Cement composition, soil conditioner, and method for inhibiting the generation of hydrogen sulfide
The cement composition with a sulfur-containing reducing agent and optional slag minimizes hydrogen sulfide generation and hexavalent chromium elution, enhancing safety and efficacy.
Patent Information
- Application Number
- JP2023052112
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing cement compositions generate hydrogen sulfide, posing safety concerns during work, despite efforts to reduce heavy metal elution.
A cement composition incorporating a reducing agent with a sulfur content of 0.2 to 0.5% by mass and optionally slag at 10 to 35% by mass, using sulfur compounds like calcium sulfide to minimize hydrogen sulfide generation.
The composition effectively reduces hydrogen sulfide generation while maintaining or improving hexavalent chromium elution control, ensuring safer working conditions.
Smart Images

Figure 2024140781000001 
Figure 2024140781000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a cement composition, a ground improvement material, and a method for inhibiting generation of hydrogen sulfide. [Background technology]
[0002] Cement clinker is produced using limestone, clay, silica, iron oxide, etc. as main raw materials. In addition to these main raw materials, various industrial by-products and industrial waste are effectively used as raw fuels in the production of cement clinker. For this reason, depending on the selection of raw materials, small amounts of heavy metals such as cadmium, chromium, lead, and molybdenum derived from various raw fuels may be mixed into the cement clinker. Therefore, techniques are known that use various reducing agents to reduce heavy metal ions derived from cement clinker and reduce the amount of elution (Patent Documents 1 to 4).
[0003] For example, Patent Document 1 proposes a technique for reducing hexavalent chromium to trivalent chromium by using a mixture of ferrous sulfate and sulfite as a solidification material for solidifying soft ground, thereby suppressing the elution of hexavalent chromium. Patent Document 2 proposes a technique for suppressing the elution of hexavalent chromium by using a ground improvement material having a specific pH and redox potential and containing a specified amount of MgO. Patent Documents 3 and 4 propose techniques for suppressing the elution of heavy metals by using a heavy metal immobilizing agent containing calcium sulfide.
[0004] The surface of calcium sulfide may decompose due to moisture and carbon dioxide in the air, generating a small amount of hydrogen sulfide. In response to this, Patent Document 4 proposes a technology for reducing the generation of hydrogen sulfide (H2S) by adding a specific ratio of calcium sulfate to calcium sulfide. Patent Document 5 also discloses a technology for similarly suppressing the generation of hydrogen sulfide by adding a specific ratio of calcium sulfite and / or calcium carbonate to calcium sulfide. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-201406 A [Patent Document 2] JP 2017-155141 A [Patent Document 3] JP 2006-102643 A [Patent Document 4] JP 2005-306911 A [Patent Document 5] JP 2022-139820 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in order to ensure safety during work, etc., there is a demand for cement compositions that further reduce the amount of H2S generated.
[0007] The present disclosure has been made in consideration of the above circumstances, and aims to provide a cement composition that reduces the amount of H2S generated while maintaining or improving the amount of elution of hexavalent chromium. [Means for solving the problem]
[0008] [1] A cement composition comprising a reducing material containing a sulfur compound, The cement composition, wherein the reducing agent has a sulfur content of 0.2 to 0.5 mass % based on the total amount of the cement composition. [2] A cement composition comprising a reducing material containing a sulfur compound and slag, A cement composition, wherein the reducing material has a sulfur content of 0.1 to 0.5 mass % and the slag content is 10 to 35 mass % relative to the total amount of the cement composition. [3] The cement composition according to [1] or [2], wherein the sulfur compound is at least one selected from the group consisting of calcium sulfide, calcium polysulfide, magnesium sulfide, barium sulfide, and thiosulfate. [4] A ground improvement material comprising any one of the cement compositions of [1] to [3]. [5] A method for inhibiting generation of hydrogen sulfide from a cement composition, comprising: The method includes a step of mixing cement, a reducing material containing a sulfur compound, and optionally, slag; The method, wherein the cement composition satisfies at least one of the following conditions (1) and (2): (1) The sulfur content in the reducing agent is 0.2 to 0.5 mass % based on the total amount of the cement composition. (2) The reducing material has a sulfur content of 0.1 to 0.5 mass % and a slag content of 10 to 35 mass % based on the total amount of the cement composition. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a cement composition that reduces the amount of H2S generated while maintaining or improving the amount of elution of hexavalent chromium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The cement composition of the present disclosure satisfies at least one of the following conditions (1) and (2): (1) A cement composition including a reducing agent containing a sulfur compound, the reducing agent having a sulfur content of 0.2 to 0.5 mass% based on the total amount of the cement composition. (2) Based on the total amount of the cement composition containing the reducing material containing a sulfur compound and the slag, the sulfur content in the reducing material is 0.1 to 0.5 mass %, and the slag content is 10 to 35 mass %.
[0011] The sulfur compound contained in the reducing agent may be at least one selected from the group consisting of calcium sulfide, calcium polysulfide, magnesium sulfide, barium sulfide, and thiosulfate. The sulfur compound may include calcium sulfide.
[0012] The content of calcium sulfide in the reducing agent may be 15 to 50 mass%, 20 to 40 mass%, or 25 to 35 mass%, from the viewpoint of sufficiently increasing the reducing action and sufficiently suppressing the elution of hexavalent chromium, etc. The content of calcium sulfide can be determined, for example, by the XRD-Rietveld method.
[0013] Regarding (1) above, the sulfur content in the reducing agent may be 0.15-0.45 mass%, 0.2-0.4 mass%, 0.2-0.35 mass%, or 0.2-0.3 mass% relative to the total amount of the cement composition. Regarding (2) above, the sulfur content in the reducing agent may be 0.15-0.45 mass%, 0.1-0.4 mass%, 0.1-0.35 mass%, or 0.1-0.3 mass% relative to the total amount of the cement composition.
[0014] The content of the reducing agent in the cement composition may be 0.1 to 1.8 mass %, or may be 0.2 to 1.5 mass %.
[0015] The reducing agent may include a calcium sulfide-containing material containing a carbon-reduced product of gypsum. The carbon-reduced product of gypsum includes calcium sulfide. The calcium sulfide-containing material containing a carbon-reduced product of gypsum may be a heat-treated product obtained by heating a composition containing a gypsum source containing gypsum and a carbon source. The gypsum source is not particularly limited, and examples thereof include waste gypsum dihydrate by-produced from a thermal power plant, natural dihydrate gypsum, natural anhydrous gypsum, and waste gypsum board. Among these, waste gypsum board is preferably used from the viewpoint of waste utilization. Examples of the carbon source include carbon-containing materials such as paper, waste plastic, carbon fiber, biomass, charcoal, coal, coal gasification slag (coal gasification course slag, etc.), and petroleum. The above composition may be heated in the air or in a reducing atmosphere with a lower oxygen concentration than the air at a temperature range of 500 to 1500°C to obtain a calcium sulfide-containing material containing a carbon-reduced product of gypsum. The molar ratio of carbon atom to CaSO4 in the raw material when producing the reducing agent may be 2 to 3. Similarly, when the reducing material contains a magnesium sulfide-containing material, a magnesium source such as magnesium sulfate or magnesium may be used as a raw material instead of gypsum, and when the reducing material contains a barium sulfide-containing material, a barium source such as barium sulfate may be used as a raw material instead of gypsum. One or more raw materials such as gypsum, magnesium source, and barium source may be used depending on the composition of the desired reducing material.
[0016] The reducing agent may further contain components such as calcium sulfite, calcium carbonate, calcium sulfate, calcium oxide, sulfur, silicon dioxide, etc. These components may be used alone or in combination of two or more.
[0017] The cement composition may contain, in addition to the reducing material, for example, cement and gypsum.
[0018] The gypsum may be any of gypsum dihydrate, gypsum hemihydrate, and anhydrous gypsum. From the viewpoint of strength development of the cement composition, the cement composition may contain gypsum dihydrate or anhydrous gypsum. For example, when obtaining a cement composition, gypsum mixed with gypsum dihydrate and anhydrous gypsum may be used. From the viewpoint of strength development when used as soil for ground improvement, the content of gypsum in the cement composition in terms of anhydride may be, for example, 1 to 25 mass%, 3 to 20 mass%, 4 to 15 mass%, or 5 to 12 mass%.
[0019] The cement may be any of various Portland cements as specified in JIS R5210:2003 "Portland cement". Among these, ordinary Portland cement or high-early-strength Portland cement may be used from the viewpoint of availability and increasing the compressive strength at a short age. The total chromium content in the cement may be, for example, 30 to 250 mg / kg or 50 to 200 mg / kg from the viewpoint of availability. The water-soluble hexavalent chromium content of the cement may be, for example, 3 to 40 mg / kg or 4 to 30 mg / kg from the same viewpoint. The total chromium content of the cement is measured in accordance with the method described in JIS R5202:2010, and the water-soluble hexavalent chromium content is measured in accordance with the method described in the Cement Association Standard Test Method I-51-1981.
[0020] The content of cement in the cement composition may be, for example, 50 to 98% by mass, 70 to 95% by mass, or 75 to 90% by mass. If the content of cement is 50% by mass or more, the strength tends to be easily exhibited when used in soil for ground improvement, etc. On the other hand, if the content of cement is 98% by mass or less, the amount of hexavalent chromium eluted from the obtained mortar, concrete, and soil for ground improvement tends to be reduced depending on the content of hexavalent chromium in the cement.
[0021] Cement clinker can be used as a substitute for cement. When using cement clinker, it is preferable to adjust it to an appropriate fineness before use.
[0022] The cement composition may contain slag. Examples of the slag include blast furnace slag powder, steel slag, and copper slag. The cement composition may contain one or more types of slag. In the case of (2) above, the oil content of the slag may be 10 to 30 mass%, 10 to 25 mass%, or 11 to 20 mass% based on the total amount of the cement composition. The Blaine specific surface area of the slag may be 3500 to 5000 cm. 2 / g, the basicity may be 1.60 to 2.00, and the vitrification rate may be 98% or more. Note that the sulfur content derived from sulfides contained in the slag is preferably as high as possible from the viewpoint of the reduction effect of hexavalent chromium, and the upper limit may be, for example, 1.10%.
[0023] In the above case (1), the content of slag in the cement composition may be 5 mass% or less, 1 mass% or less, or 0.1 mass% or less, based on the total amount of the cement composition. In the above case (1), the cement composition may be substantially free of slag.
[0024] The cement composition may further contain limestone, silica fume, fly ash, biomass ash, etc. as components other than slag and cement.
[0025] The fineness of the cement composition is not particularly limited, and the Blaine specific surface area is, for example, 1000 to 6000 cm 2 / g, and 2000 to 5500 cm 2 / g, and 3000 to 5000 cm 2 / g, and 4000 to 4500 cm 2 / g. If the range is within this range, the amount of hexavalent chromium elution can be suppressed while maintaining the strength of the resulting mortar, concrete, and ground improvement soil. This Blaine specific surface area can be measured in accordance with JIS R5201:2015 "Physical test methods for cement."
[0026] The method for producing the cement composition is not particularly limited, and the cement composition may be produced by mixing raw materials adjusted to a predetermined fineness, or by mixing and grinding the raw materials.
[0027] The method for suppressing generation of hydrogen sulfide from a cement composition of the present embodiment includes a step of mixing cement, a reducing material containing a sulfur compound, and slag as an optional component, wherein the cement composition satisfies at least one of the following conditions (1) and (2): (1) The sulfur content in the reducing agent is 0.2 to 0.5 mass% based on the total amount of the cement composition. (2) The reducing material has a sulfur content of 0.1 to 0.5 mass % and a slag content of 10 to 35 mass % based on the total amount of the cement composition.
[0028] The cement composition of the present embodiment can be used as a ground improvement material. That is, the ground improvement material of the present embodiment may contain the above-mentioned cement composition.
[0029] The improved soil of this embodiment includes the above-mentioned soil improvement material and the soil to be improved. Such improved soil is obtained by mixing the above-mentioned soil improvement material and the soil to be improved. 3 The content of the soil improvement material relative to the above may be, for example, 20 to 500 kg, 50 to 450 kg, 50 to 400 kg, or 100 to 350 kg.
[0030] The soil to be improved is not particularly limited, and may be volcanic ash clayey soil (e.g., Kanto loam) in which it is relatively difficult to suppress the elution of hexavalent chromium. By using the ground improvement material according to the present embodiment, it is possible to sufficiently suppress the elution of hexavalent chromium from the improved soil while maintaining the compressive strength of the improved soil at a high level.
[0031] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. For example, the application of the reducing material is not limited to a ground improvement material or a cement composition, and the reducing material may be mixed with incineration ash or construction generated soil, etc. EXAMPLES
[0032] The contents of the present disclosure will be described in detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0033] [Production of reducing materials] The raw material was a mixture of crushed waste gypsum board (94% by mass of gypsum dihydrate, including paper) and a carbon source (coal gasification coke slag, manufactured by UBE Corporation) in a ratio (molar ratio) of [C] / [CaSO4] = 2.4. The mixture was then tumblingly granulated in a high-speed mixer (FS100, manufactured by EarthTechnica Corporation) to obtain roughly spherical granulated raw material with a particle size of 5 mm. The granulated raw material was fed into a rotary kiln (total length approximately 3 m, rotation speed 0.5 min) at a feed rate of 100 kg / h. -1 ) while changing the temperature inside the kiln to obtain a reduced material. The amount of calcium sulfide in the reduced material was 30.6%. The amount of calcium sulfide was quantified using the XRD-Rietveld method with data measured using an X-ray diffractometer (manufactured by Bruker A.X., accelerating voltage: 30 kV, current: 10 mA, tube: Cu). Analysis software (Topas, manufactured by Bruker A.X.) was used for the Rietveld analysis.
[0034] [Preparation of ground improvement material (solidification material)] The following raw materials were prepared: Cement: High-early-strength Portland cement (total chromium content: 85 mg / kg, water-soluble hexavalent chromium content: 9.9 mg / kg) ·Anhydrite: Natural anhydrite Slag: K-ment (manufactured by Kobe Steel Slag Products Co., Ltd.) The reducing material prepared above The above raw materials were mixed in the proportions shown in Table 1 below to prepare ground improvement materials for each of the Examples and Comparative Examples.
[0035] [Table 1]
[0036] [Preparation and evaluation of ground improvement soil] Soil to be improved: Kanto loam The amount of soil improvement material mixed for the target soil (Kanto loam) is 3 300kg / m 3 The soil improvement material was mixed so that the above-mentioned consistency was achieved, and mixed in a Hobart mixer. Mixing was carried out for a total of 3 minutes, with the soil adhering to the paddle and ball being scraped off at 1 minute and 30 seconds intervals. After mixing was completed, the mixture was packed into a cylindrical formwork 50 mm in diameter x 100 mm in height in three layers using a rammer, and then sealed and cured at 20°C for 7 and 28 days.
[0037] [Evaluation of elution amount of hexavalent chromium] For each of the improved soils of the above ages, a leaching test was conducted in accordance with Environment Agency Notification No. 46 (August 23, 1991) to measure the amount of hexavalent chromium leached out. The amount of hexavalent chromium leached out was determined by quantifying the hexavalent chromium concentration in the filtrate after shaking using the diphenylcarbazide spectrophotometric method in 65.2.1 of JIS K0102;2016. During the quantitative measurement procedure, the interval between adding 3 mL of sulfuric acid (1+9) and adding 1 mL of diphenylcarbazide solution (10 g / L) was set to within 20 seconds.
[0038] [Evaluation of hydrogen sulfide gas generation rate] Of the specimens prepared above, those that were demolded at 7 days were immersed in distilled water at a solid-liquid ratio of 1:10 and cured for 28 days. After 28 days, the specimens were removed and the solution was filtered, and the iodine consumption of the filtrate was measured. Hydrogen sulfide is generally measured by directly sucking the gas into a detector tube, but when dissolved in a solution, especially when the solution is alkaline, it exists as hydrogen sulfide ions and does not gasify, making it difficult to directly measure the gas concentration. Instead, the amount of iodine consumption, which indicates the amount of sulfide in a sewer system, was calculated as specified in Article 9, Paragraph 1, Item 4 of the Enforcement Order of the Sewerage Act. The amount of iodine consumption was calculated by testing according to Article 7 of the "Ministerial Ordinance on Testing Methods for Sewage Water Quality" (Ministry of Health, Labor and Welfare / Ministry of Construction Ordinance No. 1 of 1962), and the method used was the method listed in Appendix Table 2 of the same ordinance. The test results are shown in Table 2 below.
[0039]
Table 2
[0040] (Summary of Results) <System containing only CaS> In Examples 2 and 4 where the sulfur content in CaS was in the range of 0.2 to 0.5% by mass based on the total amount of the cement composition, the elution amount of hexavalent chromium was less than 0.02 mg / L and the generation amount of H2S was also small. On the other hand, in Comparative Example 2 where the sulfur content in CaS was less than 0.2% by mass based on the total amount of the cement composition, the elution amount of hexavalent chromium was high at 28 days of age, and in Comparative Example 3 where the sulfur content in CaS exceeded 0.5% by mass based on the total amount of the cement composition, the generation amount of H2S was large at 28 days of age.
[0041] <System containing both CaS and slag> In Examples 1, 3, and 5 to 7 where the sulfur content in CaS was in the range of 0.2 to 0.5% by mass and the slag content was in the range of 10 to 35% by mass based on the total amount of the cement composition, the elution amount of hexavalent chromium was less than 0.02 mg / L and the generation amount of H2S was also small. On the other hand, in Comparative Example 1 without CaS, the elution amount of hexavalent chromium was as high as 0.02 mg / L or more. Also, in Comparative Examples 4 and 5 where the slag content was less than 10% by mass based on the total amount of the cement composition, the elution amount of hexavalent chromium exceeded 0.02 mg / L at 7 days of age, and the suppression of hexavalent chromium elution was insufficient. From this, a synergistic effect was observed between the slag content and the sulfur content in CaS, especially for the experimental results at 28 days of age.
Claims
1. A cement composition comprising a reducing material containing a sulfur compound, The cement composition, wherein the sulfur content in the reducing material is 0.2 to 0.5 mass% based on the total amount of the cement composition.
2. A cement composition comprising a reducing material containing a sulfur compound and slag, The cement composition, wherein the reducing material has a sulfur content of 0.1 to 0.5 mass% and the slag content is 10 to 35 mass% relative to the total amount of the cement composition.
3. 3. The cement composition according to claim 1, wherein the sulfur compound is at least one selected from the group consisting of calcium sulfide, calcium polysulfide, magnesium sulfide, barium sulfide, and thiosulfate.
4. A ground improvement material comprising the cement composition according to claim 1 or 2.
5. A method for inhibiting generation of hydrogen sulfide from a cement composition, comprising: The method includes a step of mixing cement, a reducing material containing a sulfur compound, and optionally, slag; The method, wherein the cement composition satisfies at least one of the following conditions (1) and (2): (1) The sulfur content in the reducing agent is 0.2 to 0.5 mass % based on the total amount of the cement composition. (2) The reducing material has a sulfur content of 0.1 to 0.5 mass % and a slag content of 10 to 35 mass % relative to the total amount of the cement composition.
Citation Information
Patent Citations
Hexavalent chromium leach reducing agent for hydraulic material, and method for reducing hexavalent chromium leach
JP2000086322A
Manufacturing method for calcium sulfide, manufacturing method for foundation improving material, and treating method for object to be treated
JP2005225742A
Efficient dosing, storage-stable composition for reducing chromium(vi) in cement
JP2009504554A
Cement additive, cement composition, and concrete
JP2018145077A
Ground improvement material, cement milk, and ground improvement method
JP2020158710A