Manufacturing method of gas diffusion layer for fuel cell and gas diffusion layer for fuel cell

The use of copper methyl acetylide to form a graphene multilayer film in a gas diffusion layer addresses manufacturing complexity and enhances conductivity and water retention, improving fuel cell efficiency.

JP2024140936AActive Publication Date: 2024-10-10TOYOTA BOSHOKU KK +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052312
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing gas diffusion layers for fuel cells require a simpler manufacturing method and improvements in conductivity, gas diffusivity, and water retention.

Method used

A method involving the use of copper methyl acetylide as a precursor, which is stirred into a wire shape, dissolved, and then applied to a porous base sheet, followed by firing at 1000°C to 1200°C to form a graphene multilayer film, creating a porous carbon structure with mesoporous hollow wire-like crystals, filling the pores and forming a microporous layer.

Benefits of technology

This method allows for the production of a gas diffusion layer with high conductivity, gas diffusivity, and effective water retention, contributing to improved fuel cell performance by adjusting catalyst layer humidity and proton transport.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140936000001_ABST
    Figure 2024140936000001_ABST
Patent Text Reader

Abstract

To easily manufacture a gas diffusion layer having a microporous layer.SOLUTION: A method for manufacturing a gas diffusion layer for a fuel cell includes a stirring step of stirring a solution containing copper methylacetylide as precursors to form the precursors into a wire-like shape and entangle the precursors with each other in the solution, an adding step of adding the precursor to a surface layer of a porous substrate sheet so as to fill pores in the surface layer, and a firing step of baking the substrate sheet and the precursor at 1000°C or more and 1200°C or less to grow a graphene multilayer film from the precursor and thermally remove copper, thereby forming porous carbon that is composed of the graphene multilayer films, has mesoporosity, and has a hollow wire-like crystal structure.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a gas diffusion layer for a fuel cell, and a gas diffusion layer for a fuel cell. [Background technology]

[0002] A solid polymer electrolyte fuel cell includes a fuel cell stack formed by stacking a plurality of unit cells. Each unit cell has a membrane electrode assembly including a solid polymer electrolyte membrane (hereinafter referred to as electrolyte membrane) and a pair of catalyst layers sandwiching the electrolyte membrane, a pair of gas diffusion layers sandwiching the membrane electrode assembly, and an anode separator and a cathode separator sandwiching the pair of gas diffusion layers.

[0003] An example of such a gas diffusion layer is the gas diffusion electrode disclosed in Patent Document 1. The gas diffusion electrode disclosed in Patent Document 1 includes a sheet-like porous substrate and a microporous layer disposed in contact with one surface of the porous substrate. The porous substrate is carbon paper, carbon cloth, carbon nonwoven fabric, or the like. The microporous layer is formed by applying a paste-like coating liquid in which conductive fine particles, a binder, a solvent, a thickener, and the like are mixed and dispersed on one surface of the porous substrate. The conductive particles are carbon black such as acetylene black having an average particle size of 20 to 150 nm. The binder is, for example, polytetrafluoroethylene (PTFE). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2022-42074 A Summary of the Invention [Problem to be solved by the invention]

[0005] Such a gas diffusion layer for a fuel cell is required to be manufactured by a simple method, and further improvements are required in the adjustment of electrical conductivity, gas diffusibility, and water retention. [Means for solving the problem]

[0006] A method for manufacturing a gas diffusion layer for a fuel cell that solves the above problems includes a stirring step of stirring a solution containing copper methylacetylide as a precursor to form the precursor into a wire-like shape and entangle the precursors in the solution; an adding step of adding the precursor to a surface portion of a porous base sheet or base sheet precursor so as to fill pores in the surface portion; and a firing step of baking the base sheet or base sheet precursor and the precursor at 1000°C or higher and 1200°C or lower to grow a graphene multilayer film from the precursor and thermally remove copper, thereby forming a porous carbon that is composed of graphene multilayer films, has mesoporosity, and has a hollow wire-like crystal structure.

[0007] According to this method, in the stirring step, a solution containing copper methylacetylide is stirred to form a wire-shaped precursor. In the subsequent heating step, the copper of the precursor becomes spherical or elliptical due to the difference in specific gravity between copper and carbon, and the carbon becomes wire-shaped, covering the copper. The wire-shaped precursors are also entangled with each other in the solution.

[0008] Next, in the application step, the precursor is applied to the surface layer portion of the porous base sheet or base sheet precursor so as to fill the pores in the surface layer portion. Subsequently, in the firing step, the precursor is fired at 1000°C or more and 1200°C or less together with the substrate sheet or substrate sheet precursor, so that the copper is sublimated and removed. The part of the carbon of the precursor that is in contact with the copper comes into contact with the molten copper at 1000°C or more. At this time, the surface tension generated in the carbon creates an ideal two-dimensional surface of the carbon, so that the carbon grows into a multilayer film of graphene. This forms porous carbon that is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other. In addition, when the substrate sheet precursor is used, the substrate sheet is formed by firing the substrate sheet precursor. Therefore, when the precursor is fired, the substrate sheet precursor can be fired at the same time to form the substrate sheet.

[0009] By calcining the copper methylacetylide precursor in this manner, the precursor is carbonized while maintaining the wire-like precursor structure. Furthermore, according to the above method, since the firing temperature is 1000° C. or higher and 1200° C. or lower, the firing temperature can be lowered compared to the conventional manufacturing method in which silver methyl acetylide is fired at 2000° C., for example. This allows the firing furnace to be made smaller and the energy required for firing to be reduced.

[0010] Copper is also more suitable than silver for growing thick graphene multilayers to enhance electrical conductivity. In this way, according to the above method, a gas diffusion layer in which the pores in the surface layer of the substrate sheet are filled with the porous carbon can be obtained by a simple process. The porous carbon functions as a microporous layer. Therefore, a gas diffusion layer having a microporous layer can be produced by a simple method.

[0011] Further, a method for manufacturing a gas diffusion layer for a fuel cell to solve the above problems includes a stirring step of stirring a solution containing copper methylacetylide as a precursor to form the precursor into a wire-like shape and entangle the precursor with each other in the solution; a first firing step of baking the precursor at 1000° C. or more and 1200° C. or less to grow the graphene multilayer film and thermally remove copper to form porous carbon composed of graphene multilayer films, having mesoporosity and a hollow wire-like crystal structure; a crushing step of crushing the porous carbon while maintaining the crystal structure; an addition step of applying or spraying a solution containing the crushed porous carbon onto a surface portion of a porous base sheet to add the porous carbon so as to fill pores in the surface portion; and a second firing step of baking the base sheet and the porous carbon to integrate the porous carbon with the base sheet.

[0012] According to this method, in the stirring step, a solution containing copper methylacetylide is stirred to form a wire-shaped precursor. In the subsequent heating step, the copper of the precursor becomes spherical or elliptical due to the difference in specific gravity between copper and carbon, and the carbon becomes wire-shaped, covering the copper. The wire-shaped precursors are also entangled with each other in the solution.

[0013] Next, in the first firing step, the precursor is fired at 1000°C or higher and 1200°C or lower, thereby sublimating and removing the copper. The part of the carbon of the precursor that is in contact with the copper comes into contact with the molten copper at 1000°C or higher. At this time, the surface tension generated in the carbon creates an ideal two-dimensional surface of the carbon, and the carbon grows into a multilayer film of graphene. As a result, porous carbon is formed that is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other.

[0014] By calcining the copper methylacetylide precursor in this manner, the precursor is carbonized while maintaining the wire-like precursor structure. Next, in the crushing step, the porous carbon is crushed while maintaining its crystal structure.

[0015] Next, in the application step, a solution containing pulverized porous carbon is applied or sprayed onto the surface layer of the porous base sheet, thereby adding the porous carbon so as to fill the pores in the surface layer.

[0016] Subsequently, in the second firing step, the base sheet and the porous carbon are fired, so that the porous carbon is bonded and integrated with the base sheet. According to the above method, since the firing temperature in the first firing step is 1000° C. or higher and 1200° C. or lower, the firing temperature can be lowered compared to the conventional manufacturing method in which, for example, silver methyl acetylide is fired at 2000° C. This makes it possible to reduce the size of the firing furnace and the energy required for firing.

[0017] Copper is also more suitable than silver for growing thick graphene multilayers to enhance electrical conductivity. In this way, a gas diffusion layer in which the pores in the surface layer of the substrate sheet are filled with the porous carbon can be obtained by a simple process. The porous carbon functions as a microporous layer. Therefore, a gas diffusion layer having a microporous layer can be manufactured by a simple method.

[0018] In addition, a gas diffusion layer for a fuel cell for solving the above problems includes a porous base sheet, the gas diffusion layer for a fuel cell has porous carbon formed integrally with the base sheet so as to fill holes in a surface layer of the base sheet, the porous carbon is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other, the wire diameter of the crystals is 100 nm or more and 500 nm or less, and the pore diameter of the holes formed by the entangled crystals is 10 nm or more and 200 nm or less.

[0019] According to this configuration, although the porous carbon itself is brittle, since it is formed integrally with the substrate sheet, the rigidity of the porous carbon can be increased. In addition, since the porous carbon is formed of a multilayer film of graphene, it has high electrical conductivity. In addition, since the wire diameter of the crystal is 100 nm or more and 500 nm or less, and the pore diameter of the pores formed by the crystals intertwined with each other is 10 nm or more and 200 nm or less, the porous carbon has high gas permeability, i.e., gas diffusibility. In addition, since water can be stored in the mesopores present in large numbers in the crystals and water can be discharged from the mesopores, the porous carbon is excellent in adjusting the amount of water retention. Therefore, the porous carbon functions as a microporous layer. In addition, in a fuel cell, when protons move from the anode to the cathode, water functions as a carrier that transports the protons. As described above, since the porous carbon of the gas diffusion layer is adjacent to the catalyst layer, the humidity of the catalyst layer is adjusted by the porous carbon. This allows the amount of water in the catalyst layer to be increased, which contributes to improving the output of the fuel cell. Effect of the Invention

[0020] According to the method for producing a gas diffusion layer for a fuel cell of the present invention, a gas diffusion layer having a microporous layer can be easily produced. In addition, the gas diffusion layer for a fuel cell of the present invention has high electrical conductivity and high gas diffusivity, and is excellent in adjusting the water retention capacity. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a cross-sectional view of a single cell of a fuel cell. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a gas diffusion layer of the first embodiment. [Diagram 3] FIG. 3 is an SEM image of the surface layer of the gas diffusion layer of the first embodiment. [Figure 4] FIG. 4 is an SEM image of the surface layer of the gas diffusion layer of the first embodiment. [Diagram 5]FIG. 5 is an SEM image of the porous carbon constituting the gas diffusion layer of the first embodiment. [Figure 6] FIG. 6 is an SEM image of the porous carbon constituting the gas diffusion layer of the first embodiment. [Figure 7] FIG. 7 is an SEM image of the porous carbon constituting the gas diffusion layer of the first embodiment. [Figure 8] FIG. 8 is an SEM image of the porous carbon constituting the gas diffusion layer of the first embodiment. [Figure 9] FIG. 9 is a TEM image of the porous carbon constituting the gas diffusion layer of the first embodiment. [Figure 10] FIG. 10 is a TEM image of the precursor during the drying step of the first embodiment. [Figure 11] FIG. 11 is a flowchart showing a manufacturing procedure of the gas diffusion layer of the first embodiment. [Figure 12] FIG. 12 is a schematic diagram showing a base sheet on which a solution containing a precursor has been applied. [Figure 13] FIG. 13 is a flowchart showing a manufacturing procedure of the gas diffusion layer of the second embodiment. [Figure 14] FIG. 14 is a schematic diagram showing how a sheet-shaped precursor is superimposed on a base sheet. [Figure 15] FIG. 15 is a flowchart showing a manufacturing procedure of the gas diffusion layer of the third embodiment. [Figure 16] FIG. 16 is a schematic diagram showing a base sheet on which a solution containing pulverized porous carbon has been applied. [Figure 17] FIG. 17 is an SEM image of the porous carbon of the comparative example. [Figure 18] FIG. 18 is an SEM image of the porous carbon of the comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] First Embodiment Hereinafter, a first embodiment of a gas diffusion layer for a fuel cell and a manufacturing method thereof will be described with reference to FIGS. 1 to 12, 17, and 18. FIG.

[0023] The polymer electrolyte fuel cell includes a fuel cell stack formed by stacking a plurality of unit cells 10 . 1, a single cell 10 has a membrane electrode assembly 13, a pair of gas diffusion layers 20 sandwiching the membrane electrode assembly 13, and an anode side separator and a cathode side separator (both not shown) sandwiching the pair of gas diffusion layers 20. The membrane electrode assembly 13 has a solid polymer electrolyte membrane (hereinafter referred to as electrolyte membrane 11) and a pair of catalyst layers 12 sandwiching the electrolyte membrane 11.

[0024] As shown in Figures 1 and 2, the gas diffusion layer 20 has a porous base sheet 21 and porous carbon 22 formed integrally with the base sheet 21 so as to fill pores in a surface layer portion 21a of the base sheet 21.

[0025] The base sheet 21 of this embodiment is a carbon cloth having a fiber diameter of about 7 μm and having pores of about 1 to 2 μm. As shown in FIGS. 3 to 8, the porous carbon 22 is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other.

[0026] As shown in FIG. 3, the carbon fibers constituting the base sheet 21, that is, the pores formed between thick fibers, are filled with porous carbon 22. As shown in FIG. 9, the porous carbon 22 has a pore structure partitioned by a multilayer film of graphene.

[0027] The diameter of the crystal wire is 100 nm to 500 nm, and the diameter of the hole formed by the intertwined crystals is 10 nm to 200 nm. Next, a manufacturing procedure for the gas diffusion layer 20 of this embodiment will be described with reference to FIG.

[0028] As shown in FIG. 11, the method for producing the gas diffusion layer 20 of this embodiment includes a precursor synthesis step, a stirring step, an adding step, a drying step, and a firing step. The precursor synthesis step is a step of synthesizing copper methylacetylide as a precursor by a well-known method.

[0029] The stirring step is a step of stirring a solution containing copper methylacetylide as a precursor to form the precursor into a wire shape and entangle the precursors in the solution. The solvent is water. The precursor can be easily stretched by adding a small amount of ethanol to the solvent.

[0030] In the stirring step, a wire-shaped precursor is formed by stirring the solution containing copper methylacetylide. In the subsequent heating step, the copper becomes spherical or elliptical due to the difference in specific gravity between copper and carbon, and the carbon becomes wire-shaped, covering the copper. The wire-shaped precursors are also entangled with each other in the solution.

[0031] As shown in FIG. 12, the adding step is a step of adding a precursor 22A to a surface layer portion 21a of a porous base sheet 21 so as to fill pores in the surface layer portion 21a. In the adding step, the precursor 22A is added to the surface layer portion 21a by applying or spraying a solution containing the precursor 22A to the surface layer portion 21a. In this embodiment, the phenol resin solution containing the precursor 22A is applied to the surface layer portion 21a of the base sheet 21, so that the solution is allowed to penetrate into the pores of the surface layer portion 21a of the base sheet 21.

[0032] The drying step is a step of heating and drying the precursor 22A applied to the surface layer portion 21a of the base sheet 21 in a vacuum to about 170° C. to 300° C. As a result, although phase separation between copper and carbon occurs, the shape of the precursor 22A is easily maintained.

[0033] FIG. 10 shows how copper and methylacetylene polymers separate during the process in which precursor 22A is heated to 60 to 200°C in the drying step, specifically, how copper becomes spherical and the methyl groups become methane and ethylene gas and are released outside the system.

[0034] The firing step is a step of firing the base sheet 21 and the precursor 22A at 1000° C. or more and 1200° C. or less to grow a multilayer film of graphene and thermally remove copper to form the porous carbon 22.

[0035] The firing step is preferably carried out under reduced pressure which is lower than normal pressure. Here, in the firing step, the precursor 22A is fired together with the base sheet 21 at 1000°C or more and 1200°C or less, whereby the copper is sublimated and removed. The carbon of the precursor 22A in contact with the copper comes into contact with the molten copper at 1000°C or more. At this time, the surface tension generated in the carbon creates an ideal two-dimensional surface of the carbon, and the carbon grows into a multilayer film of graphene. This forms the porous carbon 22, which is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other.

[0036] The melting point of copper is 1085°C, but in the case of particles of 50 nm or less, a drop in the melting point occurs, causing copper to liquefy at temperatures below 1000°C. 17 and 18 show SEM images of the porous carbon of the comparative example. The porous carbon of the comparative example was formed by dropping the precursor of the present embodiment into a furnace and baking it in a vacuum.

[0037] Next, the effects of this embodiment will be described. (1-1) The method for manufacturing the gas diffusion layer 20 includes a stirring step, an adding step, and a firing step.

[0038] According to this method, the firing temperature is 1000° C. or higher and 1200° C. or lower, so the firing temperature can be lower than that of the conventional manufacturing method in which silver methyl acetylide is fired at 2000° C., for example. This makes it possible to reduce the size of the firing furnace and the energy required for firing.

[0039] Copper is also more suitable than silver for growing thick graphene multilayers to enhance electrical conductivity. In this way, according to the above method, it is possible to obtain the gas diffusion layer 20 in which the pores of the surface layer portion 21a of the base sheet 21 are filled with the porous carbon 22 through a simple process. The porous carbon 22 functions as the microporous layer 23. Therefore, the gas diffusion layer 20 having the microporous layer 23 can be manufactured by a simple method.

[0040] In the (1-2) adding step, a solution containing the precursor 22A is applied or sprayed onto the surface layer portion 21a, thereby adding the precursor 22A to the surface layer portion 21a. According to this method, in the addition step, the precursor 22A is added to the surface layer portion 21a by applying or spraying a solution containing the precursor 22A to the surface layer portion 21a. Therefore, the precursor 22A can be easily added to the surface layer portion 21a of the porous base sheet 21 so as to fill the pores of the surface layer portion 21a.

[0041] (1-3) The gas diffusion layer 20 has a porous base sheet 21 and porous carbon 22 formed integrally with the base sheet 21 so as to fill holes in the surface layer 21a of the base sheet 21. The porous carbon 22 is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other. The wire diameter of the crystal is 100 nm or more and 500 nm or less, and the pore diameter of the holes formed by the entangled crystals is 10 nm or more and 200 nm or less.

[0042] According to this configuration, although the porous carbon 22 itself is fragile, since it is formed integrally with the base sheet 21, the rigidity of the porous carbon 22 can be increased. In addition, since the porous carbon 22 is formed of a multilayer film of graphene, it has high electrical conductivity. In addition, since the wire diameter of the crystal is 100 nm or more and 500 nm or less, and the pore diameter of the hole formed by the crystals intertwined with each other is 10 nm or more and 200 nm or less, the porous carbon 22 has high gas permeability, i.e., gas diffusibility. In addition, since water can be stored in the mesopores present in large numbers in the crystals and water can be discharged from the mesopores, the porous carbon 22 is excellent in adjusting the amount of water retention. Therefore, the porous carbon 22 functions as a microporous layer 23. In addition, in a fuel cell, water functions as a carrier that transports protons when protons move from the anode to the cathode. As described above, since the porous carbon 22 of the gas diffusion layer 20 is adjacent to the catalyst layer 12, the humidity of the catalyst layer 12 is adjusted by the porous carbon 22. This makes it possible to increase the amount of moisture in the catalyst layer 12, which contributes to improving the output of the fuel cell.

[0043] <Second embodiment> Hereinafter, the second embodiment will be described with reference to FIGS. 13 and 14, focusing on the differences from the first embodiment.

[0044] As shown in FIG. 13, the method for producing the gas diffusion layer 20 of this embodiment differs from that of the first embodiment in that a sheet forming step and a drying step are provided between the stirring step and the adding step. The sheet process is a process for forming the precursor 22A into a sheet shape.

[0045] In the sheet forming step, the wire-like precursors 22A, which are entangled with each other, are formed into a sheet. The method of forming the wire-like precursors 22A into a sheet includes, for example, a method of filtering a solution containing the precursors 22A with a filter paper to form a sheet on the filter paper, a method of applying the precursors to a flat jig, a method of spraying the precursors to a flat jig, and the like.

[0046] The drying step is a step of drying the sheet-formed precursor by heating it in a vacuum to about 170° C. to 300° C. As a result, although phase separation between copper and carbon occurs, the shape of the precursor is easily maintained.

[0047] 14, in the addition step, the sheet-shaped precursor 22A is pressed against the surface layer portion 21a in a state where the sheet-shaped precursor 22A is overlapped on the surface layer portion 21a. In this embodiment, the sheet-shaped precursor 22A is pressed against the surface layer portion 21a using a roller (not shown).

[0048] After the addition process is performed, a firing process is performed in the same manner as in the first embodiment. Next, the effects of this embodiment will be described. (2-1) The manufacturing method of the gas diffusion layer 20 includes a sheet forming step of forming the precursor 22A into a sheet shape. In the addition step, the precursor 22A in a sheet shape is pressed against the surface layer portion 21a in a state where the precursor 22A is superimposed on the surface layer portion 21a.

[0049] According to this method, the precursor 22A can be easily applied to the surface layer 21a of the porous base sheet 21 with a uniform thickness so as to fill the pores of the surface layer 21a. (2-2) Since the porous carbon 22 has a structure in which hollow wire-like crystals are entangled with each other, it is easy to make the microporous layer 23 thin. Furthermore, by making the microporous layer 23 thin, the resistance overvoltage of the microporous layer 23 can be reduced.

[0050] <Third embodiment> Hereinafter, the third embodiment will be described with reference to FIGS. As shown in FIG. 15, the method for producing the gas diffusion layer 20 of this embodiment includes a precursor synthesis step, a stirring step, a first firing step, a pulverization step, an addition step, and a second firing step.

[0051] The precursor synthesis step and the stirring step are similar to those in the first and second embodiments. The first firing step is a step of firing the precursor at 1000° C. or more and 1200° C. or less to grow a graphene multilayer film and thermally remove copper to form porous carbon 22.

[0052] The first firing step is preferably carried out under reduced pressure which is lower than normal pressure. Here, in the first firing step, the precursor 22A is fired at 1000° C. or more and 1200° C. or less, so that copper is sublimated and removed, similarly to the firing step in the first embodiment.

[0053] The pulverization step is a step of pulverizing the porous carbon 22 while maintaining the above-mentioned crystal structure. 16, the adding step is a step of adding porous carbon 22 so as to fill the pores of the surface layer 21a by applying or spraying a solution containing pulverized porous carbon 22 to the surface layer 21a of the porous base sheet 21. In this embodiment, a phenol resin solution containing pulverized porous carbon 22 is applied to the surface layer 21a of the base sheet 21, so that the solution penetrates into the pores of the surface layer 21a of the base sheet 21.

[0054] The second firing step is a step of integrating the porous carbon 22 with the base sheet 21 by firing the base sheet 21 and the porous carbon 22. Next, the effects of this embodiment will be described.

[0055] (3-1) The method for producing the gas diffusion layer 20 includes a stirring step, a first firing step, a crushing step, an adding step, and a second firing step. According to the above method, since the firing temperature in the first firing step is 1000° C. or higher and 1200° C. or lower, the firing temperature can be lowered compared to the conventional manufacturing method in which, for example, silver methyl acetylide is fired at 2000° C. This makes it possible to reduce the size of the firing furnace and the energy required for firing.

[0056] Copper is also more suitable than silver for growing thick graphene multilayers to enhance electrical conductivity. In this way, according to the above method, it is possible to obtain the gas diffusion layer 20 in which the pores of the surface layer portion 21a of the base sheet 21 are filled with the porous carbon 22 through a simple process. The porous carbon 22 functions as the microporous layer 23. Therefore, the gas diffusion layer 20 having the microporous layer 23 can be manufactured by a simple method.

[0057] <Modification> This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that there is no technical contradiction.

[0058] The fiber diameter of the carbon fibers constituting the base sheet 21 and the size of the holes in the base sheet 21 can be changed as appropriate. The base sheet 21 is not limited to carbon cloth, but may be carbon paper or carbon nonwoven fabric.

[0059] In the first and second embodiments, in the addition step, copper methyl acetylide is added as a precursor to the surface layer portion 21a of the base sheet 21, and then in the firing step, the base sheet 21 and the precursor are fired at 1000°C or higher and 1200°C or lower. Alternatively, in the addition step, copper methyl acetylide is added as a precursor to the surface layer portion of the base sheet precursor, and then in the firing step, the base sheet precursor and the precursor may be fired at 1000°C or higher and 1200°C or lower. The base sheet precursor may be any material that becomes a base sheet when fired, and is preferably, for example, a nonwoven fabric or paper made of polyacrylonitrile. Alternatively, it may be a nonwoven fabric or paper made of cellulose. In this case, the base sheet is formed by firing the base sheet precursor. Therefore, when firing the precursor, the base sheet precursor can be fired at the same time to form carbon paper or carbon nonwoven fabric as the base sheet. [Explanation of symbols]

[0060] 10...Single cell 11...Electrolyte membrane 12...Catalyst layer 13...Membrane electrode assembly 20...Gas diffusion layer 21...Base sheet 21a...surface layer 22…Porous carbon 23...Microporous layer

Claims

1. A method for manufacturing a gas diffusion layer for a fuel cell, comprising: a stirring step of stirring a solution containing copper methylacetylide as a precursor to form the precursor into a wire shape and entangle the precursor with each other in the solution; an application step of applying the precursor to a surface layer portion of a porous base sheet or base sheet precursor so as to fill pores in the surface layer portion; and a firing step of firing the substrate sheet or the substrate sheet precursor and the precursor at 1000°C or higher and 1200°C or lower to grow a graphene multilayer film on the precursor and thermally remove copper, thereby forming porous carbon that is composed of graphene multilayer films, has mesoporosity, and has a hollow wire-like crystal structure. A method for manufacturing a gas diffusion layer for a fuel cell.

2. In the adding step, the precursor is added to the surface layer portion by applying or spraying a solution containing the precursor to the surface layer portion. The method for producing the gas diffusion layer for a fuel cell according to claim 1 .

3. a sheet forming step of forming the precursor into a sheet, In the adding step, the precursor in a sheet form is pressed against the surface layer portion in a state where the precursor is superimposed on the surface layer portion. The method for producing the gas diffusion layer for a fuel cell according to claim 1 .

4. A method for manufacturing a gas diffusion layer for a fuel cell, comprising: a stirring step of stirring a solution containing copper methylacetylide as a precursor to form the precursor into a wire shape and entangle the precursor with each other in the solution; a first firing step in which the precursor is fired at 1000°C or higher and 1200°C or lower to grow a graphene multilayer film and thermally remove copper, thereby forming porous carbon composed of graphene multilayer films, having mesoporosity, and having a hollow wire-like crystal structure; a pulverization step of pulverizing the porous carbon while maintaining the crystalline structure; an adding step of applying or spraying a solution containing the pulverized porous carbon onto a surface layer portion of a porous substrate sheet to add the porous carbon so as to fill pores in the surface layer portion; a second firing step of firing the base sheet and the porous carbon to integrate the porous carbon with the base sheet, A method for manufacturing a gas diffusion layer for a fuel cell.

5. A gas diffusion layer for a fuel cell comprising a porous substrate sheet, The porous carbon is formed integrally with the base sheet so as to fill pores in a surface layer of the base sheet, the porous carbon is composed of a multilayer film of graphene and has a structure in which hollow wire-like crystals having mesoporosity are entangled with each other; The wire diameter of the crystal is 100 nm or more and 500 nm or less, The pore diameter of the pores formed by the crystals entangled with each other is 10 nm or more and 200 nm or less. Gas diffusion layer for fuel cells.

Citation Information

Patent Citations

  • Gas diffusion electrode

    JP2022042074A