Aqueous ink, ink cartridge, and inkjet recording method
By coating titanium oxide particles with alumina and silica and adjusting the surface charge ratio, the ink achieves improved storage stability and sedimentation resistance, addressing the issues of existing aqueous inks in inkjet devices.
Patent Information
- Application Number
- JP2023052459
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing aqueous inks containing titanium oxide for inkjet recording devices suffer from insufficient storage stability and sedimentation resistance, leading to potential blockages in the ink supply channels and reduced system longevity.
The ink formulation includes titanium oxide particles coated with alumina and silica, with a specific ratio of acid sites to base sites on the particle surface and controlled aluminum ion content, ensuring stable dispersion through electrostatic repulsion.
The solution provides enhanced storage stability and sedimentation resistance, preventing particle aggregation and maintaining ink quality over time, thus reducing system load and extending the life of inkjet devices.
Smart Images

Figure 2024141031000012 
Figure 2024141031000013 
Figure 2024141031000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-based ink, an ink cartridge, and an ink-jet recording method. [Background technology]
[0002] In recent years, inkjet recording devices have come to be widely used when printing advertisements and exhibits using recording media such as paper and resin film. For example, in order to express clear color images even on transparent recording media, white ink is used in addition to black and basic color inks (hereinafter, these may be collectively referred to as color inks). Specifically, a recording method is used in which white ink is applied in advance to a location on a transparent recording medium including an area where an image is to be recorded to perform base treatment, and color inks are applied on top of that, or each ink is applied in the reverse order (so-called back printing).
[0003] Titanium oxide is widely used as a coloring material for white ink because it is low cost and has excellent properties required for white ink, such as whiteness and hiding power. On the other hand, for water-based inkjet ink, titanium oxide, which is a metal oxide and has a large specific gravity, must be stably dispersed. For this reason, it is necessary to select an appropriate dispersant and perform an appropriate dispersion process at the manufacturing stage of the dispersion liquid used in the production of the ink.
[0004] Methods for stably dispersing titanium oxide have been studied. For example, a method for producing a dried titanium dioxide product has been proposed in which titanium oxide is surface-treated with silica, then further surface-treated with a silane coupling agent, and then dried to covalently bond a portion of the silane coupling agent to the surface of titanium oxide particles (see Patent Document 1). In addition, an ink containing titanium oxide surface-treated with alumina, a monovalent metal salt, and alumina fine particles has been proposed (see Patent Document 2). In addition, an ink containing titanium oxide surface-treated with alumina and silica, and then surface-treated with a silane coupling agent, a resin having an anionic group, a water-soluble organic solvent, and a basic compound has been proposed (see Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2017-521348 [Patent Document 2] International Publication No. 2018 / 190848 [Patent Document 3] JP 2011-225867 A Summary of the Invention [Problem to be solved by the invention]
[0006] It is required that the ink is unlikely to undergo an irreversible increase in particle size even when the ink is left to stand for a long period of time, such as more than six months. This performance is referred to as "storage stability" in this specification. Storage stability is important for ensuring the performance of the ink during the distribution of the ink and during the period from when the ink is set in an inkjet recording device until it is used up. In addition, it is required that the ink is unlikely to produce sediment even when the ink is left to stand for a short period of time, such as one day. This performance is referred to as "sedimentation resistance" in this specification. Although sediment can be reversibly recovered, if it is left without recovery operation, it will accumulate in the ink supply flow path and the ink flow path in the recording head, and the flow path will be blocked, increasing the load of the recovery operation of the system. Therefore, ensuring sedimentation resistance is important from the viewpoint of reducing the load on the system and extending its life.
[0007] The present inventors have studied the storage stability and sedimentation resistance of the aqueous ink prepared using the dried titanium dioxide proposed in Patent Document 1, and the aqueous inks proposed in Patent Documents 2 and 3. As a result, it was found that the storage stability and sedimentation resistance are insufficient for stable handling of titanium oxide with a large particle size required to obtain whiteness, and there is room for improvement. In addition, in Patent Document 2, it was found that the storage stability of the dispersion is improved to a certain extent by using a dispersant with high affinity for titanium oxide particles, but the storage stability of the aqueous ink produced using the dispersion is insufficient.
[0008] Therefore, an object of the present invention is to provide an aqueous inkjet ink containing titanium oxide, which has excellent storage stability and resistance to sedimentation, an ink cartridge using the aqueous ink, and an inkjet recording method. [Means for solving the problem]
[0009] The above object is achieved by the present invention, which is described below. That is, the aqueous ink according to the present invention is an aqueous ink for inkjet use containing titanium oxide particles, the titanium oxide particles being titanium oxide having at least a portion of their surface coated with alumina and silica and being dispersed at least by the action of the silica, the content (ppm) of aluminum ions in the aqueous ink is 30 ppm or less based on the total mass of the ink, and the ratio of acid sites (μmol / g) on the surface of the titanium oxide particles in the aqueous ink to basic sites (μmol / g) is 0.40 to 0.55 times. Effect of the Invention
[0010] According to the present invention, it is possible to provide an aqueous inkjet ink containing titanium oxide, which has excellent storage stability and resistance to sedimentation, an ink cartridge using the aqueous ink, and an inkjet recording method. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating an embodiment of an ink cartridge of the present invention. [Diagram 2] 1A and 1B are diagrams illustrating an example of an inkjet recording apparatus used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording apparatus, and (b) is a perspective view of a head cartridge. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in more detail below with reference to preferred embodiments. In the present invention, when the compound is a salt, the salt is present in the ink in the form of dissociation into ions, but for convenience, it is expressed as "containing a salt." Titanium oxide and titanium oxide particles may be simply referred to as "pigment." Furthermore, water-based ink for inkjet printing may be simply referred to as "ink." Physical property values are values at room temperature (25°C) unless otherwise specified.
[0013] Inorganic oxides such as titanium oxide react with water molecules constituting the aqueous medium in the aqueous ink to generate hydroxyl groups (hereinafter, sometimes referred to as "surface hydroxyl groups") on the surface. For this reason, in the case of aqueous inkjet inks, in order to utilize the generated surface hydroxyl groups while further improving the storage stability of the ink, the ink is generally used in a state where the ink is surface-treated with inorganic oxides such as alumina or silica. The surface hydroxyl groups of titanium oxide particles have properties specific to the inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the isoelectric point, which is an indicator of the strength of the acid, differs depending on the type of inorganic compound. Therefore, although titanium oxide itself is an inorganic oxide, the surface of titanium oxide particles shows the properties of an inorganic oxide corresponding to the inorganic compound used in the surface treatment, and the surface charge of titanium oxide particles is strongly dependent on the pH of the aqueous medium, the type of surface treatment agent, and the amount of the surface treatment agent used.
[0014] In order to stabilize the dispersion state of titanium oxide particles in ink and improve storage stability and sedimentation resistance, it is necessary to select titanium oxide particles that have been subjected to an appropriate surface treatment. Therefore, the present inventors have focused on the composition of the surface functional group of titanium oxide particles and investigated the composition of the surface functional group that shows good characteristics. As a result, it has been found that various characteristics can be improved by adjusting the ratio of silica and alumina coated on titanium oxide particles to a predetermined range. However, it has been found that even if titanium oxide with a uniform ratio of silica and alumina is used, sedimentation resistance may not be obtained.
[0015] As a result of further investigation, the present inventors found that in inks with reduced sedimentation resistance, a large amount of alumina was dissolved from the surface of titanium oxide particles. This is because, in the weakly alkaline pH range in which inks are usually used, the alumina on the surface of titanium oxide particles forms aluminate ions and is easily dissolved in the ink. When the aluminate ions are re-adsorbed onto the surface of titanium oxide particles, if they are accompanied by other titanium oxide particles, they are thought to cause aggregation (bridging aggregation). As a result of further investigation, the present inventors found that the storage stability and sedimentation resistance can be improved by setting the ratio of acid sites and base sites on the surface of titanium oxide particles within a specified range and setting the content of aluminum ions in the ink within a specified range.
[0016] That is, the ink of the present invention has the following characteristics. First, titanium oxide particles are used, which are titanium oxide having at least a portion of their surface coated with alumina and silica. The titanium oxide particles are dispersed at least by the action of silica. The content (ppm) of aluminum ions in the ink is 30 ppm or less based on the total mass of the ink. In addition, the ratio of acid sites (μmol / g) on the surface of titanium oxide particles in the ink to basic sites (μmol / g) is 0.40 to 0.55 times. The inventors speculate that the mechanism by which the above configuration improves storage stability and sedimentation resistance is as follows.
[0017] The titanium oxide particles are surface-treated with alumina and silica, and are dispersed at least by the action of the silica. The surface charge state of titanium oxide particles, which are titanium oxide coated with alumina and silica, changes depending on the pH of the ink. In the pH range normally used for ink, the surface hydroxyl groups derived from silica are negatively charged and form an electric double layer. Therefore, even if titanium oxide particles approach each other, aggregation can be suppressed by electrostatic repulsion, and they can be stably dispersed.
[0018] In addition, the ratio of the acid sites (μmol / g) on the surface of the titanium oxide particles to the base sites (μmol / g) in the ink is 0.40 to 0.55 times. The acid sites on the surface of the titanium oxide particles are a value that mainly depends on the amount of negatively charged components, i.e., silica covering the surface of the titanium oxide particles. As described above, the surface hydroxyl groups derived from silica tend to be negatively charged in the ink and contribute to the formation of an electric double layer. On the other hand, the acid sites on the surface of the titanium oxide particles are a value that mainly depends on the amount of positively charged components, i.e., alumina covering the surface of the titanium oxide particles. Unlike the case of silica, the surface hydroxyl groups derived from alumina tend to be positively charged in the ink. It is believed that by setting the ratio of the acid sites and the base sites within the above range, an electric double layer is efficiently formed, and the stable dispersion state of the titanium oxide particles can be maintained by electrostatic repulsion.
[0019] When the ratio is less than 0.40, that is, when the amount of alumina coating is large or the amount of silica coating is small, the negative charge of the surface hydroxyl group derived from silica is canceled, and the electric double layer becomes thin. As a result, the titanium oxide particles cannot be maintained in a stable dispersion state, and storage stability and sedimentation resistance cannot be obtained. When the ratio is more than 0.55, that is, when the amount of alumina coating is small or the amount of silica coating is large, the surface hydroxyl group derived from silica is in a large state, so the amount of cations in the ink increases and the formation of the electric double layer is inhibited. Therefore, the titanium oxide particles cannot be maintained in a stable dispersion state, and storage stability and sedimentation resistance cannot be obtained. The method for measuring the acid and base sites on the surface of the titanium oxide particles will be described in detail later.
[0020] The content (ppm) of aluminum ions in the ink is 30 ppm or less based on the total mass of the ink. By setting the content within the above range, bridging aggregation that is likely to occur when aluminate ions are re-adsorbed onto titanium oxide particles can be suppressed, and sedimentation resistance can be improved. If the content of aluminum ions is outside the above range, sedimentation resistance cannot be obtained.
[0021] <Water-based ink> The ink of the present invention is an aqueous ink for inkjet printing that contains titanium oxide particles coated with a specific inorganic oxide. This ink is preferably a white ink because titanium oxide is a white pigment. The components constituting the ink of the present invention and the physical properties of the ink are described in detail below.
[0022] (Colorant) The ink contains titanium oxide particles as a coloring material (pigment) in which the surface of titanium oxide is treated with a specific inorganic oxide. In other words, the ink contains titanium oxide particles, which are titanium oxide whose surface is coated with a specific inorganic oxide. The content (mass%) of titanium oxide particles in the ink is preferably 0.10% by mass or more and 20.00% by mass or less, based on the total mass of the ink. The content (mass%) of titanium oxide particles in the ink is more preferably 1.00% by mass or more and 20.00% by mass or less, based on the total mass of the ink. In particular, the content (mass%) of titanium oxide particles in the ink is particularly preferably 1.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink.
[0023] Titanium oxide is a white pigment, and has three crystal forms: rutile, anatase, and brookite. Among them, rutile titanium oxide is preferred. Titanium oxide can be industrially produced by the sulfuric acid method and the chlorine method, and the titanium oxide used in the present invention may be produced by either method.
[0024] The volume-based cumulative 50% particle diameter (hereinafter also referred to as the average particle diameter) of the titanium oxide particles is preferably 200 nm or more and 500 nm or less. In particular, the volume-based cumulative 50% particle diameter of the titanium oxide particles is more preferably 200 nm or more and 400 nm or less. The volume-based cumulative 50% particle diameter of the titanium oxide particles (D 50 ) is the diameter of the particle that is 50% of the total volume of the measured particles in the particle size accumulation curve, calculated from the small particle size side. 50can be measured under the following conditions: SetZero: 30 seconds, number of measurements: 3, measurement time: 180 seconds, shape: aspheric, refractive index: 2.60. A particle size analyzer using a dynamic light scattering method can be used as the particle size distribution measuring device. Of course, the measurement conditions are not limited to those described above.
[0025] Titanium oxide that has been surface-treated with alumina and silica is used. The surface treatment is expected to suppress photocatalytic activity and improve dispersibility. In this specification, "alumina" is a general term for oxides of aluminum such as aluminum oxide. In this specification, "silica" is a general term for silicon dioxide or a substance composed of silicon dioxide. Most of the alumina and silica that coat titanium oxide are present in the form of silicon dioxide and aluminum oxide.
[0026] The ratio (mass%) of titanium oxide in the titanium oxide particles is preferably 85.00% by mass or more based on the total mass of the titanium oxide particles. The ratio (mass%) of titanium oxide in the titanium oxide particles is preferably 98.50% by mass or less based on the total mass of the titanium oxide particles. The ratio (mass%) of alumina in the titanium oxide particles is preferably 1.50 times or less, more preferably 0.50 times or more and 1.00 times or less, in terms of mass ratio to the ratio (mass%) of silica. The ratio (mass%) of alumina in the titanium oxide particles is preferably 0.50% by mass or more and 9.00% by mass or less based on the total mass of the titanium oxide particles, more preferably 0.50% by mass or more and 4.00% by mass or less based on the total mass of the titanium oxide particles. The ratio (mass%) of silica in the titanium oxide particles is preferably 0.50% by mass or more and 9.00% by mass or less based on the total mass of the titanium oxide particles, more preferably 1.00% by mass or more and 4.00% by mass or less based on the total mass of the titanium oxide particles.
[0027] The ratio of alumina and silica in titanium oxide particles, i.e., the amount of alumina and silica coating, can be measured by, for example, quantitative analysis of aluminum and silicon elements by inductively coupled plasma (ICP) emission spectrometry. In this case, it is assumed that all atoms coated on the surface are oxides, and the obtained values of aluminum and silicon can be calculated by converting them to their oxides, i.e., alumina and silica. The ratio (mass%) of aluminum element in titanium oxide particles obtained by inductively coupled plasma emission spectrometry is preferably 1.70 times or less in mass ratio to the ratio (mass%) of silicon element. When this value is converted to its oxides, i.e., alumina and silica, the ratio (mass%) of alumina in titanium oxide particles is 1.50 times or less in mass ratio to the ratio (mass%) of silica.
[0028] Surface treatment methods for titanium oxide include wet treatment and dry treatment. For example, titanium oxide can be dispersed in a liquid medium and then reacted with a surface treatment agent such as sodium aluminate or sodium silicate to perform surface treatment, and the desired characteristics can be achieved by appropriately changing the ratio of these surface treatment agents. In addition to alumina and silica, inorganic oxides such as zinc oxide and zirconia, and organic substances such as polyols can also be used for surface treatment, as long as the effects of the present invention are not impaired.
[0029] As long as the effect of the present invention is not impaired, the ink may contain other pigments besides titanium oxide. In this case, the ink may be of a color other than white ink. The content (mass %) of the other pigments in the ink is preferably 0.10 mass % or more and 5.00 mass % or less, and more preferably 0.10 mass % or more and 1.00 mass % or less, based on the total mass of the ink.
[0030] The ratio of acid sites (μmol / g) on the surface of titanium oxide particles in the ink to the base sites (μmol / g) must be 0.40 to 0.55 times. As mentioned above, the acid sites and base sites on the surface of titanium oxide particles vary depending on the amount of silica and alumina that coat the titanium oxide particles. In other words, it is possible to adjust the acid sites and base sites by increasing or decreasing the amount of silica and alumina that are coated.
[0031] The acid sites (μmol / g) on the surface of the titanium oxide particles in the ink are preferably 6.0 μmol / g or more and 15.0 μmol / g or less. If the acid sites are less than 6.0 μmol / g, the titanium oxide particles will have insufficient acid sites, and the electric double layer will not be sufficiently formed, and the storage stability and sedimentation resistance may not be sufficiently obtained. On the other hand, if the acid sites are more than 15.0 μmol / g, the titanium oxide particles will have an excess of acid sites, and the formation of the electric double layer will be inhibited by salting out, and the storage stability may not be sufficiently obtained.
[0032] The basic sites (μmol / g) on the surface of the titanium oxide particles in the ink are preferably 15.0 μmol / g or more and 27.3 μmol / g or less. If the basic sites are less than 15.0 μmol / g, the negative charges of the surface hydroxyl groups derived from silica are relatively high, so salting out is likely to occur, and storage stability and sedimentation resistance may not be sufficiently obtained. If the basic sites are more than 27.3 μmol / g, the basic sites are too many, so the negative charges of the surface hydroxyl groups derived from silica are canceled, and the formation of an electric double layer may not be sufficient. As a result, storage stability and sedimentation resistance may not be sufficiently obtained.
[0033] In the present invention, the acid sites and base sites on the surface of titanium oxide particles can be quantified as follows. Specifically, n-butyl ether / triethylamine is added to titanium oxide particles, and solid components such as titanium oxide particles are filtered off. The content of triethylamine in the resulting supernatant is then quantified by gas chromatography or the like, thereby quantifying the acid sites on the surface of titanium oxide particles. The base sites on the surface of titanium oxide particles can be quantified in the same manner by using n-butyl ether / acetic acid instead of n-butyl ether / triethylamine.
[0034] (monovalent cation) The ink preferably contains a monovalent cation. In this specification, the term "monovalent cation" refers to an alkali metal ion, an ammonium ion, or an organic ammonium ion, and is a cation that has a proton (H + ) is not included. In particular, the ink preferably contains an alkali metal ion, and more preferably contains a potassium ion. The content (mass%) of monovalent cations in the ink is preferably 700 ppm or more and 1,300 ppm or less based on the total mass of the ink. By setting the content of monovalent cations within the above range, the formation of negative charges on the surface hydroxyl groups derived from silica is efficiently promoted, and the dispersed state of titanium oxide particles can be stably maintained. As a result, the storage stability and sedimentation resistance can be further improved. In addition, when the ink contains a divalent or higher cation, the content is preferably 10 ppm or less based on the total mass of the ink. The ink does not need to contain a divalent or higher cation. The content of monovalent cations in the ink can be measured, for example, by quantifying the content of various monovalent cations using ICP emission analysis or ion chromatography.
[0035] Furthermore, the aluminum ion content (ppm) in the ink must be 30 ppm or less based on the total mass of the ink. The aluminum ion content may be 0 ppm. In other words, the ink may not substantially contain aluminum ions. In particular, the aluminum ion content is preferably 5 ppm or more and 25 ppm or less based on the total mass of the ink. The aluminum ion content in the ink can be measured, for example, by removing solids in the ink by centrifugation or the like, and then quantifying the aluminum element content using ICP emission spectrometry or ion chromatography.
[0036] (Compound represented by general formula (1)) The titanium oxide particles in the ink are dispersed at least by the action of silica. In addition to these, a component that assists in dispersing the titanium oxide particles may be contained. Such a component includes a compound represented by the following general formula (1). Some of the compounds represented by general formula (1) are known as silane coupling agents. The content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.01 mass% or more and 1.00 mass% or less, and more preferably 0.02 mass% or more and 0.50 mass% or less, based on the total mass of the ink. In addition, the content (mass%) of the compound represented by general formula (1) in the ink is preferably 0.002 times or more and 0.10 times or less in mass ratio to the content (mass%) of the titanium oxide particles.
[0037] A part of OR1 bonded to silicon atoms in the compound represented by general formula (1) is hydrolyzed in an aqueous medium to form a silanol group. Therefore, it has affinity with the surface hydroxyl groups derived from silica on the titanium oxide particle surface. In addition to the structure capable of forming a silanol group as described above, the compound represented by general formula (1) also has a structure having n alkylene oxide groups having 2 to 4 carbon atoms as repeating units ((OR4) in general formula (1)) via X, which serves as a linking group. n) Hereinafter, the above structure will also be referred to as an alkylene oxide chain. Since the alkylene oxide chain is hydrophilic, it extends appropriately in an aqueous medium and exhibits a repulsive force due to steric hindrance. Therefore, the compound represented by general formula (1) has the effect of assisting the dispersion of titanium oxide particles.
[0038] [ka]
[0039] (In general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Each R4 is independently an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)
[0040] In the general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, and an n-butyl group. Among them, a methyl group is preferable from the viewpoint of ease of hydrolysis. If R1, R2, and R3 are each an alkyl group having more than 4 carbon atoms, it becomes difficult to form a silanol group by hydrolysis, and affinity with titanium oxide particles is not obtained. Therefore, titanium oxide particles cannot be stably dispersed, and storage stability and sedimentation resistance may not be sufficiently obtained. a representing the number of R1O is 1 to 3, and b representing the number of R2 is 0 to 2, and a+b=3. Among them, it is preferable that a is 3 and b is 0, that is, all three substituents of the silicon atom are R1O.
[0041] In the general formula (1), R4 is independently an alkylene group having 2 to 4 carbon atoms. Examples of the alkylene group having 2 to 4 carbon atoms include an ethylene group, an n-propylene group, an i-propylene group, and an n-butylene group. Among them, an ethylene group is preferable. The number of OR4, that is, n (average value) representing the number of alkylene oxide groups, is 6 to 24. When n is less than 6, the length of the alkylene oxide chain is too short, and the repulsive force due to steric hindrance is not sufficiently obtained, so that the dispersion stability is not sufficiently obtained. As a result, the storage stability and sedimentation resistance may not be sufficiently obtained. When n is more than 24, the length of the alkylene oxide chain is too long, so that the hydrophilicity is increased and the compound is easily liberated in the aqueous medium. Therefore, the affinity with the surface hydroxyl group derived from the silica of the titanium oxide particles is not sufficiently obtained, and the aggregation of the titanium oxide particles may be difficult to efficiently suppress. Therefore, the dispersion stability is not sufficiently obtained, and the storage stability and sedimentation resistance may not be sufficiently obtained.
[0042] In the general formula (1), X is a single bond or an alkylene group having 1 to 6 carbon atoms. When X is a single bond, it means that the silicon atom and OR4 are directly bonded. Examples of the alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, an n-propylene group, an i-propylene group, an n-butylene group, an n-pentylene group, and an n-hexylene group. Among them, an n-propylene group is preferable. When X is an alkylene group having more than 6 carbon atoms, the hydrophobicity of the compound represented by the general formula (1) becomes too high, the effect of stably dispersing titanium oxide particles is weak, and storage stability and sedimentation resistance may not be sufficiently obtained.
[0043] (resin) The ink may contain a resin. Examples of the resin include acrylic resin, urethane resin, and urea resin. Of these, acrylic resin is preferred. The content (mass%) of the resin in the ink is preferably 1.00% by mass or more and 25.00% by mass or less, and more preferably 3.00% by mass or more and 15.00% by mass or less, based on the total mass of the ink. Of these, the content is particularly preferably 5.00% by mass or more and 15.00% by mass or less.
[0044] The resin can be contained in the ink for the purpose of improving various properties of the recorded image, such as abrasion resistance and hiding power. Examples of the form of the resin include block copolymers, random copolymers, graft copolymers, and combinations thereof. The resin may be a soluble resin that can be dissolved in a liquid medium, or may be resin particles that are dispersed in the liquid medium. The resin particles do not need to encapsulate a coloring material.
[0045] In this specification, "a resin is soluble" means that when the resin is neutralized with an alkali equivalent to the acid value, the resin is present in a liquid medium in a state in which it does not form particles whose particle size can be measured by dynamic light scattering. Whether or not a resin is soluble can be determined according to the following method. First, a liquid (resin solid content: 10 mass%) containing a resin neutralized with an alkali (sodium hydroxide, potassium hydroxide, etc.) equivalent to the acid value is prepared. Next, the prepared liquid is diluted 10 times (volume basis) with pure water to prepare a sample solution. Then, when the particle size of the resin in the sample solution is measured by dynamic light scattering, if particles having a particle size are not measured, the resin can be determined to be soluble. The measurement conditions at this time can be, for example, SetZero: 30 seconds, number of measurements: 3 times, and measurement time: 180 seconds. As a particle size distribution measuring device, a particle size analyzer using a dynamic light scattering method (for example, product name "UPA-EX150", manufactured by Nikkiso) can be used. Of course, the particle size distribution measuring device and the measurement conditions are not limited to those described above.
[0046] The acid value of the water-soluble resin is preferably 80 mgKOH / g or more and 250 mgKOH / g or less, more preferably 100 mgKOH / g or more and 200 mgKOH / g or less. When resin particles are used, the acid value is preferably 0 mgKOH / g or more and 50 mgKOH / g or less. The weight average molecular weight of the water-soluble resin is preferably 1,000 or more and 30,000 or less, more preferably 5,000 or more and 15,000 or less. The weight average molecular weight of the resin constituting the resin particles is preferably 1,000 or more and 3,000,000 or less, more preferably 100,000 or more and 3,000,000 or less. The weight average molecular weight of the resin is a value measured by gel permeation chromatography (GPC) in terms of polystyrene.
[0047] (aqueous medium) The ink is an aqueous ink containing water as an aqueous medium. The ink may contain water or an aqueous medium that is a mixed solvent of water and a water-soluble organic solvent. As the water, it is preferable to use deionized water (ion-exchanged water). The content (mass %) of water in the ink is preferably 50.00 mass % or more and 95.00 mass % or less based on the total mass of the ink.
[0048] The water-soluble organic solvent is not particularly limited as long as it is water-soluble (preferably, dissolves in water at any ratio at 25°C). Specifically, monohydric or polyhydric alcohols, alkylene glycols, glycol ethers, nitrogen-containing polar compounds, sulfur-containing polar compounds, etc. can be used. The content (mass%) of the water-soluble organic solvent in the ink is preferably 3.00% by mass or more and 50.00% by mass or less, and more preferably 10.00% by mass or more and 40.00% by mass or less, based on the total mass of the ink. If the content (mass%) of the water-soluble organic solvent is less than 3.00% by mass, the ink may be stuck in the inkjet recording device, and sufficient sticking resistance may not be obtained. If the content (mass%) of the water-soluble organic solvent is more than 50.00% by mass, poor ink supply may occur.
[0049] (Other additives) In addition to the above additives, the ink may contain various additives such as surfactants, pH adjusters, rust inhibitors, preservatives, antifungal agents, antioxidants, reduction inhibitors, evaporation promoters, and chelating agents, as necessary. Among these, it is preferable that the ink contains a surfactant. The content (mass%) of the surfactant in the ink is preferably 0.10% by mass or more and 5.00% by mass or less, and more preferably 0.10% by mass or more and 2.00% by mass or less, based on the total mass of the ink. Examples of surfactants include anionic surfactants, cationic surfactants, and nonionic surfactants. Among these, nonionic surfactants are preferable because they have low affinity with titanium oxide particles and are effective in small amounts, since they are used to adjust various physical properties of the ink.
[0050] (Ink properties) Since the ink is applied to the inkjet method, it is preferable to appropriately control the physical properties of the ink. The surface tension of the ink at 25°C is preferably 10 mN / m or more and 60 mN / m or less, and more preferably 20 mN / m or more and 40 mN / m or less. The surface tension of the ink can be adjusted by appropriately determining the type and content of the surfactant in the ink. In addition, the viscosity of the ink at 25°C is preferably 1.0 mPa·s or more and 10.0 mPa·s or less. The pH of the ink at 25°C is preferably 7.0 or more and 9.0 or less, and more preferably 7.0 or more and 8.5 or less. By setting the pH of the ink in the above range, it is possible to maintain a stable dispersion state of the titanium oxide particles while suppressing the elution of alumina, which is promoted as the pH increases. The pH of the ink can be measured with a general pH meter equipped with a glass electrode or the like.
[0051] <Ink cartridges> The ink cartridge of the present invention includes ink and an ink storage section that stores the ink. The ink stored in the ink storage section is the water-based ink (white ink) of the present invention described above. FIG. 1 is a cross-sectional view that shows a schematic diagram of an embodiment of the ink cartridge of the present invention. As shown in FIG. 1, an ink supply port 12 for supplying ink to a recording head is provided on the bottom surface of the ink cartridge. The inside of the ink cartridge serves as an ink storage section for storing ink. The ink storage section is composed of an ink storage chamber 14 and an absorber storage chamber 16, which are communicated with each other via a communication port 18. The absorber storage chamber 16 is also communicated with the ink supply port 12. The ink storage chamber 14 stores liquid ink 20, and the absorber storage chamber 16 stores absorbers 22 and 24 that hold the ink in an impregnated state. The ink storage section may not have an ink storage chamber that stores liquid ink, and may be in a form in which the entire amount of ink stored is held by the absorber. The ink containing section may also be of a type that does not have an absorber and contains the entire amount of ink in a liquid state.Furthermore, the ink cartridge may be of a type that is configured to have an ink containing section and a recording head.
[0052] <Inkjet recording method> The inkjet recording method of the present invention is a method of discharging the above-described aqueous ink of the present invention from an inkjet recording head to record an image on a recording medium. Examples of the method of discharging the ink include a method of imparting mechanical energy to the ink and a method of imparting thermal energy to the ink. In the present invention, it is particularly preferable to adopt a method of discharging the ink by imparting thermal energy to the ink. Other than using the ink of the present invention, the steps of the inkjet recording method may be publicly known. For example, when recording an image using white ink, a general inkjet recording method may be applied as it is. In addition, when using white ink as a base treatment for color inks, an image may be recorded by applying color inks (inks such as black, cyan, magenta, and yellow) so as to overlap at least a part of the area to which the white ink has been applied.
[0053] Furthermore, it can also be used for back printing, in which white ink is applied so as to overlap at least a part of the area where color inks are applied. The recording medium is not particularly limited, but since the water-based ink of the present invention can be used as a white ink, it is preferable to use a transparent or colored recording medium. In addition, the recording medium may be a poorly absorbing medium (non-absorbing medium) that has low absorbency of the liquid medium, such as a resin film.
[0054] FIG. 2 is a diagram showing an example of an inkjet recording device used in the inkjet recording method of the present invention, in which (a) is a perspective view of the main part of the inkjet recording device, and (b) is a perspective view of a head cartridge. The inkjet recording device is provided with a conveying means (not shown) for conveying a recording medium 32, and a carriage shaft 34. A head cartridge 36 can be mounted on the carriage shaft 34. The head cartridge 36 includes recording heads 38 and 40, and is configured so that an ink cartridge 42 is set thereon. While the head cartridge 36 is conveyed in the main scanning direction along the carriage shaft 34, ink (not shown) is ejected from the recording heads 38 and 40 toward the recording medium 32. Then, an image is recorded on the recording medium 32 by conveying the recording medium 32 in the sub-scanning direction by a conveying means (not shown).
[0055] Multi-pass printing is preferred in which the application of ink to a unit area of a print medium is performed by multiple relative scans of the print head and the print medium. In particular, it is preferred to apply white ink and color ink to a unit area by different relative scans. This increases the time until the inks come into contact with each other, making it easier to suppress mixing. The unit area can be set as any area, such as one pixel or one band. EXAMPLES
[0056] The present invention will be described in more detail below with reference to examples, comparative examples, and reference examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. "Parts" and "%" used to describe the amounts of components are based on mass unless otherwise specified. In addition, a dispersion of titanium oxide particles is referred to as a "pigment dispersion."
[0057] <Preparation of titanium dioxide> We used untreated titanium oxide, TITANIX JR (manufactured by Teika, rutile-type titanium oxide), and titanium oxide particles prepared by surface-treating the above titanium oxide. The cumulative 50% particle diameter (D 50 ) was measured using a particle size analyzer (trade name "Nanotrac WaveII-EX150", manufactured by Microtrack Bell) using the dynamic light scattering method. The properties of titanium oxide particles are shown in Table 1.
[0058] (Measurement of the amount of alumina and silica coating) The ratio of alumina and silica in the titanium oxide particles, i.e., the amount of alumina and silica coating, was measured as follows. The prepared titanium oxide particles were added to nitric acid to prepare a liquid, and quantitative analysis of aluminum and silicon elements was performed using an inductively coupled plasma (ICP) emission spectrometer. In this case, it was assumed that all atoms coating the surface were in the form of oxides, and the obtained values of aluminum and silicon were converted to the oxides, i.e., alumina and silica, to calculate the mass ratio.
[0059] (Acid and base site measurements) Each titanium oxide particle was uniformly ground in a mortar. 0.25 g of titanium oxide particles and 3.00 g of 0.01 mol / L acetic acid / dibutyl ether solution were placed in a vial, sealed, and shaken for 1 hour. Then, the vial was filtered through a polytetrafluoroethylene (PTFE) membrane filter with a pore size of 0.1 μm to obtain a filtrate. The acetic acid content in the filtrate was quantified by gas chromatography (product name "GC-2014", manufactured by Shimadzu Corporation), to quantify the basic sites on the surface of the titanium oxide particles.
[0060] A filtrate was obtained in the same manner as above, except that a 0.01 mol / L triethylamine / dibutyl ether solution was used instead of the 0.01 mol / L acetic acid / dibutyl ether solution. The triethylamine content in the filtrate was quantified by gas chromatography as described above, thereby quantifying the acid sites on the surface of the titanium oxide particles.
[0061] (Titanium oxide particles 1-9, 11, 12) Titanium oxide particles were produced by surface treatment of the titanium oxide using a wet method. Surface treatment using the wet method involves contacting untreated titanium oxide with a surface treatment agent (sodium aluminate, sodium silicate, etc.), and the amount and ratio of the surface treatment agent used were appropriately adjusted to provide a surface treatment at any ratio.
[0062] Specifically, 300 parts of rutile-type titanium oxide (trade name "TITANIX JR", manufactured by Teika Co., Ltd.) that had not been subjected to surface treatment and 700 parts of pure water were mixed with a homogenizer. Then, the temperature was raised to 90°C while stirring, and potassium hydroxide (pH adjuster) was added to adjust the pH to 10.5. Next, sodium silicate was added, and dilute sulfuric acid (pH adjuster) was added over about 1 hour to adjust the pH to 5.0. The reaction was continued for about 1 hour. Thereafter, sodium aluminate was added little by little at 90°C. At this time, in order to maintain the pH, dilute sulfuric acid was used in combination to maintain the pH at 6.0 to 8.0. After the addition of sodium aluminate, the reaction was continued for about 1 hour to obtain a dispersion. The dispersion was cooled to 25°C, and then purified by repeatedly sedimenting with a centrifuge and redispersing in ion-exchanged water, and dried at 120°C to obtain titanium oxide particles that had been subjected to surface treatment with at least one of alumina and silica. Table 1 shows the characteristics of each titanium oxide particle.
[0063] (Titanium oxide particles 10) Untreated rutile-type titanium oxide (product name "TITANIX JR", manufactured by Teika Co., Ltd.) was used as the titanium oxide particles 10. Table 1 also shows the properties of the titanium oxide particles 10.
[0064] [Table 1]
[0065] <Preparation of the compound represented by general formula (1)> The compound represented by general formula (1) was synthesized by the following procedure. The synthesis conditions and structures of the compound synthesized as the compound represented by general formula (1) and the comparative compound are shown in Tables 2 and 3, respectively. The compound represented by general formula (1) can be synthesized by allylation and hydrosilylation of a raw material (such as a polyalkylene glycol monoalkyl ether).
[0066] The raw materials, base, and solvent shown in Table 2 were placed in a three-neck flask equipped with a stirrer and a nitrogen inlet tube, and stirred at 25°C for 30 minutes. As the "sodium hydride", a paraffin dispersion of 60% sodium hydride was used, and the dispersion was used so that the amount of sodium hydride used was as shown in Table 2. Then, the bromide shown in Table 2 was added dropwise while stirring at 25°C, and stirring was continued for 12 hours after the end of the dropwise addition to obtain a solution containing the reactants. After filtering out the unreacted sodium hydride and neutralized product (sodium bromide) from the solution containing the reactants, THF was removed under reduced pressure to obtain a concentrate. The concentrate was dissolved in 500 parts of pure water, and this aqueous solution was extracted three times with 200 mL of hexane, and then extracted with 200 mL of dichloromethane. The solvent containing the product was dried by adding magnesium sulfate, and concentrated under reduced pressure to obtain each of the allylated compounds (allylation process).
[0067] The allylated raw materials and silane compounds shown in Table 2 were placed in a dry, passivated round-bottom flask equipped with a stirrer and an argon inlet tube, and stirred at 85°C. Then, 0.54 parts of an aqueous solution of 65 mmol / L chloroplatinic acid monohydrate in isopropyl alcohol was added, and the mixture was heated at 85°C for 5 hours. After the reaction was completed, the mixture was allowed to cool to 25°C, and the excess silane compounds were removed under reduced pressure. The residue was purified by column chromatography using silica gel passivated with triethoxysilane as a carrier to obtain each compound (hydrosilylation step). The eluent used for purification by column chromatography was ethyl acetate / hexane / ethanol = 85 / 15 / 5 (by volume).
[0068] [Table 2]
[0069] [Table 3]
[0070] <Preparation of pigment dispersion> Pigment dispersions were produced according to the following procedure. The production conditions for the pigment dispersions are shown in Table 4. 40.00 parts of titanium oxide particles, a dispersant, a neutralizer, and ion-exchanged water with a total of 100.00 parts of the components shown in Table 4 were mixed, and preliminary dispersion was performed using a homogenizer. Then, dispersion treatment (main dispersion) was performed for 12 hours at 25°C using 0.5 mm zirconia beads with a paint shaker. When a neutralizer was used, the amount of the neutralizer used was appropriately adjusted so that the pH of the main dispersion was 9 to 11. The pH of the main dispersion was measured using a pH meter (trade name "Portable pH Meter D-74", manufactured by Horiba, Ltd.) at the time of starting the main dispersion. The zirconia beads were filtered off, and an appropriate amount of ion-exchanged water was added as necessary to prepare each pigment dispersion with a titanium oxide particle content of 40.00%. In Table 4, T-50 is the trade name of sodium salt of polyacrylic acid (polyacrylic acid content: 43%, weight average molecular weight: 6,000) manufactured by Toa Gosei.
[0071] [Table 4]
[0072] <Ink Preparation> The types and amounts of each component shown in the upper rows of Tables 5 to 7 were mixed and stirred. Vinyblan 2685 is the trade name of an acrylic emulsion (content of acrylic resin particles: 30%) manufactured by Nissin Chemical Industry. Acetylenol E60 (trade name) is a nonionic surfactant manufactured by Kawaken Fine Chemical. Proxel GXL (S) (trade name) is a preservative manufactured by LONZA. After that, pressure filtration was performed using a membrane filter (manufactured by Sartorius) with a pore size of 5.0 μm to prepare each ink. The content of the compound represented by general formula (1) in the ink is shown in the column "Content D (%) of specific compound" in Tables 5 to 7.
[0073] (Calculation of the content of monovalent cations in ink) The content of monovalent cations in the ink was measured by ICP emission spectrometry. Specifically, each ink was diluted with ion-exchanged water so that the pigment content of each ink was 0.04%, and the content of various monovalent cations was quantified using an ICP emission spectrometry device (product name "SPS5100 ICP-OES", manufactured by SII). In addition, the concentration of ammonium ions among the monovalent cations was measured using an ion chromatograph (product name "DX-320", manufactured by Dionex). Then, the content of monovalent cations (ppm) in the titanium oxide particle content of the ink before dilution was calculated from the quantified content of monovalent cations. The content of monovalent cations is summarized below in Tables 5 to 7, together with the characteristics of each ink.
[0074] (Calculation of aluminum ion content) The aluminum ion content in the ink was measured by ICP emission spectrometry. Specifically, the prepared inks were centrifuged to remove solids such as titanium oxide particles and resin particles. The aluminum ion content of the resulting supernatant was quantified using an ICP emission spectrometer (product name "SPS5100 ICP-OES", manufactured by SII).
[0075] [Table 5]
[0076] [Table 6]
[0077] [Table 7]
[0078] <Evaluation> The inks obtained above were evaluated for the following items. In the present invention, for each of the evaluation criteria for the following items, "AA", "A" and "B" were considered acceptable levels, and "C" was considered unacceptable. The evaluation results are shown in Table 8.
[0079] (Storage stability) The volume-based cumulative 50% particle diameter of the titanium oxide particles in the prepared ink was measured (referred to as "particle diameter before storage"). The volume-based cumulative 50% particle diameter of the titanium oxide particles (D 50) was measured using a particle size analyzer (product name "Nanotrac WaveII-EX150", manufactured by Microtrack Bell) using the dynamic light scattering method. Each ink was placed in a sealed container and stored at 70°C for 7 days. This condition is an accelerated test assuming that the ink is stored at 25°C for half a year. After the ink was returned to 25°C, the particle size of the titanium oxide particles was measured again (referred to as "particle size after storage"). The particle size change rate was calculated based on the formula "particle size change rate" (%) = 100 x ("particle size after storage" - "particle size before storage") / ("particle size before storage"), and the storage stability of the ink was evaluated according to the following evaluation criteria. AA: The rate of change in particle size was 10% or less. A: The rate of change in particle size was more than 10% but not more than 20%. B: The rate of change in particle size was more than 20% and 30% or less. C: The rate of change in particle size exceeded 30%.
[0080] (Sedimentation resistance) Each prepared ink was diluted 3,000 times (by mass). For dilution, a liquid obtained by diluting a boric acid pH standard solution (pH: 9.18) 10 times (by mass) with pure water was used. Then, the absorbance at 550 nm was measured (referred to as "A0"). For measuring the absorbance, a spectrophotometer (product name "U-3900H", manufactured by Hitachi) was used. Next, 10 mL of the diluted liquid was filled into a 10 mL graduated cylinder, sealed with a silicon stopper, and left to stand for 180 minutes. After that, the ink was sequentially removed from the top, and the absorbance at 550 nm was measured using the bottom 2 mL of ink in the same manner as above (referred to as "A1"). Then, the rate of change in absorbance was calculated based on the formula "rate of change in absorbance" (%) = 100 × ("A1" - "A0") / ("A0"), and the sedimentation resistance of the ink was evaluated according to the evaluation criteria shown below. These conditions are used to evaluate the properties of ink when it is left to stand for a short period of time (for example, about one day). If the rate of change in absorbance is low, this means that the titanium oxide particles in the ink hardly settle when left to stand for a short period of time, and that the ink has excellent sedimentation resistance. On the other hand, if the rate of change in absorbance is high, this means that the titanium oxide particles in the ink settle even when left to stand for a short period of time, and that the ink has insufficient sedimentation resistance. AA: The rate of change in absorbance was 2% or less. A: The rate of change in absorbance was more than 2% but not more than 6%. B: The rate of change in absorbance was more than 6% and 10% or less. C: The rate of change in absorbance was more than 10%.
[0081] [Table 8]
[0082] The disclosure of this embodiment includes the following configurations and methods.
[0083] [Configuration 1] A water-based inkjet ink containing titanium oxide particles, the titanium oxide particles are titanium oxide having at least a part of their surface covered with alumina and silica, and are dispersed at least by the action of the silica; the content (ppm) of aluminum ions in the aqueous ink is 30 ppm or less based on the total mass of the ink; The aqueous ink is characterized in that the ratio of acid sites (μmol / g) on the surface of the titanium oxide particles in the aqueous ink to basic sites (μmol / g) is 0.40 to 0.55 times.
[0084] [Configuration 2] 2. The aqueous ink according to claim 1, wherein the number of acid sites (μmol / g) on the surface of the titanium oxide particles in the aqueous ink is 6.0 μmol / g or more and 15.0 μmol / g or less, and the number of basic sites (μmol / g) on the surface of the titanium oxide particles is 15.0 μmol / g or more and 27.3 μmol / g or less.
[0085] [Configuration 3] 3. The aqueous ink according to claim 1 or 2, further comprising a monovalent cation.
[0086] [Configuration 4] 4. The aqueous ink according to any one of claims 1 to 3, wherein the content (ppm) of monovalent cations in the aqueous ink is 700 ppm or more and 1,300 ppm or less based on the total mass of the ink.
[0087] [Configuration 5] 5. The water-based ink according to any one of configurations 1 to 4, further comprising a compound represented by general formula (1).
[0088] [ka]
[0089] (In general formula (1), R1, R2, and R3 are each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Each R4 is independently an alkylene group having 2 to 4 carbon atoms. X is a single bond or an alkylene group having 1 to 6 carbon atoms. n is 6 to 24. a is 1 to 3, b is 0 to 2, and a+b=3.)
[0090] [Configuration 6] An ink cartridge including an ink and an ink storage section for storing the ink, 6. An ink cartridge, wherein the ink is the aqueous ink described in any one of configurations 1 to 5.
[0091] [Method 1] An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, comprising: 6. An ink-jet recording method, wherein the ink is the aqueous ink described in any one of Configurations 1 to 5.
Claims
1. A water-based inkjet ink containing titanium oxide particles, the titanium oxide particles are titanium oxide having at least a part of their surface covered with alumina and silica, and are dispersed at least by the action of the silica; the content (ppm) of aluminum ions in the aqueous ink is 30 ppm or less based on the total mass of the ink; The aqueous ink, characterized in that the ratio of acid sites (μmol / g) on the surface of the titanium oxide particles in the aqueous ink to basic sites (μmol / g) is 0.40 to 0.55 times.
2. 2. The aqueous ink according to claim 1, wherein the titanium oxide particles in the aqueous ink have a surface concentration of acid sites (μmol / g) of 6.0 μmol / g or more and 15.0 μmol / g or less, and a surface concentration of basic sites (μmol / g) of 15.0 μmol / g or more and 27.3 μmol / g or less.
3. The aqueous ink of claim 1 , further comprising a monovalent cation.
4. 2. The aqueous ink according to claim 1, wherein the content (ppm) of monovalent cations in the aqueous ink is 700 ppm or more and 1,300 ppm or less based on the total mass of the ink.
5. The water-based ink according to claim 1 , further comprising a compound represented by general formula (1): [Case 1] (In general formula (1), R 1 , R 2 , and R 3 Each of R is independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 4 are each independently an alkylene group having 2 to 4 carbon atoms; X is a single bond or an alkylene group having 1 to 6 carbon atoms; n is 6 to 24; a is 1 to 3, b is 0 to 2, and a+b=3.
6. An ink cartridge including an ink and an ink storage section for storing the ink, 6. An ink cartridge, wherein the ink is a water-based ink as claimed in claim 1.
7. An inkjet recording method for recording an image on a recording medium by ejecting ink from an inkjet recording head, comprising:
6. An ink-jet recording method, wherein the ink is a water-based ink according to claim 1.
Citation Information
Patent Citations
Method for producing aqueous pigment dispersion
JP2011225867A
Titanium dioxide
JP2017521348A
White inks
WO2018190848A1