Composition, adhesive, cured product and electronic component
The use of fumed silica and high-viscosity thiol compounds in epoxy resin compositions addresses the issue of bleeding during heat curing, enhancing adhesion and yield in electronic component manufacturing.
Patent Information
- Application Number
- JP2023051907
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional epoxy resin compositions used as adhesives tend to experience bleeding during heat curing, leading to contamination of unintended areas and reduced yield in electronic device manufacturing.
A composition comprising epoxy resin, fumed silica with dimethylsilyl or trimethylsilyl groups, a curing accelerator, and a thiol compound with a viscosity of 0.2 Pa·s or more at 25°C, which suppresses bleeding during heat treatment.
The composition effectively prevents bleeding, ensuring better adhesion and yield in electronic component assembly by maintaining composition integrity during heat curing.
Smart Images

Figure 2024140652000001 
Figure 2024140652000002 
Figure 2024140652000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composition, an adhesive, a cured product, and an electronic component. [Background technology]
[0002] Epoxy resins are used in various applications such as adhesives. For example, the following Patent Document 1 discloses a composition containing a specific epoxy resin, a specific thiol compound as a curing agent, a solid dispersion-type latent curing accelerator, and a borate ester compound. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-256013 Summary of the Invention [Problem to be solved by the invention]
[0004] When a conventional composition containing an epoxy resin is used as an adhesive or the like, the components contained in the composition may seep out from the applied portion of the composition. The phenomenon in which the components of the composition seep out is generally called bleeding. This bleeding problem becomes evident particularly when the composition is heated to harden. If bleeding occurs during heat hardening, the composition components will spread to areas that were not originally intended, which may lead to a decrease in yield in the manufacture of electronic devices and the like. For example, if bleeding occurs near wiring, the components that seep out from the composition may contaminate the wiring.
[0005] Objects of the present disclosure include providing an epoxy resin-containing composition that suppresses the occurrence of bleeding during heat treatment, providing an adhesive using the composition, providing a cured product of the composition, and providing an electronic component using the composition. [Means for solving the problem]
[0006] <1> A composition comprising an epoxy resin, fumed silica having at least one group selected from the group consisting of a dimethylsilyl group and a trimethylsilyl group, a curing accelerator, and a thiol compound having a viscosity of 0.2 Pa s or more at 25°C. <2> The viscosity of the thiol compound is within the range of 0.2 Pa s to 15 Pa s at 25°C. <1> The composition described in <3> The content of the fumed silica is within the range of 0.1% by mass to 20% by mass based on the total mass of the composition. <1> or <2> The composition described in <4> The content of the thiol compound is within the range of 1% by mass to 80% by mass based on the total mass of the composition. <1> ~ <3> 13. The composition according to any one of claims 1 to 12. <5> The thiol compound does not have a ring skeleton. <1> ~ <4> 13. The composition according to any one of claims 1 to 12. <6> The thiol compound has a ring skeleton. <1> ~ <4> 13. The composition according to any one of claims 1 to 12. <7> The thiol compound does not have an ester bond. <1> ~ <6> 13. The composition according to any one of claims 1 to 12. <8> <1> ~ <7> 2. An adhesive comprising the composition according to any one of claims 1 to 11. <9> <1> ~ <7> 2. A cured product of the composition according to claim 1. <10> <9> An electronic component comprising the cured product according to claim 1. Effect of the Invention
[0007] The present disclosure provides an epoxy resin-containing composition that suppresses the occurrence of bleeding during heat treatment, an adhesive using the composition, a cured product of the composition, and an electronic component using the composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present disclosure will be described in detail. At least one of the following embodiments may be modified as appropriate without departing from the spirit and scope of the present disclosure.
[0009] <Composition> The composition according to the present disclosure comprises the following components (A) to (D). (A) Epoxy resin (B) Fumed silica having at least one selected from the group consisting of dimethylsilyl groups and trimethylsilyl groups. (C) Curing accelerator (D) Thiol compounds that have a viscosity of 0.2 Pa·s or more at 25°C
[0010] The composition containing components (A) to (D) suppresses the occurrence of bleeding during heat treatment. This effect is presumed to be mainly due to the use of component (B) having a short-chain alkylsilyl group and component (D) having a relatively high viscosity. Component (D) showing a viscosity of 0.2 Pa·s or more at 25°C is considered to suppress the occurrence of bleeding at relatively low temperatures (e.g., room temperature). Compared with long-chain alkylsilyl groups such as octylsilyl groups, the movement of short-chain alkylsilyl groups such as dimethylsilyl groups and trimethylsilyl groups is small even at relatively high temperatures. Since the short-chain alkylsilyl groups of component (B) have a small effect on the viscosity of the composition during the temperature rise process, it is considered that bleeding is unlikely to occur even at relatively high temperatures. Therefore, the composition containing components (A) to (D) is considered to suppress the occurrence of bleeding, especially the occurrence of bleeding during heat treatment.
[0011] (Epoxy resin) The composition includes an epoxy resin. One or more epoxy resins may be used.
[0012] The epoxy resin has at least one epoxy group. In a preferred embodiment, the epoxy resin comprises an epoxy resin having at least two epoxy groups.
[0013] The epoxy equivalent of the epoxy resin is preferably within a range of 40 g / eq to 10,000 g / eq, more preferably 50 g / eq to 8,000 g / eq, and even more preferably 60 g / eq to 5,000 g / eq. In the present disclosure, "epoxy equivalent" means the mass of an epoxy resin per one epoxy group, and the method for measuring the epoxy equivalent complies with "JIS K 7236 (2009)".
[0014] The type of epoxy resin is not limited. The epoxy resin may be selected from epoxy resins used in known epoxy resin-containing compositions. Examples of the epoxy resin include polyglycidyl ether, glycidyl ether ester, polyglycidyl ester, epoxidized phenol novolac resin, epoxidized cresol novolac resin, epoxidized polyolefin, cycloaliphatic epoxy resin, and urethane-modified epoxy resin.
[0015] Examples of polyglycidyl ethers include the reaction products of polyhydric alcohols with epichlorohydrin. Examples of polyhydric alcohols include polyhydric phenols, glycerin, and polyethylene glycol. Examples of polyhydric phenols include bisphenol A, bisphenol F, bisphenol AD, catechol, and resorcinol.
[0016] Examples of glycidyl ether esters include the reaction products of hydroxycarboxylic acids with epichlorohydrin. Examples of hydroxycarboxylic acids include p-hydroxybenzoic acid and β-hydroxynaphthoic acid.
[0017] Examples of polyglycidyl esters include the reaction products of polycarboxylic acids with epichlorohydrin. Examples of polycarboxylic acids include phthalic acid and terephthalic acid.
[0018] From the viewpoint of high heat resistance and low moisture permeability, in a preferred embodiment, the epoxy resin comprises at least one selected from the group consisting of bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, biphenyl aralkyl type epoxy resin, phenol aralkyl type epoxy resin, aromatic glycidylamine type epoxy resin, and epoxy resin having a dicyclopentadiene structure. In a preferred embodiment, the epoxy resin comprises at least one selected from the group consisting of bisphenol A type epoxy resin and bisphenol F type epoxy resin.
[0019] The epoxy resin may be a liquid epoxy resin or a solid epoxy resin. A liquid epoxy resin is in a liquid state at 25°C. A solid epoxy resin is in a solid state at 25°C. Both liquid and solid epoxy resins may be used. In a preferred embodiment, the epoxy resin comprises a liquid epoxy resin. The composition is preferably in a liquid state at 25°C when used as an adhesive, and in a preferred embodiment, from the viewpoints of coatability, processability and adhesiveness, at least 50 mass% or more, preferably 60 mass% or more, more preferably 70 mass%, more preferably 80 mass%, more preferably 90 mass%, and particularly preferably 100 mass% of the total mass of the epoxy resin is a liquid epoxy resin.
[0020] Examples of liquid epoxy resins include bisphenol A type epoxy resins (e.g., "jER828EL", "jER827" and "YL980" manufactured by Mitsubishi Chemical Corporation), bisphenol F type epoxy resins (e.g., "jER807" manufactured by Mitsubishi Chemical Corporation), naphthalene type bifunctional epoxy resins (e.g., "HP4032" and "HP4032D" manufactured by DIC Corporation), mixtures of bisphenol A type epoxy resins and bisphenol F type epoxy resins (e.g., "ZX-1059" manufactured by Nippon Steel Chemical & Material Co., Ltd.), and hydrogenated epoxy resins (e.g., "jERYX8000" manufactured by Mitsubishi Chemical Corporation). In addition, examples of commercially available liquid epoxy resins include "YX7105" (manufactured by Mitsubishi Chemical Corporation) and "EXA-4850-150" (manufactured by DIC Corporation).
[0021] Examples of solid epoxy resins include naphthalene-type tetrafunctional epoxy resins (e.g., "HP4700" manufactured by DIC Corporation), dicyclopentadiene-type multifunctional epoxy resins (e.g., "HP7200" manufactured by DIC Corporation), naphthol-type epoxy resins (e.g., "ESN-475V" manufactured by Nippon Steel Chemical & Material Co., Ltd.), epoxy resins having a butadiene structure (e.g., "PB-3600" manufactured by Daicel Corporation), and epoxy resins having a biphenyl structure (e.g., "NC3000H" and "NC3000L" manufactured by Nippon Kayaku Co., Ltd. or "jERYX4000" manufactured by Mitsubishi Chemical Corporation).
[0022] The epoxy resin may contain linear hydrocarbon structural units having 4 or more carbon atoms and / or polyalkylene ether structural units having 3 or more ether oxygen atoms. An example of a linear hydrocarbon structural unit having 4 or more carbon atoms is -(CH2) x -. x is 4 or greater. x may be within a range of 4 to 20 or 4 to 20. The number of ether oxygen atoms in the polyalkylene ether structural unit may be within a range of 3 to 20 or 3 to 10.
[0023] The epoxy resin may be an epoxy resin represented by the following formula (1) or the following formula (2).
[0024] [ka]
[0025] In formula (1) and formula (2), X, X1, and X2 are each independently a divalent non-aromatic hydrocarbon group containing at least four -(CH2)- groups constituting the main skeleton of the epoxy resin, Ar, Ar1, and Ar2 are each independently a divalent hydrocarbon group containing a divalent aromatic group constituting the main skeleton of the epoxy resin, and n and m are each independently an integer of 1 to 20. The "main skeleton of the epoxy resin" means the longest skeleton connecting two epoxy groups located at the terminals of the epoxy resin.
[0026] In a preferred embodiment, the "divalent non-aromatic hydrocarbon group containing at least four -(CH)-" in X, X1 and X2 is -O-CH(-CH)-(O-(CH) p ) q -O-CH(-CH3)-, -(O-(CH2) r ) s -, -(O-CH2-CH(-CH3)) t -, -O-CH2-CH(-OH)-CH2-(O-(CH2) u ) v -O-CH2-CH(-OH)-CH2-, -(O-(CH2) w ) y -O-CH2-CH(-OH)- and -(O-CH2-CH(-CH3)) z -O-CH2-CH(-OH)-, and p, q, r, s, t, u, v, w, y and z are each independently an integer of 1 to 20.
[0027] Regarding the "divalent hydrocarbon group containing a divalent aromatic group" in Ar, Ar1 and Ar2, examples of the aromatic group include a phenylene group, a naphthalene group, an anthracene group and a biphenyl group. The phenylene group may be an orthophenylene group, a metaphenylene group or a paraphenylene group. The hydrocarbon group may contain two or more aromatic groups. When the hydrocarbon group contains two or more aromatic groups, the aromatic groups may be directly bonded to each other. The aromatic groups may be bonded to each other via an alkylene group, an ether bond, an ester bond, an amide bond or two carbons bonded by a double bond or a triple bond. Examples of preferred divalent hydrocarbon groups include a divalent hydrocarbon group represented by the following formula (3) or the following formula (4).
[0028] [ka]
[0029] The epoxy resin may be a modified bisphenol type epoxy resin represented by the following formula (5).
[0030] [ka]
[0031] In the formula (5), Y is an aliphatic hydrocarbon, Z is CH2 or C(CH3), and n is an integer of 0 to 10, preferably 1 to 8.
[0032] The epoxy resin may be a flexible epoxy resin. Commercially available examples of flexible epoxy resins include "YX7105" (Mitsubishi Chemical Corporation), "YX7110" (Mitsubishi Chemical Corporation), "YX7400" (Mitsubishi Chemical Corporation), and "EXA-4850-150" (DIC Corporation).
[0033] The content of the epoxy resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, based on the total mass of the composition. Furthermore, the content of the epoxy resin is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more, based on the total mass of the composition. The content of the epoxy resin is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on the total mass of the composition. Furthermore, the content of the epoxy resin is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, based on the total mass of the composition. For example, the content of the epoxy resin may be within a range of 5% by mass to 95% by mass, based on the total mass of the composition.
[0034] (Fumed Silica) The composition includes a fumed silica having at least one selected from the group consisting of dimethylsilyl and trimethylsilyl groups. One or more types of fumed silica may be used.
[0035] In a preferred embodiment, at least one selected from the group consisting of dimethylsilyl and trimethylsilyl groups is present at least on the surface of the fumed silica. The dimethylsilyl and trimethylsilyl groups in the fumed silica are detectable by time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0036] An example of a method for introducing dimethylsilyl or trimethylsilyl groups into fumed silica includes surface treatment with a compound having a dimethylsilyl or trimethylsilyl group. An example of a compound having a dimethylsilyl group includes dimethyldichlorosilane. An example of a compound having a trimethylsilyl group includes hexamethyldisilazane.
[0037] In a preferred embodiment, the specific surface area of the fumed silica is 5 m 2 / g~500m 2 / g. The lower limit of the specific surface area is 40 m 2 / g, 20m 2 / g or 10m 2 / g. The upper limit of the above is 200m 2 / g, 300m 2 / g or 400m 2 In the present disclosure, the specific surface area is measured by BET (nitrogen adsorption method).
[0038] Commercially available examples of fumed silica include "RX300" (manufactured by Nippon Aerosil Co., Ltd.), "R976S" (manufactured by Nippon Aerosil Co., Ltd.), and "R974" (manufactured by Nippon Aerosil Co., Ltd.).
[0039] From the viewpoint of further suppressing the occurrence of bleeding, in a preferred embodiment, the content of fumed silica is within the range of 0.1% by mass to 20% by mass based on the total mass of the composition. The lower limit of the content is preferably 2% by mass, more preferably 3% by mass, and even more preferably 5% by mass. The upper limit of the content is preferably 18% by mass, more preferably 16% by mass, and even more preferably 14% by mass.
[0040] (Cure accelerator) The composition includes a cure accelerator. One or more cure accelerators may be used.
[0041] The type of the curing accelerator is not limited. The curing accelerator may be selected from curing accelerators used in known epoxy resin-containing compositions. In a preferred embodiment, the curing accelerator includes a latent curing accelerator. The latent curing accelerator is a compound that does not contribute to the curing of the epoxy resin at room temperature (25° C.) but promotes the curing of the epoxy resin when heated.
[0042] In a preferred embodiment, the latent curing accelerator is a solid dispersion type latent curing accelerator. The solid dispersion type latent curing accelerator is a compound that is a solid that is insoluble in epoxy resin at room temperature (25°C) and is solubilized by heating to function as a curing accelerator for epoxy resin. Examples of the solid dispersion type latent curing accelerator include imidazole compounds that are solid at 25°C and solid dispersion type amine adduct type latent curing accelerators. The solid dispersion type amine adduct type latent curing accelerator is preferred.
[0043] Examples of imidazole compounds that are solid at 25° C. include 2-heptadecylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-undecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2-methylimidazolyl-(1))-ethyl-S-triazine, 2,4-diamino-6-(2'-methylimidazolyl-(1)')-ethyl Includes -S-triazine·isocyanuric acid adduct, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole-trimellitate, 1-cyanoethyl-2-phenylimidazole-trimellitate, N-(2-methylimidazolyl-1-ethyl)-urea and N,N'-(2-methylimidazolyl-(1)-ethyl)-adiboyldiamide.
[0044] Examples of the solid dispersion type amine adduct latent curing accelerator include a reaction product of an amine compound with an epoxy compound, and a reaction product of an amine compound with an isocyanate compound or a urea compound.
[0045] Examples of amine compounds used as raw materials for solid dispersion type amine adduct latent curing accelerators include compounds having at least one active hydrogen capable of addition reaction with epoxy groups and having at least one amino group selected from primary amino groups, secondary amino groups, and tertiary amino groups. Examples of such amine compounds include aliphatic amines (e.g., diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane), aromatic amine compounds (e.g., 4,4'-diaminodiphenylmethane and 2-methylaniline), and nitrogen atom-containing heterocyclic compounds (e.g., 2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine).
[0046] Among amine compounds, compounds having a tertiary amino group in the molecule are raw materials that provide latent curing accelerators with excellent curing acceleration ability. Examples of such compounds are dimethylaminopropylamine, diethylaminopropylamine, di-n-propylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, N-methylpiperazine, 2-methylimidazole, 2-ethylimidal, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazo These include 1-(2-hydroxy-3-butoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-benzimidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionic acid hydrazide, nicotinic acid hydrazide and isonicotinic acid hydrazide.
[0047] Examples of epoxy compounds used as raw materials for solid dispersion type amine adduct-based latent curing accelerators include polyglycidyl ether, glycidyl ether ester, polyglycidyl ester, glycidyl amine compound, epoxidized phenol novolac resin, epoxidized cresol novolac resin, epoxidized polyolefin, butyl glycidyl ether, phenyl glycidyl ether and glycidyl methacrylate. The epoxy compound may be a compound having one epoxy group or a compound having at least two epoxy groups.
[0048] Examples of polyglycidyl ethers include the reaction products of polyhydric alcohols with epichlorohydrin. Examples of polyhydric alcohols include polyhydric phenols, glycerin, and polyethylene glycol. Examples of polyhydric phenols include bisphenol A, bisphenol F, catechol, and resorcinol.
[0049] Examples of glycidyl ether esters include the reaction products of hydroxycarboxylic acids with epichlorohydrin. Examples of hydroxycarboxylic acids include p-hydroxybenzoic acid and β-hydroxynaphthoic acid.
[0050] Examples of polyglycidyl esters include the reaction products of polycarboxylic acids with epichlorohydrin. Examples of polycarboxylic acids include phthalic acid and terephthalic acid.
[0051] Examples of glycidyl amine compounds include the reaction product of 4,4'-diaminodiphenylmethane or m-aminophenol with epichlorohydrin.
[0052] When preparing a latent curing accelerator by reacting an amine compound with an epoxy compound, an active hydrogen compound having at least two active hydrogens in the molecule may be added. Examples of the active hydrogen compound include polyhydric phenols (e.g., bisphenol A, bisphenol F, bisphenol S, hydroquinone, catechol, resorcinol, pyrogallol and phenol novolac resins), polyhydric alcohols (e.g., trimethylolpropane), polycarboxylic acids (e.g., adipic acid and phthalic acid), 1,2-dimercaptoethane, 2-mercaptoethanol, 1-mercapto-3-phenoxy-2-propanol, mercaptoacetic acid, anthranilic acid and lactic acid.
[0053] Examples of the isocyanate compound used as a raw material for the solid dispersion type amine adduct latent curing accelerator include monofunctional isocyanate compounds (e.g., n-butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate), polyfunctional isocyanate compounds (e.g., hexamethylene diisocyanate, toluylene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate), and terminal isocyanate group-containing compounds obtained by reacting a polyfunctional isocyanate compound with an active hydrogen compound. Examples of the compound containing a terminal isocyanate group include an adduct compound having a terminal isocyanate group obtained by reacting toluylene diisocyanate with trimethylolpropane and an adduct compound having a terminal isocyanate group obtained by reacting toluylene diisocyanate with pentaerythritol.
[0054] Examples of the urea compound used as a raw material for the solid dispersion type amine adduct-based latent curing accelerator include urea and thiourea.
[0055] Commercially available examples of reaction products between amine compounds and epoxy compounds include "Amicure PN-40J" (manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-F" (manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-23" (manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Amicure PN-H" (manufactured by Ajinomoto Fine-Techno Co., Ltd.), "Novacure HX-3742" (manufactured by Asahi Kasei Corporation), and "Novacure HX-3721" (manufactured by Asahi Kasei Corporation).
[0056] Examples of commercially available reaction products of amine compounds and isocyanate compounds or urea compounds include "Fujicure FXR-1020" (manufactured by Fuji Chemical Industry Co., Ltd.) and "Fujicure FXR-1030" (manufactured by Fuji Chemical Industry Co., Ltd.).
[0057] The content of the curing accelerator is preferably within the range of 0.01 mass % to 20 mass %, more preferably 0.1 mass % to 10 mass %, and even more preferably 0.5 mass % to 5 mass %, based on the total mass of the composition.
[0058] The ratio of the total mass of the curing accelerator to the total mass of the epoxy resin is preferably within the range of 0.1 mass % to 100 mass %, more preferably 1 mass % to 60 mass %, and even more preferably 5 mass % to 30 mass %.
[0059] (Thiol compounds) The composition comprises a thiol compound exhibiting a viscosity of 0.2 Pa·s or more at 25° C. One or more types of thiol compounds may be used.
[0060] The viscosity of the thiol compound is 0.2 Pa·s or more at 25°C. From the viewpoint of further suppressing the occurrence of bleeding, the lower limit of the viscosity of the thiol compound is preferably 0.4 Pa·s, more preferably 0.6 Pa·s, and even more preferably 0.8 Pa·s. The lower limit of the viscosity of the thiol compound may be 1 Pa·s or 3 Pa·s. The upper limit of the viscosity of the thiol compound is preferably 40 Pa·s, more preferably 20 Pa·s, and even more preferably 15 Pa·s. The upper limit of the viscosity of the thiol compound may be 10 Pa·s, 8 Pa·s, or 6 Pa·s. For example, the viscosity of the thiol compound may be within a range of 0.2 Pa·s to 40 Pa·s at 25°C. In the present disclosure, the viscosity of the thiol compound is measured by a rheometer.
[0061] Examples of thiol compounds include tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC), pentaerythritol tetrakis(3-mercaptobutyrate) (e.g., "Karends MT (registered trademark) PE1" manufactured by Resonac), and pentaerythritol tripropanethiol (e.g., "Multhiol Y-3" manufactured by SC Organic Chemicals).
[0062] The molecular weight of the thiol compound is preferably within the range of 200-700, more preferably 250-500, and even more preferably 300-400.
[0063] The thiol compound has at least one thiol group. In a preferred embodiment, the thiol compound includes a compound having at least two thiol groups. The number of thiol groups in the thiol compound is preferably 2 to 6, more preferably 3 to 6, and even more preferably 3 to 5. Furthermore, the number of thiol groups in the thiol compound is preferably 3 or 4, and more preferably 3.
[0064] The thiol equivalent of the thiol compound is preferably within a range of 50 g / eq to 400 g / eq, more preferably 50 g / eq to 400 g / eq, and even more preferably 70 g / eq to 200 g / eq. Furthermore, the thiol equivalent of the thiol compound is preferably within a range of 80 g / eq to 150 g / eq. In the present disclosure, "thiol equivalent" means the mass of the thiol compound per one thiol group.
[0065] In a preferred embodiment, the thiol compound does not have an ester bond. The ester bond is a bond represented by "-C(=O)O-". Since hydrolysis based on the ester bond does not occur, moisture resistance is improved and reliability is increased.
[0066] In a preferred embodiment, the thiol compound does not have a hydroxy group. The thiol compound does not have a hydroxy group, and can improve the pot life of the composition. As a result, the composition can achieve both a long pot life and fast curing properties.
[0067] In a preferred embodiment, the thiol compound does not have a ring skeleton. When the thiol compound does not have a ring skeleton, the skeleton of the thiol compound becomes flexible, and the peel strength can be improved.
[0068] In a preferred embodiment, the thiol compound has a ring skeleton. The thiol compound having a ring skeleton can improve the shear adhesive strength. The thiol compound having a ring skeleton may be a monocyclic compound or a polycyclic compound. Examples of the ring skeleton include an alicyclic skeleton, an aromatic ring skeleton, and a heterocyclic skeleton. The ring skeleton is preferably an aromatic ring skeleton or a heterocyclic skeleton, and more preferably a heterocyclic skeleton. Examples of the heterocyclic skeleton include a heterocyclic skeleton having a 5- to 8-membered ring containing at least one nitrogen atom. Specifically, examples of the heterocyclic skeleton include an isocyanuric skeleton and a glycoluril skeleton.
[0069] In a preferred embodiment, the thiol compound includes a compound represented by the following formula (6):
[0070] [ka]
[0071] In formula (6), R1, R2, and R3 each independently represent a linear or branched divalent hydrocarbon group having 1 to 6 carbon atoms, preferably 1 to 5. The hydrocarbon group may contain a divalent group represented by the following (6a) to (6c). The number of divalent groups may be one or more.
[0072] [ka]
[0073] An example of the compound represented by formula (6) includes tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC).
[0074] From the viewpoint of the curability of the composition, in a preferred embodiment, the ratio of the number of thiol groups of the thiol compound to the number of epoxy groups of the epoxy resin (total number of thiol groups of the thiol compound / total number of epoxy groups of the epoxy resin) is preferably 0.1 to 2.0, more preferably 0.5 to 1.2. The "number of epoxy groups" refers to the value obtained by dividing the mass of the epoxy resin contained in the composition by the epoxy equivalent (mass of epoxy groups / epoxy equivalent). In addition, when a plurality of types of epoxy resins are contained in the composition, the number of epoxy groups refers to the sum of the values obtained by dividing the mass of each epoxy resin by each epoxy equivalent. The "number of thiol groups" refers to the value obtained by dividing the mass of the thiol contained in the composition by the thiol equivalent (mass of thiol groups / thiol equivalent). In addition, in addition, when a plurality of types of thiols are contained in the composition, the number of thiol groups refers to the sum of the values obtained by dividing the mass of each thiol by each thiol equivalent. When the composition contains a thiol compound other than the "thiol compound exhibiting a viscosity of 0.2 Pa s or more at 25°C," the above ratio is calculated based on the number of thiol groups of all thiol compounds contained in the composition.
[0075] From the viewpoint of further suppressing the occurrence of bleeding, in a preferred embodiment, the content of the thiol compound is within the range of 1% by mass to 80% by mass based on the total mass of the composition. The lower limit of the content is preferably 3% by mass, more preferably 5% by mass, and even more preferably 7% by mass. The upper limit of the content is preferably 75% by mass, more preferably 70% by mass, and even more preferably 60% by mass.
[0076] (Stabilizer) The composition may further comprise a stabilizer. The stabilizer can improve the storage stability of the composition. One or more storage stabilizers may be used.
[0077] Examples of the stabilizer include borate ester compounds, titanate ester compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids. In a preferred embodiment, the composition comprises at least one stabilizer selected from the group consisting of borate ester compounds, titanate ester compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids.
[0078] Examples of the borate ester compound include trimethyl borate, triethyl borate, tri-n-propyl borate, triisopropyl borate, tri-n-butyl borate, tripentyl borate, triallyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, trinonyl borate, tridecyl borate, tridodecyl borate, trihexadecyl borate, trioctadecyl borate, tris(2-ethylhexyloxy)borane, bis(1,4,7,10-tetraoxaundecyl)(1,4,7,10,13-pentaoxatetradecyl)(1,4,7-trioxaundecyl)borane, tribenzyl borate, triphenyl borate, tri-o-tolyl borate, tri-m-tolyl borate, and triethanolamine borate.
[0079] Examples of titanate compounds include tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, and tetraoctyl titanate.
[0080] Examples of aluminate compounds include triethyl aluminate, tripropyl aluminate, triisopropyl aluminate, tributyl aluminate and trioctyl aluminate.
[0081] Examples of zirconate compounds include tetraethyl zirconate, tetrapropyl zirconate, tetraisopropyl zirconate, and tetrabutyl zirconate.
[0082] Examples of the isocyanate compound include n-butyl isocyanate, isopropyl isocyanate, 2-chloroethyl isocyanate, phenyl isocyanate, p-chlorophenyl isocyanate, benzyl isocyanate, hexamethylene diisocyanate, 2-ethylphenyl isocyanate, 2,6-dimethylphenyl isocyanate, 2,4-toluene diisocyanate, toluylene diisocyanate, 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, tolidine diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, and bicycloheptane triisocyanate.
[0083] Examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, caproic acid, caprylic acid, acrylic acid, methacrylic acid, crotonic acid, monochloroacetic acid, dichloroacetic acid, glycolic acid, lactic acid, glyoxylic acid, tartaric acid, oxalic acid, malonic acid, succinic acid, maleic acid, benzoic acid, halogenated benzoic acids, toluic acid, phenylacetic acid, cinnamic acid, mandelic acid, phthalic acid, and trimesic acid.
[0084] Examples of acid anhydrides include succinic anhydride, dodecynylsuccinic anhydride, maleic anhydride, an adduct of methylcyclopentadiene and maleic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, phthalic anhydride, trimellitic anhydride and pyrrolimellitic anhydride.
[0085] Examples of mercapto organic acids include mercaptoacetic acid, mercaptopropionic acid, mercaptobutyric acid, mercaptosuccinic acid, dimercaptosuccinic acid, mercaptoaliphatic monocarboxylic acids obtained by esterification of hydroxy organic acids with mercapto organic acids, and mercaptoaromatic monocarboxylic acids (e.g., mercaptobenzoic acid).
[0086] From the viewpoints of versatility, safety, and storage stability of the composition, the stabilizer is preferably a borate ester compound, more preferably triethyl borate, tri-n-propyl borate, triisopropyl borate, or tri-n-butyl borate, and even more preferably triethyl borate.
[0087] The content of the stabilizer is preferably within the range of 0.0005% by mass to 30% by mass, more preferably 0.02% by mass to 20% by mass, and even more preferably 0.1% by mass to 10% by mass, based on the total mass of the composition.
[0088] (Other ingredients) The composition may further contain other components as necessary. Examples of the other components include a diluent, a solvent, a pigment, a flexibilizer, a coupling agent, an antioxidant, a thixotropic agent, and a dispersant.
[0089] The composition may contain fumed silica having no dimethylsilyl group and no trimethylsilyl group within the scope of the present disclosure. However, from the viewpoint of further suppressing the occurrence of bleeding, it is preferable to lower the content of fumed silica having no dimethylsilyl group and no trimethylsilyl group. The content of fumed silica having no dimethylsilyl group and no trimethylsilyl group relative to the total mass of fumed silica contained in the composition is preferably 50 mass% or less, more preferably 40 mass% or less, even more preferably 30 mass% or less, even more preferably 20 mass% or less, even more preferably 10 mass% or less, even more preferably 5 mass% or less, and particularly preferably 0 mass%. In a preferred embodiment, the composition does not contain fumed silica having no dimethylsilyl group and no trimethylsilyl group. The composition may contain inorganic fillers other than fumed silica, such as silica, calcium carbonate, alumina, zirconia, and aluminum nitride, within the scope of the present disclosure.
[0090] The composition may contain a thiol compound having a viscosity of less than 0.2 Pa·s at 25°C within the scope of the present disclosure. However, from the viewpoint of further suppressing the occurrence of bleeding, it is preferable to lower the content of the thiol compound having a viscosity of less than 0.2 Pa·s at 25°C. The content of the thiol compound having a viscosity of less than 0.2 Pa·s at 25°C is preferably within the range of 0 mass% to 3 mass%, more preferably 0 mass to 1 mass%, and even more preferably 0 mass to 0.1 mass%, based on the total mass of the composition. From the viewpoint of further suppressing the occurrence of bleeding, the ratio of the total mass of the thiol compound having a viscosity of less than 0.2 Pa·s at 25°C to the total mass of the thiol compound having a viscosity of 0.2 Pa·s or more at 25°C is preferably within the range of 0 mass% to 5 mass%, more preferably 0 mass to 3 mass%, and even more preferably 0 mass to 1 mass%. In a preferred embodiment, the composition does not contain a thiol compound having a viscosity of less than 0.2 Pa·s at 25°C.
[0091] The composition may contain an organic solvent. However, from the viewpoint of suppressing the occurrence of bleeding, it is preferable to reduce the content of the organic solvent. The content of the organic solvent is preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 1 mass% or less, even more preferably 0.1 mass% or less, and particularly preferably 0 mass% based on the total mass of the composition. In a preferred embodiment, the composition does not contain an organic solvent.
[0092] (Characteristics of the composition) In a preferred embodiment, the composition is a flowable liquid composition at 25°C.
[0093] In a preferred embodiment, the composition exhibits a viscosity in the range of 1 Pa·s to 200 Pa·s under measurement conditions of 25° C. and 2 rpm. The lower limit of the viscosity may be 20 Pa·s or 5 Pa·s. The upper limit of the viscosity may be 75 Pa·s or 110 Pa·s. In the present disclosure, the viscosity of the composition is measured using an E-type viscometer. "rpm" is an abbreviation for "revolutions per minute."
[0094] In a preferred embodiment, the composition exhibits a viscosity in the range of 1 Pa·s to 60 Pa·s at 25° C. and 20 rpm. The lower limit of the viscosity may be 20 Pa·s or 5 Pa·s. The upper limit of the viscosity may be 30 Pa·s or 40 Pa·s.
[0095] In a preferred embodiment, the thixotropy index represented by the following formula is in the range of 0.5 to 7. The lower limit of the thixotropy index is preferably 0.6, more preferably 0.8, and even more preferably 1. The upper limit of the thixotropy index is preferably 4, more preferably 5, and even more preferably 6. Formula: Thixotropy index = ([viscosity of composition obtained under measurement conditions of 25°C and 2 rpm] ÷ [viscosity of composition obtained under measurement conditions of 25°C and 20 rpm]) x 100
[0096] (Production method of the composition) As long as the desired composition can be obtained, the method for producing the composition is not limited.For example, the composition is produced by mixing an epoxy resin, a fumed silica, a curing accelerator, a thiol compound, and other components as necessary.
[0097] (Applications and Uses of the Composition) Examples of applications of the composition include casting agents, sealing agents, encapsulants, fiber-reinforced resins, coating agents, underfill agents, die-attach agents, electromagnetic shielding materials, paints, and adhesives. In a preferred embodiment, the composition is used as an adhesive. The composition may be used, for example, as an adhesive, in the assembly of electronic components. Examples of electronic components include camera modules, printed circuit boards, semiconductor elements, and integrated circuits. The electronic components may include a cured product of the composition. The composition may be injected between at least two electronic components, for example, between a semiconductor element and a substrate.
[0098] The composition can provide a cured product. For example, the composition can be cured by heat treatment. The heat treatment temperature is preferably within a range of 70° C. to 150° C., more preferably 75° C. to 120° C., and even more preferably 80° C. to 100° C. The heat treatment time is preferably within a range of 1 minute to 60 minutes, and more preferably 3 minutes to 45 minutes. EXAMPLES
[0099] The present disclosure will be described below based on examples. However, the present disclosure is not limited to the following examples. The following technical matters may be appropriately modified within the scope of the present disclosure.
[0100] <Production of Composition> Compositions containing the components shown in Tables 1 and 2 were manufactured according to the following procedure. An epoxy resin and fumed silica were added to a dedicated container. The epoxy resin and fumed silica were thoroughly mixed at room temperature of 25°C at 2000 rpm for about 30 to about 60 seconds using a mixer (Thinky Corporation, ARE-310), and then kneaded using three rolls to obtain a dispersion. A latent curing accelerator was added to the dispersion. The dispersion and the latent curing accelerator were thoroughly mixed at room temperature of 25°C at 2000 rpm for about 30 to about 60 seconds using a mixer (Thinky Corporation, ARE-310) to obtain a master batch. A thiol compound was added to the master batch. The master batch and the thiol compound were thoroughly mixed at room temperature of 25°C at 2000 rpm for about 20 seconds using a mixer (Thinky Corporation, ARE-310). The mixture was defoamed under vacuum at 900 rpm for 2 minutes using a stirring defoamer (HM-200W, manufactured by Kyoritsu Seiki Co., Ltd.) to obtain a composition. Regarding pressure control, the vacuum condition of the stirring defoamer was set to "0".
[0101] The details of the materials of the composition are as follows. The name of each material is expressed by the abbreviation of the compound name or the product name. Unless otherwise specified, the viscosity is expressed at 25°C.
[0102] (Epoxy resin) "YL980": Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, epoxy equivalent = 186g / eq, viscosity = 13Pa s, molecular weight = 372 "YX7105": Mitsubishi Chemical Corporation, flexible epoxy resin, epoxy equivalent = 489g / eq, viscosity = 69Pa·s, molecular weight = 978 "ZX-1059": Nippon Steel Chemical & Material Co., Ltd., bisphenol A type / bisphenol F type epoxy resin, epoxy equivalent = 165g / eq, viscosity = 2Pa·s, molecular weight = 330 "EXA-4850-150": DIC Corporation, epoxy equivalent = 450g / eq, viscosity = 15Pa s, molecular weight = 900
[0103] (Fumed Silica) "RX300": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface modified with trimethylsilyl group, specific surface area = 180 m 2 / g~220m 2 / g, specific gravity = approx. 40g / L "R976S": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface modified with dimethylsilyl group, specific surface area = 215 m 2 / g~265m 2 / g, specific gravity = approx. 50g / L "R974": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface modified with dimethylsilyl group, specific surface area = 150 m 2 / g~190m 2 / g, specific gravity = approx. 50g / L "RY300": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface treatment with silicone oil, specific surface area = 110 m 2 / g~140m 2 / g, specific gravity = approx. 50g / L "RY200": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface treatment with silicone oil, specific surface area = 80 m 2 / g~120m 2 / g, specific gravity = approx. 50g / L "R805": Manufactured by Nippon Aerosil Co., Ltd., fumed silica, surface modified with octylsilyl group, specific surface area = 125 m 2 / g~175m 2 / g, specific gravity=60g / L
[0104] (Latent curing accelerator) "PN-23": AmiCure (registered trademark), manufactured by Ajinomoto Fine-Techno Co., Ltd., solid dispersion type amine adduct latent curing accelerator "PN-40J": Ajinomoto Fine-Techno Co., Ltd., Amicure (registered trademark), solid dispersion type amine adduct latent curing accelerator
[0105] (Thiol compounds) "TMPIC": Kawaguchi Chemical Industry Co., Ltd., tris(3-mercaptopropyl)isocyanurate, a trifunctional thiol with an isocyanurate skeleton, thiol equivalent = 117g / eq, viscosity = 4.9Pa s, molecular weight = 351 "PE1": Resonaq, pentaerythritol tetrakis(3-mercaptobutyrate), 4-functional secondary ester thiol, thiol equivalent = 136 g / eq, viscosity = 0.9 Pa s, molecular weight = 544 "MR-123": Daito Sangyo Co., Ltd., trifunctional non-ester thiol, thiol equivalent = 300g / eq, viscosity = 14.2Pa s, molecular weight = 900 "PEPT" (Multhiol Y-3): SC Organic Chemicals, trifunctional thiol with a pentaerythritol skeleton, thiol equivalent = 124 g / eq, viscosity = 0.2 Pa s, molecular weight = 372 "TMTP": Yodo Chemical Co., Ltd., trimethylolpropane tris(3-mercaptopropionate, trifunctional primary ester thiol, thiol equivalent = 140 g / eq, viscosity = 0.1 Pa s, molecular weight = 420 "BD1": Resonaq Corporation, 1,4-bis(3-mercaptobutyryloxy)butane, bifunctional secondary ester thiol, thiol equivalent = 147g / eq, viscosity = 0.02Pa s, molecular weight = 147
[0106] The method for measuring the viscosity of each of the above-mentioned thiol compounds is as follows. A rheometer (Thermo Fisher Scientific Inc., RheoStress 6000) was used as a viscosity measuring device. A cone plate was used as a measuring tool, and the viscosity was measured at 25° C. with a shear rate of 400 s -1 The viscosity was measured when the cone plate was a C20 / 1-TiL with a diameter of 20 mm. In the viscosity measurement, the distance between the cone tip and the plate was set to 0.052 mm, and 0.04 mL of the sample was used.
[0107] <Measurement of Viscosity and Thixotropy Index> The temperature of the composition was kept at 25°C, and the viscosity of the composition was measured using an E-type viscometer (RE-85U, manufactured by Toki Sangyo Co., Ltd.). Regarding the rotor of the viscometer, an appropriate rotor was selected from the following three types of rotors based on the viscosity at 2 rpm. The specific measurement conditions are shown below. (1) Viscometer rotor: "1.34°×R24" (when the viscosity at 2 rpm is less than 20 Pa·s), "3°×R14" (when the viscosity at 2 rpm is 20 Pa·s or more and less than 50 Pa·s), or "3°×R9.7" (when the viscosity at 2 rpm is 50 Pa·s or more) (2) Rotation speed: 2 rpm or 20 rpm (3) Measurement time: 2 minutes (4) Sample volume: 1.2 mL (if the rotor is "1.34° x R24"), 0.4 mL (if the rotor is "3° x R14"), or 0.22 mL (if the rotor is "3° x R9.7")
[0108] Next, the thixotropy index was calculated according to the following formula. Formula: Thixotropy index = ([viscosity of composition obtained under measurement conditions of 25°C and 2 rpm] ÷ [viscosity of composition obtained under measurement conditions of 25°C and 20 rpm]) x 100
[0109] <Bleed width measurement> The composition was filled into a dispenser syringe (PSY-10E, manufactured by Musashi Engineering Co., Ltd.), and then centrifugal defoaming was performed using a centrifugal defoamer (AWATRON3 AW-50-3, manufactured by Musashi Engineering Co., Ltd.). The composition was applied to a copper substrate using an air dispenser (IMAGE MASTER 350PC Smart, manufactured by Musashi Engineering Co., Ltd.). Specifically, the composition was applied to the copper substrate so that the diameter of the composition on the substrate was about 500 μm. The surface roughness Ra of the copper substrate was 600 μm ± 50 μm. Next, the composition on the copper substrate was heated at 80°C for 30 minutes using a heat circulation oven (DF-610, manufactured by Yamato Scientific Co., Ltd.). Next, the composition after heating was observed using a digital microscope (VHX-7000, manufactured by Keyence Co., Ltd.), and the maximum diameter of the composition after heating in a plan view and the maximum diameter of the bleed in a plan view (the maximum diameter of the portion where the components in the composition oozed out outside the application range of the composition) were measured. The width of each bleed was calculated according to the formula below, and the average value of six measurements was calculated. Formula: Bleed width = ([Maximum diameter of bleed] - [Maximum diameter of composition after heating]) ÷ 2
[0110] The extent of bleeding was evaluated according to the following criteria, with A, B and C being acceptable levels. A: Less than 600μm B: 600μm or more and less than 700μm C: 700μm or more and less than 800μm D:800μm or more
[0111] [Table 1]
[0112] [Table 2]
[0113] The compositions used in Examples 1 to 10 contain fumed silica having at least one selected from the group consisting of a dimethylsilyl group and a trimethylsilyl group, and a thiol compound exhibiting a viscosity of 0.2 Pa s or more at 25° C. As shown in Tables 1 and 2, Examples 1 to 10 achieved a smaller bleeding width than Comparative Examples 1 to 8. In other words, Examples 1 to 10 suppressed the occurrence of bleeding more than Comparative Examples 1 to 8.
[0114] In Comparative Examples 1 and 2, which did not use a thiol compound exhibiting a viscosity of 0.2 Pa s or more at 25° C., the extent of bleeding was large and the occurrence of bleeding was not sufficiently suppressed. In Comparative Examples 3 to 8, which did not use fumed silica having at least one group selected from the group consisting of a dimethylsilyl group and a trimethylsilyl group, the extent of bleeding was large and the occurrence of bleeding was not sufficiently suppressed.
Claims
1. Epoxy resin, Fumed silica having at least one selected from the group consisting of a dimethylsilyl group and a trimethylsilyl group; A curing accelerator; A thiol compound having a viscosity of 0.2 Pa·s or more at 25°C; composition.
2. The composition according to claim 1, wherein the viscosity of the thiol compound is in the range of 0.2 Pa·s to 15 Pa·s at 25° C.
3. The composition of claim 1, wherein the content of the fumed silica is in the range of 0.1% by weight to 20% by weight, based on the total weight of the composition.
4. The composition according to claim 1, wherein the content of the thiol compound is in the range of 1% by mass to 80% by mass, based on the total mass of the composition.
5. The composition according to claim 1 , wherein the thiol compound does not have a ring skeleton.
6. The composition according to claim 1 , wherein the thiol compound has a ring skeleton.
7. The composition of claim 1 , wherein the thiol compound does not have an ester bond.
8. An adhesive comprising the composition according to any one of claims 1 to 7.
9. A cured product of the composition according to any one of claims 1 to 7.
10. An electronic component comprising the cured product according to claim 9.
Citation Information
Patent Citations
Sealing material composition for assembling liquid crystal cell
JP1995199198A
Sealing agent for plastic film liquid crystal device and display device
JP2001133796A
Epoxy resin composition and semiconductor sealing device
JP2002194180A
Thioether-containing alkoxysilane derivative and use thereof
JP2011136985A
Thermosetting liquid crystal sealing material for liquid crystal dropping method, and liquid crystal display cell using the same
JP2011150181A