Composition and surface protection method

A silicone-modified (meth)acrylic copolymer resin-based composition with controlled peeling and adhesive force properties addresses the adhesion issues of existing surface protection methods, enhancing the adhesion and durability of coatings on porous bodies.

JP2024140658APending Publication Date: 2024-10-10DENKA CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023051914
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing compositions for protecting the surface of porous bodies, such as those described in Patent Document 1, suffer from inadequate adhesion to the surface, particularly in terms of peeling perimeter and average adhesive force when dry and wet.

Method used

A composition containing a silicone-modified (meth)acrylic copolymer resin with specific structural units and properties, including a reactive silyl group, is formulated to improve adhesion by controlling peeling circumference and average adhesive force. The composition is applied in layers to form a coating with controlled viscosity and molecular weight, using a crosslinking agent to enhance adhesion.

Benefits of technology

The composition achieves excellent adhesion per unit area to the surface of porous bodies, providing a coating film with improved mechanical strength and durability, even in humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140658000011
    Figure 2024140658000011
  • Figure 2024140658000012
    Figure 2024140658000012
  • Figure 2024140658000001
    Figure 2024140658000001
Patent Text Reader

Abstract

To provide a composition capable of forming a coating film excellent in adhesion per unit area with respect to a surface of porous body.SOLUTION: A composition of the invention is one which is used for application to a surface of a porous body. The composition includes a silicone-modified (meth)acrylic copolymer resin having, in a molecule, a structural unit N having a reactive silyl group. A peeling circumference (displacement: 40 mm) during drying, which is measured by a predetermined push-out test, is 700 mm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition and a method for protecting a surface. [Background technology]

[0002] Various methods for protecting the surface of porous bodies have been developed. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a method in which a primer layer containing a silane coupling agent and a urethane resin is formed on the surface of a concrete structure, and a main material layer containing a urethane resin is formed on the primer layer (Table 1 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-017762 Summary of the Invention [Problem to be solved by the invention]

[0004] However, as a result of investigations by the present inventors, it was found that there is room for improvement in the adhesive strength (adhesion) of compositions such as the primer described in Patent Document 1 to the surface of a porous body. [Means for solving the problem]

[0005] As a result of further investigation, the inventors have found that in a composition containing a silicone-modified (meth)acrylic copolymer, the peeling circumference when dry and |average adhesion when dry - average adhesion when wet| are used as indicators, and by appropriately controlling these, it is possible to improve the adhesion per unit area of ​​the composition to the surface of a porous body, thereby completing the present invention.

[0006] According to one aspect of the present invention, the following composition and method for protecting a surface are provided. 1. A composition for use in applying to the surface of a porous body, comprising: The silicone-modified (meth)acrylic copolymer resin contains a structural unit N having a reactive silyl group in the molecule, A composition having a peel circumference (displacement: 40 mm) when dry, measured according to the procedure below, of 700 mm or less. (Procedure for measuring peel perimeter) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, and a cylindrical punch indenter with a diameter of 100 mm and a thickness of 55 mm±3 mm was formed on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. Next, the composition was applied to the surface of the test substrate using a roller in a coating amount of 0.15 [kg / m 2 ] and then cure for one day at 23±2°C and a relative humidity of 50±20% to form a dry base layer. On top of that layer, the surface protection composition obtained above was applied in a coating amount of 1.50 [kg / m 2 The mixture was left to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. A sample having an undercoat layer and a surface protective layer was obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate and the indenter was broken at room temperature of 23°C, and then the indenter was applied toward the sample at 5 mm / min. The load and displacement were measured over time. In this push-out test, the peel circumference (mm) of the sample when the displacement is 40 mm is measured. 2. A composition for use in applying to the surface of a porous body, comprising: The silicone-modified (meth)acrylic copolymer resin contains a structural unit N having a reactive silyl group in the molecule, The average adhesion when dry - average adhesion when wet measured according to the procedure below is 1.0 N / mm 2 1. A composition comprising: (Adhesion measurement procedure) - Preparation of test boards Mortar prepared according to the method specified in JIS R 5201, 10.4 (How to prepare a test specimen) is molded using a metal formwork with inner dimensions of 70mm x 70mm x 20mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it is demolded and cured in water at 20±2°C for 6 days, and then left to stand in a curing room for a further 7 days or more. After that, the underside of the molded specimen is polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface areas, and the surface is cleaned to prepare a test substrate. -Preparation of test specimen Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. The test substrate is immersed in water for one day, then taken out of the water and the water on the surface is wiped off (wetting treatment). Immediately after, the composition was applied to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 ] and dried for 24 hours at 23°C and 50% relative humidity to form a base layer. The above-obtained surface protection composition was applied on the base layer in a coating amount of 1.5 [kg / m 2] and leave it at 23°C and 50% relative humidity for 7 days to form a surface protective layer and prepare a wet test specimen. In addition, the composition and the surface protecting composition are similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment to prepare a dry test specimen. Adhesion strength measurement The wet test specimen is placed horizontally in a curing chamber, adhesive is applied to the surface on which the primer layer is formed, and a steel jig for upper tension is gently placed on top and attached by lightly rubbing it. Any adhesive that has protruded to the edges is wiped off, and after leaving it to rest for 24 hours, a tensile force is applied vertically to the test specimen surface and the maximum tensile load (N) is determined for each of the three test specimens. The load rate until breakage is 1500N / min. Adhesion strength (N / mm 2 ) is calculated using the formula "maximum tensile load (N) / 1600" and expressed as the average of three measured values. However, after making a 40mm x 40mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load is determined using the lower tensile steel jig and a steel backing plate. The adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength." 3. The composition according to 1. or 2., A composition having a viscosity of 50 mPa·s or more and 3000 mPa·s or less, measured at 25°C and a rotation speed of 10 rpm using a Brookfield viscometer. 4. The composition according to any one of 1. to 3., A composition, wherein the silicone-modified (meth)acrylic copolymer resin has a structural unit O having a terminal hydroxyl group in the molecule. 5. The composition according to any one of 1. to 4., The silicone-modified (meth)acrylic copolymer resin has a structural unit P having a perfluoroalkyl group in the molecule. 6. The composition according to any one of 1. to 5., A composition, wherein the silicone-modified (meth)acrylic copolymer resin has a structural unit M having a (meth)acrylic group in the molecule. 7. The composition according to any one of 1. to 6., The silicone-modified (meth)acrylic copolymer resin has a weight average molecular weight (Mw) of 500 or more and 50,000 or less. 8. The composition according to any one of 1. to 7., The composition, wherein the porous body is a concrete structure. 9. The composition according to any one of 1. to 8., The composition is a primer composition. 10. A surface protection method comprising the steps of applying a composition according to any one of 1. to 9. to a surface of a porous body and drying the composition to form a layer. 11. A silicone-modified (meth)acrylic copolymer resin having a structural unit N having a reactive silyl group in the molecule, A composition having a peel circumference (displacement: 40 mm) when dry, measured according to the procedure below, of 700 mm or less. (Procedure for measuring the peeling perimeter) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, and a cylindrical punch indenter with a diameter of 100 mm and a thickness of 55 mm±3 mm was formed on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. Next, the composition was applied to the surface of the test substrate using a roller in a coating amount of 0.15 [kg / m 2 ] and then cure for one day at 23±2°C and a relative humidity of 50±20% to form a dry base layer. On top of that layer, the surface protection composition obtained above was applied in a coating amount of 1.50 [kg / m 2 The mixture was left to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. A sample having an undercoat layer and a surface protective layer was obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate and the indenter was broken at room temperature of 23°C, and then the indenter was applied toward the sample at 5 mm / min. The load and displacement were measured over time. In this push-out test, the peel circumference (mm) of the sample when the displacement is 40 mm is measured. 12. A silicone-modified (meth)acrylic copolymer resin having a structural unit N having a reactive silyl group in the molecule, The average adhesion when dry - average adhesion when wet measured according to the procedure below is 1.0 N / mm 2 1. A composition comprising: (Adhesion measurement procedure) - Preparation of test boards Mortar prepared according to the method specified in JIS R 5201, 10.4 (How to prepare a test specimen) is molded using a metal formwork with inner dimensions of 70mm x 70mm x 20mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it is demolded and cured in water at 20±2°C for 6 days, and then left to stand in a curing room for a further 7 days or more. After that, the underside of the molded specimen is polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface areas, and the surface is cleaned to prepare a test substrate. -Preparation of test specimen Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. The test substrate is immersed in water for one day, then taken out of the water and the water on the surface is wiped off (wetting treatment). Immediately after, the composition was applied to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 ] and dried for 24 hours at 23°C and 50% relative humidity to form a base layer. The above-obtained surface protection composition was applied on the base layer in a coating amount of 1.5 [kg / m 2 ] and leave it at 23°C and 50% relative humidity for 7 days to form a surface protective layer and prepare a wet test specimen. In addition, the composition and the surface protecting composition are similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment to prepare a dry test specimen. Adhesion strength measurement The wet test specimen is placed horizontally in a curing chamber, adhesive is applied to the surface on which the primer layer is formed, and a steel jig for upper tension is gently placed on top and attached by lightly rubbing it. Any adhesive that has protruded to the edges is wiped off, and after leaving it to rest for 24 hours, a tensile force is applied vertically to the test specimen surface and the maximum tensile load (N) is determined for each of the three test specimens. The load rate until breakage is 1500N / min. Adhesion strength (N / mm 2 ) is calculated using the formula "maximum tensile load (N) / 1600" and expressed as the average of three measured values. However, after making a 40mm x 40mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load is determined using the lower tensile steel jig and a steel backing plate. The adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength." Effect of the Invention

[0007] According to the present invention, there are provided a composition capable of forming a coating film having excellent adhesion per unit area on the surface of a porous body, and a surface protection method using the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram for explaining an adhesion test. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a test device used in a push-out test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The composition of the present embodiment will be described.

[0010] The composition of one embodiment of the present invention contains a silicone-modified (meth)acrylic copolymer resin, and has an upper limit of the peel circumference (displacement: 40 mm) in a dry state, measured according to the following procedure, of 700 mm or less, preferably 690 mm or less, and more preferably 680 mm or less. Further, the lower limit of the peeling perimeter (displacement: 40 mm) during drying is not particularly limited, but may be, for example, 300 mm or more, or 400 mm or more.

[0011] (Procedure for measuring the peeling perimeter) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, and a cylindrical punch indenter with a diameter of 100 mm and a thickness of 55 mm±3 mm was formed on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. Next, the composition was applied to the surface of the test substrate using a roller in a coating amount of 0.15 [kg / m 2 ] and then cure for one day at 23±2°C and a relative humidity of 50±20% to form a dry base layer. On top of that layer, the surface protection composition obtained above was applied in a coating amount of 1.50 [kg / m 2 The mixture was left to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. A sample having an undercoat layer and a surface protective layer was obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate and the indenter was broken at room temperature of 23°C, and then the indenter was applied toward the sample at 5 mm / min. The load and displacement were measured over time. In this push-out test, the peel circumference (mm) of the sample when the displacement is 40 mm is measured.

[0012] In another embodiment of the present invention, the composition contains a silicone-modified (meth)acrylic copolymer resin, and the upper limit of |average adhesive strength when dry--average adhesive strength when wet|, measured according to the following procedure, is 1.0 N / mm 2 Less than or equal to 0.8N / mm 2 Less than or equal to 0.5N / mm 2 It satisfies the following: The lower limit of |average adhesive strength in dry state--average adhesive strength in wet state| is not particularly limited, but may be, for example, 0 N / mm 2 It may be more than that.

[0013] (Adhesion measurement procedure) - Preparation of test boards Mortar prepared according to the method specified in JIS R 5201, 10.4 (How to prepare a test specimen) is molded using a metal formwork with inner dimensions of 70mm x 70mm x 20mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it is demolded and cured in water at 20±2°C for 6 days, and then left to stand in a curing room for a further 7 days or more. After that, the underside of the molded specimen is polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface areas, and the surface is cleaned to prepare a test substrate. -Preparation of test specimen Here, 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. The test substrate is immersed in water for one day, then taken out of the water and the water on the surface is wiped off (wetting treatment). Immediately after, the composition was applied to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 ] and dried for 24 hours at 23°C and 50% relative humidity to form a base layer. The above-obtained surface protection composition was applied on the base layer in a coating amount of 1.5 [kg / m 2 ] and leave it at 23°C and 50% relative humidity for 7 days to form a surface protective layer and prepare a wet test specimen. In addition, the composition and the surface protecting composition are similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment to prepare a dry test specimen. Adhesion strength measurement The wet test specimen is placed horizontally in a curing chamber, adhesive is applied to the surface on which the primer layer is formed, and a steel jig for upper tension is gently placed on top and attached by lightly rubbing it. Any adhesive that has protruded to the edges is wiped off, and after leaving it to rest for 24 hours, a tensile force is applied vertically to the test specimen surface and the maximum tensile load (N) is determined for each of the three test specimens. The load rate until breakage is 1500N / min. Adhesion strength (N / mm 2 ) is calculated using the formula "maximum tensile load (N) / 1600" and expressed as the average of three measured values. However, after making a 40mm x 40mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load is determined using the lower tensile steel jig and a steel backing plate. The adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength."

[0014] The composition of the present embodiment is a composition for coating a porous body used for coating the surface of a porous body, but may be any of a primer composition, an undercoat paint, or a topcoat paint, and is preferably a primer composition.

[0015] According to the findings of the present inventors, it has been found that by using the peeling circumference when dry and |average adhesion when dry - average adhesion when wet| as indicators and appropriately controlling these, the adhesion per unit area of ​​the composition to the surface of the porous body can be improved.

[0016] In this embodiment, it is possible to control the peeling circumference when dry and |average adhesion when dry - average adhesion when wet| by appropriately selecting, for example, the type and amount of each component contained in the composition, the preparation method of the composition, etc. Among these, for example, appropriately adjusting the weight average molecular weight of the silicone modified (meth)acrylic copolymer resin, and including a structural unit O having a terminal hydroxyl group and / or a structural unit P having a perfluoroalkyl group in the silicone modified (meth)acrylic copolymer resin are listed as elements for setting the peeling circumference when dry and |average adhesion when dry - average adhesion when wet| within the desired numerical range.

[0017] In addition, silicone-modified (meth)acrylic copolymers are also known as materials that have a low environmental impact, making it possible to realize primer compositions with excellent low toxicity.

[0018] The porous body is preferably a concrete structure, but is not limited thereto. The porous body may be a member having independent pores and / or continuous pores formed on the surface. At least the surface of such a member may be made of an inorganic material. Furthermore, examples of concrete structures include, but are not limited to, parts of viaduct structures and the like, and include those used outdoors.

[0019] The composition of the present embodiment may contain a structural unit N having a reactive silyl group, and preferably contains a silicone-modified (meth)acrylic copolymer having a structural unit N represented by the following general formula (N) in the molecule.

[0020] [ka]

[0021] In the above general formula (N), R 3 is a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 3 carbon atoms, R 5represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, b represents an integer of 1 to 6, and c represents an integer of 1 to 3. In the above general formula (N), R 3 is preferably a methyl group. In the above general formula (N), R 4 and R 5 may each be a methyl group or an ethyl group, and is preferably a methyl group. In the above general formula (N), b is preferably 2 to 5, and more preferably 3 to 4. In the above general formula (N), c is preferably 2 to 3, and more preferably 3.

[0022] The silicone-modified (meth)acrylic copolymer may contain a structural unit O having a terminal hydroxyl group, and preferably contains a structural unit O represented by the following general formula (O).

[0023] [ka]

[0024] In the above general formula (O), R 6 is a hydrogen atom or a methyl group. In the above general formula (O), d is preferably 1 to 8, and more preferably 2 to 5. By making it equal to or less than the above upper limit, the hydrophilicity can be adjusted, and by making it equal to or more than the above lower limit, the hydrophobicity can be adjusted.

[0025] The silicone-modified (meth)acrylic copolymer may contain a structural unit P having a perfluoroalkyl group, or may contain a structural unit P represented by the following general formula (P), which can improve the adhesive strength in a wet environment.

[0026] [ka]

[0027] In the above general formula (P), R 7 is a hydrogen atom or a methyl group, Cf is -CF3 or CHF2, e is an integer of 1 to 6, and f is an integer of 0 to 10. In the above general formula (P), f is preferably 0 to 7, and more preferably 0 to 6. By making it equal to or less than the above upper limit, it is possible to suppress a decrease in impregnation into wet concrete. By making it equal to or more than the above lower limit, it is possible to improve impregnation into wet concrete. Although the detailed mechanism is unclear, it is believed that since the surface tension of the composition can be appropriately adjusted by the amount of perfluoroalkyl groups in general formula (P), it is possible to improve impregnation into swollen concrete.

[0028] The content of the structural unit N contained in the silicone modified (meth)acrylic copolymer is C N The content of the structural unit P is C p , the content of the structural unit O is C O Let us assume that. In this embodiment, the content of each structural unit contained in the silicone-modified (meth)acrylic copolymer refers to the proportion (mol %) of each structural unit measured by NMR based on the constituent compound information obtained by pyrolysis GC-MS. The GC-MS conditions were as follows: Equipment: JMS Q1500GC&PY 3030E Pyrolysis furnace temperature: 600℃ GC inlet temperature: 280℃ Ion source temperature: 260℃ GC-IF temperature: 280℃ Ionization method: EI Column: ZB-5MS (20 m x inner diameter: 0.18 mm x film thickness: 0.18 μm) The NMR conditions were as follows: Equipment: Bruker AVANCE NEO Probe: CPBBO Deuterated solvent: CDCl3 As a pretreatment, add 0.4 mL of deuterated chloroform to dissolve.

[0029] The C calculated above p , C N C required from p / C Nis, for example, 0.001 or more and 1.0 or less, preferably 0.005 or more and 0.5 or less, more preferably 0.01 or more and 0.2 or less. By making it equal to or more than the lower limit, it is possible to improve the impregnation into concrete in a humid environment. On the other hand, by making it equal to or less than the upper limit, it is possible to achieve a balance between the impregnation into concrete and the adhesion to concrete.

[0030] In addition, the C calculated above O , C N C required from O / C N is, for example, 0.05 to 5.0, preferably 0.1 to 3.0, and more preferably 0.2 to 1.5. By making it equal to or more than the lower limit, the adhesion to the upper layer such as the intermediate coat layer can be improved. By making it equal to or less than the upper limit, the adhesion to the upper layer and the adhesion to concrete can be balanced.

[0031] The silicone-modified (meth)acrylic copolymer may contain a structural unit M having a (meth)acrylic group, or may contain a structural unit M represented by the following general formula (M).

[0032] [ka]

[0033] In the above general formula (M), R 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group having 1 to 3 carbon atoms, and a is an integer of 0 to 3. In addition, in the above general formula (M), R 1 is preferably a methyl group. In the above general formula (M), R 2 is preferably a methyl group or an ethyl group, and more preferably a methyl group. In the above general formula (M), a is preferably 2 or less, more preferably 1 or less, and even more preferably 0.

[0034] The silicone-modified (meth)acrylic copolymer may contain a structural unit L represented by the following general formula (L).

[0035] [ka]

[0036] In the above general formula (L), R 7 is a hydrogen atom or a methyl group, R 8 is an alkyl group having 1 to 3 carbon atoms, and g is an integer of 4 to 16. In the above general formula (L), R 8 may be a methyl group or an ethyl group, and is preferably a methyl group. In the above general formula (L), g is preferably 4 to 15, more preferably 4 to 10, and even more preferably 4 to 6. By adjusting it to the upper limit or less, hydrophilicity is improved, and adhesion to concrete can be improved even in a wet environment.

[0037] The weight average molecular weight (Mw) of the silicone modified (meth)acrylic copolymer is, for example, 500 or more and 50,000 or less, preferably 1,000 or more and 45,000 or less, and more preferably 1,500 or more and 40,000 or less. By setting the thickness to be equal to or greater than the lower limit, the adhesion and film-forming properties of the primer layer can be improved, whereas by setting the thickness to be equal to or less than the upper limit, the maximum displacement in a push-out test can be increased. In the present embodiment, the weight average molecular weight is, for example, a weight average molecular weight measured by gel permeation chromatography (GPC) (solvent: tetrahydrofuran (THF)) and converted into standard polystyrene.

[0038] The silicone-modified (meth)acrylic copolymer can be obtained, for example, by blending raw material components from which the respective structural units are derived and reacting them in a predetermined solvent in the presence of a catalyst. In this specification, the term "(meth)acrylic" means at least one of acrylic and methacrylic.

[0039] The composition of the present embodiment may contain a solvent, if necessary. The solvent may include, for example, a polar organic solvent. Examples of polar organic solvents include, but are not limited to, ether-based solvents, alcohol-based solvents, ketone-based solvents, ester-based solvents, etc. These may be used alone or in combination of two or more.

[0040] The solvent may contain, for example, a solvent having a boiling point of 50° C. or higher, preferably 100° C. or higher, more preferably 120° C. or higher. This can improve the film formation stability. The upper limit of the boiling point of the solvent is not particularly limited, but may be, for example, 300° C. or lower, or 250° C. or lower.

[0041] The composition may contain additives other than the above components as long as the effects of the present invention are not impaired. Examples of additives include silicone resins other than the silicone-modified (meth)acrylic copolymer, (meth)acrylic resins, fillers, pigments, ultraviolet absorbers, light stabilizers, antioxidants, silane coupling agents, thickeners, and the like.

[0042] The composition may be substantially free of epoxy resin, for example, may be configured to contain no epoxy resin or to have an epoxy resin content of 3 mass% or less in 100 mass% of the primer composition. That is, the composition is configured to contain substantially no epoxy resin that reacts with the silicone-modified (meth)acrylic copolymer. This allows the formation of an uncured primer layer.

[0043] The viscosity of the composition at a liquid temperature of 25° C. is, for example, 50 mPa·s to 3000 mPa·s, preferably 200 mPa·s to 2000 mPa·s, and more preferably 700 mPa·s to 900 mPa·s. By setting the viscosity to be equal to or greater than the lower limit, film-forming properties can be improved. By setting the viscosity to be equal to or less than the upper limit, in-plane thickness variations can be suppressed. The viscosity in this embodiment can be measured by a standard method using a Brookfield viscometer (B-type rotational viscometer) at 25° C. and a rotation speed of 10 rpm. In addition, in this specification, the symbol "to" indicates that the upper and lower limits are included, unless otherwise specified.

[0044] The content of the non-volatile components in the composition is, for example, 20% by mass to 100% by mass, preferably 30% by mass to 70% by mass, and more preferably 40% by mass to 60% by mass. Within such ranges, film-forming properties and handling properties can be improved.

[0045] The surface protection method of this embodiment will be described.

[0046] An example of a surface protection method includes a step of applying the above-mentioned composition to the surface of a porous body such as a concrete structure and drying it to form a layer. When the composition is a primer composition, a primer layer can be formed on the surface of the porous body. The surface protection method may also include a step of applying a surface protection composition onto the primer layer and drying the composition to form a surface protection layer.

[0047] First, in the process of forming a primer layer, silanol groups and terminal hydroxyl groups formed by hydrolysis of reactive silyl groups (groups containing silicon atoms bonded to alkoxy groups) in the silicone-modified (meth)acrylic copolymer form hydrogen bonds, chemical bonds, etc. between the primer layer and a surface composed of an inorganic material such as concrete.

[0048] The primer composition may be configured so that it does not contain a crosslinking agent and / or a curing catalyst, or the content of the crosslinking agent and / or the curing catalyst is 10% by mass or less, preferably 3% by mass or less, based on 100% by mass of the primer composition. In other words, the primer composition is configured so that it does not substantially contain a crosslinking agent that reacts with the silicone-modified (meth)acrylic copolymer. This makes it possible to suppress the crosslinking reaction of the silicone-modified (meth)acrylic copolymer during the film formation process of the primer layer.

[0049] On the other hand, when the surface protection composition contains a modified silicone resin and a crosslinking agent that reacts with silanol groups, the crosslinking agent penetrates from the surface protection layer toward the uncured primer layer during the film formation process of the surface protection layer, and the silicone-modified (meth)acrylic copolymer in the primer layer, the crosslinking agent, and the modified silicone resin in the surface protection layer can form a three-dimensional network structure, thereby improving the adhesion between the surface protection layer and the primer layer. When the modified silicone resin in the surface protective layer contains a polyol in its main chain that has low adhesion to the (meth)acrylic main chain in the silicone modified (meth)acrylic copolymer, the crosslinking mechanism described above is effective in improving the adhesion between the two. Furthermore, if the surface protective layer contains a curing catalyst, this curing catalyst also permeates the uncured primer layer and accelerates the curing reaction of the silicone-modified (meth)acrylic copolymer itself, resulting in a primer layer with excellent mechanical strength.

[0050] Here, an example of the surface protecting composition will be described.

[0051] The modified silicone resin refers to a polymer having a reactive silyl group, and includes those in which a reactive silyl group is added to a polymer that serves as the main chain. The polymer to which the reactive silyl group is added is not particularly limited, but examples thereof include polyether polymers such as polyoxyethylene, polyoxypropylene, and polyoxybutylene; aliphatic hydrocarbon polymers such as polyisoprene, polyisobutylene, and polybutadiene; (meth)acrylic polymers such as poly(meth)acrylic acid and poly(meth)acrylate; and polyester polymers. These may be used alone or in combination of two or more.

[0052] As the crosslinking agent, for example, a silane coupling agent is used. Examples of silane coupling agents include aminosilane compounds such as 3-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; epoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane; vinylsilane compounds such as γ-(meth)acryloxypropyltrimethoxysilane; cationic silane compounds such as N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride; and phenylsilane compounds. The content of the crosslinking agent in the total amount of the resin composition is preferably 0.1 to 7.5 mass %, more preferably 0.5 to 5 mass %, and further preferably 1.0 to 3 mass %.

[0053] In addition to the above components, the surface protection composition may contain one or more selected from the group consisting of a silicone resin other than the above modified silicone, a filler, a curing catalyst, an organic pigment, an inorganic pigment, an ultraviolet absorber, and a light stabilizer.

[0054] The filler may be an inorganic filler or an organic filler. The inorganic filler is not particularly limited, but examples thereof include silica; oxides such as alumina, titanium oxide, and magnesium oxide; carbonates such as calcium carbonate and magnesium carbonate; hydroxides such as aluminum hydroxide and magnesium hydroxide; and inorganic fibers such as glass fibers.

[0055] Among these, it is preferable to use one or more selected from the group consisting of silica particles, aluminum particles, and calcium carbonate particles. By using such a filler, dripping tends to be suppressed.

[0056] The average particle size of the filler is preferably 400 nm or less, more preferably 1 to 200 nm, even more preferably 1 to 100 nm, and even more preferably 1 to 50 nm. When the average particle size is within the above range, dripping tends to be suppressed. In this embodiment, the average particle size refers to the primary particle size on a volume basis. The primary particle size can be measured by a laser diffraction scattering method.

[0057] The content of the filler in the total amount of the resin composition is preferably 1 to 15 mass%, more preferably 1.5 to 10 mass%, and further preferably 2.0 to 8 mass%. When the content of the filler is within the above range, dripping tends to be suppressed.

[0058] The curing catalyst is not particularly limited as long as it catalyzes the reaction of a reactive silyl group, and examples thereof include tin-based catalysts, titanium-based catalysts, aluminum-based catalysts, zinc-based catalysts, iron-based catalysts, and phosphorus-based catalysts.

[0059] The surface protection method may include a step of forming a topcoat layer on the surface protection layer (intermediate coat layer), which can further improve weather resistance and the like. The topcoat layer is not particularly limited, but may contain, for example, one or more selected from the group consisting of fluororesin, (meth)acrylic resin, (meth)acrylic silicone resin, (meth)acrylic resin, urethane resin, olefin resin, vinyl acetate resin, ethylene-vinyl acetate copolymer resin, silicone resin, and modified resins thereof.

[0060] The surface protecting composition set of the present embodiment includes the above-mentioned primer composition and a surface protecting composition containing a modified silicone resin and a crosslinking agent that reacts with a silanol group. By carrying out a surface protection method using such a surface protection composition set, it is possible to improve both the adhesion of the primer layer to the porous body and the adhesion of the primer layer to the surface protection layer.

[0061] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0062] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0063] <Synthesis of silicone-modified methacrylic copolymer> (Silicone modified methacrylic copolymer A) 94 g of methyl methacrylate, 106 g of 3-(trimethoxysilyl)propyl methacrylate, 2 g of azobisisobutyronitrile, and 200 g of methyl isobutyl ketone were placed in a flask equipped with a stirrer, a condenser, and a thermometer, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer A having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer A had a weight average molecular weight of 35,000 in terms of polystyrene as measured by GPC, and n was 47 mol % and m was 53 mol % when n+m was 100 mol %.

[0064] [ka]

[0065] (Silicone modified methacrylic copolymer B) 94 g of methyl methacrylate, 106 g of 3-(trimethoxysilyl)propyl methacrylate, 4 g of azobisisobutyronitrile, and 200 g of methyl isobutyl ketone were placed in a flask equipped with a stirrer, a condenser, and a thermometer, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer B having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer B had a weight average molecular weight of 18,000 in terms of polystyrene measured using GPC, and n was 47 mol % and m was 53 mol % when n+m was 100 mol %.

[0066] [ka]

[0067] (Silicone-modified methacrylic copolymer C) A flask equipped with a stirrer, a condenser, and a thermometer was charged with 50 g of methyl methacrylate, 18 g of 3-(trimethoxysilyl)propyl methacrylate, 72 g of butyl methacrylate, 54 g of 2-hydroxyethyl methacrylate, 6 g of 2-propenoic acid, 2-methyl-,3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluorooctyl ester, and 2 g of azobisisobutyronitrile, along with 200 g of methyl isobutyl ketone, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer C having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer C had a weight average molecular weight of 17,000 in terms of polystyrene as measured using GPC, and when n+m+L+X+Z was taken as 100 mol%, n was 25 mol%, m was 36 mol%, L was 9 mol%, X was 27 mol%, and Z was 3 mol%.

[0068] [ka]

[0069] (Silicone-modified methacrylic copolymer D) A flask equipped with a stirrer, a condenser, and a thermometer was charged with 52 g of methyl methacrylate, 20 g of 3-(trimethoxysilyl)propyl methacrylate, 74 g of butyl methacrylate, 54 g of 2-hydroxyethyl methacrylate, 2 g of azobisisobutyronitrile, and 200 g of methyl isobutyl ketone, and the mixture was reacted at 110°C for 3 hours to obtain a silicone-modified methacrylic copolymer D having a structure represented by the following chemical formula. The resulting silicone-modified methacrylic copolymer D had a weight average molecular weight of 19,000 in terms of polystyrene as measured using GPC, and when n+m+L+X was taken as 100 mol%, n was 26 mol%, m was 37 mol%, L was 10 mol%, and X was 27 mol%.

[0070] [ka]

[0071] The proportions of each component in the silicone-modified methacrylic copolymers A to D obtained above were measured by NMR based on the information on the constituent compounds obtained by pyrolysis GC-MS according to the following conditions. The GC-MS conditions were as follows: Equipment: JMS Q1500GC&PY 3030E Pyrolysis furnace temperature: 600℃ GC inlet temperature: 280℃ Ion source temperature: 260℃ GC-IF temperature: 280℃ Ionization method: EI Column: ZB-5MS (20 m x inner diameter: 0.18 mm x film thickness: 0.18 μm) The NMR conditions were as follows: Equipment: Bruker AVANCE NEO Probe: CPBBO Deuterated solvent: CDCl3 As a pretreatment, 0.4 mL of deuterated chloroform was added to dissolve the sample.

[0072] <Adjustment of Composition> The obtained silicone-modified methacrylic copolymer A was added to and mixed with 50% of methoxypropyl acetate (PGMAC, boiling point 146°C) to obtain composition A with a non-volatile content of 45% and a viscosity of 600 mPa·s. The obtained silicone-modified methacrylic copolymer B was added to the same solvent and mixed to obtain composition B having a non-volatile content of 50% and a viscosity of 600 mPa·s. The obtained silicone-modified methacrylic copolymer C was added to the same solvent and mixed to obtain composition C having a non-volatile content of 50% and a viscosity of 800 mPa·s. The obtained silicone-modified methacrylic copolymer D was added to the same solvent and mixed to obtain composition C having a non-volatile content of 50% and a viscosity of 850 mPa·s.

[0073] [Table 1]

[0074] <Surface protection composition> 80 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: XB502, viscosity at 25°C: 2000mPas, modified silicone resin having two or more silicon atoms bonded to methoxy groups at each end, having a polyoxypropylene structure as a polyether polymer, and having a dimethoxymethylsilyl group as a reactive silyl group), 20 parts by weight of modified silicone resin (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: E30, viscosity at 25°C: 30000mPas, modified silicone resin having one silicon atom bonded to a methoxy group at each end, having a polyoxypropylene structure as a polyether polymer, and having a dimethoxymethylsilyl group as a reactive silyl group), and 6 parts by weight of silica particles (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: H18, average particle size: 10nm) were added and stirred for 5 minutes to obtain a base agent. The obtained base material and 3-aminopropyltrimethoxysilane, which is a crosslinking agent, were mixed in a mass ratio of 100:4 to prepare a surface protecting composition.

[0075] <Adhesion test> In accordance with JIS-A6909:2014, the adhesion of the above composition in the wet and dry states was measured according to the following procedure.

[0076] - Preparation of test boards Mortar prepared according to the method specified in JIS R 5201, 10.4 (How to prepare a test specimen) was molded using a metal formwork with inner dimensions of 70mm x 70mm x 20mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it was demolded and cured in water at 20±2°C for 6 days, and then left to stand in a curing room for a further 7 days or more.The bottom surface of the molded specimen was then polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface areas, and the surface was cleaned to prepare a test substrate.

[0077] -Preparation of test specimen The test substrate was immersed in water for one day, taken out of the water, and the water on the surface was wiped off (wet treatment). Immediately afterwards, any one of the compositions A to D obtained above was applied as a primer composition to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 ] and dried at 23°C and 50% relative humidity for 24 hours to form a primer layer. The surface protection composition obtained above was applied on the primer layer in a coating amount of 1.5 [kg / m 2 ] and left to stand at 23°C and 50% relative humidity for 7 days to form a surface protective layer, thereby preparing a wet test specimen. Furthermore, the composition and the surface protecting composition were similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment, to prepare a dry test specimen.

[0078] Adhesion strength measurement The wet test specimens were placed horizontally in a curing chamber and adhesive (solvent-free two-component epoxy resin adhesive, Konishi, Quickmender) was applied to the surface on which the primer layer was formed. A steel jig for upper tension was then gently placed on top and attached by lightly rubbing it, as shown in Figure 1(a), and any adhesive that had protruded out from the edges was wiped off. After leaving the specimens to rest for 24 hours, a tensile force was applied vertically to the surface of the specimen as shown in Figure 1(b), and the maximum tensile load (N) was determined for each of the three test specimens. The load rate until breakage was 1500 N / min. Adhesion strength (N / mm 2) is calculated using the formula "maximum tensile load (N) / 1600" and expressed as the average of three measured values. However, after making a 40 mm x 40 mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load was determined using the lower tensile steel jig and a steel backing plate. In Table 1, the adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength."

[0079] In addition, when the fracture mode of the above adhesion test was confirmed, the fracture surfaces of Examples 2 and 3 were between the porous body surface and the primer layer, while the fracture surface of Comparative Example 1 was between the primer layer and the surface protection layer.

[0080] (Push-out test) A push-out test was carried out using a test device shown in FIG. 2 in accordance with JSCE K 533, and the displacement (mm) and load (kN) were measured for the sample 20 formed on the surface of the test substrate 10. FIG. 2(a) is a cross-sectional view of the test device, and FIG. 2(b) is a perspective view of the test device. The specific procedure for the push-through test was as follows. In accordance with the preparation of test specimens in JSCE K 533, concrete with a water / cement ratio of 44% and a sand / cement ratio of 2.7 was placed in a metal formwork with internal dimensions of 400 mm length x 600 mm width x 60 mm thickness, and cured for 24 hours at a temperature of 20±2°C and a relative humidity of 80% or more, after which it was demolded and cured in water for 6 days at a temperature of 20±2°C. After the underwater curing was completed, it was cured for 7 days or more at a temperature of 23±2°C and a relative humidity of 50±5%, to produce a concrete plate (porous body) in the shape of a top cover for a top cover type U-shaped gutter (not shown) as specified in JIS A 5372 Appendix E (Type 1, 300). Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, forming a cylindrical punch indenter 30 with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate 10. Next, the surface (the application surface) of the test substrate 10 was scraped using a disk sander, and then degreased. Next, any one of the compositions A to D obtained above was applied as a primer composition to the surface of the test substrate 10 using a roller in an amount of 0.15 [kg / m 2 ] and then cured for one day at 23±2°C and a relative humidity of 50±20% to form a dry primer layer. Onto the primer layer, the surface protective composition obtained above was applied in a coating amount of 1.50 [kg / m 2 The mixture was left to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. Sample 20 having a primer layer and a surface protective layer was obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min at room temperature of 23° C. until the bond between the test substrate 10 and the punch indenter 30 was broken, and then the punch indenter 30 was applied toward the sample 20 at 5 mm / min. At this time, the load and the amount of displacement were measured over time. The load was terminated when the sample 20 broke or when the peeling of the sample 20 reached the end face of the test substrate 10. The load and the amount of displacement were recorded every 0.05 kN, and the load was temporarily interrupted every 10 mm of the amount of displacement, and the peeled area was marked on the sample 20 and the load was recorded. In this push-out test, the load (kN) was measured when the displacement was 40 mm. The peel circumference (mm) of sample 20 was also measured when the displacement was 40 mm. Using these, Table 1 shows "load when the displacement is 40 mm" / "peel circumference when the displacement is 40 mm" as an index of adhesive strength per unit area.

[0081] Compared with Comparative Example 1, the compositions of Examples 1 to 3 exhibited better adhesive strength per unit area to the surface of a porous body in a dry state.

[0082] 10 Test Board 20 Samples 30 Push-out indenter

Claims

1. A composition for use in applying to a surface of a porous body, comprising: The silicone-modified (meth)acrylic copolymer resin includes a structural unit N having a reactive silyl group in the molecule, A composition having a peel circumference (displacement: 40 mm) when dry of 700 mm or less, as measured according to the following procedure. (Procedure for measuring peel perimeter) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, to form a cylindrical punch indenter with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. Here, 80 parts by weight of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: E30), and 6 parts by weight of silica particles (manufactured by Wacker Asahi Kasei Silicone, product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. Next, the composition was applied to the surface of the test substrate using a roller in a coating amount of 0.15 [kg / m 2 ] and then cured for one day at 23±2° C. and a relative humidity of 50±20% to form a dry undercoat layer. Onto this layer, the surface protecting composition obtained above was applied in a coating amount of 1.50 [kg / m 2 ] and allowed to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. A sample having an undercoat layer and a surface protective layer is obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate and the punch indenter was broken at room temperature of 23° C., and then the punch indenter was applied toward the sample at 5 mm / min. At this time, the load and the amount of displacement were measured over time. In this push-out test, the peel circumference (mm) of the sample is measured when the displacement is 40 mm.

2. A composition for use in applying to a surface of a porous body, comprising: The silicone-modified (meth)acrylic copolymer resin includes a structural unit N having a reactive silyl group in the molecule, |Average dry adhesion - average wet adhesion| is 1.0 N / mm 2 1. A composition comprising: (Procedure for measuring adhesion) ・Preparation of test boards Mortar prepared by the method specified in 10.4 (Preparation of test specimens) of JIS R 5201 is molded using a metal formwork with inner dimensions of 70 mm x 70 mm x 20 mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it is demolded and cured in water at 20±2°C for 6 days and then left to stand in a curing room for a further 7 days or more. After that, the underside of the molded part is polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface parts, and the surface is cleaned to prepare a test substrate. ・Preparation of test specimen Here, 80 parts by weight of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: XB502), 20 parts by weight of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: E30), and 6 parts by weight of silica particles (manufactured by Wacker Asahi Kasei Silicone, product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. The test substrate is immersed in water for one day, taken out from the water, and the water on the surface is wiped off (wet treatment). Immediately after, the composition was applied to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 On the undercoat layer, the surface protecting composition obtained above is applied in a coating amount of 1.5 [kg / m]. 2 ] and allowed to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer, thereby preparing a test specimen in a wet state. In addition, the composition and the surface protecting composition are similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment to prepare a dry test specimen. - Measurement of adhesion strength The wet test specimens are placed horizontally in a curing chamber, adhesive is applied to the surface on which the primer layer is formed, and a steel jig for upper tension is gently placed on top and attached by lightly rubbing. Any adhesive that has protruded to the edges is wiped off, and after leaving the specimens to stand for 24 hours, a tensile force is applied vertically to the surface of the test specimen to determine the maximum tensile load (N) for each of the three test specimens. The load rate until breakage is 1500 N / min. Adhesion strength (N / mm 2 ) was calculated by the formula "maximum tensile load (N) / 1600" and expressed as the average value of three measured values. However, after making a 40 mm x 40 mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load is determined using the lower tensile steel jig and a steel backing plate. The adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength."

3. 3. The composition according to claim 1 or 2, A composition having a viscosity of 50 mPa·s or more and 3000 mPa·s or less, measured using a Brookfield viscometer at 25° C. and a rotation speed of 10 rpm.

4. 3. The composition according to claim 1 or 2, A composition, wherein the silicone-modified (meth)acrylic copolymer resin has a structural unit O having a terminal hydroxyl group in the molecule.

5. 3. The composition according to claim 1 or 2, A composition, wherein the silicone-modified (meth)acrylic copolymer resin has a structural unit P having a perfluoroalkyl group in the molecule.

6. 3. The composition according to claim 1 or 2, A composition, wherein the silicone-modified (meth)acrylic copolymer resin has a structural unit M having a (meth)acrylic group in the molecule.

7. 3. The composition according to claim 1 or 2, The silicone-modified (meth)acrylic copolymer resin has a weight average molecular weight (Mw) of 500 or more and 50,000 or less.

8. 3. The composition according to claim 1 or 2, The composition, wherein the porous body is a concrete structure.

9. 3. The composition according to claim 1 or 2, The composition is a primer composition.

10. A surface protection method comprising the steps of applying the composition according to claim 1 or 2 to a surface of a porous body and drying the composition to form a layer.

11. The silicone-modified (meth)acrylic copolymer resin includes a structural unit N having a reactive silyl group in the molecule, A composition having a peel circumference (displacement: 40 mm) when dry of 700 mm or less, as measured according to the following procedure. (Procedure for measuring peel perimeter) A concrete slab (porous body) in the shape of a top cover for a U-shaped gutter with a top cover as specified in JIS A 5372 Appendix E (Type 1, 300) is prepared. Next, the obtained concrete plate was ground from the back side until it reached a position 5 mm from the front surface, to form a cylindrical punch indenter with a diameter of 100 mmφ and a thickness of 55 mm±3 mm on the test substrate. Next, the surface of the test substrate is scraped using a disk sander and then degreased. Here, 80 parts by mass of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: XB502), 20 parts by mass of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: E30), and 6 parts by mass of silica particles (manufactured by Wacker Asahi Kasei Silicone, product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. Next, the composition was applied to the surface of the test substrate using a roller in a coating amount of 0.15 [kg / m 2 ] and then cured for one day at 23±2° C. and a relative humidity of 50±20% to form a dry undercoat layer. Onto this layer, the surface protecting composition obtained above was applied in a coating amount of 1.50 [kg / m 2 ] and allowed to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer. A sample having an undercoat layer and a surface protective layer is obtained. Next, in accordance with JSCE K 533, a load was applied at 1 mm / min until the bond between the test substrate and the punch indenter was broken at room temperature of 23° C., and then the punch indenter was applied toward the sample at 5 mm / min. At this time, the load and the amount of displacement were measured over time. In this push-out test, the peel circumference (mm) of the sample is measured when the displacement is 40 mm.

12. The silicone-modified (meth)acrylic copolymer resin includes a structural unit N having a reactive silyl group in the molecule, |Average dry adhesion - average wet adhesion| is 1.0 N / mm 2 1. A composition comprising: (Procedure for measuring adhesion) ・Preparation of test boards Mortar prepared by the method specified in 10.4 (Preparation of test specimens) of JIS R 5201 is molded using a metal formwork with inner dimensions of 70 mm x 70 mm x 20 mm, and left to stand for 24 hours at a temperature of 20±2°C and humidity of 80% or more, after which it is demolded and cured in water at 20±2°C for 6 days and then left to stand in a curing room for a further 7 days or more. After that, the underside of the molded part is polished with P180 abrasive paper specified in JIS R 6252 to remove the release agent and weak surface parts, and the surface is cleaned to prepare a test substrate. ・Preparation of test specimen Here, 80 parts by mass of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: XB502), 20 parts by mass of modified silicone resin (manufactured by Wacker Asahi Kasei Silicone, product name: E30), and 6 parts by mass of silica particles (manufactured by Wacker Asahi Kasei Silicone, product name: H18) are added and stirred for 5 minutes to obtain a base material. The obtained base material is mixed with 3-aminopropyltrimethoxysilane, a crosslinking agent, in a mass ratio of 100:4 to prepare a surface protection composition. The test substrate is immersed in water for one day, taken out from the water, and the water on the surface is wiped off (wet treatment). Immediately after, the composition was applied to the surface of the wet test substrate in an amount of 0.15 [kg / m 2 On the undercoat layer, the surface protecting composition obtained above is applied in a coating amount of 1.5 [kg / m]. 2 ] and allowed to stand at 23° C. and a relative humidity of 50% for 7 days to form a surface protective layer, thereby preparing a test specimen in a wet state. In addition, the composition and the surface protecting composition are similarly applied to the surface of a test substrate in a dry state without being subjected to a moistening treatment to prepare a dry test specimen. - Measurement of adhesion strength The wet test specimens are placed horizontally in a curing chamber, adhesive is applied to the surface on which the primer layer is formed, and a steel jig for upper tension is gently placed on top and attached by lightly rubbing. Any adhesive that has protruded to the edges is wiped off, and after leaving the specimens to stand for 24 hours, a tensile force is applied vertically to the surface of the test specimen to determine the maximum tensile load (N) for each of the three test specimens. The load rate until breakage is 1500 N / min. Adhesion strength (N / mm 2 ) was calculated by the formula "maximum tensile load (N) / 1600" and expressed as the average value of three measured values. However, after making a 40 mm x 40 mm square cut around the four sides of the upper tensile steel jig attached to the test specimen, reaching the base plate, the maximum tensile load is determined using the lower tensile steel jig and a steel backing plate. The adhesion strength obtained using the dry test specimen is referred to as the "average dry adhesion strength," and the adhesion strength obtained using the wet test specimen is referred to as the "average wet adhesion strength."

Citation Information

Patent Citations

  • Method for improving tiled wall

    JP1994033565A