Solid oxide fuel cell

The laminated electrolyte layer structure in proton conductive SOFCs addresses the issue of low durability by preventing pinholes and barium carbonate formation, resulting in improved long-term cell performance.

JP2024139407APending Publication Date: 2024-10-09TOKYO GAS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023050326
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Proton conductive solid oxide fuel cells (SOFCs) face challenges with low long-term durability, despite their high power generation efficiency.

Method used

A proton conductive solid oxide fuel cell design featuring an electrolyte layer with a laminated structure, including a first layer containing compounds represented by specific formulas and a second layer without cerium, to prevent pinholes and enhance durability.

Benefits of technology

The design significantly improves the long-term durability of proton conductive SOFCs by preventing pinholes and reducing the formation of barium carbonate, leading to enhanced cell performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139407000006
    Figure 2024139407000006
  • Figure 2024139407000007
    Figure 2024139407000007
  • Figure 2024139407000001
    Figure 2024139407000001
Patent Text Reader

Abstract

To provide a proton conduction type solid oxide fuel cell with a good long period durability.SOLUTION: A solid oxide fuel cell comprises: an air electrode; a fuel electrode; and an electrolyte layer that is provided between the air electrode and the fuel electrode, and does not have a pin hole. The electrolyte layer at least includes a structure in which a first layer that is provided to a surface of the fuel electrode side of the air electrode, and contains any one of chemical compounds selected from a group consisting of a chemical compound A expressed by a formula (A), a chemical compound B expressed by a formula (B), and a chemical compound C expressed by a formula (C); and a second layer that is provided to a surface of the air electrode side of the fuel electrode, and contains the chemical compound A expressed by the formula (A) are laminated. [In the formula (A), M1:Sr or Ca, M2:Y, Yb, Sc or the like, 0≤x≤1, 0≤y≤1, 0≤z≤0.3; in the formula (B), M3:Ba, Sr or the like, M4:Yb, Sc or the like, 0≤x≤0.5; and in the formula (C), 0≤x≤1].SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a proton conducting solid oxide fuel cell. [Background technology]

[0002] Conventionally, oxygen ions (O 2- Solid oxide fuel cells (SOFCs) that use protons (H + Proton-conducting SOFCs, which use a proton-conducting solid oxide with cations of 1,2-tetrafluoroethylene (Pb) as the conductive ion as an electrolyte, are attracting attention as the next generation of fuel cells. Proton-conducting SOFCs do not generate water on the fuel electrode side, so the fuel concentration does not decrease. The power generation efficiency of a fuel cell is proportional to the current efficiency and voltage efficiency. Increasing the fuel utilization rate without decreasing the fuel concentration increases the current efficiency, which results in highly efficient power generation. Various reports have been published on proton-conducting SOFCs.

[0003] For example, Patent Document 1 discloses a fuel cell that includes a fuel electrode, an air electrode, and an electrolyte layer provided between the fuel electrode and the air electrode. 1-x M1 x (Ce 1-y Zr y ) 1-z M2 z O 3-δ (M1 is either one or both of Sr and Ca, M2 is one or more of Y, Yb, Gd, Sc, and In, 0≦x≦0.5, 0.5≦y≦1, 0.1≦z≦0.3), La 1-x M3 x M4O 3-δ (M3 is one or more of Ba, Sr, Ca, and Mg, M4 is one or more of Yb, Sc, Y, In, and Al, 0≦x≦0.5), and La 28-x W 4+x O54+δ A first layer including any one of (0≦x≦1), and a second layer including Ba 1-x M5 x (Ce 1-y Zr y ) 1-z M6 z O 3-δ (M5 is either one or both of Sr and Ca, M6 is one or more of Y, Yb, Gd, Sc, and In, 0≦x≦0.5, 0≦y≦0.5, 0.1≦z≦0.3), or La 28-x W 4+x O 54+δ (0≦x≦1), and a Ba 1-x M1 x (Ce 1-y Zr y ) 1-z M2 z O 3-δ (M1 is either one or both of Sr and Ca, and M2 is one or more of Y, Yb, Gd, Sc, and In, 0≦x≦0.5, 0.5≦y≦1, 0.1≦z≦0.3), and a second layer containing the same. Furthermore, Patent Document 2 discloses a solid oxide fuel cell (M represents at least one element selected from the group consisting of scandium, yttrium, lanthanides, and actinides) including a fuel electrode, a solid oxide electrolyte formed on one surface of the fuel electrode, an intermediate layer formed on the solid oxide electrolyte and containing a mixture of M2Ce2O7 and a solid solution of M and CeO2, and a cathode formed on the intermediate layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-17425 A [Patent Document 2] JP 2016-170976 A Summary of the Invention [Problem to be solved by the invention]

[0005] Although proton-conducting SOFC cells have high power generation efficiency, they have a problem of low long-term durability. Therefore, there is a demand for the development of proton-conducting SOFC cells with excellent long-term durability. Various methods for improving the durability of proton-conductive SOFC cells have been studied. For example, in Patent Document 1, the durability of the SOFC cell is improved by multi-layering the electrolyte layer. In addition, in Patent Document 2, in consideration of the fact that the generation of barium carbonate on the fuel electrode side can be a cause of deterioration of the proton-conductive SOFC cell, cerium (Ce), which can promote the generation of barium carbonate, is not contained in the solid oxide electrolyte in contact with the fuel electrode, but is contained in an intermediate layer provided on the solid oxide electrolyte on the air electrode side, thereby suppressing the deterioration of the SOFC cell and improving its durability. However, the techniques described in Patent Documents 1 and 2 do not sufficiently improve the long-term durability of proton-conductive SOFC cells, and there is still room for improvement.

[0006] The present disclosure has been made in consideration of the above-mentioned circumstances. An object of one embodiment of the present disclosure is to provide a proton conductive solid oxide fuel cell that is excellent in long-term durability. [Means for solving the problem]

[0007] Specific means for solving the problems include the following aspects. <1> An air electrode; A fuel electrode; an electrolyte layer provided between the air electrode and the fuel electrode and having no pinholes; Equipped with The electrolyte layer is a solid oxide fuel cell having a structure in which at least a first layer is provided on the surface of the air electrode facing the fuel electrode and contains any one compound selected from the group consisting of a compound A represented by the following formula (A), a compound B represented by the following formula (B), and a compound C represented by the following formula (C), and a second layer is provided on the surface of the fuel electrode facing the air electrode and contains a compound A represented by the following formula (A):

[0008] [ka]

[0009] In formula (A), M1 represents one metal element selected from the group consisting of Sr and Ca, M2 represents at least one metal element selected from the group consisting of Y, Yb, Gd, Sc, and In, x satisfies 0≦x≦1, y satisfies 0≦y≦1, and z satisfies 0≦z≦0.3. In formula (B), M3 represents at least one metal element selected from the group consisting of Ba, Sr, Ca, and Mg, M4 represents at least one metal element selected from the group consisting of Yb, Sc, Y, In, and Al, and x satisfies 0≦x≦0.5. In formula (C), x satisfies 0≦x≦1.

[0010] <2> The thickness of the electrolyte layer is 20 μm to 30 μm. <1> The solid oxide fuel cell according to claim 1. <3> The second layer contains a compound A in which y in formula (A) is 0. <1> or <2> The solid oxide fuel cell according to claim 1. Effect of the Invention

[0011] According to one embodiment of the present disclosure, a proton conductive solid oxide fuel cell having excellent long-term durability is provided. [Brief description of the drawings]

[0012] [Figure 1A]1 is a graph showing the relationship between output voltage and endurance time in solid oxide fuel cells of Example 1 and Comparative Example 1. [Figure 1B] 1 is a graph showing the relationship between the output voltage and the endurance time in the solid oxide fuel cells of Example 2, Comparative Example 2, and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The fuel cell of the present disclosure will be described in detail below. The following description of the requirements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0014] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the lower limit and upper limit, respectively. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0015] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0016] In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0017] [Solid oxide fuel cell] The solid oxide fuel cell of the present disclosure comprises an air electrode (also referred to as "cathode"), a fuel electrode (also referred to as "anode"), and an electrolyte layer that is free of pinholes and is provided between the air electrode and the fuel electrode. The electrolyte layer has a structure in which at least a first layer is provided on the fuel electrode side surface of the air electrode and contains any one compound selected from the group consisting of compound A represented by formula (A), compound B represented by formula (B), and compound C represented by formula (C), and a second layer is provided on the air electrode side surface of the fuel electrode and contains compound A represented by formula (A). According to the present disclosure, it is possible to provide a proton conductive solid oxide fuel cell having excellent long-term durability.

[0018] <Air electrode> The solid oxide fuel cell of the present disclosure includes a cathode. At the air electrode, oxygen in the oxidant gas captures electrons to form oxygen ions. The air electrode is preferably formed of a material that is porous, has high electronic conductivity, and is unlikely to undergo solid-state reactions with the solid oxide electrolyte at high temperatures. The material of the air electrode is, for example, BaGd 0.7 La 0.3 Co2O 6-σ (BGLC) and Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O 3-σ (BSCF) is one example. The material for the air electrode is, for example, La 0.8 Sr 0.2 MnO3(LSM), La 0.6 Ca 0.4 MnO3(LCM) and La 0.6 Sr 0.4 Fe 0.8 Co 0.2 O3(LSCF) is one example. The air electrode may be formed from a mixed material in which two or more of the above materials are mixed.

[0019] <Fuel electrode> The solid oxide fuel cell of the present disclosure includes an anode. At the fuel electrode, the oxygen ions react with the fuel in the reformed gas to release electrons. The fuel electrode is preferably, for example, porous, has high ion conductivity, and is unlikely to undergo solid-state reactions with the solid oxide electrolyte at high temperatures. Examples of the material for the fuel electrode include nickel metal (Ni) and nickel compounds such as nickel oxide (NiO). 0.8 Yb 0.2 O 3-σ A porous cermet containing Ni, such as (Ni-BZYb), is preferred. Examples of the porous cermet containing Ni include a porous cermet of yttria-stabilized zirconia (YSZ) / nickel metal, and a porous cermet of scandia-stabilized zirconia (ScSZ) / nickel metal. The fuel electrode may be made of a mixed material in which two or more of the above materials are mixed.

[0020] The fuel electrode preferably comprises a support (so-called anode support) and an active layer (so-called anode active layer). The anode support functions as a support for the cell. The anode support is preferably, for example, porous, has high ion conductivity, and is unlikely to undergo solid-state reactions with the solid oxide electrolyte at high temperatures. The materials for the anode support include those described as the materials for the fuel electrode. The anode active layer contributes to activating the reaction at the fuel electrode. The anode active layer is provided on the surface of the electrolyte layer facing the fuel electrode. The anode active layer is preferably, for example, porous, has high ion conductivity, and is unlikely to undergo solid-state reactions with the solid oxide electrolyte at high temperatures. The materials for the anode active layer include those described as the materials for the fuel electrode. The material of the anode support and the material of the anode active layer may be the same or different, but are preferably the same.

[0021] <Electrolyte layer> The solid oxide fuel cell of the present disclosure includes an electrolyte layer that is provided between an air electrode and a fuel electrode and has no pinholes. The electrolyte layer has a laminated structure including at least a first layer that is provided on the air electrode side of the air electrode and contains any one compound selected from the group consisting of compound A represented by formula (A), compound B represented by formula (B), and compound C represented by formula (C), and a second layer that is provided on the air electrode side of the fuel electrode and contains compound A represented by formula (A). The solid oxide fuel cell of the present disclosure tends to have significantly improved long-term durability due to the absence of pinholes in the electrolyte layer.

[0022] In the present disclosure, the term "pinhole" refers to a minute through hole. Furthermore, the term "no pinholes" in the electrolyte layer means that the electrolyte layer is substantially free of pinholes, and specifically, the density of pinholes on the surface of the electrolyte layer facing the air electrode is 3.5 pcs / cm 2 It means that it is less than.

[0023] The absence of pinholes in the electrolyte layer is confirmed by the following method. A laminate of a fuel electrode and an electrolyte layer (shape: disk-shaped, diameter: 21.0 mm to 22.0 mm, thickness: 1.5 mm) is used as a sample. The sample is sandwiched from above and below using two resin O-rings ("O-rings"; the same applies below), then sandwiched in a cylindrical jig, and a load is applied between the top and bottom at a level that prevents water and air from leaking between the sample and the O-rings. The top of the sample is filled with distilled water to a depth of 5 mm, and air is applied to the bottom of the sample at a pressure of 0.1 kPaG. If no air bubbles are generated from the top of the sample for one minute after the air pressure load begins, it is determined that the electrolyte layer does not have pinholes.

[0024] The presence or absence of pinholes in the electrolyte layer can be controlled by the method of forming the electrolyte layer. For example, the presence or absence of pinholes in the electrolyte layer can be controlled by the thickness of the electrolyte layer to be formed and the coating method used when forming the electrolyte layer.

[0025] For example, if the electrolyte layer is formed thick, pinholes are less likely to occur, whereas if the electrolyte layer is formed thin, pinholes tend to occur more easily. If the electrolyte layer is formed to a thickness of 20 μm or more, pinholes tend to occur less easily.

[0026] For example, when a dip coating method is used as a coating method for forming the electrolyte layer, pinholes tend not to occur in the electrolyte layer.

[0027] In addition, although it depends on the material of the electrolyte layer, the presence or absence of pinholes in the electrolyte layer can also be controlled by adjusting the sintering temperature.

[0028] The electrolyte layer has a structure in which at least a first layer provided on the surface of the air electrode facing the fuel electrode, and a second layer provided on the surface of the fuel electrode facing the air electrode are laminated together.

[0029] The first layer is provided on the surface of the air electrode facing the fuel electrode, and contains any one compound selected from the group consisting of compound A represented by formula (A), compound B represented by formula (B), and compound C represented by formula (C), and preferably contains compound A represented by formula (A).

[0030] [ka]

[0031] In the formula (A), M1 represents one metal element of either Sr or Ca, and is preferably Sr from the viewpoint of electrical conductivity, for example. In formula (A), M2 represents at least one metal element selected from the group consisting of Y, Yb, Gd, Sc, and In, and is preferably at least one metal element selected from Y, Yb, and Sc, and more preferably Y and Yb, or Y and Sc. In formula (A), x satisfies 0≦x≦1, and preferably satisfies 0.1≦x≦0.8. In formula (A), y satisfies 0≦y≦1, and preferably satisfies 0≦y≦0.7. In formula (A), z satisfies 0≦z≦0.3, and preferably satisfies 0≦z≦0.1.

[0032] In formula (B), M3 represents at least one metal element selected from the group consisting of Ba, Sr, Ca, and Mg, and is preferably at least one metal element selected from the group consisting of Sr, Ca, and Mg. In formula (B), M4 represents at least one metal element selected from the group consisting of Yb, Sc, Y, In and Al, and is preferably at least one metal element selected from Yb and Sc. In formula (B), x satisfies 0≦x≦0.5, and it is preferable that x=0.

[0033] In formula (C), x satisfies 0≦x≦1, and it is preferable that x=1.

[0034] Specific examples of materials for the first layer include BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ (BZCYYb), BaZr 0.1 Ce 0.7 Y 0.1 Sc 0.1 O 3-σ (BZCYSc0.1) and BaZr 0.4 Sc 0.6 O 3-σ (BZSc0.6).

[0035] The second layer is provided on the surface of the fuel electrode facing the air electrode, and contains a compound A represented by formula (A). The second layer is a layer in contact with the fuel electrode. The second layer preferably contains a compound A in which y in formula (A) is 0. In formula (A), y being 0 means that the compound A does not contain cerium (Ce). When carbon dioxide (CO2) is contained in the anode gas, the CO2 may react with Ba in the electrolyte layer to produce barium carbonate, which may cause cell deterioration. The production of this barium carbonate is promoted by the presence of Ce. If the second layer, which is the layer in contact with the fuel electrode, does not contain Ce, the solid oxide fuel cell of the present disclosure is less susceptible to deterioration caused by barium carbonate and tends not to lose its long-term durability.

[0036] Specific examples of materials for the second layer include BaZr 0.8 Yb 0.2 O 3-σ (BZYb) is an example.

[0037] The electrolyte layer may have a two-layer structure in which a first layer and a second layer are in contact with each other, or may have a structure in which another layer is laminated between the first layer and the second layer. The other layer may be a single layer or multiple layers. The material of the other layer may be the same as the material of the first layer, may be the same as the material of the second layer, or may be a material different from the material of the first layer and the material of the second layer.

[0038] The thickness of the electrolyte layer is, for example, preferably 20 μm to 30 μm, more preferably 21 μm to 30 μm, and further preferably 22 μm to 30 μm. The thickness of the electrolyte layer means the total thickness of the layers that make up the electrolyte layer. When the thickness of the electrolyte layer is 20 μm or more, the long-term durability of the solid oxide fuel cell tends to be superior. If the thickness of the electrolyte layer is 30 μm or less, degradation of the performance of the solid oxide fuel cell due to an increase in electrical resistance tends not to occur easily.

[0039] In this disclosure, the "thickness of the electrolyte layer" means the average thickness of the electrolyte layer. The average thickness of the electrolyte layer is a value determined by the following method. The thickness of the electrolyte layer is measured at 10 randomly selected points in the thickness direction using a thickness gauge. The arithmetic mean of the measured values ​​is calculated and this value is regarded as the average thickness of the electrolyte layer.

[0040] [Method of manufacturing solid oxide fuel cell] The method for producing the solid oxide fuel cell of the present disclosure is not particularly limited as long as it is possible to produce the solid oxide fuel cell of the present disclosure described above. The solid oxide fuel cell of the present disclosure can be suitably produced, for example, by the following method.

[0041] First, the fuel electrode is prepared. The powder of the material for the anode support is granulated and then pressed into a mold, and the pressed material is sintered on a porous zirconia substrate to produce the anode support.

[0042] Details of the material for the anode support are as described above. The granulation method is not particularly limited, and examples thereof include a spray-drying method and a method using a mortar and pestle. The firing temperature is preferably, for example, 950°C to 1050°C. The firing time is preferably, for example, 0.5 to 2.0 hours.

[0043] Next, a material for an anode active layer is applied to one surface of the prepared anode support, and then fired to form an anode active layer on the anode support.

[0044] The details of the material for the anode active layer are as described above. The coating method is not particularly limited, but a dip coating method is preferable. When the application method is a dip coating method, for example, even when the electrolyte layer is formed relatively thin, pinholes tend not to occur in the electrolyte layer. The firing temperature is preferably, for example, 950°C to 1050°C. The firing time is preferably, for example, 0.5 to 2.0 hours.

[0045] Next, the electrolyte layer is formed. A material for a second layer is applied to the surface of the anode active layer formed above opposite to the anode support side, and then fired to form a second layer on the anode active layer. A material for a first layer is applied to the surface of the second layer formed above opposite to the anode active layer side, and then fired to form a first layer on the second layer. In this manner, a laminate of the fuel electrode and electrolyte layer is obtained, which has a layer structure of fuel electrode (anode support / anode active layer) / electrolyte layer (second layer / first layer).

[0046] The details of the materials for the first layer and the second layer are as described above. When the material of the second layer is BZYb, the material of the fuel electrode (anode active layer) in contact with the second layer is preferably Ni-BZYb. When the material of the second layer is BZYb and the material of the fuel electrode (anode active layer) is Ni-BZYb, pinholes tend to be less likely to occur in the second layer. Although BZYb is a material that is difficult to sinter, it can be sintered sufficiently because the Ni contained in the fuel electrode (anode active layer) diffuses and promotes sintering, and as a result, it is presumed that pinholes are less likely to occur in the second layer.

[0047] The coating method is not particularly limited, but a dip coating method is preferable. The firing temperature is preferably, for example, 1450°C to 1550°C. If the firing temperature is 1450° C. or higher, the material is sintered sufficiently, so that pinholes tend to be less likely to occur. If the firing temperature is 1550° C. or lower, shrinkage tends to be suppressed due to the heat of each layer. The firing time is preferably, for example, 1 hour to 5 hours. The presence or absence of pinholes in the electrolyte layer can be controlled by adjusting the sintering temperature and sintering time, but the conditions for preventing pinholes from occurring in the electrolyte layer depend on the material of the electrolyte layer and cannot be determined in general. For example, when the material of the electrolyte layer is BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ In the case of (BZCYYb), the firing temperature is preferably 1470° C. and the firing time is preferably 2 hours.

[0048] Next, the surface of the anode support opposite to the electrolyte layer side of the resulting laminate is polished until the desired thickness is achieved. The polishing method is not particularly limited, but may be, for example, a method using a rotary polisher equipped with a diamond pad.

[0049] Next, the laminate after polishing is checked for the presence or absence of pinholes. The method for checking whether or not there is a pinhole is as described above, and therefore the description will be omitted.

[0050] Next, the air electrode is formed. A laminate confirmed to be free of pinholes is used to form the air electrode. A material for the air electrode is applied to the surface of the electrolyte layer (first layer) in the laminate opposite the fuel electrode, and then the material is fired on a porous plate made of zirconia (e.g., calcia-stabilized zirconia) to form an air electrode on the electrolyte layer (first layer).

[0051] The application method is not particularly limited, but is preferably a screen printing method. The firing temperature is preferably, for example, 950°C to 1050°C. The firing time is preferably, for example, 1 hour to 3 hours.

[0052] In this manner, the solid oxide fuel cell of the present disclosure can be manufactured. EXAMPLES

[0053] The solid oxide fuel cell of the present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples as long as they do not depart from the gist of the disclosure.

[0054] [Manufacturing of solid oxide fuel cells] Example 1 First, the powder of the material for the anode support was granulated. Ni-BaZr 0.8 Yb 0.2 O 3-σ Graphite (pore former) and polyvinyl butyral (PVB) (binder) were added to [Ni-BZYb (mass ratio: 60 / 40)] and then mixed. The powder obtained by this mixing was placed in a mortar, a small amount of ethanol was added, and then mixed for 15 minutes. The powder obtained by this mixing was dried and then mixed for another 30 minutes. The powder obtained by this mixing was sieved with a pore size of 150 μm. The powder that passed through the sieve was collected and placed in the mortar again, and the same operations as above (from adding ethanol to sieving) were repeated once more to obtain a granulated powder of the material of the anode support. Next, the powder granules of the material for the anode support obtained above were dried at 120° C., and then an appropriate amount was placed in a mold. The granules were filled into the mold using a vibrator, and the jig was set in a press machine and subjected to a pressure of 500 kg / cm. 2 The granules were press-molded under a pressure of 1000° C. The press-molded product was placed on a porous plate made of zirconia and fired at 1000° C. for 2 hours to prepare an anode support. Next, an anode active layer was formed on one surface of the prepared anode support. Ni-BaZr 0.8 Yb 0.2 O 3-σ[Ni-BZYb (mass ratio: 60 / 40)] was mixed with polyvinyl butyral (PVB) (binder), Triton (registered trademark) (antifoaming agent), and ethanol (solvent), and then ground using a zirconia ball mill for one day to prepare a dipping solution. The anode support was placed on a jig, and then immersed in the dipping solution mixed for 10 minutes using an ultrasonic cleaner for 10 seconds to coat one side of the anode support with the dipping solution. The anode support coated with the dipping solution was placed against a dedicated jig and dried in an electric furnace set at 120°C. The above operation of coating the anode support with the dipping solution again and drying was performed on the anode support removed from the electric furnace. The product obtained by this operation was placed on a porous plate made of zirconia and fired at 1000°C for 2 hours. In this manner, a fuel electrode having a layered structure of anode support / anode active layer was produced.

[0055] Next, a second layer constituting an electrolyte layer was formed on the surface of the anode active layer opposite to the anode support. BaZr 0.8 Yb 0.2 O 3-σ Polyvinyl butyral (PVB) (binder), Triton (registered trademark) (antifoaming agent), and ethanol (solvent) were added to (BZYb), and the mixture was ground using a zirconia ball mill for one day to prepare a dipping solution. The fuel electrode was placed on a jig, and then immersed in the dipping solution mixed for 10 minutes using an ultrasonic cleaner for 10 seconds to coat the surface of the anode active layer opposite the anode support with the dipping solution. The fuel electrode coated with the dipping solution was placed against a dedicated jig and dried in an electric furnace set at 120°C. The fuel electrode removed from the electric furnace was again coated with the dipping solution and dried, as described above. The product obtained by this operation was placed on a porous plate made of zirconia and fired at 1470°C for 2 hours. In this manner, a laminate A having a layer structure of fuel electrode (anode support / anode active layer) / electrolyte layer (second layer) was produced.

[0056] Next, a first layer constituting an electrolyte layer was formed on the surface of the second layer opposite to the anode active layer side. BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ Polyvinyl butyral (PVB) (binder), Triton (registered trademark) (antifoaming agent), and ethanol (solvent) were added to (BZCYYb), and the mixture was ground using a zirconia ball mill for one day to prepare a dipping solution. The laminate A was placed on a jig, and then immersed in the dipping solution mixed for 10 minutes using an ultrasonic cleaner for 10 seconds to coat the surface of the second layer opposite the anode active layer with the dipping solution. The laminate A coated with the dipping solution was placed on a special jig and dried in an electric furnace set at 120°C. The laminate A removed from the electric furnace was again coated with the dipping solution and dried, as described above. The product obtained by this operation was placed on a porous plate made of zirconia and fired at 1470°C for 2 hours. In this manner, a laminate B having a layer structure of fuel electrode (anode support / anode active layer) / electrolyte layer (second layer / first layer) was produced.

[0057] Next, the surface of the anode support of the obtained laminate B opposite to the electrolyte layer side was polished using a rotary polisher equipped with a diamond pad while running water.

[0058] Next, the presence or absence of pinholes in the electrolyte layer of the polished laminate B was confirmed. The method for checking for the presence or absence of a pinhole is as described above. As a result, it was confirmed that there were no pinholes.

[0059] Next, an air electrode was formed on the surface of the electrolyte layer (first layer) of laminate B opposite to the fuel electrode side. BaGd with particle size adjusted to 1μm or less 0.7 La 0.3 Co2O 6-σThe (BGLC) powder was placed in a mortar, a small amount of ethanol was added, and the powder was mixed until it was dry. A commercially available printing ink (Vehicle) was added to the dried powder and kneaded to prepare an ink for forming an air electrode. The ink for forming an air electrode was applied to the surface of the electrolyte layer (first layer) opposite the fuel electrode side by screen printing, and then dried. The dried product was placed on a porous plate made of zirconia (e.g., calcia-stabilized zirconia) and fired at 1000°C for 2 hours. As a result of the above, a solid oxide fuel cell having a layered structure of fuel electrode (anode support / anode active layer) / electrolyte layer (second layer / first layer) / air electrode was obtained.

[0060] Example 2 In Example 2, the same operations as in Example 1 were carried out except that the material of the first layer of the electrolyte layer and the material of the air electrode were changed to the materials shown in Table 1, to obtain a solid oxide fuel cell.

[0061] Comparative Example 1 In Comparative Example 1, the same operations as in Example 1 were carried out, except that the thickness of the electrolyte layer was set to the thickness shown in Table 1 when the electrolyte layer was formed, to obtain a solid oxide fuel cell.

[0062] [Comparative Example 2 and Comparative Example 3] In Comparative Example 2 and Comparative Example 3, the material of the first layer of the electrolyte layer and the material of the air electrode were changed to the materials shown in Table 1, and the thickness of the electrolyte layer was set to the thickness shown in Table 1 when the electrolyte layer was formed. Except for this, the same operations as in Example 1 were carried out to obtain solid oxide fuel cells.

[0063] [evaluation] <Long term durability> The long-term durability of solid oxide fuel cells was evaluated. Specifically, the evaluation was carried out as follows. A metal foil made of NCA-1 (ferritic stainless steel) was attached to the periphery of the solid oxide fuel cell using a glass adhesive. Next, the solid oxide fuel cell with the metal foil was placed in an electric furnace and heat-treated at 850°C for 1 hour in an air atmosphere. The gas sealing property of the adhesive interface was confirmed by the penetration of ethanol. A platinum mesh was used for the electrodes. The electrodes were attached to the air electrode (cathode) side using platinum paste, and pressure was applied to the fuel electrode (anode) side. A total of two platinum wires, one for current and one for voltage, were attached to each electrode. The solid oxide fuel cell with the metal foil was sandwiched between a jig made of alumina and placed in the electric furnace. Nitrogen gas with a hydrogen concentration of 4% was flowed on the anode side, and dry air was flowed on the cathode side. The temperature in the electric furnace was raised to 600°C, and then held for 30 minutes, after which the gas on the anode side was switched to hydrogen gas humidified at room temperature. A current was applied so that the cell voltage became 0.85 V, and this current value was maintained. The current density at this time was 0.10 mA / cm 2 ~0.60mA / cm 2 The cell voltage was measured when a constant current was applied, and if the rate at which the cell voltage decreased was less than 1% / kh, the long-term durability was judged to be good, and if the rate at which the cell voltage decreased was 1% / kh or more, the long-term durability was judged to be poor. Details of the solid oxide fuel cell and the evaluation results are shown in Table 1 and in Figures 1(A) and 1(B).

[0064] [Table 1]

[0065] Details of the compounds listed in Table 1 are shown below. <Air electrode> "BGLC":BaGd 0.7 La 0.3 Co2O 6-σ "BSCF":Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O 3-σ <Electrolytes> -First layer- "BZCYYb":BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ "BZCYSc0.1": BaZr 0.1 Ce 0.7 Y 0.1 Sc 0.1 O 3-σ -Second Layer- "BZYb":BaZr 0.8 Yb 0.2 O 3-σ <Fuel electrode> -Anode active layer- "Ni-BZYb": Ni-BaZr 0.8 Yb 0.2 O 3-σ -Anode support- "Ni-BZYb": Ni-BaZr 0.8 Yb 0.2 O 3-σ

[0066] As shown in Table 1 and Figures 1(A) and 1(B), it was clear that the solid oxide fuel cells of the Examples had significantly superior long-term durability compared to the solid oxide fuel cells of the Comparative Examples.

Claims

1. An air electrode; A fuel electrode; an electrolyte layer provided between the air electrode and the fuel electrode and having no pinholes; Equipped with The electrolyte layer is a solid oxide fuel cell having a structure in which at least a first layer is provided on the surface of the air electrode facing the fuel electrode and contains any one compound selected from the group consisting of a compound A represented by the following formula (A), a compound B represented by the following formula (B), and a compound C represented by the following formula (C), and a second layer is provided on the surface of the fuel electrode facing the air electrode and contains a compound A represented by the following formula (A): [Formula 1] In formula (A), M1 represents one metal element of Sr or Ca, M2 represents at least one metal element selected from the group consisting of Y, Yb, Gd, Sc, and In, x satisfies 0≦x≦1, y satisfies 0≦y≦1, and z satisfies 0≦z≦0.

3. In formula (B), M3 represents at least one metal element selected from the group consisting of Ba, Sr, Ca, and Mg, M4 represents at least one metal element selected from the group consisting of Yb, Sc, Y, In, and Al, and x satisfies 0≦x≦0.

5. In formula (C), x satisfies 0≦x≦1.

2. 2. The solid oxide fuel cell according to claim 1, wherein the electrolyte layer has a thickness of 20 μm to 30 μm.

3. The solid oxide fuel cell according to claim 1 , wherein the second layer contains a compound A in which y in formula (A) is 0.

Citation Information

Patent Citations

  • Fuel cell and manufacturing method thereof

    JP2020017425A

  • Solid oxide fuel cell with mixed conductor layer

    JP2020091949A

  • Solid electrolytic member, solid oxide type fuel battery, water electrolyzer, hydrogen pump and manufacturing method of solid electrolytic member

    JP2020129433A

  • Fuel electrode-solid electrolyte layer composite, fuel electrode-solid electrolyte layer composite member, fuel cell, and fuel cell manufacturing method

    JP2022119219A

  • Electrode for proton-conducting ceramic cell, manufacturing method thereof, and proton-conducting ceramic cell using the same

    JP2023006322A