Production method of thin paper for household and production system of thin paper for household

By shifting and aligning embossing unevenness through controlled folding steps, the method improves the resistance to collapse and ease of unfolding in household tissue paper, addressing alignment stability issues.

JP2024139879AActive Publication Date: 2024-10-10DAIO PAPER CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023050813
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Household tissue paper with unevenness formed by embossing faces challenges in maintaining resistance to collapse and ease of unfolding when folded, as the position of embossing unevenness affects the stability of the fold alignment.

Method used

A method involving a first folding step to shift the edges of the base paper sheet, followed by unevenness formation and a second folding step, with precise control of fold positions to ensure convex and concave portions align correctly, enhancing the resistance to collapse and ease of unfolding.

Benefits of technology

The method stabilizes the alignment of embossing unevenness, preventing collapse and facilitating easy unfolding, reducing defective products and maintaining sheet strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139879000001_ABST
    Figure 2024139879000001_ABST
Patent Text Reader

Abstract

To provide thin paper for household having unevenness in which both a property of the unevenness being hard to collapse in a folded state and easiness of expanding of a fold are easy to be improved.SOLUTION: A production method of thin paper for household includes: a first folding step (step S2) of folding a raw paper sheet G such that end portions are shifted from each other; and an emboss processing step (step S3) of forming unevenness in the raw paper sheet G1 folded in the first folding step (step S2). It is preferable that the production method includes a second folding step (step S5) of further folding the raw paper sheet G2 having unevenness formed in the emboss processing step (step S3).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and system for producing household tissue paper. [Background technology]

[0002] In recent years, in order to improve the surface strength and bulkiness of household thin paper such as toilet cleaners and kitchen cleaners, unevenness is often formed by embossing. Since household thin paper is often provided to users in a folded state, it is preferable for household thin paper with unevenness formed by embossing to be folded so that the convex part on one side of the fold overlaps the concave part on the other side of the fold when folded, and the convex part on one side of the fold fits into the concave part on the other side of the fold, in order to prevent the unevenness from being crushed when folded.

[0003] Therefore, in order to produce household tissue paper folded in this manner, a method is known in which the paper is embossed so that convex and concave portions are arranged alternately, and then the paper is folded by adjusting the position of the fold so that the convex portion on one side of the fold overlaps with the concave portion on one side of the fold (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-13484 A Summary of the Invention [Problem to be solved by the invention]

[0005] When household tissue paper is folded, the user may use it either while it is folded or after unfolding it. If the folded household tissue paper is tightly packed together, it may be difficult to unfold it.

[0006] In this regard, in order to make folded household tissue paper easier to unfold, it is possible to fold it so that the edges do not overlap exactly, but are offset by a specified width; however, when embossing is performed so that convex and concave portions are arranged alternately, as in Patent Document 1, and then the position of the fold is adjusted so that the convex portion on one side of the fold overlaps with the concave portion on the other side of the fold, the position of the fold is determined by the position of the embossed convex and concave portions, making it difficult to stably adjust the offset width of the edges to an appropriate range.

[0007] An object of the present invention is to facilitate the improvement of both the resistance of the unevenness of household tissue paper having unevenness formed thereon to being crushed when folded and the ease with which the folds can be unfolded. [Means for solving the problem]

[0008] In order to solve the above problem, the invention described in claim 1 is a method for producing household tissue paper, a first folding step of folding the base paper sheet so that the edges are offset; a concave-convex forming step of forming concave-convex on the base-paper sheet folded in the first folding step; The present invention is characterized by comprising:

[0009] The invention described in claim 2 is the method for producing household tissue paper described in claim 1, The method is characterized by including a second folding step of further folding the base-paper sheet on which the concave-convex pattern has been formed in the concave-convex pattern forming step.

[0010] The invention described in claim 3 is a method for producing household tissue paper according to claim 1 or 2, The method further comprises a cutting step of cutting the base paper sheet.

[0011] The invention described in claim 4 is the method for producing household tissue paper described in claim 3, The base paper sheet after cutting in the cutting process has a rectangular shape with all folds unfolded, and in the first folding process, the base paper sheet is folded at a first fold that is parallel to one of the sides of the base paper sheet in this state.

[0012] The invention described in claim 5 is the method for producing household tissue paper described in claim 4, The first fold is characterized in that it is a fold that is parallel to the long side of the base-paper sheet in the above-mentioned state.

[0013] The invention described in claim 6 is the method for producing household tissue paper described in claim 4, The first fold is characterized in that it is shifted by 0.5 mm to 5.0 mm from the center of the base-paper sheet in the direction perpendicular to the first fold in the above-mentioned state.

[0014] The invention described in claim 7 is the method for producing household tissue paper described in claim 6, The first fold is characterized in that it is shifted by 1.5 mm to 3.5 mm from the center of the base-paper sheet in the direction perpendicular to the first fold in the above-mentioned state.

[0015] The invention described in claim 8 is a home tissue paper manufacturing system, A folding means for folding the base paper sheet so that the edges are offset; a concave-convex forming means for forming concave-convex on the base-paper sheet folded by the folding means; The present invention is characterized by comprising: Effect of the Invention

[0016] According to the present invention, it is possible to easily improve both the resistance of the unevenness to being crushed when the paper is folded and the ease with which the folds can be unfolded for household tissue paper having unevenness formed therein. [Brief description of the drawings]

[0017] [Figure 1]3 is a flowchart showing a method for manufacturing the toilet cleaner according to the embodiment. [Diagram 2] 1 is a schematic diagram showing a toilet cleaner manufacturing system according to an embodiment, in which the thickness of a base-paper sheet is exaggerated compared to the actual thickness. [Diagram 3] FIG. 11 is a diagram showing a folding method in the first folding process of step S2 in the manufacturing method of the toilet cleaner according to the embodiment, where (a) shows the state before folding and (b) shows the state after folding along the first crease. [Figure 4] FIG. 4 is an enlarged plan view of a portion of the base-paper sheet after the embossing process in step S3 in the manufacturing method of the toilet cleaner according to the embodiment. [Diagram 5] FIG. 1 is a cross-sectional view of a cross section in a direction perpendicular to a first fold after the embossing process in step S3 in a manufacturing method for a toilet cleaner according to an embodiment. Note that the number of recesses and protrusions formed is reduced compared to the actual number, for simplification. [Figure 6] FIG. 11 shows a diagram illustrating the folding method in the second folding process of step S5 in the manufacturing method of the toilet cleaner according to the embodiment, where (a) shows the state before folding, (b) shows the state after folding along the second fold, and (c) shows the state after folding along the third fold. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described with reference to Figures 1 to 6. However, the technical scope of the present invention is not limited to the illustrated examples. In the following, as an example of household thin paper, the manufacture of a toilet cleaner, which is a wet sheet used for cleaning toilets, will be described. In the description of the present embodiment, a numerical range described using "from" includes the numerical values ​​before and after it as the lower limit and upper limit. 2, the devices constituting the toilet cleaner manufacturing system 100 are arranged in a straight line, and the explanation will be given by defining the payout direction of the base paper sheet G from the base paper roll 110 as the X direction, the width direction of the base paper sheet G perpendicular to the X direction as the Y direction, and the thickness direction of the base paper sheet G as the Z direction. In this case, the X direction is along the machine direction of the paper in the papermaking machine when the base paper sheet G is manufactured, and the Y direction is along the cross machine direction of the paper in the papermaking machine when the base paper sheet G is manufactured.

[0019] [1 Manufacturing method description] The manufacturing method for manufacturing a toilet cleaner using the toilet cleaner manufacturing system 100 of the embodiment includes a base paper feeding process (step S1), a first folding process (step S2), an embossing process (step S3), a cutting process (step S4), a second folding process (step S5), a chemical solution impregnation process (step S6), a lamination process (step S7), and a packaging process (step S8), as shown in FIG. Moreover, the toilet cleaner manufacturing system 100 is a complete manufacturing line for manufacturing toilet cleaners.

[0020] [(1) Step S1: Base paper feeding process] When a toilet cleaner is manufactured using the toilet cleaner manufacturing system 100, first, a base paper sheet G is paid out from a base roll 110 provided in the toilet cleaner manufacturing system 100.

[0021] The raw paper roll 110 is configured so that a long raw paper sheet G can be wound up and continuously unwound.

[0022] The base paper sheet G is made by processing a thin paper formed by papermaking a fiber aggregate whose main raw material is known pulp fiber or the like.

[0023] The base paper sheet G may be a sheet made of a plurality of sheets ply-processed or a single sheet, but the weight of the base paper sheet G is preferably 30 g / m 2 From 150 g / m 2 The basis weight is based on JIS P8124.

[0024] The raw fiber of the fiber assembly may be natural or synthetic, and may be a mixture of these. Suitable raw fibers include wood pulp, non-wood pulp, rayon, cotton, and other cellulosic fibers, and biodegradable fibers made of polylactic acid. These fibers may be used in combination with polyethylene fibers, polypropylene fibers, polyvinyl alcohol fibers, polyester fibers, polyacrylonitrile fibers, synthetic pulp, glass wool, and the like.

[0025] The fiber aggregate preferably contains at least pulp, and the raw pulp is preferably a mixture of bleached hardwood kraft pulp (LBKP) and bleached softwood kraft pulp (NBKP) in an appropriate ratio. The blending ratio of the pulp is preferably 50% by mass to 70% by mass.

[0026] A water-soluble binder is added to the base-paper sheet G. As the water-soluble binder, for example, a water-soluble polymer having a carboxyl group, such as carboxymethyl cellulose (hereinafter, referred to as CMC), can be used. When CMC is used as the water-soluble binder, the amount added is preferably 0.5% by mass to 1.0% by mass relative to the mass of the base-paper sheet G.

[0027] [(2) Step S2: First folding process] Next, the base paper sheet G unwound from the base roll 110 in step S1 is folded in half by a first folding device 120 provided in the toilet cleaner manufacturing system 100.

[0028] 3, the first folding device 120 folds the base paper sheet G in half at a first fold F1, which is a fold along the payout direction (X direction) from the base paper roll 110. The base paper sheet folded at the first fold F1 is referred to as a base paper sheet G1.

[0029] At this time, the first folding device 120 folds the sheet so that the edge thereof is shifted by positioning the first fold F1 at a position shifted from the center position in the direction (Y direction) perpendicular to the payout direction of the base paper sheet G from the base roll 110, as shown in FIG. 3. Specifically, it is preferable to fold the base paper sheet G such that the position of the first fold F1 is shifted 0.5 mm to 5.0 mm from the center position of the base paper sheet G in the Y direction, thereby shifting the position of the end portion of the base paper sheet G in the Y direction by 1.0 mm to 10.0 mm, and it is even more preferable to fold the base paper sheet G such that the position of the first fold F1 is shifted 1.5 mm to 3.5 mm from the center position of the base paper sheet G in the Y direction, thereby shifting the position of the end portion of the base paper sheet G in the Y direction by 3.0 mm to 7.0 mm.

[0030] [(3) Step S3: Embossing process] Next, the base paper sheet G1 folded in step S2 is embossed in an embossing device 130 provided in the toilet cleaner manufacturing system 100 to form projections and recesses.

[0031] 2, the embossing device 130 includes two rolls, a top roll 131 and a bottom roll 132. The top roll 131 and the bottom roll 132 are formed with projections and recesses corresponding to the projections and recesses pattern to be formed on the base paper sheet G1, and the projections and recesses formed on the top roll 131 and the projections and recesses formed on the bottom roll 132 are adapted to mesh with each other. By passing the base paper sheet G1 between these, the base paper sheet G1 can be compressed and unevenness can be formed.

[0032] In this case, the embossing is performed on the entire surface of the base paper sheet G1 folded at the first fold F1 so that projections and recesses are arranged alternately.

[0033] 4, convex embossments E1, which are portions that are convex on one side (upward) in the Z direction, and concave embossments E2, which are portions that are concave on one side (upward) in the Z direction (convex on the other side (downward) in the Z direction), are arranged alternately in both the X and Y directions. The flat portion between the convex embossments E1 and the concave embossments E2 is referred to as an intermediate portion M. The concave embossing E2 has a shape obtained by inverting the convex embossing E1 in the thickness direction (Z direction) of the sheet, and the middle portion M is located between the convex embossing E1 and the concave embossing E2 in the Z direction.

[0034] The shape of the convex embossments E1 and the concave embossments E2 is preferably a generally elliptical shape that is longer in the Y direction than in the X direction, as shown in FIG. 4, and a gourd shape with a narrowed portion on the long side.

[0035] Furthermore, since the embossing process is performed on the base paper sheet G1 in the state where it is folded at the first fold F1 in step S2, inevitably, as shown in FIG. 5, the unevenness formed on one side of the first fold F1 and the unevenness formed on the other side of the first fold F1 combine with each other, so that the convex portion on one side of the first fold F1 fits into the concave portion on the other side of the first fold F1.

[0036] [(4) Step S4: Cutting process] Next, in step S3, the base paper sheet G1 that has been embossed is cut by passing it through a cutting device 140 provided in the toilet cleaner manufacturing system 100. The base paper sheet after cutting is referred to as a base paper sheet G2.

[0037] As a result, the base paper sheet G2 becomes a rectangular sheet, as shown in Figure 6(a), folded by the first fold F1, which is a fold parallel to the direction (X direction) along the long side when the first fold F1 is unfolded, such that the positions of both ends in the direction (Y direction) along the short side when the first fold F1 is unfolded are shifted.

[0038] The size of the base paper sheet G2 after cutting, when the first fold F1 is unfolded, is preferably a rectangle with a long side (X direction) of 100 mm to 200 mm and a short side (Y direction) of 50 mm to 100 mm, and more preferably a rectangle with a long side (X direction) of 120 mm to 150 mm and a short side (Y direction) of 70 mm to 100 mm.

[0039] [(5) Step S5: Second folding process] The base paper sheet G2 cut in step S5 is conveyed by the first conveyor C1 to the second folding device 150 provided in the toilet cleaner manufacturing system 100, where it is folded into eight folds.

[0040] Specifically, the second folding device 150 first folds the base-paper sheet G2, which has been folded in half in the Y direction at the first fold F1 as shown in Fig. 6(a), at the second fold F2, which is a fold along the Y direction located at the center of the base-paper sheet G2 in the X direction, as shown in Fig. 6(b). As a result, the base-paper sheet is folded in four. The base-paper sheet in this state is referred to as base-paper sheet G3.

[0041] Furthermore, the second folding device 150 folds the base-paper sheet G3, which has been folded in the Y direction at the first fold F1 and in the X direction at the second fold F2 as shown in Fig. 6(b) into four folds, at the third fold F3, which is a fold along the Y direction located at the center of the X direction of the base-paper sheet G3, as shown in Fig. 6(c). As a result, the base-paper sheet is folded into eight folds. The base-paper sheet in this state is referred to as base-paper sheet G4.

[0042] [(6) Step S6: Chemical impregnation process] The base-paper sheet G4 folded in step S5 is placed on the second conveyor C2 and transported, and during transportation, is impregnated with the chemical liquid L by a chemical impregnation device 160 provided above the second conveyor C2.

[0043] The chemical liquid impregnation device 160 includes a spray nozzle 161 for spraying the chemical liquid L, a tank 162 for storing the chemical liquid L, and piping 163 for connecting the spray nozzle 161 and the tank 162. The chemical liquid L stored in the tank 162 is sprayed from the spray nozzle 161 provided above the second conveyor C2, thereby impregnating the base paper sheet G4 with the chemical liquid L.

[0044] The amount of the chemical solution L impregnated is preferably 100% to 500% by mass, and more preferably 150% to 300% by mass, based on the mass of the base-paper sheet G4.

[0045] The composition of the chemical solution L is not particularly limited, but it is preferable to use one that contains, for example, in addition to water and a crosslinking agent that crosslinks with the water-soluble binder, auxiliary agents such as glycol ethers, aqueous detergents, preservatives, disinfectants, organic solvents, and fragrances.

[0046] As the crosslinking agent, boric acid, various metal ions, etc. can be used, but when CMC is used as a water-soluble binder to be added to the base paper sheet G, it is preferable to use polyvalent metal ions. In particular, it is preferable to use one or more polyvalent metal ions selected from the group consisting of alkaline earth metals, manganese, zinc, cobalt, and nickel, because the fibers are sufficiently bonded to each other to exhibit wet strength sufficient for use while also achieving sufficient water disintegrability. Among these metal ions, it is particularly preferable to use ions of calcium, strontium, barium, zinc, cobalt, and nickel.

[0047] Glycol ethers are compounds that have a structure in which the hydroxyl groups at one or both ends of glycol, a dihydric alcohol, are etherified, and have a hydrophobic alkyl group and a hydrophilic ether group and hydroxyl group in the molecule. They have a smaller molecular weight than surfactants, and have a lower dynamic surface tension than conventional detergents that contain only surfactants, so that they can form an interface between the chemical solution and dirt more quickly. Glycol ethers also act as coupling agents that make hydrophobic oils and dirt compatible with water, and can separate dirt and prevent it from reattaching. Therefore, adding glycol ethers to the chemical solution can improve the wiping performance of toilet cleaners.

[0048] Examples of glycol ethers that may be contained include propylene glycol monomethyl ether (PGME), diethylene glycol monobutyl ether (DGME), ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol isopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol isopropyl ether, diethylene glycol monoisopropyl ether, and ethylene glycol monobutyl ether.

[0049] Of these, PGME is usually added as a cleaning component and is known to improve cleaning power, but it also has the effect of directly improving sheet strength, enhancing the sheet strength improvement effect of CMC and polyvalent metal ions. When PGME is applied to base paper sheet G, the amount applied is 20 g / m 2 From 60 g / m 2 and more preferably 26 g / m 2 From 40 g / m 2 It is.

[0050] As the aqueous detergent, for example, a surfactant as well as a lower or higher (aliphatic) alcohol can be used.

[0051] As the preservative, for example, parabens such as methylparaben, ethylparaben, and propylparaben can be used.

[0052] Examples of disinfectants that can be used include benzalkonium chloride, chlorhexidine gluconate, povidone-iodine, ethanol, benzanium cetyl oxide, triclosan, chloroxylenol, phenoxyethanol, and isopropylmethylphenol.

[0053] As the organic solvent, polyhydric alcohols such as glycol (dihydric), glycerin (trihydric), and sorbitol (tetrahydric) can be used.

[0054] As the fragrance, for example, rose oil, spearmint oil, L-citronellal, etc. can be used.

[0055] In addition, the above-mentioned auxiliary agents for the components of the drug solution can be appropriately selected, and the drug solution may contain other functional components as necessary. For example, propylene glycol (PG) can be used as an auxiliary agent for solubilizing preservatives and disinfectants.

[0056] The method of impregnating the base-paper sheet G4 with the chemical liquid L is most preferably spray application using a spray nozzle as described above, but is not limited thereto as long as it can impregnate the base-paper sheet G4 with an appropriate amount of the chemical liquid L. For example, as long as it can impregnate the base-paper sheet G4 with an appropriate amount of the chemical liquid L, it may be impregnated by a method such as nozzle impregnation or roll transfer.

[0057] [(7) Step S7: Lamination process] The base-paper sheet G4 impregnated with the chemical solution L in step S6 is transported by the second conveyor C2 to the stacking device 170 provided in the toilet cleaner manufacturing system 100, where multiple sheets are stacked. The stack of multiple base-paper sheets G4 formed after stacking is referred to as a sheet block B. The number of sheets to be laminated is not particularly limited, but about 10 sheets is preferable.

[0058] [(8) Step S8: Packaging process] The sheet blocks B stacked in step S7 are transported by the third conveyor C3 to the packaging device 180 provided in the toilet cleaner production system 100, where they are packaged. The specific packaging method is not particularly limited as long as it can suppress the evaporation of the drug solution L and prevent the sheet block B from drying out.

[0059] [2. Description of Effects] According to this embodiment, in the first folding process (step S2), the base paper sheet G is folded so that the ends are shifted by a predetermined width, and then in the embossing process (step S3), unevenness is formed on the base paper sheet G1 in the folded state in step S2. This allows the position of the crease (first fold F1) to be determined in the first folding process (step S2) without being affected by the position of the protrusions and recesses, and in the embossing process (step S3) which is performed in the folded state, the protrusion on one side of the first fold F1 and the recess on the other side of the first fold F1 will necessarily overlap.

[0060] Therefore, according to this embodiment, the deviation width of the ends when folded in the first folding process (step S2) can be easily adjusted to an appropriate width that makes it easy to unfold the first fold F1, and the convex portion on one side of the first fold F1 overlaps with the concave portion on the other side of the first fold F1, making it possible to prevent the unevenness from being crushed when folded. This makes it easier to improve both the resistance of the unevenness to being crushed when folded and the ease with which the folds can be unfolded for household tissue paper with unevenness formed therein.

[0061] In addition, when folding the paper after embossing so that the convex part on one side of the fold overlaps the concave part on the other side of the fold, even a slight deviation in the position of the fold means that the convex part on one side of the fold will not overlap the concave part on the other side of the fold, making the embossment prone to being crushed. Furthermore, household tissue paper that has lost its embossed shape must be discarded as being of poor quality, which is a factor in increasing costs. In this regard, according to the present embodiment, it is possible to ensure that the convex portion on one side of the first fold F1 overlaps with the concave portion on the other side of the first fold F1, thereby suppressing the increase in costs due to the occurrence of defective products as described above.

[0062] In addition, when the household tissue paper is used in a double layer without unfolding the first fold F1, the strength of the sheet can be improved because the unevenness fits perfectly together.

[0063] Furthermore, in the second folding process (step S5), the base paper sheet G2 in which the unevenness has been formed in the embossing process (step S3) is further folded, so that the base paper sheet G2 in which the unevenness has been formed after being folded in half in the first folding process (step S2) can be further folded to a size suitable for packaging.

[0064] Furthermore, by carrying out the first folding process (step S2) before the embossing process (step S3) and carrying out the second folding process (step S5) after the embossing process (step S3), the embossing process (step S3) is carried out on the base paper sheet G1 that has been folded once in the first folding process (step S2) and is in a double-layered state. In this regard, if the base paper sheet is overlapped during embossing, there is a risk that the unevenness formed during embossing will become unclear. However, by performing only the first folding process (step S2) before the embossing process (step S3) as described above, and performing the second folding process (step S5), in which the sheet is folded for the second or subsequent time, after the embossing process (step S3), it is possible to obtain the above-mentioned effects while suppressing the adverse effect of the unevenness caused by the embossing process becoming unclear.

[0065] Furthermore, by setting the position of the first fold F1 to a position that is shifted 0.5 mm to 5.0 mm from the center of the base-paper sheet G in the direction perpendicular to the first fold F1, the position of the end of the base-paper sheet G1 folded at the first fold F1 in the direction perpendicular to the first fold F1 can be shifted within an appropriate range of 1.0 mm to 10.0 mm, making it easier to unfold the first fold F1.

[0066] Furthermore, by setting the position of the first fold F1 to a position that is shifted 1.5 mm to 3.5 mm from the center of the base-paper sheet G in the direction perpendicular to the first fold F1, the position of the end of the base-paper sheet G1 folded at the first fold F1 in the direction perpendicular to the first fold F1 can be shifted within a more appropriate range of 3.0 mm to 7.0 mm, making it easier to unfold the first fold F1.

[0067] [3 Variations] A modification of this embodiment will now be described.

[0068] In the above description of the manufacturing method, the base paper sheet is folded in eight by folding it once in the Y direction at the first fold F1 in the first folding process (step S2), and then folding it twice in the X direction at the second fold F2 and the third fold F3 in the second folding process (step S5). In this regard, although the above-mentioned folding method is most preferable, the folding method of the base-paper sheet is not limited to this. For example, the base-paper sheet may be folded only once in the second folding step (step S5) so that the sheet is folded in four, or may be folded three or more times so that the base-paper sheet is folded even more multiple times.

[0069] In addition, in the above description of the manufacturing method, the edge portions are folded so as to be shifted only in the first folding process (step S2). In addition, the edge portions may be folded so as to be shifted by a predetermined width in the second folding process (step S5) by shifting the positions of the second fold F2 and the third fold F3 from the center in the X direction.

[0070] In this regard, the first fold F1, which is the first fold, is the most difficult to unfold when in use, and the subsequent folds (second fold F2 and third fold F3) are folded in a multiple-layered state and are often easy to unfold in the first place, so even if there is no misalignment at the ends, there are few problems with ease of unfolding. However, by allowing the ends to be misaligned in the second folding process (step S5), in which the sheet is folded from the second time onwards, the complexity of the folding process will increase, but the folds after the second fold F2 can be made even easier to unfold.

[0071] In addition, in the explanation of the above manufacturing method, the fold in the second folding process (step S5) is described as not being in a state in which the convex portion on one side of the fold overlaps the concave portion on the other side of the fold, but the fold in the second folding process (step S5) may also be such that the convex portion on one side of the fold overlaps the concave portion on the other side of the fold. In other words, by positioning the second fold F2 and the third fold F3 at the midpoint between the convex embossing E1 and the concave embossing E2 formed in the embossing process (step S3), when folded, the convex portion on one side of the fold overlaps with the concave portion on the other side of the fold, and the convex portion on one side of the fold fits into the concave portion on the other side of the fold.

[0072] In this regard, as long as the convex portion on one side of the first fold F1 overlaps the concave portion on the other side of the first fold F1, the concave portions of the sheet will overlap twice, which has the effect of improving the resistance to crushing of the concave portions when folded. However, in addition, if the convex portion on one side of the fold and the concave portion on the other side of the fold are also overlapped for the second and subsequent folds, the complexity of the folding process will increase, but the concave portions of the sheet will overlap four or more times, making it even more difficult for the concave portions to be crushed when folded.

[0073] In addition, in the explanation of the above manufacturing method, the production of a toilet cleaner used for cleaning toilets has been described as an example of household tissue paper, but the household tissue paper produced is not limited to toilet cleaner, and household tissue paper for other uses can also be produced through a similar process. For example, a manufacturing method involving steps similar to those described above can be used when producing floor cleaning sheets used for cleaning floors, kitchen cleaning sheets used for cleaning the kitchen, antiperspirant sheets for wiping the skin, and the like. [Explanation of symbols]

[0074] 100 Toilet cleaner manufacturing system 110 Original roll 120 First folding device 130 Embossing device 140 Cutting device 150 Second folding device 160 Chemical impregnation device 170 Stacking device 180 Packaging equipment G, G1, G2, G3, G4 Base Paper Sheets F1 First fold F2 Second fold F3 3rd fold E1 Convex embossing E2 concave embossing M middle part L Chemical Solution B Seat block

Claims

1. a first folding step of folding the base paper sheet so that the edges are offset; a concave-convex forming step of forming concave-convex on the base-paper sheet folded in the first folding step; A method for producing household tissue paper, comprising:

2. 2. The method for manufacturing household tissue paper according to claim 1, further comprising a second folding step of further folding the base paper sheet on which the irregularities have been formed in the irregularity forming step.

3. 3. The method for producing household tissue paper according to claim 1 or 2, further comprising a cutting step of cutting the base paper sheet.

4. The method for manufacturing household tissue paper according to claim 3, characterized in that the base paper sheet after cutting in the cutting process has a rectangular shape with all folds unfolded, and in the first folding process, the base paper sheet is folded at a first fold that is parallel to one of the sides of the base paper sheet in that state.

5. 5. The method for manufacturing tissue paper for household use according to claim 4, wherein the first fold is a fold parallel to a long side of the base paper sheet in the state.

6. The method for manufacturing household tissue paper according to claim 4, characterized in that the first fold is offset by 0.5 mm to 5.0 mm from the center of the base paper sheet in a direction perpendicular to the first fold in the said state.

7. The method for manufacturing tissue paper for household use according to claim 6, characterized in that the first fold is offset by 1.5 mm to 3.5 mm from the center of the base paper sheet in a direction perpendicular to the first fold in the said state.

8. A folding means for folding the base paper sheet so that the edges are offset; a concave-convex forming means for forming concave-convex on the base-paper sheet folded by the folding means; A household tissue paper manufacturing system comprising:

Citation Information

Patent Citations

  • Method for manufacturing household tissue paper

    JP2017035375A

  • Household tissue paper, household tissue paper laminate, production method of household tissue paper, and production method of household tissue paper laminate

    JP2019162279A

  • Cleaning sheet

    JP2021119937A

  • Production method for household tissue paper

    JP2017013484A