Method for manufacturing projection material and method for treating surface
By attaching target particles to core particles via electrostatic force and colliding them with the base material, the method addresses the limitations of existing shot materials, enabling effective function imparting and attachment to the base material surface.
Patent Information
- Application Number
- JP2023050254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing shot materials have limitations in selecting materials based on desired functions and may not properly embed or attach target particles to the surface layer of base materials, restricting the ability to impart specific functions.
A method involving the preparation of core and target particles, where target particles are attached to core particles by electrostatic force to form a shot material, followed by a surface treatment process that collides the shot material with the base material to embed or attach target particles effectively.
The method allows for appropriate imparting of functions related to target particles to the surface layer of the base material, enhancing properties such as heat dissipation and antibacterial properties, while minimizing peeling and ensuring proper attachment.
Smart Images

Figure 2024139360000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a projection material and a method for treating the surface of the projection material. [Background technology]
[0002] Patent Document 1 discloses a shot material for mechanical plating. This shot material is produced by adding steel particles as cores to a molten zinc alloy having a composition corresponding to the adherend material, stirring the molten metal, and removing the molten metal when it becomes semi-solid as the temperature of the molten metal drops, and then crushing and sieving the molten metal. This production method produces a shot material in which the outer periphery of the steel particles is coated with a zinc alloy and an Fe-Zn alloy layer is formed near the interface between the two. The shot material is collided with the surface of a workpiece made of a metal material to form a corrosion-resistant coating of zinc alloy on the surface of the workpiece. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-082322 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the projection material described in Patent Document 1, since there is a restriction on the content of each particle constituting the projection material, it may not be possible to select a material for the projection material according to the function to be imparted to the treated object (base material). In addition, depending on the material of each particle, even if the projection material is formed, the projection material may not be properly embedded or attached to the surface layer of the base material. Therefore, there is a demand for a manufacturing method and a surface treatment method for a projection material that can properly impart the function related to the target particle contained in the projection material to the surface layer of the base material. [Means for solving the problem]
[0005] A method for producing a projection material according to the present disclosure includes the steps of preparing core particles and target particles, and attaching the target particles to the core particles by electrostatic forces to form the projection material.
[0006] A surface treatment method according to another aspect of the present disclosure further includes a step of colliding the projection material produced by the above-mentioned projection material production method against a surface of a base material. Effect of the Invention
[0007] According to the present disclosure, functions related to the target particles contained in the projection material can be appropriately imparted to the surface layer of the base material. [Brief description of the drawings]
[0008] [Figure 1] 1 is a flowchart of a surface treatment method including a manufacturing method of a projection material according to an embodiment. [Diagram 2] FIG. 2 is a partial cross-sectional view showing an example of the front side of a production device for projection materials. [Diagram 3] FIG. 2 is a partial cross-sectional view showing an example of the side of a production device for projection materials. [Figure 4] FIG. 1 is a schematic diagram showing an example of a blast processing device that blasts projection materials. [Diagram 5] 1 is a flowchart of a forming process included in a manufacturing method and a surface treatment method for a projection material according to an embodiment. [Figure 6] FIG. 2 is a schematic diagram of a secondary electron image of a cross section of a base material subjected to a surface treatment method according to an embodiment. [Figure 7] 1 shows the results of elemental analysis at each measurement point on the surface layer of a base material subjected to a surface treatment method according to an embodiment. [Figure 8] 4 is a graph showing temperature characteristics of a base material subjected to a surface treatment method according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Overview of the embodiment of the present disclosure] First, an overview of the embodiment of the present disclosure will be described.
[0010] (Clause 1) A method for producing a projection material according to one aspect of the present disclosure includes a preparing step and a forming step. In the preparing step, core particles and target particles are prepared. In the forming step, the target particles are attached to the core particles by electrostatic force to form the projection material.
[0011] According to this method for producing a projection material, the target particles are attached to the core particles by electrostatic forces to form the projection material, and therefore the target particles are more likely to separate from the core particles than in projection materials in which the core particles are coated with a molten metal of the target particles or the like. Therefore, when the projection material collides with the surface of the base material to be treated, the target particles are separated from the core particles by the impact of the projection material colliding with the base material, and the target particles are appropriately embedded in or attached to the surface layer of the base material. By embedding or attaching the target particles in the surface layer of the base material, a layer having a function related to the target particles is appropriately formed in the surface layer of the base material. Therefore, this method for producing a projection material can produce a projection material that can appropriately impart a function related to the target particles contained in the projection material to the surface layer of the base material.
[0012] (Clause 2) In the method for producing a projection material described in Clause 1, the forming step may include a storing step and a stirring step. In the storing step, the core particles and the target particles are stored in a rotating container. In the stirring step, the rotating container is rotated to stir the core particles and the target particles. In this case, friction occurs when the core particles and the target particles are stirred in the stirring step. Static electricity generated by the friction allows the target particles to easily adhere to the core particles.
[0013] (Clause 3) In the method for producing a projection material according to clause 1 or 2, the core particles and the target particles may have different charging characteristics. In this case, the target particles are more likely to adhere to the core particles in the formation step.
[0014] (Clause 4) A surface treatment method according to another aspect of the present disclosure further includes a step of colliding a projection material manufactured by the projection material manufacturing method according to any one of clauses 1 to 3 against a surface of a base material.
[0015] According to this surface treatment method, in the collision step, the projection material collides with the surface of the base material, so that the target particles are separated from the core particles by the impact and are appropriately embedded in the surface layer of the base material. Therefore, this surface treatment method can appropriately impart functions related to the target particles contained in the projection material to the surface layer of the base material.
[0016] (Clause 5) In the surface treatment method according to Clause 4, the impacting step may include a step of injecting a projection material into the base material. In this case, the projection material is accelerated by the injecting step and can impact the base material, and the target particles are properly separated from the core particles. As a result, the target particles are properly embedded in or attached to the surface layer of the base material.
[0017] (Clause 6) In the spraying step of the surface treatment method described in Clause 5, the projection material may be sprayed onto the base material at a pressure of 0.01 MPa or more and 0.3 MPa or less. In the spraying step, the projection material is sprayed at a pressure of 0.01 MPa or more, so that the projection material is appropriately pressed onto the base material, adhesion between the core particles in the projection material and the target particles is suppressed, and the target particles are appropriately pressed onto the base material, and are embedded in or adhered to the surface layer of the base material. In addition, in the spraying step, a pressure of 0.3 MPa or less prevents the surface layer of the base material or the target particles adhered to the surface layer of the base material from being scraped off by the projection material. Therefore, this surface treatment method can more appropriately impart functions related to the target particles contained in the projection material to the surface layer of the base material.
[0018] (Clause 7) In the spraying step of the surface treatment method according to clause 5 or 6, the shot material is sprayed onto the base material by an air blasting device, and the average particle diameter of the core particles may be 5 μm or more, and the average particle diameter of the target particles may be smaller than the average particle diameter of the core particles. In this case, the shot material has a particle diameter that can be sprayed by the air blasting device. Since the average particle diameter of the target particles is smaller than the average particle diameter of the core particles, many target particles can adhere to the periphery of the core particles. Therefore, when the shot material is sprayed, this surface treatment method can adhere many more target particles to the base material, and can more appropriately impart the function related to the target particles to the surface layer of the base material.
[0019] [Examples of the embodiments of the present disclosure] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. In the following description, the same or equivalent elements are given the same reference numerals, and redundant description will not be repeated. The dimensional ratio of the drawings does not necessarily match that of the description. In the drawings, the X and Y directions are horizontal directions, and the Z direction is vertical.
[0020] Fig. 1 is a flowchart of a surface treatment method including a manufacturing method of a projection material according to an embodiment. The surface treatment method SM shown in Fig. 1 is a method for imparting a function related to target particles contained in the projection material to a surface layer of a base material. The surface treatment method SM includes a manufacturing method MM of the projection material. The surface treatment method SM of this embodiment imparts an additional function to the surface layer of the base material, for example. The surface treatment method SM is applied for the purpose of improving the heat dissipation property or antibacterial property of the base material, for example.
[0021] The base material is a target component that is struck by the projection material. The base material is, for example, a plate material. The material of the base material is, for example, a metal, a hard and brittle material, a resin, or a combination thereof.
[0022] The projection material is formed by attaching target particles to core particles. The projection material can be projected toward a base material. The average particle diameter of the projection material is 5 μm or more. The average particle diameter of the projection material may be 15 μm or more. When the average particle diameter of the projection material is 15 μm or more, it becomes easy to spray the projection material in the blast processing device 20 described below. Hereinafter, unless otherwise specified, the particle diameter of the projection material in this embodiment will be expressed as the average particle diameter (D50).
[0023] FIG. 2 is a partial cross-sectional view showing an example of the front side of a production apparatus for a projection material. FIG. 3 is a partial cross-sectional view showing an example of the side side of a production apparatus for a projection material. The core particles CP shown in FIG. 2 and FIG. 3 are particles to which the target particles TP can be attached at the center of the projection material. The material of the core particles CP is, for example, a metal, a hard and brittle material, a resin, or a combination thereof. The core particles CP are, for example, made of at least one hard material. The core particles CP are made of a material having a hardness that can be measured by a Rockwell hardness test, a Vickers hardness test, a Knoop hardness test, or a Brinell hardness test. The core particles CP are, for example, harder than the base material. The Vickers hardness value of the core particles CP is, for example, Hv50 or more. The particle diameter of the core particles CP is 5 μm or more.
[0024] The target particles TP are particles that adhere to the core particles CP by electrostatic force. The material of the target particles TP is, for example, a metal, a hard and brittle material, a resin, an oxide, a fluoride, a carbide, a nitride, or a combination thereof. The particle diameter of the target particles TP is smaller than the average particle diameter of the core particles CP. The particle diameter of the target particles TP is, for example, 1 μm or less. When a process for crushing the target particles TP is performed, the target particles TP may have a particle diameter of more than 1 μm.
[0025] The core particle CP and the target particle TP have different charging characteristics. The core particle CP and the target particle TP are formed of materials having different charge amounts, for example. The core particle CP and the target particle TP may be charged with different charges or may be charged with the same charge. The material of the core particle CP is, for example, glass beads. The material of the target particle TP is, for example, Fe3O4.
[0026] The manufacturing apparatus used in the manufacturing method MM for producing the projection material will be described below. The manufacturing apparatus disclosed is an example of an apparatus for realizing the manufacturing method MM, and the manufacturing method MM does not assume the use of the manufacturing apparatus disclosed herein. The manufacturing apparatus 10 shown in FIG. 2 and FIG. 3 accommodates the core particles CP and the target particles TP in a rotary container 2, and agitates the core particles CP and the target particles TP to form the projection material. The manufacturing apparatus 10 of this embodiment is a ball mill. The manufacturing apparatus 10 may be, for example, a barrel device, an agitator, a powder mixing device, or the like. The manufacturing apparatus 10 does not aim to crush the core particles CP and the target particles TP, but aims to agitate the core particles CP and the target particles TP to collide with each other and adhere the target particles TP to the core particles CP.
[0027] The manufacturing apparatus 10 has a rotating vessel 2. The rotating vessel 2 has a processing chamber therein for storing the core particles CP and the target particles TP. The processing chamber is a sealable space in which the storing process and the stirring process described below are carried out. The processing chamber is opened when storing the core particles CP and the target particles TP and when removing the projection material. The rotating vessel 2 is, for example, a cylindrical vessel. The material of the rotating vessel 2 is a material that does not affect, or has little effect on, the friction and electrostatic force between the core particles CP and the target particles TP.
[0028] The rotating vessel 2 is rotatably supported via stands 3a and 3b. Ball mill shafts 4a and 4b are connected to the center of each of the two end faces of the rotating vessel 2. The ball mill shafts 4a and 4b are each provided along a rotation axis M extending in the X direction in the drawing. The ball mill shafts 4a and 4b are rotatably supported by bearings 5a and 5b supported by the stands 3a and 3b, respectively.
[0029] The manufacturing apparatus 10 includes a driving unit 6 that rotates the rotary container 2. The driving unit 6 rotates the rotary container 2 to adhere the core particles CP and the target particles TP by electrostatic force to form the projection material. The driving unit 6 includes a motor 7, pulleys 8a and 8b, and a driving belt 9. The motor 7 is a driving source and has a motor shaft 7a that is a rotation driving shaft. The pulley 8a is provided on the motor shaft 7a, and the pulley 8b is provided on the ball mill shaft 4a. The driving belt 9 is hung on the outer periphery of the pulleys 8a and 8b. The rotational force of the motor shaft 7a is transmitted to the ball mill shaft 4a via the driving belt 9. This causes the rotary container 2 connected to the ball mill shaft 4a to rotate. In the processing chamber inside the rotary container 2, frictional force between the core particles CP and the target particles TP is generated by the rotation of the rotary container 2. This generates static electricity between the core particles CP and the target particles TP, and the target particles TP adhere to the core particles CP by the electrostatic force.
[0030] The blast processing device used in the surface treatment method SM will be described below. The blast processing device disclosed is an example of a device for realizing the surface treatment method SM, and the surface treatment method SM does not assume the use of the blast processing device disclosed herein. The blast processing device 20 shown in FIG. 4 causes a projection material formed of core particles CP and target particles TP to collide with the surface of a base material. The blast processing device 20 shown in FIG. 4 is, for example, a suction type (gravity type) blast processing device 20. The blast processing device 20 is an air blast processing device. The blast processing device 20 may be, for example, a direct pressure type or a blower type blast processing device.
[0031] The blast processing device 20 includes a storage container 30 and a nozzle 40. The storage container 30 defines a space for storing the blast material therein, and stores the blast material. The storage container 30 is supplied with the blast material from the outside. For example, an operator may supply the blast material to the storage container 30. The storage container 30 may reuse a portion of the blast material used in the blast processing. In this case, the storage container 30 is supplied with the blast material used in the blast processing from a classification mechanism 23, which will be described later. The storage container 30 is connected to the nozzle 40 via a fixed-volume supply unit 31 and a pipe 22. The fixed-volume supply unit 31 is a device that sends out the blast material stored in the storage container 30 to the pipe 22, and is, for example, a screw feeder.
[0032] A gas supply source 21 that supplies gas is connected to the piping 22. The gas supply source 21 transports the projection material to the nozzle 40 at a pressure of 0.01 MPa or more and 0.3 MPa or less. The gas supply source 21 can be, for example, a compressor or gas cylinder that supplies gas at a medium pressure (e.g., 0.1 MPa or more and 0.3 MPa or less), or a blower such as a fan or blower that supplies gas at a low pressure (e.g., 0.01 MPa or more and less than 0.1 MPa). In this embodiment, compressed air is supplied by a compressor. The gas supplied from the gas supply source 21 to the piping 22 transports the projection material sent out by the constant-volume supply unit 31 to the nozzle 40.
[0033] The nozzle 40 sprays the projection material supplied from the storage container 30 together with the gas supplied from the gas supply source 21. The nozzle 40 is housed in a processing chamber 41, and a gas-solid two-phase flow in which the projection material and the gas supplied from the storage container 30 are mixed is supplied to the nozzle 40 via piping 22. The nozzle 40 sprays the projection material together with the gas toward the base material arranged in the processing chamber 41. This causes the base material to collide with the target particles contained in the projection material. The base material is supported on a table (not shown), and the position may be adjusted by a table driving mechanism.
[0034] The lower part of the treatment chamber 41 is connected to the storage container 30 via the classification mechanism 23. The blasting material that falls to the lower part of the treatment chamber 41 is sucked into a dust collector (not shown) and passes through the classification mechanism 23. The classification mechanism 23 classifies the blasting material into reusable blasting material and other fine powders (such as blasting material in which core particles CP and target particles TP have been separated). The other fine powders are collected in the dust collector. The lower part of the classification mechanism 23 is connected to the upper part of the storage container 30. The reusable blasting material is supplied from the classification mechanism 23 to the storage container 30. If the blasting material is not reused, the blasting processing device 20 does not need to be equipped with the classification mechanism 23.
[0035] As shown in Fig. 2, Fig. 3 and Fig. 4, the manufacturing apparatus 10 and the blast processing apparatus 20 are controlled by a control device 50. The control device 50 is configured as, for example, a PLC (Programmable Logic Controller). The control device 50 may be configured as a computer system including a processor such as a CPU (Central Processing Unit), a memory such as a RAM (Random Access Memory) and a ROM (Read Only Memory), an input / output device such as a touch panel, a mouse, a keyboard and a display, and a communication device such as a network card. The control device 50 realizes the functions of the control device 50 by operating each piece of hardware under the control of the processor based on a computer program stored in the memory.
[0036] For example, the control device 50 controls the rotation speed and rotation time of the rotary container 2 for the manufacturing device 10. For example, the control device 50 controls the gas pressure of the gas supply source 21 for the blast processing device 20. The control device 50 controls the amount of blast material sent out by the constant-quantity supply unit 31. The control device 50 may adjust the distance between the nozzle 40 and the base material, or may adjust the scanning conditions of the base material (speed, feed pitch, number of scans, etc.). In addition, the control device 50 controls the injection position of the nozzle 40 with respect to the base material by moving the table supporting the base material based on the set distance between the workpiece and the nozzle and the scanning conditions of the workpiece (speed, feed pitch, number of scans, etc.). The control device 50 may control at least one of the injection amount of the blast material, the pressure at which the blast material is sprayed, the distance between the nozzle 40 and the blast material, and the scanning conditions of the base material (speed, feed pitch, number of scans, etc.).
[0037] Referring again to Fig. 1, the surface treatment method SM includes a preparation step (step S10), a formation step (step S20), and a collision step (step S30). The surface treatment method SM includes a manufacturing method MM for a projection material. The manufacturing method MM for a projection material includes a preparation step (step S10) and a formation step (step S20). In the preparation step (step S10), core particles CP and target particles TP are prepared.
[0038] Next, in the forming step (step S20), the target particles TP are attached to the core particles CP by electrostatic force to form a projection material that can be projected toward a base material. FIG. 5 is a flowchart of the forming step included in the projection material manufacturing method and surface treatment method according to the embodiment. As shown in FIG. 5, the forming step (step S20) includes a containing step (step S21) and a stirring step (step S23). First, in the containing step (step S21), the core particles CP and the target particles TP are contained in the rotating container 2 of the manufacturing apparatus 10.
[0039] Next, in the stirring step (step S23), the rotating vessel 2 is rotated to stir the core particles CP and the target particles TP. The manufacturing apparatus 10 rotates the rotating vessel 2, for example, by driving the drive unit 6. The manufacturing apparatus 10 rotates the rotating vessel 2, for example, around the ball mill shafts 4a and 4b. The rotation speed of the rotating vessel 2 is appropriately set based on the critical rotation number, and is set to 2 rpm or more and 200 rpm in one example. The manufacturing apparatus 10 stirs the core particles CP and the target particles TP at the above-mentioned speed for, for example, 5 minutes. When the stirring step (step S23) is completed, the flow chart of the forming step (step S20) shown in FIG. 5 is completed.
[0040] Referring again to FIG. 1, next, in the impacting step (step S30), the projection material is impacted against the surface of the base material. The impacting step (step S30) of this embodiment includes a step of injecting the projection material into the base material. In the injecting step, the projection material is injected into the base material by the blasting device 20, which is an air blasting device. In the injecting step, the blasting device 20 injects the projection material into the base material at a pressure of 0.01 MPa or more and 0.3 MPa or less. When the predetermined injection into the base material is completed, the impacting step (step S30) ends. When the impacting step (step S30) ends, the flowchart of the surface treatment method SM shown in FIG. 1 ends.
[0041] As described above, according to the manufacturing method MM and the surface treatment method SM of the projection material, in the forming step (step S20), the target particles TP are attached to the core particles CP by electrostatic force to form the projection material, so that the target particles TP are more likely to separate from the core particles CP than in a projection material in which the core particles CP are covered with a molten metal of the target particles TP or the like. Therefore, when the projection material collides with the surface of the base material in the collision step (step S30), the target particles TP are separated from the core particles CP by the impact when the projection material collides with the base material, and the target particles TP are appropriately embedded in the surface layer of the base material or are appropriately attached. Embedding includes that a part or all of the target particles TP are fixed from the surface of the base material to the inside of the surface layer. Attaching includes that a part or all of the target particles TP are fixed on the surface of the base material. Attaching includes that a part or all of the target particles TP are stacked on the surface of the base material. Attaching includes that the target particles TP are fixed on the surface of the base material and on the target particles TP stacked on the surface of the base material. For example, when the projection material collides with the surface layer of the base material with a force equal to or greater than a predetermined first threshold, the target particles TP are embedded in and adhere to the surface layer of the base material. For example, when the projection material collides with the surface layer of the base material with a force less than a predetermined first threshold, the target particles TP are not embedded in the surface layer of the base material, but adhere to the surface of the base material. By embedding or adhering the target particles TP in the surface layer of the base material, a layer having a function related to the target particles TP is appropriately formed in the surface layer of the base material. Therefore, the projection material manufacturing method MM and the surface treatment method SM can manufacture a projection material that can appropriately impart a function related to the target particles contained in the projection material to the surface layer of the base material. The function related to the target particles TP includes a function that is expressed by the action of the target particles TP.
[0042] Conventionally, when particles are embedded in the surface layer of a base material, for example, it is necessary to form a projection material by coating particles serving as core particles with molten metal or the like, so that the temperature characteristics of the material may not be suitable for forming the projection material. In the projection material of this embodiment, the target particles TP are attached to the core particles CP by electrostatic force, so that the influence of the temperature characteristics of the core particles CP and the target particles TP on the formation of the projection material is small. The materials of the core particles CP and the target particles TP contained in the projection material formed by the projection material manufacturing method MM and surface treatment method SM of this embodiment are not limited to the above examples. Therefore, a wide variety of materials can be selected according to the function to be imparted to the base material, and there is a large degree of freedom.
[0043] Furthermore, the forming step (step S20) in the manufacturing method MM and the surface treatment method SM of this projection material includes a storing step (step S21) and a stirring step (step S23). In this case, friction occurs when the core particles CP and the target particles TP are stirred in the stirring step (step S23). Static electricity generated by this friction allows the target particles TP to easily adhere to the core particles CP.
[0044] In addition, in the projection material manufacturing method MM and the surface treatment method SM, the core particles CP and the target particles TP have different charging characteristics. In this case, in the forming step (step S20), the target particles TP are easily attached to the core particles CP. Furthermore, by appropriately setting a threshold value of the difference in charge amount between the core particles CP and the target particles TP, the adhesion force between the core particles CP and the target particles TP can be appropriately controlled. For example, the threshold value may be set according to the impact force (pressure) when the projection material collides with the surface of the base material. In this case, while suppressing the separation of the core particles CP and the target particles TP before the projection material collides with the base material, when the projection material collides with the base material, the core particles CP and the target particles TP are appropriately separated and easily attached to the base material.
[0045] Moreover, the surface treatment method SM includes the projection material manufacturing method MM, and further includes a step (step S30) of colliding the projection material with the surface of the base material. According to this surface treatment method SM, in the collision step (step S30), the projection material collides with the surface of the base material, and the target particles TP are separated from the core particles CP by the impact and are appropriately embedded in the surface layer of the base material. Therefore, this surface treatment method SM can appropriately impart functions related to the target particles TP contained in the projection material to the surface layer of the base material.
[0046] In the surface treatment method SM, the impact step (step S30) includes a step of injecting a projection material into the base material. In this case, the projection material is accelerated by the injecting step and can impact the base material, and the target particles TP are properly separated from the core particles CP. Therefore, the target particles TP are properly embedded in the surface layer of the base material.
[0047] In the spraying step of the surface treatment method SM, the projection material is sprayed onto the base material at a pressure of 0.01 MPa or more and 0.3 MPa or less. In the spraying step, the projection material is sprayed at a pressure of 0.01 MPa or more, so that the projection material is appropriately pressed onto the base material, the adhesion between the core particles CP in the projection material and the target particles TP is eliminated, and the target particles TP are appropriately pressed onto the surface of the base material and embedded into the surface layer of the base material. In addition, by setting the pressure to 0.3 MPa or less in the spraying step, the surface layer of the base material or the target particles TP adhered to the surface layer of the base material are prevented from being scraped off by the projection material. Therefore, the surface treatment method SM can more appropriately impart the functions related to the target particles TP contained in the projection material to the surface layer of the base material.
[0048] Furthermore, in the spraying step of the surface treatment method SM, the blasting material is sprayed onto the base material by the blasting device 20, and the average particle diameter of the core particles is 5 μm or more, and the average particle diameter of the target particles is smaller than the average particle diameter of the core particles. In this case, the blasting material has a particle diameter that can be sprayed by the blasting device 20. Since the particle diameter of the target particles TP is smaller than the particle diameter of the core particles CP, many target particles can adhere to the periphery of the core particles. Therefore, when the blasting material is sprayed, the surface treatment method SM can adhere many more target particles TP to the base material, and the functions related to the target particles TP can be more appropriately imparted to the surface layer of the base material.
[0049] Moreover, the core particles CP are made of at least one hard material. For example, the core particles CP are harder than the base material. Therefore, when the projection material collides with the base material, the projection material is prevented from being elastically deformed by the impact of the collision, and the force of the impact can be efficiently converted into a force that presses the target particles TP against the base material, so that the target particles TP are appropriately embedded in the surface layer of the base material.
[0050] The surface treatment method SM embeds the target particles TP in the surface layer of the base material and causes them to adhere to the surface layer. When generating a gradient material based on a base material, peeling may occur due to differences in thermal expansion coefficients and the like in conventional film formation techniques. However, after performing the surface treatment method SM, the target particles TP are embedded in the base material and a film of the target particles TP is formed on the adhered base material, suppressing peeling of the target particles TP. Thus, the surface treatment method SM forms a strong film of the target particles TP on the base material, making it possible to manufacture a component that is expected to function as if the interface between the base material and the film formed a gradient structure.
[0051] Although the present embodiment has been described above, the present invention is not limited to the above embodiment, and can of course be implemented in various modifications within the scope of the present embodiment. For example, in the forming process (step S20), the stirring process (step S23) does not need to be performed. In this case, in the forming process (step S20), as the storing process (step S21), the particles are stored in a device such as an ion irradiation type charging device. Then, in the forming process (step S20), instead of the stirring process (step S23), as the charging process, the charging device applies static electricity to the stored core particles CP and target particles TP.
[0052] The impacting step (step S30) does not necessarily require the projection material to be impacted against the surface of the base material by the ejecting step. In this case, the impacting step (step S30) may involve, for example, allowing the projection material to fall freely toward the surface of the base material, or storing the projection material and base material in a barrel device and stirring them. In the ejecting step, the projection material may be ejected against the base material at a pressure of 0.005 MPa or more and 0.3 MPa or less.
[0053] The surface treatment method SM according to the modified example may be realized by an apparatus capable of performing the aerosol deposition method (AD method) instead of the blast processing apparatus 20 according to the above-described embodiment. In this case, the apparatus places a base material and injects a blasting material toward the base material. Compared with the normal aerosol deposition method in which a film-forming material is injected toward a substrate in a vacuum chamber, the surface treatment method SM according to the modified example has a strong effect of causing the target particles TP to collide with the base material by the core particles CP contained in the blasting material (hammer effect), so that the target particles TP are easily embedded in the surface layer of the base material or are easily attached to it. The embedding efficiency or attachment efficiency of the target particles TP to the base material is improved. In addition, in the above-described normal aerosol deposition method, if the predetermined processing conditions such as vacuum or low vacuum are not satisfied, a film cannot be formed on the substrate. However, in the surface treatment method SM, even if the processing conditions required for the normal aerosol deposition method such as vacuum or low vacuum are not set, the target particles TP can be properly embedded in the surface layer of the base material or be properly attached to it. EXAMPLES
[0054] [Confirm embedding of target particles] In order to evaluate the state in which the target particles TP are embedded in the surface layer of the base material, the surface treatment method SM was performed on the base material.
[0055] [Example 1] A process of preparing core particles and target particles was carried out. Glass beads F180 were used as the core particles. The particle diameter of the core particles was 53 μm to 90 μm. Fe3O4 was used as the target particles. The particle diameter of the target particles was about 10 μm. In the storing process (step S21) of the forming process (step S20), the core particles and the target particles were stored in a manufacturing device. The manufacturing device was a tabletop ball mill. In the stirring process (step S23), the rotation speed of the manufacturing device was set to 20 rpm and the operating time was set to 5 minutes to stir the core particles and the target particles. After the operation of the manufacturing device was completed, the blast material was removed from the manufacturing device. As a result, the mixture ratio of the target particles to the core particles became 0.75% on a weight basis. Next, the blast material was stored in a storage container of a blast processing device. The blast processing device was an air blasting device. The base material was A1070 (aluminum). The control device controlled the blast processing device at a spray pressure of 0.05 MPa, a spray angle of the projected material to the base material of 90 degrees, a distance between the base material and the nozzle of 3 mm, and a scanning speed of 1 mm / sec.
[0056] A secondary electron image of Example 1 created under the above conditions was captured. FIG. 6 is a schematic diagram of a secondary electron image in a cross section of a base material on which the surface treatment method according to the embodiment has been performed. The cross section of the base material is a surface seen from the side when the base material is cut in the depth direction of the surface layer. FIG. 6 shows the surface and the vicinity of the surface layer of the base material. As shown in FIG. 6, white target particles TP1 are embedded in the surface layer of the light gray base material BM. In this way, it was confirmed that the target particles TP1 are appropriately embedded in the surface layer of the base material BM by performing the above-mentioned surface treatment method. It was also confirmed that the target particles TP1 are appropriately attached to the surface layer of the base material BM by performing the above-mentioned surface treatment method. Furthermore, it was confirmed that the target particles TP1 are further attached to the target particles TP1 embedded (attached) in the surface layer of the base material BM by performing the above-mentioned surface treatment method. Although slight unevenness is confirmed on the surface layer of the base material due to the projection of the projection material, the surface is somewhat flat overall. From this, it was confirmed that by spraying at an appropriate pressure, scraping of the surface layer of the base material BM and the layer of embedded target particles TP1 is suppressed. The dark gray area at the top of the schematic diagram is the resin that was bonded when the secondary electron image was taken. In addition, when the spray pressure by the control device was changed to 0.1 MPa and the secondary electron image of the base material was taken under the same conditions as above, it was confirmed that more target particles were embedded in the surface layer of the base material than in the surface layer of the base material BM described above, and the density of the target particles in the surface layer of the base material was higher.
[0057] [Elemental analysis results] Elemental analysis was performed at measurement points 71 to 76 on the surface layer of the base material BM shown in Fig. 6. Energy dispersive X-ray spectroscopy was used as the elemental analysis method. Fig. 7 shows the elemental analysis results at each measurement point on the surface layer of the base material subjected to the surface treatment method according to the embodiment. As shown in Figs. 6 and 7, at measurement points 71 and 72 in the area of the base material BM where the white target particle TP1 is not embedded, the proportion of aluminum in the base material is much higher than the proportions of iron and oxygen constituting the Fe3O4 of the target particle TP1.
[0058] At measurement points 73 to 75 in the boundary region between the layer formed by embedding the white target particle TP1 and the region of the matrix BM, the proportion of aluminum in the matrix is higher than the proportion of iron and oxygen constituting the Fe3O4 of the target particle TP1, but the proportions of iron and oxygen are higher than those at measurement points 71 and 72, which are far from the surface and the boundary region. This confirmed that at least a portion of the target particle TP1 was embedded in the boundary region.
[0059] Furthermore, at measurement point 76, which is in an area close to the surface of the surface layer of the matrix BM in which the white target particles TP1 are embedded, the ratio of iron and oxygen constituting the Fe3O4 of the target particles TP1 is higher than the ratio of aluminum of the matrix BM. Also, when the results of measurement point 76 are compared with those of measurement points 71 to 75, the ratios of iron and oxygen constituting the Fe3O4 of the target particles TP1 are higher. From this, it was confirmed from the elemental analysis results that the target particles TP1 are appropriately embedded in the surface layer of the matrix BM by performing the above-mentioned surface treatment method.
[0060] [Confirmation of functionalization of target particles] In order to evaluate whether or not the base material is endowed with functions related to the target particles TP by embedding the target particles TP in the surface layer of the base material, the surface treatment method SM was performed on the base material.
[0061] [Example 2] The projection material was formed under the same conditions as in Example 1, and the projection material was sprayed against the base material. In addition, a number of comparative examples were prepared that were the same size and made of the same material as the base material in Example 2. In other words, the comparative examples were Example 2 before the above-mentioned surface treatment method was performed. Heat dissipation was evaluated for Example 2 and the comparative examples. Samples (each of the examples and the comparative examples) placed on a fixed table were heated with a ceramic heater, and the heat dissipation was evaluated by recording the temperature changes of the sample surface and room temperature. The heating temperature of the sample was 150°C, and the heating time was 300 minutes. After heating, the temperature of each sample was measured with a radiation thermometer (As One IT-314). The heat source was a ceramic heater, and power was supplied from a DC power source. Each of the examples and the comparative examples was heated while covered with a heat insulating material, and the temperature was measured. The heat insulating material was glass wool.
[0062] FIG. 8 is a graph showing the temperature characteristics of the base material subjected to the surface treatment method according to the embodiment. The vertical axis of the graph shown in FIG. 8 is the heat dissipation ΔT, and the horizontal axis of the graph is the emissivity ε. The heat dissipation ΔT is the difference between the surface temperature Ts and the ambient temperature Ta of each of the embodiment and the multiple comparative examples. The larger the heat dissipation ΔT, the greater the increase in the temperature of the measured object due to the influence of heating by the heat source, or the smaller the amount of heat dissipation of the measured object relative to the increase in the temperature of the measured object due to the influence of heating by the heat source. The emissivity ε is a value measured by a radiation thermometer. The larger the emissivity ε, the greater the radiative emittance of the measured object. Therefore, the smaller the heat dissipation ΔT and the larger the emissivity ε, the greater the heat dissipation of the measured object. As shown in FIG. 8, most of the comparative examples have a large heat dissipation ΔT and a small emissivity ε, whereas the heat dissipation ΔT of the measured object is suppressed to a small value and the emissivity ε is large in the second embodiment. Here, Fe3O4 of the target particle TP1 has a smaller heat dissipation ΔT and a larger emissivity than aluminum. Therefore, by carrying out the above-mentioned surface treatment method, the emissivity of the surface layer of the base material in which the target particles are embedded is improved, and the heat dissipation is improved. In other words, it was confirmed that by carrying out the above-mentioned surface treatment method, the function related to the target particles contained in the projection material can be appropriately imparted to the surface layer of the base material. [Explanation of symbols]
[0063] 2...rotating vessel, 6...driving unit, 10...manufacturing device, 20...blasting device, 30...storage vessel, 40...nozzle, 41...treatment chamber, 50...control device, 71-76...measurement point, BM...base material, CP...core particle, MM...manufacturing method, SM...surface treatment method, TP, TP1...target particle.
Claims
1. providing a core particle and a target particle; forming a projection material by electrostatically attaching the target particles to the core particles; A method for producing a projection material, comprising:
2. The forming step includes: containing the core particles and the target particles in a rotating vessel; rotating the rotary container to agitate the core particles and the target particles; The method for producing the projection material according to claim 1 , comprising:
3. The method for producing a projection material according to claim 1 or 2, wherein the core particles and the target particles have different charging characteristics.
4. A surface treatment method, further comprising a step of colliding the projection material manufactured by the projection material manufacturing method according to claim 1 or 2 against a surface of a base material.
5. The surface treatment method according to claim 4 , wherein the step of colliding includes a step of spraying the blast material onto the base material.
6. The surface treatment method according to claim 5 , wherein in the blasting step, the blast material is blasted onto the base material at a pressure of 0.01 MPa or more and 0.3 MPa or less.
7. In the blasting step, the blast material is blasted onto the base material by an air blast device; The average particle size of the core particles is 5 μm or more, The surface treatment method according to claim 5 , wherein an average particle size of the target particles is smaller than an average particle size of the core particles.
Citation Information
Patent Citations
Mechanical plating projection material and high corrosion resistance coating
JP2017082322A