Polyarylene sulfide resin composition, molded article, and method for producing the same

The PAS resin composition, incorporating glass fiber, silane coupling agent, and poorly water-soluble glass, addresses interfacial adhesion issues and enhances mechanical strength and resistance to moist heat and hot water, suitable for outdoor and high-heat applications.

JP2024140276APending Publication Date: 2024-10-10DIC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023051338
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing polyarylene sulfide (PAS) resin compositions, particularly glass fiber-reinforced PAS resins, suffer from decreased mechanical strength and moldability in wet heat environments due to reduced interfacial adhesion, and lack sufficient hot water resistance for applications in outdoor and high-heat devices.

Method used

A PAS resin composition is formulated with specific amounts of glass fiber, a silane coupling agent with a particular structure, and poorly water-soluble glass containing silver and/or zinc, along with oxides like B2O3, Al2O3, SiO2, and ZrO2, enhancing moist heat and hot water resistance.

Benefits of technology

The composition achieves improved mechanical strength, moldability, and resistance to moist heat and hot water, making it suitable for parts exposed to high humidity and temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140276000001
    Figure 2024140276000001
  • Figure 2024140276000002
    Figure 2024140276000002
  • Figure 2024140276000003
    Figure 2024140276000003
Patent Text Reader

Abstract

To provide a polyarylene sulfide (PAS) molded article having excellent wet and heat resistance and hot water resistance, a PAS resin composition by which the molded article can be provided and has excellent processability, and a method for producing the article.SOLUTION: Provided are a resin composition and a molded article in which 10 to 50 pts.mass of glass fiber, 0.1 to 3.5 pts.mass of silane coupling agent, and 0.1 to 10 pts.mass of hardly water-soluble glass are blended into 100 pts.mass of PAS resin, where the silane coupling agent is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound and a hydroxyl group-containing alkoxysilane compound, and the hardly water-soluble glass is glass containing silver and / or zinc and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2 and ZrO2, and a method for producing the composition and article.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyarylene sulfide resin composition, a polyarylene sulfide resin molded article, and a method for producing the same. [Background technology]

[0002] In recent years, engineering plastics with excellent productivity and moldability have been developed, and because they are lightweight, they are widely used as alternative materials to metal materials for electrical and electronic equipment, automobiles, etc. Among these, polyarylene sulfide (hereinafter sometimes abbreviated as "PAS") resins, such as polyphenylene sulfide (hereinafter sometimes abbreviated as "PPS") resin, are mainly used for electrical and electronic equipment parts, automobile parts materials, etc., because of their excellent mechanical strength, heat resistance, chemical resistance, moldability, dimensional stability, flame retardancy, etc.

[0003] In order to improve the mechanical strength of general PAS resins, inorganic fillers such as glass fibers are often added. However, in glass fiber-reinforced PAS resin compositions, the interface between the PAS resin and the glass fibers is weak in a moist and hot environment (high humidity and high temperature environment), and there is a problem that the interface adhesion decreases over time, resulting in a decrease in mechanical strength. In particular, water heater parts, building material parts, automobile parts, construction machinery parts, agricultural machinery parts, etc. are sometimes used in outdoor environments, and there has been a demand for glass fiber-reinforced PAS resins with excellent moist and heat resistance.

[0004] In addition, devices, especially in the automobile industry, are becoming smaller and more powerful, and the amount of heat generated by them is steadily increasing. Therefore, the level of hot water resistance as well as the moist heat resistance of components such as vehicle-mounted cooling components and water-related components is increasing, and various technologies have been developed to improve the properties. For example, Patent Document 1 discloses a PAS composition containing a PAS resin, glass fibers surface-treated with a bundling agent containing an epoxy resin, a urethane resin, and a silane coupling agent, a silane coupling agent having at least one functional group selected from the group consisting of an amino group and an epoxy group, and synthetic zeolite. However, in this technology, a certain degree of improvement in hot water resistance was only obtained in a hot water resistance evaluation using a long-life coolant, which is generally unlikely to reduce the mechanical strength of the glass fiber-reinforced PAS resin composition, and in addition, there was a problem that the moldability (mold releasability) of the resin composition was deteriorated due to the influence of the bundling agent and the silane coupling agent. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-132710 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the problem to be solved by the present invention is to provide a PAS molded article having excellent moist heat resistance and hot water resistance, a PAS resin composition having excellent moldability capable of providing such a molded article, and a method for producing the same. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the inventors have discovered that by blending specific amounts of glass fiber, a silane coupling agent having a specific structure, and poorly water-soluble glass with a PAS resin, the resulting resin composition and molded article exhibit excellent processability, moist heat resistance, and hot water resistance, and have thus completed the present invention.

[0008] That is, the present disclosure provides a PAS resin composition comprising a PAS resin (A), a glass fiber (B), a silane coupling agent (C), and a poorly water-soluble glass (D) as essential components, the glass fiber (B) is mixed in an amount of 10 to 50 parts by mass, the silane coupling agent (C) is mixed in an amount of 0.1 to 3.5 parts by mass, and the poorly water-soluble glass (D) is mixed in an amount of 0.1 to 10 parts by mass, relative to 100 parts by mass of the PAS resin (A); The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound; and The present invention relates to a PAS resin composition, wherein the poorly water-soluble glass (D) is a glass containing silver and / or zinc, and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2, and ZrO2.

[0009] The present disclosure also relates to a PAS resin molded article obtained by molding the above-described PAS resin composition.

[0010] The present disclosure also provides a method for producing a PAS resin composition, comprising a step of blending a PAS resin (A), a glass fiber (B), a silane coupling agent (C), and a poorly water-soluble glass (D) as essential components, and melt-kneading the blend at a temperature equal to or higher than the melting point of the PAS resin (A), the glass fiber (B) is mixed in an amount of 10 to 50 parts by mass, the silane coupling agent (C) is mixed in an amount of 0.1 to 3.5 parts by mass, and the silver ion-containing phosphate complex (D) is mixed in an amount of 0.1 to 10 parts by mass, relative to 100 parts by mass of the PAS resin (A); The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound; and The present invention relates to a method for producing a PAS resin composition, wherein the poorly water-soluble glass (D) is a glass containing silver and / or zinc and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2 and ZrO2.

[0011] The present disclosure also relates to a method for producing a molded article, comprising the steps of producing a PAS resin composition by the above-described production method and melt-molding the resulting PAS resin composition. Effect of the Invention

[0012] According to the present invention, it is possible to provide a PAS molded article having excellent moist heat resistance and hot water resistance, a PAS resin composition having excellent moldability capable of providing the molded article, and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described in detail, but the scope of the present invention is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present invention. In addition, when multiple upper and lower limit values ​​are described for a specific parameter, any upper and lower limit values ​​can be combined to form a suitable numerical range.

[0014] The PAS resin composition according to the present embodiment is a PAS resin composition comprising a PAS resin (A), a glass fiber (B), a silane coupling agent (C), and a poorly water-soluble glass (D) as essential components, the glass fiber (B) is mixed in an amount of 10 to 50 parts by mass, the silane coupling agent (C) is mixed in an amount of 0.1 to 3.5 parts by mass, and the poorly water-soluble glass (D) is mixed in an amount of 0.1 to 10 parts by mass, relative to 100 parts by mass of the PAS resin (A); The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound, and the water-insoluble glass (D) is a glass containing silver and / or zinc and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2, and ZrO2. Hereinafter, it will be described.

[0015] <PAS resin (A)> The PAS resin composition according to this embodiment is prepared by blending a PAS resin (A) as an essential component.

[0016] The PAS resin has a resin structure having a structure in which an aromatic ring and a sulfur atom are bonded as a repeating unit. Specifically, the following general formula (1)

[0017]

Chemical formula

[0018]

Chemical formula

[0019] Here, the structural part represented by the general formula (1) is particularly R 1 and R 2is preferably a hydrogen atom from the viewpoint of the mechanical strength of the PAS resin, and in that case, examples include those bonded at the para position represented by the following formula (3) and those bonded at the meta position represented by the following formula (4).

[0020] [ka] Among these, a structure in which the bond between the sulfur atom and the aromatic ring in the repeating unit is at the para position represented by the general formula (3) is particularly preferred in terms of the heat resistance and crystallinity of the PAS resin.

[0021] The PAS resin may include not only the structural moieties represented by the general formula (1) or (2) but also the structural moieties represented by the following structural formulae (5) to (8):

[0022] [ka] The structural moieties represented by the general formulae (1) and (2) may account for 30 mol % or less of the total of the structural moieties represented by the general formulae (1) and (2). In particular, in the present disclosure, it is preferable that the structural moieties represented by the general formulae (5) to (8) account for 10 mol % or less in terms of the heat resistance and mechanical strength of the PAS resin. When the PAS resin contains the structural moieties represented by the general formulae (5) to (8), the bonding mode thereof may be either a random copolymer or a block copolymer.

[0023] The PAS resin may have naphthyl sulfide bonds or the like in its molecular structure, but the amount of such bonds is preferably 3 mol % or less, and particularly preferably 1 mol % or less, relative to the total number of moles including other structural portions.

[0024] The physical properties of the PAS resin (A) used in the present embodiment are not particularly limited as long as they do not impair the effects of the present invention, and are as follows.

[0025] (Melt Viscosity) The melt viscosity of the PAS resin (A) used in this embodiment is not particularly limited, but in order to obtain a good balance between processability and mechanical strength, the melt viscosity (V6) measured at 300°C is preferably in the range of 2 Pa·s or more, and preferably in the range of 1000 Pa·s or less, more preferably in the range of 500 Pa·s or less, and further preferably in the range of 300 Pa·s or less. However, the melt viscosity (V6) is measured by using a Shimadzu flow tester, CFT-500D, at 300°C, load: 1.96×10 6 The melt viscosity is measured after holding the sample for 6 minutes at a pressure of 1 Pa and L / D = 10 (mm) / 1 (mm).

[0026] (Non-Newtonian Exponents) The non-Newtonian index of the PAS resin (A) used in this embodiment is not particularly limited, but is preferably in the range of 0.90 or more to 2.00 or less. When a linear PAS resin is used, the non-Newtonian index is preferably in the range of 0.90 or more, more preferably in the range of 0.95 or more to preferably in the range of 1.50 or less, more preferably in the range of 1.20 or less. Such a PAS resin is excellent in mechanical properties, fluidity, and abrasion resistance. However, in this disclosure, the non-Newtonian index (N value) is a value calculated using the following formula by measuring the shear rate (SR) and shear stress (SS) using a capillograph under the conditions of melting point +20°C and the ratio of the orifice length (L) to the orifice diameter (D) L / D=40. The closer the non-Newtonian index (N value) is to 1, the closer the structure is to a linear structure, and the higher the non-Newtonian index (N value), the more branched the structure is.

[0027]

number

[0028] (Terminal carboxyl group amount) The amount of terminal carboxy groups in the PAS resin (A) used in this embodiment is not particularly limited, but is preferably in the range of 10 μmol / g or more, more preferably in the range of 20 μmol / g or more, and preferably in the range of 180 μmol / g or less, more preferably in the range of 160 μmol / g or less. In such a range, the obtained composite structure has excellent mechanical properties, which is preferable. In this disclosure, the amount of terminal carboxy groups in the PAS resin (A) is measured at 630.6 cm in the infrared absorption spectrum measured with a Fourier transform infrared spectrometer. -1 Absorbance at 1705cm -1 The value was calculated from the relative intensity of absorbance.

[0029] (Manufacturing method) The method for producing the PAS resin (A) is not particularly limited, and examples thereof include (production method 1) a method in which a dihalogeno aromatic compound is polymerized in the presence of sulfur and sodium carbonate, and if necessary, a polyhalogeno aromatic compound or other copolymerization component is added, (production method 2) a method in which a dihalogeno aromatic compound is polymerized in a polar solvent in the presence of a sulfidizing agent or the like, and if necessary, a polyhalogeno aromatic compound or other copolymerization component is added, (production method 3) a method in which p-chlorothiophenol is added, and if necessary, other copolymerization components are added, and self-condensation is performed, and (production method 4) a method in which a diiodo aromatic compound and elemental sulfur are melt-polymerized under reduced pressure in the presence of a polymerization inhibitor that may have a functional group such as a carboxyl group or an amino group. Among these methods, (production method 2) is preferred because it is versatile. During the reaction, an alkali metal salt of a carboxylic acid or sulfonic acid or an alkali hydroxide may be added to adjust the degree of polymerization. Among the above-mentioned (Production Method 2) methods, there is a method for producing a PAS resin by introducing a water-containing sulfidizing agent into a mixture containing a heated organic polar solvent and a dihalogeno aromatic compound at a rate at which water can be removed from the reaction mixture, and reacting the dihalogeno aromatic compound and the sulfidizing agent in the organic polar solvent, and optionally adding a polyhalogeno aromatic compound, and controlling the amount of water in the reaction system to within a range of 0.02 to 0.5 mol per mol of the organic polar solvent (see JP-A-07-228699). Particularly preferred is a method in which a dihalogenoaromatic compound and, if necessary, a polyhalogenoaromatic compound or other copolymerization component are added in the presence of an alkali metal sulfide and an aprotic polar organic solvent, and an alkali metal hydrosulfide and an organic acid alkali metal salt are reacted while controlling the organic acid alkali metal salt in the range of 0.01 to 0.9 mol per mol of the sulfur source and the amount of water in the reaction system to be 0.02 mol or less per mol of the aprotic polar organic solvent (see WO2010 / 058713 pamphlet).Specific examples of the dihalogenoaromatic compound include p-dihalobenzene, m-dihalobenzene, o-dihalobenzene, 2,5-dihalotoluene, 1,4-dihalonaphthalene, 1-methoxy-2,5-dihalobenzene, 4,4'-dihalobiphenyl, 3,5-dihalobenzoic acid, 2,4-dihalobenzoic acid, 2,5-dihalonitrobenzene, 2,4-dihalonitrobenzene, 2,4-dihaloanisole, p,p'-dihalodiphenyl ether, 4,4'-dihalobenzophenone, 4,4'-di Examples of the polyhalogeno aromatic compounds include 1,2,3-trihalobenzene, 1,2,4-trihalobenzene, 1,3,5-trihalobenzene, 1,2,3,5-tetrahalobenzene, 1,2,4,5-tetrahalobenzene, 1,4,6-trihalonaphthalene, etc. The halogen atoms contained in the above compounds are preferably chlorine atoms or bromine atoms.

[0030] The method for post-treating the reaction mixture containing the PAS resin obtained by the polymerization step is not particularly limited, but for example, (post-treating 1) after the completion of the polymerization reaction, first, the solvent is distilled off under reduced pressure or normal pressure, either as is or after the addition of an acid or base, and then the solid matter remaining after the solvent distillation is washed once or twice or more times with a solvent such as water, the reaction solvent (or an organic solvent having a similar solubility to the low molecular weight polymer), acetone, methyl ethyl ketone, or alcohols, and then neutralized, washed with water, filtered, and dried; or (post-treating 2) after the completion of the polymerization reaction, the reaction mixture is dissolved in a solvent such as water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, or aliphatic hydrocarbons (soluble in the polymerization solvent used and poorly soluble in at least PAS). or (post-treatment 3) a method in which, after the completion of the polymerization reaction, a reaction solvent (or an organic solvent having a solubility equivalent to that of the low molecular weight polymer) is added to the reaction mixture, the mixture is stirred, the mixture is filtered to remove the low molecular weight polymer, the mixture is washed once or twice or more times with a solvent such as water, acetone, methyl ethyl ketone, or an alcohol, and then the mixture is neutralized, washed with water, filtered, and dried; (post-treatment 4) a method in which, after the completion of the polymerization reaction, water is added to the reaction mixture, the mixture is washed with water, filtered, and if necessary, an acid is added during the water washing to perform an acid treatment, and then the mixture is dried; or (post-treatment 5) a method in which, after the completion of the polymerization reaction, the reaction mixture is filtered, and if necessary, the mixture is washed once or twice or more times with the reaction solvent, and then the mixture is washed with water, filtered, and dried.

[0031] In the post-treatment methods exemplified above in (Post-treatment 1) to (Post-treatment 5), the PAS resin may be dried in a vacuum, or in air or in an inert gas atmosphere such as nitrogen.

[0032] <Glass fiber (B)> The PAS resin composition according to the present embodiment contains glass fiber (B) as an essential component for the purpose of improving mechanical properties. The glass fiber (B) may be any fiber known to those skilled in the art, and the fiber diameter, fiber length, aspect ratio, and the like may be appropriately adjusted depending on the application of the molded article. By including the glass fiber (B), a PAS resin composition having excellent moldability and mechanical properties of the resulting PAS molded article can be obtained.

[0033] The glass fiber (B) may be processed with a surface treatment agent or a sizing agent. This is preferable because it can improve the adhesive strength with the PAS resin. Examples of the surface treatment agent or sizing agent include at least one polymer selected from the group consisting of silane compounds having functional groups such as amino groups, epoxy groups, isocyanate groups, and vinyl groups, titanate compounds, acrylic resins, urethane resins, polyether resins, and epoxy resins, and those containing urethane resins are preferable from the viewpoint of suppressing excessive defibration during processing. When the surface treatment agent or sizing agent contains a urethane resin, the content is not particularly limited, but from the viewpoint of moldability, it is preferably in the range of 35 parts by mass or less, and more preferably in the range of 20 parts by mass or less. In addition, it is preferable to contain a polyether resin and an epoxy resin from the viewpoint of obtaining high moist heat resistance. When the surface treatment agent or sizing agent contains a polyether resin and an epoxy resin, the total content is not particularly limited, but from the viewpoint of moldability, it is preferably in the range of 65 parts by mass or more, and more preferably in the range of 80 parts by mass or more.

[0034] The blending ratio of the glass fiber (B) is not particularly limited within the range in which the effects of the present invention are exhibited, but from the viewpoint of obtaining better mechanical properties, particularly tensile properties and impact resistance properties, it is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and particularly preferably 40 parts by mass or more, relative to 100 parts by mass of the PAS resin (A). Also, from the viewpoint of obtaining better flowability and processability of the resin composition and surface smoothness of the molded product, it is preferably 150 parts by mass or less, more preferably 130 parts by mass or less, and even more preferably 110 parts by mass or less, relative to 100 parts by mass of the PAS resin.

[0035] <Silane coupling agent (C)> The PAS resin composition according to this embodiment contains a silane coupling agent (C) as an essential component for the purpose of improving mechanical properties, moist heat resistance, and hot water resistance.

[0036] Silane coupling agents used in the present embodiment are preferably silane coupling agents having an epoxy group, an isocyanato group, or a hydroxyl group. Examples of such silane coupling agents include epoxy group-containing alkoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, isocyanato group-containing alkoxysilane compounds such as γ-isocyanatopropyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, γ-isocyanatopropylmethyldimethoxysilane, γ-isocyanatopropylmethyldiethoxysilane, γ-isocyanatopropylethyldimethoxysilane, γ-isocyanatopropylethyldiethoxysilane, and γ-isocyanatopropyltrichlorosilane, and hydroxyl group-containing alkoxysilane compounds such as γ-hydroxypropyltrimethoxysilane and γ-hydroxypropyltriethoxysilane. These compounds can be used alone or in combination of two or more. In addition, since amino group-containing alkoxysilane compounds such as γ-aminopropyltrimethoxysilane impair the moldability of the resin composition, it is preferable to avoid using them (not to add them) in the present disclosure.

[0037] The amount of the silane coupling agent (C) is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and preferably 4 parts by mass or less, relative to 100 parts by mass of the PAS resin (A). In this range, the resin composition exhibits good processability and further improves mechanical strength, especially tensile properties, which is preferable.

[0038] <Poorly Water-Soluble Glass (D)> The PAS resin composition according to this embodiment contains water-insoluble glass (D) (hereinafter, sometimes simply referred to as "glass (D)") as an essential component for the purpose of improving the wet heat resistance and hot water resistance. In this disclosure, water-insoluble glass refers to a property in which the components contained in the glass dissolve in water and gradually dissolve (release) in the form of ions, and for example, the cumulative amount of metal ions dissolved per immersion time (1 h) is in the range of 0.00001 to 0.001 (mg / g glass) or less.

[0039] The poorly water-soluble glass applicable to this embodiment is a glass containing, as essential components, silver and / or zinc and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2, and ZrO2. When glass (D) applicable to this embodiment contains silver, it is preferable that the glass contains 0.01 to 10 parts by mass of silver, and when glass (D) contains zinc, it is preferable that the glass contains 30 to 65 parts by mass of zinc. In addition, it is preferable that the glass contains 10 to 50 parts by mass of at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2, and ZrO2.

[0040] Glass (D) contains at least one component selected from the group consisting of B2O3, Al2O3, SiO2 and ZrO as an essential component, but may also contain Na2O, K2O, CaO, MgO and P2O5. Increasing the proportions of Na2O, K2O and P2O5 tends to increase the dissolution of ions into water, while increasing the proportions of MgO, CaO, Al2O3, SiO2 and ZrO tends to decrease the dissolution of ions, so the proportions may be adjusted appropriately in consideration of the degree of dissolution into water. For example, the cumulative amount of silver ions dissolved per immersion time (1 h) can be adjusted to be in the range of 0.00001 to 0.001 (mg / 1 g glass).

[0041] The maximum particle size of the glass (D) applicable to this embodiment is not particularly limited as long as it does not impair the effects of the present invention, but from the viewpoint of excellent mechanical strength, fluidity, and surface appearance, it is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. The maximum particle size referred to here is the particle size at 98% of the cumulative particle size distribution curve (D 98 ).

[0042] The blending amount of the above glass (D) is preferably 0.1 part by mass or more, more preferably 0.3 part by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, based on 100 parts by mass of the PAS resin (A). By blending the amount of glass (D) within such range, a molded product having excellent resistance to moist heat and hot water, as well as excellent moldability and mechanical strength can be obtained.

[0043] Such glass (D) may be a commercially available product, for example, "Novalon VZ100", "Novalon VZF101", "Novalon VZF200", "Novalon VZF300", "Novalon VZN300", "Novalon VAG500", "Novalon VZ600", "Novalon VZ900", "Novalon AG100", "Novalon AG300", "Novalon AG1100", "Novalon AGZ010", "Novalon AGZ020", "Novalon AGZ330", "Novalon AGZ330N", "Novalon AGT330", "Novalon VFA701" (Toagosei Co., Ltd.), "ZF-0", "DL-7500", "DL-7700", "DL-7900" (Nippon Electric Glass Co., Ltd.), etc. These may be used alone or in combination.

[0044] The PAS resin composition according to the present embodiment may contain fillers other than the above-mentioned glass fiber (B) and glass (D) (hereinafter referred to as other fillers) as optional components within a range that does not impair the effects of the present invention. For example, fillers of various shapes such as fibrous, plate-like, and powder-like can be used. Specific examples include polyamide fiber, carbon fiber, glass flakes, milled fiber, clay, pyrophyllite, bentonite, sericite, mica, talc, attapulgite, ferrite, calcium silicate, zeolite, boehmite, silica, quartz powder, glass beads, glass powder, calcium silicate, aluminum silicate, silicates such as diatomaceous earth, iron oxide, titanium oxide, zinc oxide, and alumina, metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, fumed silica, and other plant-derived fillers such as silicon carbide, silicon nitride, boron nitride, and various metal powders can be used in combination in the present invention. Among them, hydrotalcite, calcium carbonate, talc, zinc carbonate, alumina, magnesium hydroxide, boron nitride, and magnesium carbonate can be preferably used. The size and aspect ratio can be appropriately adjusted depending on the application of the molded product.

[0045] In this embodiment, the other filler is not an essential component, but when it is blended, the blending amount is not particularly limited as long as it does not impair the effect of the present invention. The blending amount of the other filler is, for example, preferably 1 part by mass or more, more preferably 5 parts by mass or more, and preferably 600 parts by mass or less, more preferably 200 parts by mass or less, relative to 100 parts by mass of the PAS resin (A). In such a range, the resin composition shows good moldability, and the molded product has excellent mechanical properties, so it is preferable.

[0046] <Thermoplastic elastomer (E)> The PAS resin composition according to the present embodiment may contain a thermoplastic elastomer (E) as an optional component, if necessary. Examples of the thermoplastic elastomer (E) include polyolefin-based elastomers, fluorine-based elastomers, and silicone-based elastomers, among which polyolefin-based elastomers are preferred. When these elastomers are added, the amount of the elastomers is not particularly limited as long as it does not impair the effects of the present invention, but is preferably in the range of 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, to preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the PAS resin (A). In this range, the impact resistance of the resulting PAS resin composition is improved, which is preferable.

[0047] For example, the polyolefin-based elastomer may be a homopolymer of an α-olefin, a copolymer of two or more α-olefins, or a copolymer of one or more α-olefins and a vinyl polymerizable compound having a functional group. In this case, the α-olefin may be an α-olefin having 2 or more carbon atoms and 8 or less, such as ethylene, propylene, or 1-butene. In addition, the functional group may be a carboxyl group, an acid anhydride group (-C(=O)OC(=O)-), an epoxy group, an amino group, a hydroxyl group, a mercapto group, an isocyanate group, or an oxazoline group. Examples of the vinyl polymerizable compound having the functional group include one or more of vinyl acetate, α,β-unsaturated carboxylic acids such as (meth)acrylic acid, alkyl esters of α,β-unsaturated carboxylic acids such as methyl acrylate, ethyl acrylate, and butyl acrylate, metal salts of α,β-unsaturated carboxylic acids such as ionomers (metals include alkali metals such as sodium, alkaline earth metals such as calcium, and zinc, etc.), glycidyl esters of α,β-unsaturated carboxylic acids such as glycidyl methacrylate, and the like, α,β-unsaturated dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid, and derivatives of the α,β-unsaturated dicarboxylic acids (monoesters, diesters, and acid anhydrides), etc. The above-mentioned thermoplastic elastomers (E) may be used alone or in combination of two or more.

[0048] Furthermore, in addition to the above components, the PAS resin composition according to the present embodiment may further contain synthetic resins such as polyester resin, polyamide resin, polyimide resin, polyetherimide resin, polycarbonate resin, polyphenylene ether resin, polysulfone resin, polyethersulfone resin, polyaryletherketone resin, polyetheretherketone resin, polyetherketone resin, polyarylate resin, polyethylene resin, polypropylene resin, polyethylenetetrafluoroethylene resin, polyethylenedifluoroethylene resin, polystyrene resin, ABS resin, epoxy resin, phenol resin, urethane resin, and liquid crystal polymer as optional components depending on the application. The synthetic resin is not an essential component in the present invention, but when it is added, the ratio of the synthetic resin is not particularly limited as long as it does not impair the effects of the present invention, and it differs depending on each purpose and cannot be generally defined, but the ratio of the synthetic resin to be added in the resin composition according to the present invention is, for example, in the range of 5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of PAS resin (A). In other words, the ratio of the PAS resin to the total of the PAS resin (A) and the synthetic resin is preferably in the range of (100 / 115) or more, and more preferably in the range of (100 / 105) or more, on a mass basis.

[0049] In addition, the PAS resin composition according to the present embodiment may contain other known and commonly used additives as optional components, such as colorants, antistatic agents, antioxidants, heat stabilizers, UV stabilizers, UV absorbers, foaming agents, flame retardants, flame retardant assistants, rust inhibitors, and release agents (metal salts or esters of fatty acids having 18 to 30 carbon atoms, including stearic acid or montanic acid, polyolefin waxes such as polyethylene, etc.) as needed. These additives are not essential components, and may be used in an amount of, for example, preferably 0.01 parts by mass or more, and preferably 1000 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the PAS resin (A), as appropriate for the purpose or use so as not to impair the effects of the present invention.

[0050] <Method for producing PAS resin composition> The method for producing a PAS resin composition according to this embodiment is a method for producing a PAS resin composition comprising, as essential components, a PAS resin (A), glass fibers (B), a silane coupling agent (C), and hardly water-soluble glass (D), and having a step of melt-kneading at a temperature equal to or higher than the melting point of the PAS resin (A). Based on 100 parts by mass of the PAS resin (A), 10 to 50 parts by mass of the glass fibers (B), 0.1 to 3.5 parts by mass of the silane coupling agent (C), and 0.1 to 10 parts by mass of the silver ion-containing phosphate composite (D) are blended. The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound, and The hardly water-soluble glass (D) is characterized by being a glass containing silver and / or zinc and at least one oxide selected from the group consisting of B2O3, Al2O3, SiO2, and ZrO2. This will be described in detail below.

[0051] The method for producing a PAS resin composition according to this embodiment has a step of blending the above essential components and melt-kneading in a temperature range equal to or higher than the melting point of the PAS resin (A). More specifically, the PAS resin composition according to this embodiment is obtained by blending each essential component and, if necessary, other optional components. The method for producing the resin composition used in the present invention is not particularly limited, but a method of blending essential components and optional components as necessary and melt-kneading, more specifically, a method of uniformly dry-blending with a tumbler or a Henschel mixer as necessary and then charging into a twin-screw extruder for melt-kneading can be mentioned.

[0052] The melt-kneading can be carried out by heating to a temperature in the range where the resin temperature is equal to or higher than the melting point of the PAS resin (A), preferably in the range of the melting point + 10°C or higher, more preferably the melting point + 10°C or higher, still more preferably the melting point + 20°C or higher, and preferably up to the melting point + 100°C or lower, more preferably the melting point + 50°C or lower.

[0053] As the melt kneader, a twin-screw kneading extruder is preferable from the viewpoints of dispersibility and productivity. For example, it is preferable to perform melt kneading while appropriately adjusting the range of the discharge amount of the resin component to 5 to 500 (kg / hr) and the range of the screw rotation speed to 50 to 500 (rpm), and it is more preferable to perform melt kneading under the condition that the ratio thereof (discharge amount / screw rotation speed) is in the range of 0.02 to 5 (kg / hr / rpm). Further, the addition and mixing of each component to the melt kneader may be performed simultaneously or separately. For example, when adding glass fiber (B) as an essential component and other fibrous fillers as necessary among the above components, it is preferable from the viewpoint of dispersibility to introduce them into the extruder from the side feeder of the twin-screw kneading extruder. The position of such a side feeder is preferably such that the ratio of the distance from the resin charging part (top feeder) of the twin-screw kneading extruder to the side feeder to the total length of the screw of the twin-screw kneading extruder is 0.1 or more, and more preferably 0.3 or more. Further, it is preferable that such a ratio is 0.9 or less, and more preferably 0.7 or less.

[0054] The PAS resin composition according to this embodiment obtained by such melt kneading is a molten mixture containing the above essential components, optional components added as necessary, and their derived components. Therefore, the PAS resin composition according to this embodiment has a morphology in which the PAS resin (A) forms a continuous phase and other essential components and optional components are dispersed.

[0055] The PAS resin composition according to this embodiment, after the melt kneading, is preferably processed into forms such as pellets, chips, granules, powders, etc. by a known method, for example, by extruding the resin composition in a molten state into strands, and then, if necessary, pre-drying is performed in a temperature range of 100 to 150°C.

[0056] <PAS resin molded article, method for manufacturing PAS resin molded article> The molded article according to this embodiment is produced by melt molding the PAS resin composition. The manufacturing method of the molded article according to this embodiment includes a step of melt molding the PAS resin composition. Therefore, the molded article according to this embodiment has a morphology in which the PAS resin (A) forms a continuous phase and other essential components and optional components are dispersed. The PAS resin composition having such a morphology allows the production of a molded article having excellent thermal conductivity and mechanical strength.

[0057] The PAS resin composition according to the present embodiment can be subjected to various molding processes such as injection molding, compression molding, extrusion molding of composites, sheets, pipes, pultrusion molding, blow molding, and transfer molding, but is particularly suitable for injection molding because of its excellent releasability. When molding by injection molding, various molding conditions are not particularly limited, and molding can be performed by a normal general method. For example, in an injection molding machine, the PAS resin composition is melted at a resin temperature in a temperature range of the melting point of the PAS resin (A) or higher, preferably in a temperature range of the melting point +10°C or higher, more preferably in a temperature range of the melting point +10°C to the melting point +100°C, and even more preferably in a temperature range of the melting point +20 to the melting point +50°C, and then the resin is injected into a mold from a resin discharge port and molded. At that time, the mold temperature may also be set to a known temperature range, for example, room temperature (23°C) to 300°C, preferably 130 to 190°C.

[0058] The method for producing a molded article according to this embodiment may include a step of annealing the molded article. The optimum conditions for the annealing treatment are selected depending on the application or shape of the molded article, and the annealing temperature is in a temperature range of the glass transition temperature of the PAS resin (A) or higher, preferably in a temperature range of the glass transition temperature +10°C or higher, and more preferably in a temperature range of the glass transition temperature +30°C or higher. On the other hand, it is preferably in a range of 260°C or lower, and more preferably in a range of 240°C or lower. The annealing time is not particularly limited, but is preferably in a range of 0.5 hours or higher, and more preferably in a range of 1 hour or higher. On the other hand, it is preferably in a range of 10 hours or lower, and more preferably in a range of 8 hours or lower. In such a range, not only the distortion of the molded article obtained is reduced and the crystallinity of the resin is improved, but also the thermal conductivity, mechanical properties, and chemical resistance are further improved, which is preferable. The annealing treatment may be performed in air, but is preferably performed in an inert gas such as nitrogen gas.

[0059] The resin composition and molded article of the present disclosure, which contain the above essential components, are excellent in hot water resistance and wet heat resistance. In the present disclosure, wet heat resistance refers to the property of suppressing the decrease in physical properties in a high humidity and high temperature environment, and hot water resistance refers to the property of suppressing the decrease in physical properties when contacted with a high temperature aqueous solution. The reason why such an effect is obtained is not necessarily clear, but it is presumed to be due to the following mechanism. First, water molecules that have penetrated into the bulk of the resin composition in a wet heat environment or in hot water dissolve silver ions and zinc ions contained in the poorly water-soluble glass (D). These metal ions suppress the hydrolysis and decrease in adhesion of the interface between the PAS resin (A) and the glass fiber (B) and the silane coupling agent (C), thereby suppressing the decrease in physical properties. Therefore, in a composition containing a small amount of glass fiber, the effect of adding the poorly soluble glass to improve physical properties such as wet heat resistance and hot water resistance is small, and conversely, the effect of the poorly soluble glass (D) is greater when the amount of glass fiber is large. It should be noted that the above mechanism is merely speculation, and even if the effects of the present invention are achieved for other reasons, they are still included in the technical scope of the present invention.

[0060] The PAS resin molded product according to the present embodiment is characterized by excellent hot water resistance and moist heat resistance, and is therefore particularly suitable for parts that come into contact with fluids and their vapors. Examples include pipes, lining pipes, cap nuts, pipe joints (elbows, headers, tees, reducers, joints, couplers, etc.), various valves, flow meters, gaskets (seals, packings), and other piping and various parts attached to piping for transporting fluids. More specifically, the PAS resin molded product can be suitably used for water-related parts such as water heaters, bath water volume and temperature sensors, and vehicle fuel parts such as fuel tanks, fuel tubes, fuel sensors, fuel pumps, vane pumps, and auto-ratio flow meters. The molded product according to the present embodiment can be not only the above-mentioned, but also the following ordinary resin molded products. For example, protective and supporting materials for box-shaped electric and electronic component integrated modules, multiple individual semiconductors or modules, sensors, LED lamps, connectors, sockets, resistors, relay cases, switches, coil bobbins, capacitors, variable capacitor cases, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, terminal blocks, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, motor brush holders, parabolic antennas, computer-related parts, and other representative electric and electronic parts; VTR parts, television parts, irons, headsets, etc. Home and office electrical appliance parts such as air dryers, rice cooker parts, microwave oven parts, audio parts, audio / visual equipment parts such as laser discs, compact discs, DVD discs, and Blu-ray discs, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, and water-related equipment parts such as water heaters, bath water volume and temperature sensors; office computer related parts, telephone related parts, facsimile related parts, copier related parts, cleaning jigs, motor parts, lighters, typewriters, and other machine related parts; optical equipment and precision machinery related parts such as microscopes, binoculars, cameras, and watches;Alternator terminals, alternator connectors, brush holders, slip rings, IC regulators, potentiometer bases for light dimmers, relay blocks, inhibitor switches, various valves such as exhaust gas valves, various pipes for fuel, exhaust and intake systems, air intake nozzle snorkels, intake manifolds, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, temperature sensors, air flow meters, brake pad wear sensors, thermostat bases for air conditioners, heating hot air flow control valves, radiators Examples of automotive and vehicle related parts include brush holders for motors, water pump impellers, turbine vanes, wiper motor related parts, distributors, starter switches, ignition coils and bobbins, motor insulators, motor rotors, motor cores, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, coils for fuel-related electromagnetic valves, fuse connectors, horn terminals, electrical component insulating plates, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil filters, ignition device cases, and other various applications. EXAMPLES

[0061] The present invention will be described below using examples and comparative examples, but is not limited to these examples. In the following, unless otherwise specified, "%" and "parts" are based on mass.

[0062] <Examples 1 to 10 and Comparative Examples 1 to 10> Each material was mixed according to the composition and mixing amounts shown in Table 1. Then, these mixed materials were fed into a vented twin screw extruder "TEX-30α (product name)" manufactured by Japan Steel Works, Ltd., and melt-kneaded at a resin component discharge rate of 30 kg / hr, a screw rotation speed of 200 rpm, and a set resin temperature of 320°C to obtain pellets of the resin composition. The glass fiber was fed from the side feeder (S / T ratio 0.5), and the other materials were mixed uniformly in a tumbler in advance and fed from the top feeder. The pellets of the obtained resin composition were dried in a gear oven at 140°C for 2 hours, and then injection molded to prepare various test pieces, and the following tests were performed.

[0063] <Evaluation>

[0064] (1) Evaluation of formability The moldability (mold releasability) of each resin composition of each Example and Comparative Example was evaluated by injection molding using a single-gate ISO TYPE-A dumbbell piece mold. The cylinder temperature of the injection molding machine was set to 310°C, and the mold temperature was set to 150°C. For the evaluation, pellets of the resin composition were injected into a mold, held for 15 seconds or more to solidify, and then the mold was opened to check whether the dumbbell pieces stuck to the mold. Injection molding was performed 20 times, and evaluation was performed according to the following criteria. The results are shown in Tables 1 and 2. 〇: It does not stick to the mold and molding can be done continuously. ×: Sticks to the mold 1 to 20 times, making it impossible to mold continuously

[0065] (2) Measurement of tensile properties The pellets obtained in each Example and Comparative Example were fed to a Sumitomo Heavy Industries injection molding machine (SE-75D-HP) with a cylinder temperature set to 310°C, and injection molding was performed using an ISO Type 1A dumbbell specimen molding die with a mold temperature controlled to 150°C to obtain an ISO Type-1A dumbbell-shaped test specimen. The resin was injected from a single gate so that the test specimen did not include a welded portion. The tensile strength of the obtained test specimen was measured using a measurement method based on ISO 527-1 and 2. The results are shown in Tables 1 and 2.

[0066] (3) Evaluation of hot water resistance Test pieces prepared under the same conditions as in (2) were sealed in an autoclave together with water and left at a temperature of 90°C or 120°C for 1000 hours. The test pieces were then slowly cooled to room temperature, and their tensile strength (MPa) was measured in the same manner as in (2). From the obtained values, the strength retention rates (tensile strength after being left in hot water / tensile strength before being left in hot water × 100 (%)) were calculated. The measured values ​​and calculated retention rates are shown in Tables 1 and 2.

[0067] (4) Evaluation of humidity and heat resistance Test pieces prepared under the same conditions as in (2) were left for 1000 hours under high temperature and high humidity conditions at a temperature of 121°C and a humidity of 100%. The test pieces were then slowly cooled to room temperature, and their tensile strength (MPa) was measured in the same manner as in (2). From the obtained values, the strength retention rates (tensile strength after leaving under high temperature and high humidity conditions / tensile strength before leaving under high temperature and high humidity conditions × 100 (%)) were calculated. The measured values ​​and calculated retention rates are shown in Tables 1 and 2.

[0068] [Table 1]

[0069] [Table 2]

[0070] The blending ratios of the blended components in Tables 1 and 2 are as follows: ·PAS resin (A) A-1: PPS resin, linear type, melt viscosity (V6) 106 Pa·s, terminal carboxyl group amount 33 μmol / g, non-Newtonian index 1.07 Glass fiber (B) B-1: "CS03T-717H" manufactured by Nippon Electric Glass Co., Ltd., average fiber length 3.5 mm, average fiber diameter 10 μm, silane coupling agent (C) C-1: Trimethoxyepoxysilane "KBM-403" manufactured by Shin-Etsu Chemical Co., Ltd. C-2: Triethoxyaminosilane "KBE-904" manufactured by Shin-Etsu Chemical Co., Ltd. Poorly water-soluble glass (D) D-1: "Novalon VZ100" manufactured by Toagosei Co., Ltd., average particle size 5 μm D-2: "ZF-0" manufactured by Nippon Electric Glass Co., Ltd., average particle size 10 μm D-3: "Novalon VAG500" manufactured by Toagosei Co., Ltd., average particle size 8 μm Thermoplastic elastomer (E) E-1: Sumitomo Chemical Co., Ltd. Subsidiary "Bond First 7L" ·Optional ingredients F-1: Calcium carbonate, average particle size 22 μm F-2: Potters Barotini glass beads "EBG731B", average particle size 18μm F-3: Glass frit "CY5600M1" manufactured by Takara Standard Co., Ltd., average particle size 15 μm

[0071] In Tables 1 and 2, comparing the Examples with Comparative Examples 1, 7, 8, and 10, it was shown that by blending poorly water-soluble glass in the composition, the molded product obtained exhibited high moist heat resistance and hot water resistance. Comparing the Examples with Comparative Examples 2-4, it was shown that when other inorganic fillers were used as a substitute for poorly water-soluble glass, the molded product had poor moist heat resistance and hot water resistance. Comparing the Examples with Comparative Examples 5-6, it was shown that the mechanical strength was poor because glass fiber was not blended. It was also shown that there was no effect of adding poorly water-soluble glass when glass fiber was not blended. Comparing the Examples with Comparative Example 9, it was shown that the moldability was poor when a silane coupling agent containing an amino group was blended.

Claims

1. A polyarylene sulfide resin composition comprising a polyarylene sulfide resin (A), a glass fiber (B), a silane coupling agent (C), and a poorly water-soluble glass (D) as essential components, the glass fiber (B) is mixed in an amount of 10 to 50 parts by mass, the silane coupling agent (C) is mixed in an amount of 0.1 to 3.5 parts by mass, and the poorly water-soluble glass (D) is mixed in an amount of 0.1 to 10 parts by mass, relative to 100 parts by mass of the polyarylene sulfide resin (A); The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound; and The water-insoluble glass (D) is made of silver and / or zinc and B 2 O 3 , Al 2 O 3 , SiO 2 and ZrO 2 and at least one oxide selected from the group consisting of:

2. The poorly water-soluble glass (D) further contains MgO and / or P 2 O 5 The polyarylene sulfide resin composition according to claim 1, which is a composite comprising:

3. A molded article obtained by melt molding the polyarylene sulfide resin composition according to claim 1 or 2.

4. A water-related part obtained by melt molding the polyarylene sulfide resin composition according to claim 1 or 2.

5. A method for producing a polyarylene sulfide resin composition, comprising a step of blending a polyarylene sulfide resin (A), a glass fiber (B), a silane coupling agent (C), and a poorly water-soluble glass (D) as essential components, and melt-kneading the blend at a temperature equal to or higher than the melting point of the polyarylene sulfide resin (A), the glass fiber (B) is mixed in an amount of 10 to 50 parts by mass, the silane coupling agent (C) is mixed in an amount of 0.1 to 3.5 parts by mass, and the silver ion-containing phosphate complex (D) is mixed in an amount of 0.1 to 10 parts by mass, relative to 100 parts by mass of the polyarylene sulfide resin (A); The silane coupling agent (C) is at least one selected from the group consisting of an epoxy group-containing alkoxysilane compound, an isocyanato group-containing alkoxysilane compound, and a hydroxyl group-containing alkoxysilane compound; and The water-insoluble glass (D) is made of silver and / or zinc and B 2 O 3 , Al 2 O 3 , SiO 2 and ZrO 2 and at least one oxide selected from the group consisting of:

6. The poorly water-soluble glass (D) further contains MgO and / or P 2 O 5 The method for producing a polyarylene sulfide resin composition according to claim 5, which is a composite comprising:

7. A method for producing a polyarylene sulfide resin molded product, comprising: a step of producing a resin composition by the production method according to claim 5 or 6; and a step of melt-molding the resin composition at a temperature equal to or higher than the melting point of the polyarylene sulfide resin (A).

Citation Information

Patent Citations

  • Polyarylene sulfide resin composition

    JP1998324804A

  • Antibacterial glass and resin composition containing the same

    JP2001226139A

  • Epoxy resin composition and resin-sealed semiconductor device

    JP2003252960A

  • Sheet molding compound

    JP2004182964A

  • Antibacterial polycarbonate resin composition

    JP2017132913A