in the total weight was 0.2 mass% and the amount of Si binder in the total weight was 0.01 mass%.
[0162] [Example 10] In Example 3, the coating liquid was prepared by the same process as in Example 3, except that the amounts of TEOS and titania sol were adjusted and added so that the mass ratio of TiO2 in the total weight was 0.2 mass% and the amount of Si binder in the total weight was 10 mass%.
[0163] [Example 11] In Example 3, the coating liquid was prepared by the same process as in Example 3, except that the amount of TEOS and titania sol were adjusted and added so that the mass ratio of TiO2 in the total weight was 2 mass% and the amount of Si binder in the total weight was 0.1 mass%.
[0164] [Example 12] In Example 3, the coating liquid was prepared by the same process as in Example 3, except that the amount of TEOS and titania sol was adjusted and added so that the mass ratio of TiO2 in the total weight was 0.2 mass% and the amount of Si binder in the total weight was 10 mass%.
[0165] [Example 13] In Example 1, titania sol was obtained by the [method of preparing photocatalytic titanium oxide]. Then, a hydrothermal reaction was carried out in an autoclave at 160°C for 4 hours to obtain a titania sol with an adjusted particle size. The particles were confirmed to be 20 nm in size by TEM. A coating liquid was prepared using the obtained titania sol in the same manner as in Example 3.
[0166] [Example 14] In Example 1, titania sol was obtained by the [method of preparing photocatalytic titanium oxide]. Then, a hydrothermal reaction was carried out in an autoclave at 240°C for 24 hours to obtain a titania sol with an adjusted particle size. The particles were confirmed to be 50 nm by TEM. A coating liquid was prepared using the obtained titania sol in the same manner as in Example 3.
[0167] [Example 15] A coating liquid was prepared in the same manner as in Example 3, except that 1-propanol was changed to 1-butanol.
[0168] [Example 16] A coating liquid was prepared in the same manner as in Example 15, except that 30 g of acetic acid was changed to 30 g of nitric acid.
[0169] [Comparative Example 1] Water was added to Ishihara Sangyo Kaisha (ST-01) so that the mass concentration was 2.5 mass % to prepare a titania slurry.
[0170] When the sample was heated to 600°C at a rate of 3°C / min in an air atmosphere using an Ishihara Sangyo Kaisha (ST-01) TG-DTA, no mass loss was observed above 200°C, suggesting that no organic matter was attached to the surface.
[0171] Thereafter, 9 g, 9 g, and 369 g of tetraethyl orthosilicate and 1-propanol were added, respectively, in the same manner as in Example 1. The obtained coating liquid was stirred with an ultrasonic homogenizer to obtain a translucent dispersion liquid.
[0172] [Comparative Example 2] Water was added to Ishihara Sangyo Kaisha (ST-01) so that the mass concentration was 2.5 mass % to prepare a titania slurry.
[0173] When the sample was heated to 600°C at a rate of 3°C / min in an air atmosphere using an Ishihara Sangyo Kaisha (ST-01) TG-DTA, no mass loss was observed above 200°C, suggesting that no organic matter was attached to the surface.
[0174] Then, 9 g, 0.45 g, and 369 g of tetraethyl orthosilicate and 1-propanol were added, respectively. Furthermore, 0.5 mL of nitric acid was added as a catalyst for the sol-gel reaction to start the reaction. The container was loosely covered to prevent the solvent from volatilizing and kept at 60°C for 12 hours. The obtained coating liquid was stirred with an ultrasonic homogenizer to obtain a translucent dispersion liquid.
[0175] [2] Evaluation of coating composition The resulting coating compositions were each evaluated as follows.
[0176] [Transparency] The transmittance (transparency) of the coating compositions obtained in the examples and comparative examples was measured using an ultraviolet-visible spectrophotometer (Shimadzu UV3400). The highest transmittance value in the wavelength range of 400 nm to 800 nm was taken as the transmittance of the composition.
[0177] The transparency criteria are as follows: ◎: The highest transmittance is 80% or more. ◯: The highest transmittance is 50% or more. △: The highest transmittance is 20% or more. ×: The highest transmittance is less than 20%.
[0178] [Dispersion stability] The coating compositions obtained in the examples and comparative examples were allowed to stand for 480 hours at 60° C. After standing, the dispersions were visually inspected to evaluate the dispersion stability.
[0179] The criteria for judging the dispersion stability are as follows: ⊚: No precipitation or gelation was observed. ○: Separation is observed, but it can be easily dispersed by stirring by hand. △: Separation is observed, but it can be redispersed by applying external force such as ultrasound. ×: Precipitation and gelation occurred and the sample was not redispersed.
[0180] [Adhesion of dispersion liquid] The coating compositions obtained in the examples and comparative examples were used to prepare coating films by spin coating. The spin coating conditions were 2,000 rpm and 60 seconds. The films were then dried at 60°C for 60 minutes. The adhesion was checked by touching with a finger, and then evaluated according to the JIS K 5600_5_6 cross-cut test method.
[0181] The criteria for judging the adhesion are as follows. ⊚: Peeling of the coating is 5% or less. ◯: Peeling of the coating is 20% or less. △: Peeling of the coating is 50% or less. ×: More than 50% of the coating film peeled off, or the coating film peeled off when touched with a finger.
[0182] [Photocatalytic decomposition activity] The obtained dispersion was applied (spin-coated) to a glass substrate with a thickness of 1 mm, and the substrate was dried at 120°C. The transmittance of the 587.6 nm (d-line: wavelength close to the absorption peak of methylene blue) was measured using an ultraviolet-visible spectrometer (Shimadzu UV3400). This transmittance is designated as Ta.
[0183] Next, a 1 mmol / L solution of methylene blue was dropped onto the substrate, and after drying to remove excess solution, the transmittance of the light at 587.6 nm (d-line: a wavelength close to the absorption peak of methylene blue) was measured using an ultraviolet-visible spectrometer (Shimadzu UV3400). This transmittance was designated as Tb.
[0184] Thereafter, ultraviolet light with a peak wavelength of 352 nm was irradiated using a black light, and measurements were taken every hour. The time it took for Tb / Ta to reach >90% was measured, and the decomposition activity of the photocatalyst was evaluated.
[0185] The criteria for judging photocatalytic properties are as follows: ◎: The time required for Tb / Ta to reach > 90% is within 3 hours. ◯: The time required for Tb / Ta to reach >90% is 4 to 12 hours. △: The time required for Tb / Ta to reach >90% is within 13 to 24 hours. ×: The time required for Tb / Ta to be greater than 90% is 25 hours or longer.
[0186] [Antiviral test] In Examples 1 and 2, after drying, an antiviral test was carried out in a dark place in accordance with ISO 21702 using Qβ phage (non-enveloped virus).
[0187] <Method for measuring antiviral activity value> A virus liquid is dropped onto a 5cm square test piece (antiviral treated and untreated), and then covered with a 4cm square film.
[0188] The test piece is left to stand at 25°C for 7 hours.
[0189] After leaving it to stand, the virus on the test piece is washed off and collected, and the virus infectivity is measured.
[0190] The antiviral activity value is calculated according to the following formula (1).
[0191] R=Ut-At (1) R: Antiviral activity value Ut: Virus infectivity (PFU / cm) after leaving unprocessed product for 7 hours 2 ) average of the base 10 logarithm At: Virus infectivity (PFU / cm) after leaving the antiviral processed product for 24 hours 2 ) average of the base 10 logarithm
[0192] The antiviral evaluation criteria are as follows. ◎: Antiviral activity value is 2 or higher. ×: Antiviral activity value is less than 2.
[0193] Below are tables of examples and comparative examples.
[0194] [Table 1]
[0195] [Table 2]
[0196] [Table 3]
[0197] The compositions of Examples 1 to 16 were excellent in transparency, adhesion, and solvent stability. It was clear that the compositions of Examples 1 and 2 exhibited even more excellent antibacterial and antiviral properties.
[0198] The composition of Comparative Example 1 was a composite of commercially available titanium oxide and TEOS, and a white precipitate thought to be an agglomeration of titanium oxide was observed, and a transparent composition could not be obtained. The composition of Comparative Example 1 did not react because it did not contain an acid component of the reaction initiator, and after application to the substrate, it had no adhesion and easily peeled off by hand.
[0199] The composition of Comparative Example 2 was prepared by compounding commercially available titanium oxide with TEOS and adding nitric acid as a reaction initiator. The composition obtained in Comparative Example 2 had a white precipitate, which was believed to be an agglomeration of titanium oxide, and a transparent composition could not be obtained. The composition in Comparative Example 2 was easily peeled off when rubbed with a hand after being applied to a substrate, and therefore it was clear that the composition had poor adhesion.
[0200] [3] Industrial Applicability In the present invention, a good composition with excellent transparency, adhesion, and solvent stability was obtained by using titanium oxide having an organic chain on the surface and reacting it with a silicon binder in a sol-gel manner. By using this coating agent, it becomes possible to fix the photocatalytic titanium oxide to various substrates, and it becomes possible to form various articles having a coating layer.
Claims
1. A composition containing a Ti compound, a Si compound, and a solvent, The Si compound is a hydrolyzate of an alkylsilane, The Ti compound has a mass loss of 0.1% by mass or more at 200°C or higher when the Ti compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomeasuring device; The average primary particle size of the Ti compound is 1 nm to 50 nm, The composition, wherein the solvent comprises water and alcohol.
2. 2. The composition according to claim 1, wherein the Ti compound exhibits a mass loss of 1% or more at 200° C. or higher when the Ti compound is heated to 600° C. using a simultaneous differential thermogravimetry and thermomechanical analysis apparatus.
3. 2. The composition according to claim 1, wherein the Ti compound exhibits a mass loss of 5% by mass or more at 200° C. or higher when the Ti compound is heated to 600° C. using a simultaneous differential thermogravimetry and thermomechanical analysis apparatus.
4. 2. The composition according to claim 1, wherein the average primary particle size of the Ti compound is 1 nm to 20 nm.
5. 2. The composition according to claim 1, wherein the average primary particle size of the Ti compound is 1 nm to 10 nm.
6. The composition according to claim 1 , wherein the Ti compound has an organic chain bonded to a surface thereof.
7. 2. The composition according to claim 1, wherein the Ti compound has at least one organic chain selected from the group consisting of an acetyl group and an acetoxy group bonded to a surface thereof.
8. The composition according to claim 1, wherein the content of the Ti compound in the composition is 0.01% by mass to 5% by mass.
9. The composition according to claim 1, wherein the content of the Si compound in the composition is 0.01% by mass to 20% by mass.
10. 2. The composition according to claim 1, wherein the Ti compound and the Si compound are contained in a mass ratio of 0.02 to 20 in the composition relative to the Si compound.
11. 2. The composition according to claim 1, wherein the Ti compound and the Si compound are contained in a mass ratio of 0.1 to 1 relative to the Si compound in the composition.
12. 2. The composition of claim 1, wherein the Si compound is a hydrolysis product of TEOS.
13. 10. The composition of claim 1, further comprising at least one metal selected from the group consisting of silver, copper, and platinum.
14. An antibacterial and antiviral coating film comprising the composition according to any one of claims 1 to 13.
15. A method for producing a composition containing a Ti compound, a Si compound, and a solvent, comprising the steps of: (1) bonding an organic chain to the surface of a Ti compound in a solvent; and (2) mixing the Ti compound having the organic chain bonded thereto obtained in step (1) with a Si compound in a solvent to hydrolyze the Si compound; A manufacturing method comprising:
Citation Information
Patent Citations
Coating liquid
JP2021155664A
Metal-carrying titania nanoparticle, and production method thereof
JP2022155211A
Method for producing platinum nanoparticle
JP2022156809A
Stainproof plate
JP1997075243A
Fine particle titanium dioxide and its manufacturing method
JP6607407B2
Cited By
Porous coating materials
JP2026166140A