Detection method of breakout, operation method of continuous casting facility, and manufacturing method of casting piece
By dynamically adjusting molten steel supply and monitoring nozzle deviations and level height with data-driven thresholds, the method enhances breakout detection accuracy and reduces delays in continuous steel casting.
Patent Information
- Application Number
- JP2023051183
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing methods for detecting breakouts in continuous steel casting equipment are inadequate in predicting or detecting breakouts immediately after the start of casting, particularly due to transient states and insufficient light conditions, leading to delayed detection or false negatives.
A method that adjusts the supply of molten steel and monitors nozzle opening deviations and molten steel level height using dynamic threshold values derived from past operational data to detect breakouts, allowing for early and accurate detection.
Enables quick and precise breakout detection even in transient states, reducing false positives and improving production efficiency by seamlessly integrating with continuous casting operations.
Smart Images

Figure 2024140165000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for detecting a breakout, a method for operating a continuous casting facility, and a method for producing a cast strip. [Background technology]
[0002] In a conventional method for detecting breakouts in a continuous steel casting facility, a camera attached directly below the mold detects breakouts by judging a change in the amount of light captured by the camera using a threshold value, as described in Patent Documents 1 and 2. When a breakout is detected, measures such as stopping the supply of molten steel are taken as soon as possible.
[0003] Also, various methods have been proposed for predicting breakout, and Patent Document 3, for example, discloses a method using a temperature measuring device. In the method of Patent Document 3, temperature measuring rows in which multiple temperature measuring devices are arranged horizontally are arranged in multiple stages in the pouring direction below the molten metal surface of the mold of a continuous casting machine, and for any two stages among the multiple stages, the temperature measuring device arranged in the upper temperature measuring row and the temperature measuring device arranged in the lower temperature measuring row are arranged on the same straight line. Then, the measured values of the temperature measuring devices in the upper and lower stages on the same straight line are transmitted to a calculation device, and the breakout is judged using the relationship between these measured values.
[0004] Furthermore, Patent Documents 4 and 5 disclose a method for determining a breakout based on a deviation between a threshold value of the molten steel level or a molten steel level to be controlled, and an actual molten steel level. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2001-25851 A [Patent Document 2] Japanese Patent Application Publication No. 2-235561 [Patent Document 3] JP 2017-154155 A [Patent Document 4] JP 2004-160525 A [Patent Document 5] Japanese Patent Application Publication No. 47-21331 Summary of the Invention [Problem to be solved by the invention]
[0006] Various methods have been proposed for predicting breakouts, such as those in Patent Document 3, and although they can predict breakouts with a certain degree of accuracy based on signs of breakouts, they cannot predict all breakouts completely. Therefore, it is necessary to detect breakouts using a camera installed directly below the mold, as in Patent Documents 1 and 2.
[0007] Furthermore, immediately after the start of casting, the methods disclosed in Patent Documents 1 to 3 were unable to predict or detect a breakout for the following reasons. The method of predicting a breakout is based on the temperature of the mold, but immediately after the start of casting, the mold is in a transitional state where the temperature is rising from room temperature, and does not show the same behavior every time. Therefore, it is difficult to predict a breakout immediately after the start of casting. Also, the amount of molten steel inside the mold is less than in normal conditions, even for the camera below the mold, so the amount of light is insufficient and it is difficult to detect a breakout.
[0008] Furthermore, in Patent Documents 4 and 5, breakout is detected by determining a lower limit of the molten metal level using a certain threshold value, or by creating a threshold value based on the deviation from the control value. Since it is based on the molten metal level, it is possible to detect breakout even in a transient state immediately after the start of casting. However, in the early stages of casting, the casting speed is often controlled using a certain pattern, and in this case, the molten metal level is prone to hunting immediately after the casting speed is increased or immediately after the casting speed is made constant. For this reason, if a certain threshold value is used to make a judgment at the early stages of casting, it is necessary to set the threshold value according to the part with large variations, and there is a problem that a delay occurs in the time to detect breakout at other times.
[0009] Therefore, the present invention has been made in consideration of the above-mentioned problems, and has an object to provide a method for detecting a breakout, a method for operating a continuous casting equipment, and a method for manufacturing a cast slab, which are capable of quickly detecting a breakout even in a transient state immediately after the start of casting. [Means for solving the problem]
[0010] (1) According to one aspect of the present invention, there is provided a method for detecting a breakout in continuous steel casting equipment, comprising: monitoring at least one of a molten steel level height of molten steel supplied into a mold at the start of casting and an aperture deviation of a nozzle that adjusts the amount of molten steel supplied into the mold; and detecting that a breakout has occurred in at least one of the cases where the molten steel level height falls below a lower limit H0 of the allowable height over time after the start of casting and where the aperture deviation exceeds an upper limit S0 of the allowable deviation over time after the start of casting.
[0011] (2) In the above configuration (1), the allowable lower limit height H0 is calculated by the formula (1) based on multiple operational data from the start of past casting. H0 = H-Aσ1 (1) Where: H0: Lower limit of allowable height H: Average value of the mold surface height from multiple past operation data A: Coefficient σ1: Standard deviation of the mold surface height from multiple past operational data
[0012] (3) In the above configuration (1) or (2), the allowable deviation upper limit S0 is calculated by the formula (2) based on multiple operational data from the start of past casting. S0 = S + Bσ2 (2) Where: S0: Upper limit of allowable deviation S: Average nozzle opening deviation from multiple past operation data B: Coefficient σ2: Standard deviation of nozzle opening deviation from multiple past operational data
[0013] (4) In any one of the configurations (1) to (3) above, when the molten metal level height is less than the lower limit H0 of the allowable height and the opening deviation exceeds the upper limit S0 of the allowable deviation, it is detected that a breakout has occurred.
[0014] (5) According to one aspect of the present invention, there is provided a method for operating a continuous casting facility for continuously casting steel, comprising the steps of: There is provided a method for operating a continuous casting facility, comprising: detecting a breakout at the start of casting using the breakout detection method according to any one of the configurations (1) to (4) above; and interrupting the supply of molten steel to a mold when the breakout is detected.
[0015] (6) According to one aspect of the present invention, there is provided a method for producing a slab by continuously casting steel using the method for operating a continuous casting facility as configured in (5) above. Effect of the Invention
[0016] According to one aspect of the present invention, there are provided a method for detecting a breakout, a method for operating a continuous casting facility, and a method for producing a cast slab, which are capable of quickly detecting a breakout even in a transient state immediately after the start of casting. [Brief description of the drawings]
[0017] [Figure 1] 1 is a configuration diagram showing a continuous casting facility according to an embodiment of the present invention. FIG. [Diagram 2] FIG. 2 is a schematic diagram showing a state of the continuous casting equipment at the start of casting. [Diagram 3] 1 is a graph showing the allowable lower limit of height and the molten metal surface height at the time of breakout occurrence in an embodiment. [Figure 4] 11 is a graph showing an allowable upper limit of deviation and an opening deviation when a breakout occurs in an embodiment. [Diagram 5] 13 is a graph showing the relationship between the coefficient A and the number of detections in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] In the following detailed description, an embodiment of the present invention will be described with reference to the drawings. In the description of the drawings, identical or similar parts are given identical or similar symbols, and duplicated explanations are omitted. Each drawing is schematic and may differ from the actual one. In addition, the embodiments shown below are examples of devices and methods for embodying the technical idea of the present invention, and the technical idea of the present invention does not specify the materials, structures, arrangements, etc. of the components as described below. The technical idea of the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.
[0019] <Device configuration> FIG. 1 is a schematic diagram showing a continuous steel casting equipment 1 according to an embodiment of the present invention. The continuous casting equipment 1 includes a tundish 10, a sliding nozzle 11, a submerged nozzle 12, a mold 13, a plurality of support rolls 14, a molten steel level gauge 15, and a judgment unit 16. In the continuous casting equipment 1, molten steel 2 contained in the tundish 10 is poured into the mold 13 through the sliding nozzle 11 and the submerged nozzle 12, and is cooled to form a solidified shell at the boundary between the mold 13 and the molten steel 2. The solidified shell is then pulled out while being supported by the support rolls 14, and is further cooled by cooling water or the like to form a cast piece having a predetermined cross-sectional shape.
[0020] The sliding nozzle 11 has a plate 110 with holes formed therein, and the plate 110 slides to control the amount of molten steel 2 supplied from the tundish 10 to the mold 13. Specifically, the amount of molten steel 2 supplied is controlled by controlling the overlapping area between the holes in the plate 110 and the holes formed in the bottom of the tundish 10. The ratio of the sliding amount based on the relative position of the plate 110 in the sliding direction with respect to the tundish 10 is called the nozzle opening degree (%). For example, the nozzle opening degree may be 100% when the hole in the plate 110 and the hole in the bottom of the tundish 10 completely overlap in the sliding direction, and 0% when the two holes do not overlap. Furthermore, the difference (variation) of the nozzle opening degree after the average value of the nozzle opening degree for a certain period from the start of casting is called the opening degree deviation. In this embodiment, the determination unit 16 calculates the opening degree deviation from the measurement result of the nozzle opening degree. The certain period for calculating the average value of the nozzle opening degree is not particularly limited, but is preferably about 50 seconds.
[0021] The molten steel level gauge 15 is a measuring device that measures the molten steel level height, which is the height of the bath surface of the molten steel 2 in the mold 13. The measurement method of the molten steel level gauge 15 is not particularly limited as long as it is a known measurement method capable of measuring the molten steel level height. For example, a vortex type molten steel level gauge may be used for the molten steel level gauge 15. The molten steel level height is not particularly limited as long as it is capable of grasping the vertical position of the bath surface of the molten steel 2 in the mold 13, and may be, for example, the height (vertical distance) from the bottom surface of the mold 13 or a predetermined position inside the mold 13.
[0022] In the continuous casting equipment 1, the amount of molten steel 2 supplied to the mold 13 is adjusted by an adjustment mechanism (not shown). The adjustment of the amount of molten steel 2 supplied by this adjustment mechanism is performed by adjusting the nozzle opening based on the measurement result of a molten steel level gauge 15 so that the molten steel level is at a predetermined height.
[0023] The determination unit 16 is a calculation device such as a computer that detects a breakout at the start of casting based on at least one of the nozzle opening degree and the molten metal level. A method for detecting a breakout by the determination unit 16 will be described in detail later.
[0024] In this embodiment, the period during which continuous casting is performed will be described by dividing it into a casting start time and a steady casting time. The casting start time is the period from immediately after the start of continuous casting until the casting speed reaches the steady casting speed. The steady casting time is the period after the casting start time, that is, the period after the casting speed reaches the steady casting speed.
[0025] At the start of casting, continuous casting is started in the state shown in Fig. 2. As shown in Fig. 2, at the start of continuous casting, a dummy bar 17 is inserted into the continuous casting equipment 1, and the tip of the dummy bar 17 (dummy bar head) is placed in the mold 13. Then, with the tip of the dummy bar 17 at the bottom of the mold 13, molten steel 2 is poured into the mold 13, thereby starting continuous casting. Then, after a predetermined time has elapsed since the molten steel 2 was poured, the dummy bar 17 is pulled out. Then, at a predetermined position, the dummy bar 17 is separated from the slab, and the casting speed is increased to a steady casting speed.
[0026] At the start of casting, the judgment unit 16 continuously judges whether or not a breakout has occurred, thereby detecting a breakout. Note that since a breakout cannot occur when the dummy bar 17 is present inside the mold 13, the breakout is detected after the dummy bar 17 is pulled out of the mold 13. If a breakout is detected, the supply of molten steel 2 to the mold 13 is stopped, and casting is interrupted. On the other hand, if a breakout is not detected, casting is continued, and the breakout detection is also continued. The steady casting period is not particularly limited, and continuous casting is performed at a steady casting speed using a known continuous casting method.
[0027] <How to detect a breakout> The method for detecting a breakout according to the present embodiment will now be described. In the present embodiment, as described above, the method for detecting a breakout is performed based on at least one of the molten metal level height and the opening deviation at the start of casting.
[0028] (Detection method based on molten metal surface height) First, a method for detecting a breakout based on the molten steel level height will be described. In the detection method based on the molten steel level height, first, when continuous casting is started, the molten steel level gauge 15 continuously measures the molten steel level height, and the measurement results are sent to the judgment unit 16, thereby monitoring the molten steel level height. Note that, as the molten steel level height, an actual distance (mm) may be used, or an output value (%) of the molten steel level gauge 15 corresponding to the actual distance may be used.
[0029] Next, the judgment unit 16 judges whether or not the measured molten metal level becomes less than the allowable height lower limit H0 over time after the start of casting. Then, the judgment unit 16 judges that a breakout has occurred when the molten metal level becomes less than the allowable height lower limit H0, and judges that a breakout has not occurred when the molten metal level becomes equal to or greater than the allowable height lower limit H0.
[0030] When a breakout occurs, the molten steel 2 breaks through the solidified shell and leaks out inside the continuous casting equipment 1, and the amount of molten steel 2 discharged from the mold 13 becomes greater than the amount of molten steel 2 supplied from the tundish 10, causing a drop in the molten steel level. For this reason, by setting a lower limit H0 of the allowable height as a threshold value for detecting a breakout, it is possible to detect a breakout in the early stages of casting. The lower limit H0 of the allowable height is a value at the time elapsed after the start of casting, and is set for each elapsed time. For example, the lower limit H0 of the allowable height may be set for each measurement time interval of the molten steel level.
[0031] Furthermore, it is preferable that the allowable height lower limit H0 is calculated by the formula (1) based on multiple operation data from the start of past casting. Note that the multiple operation data from the past are obtained under conditions where no breakout occurs. Moreover, it is preferable that the coefficient A is 5.0 or more and 10.0 or less. H0 = H-Aσ1 (1) Where: H0: Lower limit of allowable height H: Average value of the mold surface height from multiple past operation data A: Coefficient σ1: Standard deviation of the mold surface height from multiple past operational data
[0032] The number of past operation data is preferably 50 or more in order to evaluate the variation (standard deviation) of the molten metal level height, while the number of past operation data is preferably 200 or less in order to deal with changes in patterns due to long-term fluctuations.
[0033] (Detection method based on opening deviation) Next, a method for detecting a breakout based on the opening deviation will be described. In the method for detecting a breakout based on the opening deviation, first, when continuous casting is started, the judgment unit 16 continuously acquires the nozzle opening of the sliding nozzle 11 and calculates the opening deviation, thereby monitoring the opening deviation.
[0034] Next, the determination unit 16 determines whether the obtained opening deviation exceeds the upper limit S0 of the allowable deviation over time after the start of casting. If the opening deviation exceeds the upper limit S0 of the allowable deviation, the determination unit 16 determines that a breakout has occurred, and if the opening deviation is equal to or smaller than the upper limit S0 of the allowable deviation, the determination unit 16 determines that a breakout has not occurred.
[0035] When a breakout occurs, the molten steel level drops as described above, and control is performed to increase the nozzle opening to increase the amount of molten steel 2 supplied from the tundish 10. The supply amount at this time is greater than when no breakout occurs, and the nozzle opening and opening deviation are also greater than usual. For this reason, by setting an allowable deviation upper limit S0 as a threshold value for detecting a breakout, it is possible to detect a breakout in the early stages of casting. Furthermore, the allowable deviation upper limit S0 is a value at the time elapsed after the start of casting, and is set for each elapsed time. For example, the allowable deviation upper limit S0 may be set for each measurement time interval of the molten steel level height.
[0036] Furthermore, it is preferable that the allowable deviation upper limit S0 is calculated by the formula (2) based on multiple operation data from the start of past casting. Note that the multiple operation data from the past are obtained under conditions where no breakout occurs. Moreover, it is preferable that the coefficient B is 5.0 or more and 10.0 or less. S0 = S + Bσ2 (2) Where: S0: Upper limit of allowable deviation (%) S: Average value (%) of the opening deviation of multiple past operation data B: Coefficient σ2: Standard deviation of the opening deviation of multiple past operation data
[0037] In addition, the number of past operation data is preferably 50 or more in order to evaluate the variation (standard deviation) of the opening deviation, while the number of past operation data is preferably 200 or less in order to deal with changes in patterns due to long-term fluctuations.
[0038] (Detection method based on the level of the molten metal and the deviation of the opening) Furthermore, in this embodiment, a breakout may be detected based on both the molten metal level height and the opening deviation. In this case, the judgment unit 16 monitors both the molten metal level height and the opening deviation, and judges that a breakout has occurred when the molten metal level height is less than the lower limit H0 of the allowable height and the opening deviation exceeds the upper limit S0 of the allowable deviation. On the other hand, when the molten metal level height is less than the lower limit H0 of the allowable height and the opening deviation does not exceed the upper limit S0 of the allowable deviation, the judgment unit 16 judges that a breakout has not occurred. Note that it is also possible to monitor both the molten metal level height and the opening deviation, and judge that a breakout has occurred when the molten metal level height is less than the lower limit H0 of the allowable height or the opening deviation exceeds the upper limit S0 of the allowable deviation.
[0039] As described above, in this embodiment, the occurrence of a breakout is detected by making a judgment based on at least one of the molten metal level height and the nozzle aperture deviation. Since the judgment of the occurrence of a breakout is made based on at least one of the lower limit H0 of the allowable height and the upper limit S0 of the allowable deviation over time after the start of casting, it is possible to make a judgment with higher accuracy even in the transient state immediately after the start of casting compared to the case where the judgment is made based on a fixed threshold value for the molten metal level height or the nozzle aperture.
[0040] Furthermore, by setting the allowable height lower limit H0 using a plurality of past operation data and formula (1), or by setting the allowable deviation upper limit S0 using a plurality of past operation data and formula (2), breakout can be detected with high accuracy. The molten metal level is automatically controlled to be a constant value, but in reality it is not constant and varies within a certain range. Since the operation is based on a constant operation immediately after the start of casting, the speed pattern is similar, but the molten metal level is prone to hunting immediately after the casting speed is increased or immediately after the casting speed is made constant, so the average and variation of the molten metal level depend on the passage of time. For this reason, by setting the allowable height lower limit H0 and the allowable deviation upper limit S0 for each elapsed time, breakout can be detected with higher accuracy. Furthermore, by increasing the detection accuracy, false detection can be prevented and productivity can be improved. Furthermore, since breakout can be detected more quickly than in conventional detection methods such as those in Patent Documents 3 and 4, the impact on production caused by breakout can be reduced. Furthermore, since breakout can be detected directly compared to detection methods based on the mold temperature, detection can be performed without missing any.
[0041] Furthermore, unlike the molten metal surface height, the nozzle opening degree is not constant, depending on the size (width and thickness) of the mold 13 and various other conditions. For this reason, by making a judgment using the opening deviation, which is the fluctuation value from the average value for a certain period of time from the start of casting during the chance to make the judgment (the unit of continuous casting), it becomes possible to detect breakout using the same judgment criteria regardless of the size of the mold 13.
[0042] Furthermore, by detecting a breakout based on both the molten metal surface height and the opening deviation, it is possible to detect a breakout with higher accuracy.
[0043] Furthermore, in this embodiment, it is preferable to set the coefficients A and B in formulas (1) and (2) to 5.0 or more and 10.0 or less, in other words, to detect a breakout when there is a fluctuation of 5 to 10 times the standard deviation of the molten metal level height and the opening deviation of the past operation data. In this way, it is possible to determine a breakout without erroneous detection.
[0044] <Modification> Although the present invention has been described above with reference to specific embodiments, it is not intended that the invention be limited by these descriptions. By referring to the description of the present invention, other embodiments of the present invention including various modifications in addition to the disclosed embodiments will be apparent to those skilled in the art. Therefore, it should be understood that the embodiments of the invention described in the claims also include embodiments including these modifications described herein, either alone or in combination.
[0045] For example, in the present embodiment, the method for detecting a breakout has been described, but the present invention is not limited to such an example. The present invention can also be applied to a method for operating a continuous casting facility and a method for manufacturing a slab. A method for operating a continuous casting facility according to one aspect of the present invention is a method for operating a continuous casting facility 1 that continuously casts steel, and detects a breakout using the method for detecting a breakout according to the above embodiment at the start of casting. If a breakout is detected, the supply of molten steel 2 to the mold 13 is interrupted, and if a breakout is not detected, the supply of molten steel 2 to the mold 13 is continued. In addition, a method for manufacturing a slab according to one aspect of the present invention continuously casts steel using the above method for operating the continuous casting facility 1. EXAMPLES
[0046] The inventors of the present invention conducted an example, in which the allowable height lower limit H0 and the allowable deviation upper limit S0 were calculated from the data of 200 past operations using formulas (1) and (2), and the mold surface height and the aperture deviation at the time of breakout occurrence for two chances were compared.
[0047] FIG. 3 shows the behavior of the molten steel surface height at the time of the occurrence of the breakout for two chances with respect to the elapsed time, as compared with the lower limit H0 of the allowable height and the molten steel surface height at the time of the occurrence of the breakout for two chances. In FIG. 3, the vertical axis indicates the molten steel surface height, and the horizontal axis indicates the elapsed time (sec) from the start of the withdrawal of the dummy bar. The molten steel surface height on the vertical axis is the output value (%) of the molten steel level gauge 15 corresponding to the actual distance, and is controlled to be 45%. The elapsed time on the horizontal axis indicates the start of pouring the molten steel 2 into the mold 13 at -50 sec, and the start of the withdrawal of the dummy bar at 0 sec. In the example shown in FIG. 3, the coefficient A is set to 7, that is, the average value of the molten steel surface height is set to 7 times the standard deviation as a threshold value. In the example shown in FIG. 3, the timing when the molten steel surface height falls below the lower limit H0 of the allowable height is 10 to 20 seconds before the breakout detection that is currently dependent on the operator, and it was confirmed that the breakout can be detected quickly and accurately.
[0048] In the example shown in FIG. 3, the threshold value changes with time, and it was confirmed that it reaches a maximum about 20 seconds after the start of casting. This is because the casting speed is changed about 20 seconds after the start of casting, which causes the variation in the molten metal level to increase, but it was confirmed that it then falls to about 1 / 3 of the peak. Here, in the detection methods such as those in Patent Documents 4 and 5, detection is performed using a constant threshold value that matches the peak of the variation, so the threshold value must be set large over the entire time period. However, in the detection method according to the above embodiment, the optimal threshold value is selected according to the passage of time from past operation data, so it is possible to detect breakout more quickly than conventional detection methods.
[0049] FIG. 4 shows the behavior of the opening deviation at the time of breakout occurrence for the obtained allowable deviation upper limit S0 and two chances with respect to the elapsed time. In FIG. 4, the vertical axis is the opening deviation, and the horizontal axis is the elapsed time (sec) from the start of the dummy bar withdrawal, as in FIG. 3. The opening deviation on the vertical axis is the difference from the average nozzle opening from -50 sec to 0 sec, and is shown after the elapsed time of 0 sec. In addition, in the example shown in FIG. 4, the coefficient B is set to 4, that is, the average opening deviation is given a threshold value of 4 times the standard deviation. Furthermore, the breakout occurrence chance in FIG. 4 is the same as that in FIG. 3. As is clear from FIG. 4, it was confirmed that breakout can be detected more quickly than the conventional method even when the opening deviation is used, as in the case of using the molten metal level.
[0050] Furthermore, the effect of the coefficients A and B in the formulas (1) and (2) on the detection accuracy and the occurrence of false positives was also investigated. Figure 5 shows the relationship between the coefficients A and B and the number of breakout detections when the coefficients A and B are changed from 1.0 to 10.0. In Figure 5, the graph shown with "Both" is the case where both the detection methods of the molten metal level and the opening deviation are used, and a breakout is detected as having occurred only when a breakout is detected in both the molten metal level and the nozzle opening. In this investigation, the number of breakouts that actually occurred was two. It was confirmed that by decreasing the coefficients A and B, the number of false positives decreased but the number of overdetections increased, while by increasing the coefficients A and B, the number of overdetections decreased but the number of false positives increased. For this reason, it was confirmed that the coefficients A and B are appropriate for the equipment of this embodiment, from 3.0 to 8. Furthermore, in this embodiment, the coefficients A and B were set to 4, and the number of detections was two under the condition of using both the detection methods of the molten metal level and the opening deviation, and it was confirmed that there were no overdetections or false positives. For this reason, it was confirmed that the occurrence of a breakout can be detected with high accuracy by detecting both the molten metal surface height and the opening deviation. [Explanation of symbols]
[0051] 1. Continuous casting equipment 10 Tundish 11 Sliding nozzle 110 Plate 12 Submerged nozzle 13 Mold 14 Support roll 15 Molten Steel Level Gauge 16 Judgment section 17 Dummyba 2. Molten Steel
Claims
1. In a continuous steel casting facility, at least one of a level of a molten steel surface to be supplied into a mold at a time when casting is started and an opening deviation of a nozzle for adjusting a supply amount of the molten steel to be supplied into the mold is monitored; The molten metal level is equal to the lower limit H 0 If the opening deviation is less than the allowable deviation upper limit S 0 A method for detecting a breakout, which detects that a breakout has occurred in at least one of the cases where the price exceeds the breakout threshold.
2. The allowable height lower limit H 0 The method for detecting a breakout according to claim 1, wherein is calculated using formula (1) based on multiple pieces of operational data from the start of casting in the past. H 0 =H-Aσ 1 ・・・(1) Where: H 0 : Lower limit of allowable height H: Average value of the molten metal level from multiple past operation data A: Coefficient σ 1 : Standard deviation of the mold level height from multiple past operation data
3. The allowable deviation upper limit S 0 The method for detecting a breakout according to claim 1, wherein is calculated using formula (2) based on multiple operation data from the start of casting in the past. S 0 =S+Bσ 2 ・・・(2) Where: S 0 : Upper limit of allowable deviation S: Average value of nozzle opening deviation from multiple past operation data B: Coefficient σ 2 : Standard deviation of nozzle opening deviation from multiple past operation data
4. The molten metal level is equal to the allowable lower limit H 0 and the opening deviation is less than the allowable deviation upper limit S 0 The method for detecting a breakout according to claim 1, further comprising detecting that a breakout has occurred when the first and second values of the first and second values of the second and third ...
5. A method for operating a continuous casting facility for continuously casting steel, comprising the steps of: At the start of casting, detecting the breakout using the breakout detection method according to any one of claims 1 to 4, The method for operating a continuous casting facility further comprises interrupting the supply of molten steel to the mold when the breakout is detected.
6. A method for producing a cast slab, comprising the steps of: continuously casting steel using the method for operating a continuous casting facility according to claim 5 to produce the cast slab.
Citation Information
Patent Citations
Threshold value setting device
JP1991291526A
Method for predicting breakout of continuous casting mold
JP1992037458A
Casting method at the time of lacking in continuous casting
JP1993305408A
Control method of molten steel surface level inside mold in continuous casting machine
JP2003245761A
Method and system for controlling flow passage opening / closing means at occurrence of breakout