Laminate and method for manufacturing semiconductor device
The laminate with controlled absorbance and elastic modulus facilitates precise and debris-free laser transfer of semiconductor elements, addressing adhesive residue and positional accuracy issues in micro-LED manufacturing.
Patent Information
- Application Number
- JP2024045518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-09
AI Technical Summary
Existing laser transfer methods for semiconductor elements, particularly micro-LEDs, face issues with adhesive residue and debris generation, leading to potential device damage and inadequate positional accuracy during high-speed transfer.
A laminate is developed with specific optical and elastic properties, including a resin film with controlled absorbance and elastic modulus, allowing for precise transfer of semiconductor elements by laser irradiation without generating debris and ensuring high positional accuracy.
The laminate enables debris-free and highly accurate transfer of semiconductor elements, even when they fly over distances twice their height, improving manufacturing throughput and reducing defects.
Smart Images

Figure 2024139736000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate and a method for manufacturing a semiconductor device, more particularly to a laminate suitable for use when mounting a semiconductor element by laser transfer, and a method for manufacturing a semiconductor device using the laminate. [Background technology]
[0002] In general, elements to be incorporated in a semiconductor device are transferred and mounted on a circuit board or the like by a pick-and-place method using a flip-chip bonder or the like. In recent years, semiconductor devices have become more sophisticated and smaller in size, and accordingly, elements to be incorporated in the semiconductor device have become smaller and thinner, and the number of elements mounted in the semiconductor device has also increased. In recent years, displays in which light-emitting diodes (LEDs), a type of semiconductor element, and in particular micro LEDs, which are small LEDs with sides of about 10 to several μm, are arranged in each pixel, have attracted attention because of their high brightness, low power consumption, and high image quality. When manufacturing this micro LED display, the above mounting method takes too much time, so new methods are being considered.
[0003] As a method for mounting a large number of small semiconductor elements, a laser transfer technology has been proposed in which a laminate having an adhesive layer on a support substrate is prepared by mounting semiconductor elements on the surface of the adhesive layer opposite the support substrate side, and then a laser is irradiated from the support substrate side of the laminate to selectively transfer and mount the semiconductor elements to a counter substrate such as a circuit board located below the laminate at a certain distance from the laminate, so that the semiconductor elements are spaced apart at the desired interval. This method has the advantage that the semiconductor elements can be transferred quickly and over a wide area by irradiating the laser while moving the stage of the laminate and / or the counter substrate at high speed. Note that "transfer" refers to the transfer of the semiconductor elements from the original substrate to another substrate.
[0004] The laser transfer technology includes a transfer technology that uses a laminate with a thin adhesive layer having a thickness of 0.1 μm or more and 0.5 μm or less, and ablates and eliminates all the adhesive layer present between the support substrate and the semiconductor element by laser irradiation, thereby enabling the transfer of the semiconductor element to the opposing substrate while removing all the adhesive layer residue on the semiconductor element (for example, Patent Document 1). In addition, a technology is also included in which the adhesive layer located at the interface between the support substrate and the adhesive layer is ablated by laser irradiation, and the gas generated thereby accumulates at the interface between the adhesive layer and the support substrate to form a void (blister), and the element peels off and separates due to the change in shape of the adhesive layer, thereby transferring the semiconductor element to the opposing substrate (for example, Patent Document 2). In addition, a technology is also included in which a semiconductor element is transferred without any adhesive layer residue by applying an adhesive layer with controlled absorbance and adhesive strength (for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-188037 A [Patent Document 2] International Publication No. 2022 / 153745 [Patent Document 3] International Publication No. 2022 / 210155 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, in order to avoid residues on the adhesive layer on the surface of the semiconductor element, it is necessary to irradiate excessive laser light and remove all of the adhesive layer by ablation, which causes problems such as contamination of the opposing substrate due to scattering of the adhesive layer and damage to the semiconductor element (hereinafter, the residue of the adhesive layer on the surface of the semiconductor element may be referred to as glue residue, and the scattered residue of the adhesive layer may be referred to as debris). In Patent Documents 2 and 3, while it is possible to transfer semiconductor elements while suppressing the generation of residues and debris, it is insufficient to transfer semiconductor elements such as micro LEDs, which are fine and densely mounted, with high accuracy. Furthermore, in order to improve the throughput during laser transfer, it is necessary to irradiate the laser while moving the stage of the laminate and / or the opposing substrate at high speed, and it is required to leave an interval so that the laminate and the opposing substrate can move without contacting each other. At this time, in the case of a fine semiconductor element such as a micro LED, it is necessary to transfer with high positional accuracy even if the semiconductor element flies a distance of more than twice the height of the semiconductor element itself.
[0007] In view of the above circumstances, the present invention aims to provide a laminate capable of transferring fine, densely packed semiconductor elements with high positional accuracy without generating debris, even when the semiconductor elements fly a distance more than twice the height of the semiconductor elements, and a method for manufacturing semiconductor elements using the laminate. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention relates to the following 1 to 16. 1. A laminate in which a first substrate having optical transparency and a resin film are laminated in this order, the resin film has an absorbance of 0.4 or more and 5.0 or less at a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm; Furthermore, the resin film has an average elastic modulus at 25° C. of 0.06 GPa or more and 1.0 GPa or less at a depth of 500 to 1000 nm from the surface opposite to the surface in contact with the first substrate. 2. A laminate in which a first substrate having optical transparency, a resin film, and a semiconductor element are laminated in this order, the resin film has an absorbance of 0.4 or more and 5.0 or less at a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm; Furthermore, the resin film has an average elastic modulus at 25° C. of 0.06 GPa or more and 1.0 GPa or less at a depth of 500 to 1000 nm from the surface opposite to the surface in contact with the first substrate. 3. The laminate according to 1 or 2 above, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any one of wavelengths of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm and 1064 nm. 4. The laminate according to any one of 1 to 3 above, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any one of wavelengths of 248 nm, 266 nm and 355 nm. 5. The laminate according to any one of 1 to 4 above, wherein the resin film has a thickness of 8.0 μm or more and 23.0 μm or less. 6. The laminate according to any one of 1 to 5 above, wherein the resin film has an adhesive strength of 0.02 N / cm or more and 0.3 N / cm or less on the surface opposite to the surface in contact with the first substrate. 7. The laminate according to any one of 2 to 6 above, wherein the semiconductor element is embedded in the resin film to a depth of 0.1 μm or more and 2.0 μm or less. 8. The laminate described in any one of 1 to 7 above, wherein the average elastic modulus at 25°C at a depth of 20 to 40 nm from the surface of the resin film opposite to the surface in contact with the first substrate is 1.0 GPa or more and 7.0 GPa or less. 9. The laminate described in any one of 1 to 8 above, wherein the resin film contains one or more resins selected from the group consisting of polyimide having a repeating structural unit of the following formula (1), polyimide precursor having a repeating structural unit of the following formula (2), polybenzoxazole having a repeating structural unit of the following formula (3), polybenzoxazole precursor having a repeating structural unit of the following formula (4), and copolymers thereof.
[0009] [ka]
[0010] (In formulas (1) to (4), R 1 , R 3 , R 7 and R 9 each independently represents a tetravalent organic group having 6 to 40 carbon atoms; R 2 , R 4 , R 6 and R 8 R each independently represents a divalent organic group having 2 to 40 carbon atoms. 5 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. 10. The laminate according to 9 above, wherein the resin has at least one of a dimethylsiloxane structure represented by the following formula (5) and a diphenylsiloxane structure represented by the following formula (6).
[0011] [ka]
[0012] (In formula (5) and formula (6), l and m each independently represent an integer of 4 to 40.) 11. The resin contains a polyimide having a repeating structural unit of the formula (1), The polyimide having the repeating structural unit of the formula (1) contains 20 mol % to 100 mol % of acid dianhydride residues represented by the following formula (7) based on 100 mol % of all acid dianhydride residues of the polyimide having the repeating structural unit of the formula (1), and 11. The laminate according to item 9 or 10, wherein the diamine residues represented by the following formula (8) account for 60 mol % or more and 100 mol % or less of all diamine residues in the polyimide having the repeating structural unit of the formula (1):
[0013] [ka]
[0014] In formula (7), * represents a bond, X represents a single bond, -CH2-, -SO2- or -CO-, in formula (8), * represents a bond, n represents an integer of 4 to 40, R 10 and R 11 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms.) 12. The laminate according to any one of 1 to 11 above, wherein the resin film has a 1% weight loss temperature of 300° C. or higher. 13. The laminate according to any one of 1 to 12 above, wherein the resin film contains at least one of an ultraviolet absorber and a dye. 14. A method for producing a semiconductor device using the laminate according to any one of 2 to 13 above, placing a second substrate opposite to the surface of the stack on which the semiconductor elements are stacked; A method for manufacturing a semiconductor device, comprising the step of irradiating the laminate with laser light from the first substrate side to transfer the semiconductor element to the second substrate. 15. The method for producing a semiconductor device according to claim 14, wherein the laser light has a wavelength of any one of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm and 1064 nm. 16. The method for producing a semiconductor device according to claim 14 or 15, wherein the second substrate is a circuit substrate. Effect of the Invention
[0015] The laminate of the present invention makes it possible to transfer fine, densely mounted semiconductor elements with high positional accuracy without generating debris, even if the semiconductor elements fly a distance twice or more their height. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram illustrating a method for producing a second laminate. [Diagram 2] FIG. 2 is a diagram illustrating a method for producing a second laminate using a temporary adhesive. [Diagram 3]FIG. 3 is a diagram illustrating a method for producing a second laminate using laser lift-off. [Figure 4] FIG. 4 is a diagram illustrating the embedding depth of a semiconductor element in a resin film. [Diagram 5] FIG. 5 is a diagram illustrating another method for producing the second laminate using a semiconductor substrate. [Figure 6] FIG. 6 is a diagram illustrating a step of opposing the semiconductor element surface of the second laminate to a second substrate in the method for manufacturing a semiconductor device. [Figure 7A] FIG. 7A is a diagram illustrating a step of transferring a semiconductor element to a second substrate by irradiating with laser light. [Figure 7B] FIG. 7B is a diagram illustrating a step of transferring a semiconductor element to a second substrate by irradiating with laser light. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The laminate according to one embodiment of the present invention is a laminate in which a first substrate having optical transparency and a resin film are laminated in order, and the resin film has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm, and further, the average elastic modulus at 25 ° C. in a region of 500 to 1000 nm deep from the surface of the resin film opposite to the surface contacting the first substrate is 0.06 GPa or more and 1.0 GPa or less. The laminate of this aspect is hereinafter referred to as the first laminate. The first laminate according to an embodiment of the present invention and the second laminate according to an embodiment of the present invention described later may be collectively referred to simply as the laminate according to an embodiment of the present invention.
[0018] The configuration of the first laminate according to an embodiment of the present invention will be described below. The first substrate having optical transparency refers to a substrate having an absorbance of 0.1 or less at any wavelength of at least 200 to 1100 nm. The absorbance in any wavelength of 200 to 1100 nm being within a specific range means, for example, that when the absorbance is measured in the wavelength range of 200 to 1100 nm, the absorbance in at least one value of the wavelength is within a specific range for the absorbance in the case where the wavelength is an integer value. Examples of substrates having such absorbance include inorganic substrates such as quartz, sapphire, alkali glass, non-alkali glass, and borosilicate glass. The thickness of the substrate can be selected within a range that does not impair the above-mentioned absorbance, and is preferably, for example, 0.1 mm to 5.0 mm. That is, from the viewpoint of ease of handling of the substrate, the thickness of the substrate is more preferably 0.3 mm or more. On the other hand, from the viewpoint of ease of availability and versatility, the thickness of the substrate is more preferably 2.0 mm or less. It is to be noted that the first substrate is preferably a substrate through which the laser light used for irradiating the laser light from the side of the first substrate described later can be transmitted.
[0019] For the first substrate having optical transparency, an organic substrate such as PET, aramid, polyester, polypropylene, or cycloolefin may be used. When an organic substrate is used, the thickness of the substrate can be selected within a range that does not impair the absorbance, and is preferably 0.05 mm to 3.0 mm, for example. From the viewpoint of ease of handling of the substrate, the thickness of the substrate is more preferably 0.1 mm or more. On the other hand, the thickness of the substrate is more preferably 1.0 mm or less, since light scattering during laser irradiation can be suppressed.
[0020] Next, the resin film will be described. The resin film is a film containing at least a resin, and has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm. When the absorbance is 0.4 or more, when a semiconductor element is transferred to an opposing substrate by irradiating a laser beam from a first substrate side having optical transparency to the resin film side, the irradiated laser beam is absorbed intensively by the resin film located at the interface with the first substrate, and ablation occurs efficiently, and accordingly, decomposition gas of the resin film is rapidly generated at the interface between the first substrate and the resin film, and a gap is generated at the interface between the first substrate and the resin film. The kinetic energy of the resin film generated by the momentary increase in the internal pressure of the gap is efficiently propagated to the semiconductor element, and the transfer can be performed with high accuracy. Since the resin film can absorb the laser beam intensively on the interface side with the first substrate, and the kinetic energy of the resin film is easily increased, the transfer can be performed with a laser beam of low energy density, and the processing margin is expanded, so that the absorbance is more preferably 0.6 or more. From the viewpoint of material design, the absorbance is preferably 4.5 or less, and since a versatile resin can be used, the absorbance is more preferably 4.0 or less.
[0021] Examples of the resin contained in the resin film include, but are not limited to, polyamide, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, urethane resin, novolac resin, polyhydroxystyrene, polyester resin, acrylic resin, aramid resin, polysiloxane, and polyimidesiloxane, which have absorption at any wavelength of 200 to 1100 nm.
[0022] These resins preferably have a conjugated structure in the structure. By the resin having a conjugated structure, the absorbance of 200 to 1100 nm converted into a film thickness of 1.0 μm can be adjusted to a range of 0.4 or more and 5.0 or less. Examples of structures having a conjugated structure include aromatic structures, and among them, structures such as biphenyl, imide, benzoxazole, and benzophenone are preferable. The above absorbance can be achieved by making 60 mol % or more of the monomer residues having a conjugated structure when all the monomer residues constituting the resin are taken as 100 mol %. These resins may be contained alone or in a plurality in the resin film.
[0023] The above absorbance can also be achieved by adding additives such as ultraviolet absorbers, dyes, pigments, etc. to the resin film. It is preferable that the resin film contains at least one of an ultraviolet absorber and a dye, since this can increase the absorbance of the resin film and enable efficient ablation. Examples of ultraviolet absorbers and dyes contained in the resin film include ultraviolet absorbers such as Tinuvin PS, Tinuvin 99-2, Tinuvin 326, Tinuvin 328, Tinuvin 384-2, Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479, Tinuvin 900, Tinuvin 928, Tinuvin 1130 (all trade names, manufactured by BASF), DAINSORB T-0, DAINSORB T-7, DAINSORB T-31, DAINSORB T-52, DAINSORB T-53, DAINSORB T-84, DAINSORB P-6, and DAINSORB P-7 (all trade names, manufactured by Daiwa Chemical Industry Co., Ltd.); Examples of the dyes, dyes and pigments include Red 168, Solvent Red 207, Solvent Red 52, Solvent Red 179, Solvent Blue 36, Solvent Blue 94, Solvent Blue 63, Solvent Blue 104, Solvent Blue 97, Solvent Green 20, Solvent Violet 13, Solvent Violet 36 (all trade names, manufactured by Tokyo Chemical Industry Co., Ltd.), carbon black, perylene black, cyanine black, aniline black, etc. These may be contained alone or in multiple types in the resin film.
[0024] Among them, the resin film preferably contains one or more compounds selected from the group consisting of benzotriazole-based compounds, triazine-based compounds, benzophenone-based compounds, and benzoate-based compounds. These compounds have high heat resistance and are therefore unlikely to decompose when the resin film is heated and cured. In addition, since they have absorption for wavelengths in the range of 200 to 400 nm, they can efficiently absorb laser light when laser transfer is performed using a laser light with a wavelength in the range of 200 to 400 nm, and can transfer with high accuracy even with laser light with a relatively low energy density.
[0025] The content of the additive to bring the absorbance into the above range is preferably 0.1 parts by mass or more per 100 parts by mass of the resin film, and from the viewpoint of stability in the varnish state before forming the laminate, it is preferably 50 parts by mass or less.
[0026] In the embodiment of the present invention, the wavelength at which the resin film satisfies the above absorbance is preferably any one or more of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm, and 1064 nm. The wavelength at which the resin film satisfies the above absorbance is more preferably any one or more of 248 nm, 266 nm, and 355 nm.
[0027] The resin film preferably has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any one or more wavelengths of 248 nm, 266 nm, 308 nm, 532 nm, and 1064 nm, and more preferably has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any one or more wavelengths of 248 nm, 266 nm, and 355 nm. By satisfying the above-mentioned range of absorbance of the resin film at these wavelengths, laser light is efficiently absorbed, so that when laser transfer is performed using this laminate, even if a laser light with a relatively low energy density is applied, high-precision transfer can be performed.
[0028] In the laminate according to the embodiment of the present invention, the average modulus of elasticity at 25°C in a region of 500 to 1000 nm deep from the surface of the resin film opposite to the surface in contact with the first substrate (hereinafter referred to as the bulk modulus of elasticity of the resin film) is 0.06 GPa or more and 1.0 GPa or less. The bulk modulus of elasticity is a physical property that serves as an index of whether the kinetic energy of the resin film generated by the ablation of the resin film is efficiently transmitted in the transfer direction during laser transfer using this laminate. By having a bulk modulus of elasticity of 0.06 GPa or more, the kinetic energy of the resin film generated by the ablation of the resin film is prevented from diffusing and dissipating within the resin film during laser transfer using this laminate, and energy is efficiently transmitted in the transfer direction of the semiconductor element, and in particular, laser transfer can be performed with high accuracy even when the distance between the semiconductor element and the opposing substrate is more than twice the height of the semiconductor element. Since energy can be transmitted more efficiently and positional accuracy can be increased, the bulk modulus is more preferably 0.10 GPa or more, and even more preferably 0.20 GPa or more. In addition, since the elastic modulus is 1.0 GPa or less, even if a laser beam with a low energy density is applied during laser transfer using the laminate, the energy generated by the ablation of the resin film is sufficiently transmitted, and transfer can be performed with high positional accuracy. Since the positional accuracy can be further improved, the bulk elastic modulus is more preferably 0.80 GPa or less, and even more preferably 0.60 GPa or less.
[0029] The bulk modulus can be measured by nanoindentation measurement. In the case of the second laminate, the semiconductor element in the range required for the elastic modulus measurement is physically removed to expose the resin film surface, and the measurement can be performed. The semiconductor element can be removed by directly removing it with tweezers, or by superposing a substrate or film with strong adhesive strength such as dicing tape on the upper surface of the semiconductor element and peeling it off. The bulk modulus is measured by a Berkovich indenter (triangular pyramidal diamond indenter) at 25°C ± 2°C in the atmosphere, by pressing the resin film surface vertically into the first substrate side having optical transparency, and then removing the load, in an indentation load / unloading test. At this time, the measurement is performed at a measurement frequency of 100 Hz using a continuous stiffness measurement method. From the obtained load-indentation depth diagram, the elastic modulus is calculated from the average value of the values at a depth of 500 to 1000 nm from the resin film surface.
[0030] In order to set the bulk modulus of the resin film within the above range, it is preferable that the resin film contains a crosslinking agent. By adding the crosslinking agent, the structure in the resin film is partially crosslinked, thereby adjusting the bulk modulus of the resin film.
[0031] The type of crosslinking agent is not limited as long as it is a compound that undergoes a crosslinking reaction when heated at 100°C or more and 300°C or less, and examples thereof include compounds having functional groups such as epoxy groups, oxetanyl groups, alkoxymethyl groups, or methylol groups. Compounds having two or more functional groups per molecule are preferred, more preferably three or more, and even more preferably five or more. By having two or more functional groups per molecule, the crosslinking density is increased, and the bulk elastic modulus of the resin film is easily adjusted to the above range. Furthermore, it is preferable that the functional group equivalent is 50g / eq. or more and 150g / eq. or less, since it is easy to improve the crosslinking density and adjust the bulk elastic modulus of the resin film to the above range. In addition, the compound having one or more aromatic rings per molecule is preferred. By having one or more aromatic rings per molecule, the crosslinking points become rigid, and it is easy to adjust the bulk elastic modulus of the resin film to the above range, which is preferred. From the viewpoint of obtaining the above-mentioned effects, the compound having two or more aromatic rings per molecule is more preferable.
[0032] Examples of the crosslinking agent include compounds having an alkoxymethyl group or a methylol group, such as DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DMLBisOCHP-Z, DML-BPC, DML-BisOC-P, DMOM-PC, DMOM-PTBP, DM Examples of such compounds include OM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, and HMOM-TPHAP (all trade names, manufactured by Honshu Chemical Industry Co., Ltd.), and "NIKALAC (registered trademark)" MX-290, NIKALAC MX-280, NIKALAC MX-270, NIKALAC MX-279, NIKALAC MW-100LM, and NIKALAC MX-750LM (all trade names, manufactured by Sanwa Chemical Co., Ltd.).
[0033] It is also preferable to include a compound having an epoxy group as a crosslinking agent. Examples of the compound having an epoxy group include, but are not limited to, bisphenol A type epoxy resin and bisphenol F type epoxy resin. Specific examples include Epicron 850-S, Epicron HP-4032, Epicron HP-7200, Epicron HP-820, Epicron HP-4700, Epicron EXA-4710, Epicron HP-4770, Epicron EXA-859CRP, Epicron EXA-1514, Epicron EXA-4880, Epicron EXA-4850-150, Epicron EXA-4850-1000, Epicron EXA-4816, Epicron EXA-4822 (all trade names, manufactured by DIC Corporation), and Rikaresin. Examples include BEO-60E (hereinafter referred to as product name, manufactured by New Japan Chemical Co., Ltd.), EP-4003S, EP-4000S (all product names, manufactured by Adeka Corporation), JER871, JER872, YX-4000, YX-4000H (all product names, manufactured by Mitsubishi Chemical Corporation), Celloxide 2021P (all product names, manufactured by Daicel Corporation), Showfree BATG (all product names, manufactured by Resonac Corporation), Denacol EX-201-IM (all product names, manufactured by Nagase ChemteX Corporation), and TEPIC-VL (all product names, manufactured by Nissan Chemical Co., Ltd.).
[0034] It is also preferable to have a crosslinking agent having an oxetanyl group, and specific examples include OXT-121, OXT-221, OX-SQ-H, OXT-191, PNOX-1009, RSOX (all trade names, manufactured by Toagosei Co., Ltd.), "Etanacol (registered trademark)" OXBP, and "Etanacol" OXTP (all trade names, manufactured by UBE Corporation).
[0035] The resin film may contain two or more kinds of crosslinking agents, and the bulk modulus can be adjusted to a preferred range by preferably containing 0.1 parts by mass or more in 100 parts by mass of the resin film. The crosslinking agent is preferably contained in an amount of 30 parts by mass or less in 100 parts by mass of the resin film. Within this range, the resin film maintains a certain degree of flexibility, and the kinetic energy of the resin film caused by the ablation of the resin film during laser irradiation is sufficiently transmitted to the semiconductor element, while the resin film does not break when the semiconductor element is transferred. In addition, from the viewpoint of storage stability in the state of the varnish before forming the laminate, the content of the crosslinking agent is more preferably 20 parts by mass or less.
[0036] In addition, a curing accelerator may be included for the purpose of promoting curing by a crosslinking agent. Examples of the curing accelerator include imidazoles, tertiary amines or their salts, and organic boron salt compounds, among which imidazoles are preferred. Specific examples of imidazoles include imidazole, 2-methylimidazole, 2-ethylimidazole, 2-isopropylimidazole, 2-n-propylimidazole, 2-undecyl-1H-imidazole, 2-heptadecyl-1H-imidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-1H-imidazole, 4-methyl-2-phenyl-1H-imidazole, 2-phenyl-4-methylimidazole, 1-beta-imidazole, 2 ... 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazolium trimellitate, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-di Amino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2- Examples of the compound include methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 1-cyanoethyl-2-phenyl-4,5-di(2-cyanoethoxy)methylimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 1-benzyl-2-phenylimidazole hydrochloride, and 1-benzyl-2-phenylimidazolium trimellitate.Preferable examples of commercially available imidazoles include Curesol C17Z, Curesol 2MZ, Curesol 1B2MZ, Curesol 2E4MZ, Curesol 2E4MZ-CN, Curesol 2MZ-AZINE, and Curesol 2MZ-OK (all trade names, manufactured by Shikoku Chemical Industry Co., Ltd.).
[0037] The content of the curing accelerator in the resin film is preferably 0.1 parts by mass or more and 5.0 parts by mass or less with respect to 100 parts by mass of the resin film. Within this range, it is easy to obtain a sufficient crosslinking promotion effect. In addition, from the viewpoint of maintaining the stability of the varnish in a state before forming the laminate, the content of the curing accelerator in the resin film is more preferably 0.5 to 2.0 parts by mass.
[0038] A laminate according to one embodiment of the present invention is a laminate in which a first substrate having optical transparency, a resin film, and a semiconductor element are laminated in this order, the resin film has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any wavelength of 200 to 1100 nm, and further, the resin film has an average elastic modulus of 0.06 GPa or more and 1.0 GPa or less at 25° C. in a region of a depth of 500 to 1000 nm from the surface of the resin film opposite to the surface in contact with the first substrate. The laminate of this embodiment is called a second laminate.
[0039] The description of the first substrate having optical transparency and the resin film in the second laminate is the same as that in the first laminate.
[0040] Next, a semiconductor device according to an embodiment of the present invention will be described. The semiconductor element in the embodiment of the present invention includes semiconductors such as GaN, AlN, InN, InP, GaAs, Si, and SiC that are made into an element. These semiconductor elements include those in which different types of semiconductors are further stacked, and those in which electrode materials, sapphire substrates, glass substrates, wiring, etc. are stacked. The size of the semiconductor element is preferably 5 μm or more and 5.0 mm or less on one side. More preferably, it is 3.0 mm or less. This allows the laser to be focused and irradiated with a small spot diameter, making it possible to transfer with high positional accuracy. For example, the size of a particularly fine micro LED is exemplified as being 0.2 μm or more and 100 μm or less on one side.
[0041] The number of semiconductor elements mounted on the second laminate according to the embodiment of the present invention is 5 / cm per unit area. 2 More preferably, 50 / cm 2 That's it. By increasing the number of semiconductor elements beyond this, the effect of improving throughput by using laser transfer becomes greater. Also, since the laser can be precisely irradiated onto each semiconductor element, it is possible to achieve a throughput of 500,000 elements / cm. 2 Preferably less than 100,000 particles / cm, more preferably 100,000 particles / cm 2 The following is the result.
[0042] The stacking order of the second laminate according to the embodiment of the present invention may be a first substrate having optical transparency, a resin film, and a semiconductor element, with another layer being present between them. However, the semiconductor element is formed in contact with the resin film, and the first substrate having optical transparency and the semiconductor element are located on the outermost surface of the second laminate. That is, the first substrate is located on one outermost surface of the second laminate, and the semiconductor element is located on the other outermost surface of the second laminate.
[0043] In the laminate according to the embodiment of the present invention, the thickness of the resin film is preferably 8.0 μm or more and 23.0 μm or less. By being 8.0 μm or more, the curvature of the resin film surface deformed by the gap between the resin film and the first substrate interface generated when irradiated with laser light is reduced, suppressing the tilt of the emission angle of the semiconductor element, and improving the positional accuracy. In addition, if it is 23.0 μm or less, the kinetic energy of the resin film generated by ablation of the resin film by irradiation with laser light from the first substrate side having optical transparency is efficiently transmitted to the semiconductor element, and as a result, the semiconductor element can be transferred with higher accuracy. From the viewpoint of obtaining the above effect, the thickness of the resin film is more preferably 9.0 μm or more and 21.0 μm or less, and even more preferably 10.0 μm or more and 18.0 μm or less.
[0044] The resin film in the laminate according to the embodiment of the present invention preferably has an adhesive strength of 0.02 N / cm or more and 0.3 N / cm or less on the surface of the resin film opposite to the surface where the resin film contacts the first substrate. The adhesive strength mentioned here indicates a value obtained from a 90° peel test of a Kapton film attached to the surface of the resin film. In the case of the second laminate, the hardness can be measured by physically removing the semiconductor element in the range required for hardness measurement from the second laminate to expose the surface of the resin film. A Kapton film cut to 1 cm x 9 cm is pressed onto the surface of the resin film with a vacuum laminator under conditions of 0.6 MPa and 35°C, and the pressed Kapton tape is peeled off at a constant speed of 2 mm / sec in a direction perpendicular to the resin film with a tensile tester at 25°C.
[0045] When the adhesive strength is 0.02 N / cm or more, the semiconductor element can be stably held when stacked on the resin film. When the adhesive strength is 0.3 N / cm or less, the force acting on the semiconductor element to pull it back toward the resin film in the opposite direction to the transfer direction when the semiconductor chip is separated from the resin film surface is reduced, and the inclination of the semiconductor element when it is separated from the resin film is reduced, improving the positional accuracy. The adhesive strength is more preferably 0.2 N / cm or less. In order to set the adhesive strength of the resin film within the above range, it is preferable that the resin film contains a flexible component or a bent component. By introducing a flexible component or a bent component, the resin can be given flexibility and adhesive strength. Examples of components that give flexibility and bendability include a flexible structure derived from an aliphatic or silane such as an alkylene group, a siloxane, or the like, a flexible structure derived from an ether group such as an alkylene glycol or a biphenyl ether, an alicyclic structure, and a bent structure such as an olefin. When all monomer residues constituting the resin contained in the resin film are taken as 100 mol%, the adhesive strength can be made 0.02 N / cm or more by containing 20 mol% or more of monomer residues having such a structure that gives flexibility. In addition, the adhesive strength can be made 0.3 N / cm or less by setting the monomer residue content to 70 mol% or less.
[0046] In the laminate according to the embodiment of the present invention, the average elastic modulus at 25°C in a region of 20 to 40 nm deep from the surface of the resin film opposite to the surface in contact with the first substrate (hereinafter referred to as the surface elastic modulus of the resin film) is preferably 1.0 GPa or more and 7.0 GPa or less. The surface elastic modulus is a physical property that serves as an index of the embedding depth of the semiconductor element in the resin film in this laminate. By having a surface elastic modulus of 1.0 GPa or more, the embedding depth of the semiconductor element in the resin film can be reduced, and the semiconductor element can be easily peeled off from the resin film during laser transfer, so that laser transfer can be performed with high accuracy, especially even when the distance between the semiconductor element and the opposing substrate is more than twice the height of the semiconductor element. In addition, by having a surface elastic modulus of 7.0 GPa or less, the semiconductor element can be easily held on the resin film, improving handleability.
[0047] The surface modulus can be measured by nanoindentation measurement, similar to the bulk modulus. In the case of the second laminate, the semiconductor element in the range required for the elastic modulus measurement is physically removed to expose the resin film surface, and the measurement can be performed. The semiconductor element can be removed by directly removing it with tweezers, or by superposing a substrate or film with strong adhesive strength, such as dicing tape, on the upper surface of the semiconductor element and peeling it off. The surface modulus is measured by a Berkovich indenter (triangular pyramidal diamond indenter) at 25°C ± 2°C in air, by pressing the resin film surface vertically into the first substrate side having optical transparency, and then removing the load, in an indentation load / unloading test. At this time, the measurement is performed at a measurement frequency of 100 Hz using a continuous stiffness measurement method. From the obtained load-indentation depth diagram, the elastic modulus is calculated from the average value of the value at a depth of 20 to 40 nm from the resin film surface.
[0048] In the laminate according to the embodiment of the present invention, the embedment depth of the semiconductor element in the resin film is preferably 0.1 μm or more and 2.0 μm or less. When the embedment depth is 0.1 μm or more, the adhesive state between the resin film and the semiconductor element is easily stabilized, and the handling property is improved. When the embedment depth is 2.0 μm or less, the semiconductor element can be easily peeled off from the resin film during laser transfer, and the positional accuracy of the laser transfer is improved. The embedment depth is more preferably 1.5 μm or less, and further preferably 1.0 μm or less. The embedment depth of the semiconductor element in the resin film corresponds to the height between the top and bottom of the contact surface between the semiconductor element and the resin film, when the side where the semiconductor element and the resin film are in contact is taken as the bottom and the side opposite to the contact surface between the semiconductor element and the resin film is taken as the top. More specifically, the embedment depth in the resin film is determined as the height between the top (H a ) and the bottom (H b ) between the ab ) Note that, if one semiconductor element has multiple contact surfaces with the resin film, the height between the top and bottom of each contact surface is measured, and the largest value is used. The embedding depth can be measured from an image obtained by cutting out a cross section of the laminate using focused ion beam (FIB) processing and observing it with a scanning electron microscope (SEM).
[0049] In order to set the embedding depth of the semiconductor element in the resin film within the above-mentioned preferred range, the surface elastic modulus of the resin film is preferably 1.0 GPa or more and 7.0 GPa or less. When the surface elastic modulus of the resin film is 1.0 GPa or more, the reaction force against the external force applied from the semiconductor element side toward the resin film side when stacking the semiconductor element on the resin film, and / or the elastic force that the resin film surface tries to return to the state before stacking the semiconductor element after stacking the semiconductor element on the resin film is applied strongly, and the semiconductor element can be prevented from being deeply embedded in the resin film under the recommended stacking conditions. On the other hand, when the surface elastic modulus of the resin film is 7.0 GPa or less, the stacked semiconductor element is less likely to come off the resin film surface, improving the handling property. In order to set the embedding depth within the above-mentioned preferred range, it is also possible to adjust the lamination conditions when laminating the semiconductor element on the resin film, as described later.
[0050] In the laminate according to the embodiment of the present invention, the resin film preferably contains one or more resins selected from the group consisting of polyimide having a repeating structural unit of formula (1), polyimide precursor having a repeating structural unit of formula (2), polybenzoxazole having a repeating structural unit of formula (3), polybenzoxazole precursor having a repeating structural unit of formula (4), and copolymers thereof. The repeating structural unit of formula (1) is also referred to as the structure of formula (1). The same applies to formulas (2) and onward.
[0051] [ka]
[0052] In formulas (1) to (4), R 1 , R 3 , R 7 and R 9 each independently represents a tetravalent organic group having 6 to 40 carbon atoms; R 2 , R 4 , R 6 and R 8R each independently represents a divalent organic group having 2 to 40 carbon atoms. 5 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
[0053] Polyimide and polybenzoxazole are resins having a cyclic structure of an imide ring or an oxazole ring in the main chain structure. In addition, their precursors, polyimide precursors and polybenzoxazole precursors, are resins that form an imide ring or a benzoxazole ring structure by dehydration ring closure. It is preferable that the resin contains 10 to 100,000 repeating structural units represented by formulas (1) to (4). Within this range, the resin film can be applied with a preferred film thickness.
[0054] Polyimides can be obtained by reacting tetracarboxylic acids, corresponding tetracarboxylic dianhydrides, tetracarboxylic diester dichlorides, etc. with diamines, corresponding diisocyanate compounds, trimethylsilylated diamines, etc., and have tetracarboxylic acid residues and diamine residues. For example, polyamic acid, which is one of the polyimide precursors obtained by reacting tetracarboxylic dianhydrides with diamines, can be obtained by dehydrating and ring-closing the polyimide by heat treatment. During this heat treatment, a solvent that forms an azeotrope with water, such as m-xylene, can also be added. Alternatively, polyimides can be obtained by adding a dehydrating condensing agent such as a carboxylic anhydride or dicyclohexylcarbodiimide, or a ring-closing catalyst such as a base such as triethylamine, and dehydrating and ring-closing the polyimide by chemical heat treatment. Alternatively, polyimides can be obtained by adding a weakly acidic carboxylic acid compound and dehydrating and ring-closing the polyimide by heat treatment at a low temperature of 100°C or less.
[0055] Polybenzoxazole can be obtained by reacting a bisaminophenol compound with a dicarboxylic acid, a corresponding dicarboxylic acid chloride, a dicarboxylic acid active ester, or the like, and has a dicarboxylic acid residue and a bisaminophenol residue. For example, it can be obtained by dehydrating and ring-closing polyhydroxyamide, which is one of the polybenzoxazole precursors obtained by reacting a bisaminophenol compound with a dicarboxylic acid, through a heat treatment. Alternatively, it can be obtained by adding phosphoric anhydride, a base, a carbodiimide compound, or the like, and dehydrating and ring-closing through a chemical treatment.
[0056] In formula (1) and formula (2), R 1 and R 3 (COOR 5 R 2 preferably represents a tetracarboxylic acid residue. 1 or R 3 (COOR 5Examples of the tetracarboxylic acid residue constituting the tetracarboxylic acid residue of 2 include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, Examples of the tetracarboxylic acid residue include aromatic tetracarboxylic acid residues derived from benzene, bis(3,4-dicarboxyphenyl)methane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, and the like, and aliphatic tetracarboxylic acid residues derived from butanetetracarboxylic acid, 1,2,3,4-cyclopentanetetracarboxylic acid, and the like. In addition, two or more of these tetracarboxylic acid residues may be contained. As the tetracarboxylic acid residue, those having aromaticity are preferable from the viewpoint of making the absorbance suitable.
[0057] In formula (1) and formula (2), R 2 and R 4 R preferably represents a diamine residue. 2 and R 4Examples of the diamine residue constituting the above include hydroxyl group-containing diamine residues derived from 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)methane, bis(3-amino-4-hydroxyphenyl)ether, 3,3'-diamino-4,4'-biphenol, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, and the like. Sulfonic acid group-containing diamine residues derived from 4,4'-diaminodiphenyl ether, etc., thiol group-containing diamine residues derived from dimercaptophenylenediamine, etc., 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl methane, 4,4'-diaminodiphenyl methane, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 1,4-bis(4-aminopheno )benzene, benzidine, m-phenylenediamine, p-phenylenediamine, 1,5-naphthalenediamine, 2,6-naphthalenediamine, bis(4-aminophenoxyphenyl)sulfone, bis(3-aminophenoxyphenyl)sulfone, bis(4-aminophenoxy)biphenyl, bis{4-(4-aminophenoxy)phenyl}ether, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-diethyl-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-diethyl-4,4 Examples of the aromatic diamine residues include aromatic diamine residues derived from 2,2',3,3'-diaminobiphenyl, 2,2',3,3'-tetramethyl-4,4'-diaminobiphenyl, 3,3',4,4'-tetramethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, and the like; compounds in which some of the hydrogen atoms in these aromatic rings are substituted with alkyl or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, or the like; and alicyclic diamine residues derived from cyclohexyldiamine, methylenebiscyclohexylamine, and the like.Two or more of these diamine residues may be contained in combination.
[0058] In formula (2), R 5 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. Examples of the organic group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, a cyclohexyl group, an octyl group, a dodecyl group, and a phenyl group. In view of the ease of obtaining raw materials for polymerization, R 5 is preferably a methyl group or an ethyl group.
[0059] In formula (3) and formula (4), R 6 and R 8 preferably represents a dicarboxylic acid residue, a tricarboxylic acid residue or a tetracarboxylic acid residue.
[0060] Examples of dicarboxylic acid residues include residues derived from terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, triphenyl dicarboxylic acid, etc., and examples of tricarboxylic acid residues include residues derived from trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, biphenyl tricarboxylic acid, etc. Examples of tetracarboxylic acid residues include R 1 and R 3 These are the same as the residues given as examples of 1. Two or more of these may be used.
[0061] In formula (3) and formula (4), R 7 and R 9(OH)2 preferably represents a bisaminophenol derivative residue. Specific examples of the bisaminophenol derivative residue include residues derived from 3,3'-diamino-4,4'-dihydroxybiphenyl, 4,4'-diamino-3,3'-dihydroxybiphenyl, bis(3-amino-4-hydroxyphenyl)propane, bis(4-amino-3-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)sulfone, bis(4-amino-3-hydroxyphenyl)sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, etc., but are not limited thereto. These compounds may be contained alone or in combination of two or more kinds.
[0062] In addition, it is preferable to cap the terminals of the resins represented by formulas (1) to (4) with a monoamine, an acid anhydride, an acid chloride, or a monocarboxylic acid having an acidic group, since this can improve the stability of the resin.
[0063] Preferred examples of such monoamines include 2-aminophenol, 3-aminophenol, 4-aminophenol, etc. Two or more of these may be used.
[0064] Preferable examples of such acid anhydrides, acid chlorides, and monocarboxylic acids include known compounds such as phthalic anhydride, maleic anhydride, nadic anhydride, etc. Two or more of these compounds may be used.
[0065] The above-mentioned resin preferably has at least one of a dimethylsiloxane structure represented by formula (5) and a diphenylsiloxane structure represented by formula (6).
[0066] [ka]
[0067] In formula (5) and formula (6), l and m each independently represent an integer of 4 to 40.
[0068] It is preferable that the resin structure has at least one of the structure shown in formula (5) and the structure shown in formula (6), since this can impart appropriate ranges of flexibility, elastic modulus, and adhesive strength to the resin film. Specific examples of such structures include α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiethylsiloxane, α,ω-bis(3-aminopropyl)polydipropylsiloxane, α,ω-bis(3-aminopropyl)polydibutylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, α,ω-bis(2-aminoethyl)polydimethylsiloxane, and α,ω-bis(2-aminoethyl) Examples of the residue include those derived from polydiphenoxysiloxane, α,ω-bis(4-aminobutyl)polydimethylsiloxane, α,ω-bis(4-aminobutyl)polydiphenoxysiloxane, α,ω-bis(5-aminopentyl)polydimethylsiloxane, α,ω-bis(5-aminopentyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, α,ω-bis(4-aminophenyl)polydiphenoxysiloxane, etc. The residue of the siloxane diamine may be one kind or may contain two or more kinds.
[0069] Furthermore, it is preferable that the resin contains a polyimide having a structure of formula (1), and the polyimide having the structure of formula (1) contains 20 mol% to 100 mol% of acid dianhydride residues represented by formula (7) in 100 mol% of all acid dianhydride residues of the polyimide having the structure of formula (1), and contains 60 mol% to 100 mol% of diamine residues represented by formula (8) in 100 mol% of all diamine residues of the polyimide having the structure of formula (1). By containing such a structure, the resin film can have a preferable bulk elastic modulus for efficiently transmitting the kinetic energy of the resin film to the semiconductor element while maintaining flexibility that allows the shape of the resin film to follow voids generated by ablation of the resin film at the interface between the first substrate and the resin film during laser transfer. Furthermore, by including such a structure in the resin, the embedment depth of the semiconductor element in the resin film is reduced, and the semiconductor element is easily peeled off from the resin film during laser transfer, and the resin film can have a preferable surface elasticity for high-precision laser transfer, especially when the distance between the semiconductor element and the opposing substrate is more than twice the height of the semiconductor element. Since the bulk elasticity can be adjusted to be higher, it is more preferable that the acid dianhydride residue represented by formula (7) is contained in an amount of 30 mol% to 100 mol% out of 100 mol% of all acid dianhydride residues. Furthermore, since the surface elasticity can be adjusted to be higher, it is more preferable that the acid dianhydride residue represented by formula (7) is contained in an amount of 50 mol% to 100 mol% out of 100 mol% of all acid dianhydride residues. Furthermore, since the resin film has sufficient adhesion to hold the semiconductor element, it is more preferable that the diamine residue represented by formula (8) is contained in an amount of 70 mol% to 100 mol% out of 100 mol% of all diamine residues.
[0070] [ka]
[0071] In formula (7), * represents a bond, and X represents a single bond, -CH2-, -SO2- or -CO-. In formula (8), * represents a bond, n represents an integer of 4 to 40, and R 10 and R11 each independently represents an alkylene group having 1 to 30 carbon atoms or a phenylene group.
[0072] In the laminate according to the embodiment of the present invention, the 1% weight loss temperature of the resin film is preferably 300°C or higher. Here, the 1% weight loss temperature of the resin film represents a value obtained from a measurement using a sample obtained by heating the resin film at 250°C for 30 minutes. Even if the resin film has already been heat-treated (heat-treated to harden the resin film), the sample can be further heat-treated at 250°C for 30 minutes and the 1% weight loss temperature of the resin film can be measured in the same manner. By having a 1% weight loss temperature of 300°C or higher, the resin film in the surrounding non-laser-irradiated area is damaged by heat generated by ablation of the resin film located at the interface with the first substrate during laser light irradiation, and the range in which voids are generated can be prevented from spreading, and as a result, the positional accuracy of the adjacent semiconductor element can be prevented from being reduced due to the voids when the adjacent semiconductor element is laser-transferred.
[0073] In order to make the 1% weight loss temperature 300°C or higher, it is preferable that the resin film contains a component with high thermal stability. Specific examples of components with high thermal stability include rigid components such as aromatic rings, siloxanes with relatively high thermal stability among flexible structures, and combinations thereof. When all monomer residues constituting the resin are taken as 100 mol%, the 1% weight loss temperature can be made 300°C or higher by having 50% or more of the monomer residues with high thermal stability as described above. Since the resin film is efficiently decomposed by heat generation due to laser absorption during laser transfer, which increases the energy transmitted to the semiconductor element, it is preferable that the 1% weight loss temperature is 600°C or lower.
[0074] In addition, the resin film may further contain other additives as necessary. For example, the resin film may contain a silane compound. By containing a silane compound, the adhesion between the resin film and the first substrate having optical transparency can be adjusted. This makes it possible to prevent the resin film in the portion not irradiated with the laser light from peeling off from the first substrate having optical transparency. Specific examples of the silane compound include the silane compounds described in International Publication No. 2022 / 210155. Furthermore, the resin film may contain a surfactant, if necessary, for the purpose of improving the coatability with the first substrate having optical transparency during film formation and forming a resin film with a uniform thickness.
[0075] Next, a method for producing a laminate according to an embodiment of the present invention will be described. The first laminate can be produced by forming a resin film on a first substrate having optical transparency. An example of a method for producing the first laminate will be described. A varnish in which the components of the resin film are dissolved in a solvent is applied onto a first substrate having optical transparency, and the resin film is produced by heating and curing. When the resin film is produced by a coating method, any coating method can be selected, and examples of the method include spin coating using a spinner, spray coating, roll coating, and slit die coating. The resin film after coating is preferably dried for 1 minute to several tens of minutes at a temperature in the range of 50°C to 150°C using a hot plate, a drying oven, infrared rays, etc. After that, it is preferably heated and cured for several minutes to several hours at a temperature in the range of 100°C to 500°C.
[0076] Next, an example of a method for stacking semiconductor elements to produce a second stack will be described with reference to the drawings. FIG. 1 illustrates a method for producing the second laminate 120. When producing the second laminate by the method of FIG. 1, the semiconductor element 14 is directly arranged on the resin film 12 of the first laminate 110 in which the resin film 12 is laminated on the first substrate 11 having optical transparency, and laminated by pressing with a pressing device 41 such as a vacuum laminator, a wafer bonder, or a press machine. Alternatively, as shown in FIG. 2, a semiconductor element temporary bonding substrate 130 in which the semiconductor element 14 is temporarily bonded on another support 15 via a temporary adhesive 16 is prepared, and the semiconductor element 14 on the temporary adhesive 16 and the resin film 12 surface of the first laminate 110 are overlapped and pressed with the above-mentioned pressing device 41. Thereafter, the temporary adhesive 16 and the support 15 are removed from the semiconductor element 14, and the second laminate 120 can be produced. Further, as shown in FIG. 3, a semiconductor element-attached substrate 140 in which a semiconductor element 14 is directly formed on a crystal growth substrate 17 such as sapphire is stacked with the semiconductor element 14 surface facing the resin film 12 surface, and pressure-bonded by the above-mentioned device 41. Thereafter, the second stack 120 can be produced by a method such as irradiating a laser beam 31 from the crystal growth substrate 17 side and laser lifting off the semiconductor element 14 from the crystal growth substrate 17 to the first stack 110 side. The pressure when stacking the semiconductor elements can be selected from an optimum value depending on the adhesive strength of the resin film, and is selected in the range of 0.05 MPa to 5.0 MPa. By suppressing the embedding of the semiconductor element in the resin film, the semiconductor element can be easily peeled off from the resin film during laser transfer, and the positional accuracy of the laser transfer is improved, so the pressure is more preferably 2.0 MPa or less. When stacking the semiconductor elements, it is also possible to apply pressure while heating as necessary. Heating increases the flexibility of the resin film, further increasing the adhesive strength between the semiconductor element and the resin film, and improving the mounting yield of the semiconductor element on the resin film. The temperature when stacking the semiconductor elements is preferably selected in the range of 15°C to 200°C. In order to reduce the thermal expansion of the laminate, 120°C or less is more preferable.
[0077] Furthermore, from the viewpoint of being able to set the embedding depth of the semiconductor element into the resin film within the above-mentioned preferred range, the temperature when laminating the semiconductor element onto the resin film is preferably 15°C or higher and 80°C or lower, and the pressure is preferably 0.05 MPa or higher and 1.0 MPa or lower.
[0078] Further, another method for producing the second laminate will be described with reference to FIG. 5. The semiconductor substrate 18 before being singulated is bonded to another support 15 via a temporary adhesive 16. Furthermore, varnish is applied onto the semiconductor substrate 18 before being singulated, and the varnish is heated and cured to form a resin film 12, thereby producing a resin-film-attached semiconductor substrate temporary adhesive substrate 150. In this state, the first substrate 11 having optical transparency and the resin-film-attached semiconductor substrate temporary adhesive substrate 150 are bonded facing each other. The support 15 and the temporary adhesive 16 adjacent to the support 15 are peeled off and removed, and then the semiconductor substrate 18 is singulated to produce semiconductor elements 14, thereby producing the second laminate 120.
[0079] Next, a method for manufacturing the semiconductor device will be described. A manufacturing method of a semiconductor device according to an embodiment of the present invention is a manufacturing method of a semiconductor device using a second laminate, and includes a step of placing a second substrate opposite the surface of the second laminate on which the semiconductor element is laminated, and a step of irradiating the second laminate with laser light from the first substrate side to transfer the semiconductor element to the second substrate.
[0080] The process of opposing the semiconductor element surface of the second laminate to a second substrate will be described with reference to the drawings. Fig. 6 illustrates an example of a method for manufacturing a semiconductor device. The semiconductor element surface refers to the surface of the second laminate 120 that has the semiconductor element 14 (the surface on which the semiconductor element is laminated).
[0081] Regarding the second laminate 120 and the second substrate 21 produced by the above-mentioned method, the surface of the second laminate 120 on which the semiconductor element 14 is held is faced to the second substrate 21, and the substrate is fixed so that the second laminate 120 and the second substrate 21 are parallel to each other. In order to prevent misalignment due to the weight of the semiconductor element 14 during transfer, the second laminate 120 and the second substrate 21 are placed facing each other with the second laminate 120 on top. The second laminate 120 and the second substrate 21 are placed at a certain distance. The distance between the semiconductor element surface and the second substrate can be selected depending on the size and thickness of the semiconductor element, and is selected in the range of several μm to several hundreds of μm, for example. In order to improve throughput, the distance between the semiconductor element surface of the second laminate and the surface of the second substrate is preferably 30 μm or more, more preferably 50 μm or more, so that there is no risk of contact between the second laminate and the second substrate. In order to prevent a decrease in positional accuracy during laser transfer, the distance between the surface of the semiconductor element of the second laminate and the surface of the second substrate is preferably 500 μm or less. The second substrate may be any substrate, such as a glass substrate, a resin substrate, a metal substrate, or a circuit substrate on which wiring has already been formed. In addition, the second substrate may have an adhesive layer to hold the semiconductor element after transfer. The adhesive layer may be made of a material having adhesive properties, such as polysiloxane resin, acrylic resin, polyester resin, polyurethane resin, or a resin film similar to the resin film in the laminate according to the embodiment of the present invention. The thickness of the adhesive layer is selected, for example, within the range of 0.5 μm to 100 μm, depending on the size of the semiconductor element and the distance between the semiconductor element and the second substrate. When a circuit board is used as the second substrate, a conductive bonding material such as an anisotropic conductive film (ACF), conductive silver paste, or solder may be formed on the wiring. Furthermore, for the purpose of transfer alignment, an alignment mark may also be provided on the second substrate.
[0082] Next, the process of transferring the semiconductor element to the second substrate by irradiating the second laminate with laser light from the first substrate side having optical transparency will be described with reference to the drawings. FIG. 7A shows an example of the transfer process.
[0083] In the second laminate 120 and the second substrate 21 arranged by the above-mentioned method, the semiconductor element is irradiated with laser light 31 from the light-transmitting first substrate 11 side of the second laminate 120 through the light-transmitting first substrate 11. The type of laser light includes solid lasers such as YAG laser, YVO4 laser, fiber laser, and semiconductor laser, and gas lasers such as carbon dioxide laser, excimer laser, and argon laser, and can be selected according to the wavelength to be used. The beam shape of the irradiated laser light is not limited, and the laser spot size may be smaller than the size of the semiconductor element. However, the size is set so that the laser light does not hit the semiconductor element adjacent to the semiconductor element to be transferred. Since the kinetic energy generated by the ablation of the resin film during laser transfer is transmitted to the entire semiconductor element to be transferred, improving the positional accuracy, the beam shape of the irradiated laser light is preferably rectangular, and the laser spot size is preferably a size adjusted within a range of ±10 μm in both the short axis direction and the long axis direction based on the same size as the semiconductor element, although it depends on the size of the semiconductor element and the interval between the adjacent semiconductor elements. Moreover, it is preferable that the center of the laser spot is located at the center of the semiconductor element.
[0084] Furthermore, when the spot size of the laser light is large enough to impinge on adjacent semiconductor elements, it is also possible to irradiate the laser light 31 through a photomask 51 so that the spot of the laser light does not impinge on the adjacent semiconductor elements, as shown in FIG. 7B. The laser light can be selected with any energy density. From the viewpoint of the stability of the energy density of the laser light, the energy density of the laser light is set to 10 mJ / cm. 2 The above is preferable, and 1000 mJ / cm is preferable because damage to the semiconductor element can be prevented. 2 More preferably, the energy density of the laser beam is 100 mJ / cm or less. 2 More than 700mJ / cm 2 The following is the result.
[0085] By using the second laminate according to the embodiment of the present invention, laser transfer is possible even with a laser beam of low energy density, and further, even when the energy density of the laser beam is changed, the effects on positional accuracy, debris, and adhesive residue can be reduced. The energy density of the irradiated laser beam may have output unevenness for each pulse, and in order to reduce the effects of output unevenness on positional accuracy, it is preferable that the second laminate can achieve the same level of positional accuracy with laser beams of a wide range of energy densities. The range of energy densities of laser beams that can achieve the same level of positional accuracy is 30 mJ / cm. 2 It is preferable to have a margin of at least 50 mJ / cm. 2 More preferably, 100 mJ / cm or more. 2 The above is particularly preferred.
[0086] In addition, when transferring the semiconductor element by laser, the second substrate can be heated. In particular, when an adhesive layer is formed on the second substrate, the retention of the transferred semiconductor element is improved, which is preferable. When heating the second substrate, the heating temperature is preferably 120° C. or less, since this prevents the second substrate from warping due to heat and allows the semiconductor element to be transferred with high positional accuracy.
[0087] The transfer of the semiconductor element is performed while adjusting the position according to the actual mounting location of the semiconductor element in the semiconductor device to be manufactured. For example, when manufacturing an LED display, the LED element is transferred while shifting the pitch according to the pixel size of the display and the arrangement of RGB. Next, the second substrate on which the LED element is transferred and the circuit substrate on which the conductive bonding material is mounted according to the circuit are faced and pressure-bonded to produce a circuit substrate on which the LED element is mounted. When laser transfer is performed using the laminate according to the embodiment of the present invention, the transfer can be performed with high positional accuracy, so that the semiconductor element can be transferred without being misaligned from the circuit of the substrate to be finally mounted, and mounting defects caused by misalignment can be reduced.
[0088] The laser light preferably has a wavelength of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm, or 1064 nm, and more preferably has a wavelength that has an absorbance of 0.4 or more in the resin film. By using these laser lights, the transfer can be performed with high accuracy.
[0089] In the method for producing a semiconductor device of the present invention, the laser light preferably has a wavelength of 248 nm, 266 nm, or 355 nm. As the laser light of 248 nm, 266 nm, or 355 nm, an excimer laser or a YAG laser is particularly preferable.
[0090] In addition, in the method for manufacturing a semiconductor device of the present invention, the second substrate is preferably a circuit substrate. If the second substrate is a circuit substrate, the substrate transferred by the above method can be used as a semiconductor device as is. In addition, there is no concern about misalignment of the semiconductor element due to handling of the substrate after transfer, and the positional accuracy can be further improved. As the circuit substrate, a known one such as a TFT substrate or a printed wiring substrate can be used. EXAMPLES
[0091] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the evaluation methods used in each example and comparative example will be described.
[0092] (1) Method for producing laminate A resin film varnish prepared by the method described below was applied to a 4-inch quartz glass substrate with a thickness of 0.6 mm (manufactured by Taiko Seisakusho Co., Ltd., absorbance at wavelengths of 248 nm, 266 nm, and 355 nm at a thickness of 0.6 mm is 0.01) using a spinner, pre-baked on a hot plate at 120°C for 3 minutes, and then heated and cured at a specified temperature for a specified time to prepare a resin film on the glass substrate, thereby producing a first laminate. The film thickness of the resin film was measured with an optical film thickness meter (manufactured by Dainippon Screen Co., Ltd., Lambda Ace, refractive index = 1.543). The refractive index used can be selected according to the type of resin in order to increase the accuracy of the measurement. Separately, a 4-inch LED substrate (EPILEDS, with alignment marks, a substrate with LEDs formed as semiconductor elements on a sapphire substrate) was prepared and cut into 20 x 15 mm squares using a dicer. The LEDs mounted are as follows. The size of the semiconductor element, the size of the protruding electrode part, and the distance between adjacent elements were measured using a scanning electron microscope (Hitachi High-Technologies Corporation, S-4800). Crystal growth substrate: Sapphire (thickness 0.8 mm) Semiconductor element type: GaN Semiconductor element size: 19.2μm×37.5μm×7.6μm (including electrodes) Number of electrodes: 2 on each side Electrode size: 14.9μm×10.7μm×2.2μm Electrode type: Au Distance between adjacent elements: 13.8 μm in both width and length directions
[0093] The resin film surface of the first laminate and the semiconductor element surface of the cut LED substrate were placed together so that they were in contact with each other, and then bonded together using a flip chip bonder (FC-3000WS, manufactured by Toray Engineering Co., Ltd.) under the conditions described in Tables 4 to 6. After that, a 266 nm wavelength laser device (HSL-5500IIISUV, manufactured by HOYA Corporation, pulse width 5 to 7 nsec, energy density 600 mJ / cm) was used from the first substrate side. 2) a laser was irradiated onto the entire surface of the LED substrate, and the sapphire substrate was separated at the interface between the sapphire substrate and the semiconductor element in the LED substrate, thereby producing a second laminate.
[0094] (2) Measurement of resin film absorbance As a reference, the same substrate as the quartz glass substrate used for the first laminate in (1) was prepared, and the absorbance from 200 nm to 1100 nm was continuously measured using an ultraviolet-visible spectrophotometer (U-2910, manufactured by Hitachi High-Tech Science Corporation). Next, a first laminate for absorbance measurement was prepared in the same manner as in (1), in which a resin film was applied to a thickness of 0.5 to 1.5 μm, and the film thickness of the resin film of the first laminate for absorbance measurement prepared was measured with an optical film thickness meter (Lambda Ace, manufactured by Dainippon Screen, refractive index = 1.543). The absorbance of the first substrate for absorbance measurement was measured in the same manner as described above, and the absorbance of the reference was subtracted. From the values at 248 nm, 266 nm, and 355 nm were read, and the absorbance per film thickness of 1.0 μm was calculated according to the following formula. For the second laminate produced by the method (1) described above, a dicing tape (UDT-1025MC, manufactured by Denka Co., Ltd.) was attached to the semiconductor element surface and then peeled off to remove the semiconductor element from the resin film, and the absorbance was calculated in the same manner as described above. Absorbance per 1.0 μm of film thickness = absorbance (-) / film thickness of resin film (μm)
[0095] (3) Measurement of adhesive strength of resin film (3)-1 Measurement of adhesive strength of the surface of the resin film of the first laminate For the first laminate produced in (1), a Kapton film cut into a strip of 1 cm x 9 cm was pressed onto the surface of the resin film using a vacuum laminator at 0.6 MPa and 35°C. The sample was set in a tensile tester (Nidec-Shimpo Corporation, FGS-VC), and the pressed Kapton film was peeled off in the vertical direction at a constant speed of 50 mm / min. The peel strength at this time was measured using a digital force gauge (Nidec-Shimpo Corporation, FGJN-5). The measurement was performed three times using different samples, and the average value was taken as the adhesive strength. (3)-2 Measurement of adhesive strength between the resin film of the second laminate and the semiconductor element In the second laminate produced in (1), a dicing tape (UDT-1025MC, manufactured by Denka Co., Ltd.) was attached to the semiconductor element surface and peeled off to remove the semiconductor element from the resin film. A Kapton film was pressed onto the surface of the resin film from which the semiconductor element had been peeled off in the same manner as in (3)-1, and the adhesive strength was measured in the same manner as in (3)-1.
[0096] (4) Measurement of bulk elastic modulus of resin film The elastic modulus was measured using a nanoindenter (Triboindenter TI950, manufactured by Hysitron). A dicing tape (UDT-1025MC, manufactured by Denka Co., Ltd.) was attached to the semiconductor element surface of the first laminate or the second laminate, and then peeled off to remove the semiconductor element from the second laminate, thereby producing a sample with the resin film exposed, which was then cut to a size of approximately 10 mm x 10 mm. The prepared sample was fixed to a dedicated sample fixing stand via an adhesive (Aron Alpha (registered trademark) fast acting multi-purpose, manufactured by Toagosei Co., Ltd.), and a Berkovich indenter (triangular pyramidal diamond indenter) was used to indent the surface of the resin film toward the first substrate, and then the load was removed to measure the bulk elastic modulus by an indentation load / unload test. The measurement point was the thickest part of the remaining resin film after the semiconductor element was peeled off. The thickness of the resin film was measured using a laser microscope and a step gauge. The elastic modulus measurement conditions are shown below. [Measurement conditions] Measurement environment: 25±2℃, air Measurement frequency: 100Hz Measurement method: Continuous stiffness measurement method From the obtained load-indentation depth diagram, the elastic modulus was calculated from the average value of the values at a depth of 500 to 1000 nm from the surface of the resin film.
[0097] (5) Surface elasticity measurement of resin film The surface elastic modulus was measured using a nanoindenter (Triboindenter TI950, manufactured by Hysitron). A dicing tape (UDT-1025MC, manufactured by Denka Co., Ltd.) was attached to the semiconductor element surface of the first laminate or the second laminate, and then peeled off to remove the semiconductor element from the second laminate, thereby producing a sample with the resin film exposed, which was then cut to a size of approximately 10 mm x 10 mm. The prepared sample was fixed to a dedicated sample fixing stand via an adhesive (Aron Alpha (registered trademark) fast acting multi-purpose, manufactured by Toagosei Co., Ltd.), and a Berkovich indenter (triangular pyramidal diamond indenter) was used to indent the surface of the resin film toward the first substrate, and then the load was removed to measure the surface elastic modulus by an indentation load / unload test. The measurement point was the thickest part of the remaining resin film after the semiconductor element was peeled off. The thickness of the resin film was measured using a laser microscope and a step gauge. The elastic modulus measurement conditions are shown below. [Measurement conditions] Measurement environment: 25±2℃, air Measurement frequency: 100Hz Measurement method: Continuous stiffness measurement method From the obtained load-indentation depth diagram, the elastic modulus was calculated from the average value of the values at a depth of 20 to 40 nm from the resin film surface.
[0098] (6) Measurement of the thermal decomposition temperature of the resin film Only the resin film was scraped off from the first laminate or the second laminate from which the semiconductor element was peeled off, and treated at 250°C for 30 minutes under a nitrogen atmosphere, and then about 15 mg was packed into a standard aluminum container and measured using a thermogravimetric analyzer (Shimadzu Corporation, TGA-50). The measurement conditions were as follows: after holding at 120°C for 30 minutes, the temperature was raised to 500°C at a heating rate of 5°C / min. The temperature at which the weight was reduced by 1% was read from the obtained weight reduction curve, and this temperature was defined as the 1% weight reduction temperature.
[0099] (7) Evaluation of mounting yield of semiconductor elements The mounting yield of the semiconductor elements mounted on the second laminate was determined by observing and photographing an area on the surface of the second laminate on which the semiconductor elements were mounted using a digital microscope (Keyence Corporation, VHS-6000) that should contain 5,000 semiconductor elements, calculated from the size and spacing of the semiconductor elements, counting the number of semiconductor elements that were actually mounted, and calculating the ratio to 5,000.
[0100] (8) Measurement of embedding depth of semiconductor element in resin film A cross section of the semiconductor element mounting portion of the second laminate was cut out using focused ion beam (FIB) processing, and the embedding depth of the semiconductor element into the resin film was measured from the observation image obtained using a field emission scanning electron microscope (FE-SEM, FEI, Helios G4-CX).
[0101] (9) Laser transfer test of semiconductor elements (9)-1 Preparation of the opposing substrate (second substrate) Polydimethylsiloxane was diluted with toluene on a 4-inch alkali-free glass substrate (Corning, Eagle XG) having a thickness of 0.5 mm, and the diluted solution was adjusted so that the mass ratio of polydimethylsiloxane to toluene was 1:3. The diluted solution was applied using a spinner and cured by heating on a hot plate at 120°C for 3 minutes to form an adhesive layer on the glass substrate. The thickness of the adhesive layer after thermal curing was measured with an optical film thickness meter (Dainippon Screen, Lambda Ace, refractive index = 1.543), and a second substrate was prepared as an opposing substrate with an adhesive layer thickness of 5.0 μm.
[0102] (9)-2 Laser transfer of semiconductor elements The laser light source, the second laminate produced by the above-mentioned method, and the second substrate were arranged in this order in the vertical direction. At this time, the surface of the second laminate on which the semiconductor element is held and the surface of the second substrate on which the adhesive layer is formed were held facing each other so that the distance between the semiconductor element surface and the adhesive layer surface was about 42.0 μm (about 5 times the height of the semiconductor element). The spot size of the laser light was a rectangle of 18 μm × 36 μm, and the positions of the laser light source and the laminate were adjusted so that one semiconductor element was placed in the center of the laser light spot, and the laser light was not irradiated on adjacent semiconductor elements. The laser light source used was an excimer laser with a wavelength of 248 nm (manufactured by OptoSystems, CL-7700), a YAG laser with a wavelength of 266 nm (manufactured by HOYA Corporation, HSL-5500IIISUV), or a YAG laser with a wavelength of 355 nm (manufactured by HOYA Corporation, HSL-5500IIIST). A laser beam with a wavelength of 248 nm, 266 nm or 355 nm is applied to the semiconductor element placed at the laser beam irradiation position at a rate of 250 mJ / cm. 2 ~400mJ / cm 2 Between 50mJ / cm 2 The irradiation was performed while changing the energy density step by step. For each energy density, a laser transfer test was performed on 10 semiconductor elements.
[0103] (9)-3 Evaluation of transfer performance The second substrate was observed after irradiation with the laser light, and the number of semiconductor elements that were actually transferred to the second substrate out of the 10 transferred semiconductor elements, and the number of semiconductor elements that were transferred without being inverted, rolled over, or damaged, were counted.
[0104] (9)-4 Evaluation of position accuracy Using a CCD camera projected from a lens installed coaxially with the laser light source, images of the semiconductor elements on the second laminate before laser transfer and images of the semiconductor elements on the second substrate after laser transfer were acquired, and the amount of positional deviation of the center of the semiconductor elements before and after transfer was calculated from the central coordinates of the semiconductor elements in each acquired image, and the positional accuracy was judged from the average value as follows: The amount of positional deviation was calculated only for semiconductor elements that could be transferred to the second substrate without inversion or tipping over, and the average value was assigned as "5" if it was 0 μm or more and less than 2 μm, "4" if it was 2 μm or more and less than 3 μm, "3" if it was 3 μm or more and less than 4 μm, "2" if it was 4 μm or more and less than 5 μm, "1" if it was 5 μm or more, and "0" if all were tipping over.
[0105] (9)-5 Evaluation of glue residue Without cleaning the second substrate after irradiation with the laser light, the electrode surface of the semiconductor element after transfer was measured using time-of-flight secondary ion mass spectrometry (TOF-SIMS). If Au-derived ions were detected, it was judged that there was no adhesive residue. If no Au-derived ions were detected, it was judged that there was adhesive residue. The measurement conditions for TOF-SIMS are as follows: [Measurement conditions] Equipment: TOF.SIMS 5 (ION-TOF) Primary ion: Bi3 ++ Secondary ion polarity: negative
[0106] (9)-6 Debris evaluation After irradiation with the laser light, the opposing substrate was observed with a field emission scanning electron microscope (FE-SEM, FEI, Helios G4-CX) without being cleaned. If foreign matter of 1 μm or more was present on the surface of the adhesive layer around the transferred semiconductor element, it was judged as "present"; if no foreign matter was found, it was judged as "absent."
[0107] (10) Method for measuring the solid content of a resin solution Approximately 1 g of the resin solution produced by the method described below was weighed out into an aluminum cup, placed on a hot plate at 120°C and heated for 3 minutes, then heated to 250°C, and heated for 30 minutes after reaching 250°C. The mass of the resin remaining after heating was measured, and the solid content was calculated using the following formula. Solid content (mass%) = mass of resin after heating (g) / mass of resin solution before heating (g) × 100. The names and abbreviations of the acid dianhydrides, diamines, additives and solvents shown in the following Preparation Examples are as follows. PMDA: Pyromellitic anhydride (manufactured by Daicel Corporation) BPDA: 3,3',4,4'-biphenyltetracarboxylic anhydride (manufactured by Mitsubishi Chemical Corporation) BTDA: 3,3',4,4'-benzophenonetetracarboxylic anhydride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) DSDA: 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride (Tokyo Chemical Industry Co., Ltd.) PA: Phthalic anhydride (Tokyo Chemical Industry Co., Ltd.) PDA: p-phenylenediamine (Tokyo Chemical Industry Co., Ltd.) BAHF: 4,4'-dihydroxy-3,3'-diaminophenylhexafluoropropane (Merck) APPS1: α,ω-bis(3-aminopropyl)polydimethylsiloxane (average molecular weight: 860, q=9 (average value)) (manufactured by Shin-Etsu Chemical Co., Ltd.) APPS2: α,ω-bis(3-aminopropyl)polydimethylsiloxane (average molecular weight: 1600, q=19 (average value)) (manufactured by Shin-Etsu Chemical Co., Ltd.) SiDA: 1,3-bis(3-aminopropyl)tetramethyldisiloxane (Shin-Etsu Chemical Co., Ltd.) NMP: 2-methyl-1-pyrrolidone (manufactured by Mitsubishi Chemical Corporation) CHN: Cyclohexanone (manufactured by Toyo Gosei Co., Ltd.) Tinuvin 477: A propylene glycol monomethyl ether acetate solution containing 81.0% by mass of a hydroxyphenyltriazine UV absorber (manufactured by BASF) TG-129: γ-butyrolactone solution containing 19.9% by mass of a crosslinking agent having an alkoxymethyl group represented by the structure of the following formula (9) (manufactured by Sanwa Chemical Co., Ltd.).
[0108] [ka]
[0109] Production example 1 (resin solution: P-1) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF, and 192.63g of CHN were charged and dissolved by stirring at 50℃ for 15 minutes. Then, 10.07g (0.068mol) of PA and 23.69g of CHN were added and stirred at 60℃ for 15 minutes. Next, 49.76 g (0.23 mol) of PMDA, 22.41 g (0.076 mol) of BPDA, and 24.08 g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-1 solution with a solid content of 62.0 mass%.
[0110] Production example 2 (resin solution: P-2) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 204.68g (0.24mol) of APPS1, 26.35g (0.017mol) of APPS2, 31.13g (0.085mol) of BAHF, and 195.37g of CHN were charged, and after stirring for 15 minutes at 50°C to dissolve, 2.01g (0.014mol) of PA and 24.42g of CHN were added and stirred for 15 minutes at 60°C. Next, 53.14g (0.17mol) of BTDA, 49.01g (0.17mol) of BPDA, and 24.42g of CHN were added and stirred at 95°C for 1 hour, and then the temperature was raised to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-2 solution with a solid content of 64.0% by mass.
[0111] Production example 3 (resin solution: P-3) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF and 193.77g of CHN were charged and dissolved by stirring at 50℃ for 15 minutes. Then, 10.07g (0.068mol) of PA and 24.22g of CHN were added and stirred at 60℃ for 15 minutes. Next, 49.76 g (0.23 mol) of PMDA, 24.54 g (0.076 mol) of BTDA, and 24.08 g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-3 solution with a solid content of 62.0 mass%.
[0112] Production example 4 (resin solution: P-4) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF and 195.24g of CHN were charged and dissolved by stirring at 50℃ for 15 minutes. Then, 10.07g (0.068mol) of PA and 24.40g of CHN were added and stirred at 60℃ for 15 minutes. Next, 49.76 g (0.23 mol) of PMDA, 27.29 g (0.076 mol) of DSDA, and 24.40 g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-4 solution with a solid content of 65.0 mass%.
[0113] Production example 5 (resin solution: P-5) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF and 195.72g of CHN were charged and dissolved by stirring at 50℃ for 15 minutes. Then, 10.07g (0.068mol) of PA and 23.69g of CHN were added and stirred at 60℃ for 15 minutes. Next, 33.19 g (0.15 mol) of PMDA, 44.75 g (0.15 mol) of BPDA, and 24.46 g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-5 solution with a solid content of 65.0 mass%.
[0114] Production example 6 (resin solution: P-6) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating and cooling device using hot water and cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF, and 204.15g of CHN were charged, and the mixture was stirred at 50°C for 15 minutes to dissolve it. Then, 10.07g (0.068mol) of PA and 25.52g of CHN were added, and the mixture was stirred at 60°C for 15 minutes. Then, 48.75g (0.15mol) of BTDA, 45.01g (0.15mol) of BPDA, and 25.52g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then the mixture was heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-6 solution with a solid content of 61.9% by mass.
[0115] Production example 7 (resin solution: P-7) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating and cooling device using hot water and cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF, and 204.33g of CHN were charged, and after stirring for 15 minutes at 50°C to dissolve, 2.01g (0.014mol) of PA and 25.54g of CHN were added and stirred for 15 minutes at 60°C. Next, 53.14g (0.17mol) of BTDA, 49.01g of BPDA (0.17mol) and 25.54g of CHN were added and stirred at 95°C for 1 hour, and then the temperature was raised to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-7 solution with a solid content of 62.9% by mass.
[0116] Production example 8 (resin solution: P-8) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 204.68g (0.24mol) of APPS1, 26.35g (0.017mol) of APPS2, 8.43g (0.034mol) of SiDA, 18.68g (0.051mol) of BAHF and 193.23g of CHN were charged and dissolved by stirring at 50℃ for 15 minutes, after which 2.01g (0.014mol) of PA and 24.15g of CHN were added and stirred at 60℃ for 15 minutes. Next, 53.14 g (0.17 mol) of BTDA, 49.01 g (0.17 mol) of BPDA, and 24.15 g of CHN were added, and the mixture was stirred at 95° C. for 1 hour, and then heated to 150° C. and reacted for 4 hours to obtain a polyimidesiloxane P-8 solution with a solid content of 62.1 mass %.
[0117] Production example 9 (resin solution: P-9) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating and cooling device using hot water and cooling water, and a stirrer, 233.92g (0.27mol) of APPS1, 26.35g (0.017mol) of APPS2, 18.68g (0.051mol) of BAHF and 189.54g of CHN were charged, and the mixture was stirred at 50°C for 15 minutes to dissolve it. Then, 10.07g (0.068mol) of PA and 23.69g of CHN were added and stirred at 60°C for 15 minutes. Then, 66.37g (0.30mol) of PMDA and 23.69g of CHN were added, and the mixture was stirred at 95°C for 1 hour, and then heated to 150°C and reacted for 4 hours to obtain a polyimidesiloxane P-9 solution with a solid content of 62.5% by mass.
[0118] Production example 10 (resin solution: P-10) In a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 33.54g (0.039mol) of APPS1 and 154.99g of NMP were charged and dissolved at 40°C. 9.84g (0.091mol) of PDA and 19.37g of NMP were added and dissolved. Next, 19.12g (0.065mol) of BPDA and 20.53g (0.064mol) of BTDA were added together with 19.37g of NMP. The mixture was reacted at 60°C for 4 hours to obtain a polyimide precursor P-10 solution with a solid content of 30% by mass.
[0119] The resin solutions obtained in Production Examples 1 to 10 were mixed and stirred with additives and solvents according to the contents of Tables 1 to 3 to prepare varnishes for resin films. The varnishes were filtered through a PTFE filter with a pore size of 0.1 μm. Using these varnishes, first laminates and second laminates were prepared by the above-mentioned method (Examples 1 to 22, Comparative Examples 1 to 4). Details of the prepared laminates and various evaluation results are summarized in Tables 4 to 9.
[0120] [Table 1]
[0121] [Table 2]
[0122]
Table 3
[0123]
Table 4
[0124]
Table 5
[0125]
Table 6
[0126]
Table 7
[0127]
Table 8
[0128]
Table 9
[0129] From the results of Tables 4 to 9, in the laminates of Examples 1 to 22, since the bulk modulus of the resin film was within a specific range, the semiconductor element could be transferred from the second laminate with excellent positional accuracy by a laser of a wide range of energy density. Furthermore, since at least one of the film thickness and adhesive strength in addition to the bulk modulus was within a specific preferred range, the semiconductor element could be transferred with even better positional accuracy. Furthermore, since the bulk modulus, film thickness, adhesive strength and surface modulus were within a specific preferred range, the semiconductor element could be transferred with even better positional accuracy by a laser beam of a wide range of energy density. On the other hand, the laminates of Comparative Examples 1 to 4 showed poor positional accuracy when transferring the semiconductor element. [Explanation of symbols]
[0130] 11. First substrate having optical transparency 12 Resin film 14 Semiconductor elements 15 Support 16 Temporary adhesive 17 Crystal growth substrate 18 Semiconductor Substrate 21 Second Board 31 Laser Light 41 Crimping device 51 Photomask 110 First laminate 120 Second laminate 130 Semiconductor element temporary adhesive substrate 140 Substrate with semiconductor element 150 Semiconductor substrate with resin film, temporary adhesive substrate
Claims
1. A laminate in which a first substrate having optical transparency and a resin film are laminated in this order, the resin film has an absorbance of 0.4 or more and 5.0 or less at a wavelength of 200 to 1100 nm when the film thickness is converted to 1.0 μm; Furthermore, the resin film has an average elastic modulus at 25° C. of 0.06 GPa or more and 1.0 GPa or less at a depth of 500 to 1000 nm from the surface opposite to the surface in contact with the first substrate.
2. A laminate in which a first substrate having optical transparency, a resin film, and a semiconductor element are laminated in this order, the resin film has an absorbance of 0.4 or more and 5.0 or less at a wavelength of 200 to 1100 nm when the film thickness is converted to 1.0 μm; Furthermore, the resin film has an average elastic modulus at 25° C. of 0.06 GPa or more and 1.0 GPa or less at a depth of 500 to 1000 nm from the surface opposite to the surface in contact with the first substrate.
3. 3. The laminate according to claim 1, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less in terms of a film thickness of 1.0 μm at any one of wavelengths of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm and 1064 nm.
4. 3. The laminate according to claim 1, wherein the resin film has an absorbance of 0.4 or more and 5.0 or less when converted into a film thickness of 1.0 μm at any one of wavelengths of 248 nm, 266 nm and 355 nm.
5. 3. The laminate according to claim 1, wherein the resin film has a thickness of 8.0 μm or more and 23.0 μm or less.
6. 3. The laminate according to claim 1, wherein the resin film has an adhesive strength of 0.02 N / cm or more and 0.3 N / cm or less on the surface opposite to the surface in contact with the first substrate.
7. 3. The laminate according to claim 2, wherein the semiconductor element is embedded in the resin film to a depth of 0.1 μm or more and 2.0 μm or less.
8. 3. The laminate according to claim 1, wherein the resin film has an average elastic modulus at 25° C. of 1.0 GPa or more and 7.0 GPa or less at a depth of 20 to 40 nm from the surface opposite to the surface in contact with the first substrate.
9. 3. The laminate according to claim 1 or 2, wherein the resin film contains one or more resins selected from the group consisting of polyimide having a repeating structural unit represented by the following formula (1), polyimide precursor having a repeating structural unit represented by the following formula (2), polybenzoxazole having a repeating structural unit represented by the following formula (3), polybenzoxazole precursor having a repeating structural unit represented by the following formula (4), and copolymers thereof. 【Chemistry 1】 (In formulas (1) to (4), R 1 , R 3 , R 7 and R 9 each independently represents a tetravalent organic group having 6 to 40 carbon atoms; R 2 , R 4 , R 6 and R 8 R each independently represents a divalent organic group having 2 to 40 carbon atoms. 5 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.
10. The laminate according to claim 9 , wherein the resin has at least one of a dimethylsiloxane structure represented by the following formula (5) and a diphenylsiloxane structure represented by the following formula (6): 【Chemistry 2】 (In formula (5) and formula (6), l and m each independently represent an integer of 4 to 40.)
11. the resin contains a polyimide having a repeating structural unit of formula (1), The polyimide having the repeating structural unit of the formula (1) contains 20 mol % to 100 mol % of acid dianhydride residues represented by the following formula (7) based on 100 mol % of all acid dianhydride residues of the polyimide having the repeating structural unit of the formula (1), and The laminate according to claim 9, wherein the diamine residue represented by the following formula (8) is contained in an amount of 60 mol % to 100 mol % based on 100 mol % of all diamine residues of the polyimide having the repeating structural unit of formula (1): 【Chemistry 3】 In formula (7), * represents a bond, X represents a single bond, -CH 2 -, -SO 2 In formula (8), * represents a bond, n represents an integer of 4 to 40, and R 10 and R 11 each independently represents an alkylene group or a phenylene group having 1 to 30 carbon atoms.
12. 3. The laminate according to claim 1, wherein the resin film has a 1% weight loss temperature of 300° C. or higher.
13. The laminate according to claim 1 , wherein the resin film contains at least one of an ultraviolet absorbing agent and a dye.
14. A method for manufacturing a semiconductor device using the laminate according to claim 2, comprising the steps of: placing a second substrate opposite to the surface of the stack on which the semiconductor elements are stacked; A method for manufacturing a semiconductor device, comprising the step of irradiating the laminate with laser light from the first substrate side to transfer the semiconductor element to the second substrate.
15. 15. The method of claim 14, wherein the laser light has a wavelength of any one of 248 nm, 266 nm, 308 nm, 355 nm, 532 nm, and 1064 nm.
16. The method for manufacturing a semiconductor device according to claim 14 or 15, wherein the second substrate is a circuit substrate.
Citation Information
Patent Citations
Manufacturing method of display device and source substrate structure
JP2020188037A
Workpiece handling sheet and device manufacturing method
WO2022153745A1
Laminate, resin composition, and method for manufacturing semiconductor device
WO2022210155A1
Cited By