Rare earth bond magnet

The rare earth bonded magnet with isotropic Nd-Fe-B powder and cured epoxy resin addresses the issues of mechanical strength and electrical resistance, improving motor performance and efficiency.

JP2024139696APending Publication Date: 2024-10-09MINEBEAMITSUMI INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024021609
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-02-16
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing rare earth bonded magnets face issues with increased inertia, number of parts, and cost due to protective covers, and insufficient electrical resistance leading to eddy current loss in high-speed motors, necessitating improved mechanical strength and electrical resistance without compromising magnetic properties.

Method used

A rare earth bonded magnet composed of isotropic Nd-Fe-B magnet powder and a cured epoxy resin, with a porosity of less than 5% and electrical resistivity of 100 μΩ·m or more, achieving a radial crushing strength of 60 MPa or more.

Benefits of technology

The solution provides high radial crushing strength and electrical resistance without significantly deteriorating magnetic properties, enhancing motor performance and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139696000003
    Figure 2024139696000003
  • Figure 2024139696000001
    Figure 2024139696000001
  • Figure 2024139696000002
    Figure 2024139696000002
Patent Text Reader

Abstract

To provide a rare earth bond magnet which has high radial crushing strength and electric resistance, without drastically reducing magnetic characteristics.SOLUTION: A rare earth bond magnet contains rare earth magnet powder and a resin cured product of a thermosetting resin, wherein the rare earth bond magnet powder is isotropic Nd-Fe-B-based magnet powder, the thermosetting resin is an epoxy resin, more than 5 wt.% and 6.5 wt.% or less of the resin cured product is contained in 100 wt.% of the rare earth bond magnet, and the rare earth bond magnet has a porosity of less than 5%, radial crushing strength of 60 Mpa or more and electric resistance of 100 μΩ m or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rare earth bonded magnet. [Background technology]

[0002] In recent years, rare earth permanent magnets have been applied in a wide range of fields, including rotating equipment such as motors, general home appliances, audio equipment, medical equipment, and general industrial equipment, due to their excellent magnetic properties. In particular, rare earth bonded magnets obtained from rare earth magnet powder and a binder (resin) that binds the powder have a high degree of freedom in shape, which contributes to the miniaturization and high performance of the above-mentioned equipment. As such rare earth bonded magnets, rare earth bonded magnets have been proposed that consist of Nd-Fe-B magnet powder as the rare earth magnet powder and epoxy resin as the binder, which is a thermosetting resin (see, for example, Patent Document 1).

[0003] In the rare earth bonded magnet of Patent Document 1, Nd-Fe-B quenched magnet powder is used as the rare earth magnet powder, and epoxy resin is used as the binder resin, with approximately 2.5 wt % epoxy resin mixed in.

[0004] Furthermore, when a rare earth bonded magnet is incorporated into a motor that rotates at high speed, a large centrifugal force acts on the rotor to which the rare earth bonded magnet is attached, and there is a risk that the rare earth bonded magnet will break and fly apart. As a means to prevent the rare earth bonded magnet from flying apart, a configuration has been proposed in which a protective cover made of reinforced plastic is provided on the rare earth bonded magnet (for example, see Patent Document 2). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-314605 [Patent Document 2] Japanese Patent Application Publication No. 8-107641 Summary of the Invention [Problem to be solved by the invention]

[0006] If a protective cover made of reinforced plastic as described in Patent Document 2 is provided on a rare earth bonded magnet as described in Patent Document 1, it is possible to prevent the rare earth bonded magnet from scattering, but there are problems such as an increase in the weight of the rotor, greater inertia, an increase in the number of parts, and an increase in installation steps, which increases costs, etc. For this reason, it is necessary to increase the mechanical strength (radial crushing strength) of the rare earth bonded magnet.

[0007] Furthermore, compared to rare earth sintered magnets, rare earth bonded magnets have the advantage of high electrical resistance due to the presence of insulating resin between the magnet powder particles. However, when a rare earth bonded magnet containing conventional Nd-Fe-B magnet powder and 2wt% to 3wt% resin is incorporated into a high-speed motor, the electrical resistance is not necessarily high, which causes problems such as large eddy current loss and reduced motor efficiency. For this reason, it is necessary to increase the electrical resistance.

[0008] As described above, in a configuration in which a rare earth bonded magnet containing a thermosetting resin is used in a motor that rotates at high speed, there is room for further improvement with respect to the rare earth bonded magnet.

[0009] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a rare earth bonded magnet that has high radial crushing strength and electrical resistance without causing a significant decrease in the magnetic properties of the rare earth bonded magnet. [Means for solving the problem]

[0010] In order to solve the above-mentioned problems and achieve the object, a rare earth bonded magnet according to one embodiment of the present invention is a rare earth bonded magnet comprising rare earth magnet powder and a cured resin of a thermosetting resin, wherein the rare earth magnet powder is an isotropic Nd-Fe-B based magnet powder, the thermosetting resin is an epoxy resin, the cured resin is contained in an amount of more than 5 weight % and not more than 6.5 weight % based on 100 weight % of the rare earth bonded magnet, and the rare earth bonded magnet has a porosity of less than 5%, a radial crushing strength of 60 MPa or more, and an electrical resistivity of 100 μΩ·m or more. Effect of the Invention

[0011] According to one aspect of the present invention, a rare earth bonded magnet having high radial crushing strength and electrical resistivity can be obtained without causing a significant decrease in the magnetic properties of the rare earth bonded magnet. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing the ratio (Vol %) of rare earth magnet powder, hardened thermosetting resin, and voids in a rare earth magnet bond. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Note that the present invention is not limited to this embodiment. In addition, the components in the following embodiments include those that are replaceable and easy for a person skilled in the art, or those that are substantially the same.

[0014] <Embodiment 1> The rare earth bonded magnet of the first embodiment includes a rare earth magnet powder and a resin cured product of a thermosetting resin. The rare earth magnet powder is an isotropic Nd (neodymium)-Fe (iron)-B (boron) magnet powder. Examples of the isotropic Nd-Fe-B magnet powder include MQP-14-12 (product name), MQP-8-5 (product name), MQP-10-8.5HD (product name), MQP-11-8 (product name), and MQP12-8HD (product name) manufactured by Magnequench.

[0015] Alternatively, for example, Nd-Fe-B magnet powder produced by a rapid cooling method may be used. Specifically, an Nd-Fe-B alloy is melted by high-frequency induction heating under reduced pressure or in an argon atmosphere. The melted alloy is then sprayed onto a rotating copper roll for rapid cooling (rapid cooling) to produce ribbon-shaped strips. The strips are then broken into pieces of, for example, several mm to several tens of mm, and then crushed by a crusher or the like to obtain powder. The crushed powder is classified using a sieve with a predetermined mesh, and then heat-treated to produce rare earth magnet powder. This rare earth magnet powder is magnetically isotropic because the magnetization easy axis of each crystal grain is not aligned in one direction.

[0016] The rare earth magnet powder preferably has a particle size in the range of 45 μm or more and less than 175 μm. The rare earth magnet powder may have a particle size in the range of 45 μm or more and less than 75 μm, or may have a particle size in the range of 75 μm or more and less than 175 μm. The particle size range can be adjusted by classification using a sieve with a specified mesh.

[0017] The cured thermosetting resin contained in the rare earth bonded magnet of embodiment 1 is specifically a cured epoxy resin, that is, the thermosetting resin is an epoxy resin.

[0018] The rare earth bonded magnet contains more than 5% by weight and not more than 6.5% by weight of the cured resin. The rare earth magnet powder is contained in an amount of 93.5% by weight or more and less than 95% by weight. In the rare earth bonded magnet of embodiment 1, it is preferable that the rare earth magnet powder and the cured resin of the thermosetting resin are uniformly mixed. Conventionally, when producing a bonded magnet using a thermosetting resin, the binder ratio is used in an amount of 2% by weight or more and not more than 3% by weight.

[0019] The rare earth bonded magnet of embodiment 1 has a porosity of less than 5%. Thus, since the rare earth bonded magnet of embodiment 1 contains the above amount of cured thermosetting resin, the porosity is low and the radial crushing strength is high. In other words, the rare earth bonded magnet of embodiment 1 has a radial crushing strength of 60 MPa or more. Furthermore, since the rare earth bonded magnet of embodiment 1 has a low porosity and a relatively high volume ratio of rare earth magnet powder, the deterioration of magnetic properties is also suppressed.

[0020] Furthermore, since the rare earth bonded magnet of embodiment 1 contains the above amount of cured thermosetting resin, it has high electrical resistance, that is, the rare earth bonded magnet of embodiment 1 has an electrical resistivity of 100 μΩ·m or more.

[0021] The rare earth bonded magnet of the first embodiment can be produced, for example, as follows. First, the rare earth magnet powder and the components constituting the cured resin in the rare earth bonded magnet (the raw material components of the cured resin) are mixed in a predetermined mixing ratio to produce a compound. The mixing ratio of the rare earth magnet powder and the raw material components of the cured resin is considered to be the same as the ratio of the rare earth magnet powder and the cured resin in the rare earth bonded magnet after production. The raw material components of the cured resin include a thermosetting resin (e.g., epoxy resin) as a binder, and a curing agent. Furthermore, when producing the compound, a small amount of a lubricant (e.g., calcium stearate) may be added. Specifically, the lubricant may be mixed in an amount of 0.02% by weight or more and less than 0.5% by weight with respect to the total 100% by weight of the rare earth magnet powder and the raw material components of the cured resin.

[0022] Next, the compound is filled into the cavity of the mold and compressed under a predetermined pressure to produce a green body. The green body is then removed from the mold and placed in an oven, where it is thermally cured at a predetermined temperature for a predetermined time to produce a cured body (thermosetting body) containing the rare earth magnet powder and the cured resin. It is also preferable to apply a rust prevention means to the surface of the cured body to prevent oxidation. As the rust prevention means, known means such as electrocoating and spray coating can be applied. In this way, the rare earth bonded magnet of embodiment 1 is obtained.

[0023] <Embodiment 2> One of the objectives of the second embodiment is to prevent a significant decrease in the magnetic properties of the rare earth bonded magnet even when the rare earth magnetic powder is small.

[0024] In order to solve the above-mentioned problems and achieve the object, the rare earth bonded magnet according to the second embodiment is a rare earth bonded magnet containing rare earth magnet powder and a resin cured product of a thermosetting resin, the rare earth magnet powder is an isotropic Nd-Fe-B magnet powder, the thermosetting resin is an epoxy resin, the resin cured product is contained in an amount of more than 5% by weight and not more than 6.5% by weight in 100% by weight of the rare earth bonded magnet, the particle size of the rare earth magnet powder is 45 μm or less, and the surface of the rare earth magnet powder is coated with a compound containing phosphorus. In the second embodiment, as in the first embodiment, the rare earth bonded magnet preferably has a porosity of less than 5%, a ring strength of 60 MPa or more, and an electrical resistivity of 100 μΩ·m or more.

[0025] By subjecting the rare earth magnet powder to a phosphate treatment after crushing, it is possible to prevent the magnet powder from being oxidized and degraded, thereby preventing a significant decrease in the magnetic properties of the rare earth bonded magnet.

[0026] Furthermore, when the above-mentioned phosphate treatment is performed, even if the particle size of the rare earth magnet powder is greater than 0 μm and less than 45 μm, it is possible to provide a rare earth bonded magnet without preventing a significant deterioration in the magnetic properties of the rare earth bonded magnet.

[0027] Furthermore, the rare earth magnet powder is not limited to Nd-Fe-B quenched magnet powder, but may be isotropic Sm-Fe-N, anisotropic Sm-Fe-N, anisotropic Nd-Fe-B magnet powder (product name d-HDDR), or SmCo magnet powder (pulverized anisotropic magnet powder).

[0028] Furthermore, the thermosetting resin may be a conductive epoxy resin. In this case, in the process of electrocoating in which an electric current is passed through the magnet to coat the conductive epoxy resin for rust prevention, the magnet itself is conductive, so that the electrocoating adheres easily and the film-forming properties of the electrocoating can be improved. The manufacturing methods of the rare earth magnet powder, the cured resin of the thermosetting resin, and the rare earth bonded magnet are the same as those of embodiment 1 except for the above.

[0029] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The following examples correspond to embodiment 1.

[0030] [Example] <Production of rare earth bonded magnets> Isotropic Nd-Fe-B magnet powder was used as the rare earth magnet powder. MQP-14-12 (product name) manufactured by Magnequench was prepared as the isotropic Nd-Fe-B magnet powder. The particle size of MQP-14-12 was classified into two groups, 75 μm or more and less than 150 μm, and 45 μm or more and less than 75 μm. In this case, the classification was performed using a sieve with a specified mesh. Next, for each of the two groups, a compound was prepared by mixing isotropic Nd-Fe-B magnet powder with raw material components for the cured resin, including an epoxy resin binder and a curing agent (manufactured by Pernock, model number XW2310), in a specified mixing ratio. Here, the mixing ratio of the rare earth magnet powder and the raw material components for the cured resin was 2.5% by weight, and 97.5% by weight of the raw material components for the cured resin, with the total weight being 100% by weight. Furthermore, compounds were also prepared for the following cases: when the raw material components of the resin cured product were 5% by weight and the rare earth magnet powder was 95% by weight; when the raw material components of the resin cured product were 5.5% by weight and the rare earth magnet powder was 94.5% by weight; when the raw material components of the resin cured product were 6% by weight and the rare earth magnet powder was 94% by weight; when the raw material components of the resin cured product were 6.5% by weight and the rare earth magnet powder was 93.5% by weight; and when the raw material components of the resin cured product were 7.5% by weight and the rare earth magnet powder was 92.5% by weight. The compounds were prepared by mixing the raw material components of the resin cured product dissolved in a solvent with the rare earth magnet powder, evaporating the solvent, and then crushing and classifying the mixture. All the compounds were prepared with the same particle size, and the fluidity conditions for filling the cavity of the mold were the same. Next, the compound is filled into the cavity of the mold and pressed under a specified pressure (molding pressure: surface pressure 5 ton / cm 2 ) was added and compressed to produce a green body. The green body had a cylindrical shape with a diameter of Φ10 mm and a height of 7 mm. Next, the green body was removed from the mold and placed in an oven, where it was thermally cured at a specified temperature (150°C) for a specified time to produce a cured body (thermosetting body). The cured body had a cylindrical shape with a diameter of Φ10 mm and a height of 7 mm. Thus, there was no difference in size between the green body and the cured body. Next, a rust prevention measure (specifically, electrodeposition coating) was applied to the surface of the cured body to prevent oxidation. In this manner, rare earth bonded magnets (samples 1 to 12) containing rare earth magnet powder and a cured thermosetting resin were produced, where samples 3 to 5 and 9 to 11 are examples, and samples 1, 2, 6, 7, 8 and 12 are comparative examples.

[0031] <Evaluation method> (porosity) The porosity was calculated from the apparent density relative to the true density. The evaluation criteria were as follows: A: The porosity is less than 5%. △: Porosity is 5% or more and less than 15%. ×: The porosity is 15% or more.

[0032] (Ring crushing strength) The radial crushing strength was measured based on JIS Z 2507. The evaluation criteria are as follows: ◎: Radial crushing strength is 100 MPa or more. ◯: The radial crushing strength is 60 MPa or more and less than 100 MPa. △: The radial crushing strength is 50 MPa or more and less than 60 MPa. ×: The radial crushing strength is less than 50 MPa.

[0033] (Electrical resistivity) The electrical resistivity was measured using a four-point probe method. The magnet sample shape was Φ10 mm and height 7 mm, and the average electrical resistivity was calculated for N5 evaluations. The evaluation criteria were as follows: ◎: Electrical resistivity is 100 μΩ·m or more. ○: Electrical resistivity is 10 μΩ·m or more and less than 100 μΩ·m. △: Electrical resistivity is less than 10 μΩ·m.

[0034] (comprehensive evaluation) A comprehensive evaluation was performed on Samples 1 to 12. The evaluation criteria were as follows. ◯: The evaluation results for both radial crushing strength and electrical resistivity are ◯. ×: Other than the above. The evaluation results of Samples 1 to 12 are shown in Tables 1 and 2 below. In Table 1, "45-75" for the magnetic powder particle size (μm) indicates that the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 45 μm or more and less than 75 μm. In Table 2, "75-150" for the magnetic powder particle size (μm) indicates that the particle size of the isotropic Nd-Fe-B magnet powder is in the range of 75 μm or more and less than 150 μm.

[0035] [Table 1]

[0036] Table 1 shows samples 1 to 6, which are rare earth bonded magnets with isotropic Nd-Fe-B magnet powder particle sizes in the range of 45 μm or more and less than 75 μm. Sample 1, in which the amount of raw material components in the resin cured material is 2.5% by weight, has a porosity of 15% or more, and both the radial crushing strength and electrical resistance (surface resistivity) were evaluated as fair. This is because the amount of raw material components in the resin cured material is almost the same as that of conventional rare earth bonded magnets. Sample 6, in which the amount of raw material components in the resin cured material is 7.5% by weight, was not evaluated because some of the binder leaked out of the cavity, which caused problems in production. This is because the amount of raw material components in the resin cured material was too high. The evaluations of samples 3 to 5, other than the samples with the amounts of raw material components of the resin cured product of 2.5 wt%, 5 wt%, and 7.5 wt%, were all rated as ⊚. Therefore, the overall evaluation of samples 3 to 5 shown in Table 1 was rated as ◯. The results in Table 1 show that as the porosity in the rare earth bonded magnet decreases, the radial crushing strength and electrical resistivity increase. In the examples, Samples 3 to 5, both the radial crushing strength and electrical resistivity can be increased. In addition, compared to sample 1 (comparative example), in which the amount of raw material components in the cured resin product was 2.5% by weight, samples 3 to 5 have an increased amount of raw material components in the cured resin product, resulting in a slightly lower filling ratio of the magnetic powder. However, this is only a slight decrease compared to the magnetic properties of the rare earth bonded magnet of sample 1 (comparative example), and it has been confirmed that magnetic properties that are comparable to those of the rare earth bonded magnet of sample 1 (comparative example) can be obtained.

[0037] [Table 2]

[0038] Table 2 shows the evaluation of samples 7 to 12, which are rare earth bonded magnets with isotropic Nd-Fe-B magnet powder particle sizes in the range of 75 μm or more and less than 150 μm. Sample 7, in which the amount of raw material components in the resin cured material is 2.5% by weight, has a porosity of 15% or more, and both the radial crushing strength and electrical resistivity were evaluated as fair. This is because the amount of raw material components in the resin cured material is almost the same as that of conventional rare earth bonded magnets. Sample 12, in which the amount of raw material components in the resin cured material is 7.5% by weight, was not evaluated because some of the binder leaked out of the cavity, which caused problems in production. This is because the amount of raw material components in the resin cured material was too high. The evaluations of Samples 9 to 11, other than the samples with the amounts of raw material components of the resin cured product of 2.5 wt%, 5 wt%, and 7.5 wt%, were all rated as ⊚. Therefore, the overall evaluation of Samples 9 to 11 shown in Table 2 was rated as ◯. The results in Table 2 show that as the porosity in the rare earth bonded magnet decreases, the radial crushing strength and electrical resistivity increase. In Samples 9 to 11, which are examples, both the radial crushing strength and electrical resistivity can be increased. In addition, compared to sample 7 (comparative example), which has a raw material component amount of 2.5 weight % of the cured resin material, as in the conventional case, samples 9 to 11 have an increased amount of raw material components of the cured resin material, resulting in a slightly lower filling ratio of the magnetic powder.However, this is only a slight decrease compared to the magnetic properties of the rare earth bonded magnet of sample 7 (comparative example), and it has been confirmed that magnetic properties that are comparable to those of the rare earth bonded magnet of sample 7 (comparative example) can be obtained.

[0039] FIG. 1 shows the ratio (Vol%) of rare earth magnet powder, hardened thermosetting resin, and voids in the rare earth magnet bond. Specifically, samples 1 to 6 are shown. Samples 3 to 5 have a reduced ratio of voids, which indicates that the radial crushing strength is higher. Samples 3 to 5 also have almost no reduction in the ratio of rare earth magnet powder, which indicates that the deterioration of the magnetic properties is suppressed. The void ratio was calculated as follows. Magnetic powder density 7.6 [g / cm 3 ], resin specific gravity 0.92[g / cm 3The true density of the prototype magnet was calculated from the volume ratio of magnetic powder to resin in the true density, and the remainder was taken as the porosity.

Claims

1. A rare earth bonded magnet containing rare earth magnet powder and a cured resin of a thermosetting resin, the rare earth magnet powder is an isotropic Nd—Fe—B magnet powder, the thermosetting resin is an epoxy resin, The cured resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight based on 100% by weight of the rare earth bonded magnet, The rare earth bonded magnet has a porosity of less than 5%, a radial crushing strength of 60 MPa or more, and an electrical resistivity of 100 μΩ·m or more. Rare earth bonded magnet.

2. A rare earth bonded magnet containing rare earth magnet powder and a cured resin of a thermosetting resin, the thermosetting resin is an epoxy resin, The cured resin is contained in an amount of more than 5% by weight and not more than 6.5% by weight based on 100% by weight of the rare earth bonded magnet, The rare earth magnet powder has a particle size of 45 μm or less, The surface of the rare earth magnet powder is coated with a compound containing phosphorus. Rare earth bonded magnet.

3. The rare earth magnet powder is an isotropic Nd—Fe—B magnet powder.

3. The rare earth bonded magnet according to claim 2.

4. The rare earth magnet powder is anisotropic Nd—Fe—B magnet powder.

3. The rare earth bonded magnet according to claim 2.

5. The rare earth magnet powder is an isotropic Sm—Fe—N magnet powder.

3. The rare earth bonded magnet according to claim 2.

6. The rare earth magnet powder is anisotropic Sm—Fe—N magnet powder.

3. The rare earth bonded magnet according to claim 2.

7. The rare earth magnet powder is anisotropic SmCo-based magnet powder.

3. The rare earth bonded magnet according to claim 2.

8. The epoxy resin has electrical conductivity.

3. The rare earth bonded magnet according to claim 2.

Citation Information

Patent Citations

  • Manufacture of rare earth bonded magnet

    JP1994314605A

  • Dc brushless motor

    JP1996107641A