Benefits of technology

【0010】 本発明により、1回の冷間圧延および最終焼鈍によるプロセスで加工性に優れたフェライト系ステンレス鋼板が得られる熱延鋼板を提供することが可能である。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140802000001
    Figure 2024140802000001
  • Figure 2024140802000002
    Figure 2024140802000002
  • Figure 2024140802000003
    Figure 2024140802000003
Patent Text Reader

Abstract

To provide a hot rolled steel sheet for obtaining a ferritic stainless steel sheet having excellent processability by one-time cold rolling and final annealing without performing hot rolled sheet annealing by a process.SOLUTION: A ferritic stainless hot rolled steel sheet contains Cr:11.0% or more and 30.0% or less, C:0.030% or less, Si:1.00% or less, Mn:1.00% or less, P:0.005% or more and 0.100% or less, S:0.0100% or less, Al:0.50% or less, N:0.030% or less, furthermore, Ti:0.05% or more and 0.50% or less and / or Nb:0.05% or more and 0.50% or less in mass%, and the balance consists of Fe with impurities, where a recrystallization ratio is 5% or less, a random intensity ratio of {112}<110>crystal orientation on a plane parallel to a rolled surface at a 1 / 2 position the sheet thickness of the steel sheet is 7 or more, and Vickers hardness at a sheet thickness central part on across section is 150 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ferritic stainless steel sheet. [Background technology]

[0002] Ferritic stainless steel has excellent corrosion resistance and is used in applications where appearance is important, such as kitchens, and in applications exposed to corrosive environments, such as automobile exhaust system parts. In recent years, its use as a highly workable material has expanded, as typified by its use in automobile exhaust system parts and utensils. Ferritic stainless steel as a processing material is required to have a high average r-value, which is an index of deep drawing processing characteristics. The average r-value is calculated as (r0+2×r45+r90) / 4. Many methods have been proposed to improve the average r-value.

[0003] Patent Documents 1 and 2 disclose methods for obtaining a high r-value having an average r-value of about 2.1 to 2.7. However, the manufacturing costs increase due to the additional steps, such as performing cold rolling twice, annealing hot-rolled sheet, and intermediate annealing. Various methods for improving the r-value by one cold rolling without performing hot-rolled sheet annealing are shown in Non-Patent Document 1 and the like. For example, Non-Patent Document 1 proposes a method for further improving the average r-value of so-called IF-based stainless steel, which contains Ti, Nb, etc. and fixes C and N. As shown in Non-Patent Document 1, many methods have been reported, such as a method for increasing the cold rolling reduction rate and a method for growing grains by performing high-temperature annealing in the final annealing process. However, excessive inclusion of Ti or Nb or an excessive increase in the cold rolling reduction rate reduces the average r-value, and excessive grain growth in the final annealing process causes problems such as increasing roughness during subsequent processing, so there is a limit to the average r-value that can be obtained. Therefore, the method for improving workability is limited to optimizing the in-plane anisotropy of the r-value. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-163139 A [Patent Document 2] JP 2003-138349 A [Patent Document 3] International Publication No. 2021 / 065738 [Non-patent literature]

[0005] [Non-Patent Document 1] Sawatani, Sei, et al., r-value and texture of Ti-added low C, N-17% Cr stainless steel sheet, Tetsu-to-Haganen, 63 (1977), p.843 [Non-Patent Document 2] Hiroshi Inoue, Three-dimensional Orientation Analysis of Texture, Light Metals, vol42, No6(1992), p358 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to obtain a ferritic stainless steel sheet having excellent workability even without processes such as hot-rolled sheet annealing, and to provide such a ferritic stainless steel sheet. [Means for solving the problem]

[0007] Many of the methods for improving the r-value of stainless steel sheets involve controlling the texture after final annealing by accumulating strain before the final annealing process, increasing grain boundaries before final cold rolling, reducing solute C and solute N, and growing grains, leading to an improvement in the r-value. For example, Patent Document 1 and Patent Document 3 disclose a method for improving the r-value after cold rolling annealing by accumulating strain in the hot rolling process to increase the amount of strain after the subsequent cold rolling, but there is no knowledge about the hot rolling texture. Patent Document 2 discloses a method for obtaining a high r-value by cold rolling annealing a pre-cold rolling annealed sheet with fine recrystallized grains with a high {111} concentration before final cold rolling, but hot rolled sheet annealing is performed to control the texture before cold rolling. On the other hand, there is little known about a method for controlling the texture after hot rolling to control the texture in the subsequent cold rolling and final annealing without annealing.

[0008] Therefore, the present inventors investigated the relationship between the structure of hot-rolled steel sheets and the texture and r-value after one cold rolling and final annealing without annealing after hot rolling. <110> It was found that the more orientations there are, the higher the r-value after final annealing becomes, even without hot-rolled sheet annealing. The present invention was made based on this finding, and the gist of the present invention is as follows.

[0009] [1] In mass%, Cr: 11.0% or more and 30.0% or less, C: 0.030% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.005% or more and 0.100% or less, S: 0.0100% or less, Al: 0.50% or less, and N: 0.030% or less, including moreover, Ti: 0.05% to 0.50% Nb: 0.05% or more and 0.50% or less, or both; The balance is Fe and impurities. The recrystallization rate is 5% or less, and the {112} <110> A ferritic stainless hot-rolled steel sheet characterized in that the random strength ratio of crystal orientation is 7 or more and the Vickers hardness at the center of the sheet thickness in the cross section is 150 or more. [2] Further, in mass%, Sn: 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, Sb: 0.50% or less, B: 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Y: 0.20% or less, Hf: 0.20% or less, and REM: 0.10% or less The ferritic stainless steel hot-rolled sheet according to [1], characterized in that it contains one or more selected from the following: Effect of the Invention

[0010] According to the present invention, it is possible to provide a hot-rolled steel sheet from which a ferritic stainless steel sheet having excellent workability can be obtained by a process of one cold rolling and final annealing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiment of the present invention (hereinafter, simply referred to as the present invention) will be described in detail. The "%" indication for the content of each element means "mass%" unless otherwise specified. When no lower limit is specified or the lower limit is 0%, it also includes the case where no element is contained (0%).

[0012] [Chemical composition] The reasons for limiting the chemical components are explained below.

[0013] Cr:11.0% or more and 30.0% or less Cr is an element that improves corrosion resistance, which is a basic property of stainless steel. If the content is too low, sufficient corrosion resistance cannot be obtained, so the lower limit is set to 11.0%. From the viewpoint of corrosion resistance, it is preferably 14.0% or more, and more preferably 16.0% or more. On the other hand, an excessive content promotes the formation of intermetallic compounds equivalent to σ, which promotes cracking during manufacturing and reduced formability, so the upper limit is set to 30.0%. From the viewpoint of stable manufacturing (yield, rolling defects, etc.), it is preferably 25.0% or less, and more preferably 20.0% or less.

[0014] C: 0.030% or less C is an element that reduces formability (r value), which is important in the present invention, so the less C the better, with the upper limit set at 0.030%. From the viewpoint of formability, 0.018% or less is preferable. There is no particular lower limit, but an excessive reduction leads to an increase in refining costs, so 0.001% or more is preferable, and 0.002% or more is more preferable.

[0015] Si: 1.00% or less Silicon is an element that improves oxidation resistance, but excessive content leads to a decrease in formability, so the upper limit is set to 1.00%. From the viewpoint of formability, 0.30% or less is preferable. There is no particular lower limit, but an excessive decrease leads to an increase in raw material costs, so 0.01% or more is preferable, and 0.05% or more is more preferable.

[0016] Mn: 1.00% or less Like Si, a large content of Mn leads to a decrease in formability, so the upper limit is set to 1.00%. From the viewpoint of formability, 0.30% or less is preferable. There is no particular lower limit, but an excessive decrease leads to an increase in raw material costs, so 0.01% or more is preferable, and 0.05% or more is more preferable.

[0017] P: 0.005% or more and 0.100% or less P is an element that inhibits the development of {111} at the time of recrystallization in the final annealing process and reduces formability (r-value and product elongation), so the lower the content, the better, with the upper limit set to 0.100%. From the viewpoint of formability, 0.070% or less is preferable, and 0.05% or less is more preferable. However, a small amount of phosphorus-containing precipitates precipitated during final annealing contributes to texture control and r-value improvement, and excessive reduction not only increases raw material costs but also reduces the r-value, so from the viewpoints of raw material costs and r-value, the content is set to 0.005% or more. It is preferably 0.010% or more, and more preferably 0.020% or more.

[0018] S: 0.0100% or less S is an impurity element that deteriorates corrosion resistance and promotes cracking during manufacturing, so the lower the content, the better, with the upper limit set at 0.0100%. From the viewpoint of corrosion resistance and manufacturability, the content is preferably 0.0030% or less, and more preferably 0.0020% or less. There is no particular lower limit, but an excessive decrease leads to an increase in refining costs, so the content is preferably 0.0003% or more, and more preferably 0.0004% or more.

[0019] Al: 0.50% or less Al is an effective element for improving corrosion resistance or oxidation resistance, but an excessive content not only reduces formability, but also leads to an increase in alloy costs and hinders manufacturability, so the upper limit is set to 0.50%. From the viewpoint of manufacturability, the preferred upper limit is 0.30%. There is no particular lower limit, but an excessive decrease leads to an increase in refining costs, so the lower limit is preferably 0.005% or more, and more preferably 0.01% or more.

[0020] N: 0.030% or less N is an element that reduces formability (r value) like C, and the upper limit is set to 0.030%. From the viewpoint of formability, 0.015% or less is preferable. There is no particular lower limit, but since an excessive reduction leads to an increase in refining costs, 0.002% or more is preferable, and from the viewpoint of refining costs, 0.005% or more is even more preferable.

[0021] One or both of Ti: 0.05% to 0.50% and Nb: 0.05% to 0.50% Ti improves formability by improving the r-value and product elongation through high purification by fixing C and N as precipitates. To obtain this effect, the lower limit of Ti is set to 0.05%. From the viewpoint of formability, 0.07% or more is preferable, and 0.10% or more is more preferable. On the other hand, since an excessive content leads to an increase in alloy cost and a decrease in r-value, the upper limit of Ti is set to 0.50%. From the viewpoint of alloy cost and manufacturability, 0.40% or less is preferable, and 0.30% or less is more preferable.

[0022] Like Ti, Nb also acts as a stabilizing element that fixes C and N, thereby improving the purity of steel and improving formability by improving the r-value and product elongation. Furthermore, it contributes to texture control through the accumulation of strain due to strain recovery and suppression of recrystallization during the hot rolling process, and contributes to improving the r-value of the product. To obtain these effects, the lower limit of Nb is set to 0.05%. From the viewpoint of formability, 0.07% or more is preferable. On the other hand, excessive content leads to an increase in alloy cost and an increase in r-value anisotropy, so the upper limit of Nb is set to 0.50%. From the viewpoint of alloy cost and formability, 0.40% or less is preferable, and 0.30% or less is even more preferable.

[0023] The effect is obtained by including at least one of Ti and Nb. Of course, both Ti and Nb may be included, and even in that case, the content of each element is the same as when each element is included alone.

[0024] In addition to the above components, the following elements may be selectively contained. Of course, they do not have to be contained, so the lower limit of the content of these elements is 0%. For convenience, the elements are divided into groups A, B, and C according to their effects, but one or more elements from all the elements belonging to groups A, B, and C can be contained.

[0025] Group A elements: Sn: 0.005% or more and 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less, W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, Sb: 0.50% or less Sn, Ni, Cu, Mo, W, Co, V, Zr, and Sb are elements effective for improving corrosion resistance or oxidation resistance, and one or more of these elements may be contained as necessary. However, excessive content not only leads to a decrease in formability, but also leads to an increase in alloy cost and an impairment of manufacturability, so the upper limit of Ni, Cu, and W is 1.00%, and the upper limit of Mo is 2.00%. The upper limit of Sn, Co, V, Zr, and Sb is 0.50%. Although there is no particular limit, the more preferable lower limit of the content of Sn and Sb is 0.005%, and the more preferable lower limit of the content of Ni, Cu, Mo, W, Co, V, and Zr is 0.05%.

[0026] Group B elements: B: 0.0001% or more and 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less B, Ca, and Mg are elements that improve hot workability and secondary workability, and one or more of these elements may be contained as necessary. Although there is no particular lower limit, from the viewpoint of hot workability and secondary workability, B is preferably 0.0001% or more, and Ca and Mg are preferably 0.0002% or more. However, since excessive content leads to impaired manufacturability, the upper limit of B is set to 0.0025%, and the upper limit of Ca and Mg is set to 0.0050%. From the viewpoint of manufacturability, B is preferably 0.0012% or less, and Ca and Mg are preferably 0.0010% or less.

[0027] Group C elements: Y: 0.20% or less, Hf: 0.20% or less, REM: 0.10% or less Y, Hf, and REM are elements effective for improving hot workability and cleanliness of steel as well as oxidation resistance, and one or more of these elements may be contained as necessary. When contained, the upper limit of Y and Hf is 0.20%, and the upper limit of REM is 0.10%. There is no particular restriction on the lower limit, but from the viewpoint of cleanliness and oxidation resistance, the preferable lower limit when contained is 0.001%. Here, REM is an element with an atomic number of 57 to 71, such as La, Ce, Pr, and Nd.

[0028] In addition to the above-described elements, other elements may be contained within a range that does not impair the effects of the present invention. For example, it is preferable to reduce Bi, Pb, Se, H, Ta, etc. as much as possible, but one or more of Bi: 100 ppm or less, Pb: 100 ppm or less, Se: 100 ppm or less, H: 100 ppm or less, and Ta: 500 ppm or less may be contained as necessary within a range that does not affect the effects of the present invention.

[0029] The balance of the components other than those described above is Fe and impurities. Here, the term "impurities" refers to components that are inevitably mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, during industrial production of steel, and are acceptable within a range that does not adversely affect the present invention.

[0030] [Recrystallization rate] When hot-rolled steel recrystallizes, the crystal orientation changes to produce the {112} <110> Not only does the orientation decrease, but the amount of strain in the hot-rolled steel sheet also decreases, resulting in a decrease in the r-value after final annealing. Therefore, the recrystallization rate is set to 5% or less. From the viewpoint of improving the r-value, the recrystallization rate is preferably 3% or less, and more preferably 1% or less. The recrystallization rate is measured in a cross section parallel to the sheet thickness direction and the rolling direction.

[0031] [Collective organization:{112} <110> Random intensity ratio of crystal orientation] In the crystal orientation of the plane parallel to the rolling surface at the 1 / 2 position of the plate thickness of the hot-rolled steel plate (the position at the distance of 1 / 2 of the plate thickness from the surface of the plate in the thickness direction, i.e., the center of the plate in the thickness direction), the {112} <110> The random strength ratio of the crystal orientation is 7 or more. <110> By developing the orientation, the {112} <110> It is possible to obtain a strongly developed rolling texture with the {112} orientation as the main orientation, and it is possible to improve the r-value after final annealing. <110> The crystal orientation intensity is preferably 9 or more, and more preferably 10 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, 16 or more, 17 or more, 18 or more, or 20 or more. The rolled surface refers to the surface that is in contact with the rolling rolls during rolling, and in the case of a steel sheet, the so-called front and back surfaces of the steel sheet are the rolled surfaces.

[0032] The method for measuring the random intensity ratio of the crystal orientation will be described. X-ray diffraction is performed on a plane parallel to the rolling surface at the 1 / 2 position of the thickness of the steel plate. The 1 / 2 position of the thickness often shows the average texture of the steel material, and can be an index of formability. Using the obtained data, a 3D orientation analysis is performed using the Bunge method (see, for example, Non-Patent Document 2), and the random intensity ratio in each orientation can be read from the crystal orientation distribution diagram. The 1 / 2 position of the thickness does not need to be the exact center position in the thickness direction of the steel plate, and when the thickness of the steel plate is t, it is sufficient if it is within a range of ±0.1t from the position of 1 / 2t in the thickness direction from the surface of the steel plate (i.e., within a range from a depth of 40% of the thickness to a depth of 60% of the thickness from the surface of the steel plate in the thickness direction) (this region is called the 1 / 2 position of the thickness). The same applies to the hardness at the center of the thickness.

[0033] [Vickers hardness at center of plate thickness] The Vickers hardness at the 1 / 2 thickness position in a cross section parallel to the rolling direction and thickness direction of the hot-rolled steel sheet is set to 150 or more. It is possible to improve the r-value after final annealing by increasing the strain imparted by hot rolling. From the viewpoint of the r-value, the Vickers hardness at the 1 / 2 thickness position is preferably 155 or more, and more preferably 160 or more.

[0034] [Manufacturing method] Next, a method for producing a hot-rolled ferritic stainless steel sheet according to the present invention will be described. The method for producing the hot-rolled ferritic stainless steel sheet according to the present invention is one embodiment for obtaining the steel sheet according to the present invention, and the method is not limited to this method. As long as the steel sheet according to the present invention can be obtained, the method for producing the hot-rolled ferritic stainless steel sheet according to the present invention is not limited.

[0035] The stainless steel slab may be manufactured by a conventional manufacturing method. For example, in steelmaking, a method is suitable in which steel containing the components adjusted to the above-described components is melted in a converter or electric furnace, followed by secondary refining. The molten steel thus adjusted to the desired components can be used to obtain a slab by a known casting method (for example, a continuous casting method).

[0036] [Hot rolling] After heating, the stainless steel slab is subjected to hot rolling, which includes rough rolling and finish rolling, to produce a hot-rolled sheet.

[0037] [Slab heating temperature] If the slab heating temperature exceeds 1250°C, Ti carbosulfide (Ti4C2S2) dissolves during heating, increasing the amount of solute carbon, and reprecipitation during the hot rolling process delays recrystallization. These phenomena lead to roping due to poor recrystallization after finish hot rolling. In addition, the crystal grains are significantly enlarged during slab heating, and coarse extended grains are formed in the hot rolling process, causing deterioration of the workability of the product sheet and roping. Therefore, the slab heating temperature should be 1250°C or less. It is preferably 1230°C or less, or 1210°C or less. On the other hand, if the slab heating temperature is less than 1100°C, it will cause surface defects and cause deterioration of corrosion resistance due to rust from the defects. For this reason, the slab heating temperature is preferably 1100°C or more. More preferably, the slab heating temperature is 1130°C or more, or 1150°C or more.

[0038] [Finish hot rolling temperature] When the temperature of each pass of the hot rolling exceeds 950℃, the crystal orientation rotation becomes difficult, and the concentration increases with the crystal orientation rotation, resulting in the formation of {112} <110> In addition, if the temperature of each pass of the finish hot rolling is below 700°C, the rolling reaction force increases, which causes defects in the sheet shape and surface defects. Therefore, it is effective to roll the sheet so that the specified reduction ratio is obtained when the temperature of each pass of the finish hot rolling is in the range of 700°C to 950°C. <110> In order to develop the orientation, the reduction ratio of the finish hot rolling between 950°C and 700°C where the texture develops is set to 85% or more. From the viewpoint of hot rolling texture development, the reduction ratio of the finish hot rolling between 950°C and 700°C is preferably 86% or more, 87% or more, 88% or more, or 89% or more, and more preferably 90% or more. The finish hot rolling may include rolling in a temperature range higher than 950°C or lower than 700°C, so long as the above-mentioned rolling reduction is obtained in the temperature range of 950°C to 700°C.

[0039] In addition, the average strain rate in each pass of the finish hot rolling should be 20 / s or more and 100 / s or less. If the strain rate is higher than 100 / s, the strain applied by processing heat is recovered, so the {112} <110> This is the upper limit because orientation does not develop. If the strain rate is slower than 20 / s, the amount of strain that can be imparted becomes small, leading to a decrease in the r-value, so this is the lower limit. From the perspective of strain accumulation, 30 / s to 80 / s is preferable.

[0040] In addition, the finishing temperature of the finish hot rolling (the temperature at the final pass) is preferably 850°C or less. If the finishing temperature is higher than 850°C, recovery occurs during rolling and in the cooling process from rolling to coiling, reducing the amount of strain in the hot-rolled sheet and reducing the hardness of the cross section of the hot-rolled sheet to 150 Vickers hardness or less. The reduction in the amount of strain in the hot-rolled steel sheet reduces the r-value after final annealing. From the viewpoint of the amount of hot rolling strain and the r-value, the finishing temperature of the finish hot rolling is more preferably 830°C or less.

[0041] [Winding temperature] If the coiling temperature is high, strain recovery and recrystallization occur as the hot-rolled coil gradually cools. If the recrystallization rate exceeds 5%, the texture of the hot-rolled sheet changes, so the upper limit of the coiling temperature is set to 600°C. From the viewpoint of suppressing recrystallization, the coiling temperature is more preferably 550°C or less.

[0042] [Hot-rolled sheet annealing omitted] The above hot rolling process resulted in {112} <110> Since a hot-rolled steel sheet with developed orientation can be obtained, there is no need to perform hot-rolled sheet annealing.

[0043] By manufacturing in this way, <110> It is possible to obtain hot-rolled steel sheets with well-developed orientation, and the {112} <110> It is possible to obtain a rolling texture that is strongly developed with the orientation as the main orientation, and the r-value after final annealing can be improved. The process after hot rolling is not particularly limited. For example, cold rolling and final annealing can be performed as shown below. Below, an example of the process after hot rolling is shown, but the manufacturing method is not limited to this example.

[0044] [Descaling] If surface scale is formed and problems such as surface defects occur in subsequent processes, it is preferable to carry out a descaling treatment such as pickling as necessary.

[0045] [Cold rolling] Then, cold rolling is performed to the specified plate thickness. In the subsequent annealing process, in order to accumulate sufficient strain for recrystallization, the cold rolling reduction is preferably 40% or more. Since an excessive increase in the cold rolling reduction leads to a decrease in the average r-value, the cold rolling reduction is preferably 85% or less.

[0046] [Finishing annealing (final annealing)] After cold rolling, it is preferable to perform finish annealing for the purpose of recrystallization and grain growth. When the recrystallization temperature is Ts, the finish annealing is performed in the range of Ts+50°C to Ts+120°C. Within this temperature range, it is sufficient to perform the finish annealing at an appropriate temperature according to the required characteristics. If the annealing is performed at a temperature exceeding Ts+120°C, the crystal grain size becomes too large and roughness after processing becomes noticeable, so this temperature is preferably set as the upper limit. In addition, in consideration of productivity in industrial production, the heat treatment time is preferably within 3 minutes.

[0047] The recrystallization temperature Ts can be determined, for example, by the following method. The cold-rolled steel sheet is heated to a specified temperature (annealing temperature), held for one minute, and then cooled to room temperature to measure the recrystallization rate. The annealing temperature is changed in increments of 10°C, and the lowest temperature at which the recrystallization rate is 98% or more is defined as the recrystallization temperature Ts. EXAMPLES

[0048] Next, an embodiment of the present invention will be described. The stainless steels shown in Table 1 were melted and then hot-rolled under the conditions shown in Table 2 to produce hot-rolled steel sheets. The steel sheets were then cold-rolled and final annealed under the conditions shown in Table 3 to produce product sheets, and the results of evaluating their properties are also shown.

[0049] The evaluation method will be explained. [Texture of hot-rolled steel sheet] X-ray diffraction was performed on the hot-rolled steel sheet at the 1 / 2 thickness position on a plane parallel to the rolling surface. Analysis was performed using the method described in the texture section above, and the {112} <110> The random intensity ratio was calculated.

[0050] [Recrystallization rate of hot-rolled steel sheet] The recrystallization rate is measured at an arbitrary observation cross section that is parallel to the plate thickness direction and the rolling direction, has a width of 1 mm, and extends through the entire thickness. After etching the observation cross section of the hot-rolled steel sheet, five observation cross sections are selected and the structure is observed at 50x magnification using an optical microscope. The region of the extended crystal grains with an aspect ratio of 5 or more is considered to be a non-recrystallized region, and the region of the crystal grains with an aspect ratio of less than 5 is considered to be a recrystallized region, and the area ratio (%) of the recrystallized region (recrystallized region / (recrystallized region+non-recrystallized region)) is considered to be the recrystallization rate. The aspect ratio is defined as the major axis / minor axis of each crystal grain. The arithmetic average of the area ratios (%) of the recrystallized region measured at each of the five observation cross sections is considered to be the area ratio (%) of the recrystallized region of the steel sheet.

[0051] [Vickers hardness at the center of the thickness of hot-rolled steel plate] The Vickers hardness of hot-rolled steel sheet is a value measured at 1 / 2 the sheet thickness position (center of sheet thickness) of the steel sheet on a cross section parallel to the sheet thickness direction and rolling direction, using a load of 5 kg in accordance with JIS Z2244:2009 (Vickers hardness test - Test method (equivalent to ISO 6507-4:2005)).

[0052] [Average r-value of cold-rolled steel sheets] The average r-value of the cold-rolled steel sheet was calculated by the plastic strain ratio test method in accordance with JIS Z 2254:2008.

[0053] [Characteristics evaluation] As shown in Examples C1 to C17, the recrystallization rate is set to 5% or less, and the {112} <110> It was confirmed that by using hot-rolled steel sheet with a random strength ratio of 7 or more and a cross-sectional Vickers hardness exceeding 150, it is possible to increase the r-value of the stainless steel sheet after cold rolling and final annealing to 1.7 or more, which corresponds to a limiting drawing ratio (LDR) of 2.3 or more, and thus provides sufficiently high workability.

[0054] Comparative examples c1, c4, c5, c10, c11, c12, and c13 have low r-values ​​because C, P, N, Ti, and Nb are outside the specified range. c2, c7, and c8 have low r-values ​​because the texture of the hot-rolled steel sheet cannot be controlled. c3, c6, and c9 have low r-values ​​because the recrystallization rate of the hot-rolled steel sheet exceeds 5% and the accumulated strain of the hot-rolled steel sheet is small. Comparative examples c14, c15, c16, and c17 have chemical compositions within the prescribed range, but the manufacturing conditions are outside the preferred range and the r values ​​are low.

[0055] [Table 1]

[0056] [Table 2]

[0057] [Table 3] [Industrial Applicability]

[0058] The present invention can be utilized not only in the steel industry which produces ferritic stainless steels, but also in all industries which use ferritic stainless steel products.

Claims

1. In mass%, Cr: 11.0% or more and 30.0% or less, C: 0.030% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.005% or more and 0.100% or less, S: 0.0100% or less, Al: 0.50% or less, and N: 0.030% or less, moreover, Ti: 0.05% or more and 0.50% or less; Nb: 0.05% or more and 0.50% or less, The balance is Fe and impurities, A ferritic stainless steel hot-rolled sheet characterized in that the recrystallization rate is 5% or less, the random intensity ratio of the {112}<110> crystal orientation in a plane parallel to the rolling surface at a position 1 / 2 of the sheet thickness of the steel sheet is 7 or more, and the Vickers hardness at the center of the sheet thickness of the cross section is 150 or more.

2. Further, in mass%, Sn: 0.50% or less, Ni: 1.00% or less, Cu: 1.00% or less, Mo: 2.00% or less, W: 1.00% or less, Co: 0.50% or less, V: 0.50% or less, Zr: 0.50% or less, Sb: 0.50% or less, B: 0.0025% or less, Ca: 0.0050% or less, Mg: 0.0050% or less, Y: 0.20% or less, Hf: 0.20% or less, and REM: 0.10% or less 2. The hot-rolled ferritic stainless steel sheet according to claim 1, further comprising one or more selected from the group consisting of:

Citation Information

Patent Citations

  • Ferritic stainless steel sheet with excellent workability, and its manufacturing method

    JP2006193771A

  • Nb CONTAINING FERRITIC STAINLESS STEEL HOT ROLLED COIL AND MANUFACTURING METHOD

    JP2012140688A

  • Ferritic stainless steel hot rolled steel sheet for flange and manufacturing method therefor

    JP2017095789A

  • Ti-CONTAINING FERRITIC STAINLESS STEEL SHEET FOR EXHAUST TUBE FLANGE COMPONENT AND MANUFACTURING METHOD

    JP2017206723A

  • Hot rolled and unannealed ferritic stainless steel sheet having excellent impact toughness, and manufacturing method therefor

    US20220042151A1