Method for producing nickel diatomaceous earth catalyst

By selecting diatomaceous earth with a high specific surface area increase in sodium carbonate and optimizing nickel precipitation, the method produces a nickel diatomaceous earth catalyst with improved hydrogenation activity and reduced nickel elution.

JP2024140688APending Publication Date: 2024-10-10JGC CATALYSTS & CHEMICALS LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023051978
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing methods for producing nickel diatomaceous earth catalysts face challenges in achieving high hydrogenation activity when using diatomaceous earth with a small initial specific surface area.

Method used

A production method that involves selecting diatomaceous earth with a high specific surface area increase rate in an aqueous sodium carbonate solution, adjusting pH during nickel precipitation, and aging the catalyst precursor to enhance pore formation and nickel deposition.

Benefits of technology

The method results in a nickel diatomaceous earth catalyst with enhanced catalytic activity, as evidenced by higher hydrogenation activity and reduced nickel elution, even when starting with diatomaceous earth with a small initial specific surface area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140688000001
    Figure 2024140688000001
Patent Text Reader

Abstract

To provide a production method capable of obtaining a nickel diatomaceous earth catalyst having high hydrogenation activity even when diatomaceous earth having a small initial specific surface area is used.SOLUTION: There is provided a method for producing a nickel diatomaceous earth catalyst for a hydrogenation reaction, which comprises: an acidic suspension preparation step of adding soluble nickel and diatomaceous earth to water to prepare an acidic suspension; a step of dissolving sodium carbonate in water to prepare a basic aqueous solution; a neutralization treatment step of adding the basic aqueous solution to the acidic suspension to form a raw material slurry, followed by forming a catalyst precursor in which nickel is deposited on diatomaceous earth; a separation step of solid-liquid separating the catalyst precursor from the raw material slurry; and a sintering step of sintering the separated catalyst precursor, wherein diatomaceous earth having an increase rate in specific surface area in a sodium carbonate aqueous solution of 60% or more is used.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nickel diatomaceous earth catalyst. [Background technology]

[0002] There is a known method of generating ethane by passing ethylene and hydrogen over reduced nickel (metallic nickel), and various nickel catalysts using this nickel as the active ingredient have been developed to date. A representative nickel catalyst is the nickel-diatomaceous earth catalyst, in which nickel is supported on the surface of diatomaceous earth. In nickel-diatomaceous earth catalysts, nickel acts as the active ingredient, and diatomaceous earth acts as a carrier to disperse the active ingredient.

[0003] Non-Patent Document 1 discloses a general method for producing nickel diatomaceous earth catalysts, in which diatomaceous earth is added to an aqueous solution of nickel nitrate (industrially nickel sulfate), and then an aqueous solution of sodium carbonate (or sodium hydroxide, ammonium carbonate) is added while stirring, causing basic nickel carbonate (or nickel hydroxide) to precipitate on the diatomaceous earth.

[0004] The catalytic activity of nickel diatomaceous earth catalysts is affected by various conditions even in the general manufacturing method of nickel diatomaceous earth catalysts mentioned above. One of these is the selection of diatomaceous earth. Diatomaceous earth is a natural mineral formed by the accumulation of fossilized shells of diatoms, a type of algae. The properties of diatomaceous earth vary greatly depending on the place of origin and the variety. For this reason, the selection of diatomaceous earth is important in the manufacture of nickel diatomaceous earth catalysts, and is considered from various perspectives.

[0005] For example, Patent Document 1 discloses a nickel catalyst containing nickel on a solid silica carrier, and discloses diatomaceous earth as a suitable solid silica carrier. This silica carrier is said to be highly porous, with a specific pore volume of about 0.4 to 2 ml / g, preferably about 1.6 to 1.8 ml / g.

[0006] Patent Document 2 also discloses a method for producing a nickel diatomaceous earth catalyst using a precipitation method. In this method, attention is paid to the calcined state of the diatomaceous earth, and it is disclosed that deposition of basic nickel carbonate on the diatomaceous earth is unlikely to occur if only the calcined product is used, whereas deposition on the nickel diatomaceous earth is likely to occur if only the uncalcined product is used. Furthermore, from the viewpoint of reducibility, a production method is disclosed in which diatomaceous earth is selected based on the amount of eluted Si when treated with a precipitant in an alkaline solution. Thus, various methods for selecting diatomaceous earth have been considered for producing nickel diatomaceous earth catalysts. [Prior art documents] [Non-patent literature]

[0007] [Non-Patent Document 1] "Catalyst Preparation," edited by Takayasu Shirasaki and Takayuki Todo, Kodansha, 1974 [Patent documents]

[0008] [Patent Document 1] Special Publication No. 2014-530098 [Patent Document 2] International Publication No. WO2017 / 077969 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention provides a production method that can obtain a nickel diatomaceous earth catalyst with high hydrogenation activity even when diatomaceous earth with a small initial specific surface area is used. [Means for solving the problem]

[0010] The present inventors have investigated a method for producing a nickel diatomaceous earth catalyst, focusing on the selection of diatomaceous earth. As a result, they have found that there are diatomaceous earths whose specific surface area increases significantly in the presence of sodium carbonate, and other diatomaceous earths whose specific surface area does not increase significantly in the presence of sodium carbonate. They have found that a nickel diatomaceous earth catalyst with high hydrogenation activity can be obtained by using this diatomaceous earth whose specific surface area increases significantly in the presence of sodium carbonate, and preferably by adjusting the pH of the solution during nickel precipitation and aging it, and have completed the production method of the present invention.

[0011] The manufacturing method of the present invention is a method for producing a nickel-diatomaceous earth catalyst, which includes an acidic suspension preparation step of adding soluble nickel and diatomaceous earth to water to prepare an acidic suspension, a step of dissolving sodium carbonate in water to prepare a basic aqueous solution, a neutralization step of adding the basic aqueous solution to the acidic suspension to form a raw material slurry to form a catalyst precursor in which nickel is deposited on the diatomaceous earth, a separation step of performing solid-liquid separation of the catalyst precursor from the raw material slurry, and a calcination step of calcining the separated catalyst precursor, and is characterized in that diatomaceous earth having a specific surface area increase rate of 60% or more in an aqueous sodium carbonate solution is used. Effect of the Invention

[0012] According to the manufacturing method of the present invention, even if diatomaceous earth with a small initial specific surface area is used, the specific surface area of ​​the diatomaceous earth is increased in the neutralization treatment and nickel is deposited thereon, thereby enhancing the catalytic effect of nickel and producing a nickel diatomaceous earth catalyst with high hydrogenation activity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The production method of the present invention will be described in detail below. [Production method of the present invention] The present invention is a method for producing a nickel-diatomaceous earth catalyst for hydrogenation reactions, comprising: an acidic suspension preparation step of adding soluble nickel and diatomaceous earth to water to prepare an acidic suspension; a step of dissolving sodium carbonate in water to prepare a basic aqueous solution; a neutralization step of adding the basic aqueous solution to the acidic suspension to form a raw material slurry to form a catalyst precursor in which nickel is deposited on the diatomaceous earth; a separation step of performing solid-liquid separation of the catalyst precursor from the raw material slurry; and a calcination step of calcining the separated catalyst precursor, wherein the method is characterized in that diatomaceous earth having a specific surface area increase rate of 60% or more in an aqueous sodium carbonate solution is used.

[0014] [Acid suspension preparation process] The manufacturing method of the present invention includes a step of preparing an acidic suspension by adding soluble nickel and diatomaceous earth to water to prepare an acidic suspension. The acidic suspension is a suspension in which diatomaceous earth is dispersed as a solid in an acidic aqueous solution in which nickel is dissolved.

[0015] As the soluble nickel used in the acidic suspension, at least one selected from nickel sulfate, nickel nitrate, nickel chloride, nickel carbonate, nickel acetate, etc. can be used. As nickel having good solubility in water, it is preferable to use at least one selected from nickel sulfate, nickel nitrate, nickel chloride, and nickel acetate. Even if it is not soluble in water, it can be dissolved in water with an acid. For example, a liquid in which metallic nickel is dissolved in sulfuric acid or nitric acid can be used as the soluble nickel.

[0016] The nickel concentration of the acidic suspension is preferably in the range of 1% by mass to 10% by mass, more preferably 3% by mass to 8% by mass, calculated as Ni. The pH of the acidic suspension is preferably in the range of 1.00 to 6.00, more preferably 3.00 to 6.00. By adjusting the nickel concentration and pH to these ranges, the productivity of the nickel diatomaceous earth catalyst having the effects of the present invention can be increased.

[0017] The diatomaceous earth used in the acidic suspension is one that exhibits an increase in specific surface area of ​​60% or more in an aqueous sodium carbonate solution. Diatomaceous earth is a natural mineral formed by the accumulation of fossilized shells of diatoms, a type of algae, and its properties vary greatly depending on the place of origin and the variety.

[0018] In general, when diatomaceous earth is used as a nickel catalyst carrier, it is required to use diatomaceous earth that is highly porous and has a large specific surface area in order to enhance the catalytic effect. Specifically, as described in Patent Document 1, the pore volume of the catalyst precursor is said to be about 0.4 to 2 ml / g, preferably about 1.6 to 1.8 ml / g. Also, Patent Document 2 states that the specific surface area of ​​the nickel diatomaceous earth catalyst is 50 to 180 m 2 However, because diatomaceous earth is a natural mineral, there are many different types, ranging from diatomaceous earth with a large specific surface area to diatomaceous earth with a small specific surface area, and the properties of diatomaceous earth vary from diatomaceous earth with a small specific surface area in a sodium carbonate aqueous solution to diatomaceous earth with a large specific surface area.

[0019] The manufacturing method of the present invention is capable of manufacturing a nickel diatomaceous earth catalyst with high catalytic activity by using diatomaceous earth as a raw material, which has a small initial specific surface area but has a high rate of increase in specific surface area in an aqueous sodium carbonate solution. Specifically, diatomaceous earth with a specific surface area increase rate of 60% or more in an aqueous sodium carbonate solution is used. It is believed that when an aqueous sodium carbonate solution is added to diatomaceous earth whose specific surface area increases, the sodium carbonate further forms pores in the diatomaceous earth.

[0020] The increase in the specific surface area of ​​diatomaceous earth in an aqueous sodium carbonate solution can be determined by comparing the specific surface area A of the diatomaceous earth before it is placed in the aqueous sodium carbonate solution with the specific surface area B of the diatomaceous earth after it is placed in the aqueous sodium carbonate solution. Specifically, for example, 100 mL of a 10% by mass aqueous sodium carbonate solution is added to 10 g of diatomaceous earth and kept at 70°C for 2 hours. The solid matter is then filtered and collected, and dried at 120°C for 12 hours. The specific surface area B of this dried solid matter is measured. This specific surface area B is compared to the specific surface area A before it is placed in the aqueous sodium carbonate solution, and the specific surface area increase rate X% is calculated from the following formula [1]. The specific surface areas A and B can be determined by BET specific surface area, etc. Specific surface area increase rate X%=(BA) / A×100 [1]

[0021] It is believed that by using diatomaceous earth, whose specific surface area increases in an aqueous sodium carbonate solution, many pores are formed in the diatomaceous earth at the same time that nickel precipitates are produced by the sodium carbonate, and the nickel precipitates penetrate into these pores and are fixed there, resulting in a nickel-diatomaceous earth catalyst with high hydrogenation activity.

[0022] In the manufacturing method of the present invention, the initial specific surface area is 1.0 m 2 / g or more ~100m 2 / g or less, and the initial specific surface area is 1.0 m 2 / g or more ~60m 2 / g or less can be used. In the manufacturing method of the present invention, diatomaceous earth having an initial pore volume of 0.005 mL / g or more and 0.200 mL / g or less can be used, and further, diatomaceous earth having an initial pore volume of 0.010 mL / g or more and 0.100 mL / g or less can be used. Even with such diatomaceous earth having a small initial specific surface area and pore volume, a nickel diatomaceous earth catalyst having a high hydrogenation activity can be obtained as long as the specific surface area increase rate in an aqueous sodium carbonate solution is 60% or more. In particular, even if diatomaceous earth having an initial pore volume of 0.010 mL / g or more and 0.050 mL / g or less is used, it is advantageous that a nickel diatomaceous earth catalyst having a high hydrogenation activity can be obtained.

[0023] The diatomaceous earth used in the acidic suspension may be any commercially available diatomaceous earth that meets the above conditions, or multiple commercially available products may be blended together to create a diatomaceous earth that meets the above conditions. Incidentally, the properties of diatomaceous earth vary greatly depending on the place of origin and variety, so even the same variety may have different properties depending on the place of origin. In such cases, it is advisable to adjust the blend ratio of the diatomaceous earth in advance to meet the above conditions.

[0024] The lower limit of the diatomaceous earth concentration in the acidic suspension is preferably 1% by mass or more, and the upper limit is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less. By lowering the diatomaceous earth concentration in the acidic suspension, the productivity of the nickel diatomaceous earth catalyst having the effects of the present invention can be increased.

[0025] The pH of the acidic suspension is preferably in the range of 3.00 to 7.00, more preferably 4.00 to 6.50, and particularly preferably 4.50 to 6.00. By controlling the pH of the acidic suspension within the above range, it is possible to suppress fluctuations in the specific surface area of ​​the diatomaceous earth.

[0026] [Basic aqueous solution preparation process] The production method of the present invention includes a step of dissolving sodium carbonate in water to prepare a basic aqueous solution. The pH of the basic aqueous solution is preferably in the range of 9.00 to 14.00, more preferably 10.00 to 13.00. The sodium concentration of the basic aqueous solution is in the range of 5% by mass to 30% by mass, preferably 10% by mass to 25% by mass. By controlling the pH of the basic aqueous solution within the above range, the productivity of the nickel diatomaceous earth catalyst having the effects of the present invention can be increased.

[0027] [Neutralization process] The manufacturing method of the present invention includes a neutralization step in which the basic aqueous solution is added to the acidic suspension to form a raw material slurry, and a catalyst precursor in which nickel is deposited on the diatomaceous earth is formed. In this step, the nickel dissolved in the acidic suspension is neutralized by the sodium in the basic aqueous solution to form a precipitate, which is deposited on the surface of the diatomaceous earth (including the surface of the pores) to form a solid (catalyst precursor). This catalyst precursor is dispersed in the raw material slurry. At the same time, the diatomaceous earth in the acidic suspension is eroded by nickel carbonate, pores are formed on the surface of the diatomaceous earth, and nickel is deposited in the pores. In this way, the formation of pores and the deposition of nickel proceed in parallel, resulting in a large area of ​​nickel deposition and an increased amount of nickel deposition.

[0028] In this step, it is preferable to adjust the pH of the raw material slurry to a basic range of 9.00 to 10.00 inclusive. By adjusting the pH of the raw material slurry to this range, the formation of pores on the surface of the diatomaceous earth is promoted.

[0029] In this step, the temperature of the acidic suspension and the basic aqueous solution is preferably in the range of 50° C. to 90° C., more preferably in the range of 60° C. to 80° C. By controlling the temperatures of the acidic suspension and the basic aqueous solution within the above range, deposition of dissolved nickel and formation of pores on the diatomaceous earth surface are promoted.

[0030] In this neutralization step, it is preferable to age the raw slurry. Specifically, it is preferable to age the raw slurry until the pH becomes 0.20 or more lower than the reference pH (pH becomes −0.20 or less than the reference pH), based on the pH of the raw slurry immediately after adding the entire amount of the basic aqueous solution to the acidic suspension.

[0031] The aging pH is preferably in the range of -0.20 to -0.50 lower than the reference pH, and more preferably in the range of -0.20 to -0.40 lower than the reference pH. This aging promotes the formation of pores in the diatomaceous earth and the deposition of nickel, making it possible to obtain a catalyst with high hydrogenation activity.

[0032] During this aging, it is preferable to maintain the raw slurry in a stirred state. The temperature of the raw slurry during aging is preferably in the range of 60° C. to 90° C., more preferably in the range of 70° C. to 90° C. By adjusting the temperature of the raw slurry within this range, aging is accelerated.

[0033] [Separation process] The production method of the present invention includes a separation step of performing solid-liquid separation of the catalyst precursor from the raw material slurry. The catalyst precursor can be separated from the raw material slurry by a conventionally known method. For example, a method of removing water using a dryer, a method of separating water by filtration, a method of separating water by centrifugation, etc. can be used.

[0034] The separated catalyst precursor may be washed with water or the like as necessary. For example, impurities (such as sulfate radicals, nitrate radicals, etc.) generated by the neutralization reaction can be removed. Specifically, impurities can be removed by suspension washing, in which the catalyst precursor is suspended in water and stirred, and then separated again, or flow washing, in which a washing liquid such as water is passed through the catalyst precursor to wash it. In particular, when the catalyst precursor contains a large amount of sulfate radicals, it is preferable to remove them by washing, since there is a risk of reducing the catalytic activity. Furthermore, when nitrate radicals are contained, they are removed by washing, since NO 2 is removed in the calcination step described later. X This can cause problems, so it is preferable to remove this as well by washing.

[0035] The separated catalyst precursor can be molded into various shapes as necessary. Specifically, it can be molded into a cylindrical tablet having a diameter of about 3 to 10 mm and a height of about 3 to 10 mm using a tableting machine, or into a cylindrical shape having a diameter of about 1 to 4 mm and a length of about 2 to 10 mm using an extrusion machine, or into a powder or granules using a mill or crusher.

[0036] [Firing process] The production method of the present invention includes a calcination step of calcining the recovered catalyst precursor. During the calcination step, nickel precipitate contained in the catalyst precursor is decomposed into nickel oxide to obtain a nickel diatomaceous earth catalyst.

[0037] The calcination means may be, for example, a muffle furnace, a rotary kiln, a gas furnace, or the like. The calcination temperature may be any temperature at which the nickel precipitate contained in the catalyst precursor is decomposed into nickel oxide. From the viewpoint of productivity, a calcination temperature of 300°C or more to 500°C or less is preferable. The calcination time may also be a time sufficient for the nickel precipitate contained in the catalyst precursor to be decomposed into nickel oxide. From the viewpoint of productivity, a calcination time of 1 hour or more to 24 hours or less is preferable. Furthermore, the calcination atmosphere may be any atmosphere at which the nickel precipitate contained in the catalyst precursor is decomposed into nickel oxide. For example, it may be an atmosphere that does not contain oxygen, or may be an atmosphere that contains oxygen. From the viewpoint of productivity, it is preferable to use an air atmosphere, and it is more preferable to perform the calcination in a state where the air is circulated.

[0038] In this step, the catalyst precursor may be calcined to obtain a nickel diatomaceous earth catalyst, and then the nickel oxide contained in the nickel diatomaceous earth catalyst may be reduced with hydrogen or the like. For example, the nickel diatomaceous earth catalyst may be held at a temperature of 350°C to 500°C, preferably 380°C to 450°C, in a hydrogen atmosphere for 1 hour to 48 hours, thereby reducing the nickel oxide to metallic nickel. In addition, metallic nickel may generate heat and burn if exposed to the air as it is due to an oxidation reaction, so after reduction to metallic nickel, oxygen may be gradually supplied to form a coating of nickel oxide on the surface of metallic nickel. In addition, carbon dioxide or the like may be adsorbed on the surface of metallic nickel. The nickel diatomaceous earth catalyst that has been subjected to such a treatment is also called a reduced and stabilized nickel diatomaceous earth catalyst.

[0039] [Nickel diatomaceous earth catalyst] The catalyst produced by the method of the present invention can be used as a nickel diatomaceous earth catalyst for hydrogenation reactions. This hydrogenation reaction is a reaction in which hydrogen is added to the unsaturated bond between carbon atoms to make it a saturated bond. For example, the nickel diatomaceous earth catalyst obtained by the production method of the present invention can be used in a reaction in which hydrogen is added to the double bond of ethylene to produce ethane, or in a reaction in which hydrogen is added to the double bond of benzene to produce cyclohexane. However, the nickel diatomaceous earth catalyst obtained by the production method of the present invention is not limited to these reactions.

[0040] These reactions are believed to occur on the surface of metallic nickel. Therefore, when using the nickel diatomaceous earth catalyst of the present invention for these reactions, the nickel oxide contained in the nickel diatomaceous earth catalyst is reduced to metallic nickel using hydrogen or the like before use. In this case, a reduced and stabilized nickel diatomaceous earth catalyst is preferable because it can reduce nickel oxide to metallic nickel in a short time.

[0041] The constituent elements of the nickel-diatomaceous earth catalyst obtained by the manufacturing method of the present invention are nickel derived from nickel oxide or metallic nickel, and silicon derived from diatomaceous earth. In addition to these, elements derived from impurities contained in diatomaceous earth and elements that act as promoters may be included. Therefore, the constituent elements of the nickel-diatomaceous earth catalyst obtained by the manufacturing method of the present invention are not limited to only nickel and silicon.

[0042] The nickel content of the nickel diatomaceous earth catalyst obtained by the production method of the present invention may be in the range of 1 to 80 mass%, or 5 to 75 mass%, or 10 to 70 mass%, calculated as NiO, when the nickel diatomaceous earth catalyst is taken as 100 mass%. When the nickel content is in the above range, a nickel diatomaceous earth catalyst having higher hydrogenation activity can be obtained.

[0043] The silicon content of the nickel diatomaceous earth catalyst obtained by the production method of the present invention may be in the range of 20% by mass to 99% by mass, 25% by mass to 95% by mass, or 30% by mass to 90% by mass, calculated as SiO2, when the nickel diatomaceous earth catalyst is taken as 100% by mass. When the silicon content is in the above range, the effects of the present invention are more likely to be obtained.

[0044] The impurities contained in the nickel catalyst obtained by the production method of the present invention are preferably 10 mass% or less, more preferably 5 mass% or less, and particularly preferably 1 mass% or less, calculated as elements, relative to 100 mass% of the nickel catalyst.

[0045] The promoter content of the nickel diatomaceous earth catalyst obtained by the production method of the present invention is preferably in the range of 1 mass% or more to 10 mass% or less, more preferably in the range of 2 mass% or more to 8 mass% or less, and particularly preferably in the range of 3 mass% or more to 7 mass% or less, calculated as an element. Examples of elements that serve as promoters include sodium, potassium, magnesium, aluminum, chromium, copper, manganese, etc. By including these elements, in addition to the effects of the present invention, effects such as suppression of side reactions and increased life can be obtained.

[0046] The present invention will be described in more detail below with reference to examples. The present invention is not limited to these examples. Various measurement methods and evaluation methods are described below.

[0047] [1]pH measurement The pH was measured at a liquid temperature of 40°C using a pH meter (manufactured by Yamagata Toa DKK, "MM43-X") and a pH electrode (manufactured by Yamagata Toa DKK, "GST-5841C"). [2] Composition analysis The sample was dissolved in acid, and the filtrate was diluted with water to an appropriate concentration, after which the nickel content was measured using an ICP optical emission spectrometer (Agilent Technologies, 730ICP-OES, inductively coupled plasma optical emission spectrometry). The nickel content was calculated in terms of NiO, based on the total amount of the sample.

[0048] [3] Specific surface area measurement The specific surface area of ​​the sample was calculated by the nitrogen adsorption method (BET method). Specifically, a specific surface area measuring device (Macsorb1220, manufactured by Mountech) was used, and about 0.1 g of the sample was placed in a measurement cell, and degassed for 40 minutes at 250°C in a nitrogen gas flow. The sample was then kept at liquid nitrogen temperature in a mixed gas flow of 30% by volume of nitrogen and 70% by volume of helium, and nitrogen was adsorbed into the sample at equilibrium. The temperature of the sample was then gradually raised to room temperature while the mixed gas was flowing, and the amount of nitrogen desorbed during that time was measured, and the specific surface area of ​​the sample was calculated by dividing the amount by the weight of the sample after measurement.

[0049] [4] Pore volume measurement N2 adsorption measurements were carried out under the following conditions, and the pore volume was calculated from the adsorption isotherm obtained from the N2 adsorption measurements. Measurement method: Nitrogen adsorption method Measurement device: BEL SORP-miniII (Microtrack BEL Co., Ltd.) Sample size: approx. 0.1g Pretreatment: 250℃, 3 hours (under vacuum) Relative pressure range: 0~1.0 Calculation method: BJH method

[0050] [5] Increase in specific surface area in sodium carbonate aqueous solution 100 mL of a 10% by weight aqueous solution of sodium carbonate was added to 10 g of diatomaceous earth and kept at 70°C for 2 hours. The residue was then collected by filtration and dried at 120°C for 12 hours. The specific surface area of ​​the resulting dried diatomaceous earth was measured using the method [3] above. The specific surface area of ​​the diatomaceous earth before immersion in the aqueous sodium carbonate solution was A, and the specific surface area of ​​the dried diatomaceous earth was B, and the increase rate X of the specific surface area was calculated from the following formula [1] Specific surface area increase rate X%=(BA) / A×100 [1] In the following, this will simply be referred to as the specific surface area increase rate.

[0051] [6] Hydrogenation activity evaluation The hydrogenation activity of the sample was calculated using the hydrogenation reaction of toluene as a model reaction. Specifically, 0.40 g of the sample sized to 1 to 2 mm was filled into a reaction tube, and 2 mmφ glass beads were further filled, followed by pretreatment reduction in a hydrogen atmosphere at 200°C. After the reduction was completed and the sample temperature was stabilized at 60°C, vaporized toluene equivalent to the vapor pressure was introduced into the reaction system and reacted, and 20 minutes after the start of the reaction, the amount of toluene and methylcyclohexane was measured by gas chromatography to obtain the conversion rate. The same operation as the above reaction was performed at 65°C and 70°C, and an Arrhenius plot was created from the sample temperature and conversion rate at each temperature. From the obtained Arrhenius plot, the reaction rate constant at a reaction temperature of 100°C was calculated with the reaction order as first order, and the reaction rate constant in the evaluation using the catalyst of Example 1 was set to 100%, which was taken as the hydrogenation activity (relative activity).

[0052] [7] Nickel elution rate evaluation 20g of nickel diatomaceous earth catalyst was immersed in 50mL of 2M hydrogen chloride solution at 50℃ for 24 hours, and the amount of nickel eluted in the hydrogen chloride solution after immersion, M, was measured using an ICP emission spectrometer (Agilent Technologies, 730ICP-OES). The nickel elution rate Y% was calculated from this amount of eluted nickel, M, and the amount of nickel contained in the nickel diatomaceous earth catalyst before immersion in the hydrogen chloride solution, N, using the following formula [2]. Nickel elution rate Y% = M / N x 100…[2]

[0053] [Example 1] Acidic suspension preparation process 900g of nickel sulfate hydrate [Ni(SO4)2·6H2O] (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in 3.2L of tap water and heated to 70℃ to prepare an acidic aqueous solution. 140g of diatomaceous earth (Chuo Kagaku Co., Ltd. product 100F, specific surface area increase rate 186%) was then added and stirred for 60 minutes to obtain an acidic suspension with a nickel concentration of 4.3% by mass and a diatomaceous earth concentration of 3.3% by mass. The pH of this acidic suspension was 5.46.

[0054] Basic aqueous solution preparation process 2.8 L of tap water was poured into a 15 L stirring tank, 633 g of sodium carbonate (Na2CO3, Kanto Chemical Co., Ltd.) was dissolved in it, and heated to 70° C. to obtain a basic suspension with a sodium concentration of 8.0 mass %. The pH of this basic suspension was 11.70.

[0055] Neutralization process The entire amount of the basic aqueous solution was added to the acidic suspension over 80 minutes using a tube pump to obtain a raw material slurry. The pH of the raw material slurry immediately after the entire amount of the basic aqueous solution was added was 9.50. The raw material slurry was then held at 70°C for 1 hour while being stirred. The pH of the raw material slurry after holding was 9.29.

[0056] Separation process The raw material slurry was filtered under reduced pressure using a Nutsche filter to obtain a cake-like solid. The solid was added to 6 L of warm water adjusted to 40°C, filtered, and suspended and washed. The same process was repeated, and the washing was terminated when the electrical conductivity of the filtrate reached 1.5 mS / cm. The washed solid was dried at 120°C for 12 hours using a box dryer. The solid was then pulverized using a hammer crusher mill to obtain a powdered catalyst precursor.

[0057] Firing process The powdered catalyst precursor was calcined in a muffle furnace at 370°C for 6 hours to obtain a nickel diatomaceous earth catalyst. The nickel diatomaceous earth catalyst was then reduced in a hydrogen atmosphere at 430°C for 10 hours to convert the nickel on the diatomaceous earth surface to metallic nickel. Next, low-concentration oxygen was gradually added at 80°C to form an oxide film on the surface of the metallic nickel, obtaining a reduced and stabilized nickel diatomaceous earth catalyst. This was used as a sample to measure its properties. The results are shown in Table 1.

[0058] [Example 2] A reduced and stabilized nickel diatomaceous earth catalyst was obtained in the same manner as in Example 1, except that diatomaceous earth (Chuo Kagaku Co., Ltd. product 300S, specific surface area increase rate 124%) was used in the acid suspension preparation step. This was used as a sample and its properties were measured. The results are shown in Table 1.

[0059] [Example 3] A reduced and stabilized nickel diatomaceous earth catalyst was obtained in the same manner as in Example 1, except that diatomaceous earth (Imerys product C512, specific surface area increase rate 113%) was used in the acidic suspension preparation step. This was used as a sample and its properties were measured. The results are shown in Table 1.

[0060] [Comparative Example 1] A reduced and stabilized nickel diatomaceous earth catalyst was obtained in the same manner as in Example 1, except that diatomaceous earth (Imerys product C645, specific surface area increase rate 113%) was used in the acidic suspension preparation step. This was used as a sample and its properties were measured. The results are shown in Table 1.

[0061] [Comparative Example 2] A reduced and stabilized nickel diatomaceous earth catalyst was obtained in the same manner as in Example 1, except that diatomaceous earth (Chuo Kagaku Co., Ltd. product W-3050, specific surface area increase rate 55%) was used in the acidic suspension preparation step. This was used as a sample and its properties were measured. The results are shown in Table 1.

[0062] [Comparative Example 3] A reduced and stabilized nickel diatomaceous earth catalyst was obtained in the same manner as in Example 1, except that diatomaceous earth (Imerys product C545, specific surface area increase rate 36%) was used in the acidic suspension preparation step. This was used as a sample and its properties were measured. The results are shown in Table 1.

[0063] The hydrogenation activity of the nickel diatomaceous earth catalysts of Examples 1 to 3, which use diatomaceous earth with a high specific surface area increase rate in an aqueous sodium carbonate solution, is significantly higher than the hydrogenation activity of the nickel diatomaceous earth catalysts of Comparative Examples 1 to 3, which use diatomaceous earth with a low specific surface area increase rate.

[0064] When the nickel diatomaceous earth catalysts of Examples 1 to 3 and Comparative Examples 1 to 3 were immersed in a hydrochloric acid solution, the amount of nickel eluted from the nickel diatomaceous earth catalysts of Examples 1 to 3 was 17.1% to 20.2%, which was relatively small. From these results, it is presumed that more of the nickel contained in the nickel diatomaceous earth catalysts of Examples 1 to 3 was trapped in the pores of the diatomaceous earth, resulting in less nickel eluting into the hydrochloric acid solution. On the other hand, the nickel diatomaceous earth catalysts of Comparative Examples 1 to 3 had an amount of nickel eluted into the hydrochloric acid solution of 22.7% to 27.1%, which was greater than that of Examples 1 to 3.

[0065] These results show that the nickel diatomaceous earth catalyst of the present invention, which uses diatomaceous earth with a high rate of increase in specific surface area in the presence of an aqueous sodium carbonate solution, has a high rate of increase in specific surface area of ​​the diatomaceous earth, so that more nickel is trapped in the pores on the surface of the diatomaceous earth, making it difficult for the nickel to sinter, resulting in a nickel diatomaceous earth catalyst with high hydrogenation activity.

[0066] [Table 1]

Claims

1. an acidic suspension preparation step of adding soluble nickel and diatomaceous earth to water to prepare an acidic suspension; dissolving sodium carbonate in water to prepare a basic aqueous solution; a neutralization step of adding the basic aqueous solution to the acidic suspension to form a raw material slurry, thereby forming a catalyst precursor in which nickel is deposited on the diatomaceous earth; a separation step of performing solid-liquid separation of the catalyst precursor from the raw material slurry; A production method having a calcination step of calcining the separated catalyst precursor, A method for producing a nickel diatomaceous earth catalyst for hydrogenation reactions, comprising using diatomaceous earth having a specific surface area increase rate of 60% or more in an aqueous sodium carbonate solution.

2. 2. The method for producing a nickel diatomaceous earth catalyst for hydrogenation reactions according to claim 1, further comprising a maturation step of maturing the raw material slurry to a pH value that is 0.20 or more lower than the reference pH (a pH value that is −0.20 or less than the reference pH) of the raw material slurry immediately after the addition of the basic aqueous solution to the acidic suspension, in the neutralization step.

Citation Information

Patent Citations

  • Nickel-metal hydride catalyst

    JP2014530098A

  • Nickel diatomaceous earth catalyst and method for producing same

    WO2017077969A1