Method for producing composition

By adding an organic compound with a cyclic ether structure to a vinyl polymer produced via living radical polymerization, the method addresses the issues of discoloration and inferior tensile properties in (meth)acrylic acid alkyl ester polymers, resulting in improved flexibility and weather resistance.

JP2024141073AInactive Publication Date: 2024-10-10AGC INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052523
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing (meth)acrylic acid alkyl ester polymers with reactive silicon groups using living radical polymerization often result in inferior tensile properties and are prone to discoloration due to the random introduction of reactive silicon groups and the use of halogen compounds as initiators.

Method used

A method involving the addition of an organic compound with a cyclic ether structure to a vinyl polymer produced via living radical polymerization using an organic halide initiator, controlled by a specific catalyst, to suppress discoloration and improve tensile properties.

Benefits of technology

The method effectively suppresses discoloration and enhances the tensile properties of the resulting polymer, making it suitable for applications requiring flexibility and weather resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141073000001
    Figure 2024141073000001
Patent Text Reader

Abstract

To provide a method for producing a polymer that can reduce the coloration of vinyl polymers with lapse of time when the polymer is stored at a high temperature.SOLUTION: There is provided a method for producing a composition containing a vinyl polymer (A) and an organic compound having a cyclic ether structure, wherein the vinyl polymer (A) is obtained by subjecting a vinyl compound (a) to a living radical polymerization reaction with an initiator that is an organic halide having at least one halogen atom in the presence of a catalyst (C), and wherein an addition amount of the organic compound having a cyclic ether structure is 0.5 to 5 pts.mass with respect to 100 pts.mass of the vinyl polymer (A).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a composition. [Background technology]

[0002] Oxyalkylene polymers having a reactive silicon group are widely used in curable compositions for applications such as sealants, adhesives, paints, etc., because they give cured products excellent in flexibility, tensile properties, coating workability, etc. It is known that the weather resistance of the cured product of a curable composition containing an oxyalkylene polymer having a reactive silicon group can be improved by adding a (meth)acrylic acid alkyl ester polymer having a reactive silicon group.

[0003] Conventionally, a (meth)acrylic acid alkyl ester polymer having a reactive silicon group has been produced by a method using a radical polymerization initiator having a reactive silicon group, a chain transfer agent, etc. In such a production method, reactive silicon groups are likely to be irregularly introduced into the side chain of the main chain skeleton of the carbon-carbon bond chain of the (meth)acrylic acid alkyl ester polymer, and the obtained polymer has inferior tensile properties compared to an oxyalkylene polymer having a reactive silicon group.

[0004] In recent years, in order to improve such physical properties, studies have been made on controlling the introduction of reactive silicon groups into alkyl (meth)acrylate polymers using living radical polymerization methods.

[0005] For example, Patent Document 1 describes living radical polymerization by atom transfer radical polymerization (ATRP) using an organic halide or a sulfonyl halide compound as an initiator and a transition metal complex such as a copper bromide-pentamethyldiethylenetriamine complex as a catalyst. It describes that in this living radical polymerization by ATRP, a polymer having a terminal halogen is obtained, and a vinyl polymer ((meth)acrylic acid alkyl ester polymer) having a crosslinkable silicon group (reactive silicon group) at the molecular end is obtained by a conversion reaction of the terminal halogen.

[0006] Patent Document 2 describes a reversible coordination mediated polymerization (RCMP) type living radical polymerization method using a halogen-containing compound as an initiator. It describes that this RCMP type living radical polymerization method can obtain a vinyl polymer ((meth)acrylic acid alkyl ester polymer) having a hydrolyzed silicon group (reactive silicon group) near the molecular end by polymerizing a vinyl monomer having a hydrolyzed silicon group (reactive silicon group). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2005 / 095492 [Patent Document 2] Patent Publication No. 2022-75627 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the living radical polymerization described in Patent Document 1 and Patent Document 2, a halogen compound is used as an initiator, and therefore, there is a problem that a composition containing the polymer is likely to become discolored over time when stored at high temperatures. [Means for solving the problem]

[0009] The present invention is based on the discovery that a composition comprising a vinyl polymer obtained by living radical polymerization using an initiator that is an organic halide having a halogen atom, and an organic compound having a cyclic ether structure added thereto, can suppress coloration of the composition over time during storage at high temperatures.

[0010] The present invention provides the following means. [1] A method for producing a composition comprising a vinyl polymer (A) and an organic compound having a cyclic ether structure, wherein the vinyl polymer (A) is obtained by subjecting a vinyl compound (a) to a living radical polymerization reaction with an initiator which is an organic halide having at least one halogen atom in the presence of a catalyst (C). [2] The method for producing a composition according to [1], wherein the amount of the organic compound having a cyclic ether structure added is 0.5 to 5 parts by mass per 100 parts by mass of the vinyl polymer (A). [3] The method for producing the composition according to [1] or [2], wherein the catalyst (C) is a compound represented by the following formula 2: R 4 4N + (X 2 ) - ...Formula 2 (In the above formula 2, R 4 represents a linear or branched alkyl group having 1 to 10 carbon atoms, a linear or branched alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or a heteroaryl group having 5 to 10 carbon atoms. The alkyl group, aryl group, and heteroaryl group may each have a substituent, and when they have a substituent, the number of carbon atoms included in the number of carbon atoms of the substituent. 4 may be the same or different. 2 represents a halogen atom. [4] The method for producing the composition according to any one of [1] to [3], wherein the initiator is an organic iodine compound. [5] A method for producing any one of the compositions [1] to [4], comprising maintaining the composition at 50 to 300°C for 2 hours or more. [6] The method for producing the composition according to any one of [1] to [5], wherein the vinyl compound (a) comprises a vinyl compound (a1) having a (meth)acryloyloxy group. [7] A method for producing the composition according to [6], wherein the vinyl compound (a1) comprises either or both of a vinyl compound (a11) having no reactive silicon group and represented by the following formula 1, and a vinyl compound (a12) having a reactive silicon group and represented by the following formula 1: -SiR 1 3-a X a ...Formula 1 (In the above formula 1, R 1 represents a monovalent organic group having 1 to 20 carbon atoms not containing a hydrolyzable group, X represents a hydroxyl group, a halogen atom or a hydrolyzable group, and a is an integer of 1 to 3. When a is 1, two R 1 may be the same or different, and when a is 2 or 3, multiple Xs may be the same or different. [8] The method for producing the composition according to [7], comprising subjecting the vinyl compound (a11) and the vinyl compound (a12) to a living radical polymerization reaction in the presence of the catalyst (C), to the initiator, and then further adding the vinyl compound (a12) to perform a living radical polymerization reaction to obtain the vinyl polymer (A). [9] The method for producing the composition according to [7] or [8], wherein the vinyl polymer (A) has an average of 0.5 to 20.0 reactive silicon groups represented by the formula 1 per molecule.

[10] The method for producing the composition according to any one of [1] to [9], wherein the vinyl polymer (A) has a number average molecular weight of 1,000 to 300,000. Effect of the Invention

[0011] According to the method for producing a composition of the present invention, it is possible to suppress coloration over time during high-temperature storage of a composition containing a vinyl polymer obtained by living radical polymerization using an initiator that is an organic halide having a halogen atom. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] As used in the specification and claims, the following terms have the following definitions: "(Meth)acrylic acid" is a general term for acrylic acid and methacrylic acid. Similarly, for example, (meth)acrylic acid ester is a general term for acrylic acid ester and methacrylic acid ester, (meth)acrylic acid alkyl ester is a general term for acrylic acid alkyl ester and methacrylic acid alkyl ester, and (meth)acrylic acid alkoxyalkyl ester is a general term for acrylic acid alkoxyalkyl ester and methacrylic acid alkoxyalkyl ester. The number average molecular weight (hereinafter, referred to as "Mn") and weight average molecular weight (hereinafter, referred to as "Mw") of the polymer are polystyrene equivalent molecular weights obtained by GPC measurement. The molecular weight distribution is a value calculated from Mw and Mn, and is the ratio of Mw to Mn (hereinafter, referred to as "Mw / Mn"). A numerical range expressed by "to" means that the numerical values ​​before and after the "to" are the lower and upper limits of the numerical range.

[0013] The method for producing a composition according to the present embodiment is a method for producing a composition containing a vinyl polymer (A) and an organic compound having a cyclic ether structure. The vinyl polymer (A) is obtained by subjecting a vinyl compound (a) to a living radical polymerization reaction with an initiator, which is an organic halide having at least one halogen atom, in the presence of a catalyst (C).

[0014] [Method for producing vinyl polymer (A)] The vinyl polymer (A) (hereinafter, sometimes simply referred to as "polymer (A)") is produced by subjecting a vinyl compound (a) to living radical polymerization in the presence of a catalyst (C) using an organic halide having at least one halogen atom as an initiator (hereinafter, sometimes referred to as "initiator (I)"). Examples of living radical polymerization include atom transfer radical polymerization (ATRP) and reversible coordination-mediated polymerization (RCMP). Examples of atom transfer radical polymerization (ATRP) include already known manufacturing methods, such as those described in JP-A-2005-232419 and JP-A-2006-291073. Examples of reversible coordination-mediated polymerization (RCMP) include already known manufacturing methods, such as those described in JP-A-2022-75627. In this embodiment, reversible coordination-mediated polymerization (RCMP) is preferred as the living radical polymerization because it is easier to confirm the effect of suppressing coloration of the composition over time. The vinyl compound (a) preferably contains either or both of a vinyl compound having no reactive silicon group represented by the following formula 1 and a vinyl compound having a reactive silicon group represented by the following formula 1. The vinyl compound (a) is preferably a vinyl compound having a (meth)acryloyl group, more preferably a vinyl compound (a1) having a (meth)acryloyloxy group. The vinyl compound (a) is particularly preferably one or both of the vinyl compound (a11) having no reactive silicon group represented by the following formula 1 and having a (meth)acryloyloxy group and the vinyl compound (a12) having a reactive silicon group represented by the following formula 1 and having a (meth)acryloyloxy group. -SiR 1 3-a X a ...Formula 1 (In the above formula 1, R 1 represents a monovalent organic group having 1 to 20 carbon atoms not containing a hydrolyzable group, X represents a hydroxyl group, a halogen atom or a hydrolyzable group, and a is an integer of 1 to 3. When a is 1, two R 1 may be the same or different, and when a is 2 or 3, multiple Xs may be the same or different.

[0015] [Reactive silicon group] In the above formula 1, R 1Examples of the monovalent organic group having 1 to 20 carbon atoms and containing no hydrolyzable group, which is represented by the formula (1), include a hydrocarbon group, a halohydrocarbon group, and a triorganosiloxy group. Among these, an alkyl group, a cycloalkyl group, an aryl group, a 1-chloroalkyl group, and a triorganosiloxy group are preferred.

[0016] R 1 is more preferably a linear or branched alkyl group having 1 to 4 carbon atoms, a cyclohexyl group, a phenyl group, a benzyl group, a chloromethyl group, a trimethylsiloxy group, a triethylsiloxy group, or a triphenylsiloxy group. From the viewpoint of obtaining a better balance between the curability and stability of the composition, R 1 is preferably a linear or branched alkyl group having 1 to 4 carbon atoms, more preferably a methyl group or an ethyl group. 1 is preferably a chloromethyl group. From the viewpoint of easy availability, R 1 is particularly preferably a methyl group.

[0017] In the above formula 1, X represents a hydroxyl group, a halogen atom or a hydrolyzable group. Examples of hydrolyzable groups include alkoxy groups, acyloxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, sulfanyl groups, and alkenyloxy groups. Of these, X is preferably an alkoxy group from the viewpoint of mild hydrolysis and easy handling. As the alkoxy group, methoxy groups, ethoxy groups, and isopropoxy groups are preferred, and methoxy groups and ethoxy groups are more preferred. When the alkoxy group is a methoxy group or an ethoxy group, it is easy to quickly form a siloxane bond and form a crosslinked structure in the cured product, and the physical properties of the cured product tend to be good.

[0018] In the formula 1, a is an integer of 1 to 3. When a is 1, two R 1 may be the same or different, and when a is 2 or 3, multiple Xs may be the same or different. It is preferable that a is 2, as this tends to result in good curability.

[0019] Examples of the reactive silicon group represented by the formula 1 include methyldimethoxysilyl group, methyldiethoxysilyl group, ethyldimethoxysilyl group, ethyldiethoxysilyl group, methyldiisopropoxysilyl group, methoxymethyldiethoxysilyl group, methoxymethyldimethoxysilyl group, chloromethyldimethoxysilyl group, chloromethyldiethoxysilyl group, trimethoxysilyl group, triethoxysilyl group, etc. Among these, from the viewpoint of high activity and easy achievement of good curing properties, methyldimethoxysilyl group and methyldiethoxysilyl group are preferred, and methyldimethoxysilyl group is more preferred.

[0020] <Vinyl compounds (a11)> The vinyl compound (a11) is a vinyl compound having a (meth)acryloyloxy group and no reactive silicon group represented by the formula 1. The vinyl compound (a11) is preferably a (meth)acrylic acid alkyl ester having no reactive silicon group represented by the formula 1. The vinyl compound (a11) may be used alone or in combination of two or more kinds.

[0021] Examples of the vinyl compound (a11) include (meth)acrylic acid alkyl esters having a straight or branched alkyl group having 1 to 20 carbon atoms, which may have a substituent other than the reactive silicon group. More specifically, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, isodecyl (meth)acrylate, decyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, stearyl (meth)acrylate, and the like. These may be used alone or in combination of two or more. Among these, from the viewpoint of less influence on the reaction, the (meth)acrylic acid alkyl ester is preferably a (meth)acrylic acid alkyl ester having a straight or branched alkyl group having 1 to 18 carbon atoms, which may have a substituent other than the reactive silicon group, and more preferably at least one (meth)acrylic acid alkyl ester selected from methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate. In addition, when a substituent is present, the carbon number includes the carbon number of the substituent. Examples of the substituent include a glycidyl group, an aryl group, and a polyoxyalkylene group.

[0022] When the vinyl compound (a11) has a substituent, specific examples thereof include polyoxyethylene alkyl (meth)acrylate, polyoxypropylene alkyl (meth)acrylate, polyoxybutylene alkyl (meth)acrylate, and the like.

[0023] <Vinyl compounds (a12)> The vinyl compound (a12) is a compound in which at least one hydrogen atom in the vinyl compound (a11) is substituted with a reactive silicon group represented by the above formula 1. As the vinyl compound (a12), a (meth)acrylic acid alkyl ester having a reactive silicon group represented by the above formula 1 is preferred. More specifically, preferred are compounds in which at least one hydrogen atom in the alkyl group of a (meth)acrylic acid alkyl ester is substituted with a reactive silicon group represented by the above formula 1, and more preferred are compounds in which at least one hydrogen atom at the molecular terminal of the alkyl group of a (meth)acrylic acid alkyl ester is substituted with a reactive silicon group represented by the above formula 1. The vinyl compounds (a12) may be used alone or in combination of two or more.

[0024] The alkyl group in the (meth)acrylic acid alkyl ester having a reactive silicon group is preferably a linear or branched alkyl group having 1 to 8 carbon atoms, more preferably a linear or branched alkyl group having 1 to 6 carbon atoms, and particularly preferably a linear or branched propyl group having 3 carbon atoms. These alkyl groups may have a substituent other than the reactive silicon group represented by the formula 1. When the alkyl group has a substituent, the carbon number includes the carbon number of the substituent. Examples of the substituent include a glycidyl group and an aryl group. However, the carbon number does not include the carbon number of the reactive silicon group.

[0025] Examples of such (meth)acrylic acid alkyl esters include (trimethoxysilyl)methyl (meth)acrylic acid alkyl ester, 3-(methyldimethoxysilyl)propyl (meth)acrylic acid alkyl ester, 3-(trimethoxysilyl)propyl (meth)acrylic acid alkyl ester, 3-(methyldiethoxysilyl)propyl (meth)acrylic acid alkyl ester, and 3-(triethoxysilyl)propyl (meth)acrylic acid alkyl ester.

[0026] The number of reactive silicon groups represented by the above formula 1 that the vinyl compound (a12) has is preferably 1 to 6, and more preferably 1 to 4, from the viewpoint of the elongation properties of the cured product obtained by curing the composition.

[0027] When the vinyl compound (a11) and the vinyl compound (a12) are used in combination, the ratio of the vinyl compound (a12) to 100 parts by mass of the vinyl compound (a11) is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and particularly preferably 0.05 to 3 parts by mass. When the ratio of the vinyl compound (a12) is within the above range, the elongation properties of the cured product obtained by curing the composition tend to be good.

[0028] <Other monomers> Examples of the other monomer include acrylic acid and acrylamide, which are vinyl compounds other than the vinyl compound (a11) and the vinyl compound (a12) of the present embodiment. The other monomer may be used alone or in combination of two or more.

[0029] <Initiator (I)> The initiator (I) is an organic halide having at least one halogen atom. At least one halogen atom of the initiator (I) is eliminated to generate a carbon radical, and living radical polymerization is started. Therefore, "at least one halogen atom" of the initiator (I) means a halogen atom that can be eliminated from the initiator to generate a carbon radical.

[0030] Specific examples of the initiator (I) for atom transfer radical polymerization (ATRP) include the organic halides described in JP 2005-232419 A, paragraphs

[0040] to

[0064] . Examples of the initiator (I) for reversible coordination-mediated polymerization (RCMP) include the organic halides described in JP 2022-75627 A, paragraphs

[0014] to

[0021] . The halogen atom of the organic halide forms an ionic bond with the carbon atom in the initiator (I). That is, the carbon atom in the initiator (I) is in a cationic state, and the halogen atom is ionic bonded to the carbon atom as a halide ion. The halogen atom is preferably a bromine atom or an iodine atom, and more preferably an iodine atom, i.e., the initiator (I) is preferably an organic iodine compound.

[0031] Specific examples of the initiator (I) include methyl chloride, methylene chloride, chloroform, chloroethane, dichloroethane, trichloroethane, bromomethyl, dibromomethane, bromoform, bromoethane, dibromoethane, tribromoethane, tetrabromoethane, bromotrichloromethane, dichlorodibromomethane, chlorotribromomethane, iodotrichloromethane, dichlorodiiodomethane, iodotribromomethane, dibromodiodomethane, bromotriiodomethane, iodoform, diiodomethane, and methyl iodide. , isopropyl chloride, t-butyl chloride, isopropyl bromide, t-butyl bromide, triiodoethane, ethyl iodide, diiodopropane, isopropyl iodide, t-butyl iodide, bromodichloroethane, chlorodibromoethane, bromochloroethane, iododichloroethane, chlorodiiodoethane, diiodopropane, chloroiodopropane, iododibromoethane, bromoiodopropane, 2-iodo-2-polyethyleneglycosylpropane, 2-iodo-2-amidinopropane, 2-iodo-2-cyanobutane, 2 -Iodo-2-cyano-4-methylpentane, 2-iodo-2-cyano-4-methyl-4-methoxypentane, 4-iodo-4-cyano-pentanoic acid, methyl-2-iodoisobutyrate, 2-iodo-2-methylpropanamide, 2-iodo-2,4-dimethylpentane, 2-iodo-2-cyanobutanol, cyano-4-methylpentane, 2-iodo-2-methyl-N-(2-hydroxyethyl)propionamide-4-methylpentane, 2-iodo-2-methyl-N-(1,1-bis(hydroxymethyl)-2-hydroxypentane, hydroxyethyl)propionamide 4-methylpentane, 2-iodo-2-(2-imidazolin-2-yl)propane, 2-iodo-2-(2-(5-methyl-2-imidazolin-2-yl)propane, ethyl-2-iodopropionate, ethyl-2-iodo-2-methylpropionate, ethylene glycol bis(2-iodoisobutyrate), 1,4-diiodooctafluorobutane, diethyl 2,5-diiodoadipate, 2-iodoisobutyronitrile, 2-iodoisopentanitrile, 2-iodo-2,Examples of the iodoisobutyronitrile include 4-dimethylpentanitrile, fluoroiodomethane, difluoroiodomethane, trifluoroiodomethane, iodopentafluoroethane, heptafluoro-1-iodopropane, heptafluoro-2-iodopropane, 1-iodoperfluorobutane, 2-iodononafluorobutane, 1-iodoperfluorohexane, 2-iodoperfluorohexane, 3-iodoperfluorohexane, and diethyl 2,5-dibromoadipate. 2-iodoisobutyronitrile, 2-iodoisopentanitrile, 2-iodo-2,4-dimethylpentanitrile, ethyl 2-iodopropionate, ethyl 2-iodo-2-methylpropionate, 1-iodoperfluorobutane, 1-iodoperfluorohexane, and diethyl 2,5-dibromoadipate are preferred, and 1-iodoperfluorobutane is more preferred.

[0032] <Catalyst (C)> Examples of the catalyst (C) for atom transfer radical polymerization (ATRP) include transition metal complexes. The transition metal complex is not particularly limited, but is preferably a metal complex having a central metal of an element of Group 7, 8, 9, 10, or 11 of the long periodic table. More preferred examples include complexes having zero-valent copper, monovalent copper, divalent ruthenium, divalent iron, or divalent nickel as a central metal. Among these, copper complexes are preferred. Copper complexes can be obtained by mixing a copper compound with a ligand. Examples of monovalent copper compounds include cuprous chloride, cuprous bromide, cuprous iodide, cuprous cyanide, cuprous oxide, and cuprous perchlorate. When a copper compound is used, it is preferable to add 2,2'-bipyridyl or a derivative thereof, 1,10-phenanthroline or a derivative thereof, or a polyamine such as tetramethylethylenediamine, pentamethyldiethylenetriamine, or hexamethyltris(2-aminoethyl)amine as a ligand in order to enhance catalytic activity. In addition, a tristriphenylphosphine complex of divalent ruthenium chloride (RuCl2(PPh3)3) is also suitable as a catalyst. When a ruthenium compound is used as a catalyst, an aluminum alkoxide is added as an activator. In addition, a bistriphenylphosphine complex of divalent iron (FeCl2(PPh3)2), a bistriphenylphosphine complex of divalent nickel (NiCl2(PPh3)2), and a bistributylphosphine complex of divalent nickel (NiBr2(PBu3)2) are also suitable as catalysts. Examples of the catalyst (C) for reversible coordination-mediated polymerization (RCMP) include organic catalysts, such as those described in paragraph

[0022] of JP-A-2022-75627. Since a purification step for removing the transition metal complex is not required when producing the polymer (A), an organic catalyst for reversible coordination-mediated polymerization (RCMP) is preferred.

[0033] The catalyst (C) for the reversible coordination-mediated polymerization (RCMP) is more preferably a compound represented by the following formula 2. R 4 4N + (X 2 ) - formula 2 (In the above formula 2, R 4represents a linear or branched alkyl group having 1 to 10 carbon atoms, a linear or branched alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or a heteroaryl group having 5 to 10 carbon atoms. The above alkyl group, aryl group, and heteroaryl group may each have a substituent, and when they have a substituent, the number of carbon atoms included in the number of carbon atoms of the substituent is included in the number of carbon atoms of the substituent. 4 may be the same or different. 2 represents a halogen atom.

[0034] In the above formula 2, four R 4 each independently may have a substituent; R 4 is preferably a linear or branched alkyl group having 1 to 10 carbon atoms, and more preferably a linear or branched alkyl group having 2 to 6 carbon atoms. 2 is preferably the same as the halogen atom of the initiator (I). 2 However, an iodine atom is more preferable for both.

[0035] Among the compounds represented by the above formula 2, quaternary ammonium iodide salts are preferred, and compounds represented by the following formula 3 are more preferred. R 5 4N + I - formula 3 (In the above formula 3, R 5 is an alkyl group having 1 to 8 carbon atoms, and four R 5 may be the same or different.)

[0036] The catalyst (C) preferably contains one or more selected from the group consisting of tetramethylammonium iodide, tetrabutylammonium iodide, and tetraoctylammonium iodide, and more preferably contains tetrabutylammonium iodide. When the catalyst (C) contains the above compound, it is easy to control the polymer structure.

[0037] The amount of the catalyst (C) is preferably 0.1 to 50 parts by mass, more preferably 1 to 40 parts by mass, based on 100 parts by mass of the content of the initiator (I). When the amount of the catalyst (C) is within the above range, it is easy to control the Mw / Mn of the polymer (A).

[0038] The amount of the catalyst (C) is preferably 0.1 to 5.0 parts by mass per 100 parts by mass of the total of the vinyl compounds (a). When the amount of the catalyst (C) is within the above range, the molecular weight of the polymer can be easily adjusted to the desired range.

[0039] <Other ingredients> In the method for producing the polymer (A), components other than the vinyl compound (a), the initiator (I) and the catalyst (C) may be added to the reaction system within the range that does not impair the effects of the present invention. Examples of the other components include a reaction regulator and a solvent. These other components may be used alone or in combination of two or more, as necessary.

[0040] Examples of the reaction inhibitor include iodine and tetrabutylammonium triiodide. When using such a reaction inhibitor, it is preferable to add it to the reaction system at the start of polymerization. The amount of the reaction inhibitor is preferably 0.5 to 5 moles per 10,000 moles of the vinyl compound (a). As the solvent, any solvent conventionally used in living radical polymerization can be used without any particular limitation.

[0041] <Production conditions of polymer (A)> Examples of atom transfer radical polymerization (ATRP) include the method described in JP 2005-232419 A. Among them, a preferred method is to use an organic halide (e.g., a sulfonyl halide compound) as an initiator and a transition metal complex such as copper bromide-pentamethyldiethylenetriamine complex as a catalyst to polymerize a vinyl compound (a) to obtain a vinyl polymer having a terminal halogen, react the vinyl polymer with a compound having at least two alkenyl groups with low polymerizability (hereinafter, also referred to as a diene compound) to obtain a vinyl polymer having an alkenyl group at the terminal, and hydrosilylate the vinyl polymer using a silylating agent in the presence of a hydrosilylation catalyst.

[0042] In atom transfer radical polymerization (ATRP), vinyl compound (a11) and vinyl compound (a12) can be added at the start of polymerization or during polymerization, or both. For example, the vinyl compound (a11) is polymerized, and then vinyl compound (a12) is added to polymerize, the vinyl compound (a12) is polymerized, and then vinyl compound (a11) is added to polymerize, the vinyl compound (a11) and vinyl compound (a12) are polymerized, and then vinyl compound (a11) is added to polymerize, the vinyl compound (a11) and vinyl compound (a12) are polymerized, and then vinyl compound (a12) is added to polymerize, the vinyl compound (a11) and vinyl compound (a12) are polymerized, and then vinyl compound (a12) is added to polymerize, the vinyl compound (a11) and vinyl compound (a12) are polymerized, the vinyl compound (a11) is polymerized, and then vinyl compound (a11) and vinyl compound (a12) are polymerized, the vinyl compound (a11) is polymerized, and then vinyl compound (a12) is added to polymerize, the vinyl compound (a12) is polymerized, and then vinyl compound (a11) and vinyl compound (a12) are polymerized, and ... In addition, a method of polymerizing only the vinyl compound (a12) without using the vinyl compound (a11) or a method of polymerizing only the vinyl compound (a11) without using the vinyl compound (a12) may be used. In atom transfer radical polymerization (ATRP), a method of polymerizing only the vinyl compound (a11) without using the vinyl compound (a12) is preferred.

[0043] Examples of the diene compound include a diene compound having a double bond only at the molecular terminal and a diene compound having a double bond both at the molecular terminal and within the molecule, with a diene compound having a double bond only at the molecular terminal being preferred.

[0044] As the diene compound having a double bond only at the molecular terminal, a diene compound represented by the following formula 4 is preferred. CH2=C(R 2 )-R 3 -C(R 2 )=CH2 formula 4 In the above formula 4, R 2 is hydrogen or a monovalent organic group having 1 to 20 carbon atoms; R 3 is a single bond or a divalent organic group having 1 to 20 carbon atoms, and R 2 and R 3 may be bonded to each other to form a cyclic structure. 2 may be the same or different. 2 is preferably a hydrogen atom or a methyl group. 3 is preferably a single bond or an alkylene group having 1 to 20 carbon atoms.

[0045] As the diene compound having a double bond at the molecular end and within the molecule, a diene compound represented by the following formula 5 is preferred. CH2=C(R 2 )-R 3 -C(R 2 )=C(R 2 )-R 6 formula 5 In the above formula 5, R 2 is hydrogen or a monovalent organic group having 1 to 20 carbon atoms; R 3 is a single bond or a divalent organic group having 1 to 20 carbon atoms, and R 6 is a monovalent organic group having 1 to 20 carbon atoms, R 2 and R 3 may be bonded to each other to form a cyclic structure. 2 may be the same or different. 2 is preferably a hydrogen atom or a methyl group. 3 is preferably a single bond or an alkylene group having 1 to 20 carbon atoms. 6 is preferably an alkyl group having 1 to 20 carbon atoms.

[0046] Specific examples of the diene compound include isoprene, piperylene, butadiene, myrcene, 1,5-hexadiene, 1,7-octadiene, 1,9-decadiene, and 4-vinyl-1-cyclohexene, with 1,5-hexadiene, 1,7-octadiene, and 1,9-decadiene being preferred.

[0047] There is no particular limitation on the hydrosilylation catalyst, and any may be used. Specific examples include chloroplatinic acid; platinum alone; solid platinum supported on a support such as alumina, silica, or carbon black; platinum-vinylsiloxane complexes {e.g., Pt n (ViMe2SiOSiMe2Vi) n , Pt〔(MeViSiO)4〕 m}; platinum-phosphine complexes {e.g., Pt(PPh3)4, Pt(PBu3)4}; platinum-phosphite complexes {e.g., Pt[P(OPh)3]4, Pt[P(OBu)3]4} (wherein Me represents a methyl group, Bu represents a butyl group, Vi represents a vinyl group, Ph represents a phenyl group, and n and m represent integers); complexes of chloroplatinic acid with alcohols, aldehydes, ketones, etc.; platinum-olefin complexes (e.g., Pt(CH2=CH2)2(PPh 3)2, Pt(CH2=CH2)2Cl2; Pt(acac)2 (wherein acac represents acetylacetonate); dicarbonyldichloroplatinum; Karstedt's catalyst; platinum-hydrocarbon complexes described in U.S. Pat. Nos. 3,159,601 and 3,159,662 to Ashby et al.; platinum alcoholate catalysts described in U.S. Pat. No. 3,220,972 to Lamoreaux et al., and the like. Furthermore, platinum chloride-olefin complexes described in U.S. Pat. No. 3,516,946 to Modic are also useful in this embodiment. Examples of catalysts other than platinum compounds include RhCl(PPh3)3, RhCl3, Rh / Al2O3, RuCl3, IrCl3, FeCl3, AlCl3, PdCl2·2H2O, NiCl2, TiCl4, and the like. These catalysts may be used alone or in combination of two or more. From the viewpoint of catalytic activity, chloroplatinic acid, platinum-olefin complexes, platinum-vinylsiloxane complexes, Pt(acac)2, and the like are preferred.

[0048] <Silylating agent> The silylating agent is a compound having both a group capable of reacting with an unsaturated group to form a bond (e.g., a sulfanyl group) and a reactive silicon group represented by the above formula 1, a hydrosilane compound (e.g., HSiR a X 3-a The definitions of R, X, and a are the same as those in formula 1.

[0049] Specific examples of the silylating agent include trimethoxysilane, triethoxysilane, triisopropoxysilane, tris(2-propenyloxy)silane, triacetoxysilane, dimethoxymethylsilane, diethoxymethylsilane, dimethoxyethylsilane, diethoxyethylsilane, diisopropoxymethylsilane, (α-chloromethyl)dimethoxysilane, and (α-chloromethyl)diethoxysilane. In terms of high activity and good curing properties, trimethoxysilane, triethoxysilane, dimethoxymethylsilane, and diethoxymethylsilane are preferred, and dimethoxymethylsilane or trimethoxysilane is more preferred.

[0050] In reversible coordination mediated polymerization (RCMP), vinyl compound (a11) and vinyl compound (a12) can be added at the start of polymerization or during polymerization, or both. For example, a method of polymerizing vinyl compound (a11) and then adding vinyl compound (a12) to polymerize, a method of polymerizing vinyl compound (a12) and then adding vinyl compound (a11) to polymerize, a method of polymerizing vinyl compound (a11) and vinyl compound (a12) and then adding vinyl compound (a11) to polymerize, a method of polymerizing vinyl compound (a11) and vinyl compound (a12) and then adding vinyl compound (a12) to polymerize, a method of polymerizing vinyl compound (a11) and vinyl compound (a12), a method of polymerizing vinyl compound (a11) and vinyl compound (a12) and then adding vinyl compound (a11) to polymerize, a method of polymerizing vinyl compound (a11) and vinyl compound (a12), a method of polymerizing vinyl compound (a11) and vinyl compound (a12) and then adding vinyl compound (a11) and vinyl compound (a12) to polymerize, a method of polymerizing vinyl compound (a12) and then adding vinyl compound (a11) and vinyl compound (a12) to polymerize, and a method of polymerizing vinyl compound (a12) and then adding vinyl compound (a11) and vinyl compound (a12) to polymerize. It is also possible to use a method in which only the vinyl compound (a12) is polymerized without using the vinyl compound (a11), or a method in which only the vinyl compound (a11) is polymerized without using the vinyl compound (a12).

[0051] In the reversible coordination mediated polymerization (RCMP), it is preferable to polymerize the vinyl compound (a11) and the vinyl compound (a12) and then add the vinyl compound (a12). That is, it is preferable to carry out a living radical polymerization reaction of the vinyl compound (a11) and the vinyl compound (a12) with the initiator (I) in the presence of the catalyst (C) (step (i)), and then to add the vinyl compound (a12) and carry out a living radical polymerization reaction (step (ii)) to obtain the polymer (A). This allows reactive silicon groups to be introduced at intervals into the polymer (A), and when the polymer is cured, it is possible to obtain better elongation properties.

[0052] When the vinyl compound (a12) is added to the reaction system in two separate portions, the first addition is preferably at the start of the reaction, which allows a sufficient distance to be obtained between the site where the vinyl compound (a12) added in the first portion is introduced and the site where the vinyl compound (a12) added in the second portion is introduced.

[0053] When the vinyl compound (a12) is added to the reaction system in two portions, the timing of the second addition is preferably when the total reaction rate of the vinyl compound (a11) and the vinyl compound (a12) reaches 30 to 90 mol%, more preferably when it reaches 40 to 85 mol%, and particularly preferably when it reaches 50 to 80 mol%.

[0054] By adding the vinyl compound (a11) for the second time when the total reaction rate of the vinyl compound (a12) reaches or exceeds the lower limit, a sufficient distance can be obtained between the site where the vinyl compound (a12) added for the first time is introduced and the site where the vinyl compound (a12) added for the second time is introduced. By adding the vinyl compound (a12) for the second time when the total reaction rate of the vinyl compound (a11) and the vinyl compound (a12) reaches the upper limit value or less, the vinyl compound (a12) added for the second time can be sufficiently reacted.

[0055] The reaction rate is 1This refers to a value calculated using H-NMR by applying the peak area value corresponding to the monomer and the peak area value corresponding to the polymer to the following formula f1. Conversion rate = (polymer peak area) / ((sum of monomer peak areas)+(polymer peak area))×100 Formula f1

[0056] The total reaction rate of the vinyl compound (a11) and the vinyl compound (a12) means a reaction rate calculated from the total peak area of ​​the vinyl compound (a11) and the vinyl compound (a12). In the method for producing the vinyl polymer (A), "((total peak area of ​​monomers)+(peak area of ​​polymer))" in formula f1 corresponds to the total peak area of ​​vinyl compound (a11) and vinyl compound (a12) at the start of polymerization. However, after the second addition, "((total peak area of ​​monomers)+(peak area of ​​polymer))" in formula f1 becomes "(total peak area of ​​monomers)+(peak area of ​​polymer)". Furthermore, "((sum of peak areas of monomers))" in formula f1 at a certain point in time during the reaction corresponds to the sum of the peak area of ​​the vinyl compound (a11) and the peak area of ​​the vinyl compound (a12) remaining at that point in time.

[0057] The vinyl compound (a12) added in step (i) and step (ii) may be the same or different. It is preferable that the vinyl compound (a12) added in step (i) (the vinyl compound (a12) added to the reaction system at the start of polymerization) is the same as the vinyl compound (a12) added in step (ii) (the vinyl compound (a12) added to the reaction system during polymerization). The amount of vinyl compound (a11) added in step (i) is preferably 10 to 1000 molar equivalents, more preferably 50 to 500 molar equivalents, relative to 1 mole of initiator (I). The amount of vinyl compound (a12) added is preferably 0.1 to 10 molar equivalents, more preferably 0.3 to 8 molar equivalents, relative to 1 mole of initiator (I). When two or more monomers are used as vinyl compound (a11), the molar equivalent value is the total amount of two or more vinyl compounds (a11). When two or more vinyl compounds (a12) are used as vinyl compound (a12), the molar equivalent value is the total amount of two or more vinyl compounds (a12), similar to vinyl compound (a11). If the amounts of vinyl compound (a11) and vinyl compound (a12) added are within the above ranges, the elongation properties of the cured product when made into a curable composition are easily expressed.

[0058] The polymerization temperature in the step (i) is preferably 100 to 150° C., more preferably 110 to 140° C., from the viewpoint of easy control of the polymerization reaction rate and molecular weight distribution. The polymerization time in the step (i) is not particularly limited as long as it is a time until the total reaction rate of the vinyl compound (a11) and the vinyl compound (a12) reaches 30 to 90 mol%.

[0059] The amount of the vinyl compound (a12) added in the step (ii) is preferably from 0.1 to 10 molar equivalents, more preferably from 0.3 to 8 molar equivalents, relative to 1 mole of the initiator (I). Similarly to step (i), the polymerization temperature in step (ii) is preferably 100 to 150° C., more preferably 110 to 140° C., from the viewpoint of easy control of the polymerization reaction rate and molecular weight distribution. The polymerization time in step (ii) is appropriately adjusted depending on the reaction rates of all the monomers introduced in steps (i) and (ii). It is usually the time until the reaction rate reaches 90 mol% or more.

[0060] Polymer (A) is obtained by polymerizing vinyl compound (a). When a solvent is contained in addition to polymer (A), polymer (A) is obtained by removing the solvent contained in the solution under reduced pressure. The solution containing polymer (A) may be purified before removing the solvent contained in the solution under reduced pressure. As a purification method, a method of washing the solution containing the obtained polymer (A) with a purification solvent can be mentioned. As the purification solvent, methanol, ethanol, and isopropanol can be mentioned because they are easily removed in the subsequent decompression step. After purification, the solution containing the polymer (A) is preferably dried under reduced pressure of -101.3 to -95 kPa at 70 to 95° C. for 1 to 4 hours. Through these steps, the polymer (A) can be obtained. In the case of reversible coordination-mediated polymerization (RCMP), a method can also be selected in which a vinyl polymer is obtained, and then the diene compound is reacted therewith, followed by hydrosilylation using a silylating agent in the presence of a hydrosilylation catalyst.

[0061] The Mn of the polymer (A) is preferably 1,000 or more, more preferably 5,000 or more, further preferably 6,000 or more, and particularly preferably 10,000 or more. The Mn of the polymer (A) is preferably 300,000 or less, more preferably 100,000 or less, further preferably 60,000 or less, and particularly preferably 40,000 or less. When the Mn of the polymer (A) is within the above range, the workability of the curable composition tends to be good.

[0062] The Mw / Mn of the polymer (A) is preferably from 1.0 to 3.0, more preferably from 1.3 to 2.4. The polymer (A) obtained by the above production method tends to be characterized by a narrow molecular weight distribution and a small amount of low molecular weight components.

[0063] The average number of reactive silicon groups represented by the formula 1 in the polymer (A) per molecule is preferably 0.5 or more, more preferably 0.8 or more, even more preferably 0.9 or more, and particularly preferably 1.0 or more. The average number of reactive silicon groups represented by the formula 1 in the polymer (A) per molecule is preferably 20.0 or less, more preferably 8.0 or less, and particularly preferably 6.0 or less.

[0064] In atom transfer radical polymerization (ATRP), the average number of reactive silicon groups per molecule in the polymer can be controlled by adjusting the type and amount of vinyl compound having a reactive silicon group and the type and amount of silylating agent. In atom transfer radical polymerization (ATRP), it is preferable to control the average number of reactive silicon groups per molecule in the polymer by adjusting the type and amount of silylating agent without using a vinyl compound having a reactive silicon group. In reversible coordination mediated polymerization (RCMP), the average number of reactive silicon groups per molecule in the polymer can be controlled by adjusting the type and amount of vinyl compound having reactive silicon group and the type and amount of silylating agent. In reversible coordination mediated polymerization (RCMP), it is preferable to control the average number of reactive silicon groups per molecule in the polymer by adjusting the type and amount of vinyl compound having reactive silicon group without using silylating agent.

[0065] <Organic compounds having a cyclic ether structure> The organic compound having a cyclic ether structure of this embodiment (hereinafter also referred to as "compound (B)") is not particularly limited, but is preferably an organic compound having a cyclic ether structure in which the hydrocarbon constituting the ring has 3 to 6 carbon atoms, more preferably an organic compound having a cyclic ether structure in which the hydrocarbon has 3 carbon atoms, and particularly preferably an epoxy compound. Examples of epoxy compounds include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxycyclohexylmethyl (meth)acrylate, methyl glycidyl ether, ethyl glycidyl ether, propyl glycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, glycidol, ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, triethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, dipropylene glycol diglycidyl ether, and tripropylene glycol. diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, bisphenol A diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, 3,4-epoxycyclohexenylmethyl-3',4'-epoxycyclohexene carboxylate, 1,2-epoxy-4-vinylcyclohexane, 1,2:8,9 diepoxy limonene, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl triethoxysilane, γ-glycidoxypropyl methyl dimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl triethoxysilane.

[0066] When the compound (B) is an epoxy compound, the epoxy group is preferably a glycidyl group, for example, 2-ethylhexyl glycidyl ether, from the viewpoint of suppressing coloration of the composition over time. The compound (B) may be used alone or in combination of two or more kinds.

[0067] <Method of adding compound (B)> There is no limitation on the timing of adding the compound (B), and the compound (B) can be added at any time before the start of the polymerization process of the polymer (A), during the polymerization process, or after the completion of the polymerization process.

[0068] The amount of compound (B) added is preferably 0.5 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, and even more preferably 0.9 to 3 parts by mass, based on 100 parts by mass of polymer (A). When the amount of compound (B) added is equal to or greater than the lower limit, the effect of inhibiting coloration over time is more easily obtained. When the amount of compound (B) added is equal to or less than the upper limit, the viscosity of the composition is less likely to increase. From the viewpoint of more easily obtaining the effect of inhibiting coloration of the composition over time, the composition containing the vinyl polymer (A) and the compound (B) is preferably kept at 50 to 300° C., and more preferably kept at 80 to 250° C. The keeping time is preferably 2 hours or more, more preferably 2 to 6 hours, and even more preferably 2 to 4 hours.

[0069] <Composition> The composition of the present embodiment is considered to contain a polymer (A), a compound (B), a halogen ion, a reaction product of the halogen ion and the compound (B), a catalyst (C), and an unreacted initiator (I). The polymer (A) includes not only the polymer obtained by the above-mentioned production method, but also a polymer produced by elimination of a halogen ion derived from the initiator (I) unit in the polymer.

[0070] <Mechanism of action> The coloring of a composition containing polymer (A) over time during storage at high temperature is believed to be due to halogen ions contained in the composition. The halogen ions are believed to originate from the initiator (I) units in polymer (A), from unreacted initiator (I), or from catalyst (C). According to the studies of the inventors of the present application, it is believed that the halogen ions are most likely to originate from the initiator (I) units in polymer (A). The composition of the present embodiment contains compound (B). It is believed that the cyclic ether structure in compound (B) reacts with the halogen ions, causing compound (B) to trap the halogen ions, thereby reducing the halogen ions in the composition and suppressing coloration over time.

[0071] <Curable composition> The composition of the present embodiment can be used as a curable composition. The composition of the present embodiment may contain other optional components. Examples of other optional components include polymers other than the polymer (A), curing catalysts (silanol condensation catalysts), curable compounds, fillers, plasticizers, thixotropy-imparting agents, stabilizers (antioxidants, light stabilizers, ultraviolet absorbers, etc.), adhesion-imparting agents, physical property adjusters, tackifying resins, reinforcing materials such as fillers, surface modifiers, flame retardants, foaming agents, solvents, and silicates.

[0072] The cured product obtained from the curable composition can be suitably used in fields where weather resistance is required, such as for sealants (e.g., elastic sealants for construction, sealants for insulating glass, anti-rust and waterproof sealants for glass edges, sealants for the backside of solar cells, sealants for buildings, sealants for ships, sealants for automobiles, and sealants for roads), electrical insulating materials (insulating coating materials for electric wires and cables), and as a raw material for adhesives. EXAMPLES

[0073] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. In the examples, Examples 1 to 8 are working examples, and Examples 9 and 10 are comparative examples.

[0074] <Measurement method etc.> [Mn and Mw] In the following examples, Mn and Mw are polystyrene-equivalent molecular weights obtained by measuring by gel permeation chromatography (GPC) under the following conditions.

[0075] (GPC measurement conditions) Model used: HLC-8220GPC (Tosoh Corporation) Data processing device: SC-8020 (Tosoh Corporation) Columns used: Two TSKgel SuperHZ 4000 columns (manufactured by Tosoh Corporation) and two TSKgel SuperHZ 2500 columns (manufactured by Tosoh Corporation) were connected in series. Column temperature: 40℃ Detector: RI Solvent: Tetrahydrofuran Flow rate: 0.35ml / min Sample concentration: 0.5% by mass Sample injection volume: 20 μl Standard sample for creating calibration curve: Polystyrene "EasiCal(R) PS-2", manufactured by Agilent Technologies, Inc.

[0076] [Polymer viscosity] 1 mL of the sample was taken and the viscosity was measured using an E-type viscometer (Toki Sangyo Co., Ltd. product name: RE80 type) under rotor No. 4 conditions. JS14000 (Japan Grease Co., Ltd. product name) was used as the calibration standard liquid. The measurement temperature was 25±2°C.

[0077] [Polymer reaction rate] The reaction rate of the polymer is calculated by the following conditions: 1 The peak area was measured by 1 H-NMR and calculated from the sum of the peak areas of the monomers and the peak area of ​​the polymer according to the above formula f1.

[0078] ( 1 H-NMR measurement conditions) Model used: JNM-ECZ400S FT-NMR (JEOL) Deuterated solvent: deuterated chloroform Measured polymer concentration: Approximately 1 to 10% by mass Number of times: 8

[0079] [Measurement of the average number of reactive silicon groups per polymer molecule] 1 The concentration (mol / g) of reactive silicon groups in the polymer was measured using 1 H-NMR, and the average number of reactive silicon groups per polymer molecule was calculated as follows. Average number of reactive silicon groups per polymer molecule = (concentration of reactive silicon groups in polymer (mol / g)) x (number average molecular weight of polymer (Mn))

[0080] [Number of polymer colors] A composition containing polymer (A) was filled into a 10 mm plastic cell CM-A131 (Konica Minolta, Inc.) up to the upper scale line, and allowed to stand in a thermostatic chamber at 80° C. for 30 minutes. After that, it was allowed to stand until it reached room temperature, and then the film on the plastic cell was peeled off and it was set in a color / turbidity simultaneous measuring instrument COH-400 (Nippon Denshoku Industries Co., Ltd.) to measure the Gardner color number (hereinafter referred to as "initial (Gardner color number)"). 30 g of the composition containing polymer (A) was weighed into a 50 mL glass bottle, and left to stand for one week in a thermostatic bath at 110° C. without replacing the gas phase with nitrogen and without covering the bottle. After removing it from the thermostatic bath and leaving it to stand until it reaches room temperature, a 10 mm plastic cell CM-A131 was filled with the composition containing polymer (A) up to the upper scale line, and left to stand in a thermostatic bath at 80° C. for 30 minutes. After leaving it to stand until it reaches room temperature, the film on the plastic cell was peeled off, and it was set in a color / turbidity simultaneous measuring instrument COH-400, and the Gardner color number was measured (hereinafter referred to as "after accelerated test (Gardner color number)"). The evaluation was based on the following criteria. ○: (After accelerated testing (Gardner color scale)) - (Initial (Gardner color scale)) value is less than 3 △: (After accelerated testing (Gardner color scale)) - (Initial (Gardner color scale)) value is 3 or more and less than 5 ×: (After accelerated test (Gardner color scale)) - (Initial (Gardner color scale)) value is 5 or more

[0081] [Synthesis Example 1: Synthesis of Polymer (A1)] In a 2L flask equipped with a reflux tube, a stirrer, and a thermometer, 800g of butyl acrylate (hereinafter referred to as "BA"), 100g of lauryl acrylate (hereinafter referred to as "LA"), and 100g of stearyl acrylate (hereinafter referred to as "StA") were charged. Then, 27g of 1-iodononafluorobutane (hereinafter referred to as "C4F9I"), 10.4g of 3-methacryloxypropylmethyldimethoxysilane (hereinafter referred to as "MPDMS"), and 10.5g of tetrabutylammonium iodide (hereinafter referred to as "BNI") were charged. Next, after replacing the atmosphere in the flask with nitrogen, the reaction system was stirred and polymerized for 6 hours at an internal temperature of 130°C. The reaction rate after 6 hours from the start of polymerization was 72 mol%. Next, 10.4g of MPDMS was added, and polymerization was further carried out at 130°C for 4 hours. The reaction rate of the obtained polymer was 91 mol%. Next, a solution prepared by dissolving 6.2 g of 2,2'-azobis-2-methylbutyronitrile (product name: "V-59", Fujifilm Wako Pure Chemical Industries, Ltd.) in 12.5 g of butyl acetate was added dropwise to the polymer solution over 2 hours. The reaction rate of the polymer obtained after the dropwise addition was 99 mol%. Thereafter, the solution was dried under reduced pressure at a vacuum degree of 0.3 kPa and 130°C for 2 hours to obtain a solution containing polymer (A1).

[0082] The Mn of the obtained polymer (A1) was 15,500, the Mw / Mn was 2.26, and the average number of reactive silicon groups per molecule was 1.4. The viscosity of the polymer (A) after polymerization was measured and found to be 64 Pa s at 25°C.

[0083] [Synthesis Example 2: Synthesis of Polymer (A2)] A 2L flask equipped with a reflux condenser, a stirrer, and a thermometer was charged with 8.4g of CuBr, and the inside of the reaction vessel was replaced with nitrogen. Next, 88g of acetonitrile was added, and the mixture was stirred in an oil bath at 70°C for 30 minutes. 160g of BA, 20g of LA, 20g of StA, 17.6g of diethyl 2,5-dibromoadipate, and 0.34g of pentamethyldiethylenetriamine (hereinafter referred to as "PMEDTA") were added to the mixture to start the reaction. 640g of BA, 80g of LA, 80g of StA, and 1.16g of PMEDTA were continuously added while heating and stirring at 70°C. When the monomer reaction rate reached 96mol%, the remaining monomer and acetonitrile were degassed at 70°C. 107g of 1,7-octadiene was added to the obtained polymer, 264g of acetonitrile was further added, 3.4g of PMEDTA was added, and the mixture was heated and stirred at 70°C. After 10 hours, the reaction mixture was heated and degassed at 70°C to remove the residual monomer and acetonitrile. The mixture was diluted with 1000g of toluene and passed through a column packed with 1000g of activated alumina to remove the polymerization catalyst. The polymer solution was concentrated, and the polymer was dissolved in 1000g of methylcyclohexane, to which 10g of Kyoward 500SH and 10g of Kyoward 700SEN-S (both manufactured by Kyowa Chemical Industry Co., Ltd.) were added. The mixture was heated and stirred in an oxygen / nitrogen mixed gas atmosphere with an oxygen concentration of 6% by volume, and insoluble solids were removed by filtering. Thereafter, the mixture was heated and degassed at 180°C for 6 hours (vacuum pressure: 0.3 KPa), and then 2.6 g of dimethoxymethylsilane, 0.86 g of methyl orthoformate, 0.04 g of a xylene solution of [bis(1,3-divinyl-1,1,3,3-tetramethyldisiloxane)] platinum complex catalyst (hereinafter referred to as "platinum catalyst") (10 mg of platinum per kg of polymer) was mixed with the polymer, and the mixture was heated and stirred at 80°C for 1 hour under a nitrogen atmosphere to obtain a solution containing polymer (A2).

[0084] The Mn of the obtained polymer (A2) was 26,600, the Mw / Mn was 1.67, and the average number of reactive silicon groups per molecule was 1.6. The viscosity of the purified polymer (A2) was measured and found to be 161 Pa s at 25°C.

[0085] (Example 1) 10 g of 2-ethylhexyl glycidyl ether (represented as "2EHGE" in Table 1), which is compound (B), was added to the solution containing polymer (A1), and the mixture was heated and stirred at 90° C. for 2 hours. The amount of 2-ethylhexyl glycidyl ether added was 0.95 parts by mass relative to 100 parts by mass of polymer (A1).

[0086] (Examples 2 to 5) The same operation as in Example 1 was carried out, except that the temperature after the addition of 10 g of 2-ethylhexyl glycidyl ether as compound (B) was set to the temperature shown in Table 1.

[0087] (Example 6) In Synthesis Example 1, 10 g of 2-ethylhexyl glycidyl ether, which is the compound (B), was added before the start of polymerization, and polymerization was initiated. After the polymerization was completed, the mixture was heated and stirred for 2 hours at 130° C. The amount of 2-ethylhexyl glycidyl ether added was 0.95 parts by mass relative to 100 parts by mass of the polymer (A1).

[0088] (Example 7) In Synthesis Example 1, after polymerization for 6 hours at an internal temperature of 130° C., MPDMS was added, and before polymerization for a further 4 hours at 130° C., 10 g of 2-ethylhexyl glycidyl ether, which is compound (B), was added, and after polymerization was completed, the mixture was heated and stirred for 2 hours at 130° C. The amount of 2-ethylhexyl glycidyl ether added was 0.95 parts by mass relative to 100 parts by mass of polymer (A1).

[0089] (Example 8) 10 g of 2-ethylhexyl glycidyl ether, which is compound (B), was added to the solution containing polymer (A2), and the mixture was heated and stirred for 2 hours at 130° C. The amount of 2-ethylhexyl glycidyl ether added was 0.95 parts by mass relative to 100 parts by mass of polymer (A2).

[0090] (Example 9) No compound (B), 2-ethylhexyl glycidyl ether, was added to the solution containing polymer (A1).

[0091] (Example 10) No compound (B), 2-ethylhexyl glycidyl ether, was added to the solution containing polymer (A2).

[0092] In Table 1, the evaluation was performed according to the above evaluation criteria.

[0093] [Table 1]

[0094] As shown in Table 1, the compositions obtained in the Examples all suppressed the increase in coloration during the accelerated test.

Claims

1. A method for producing a composition containing a vinyl polymer (A) and an organic compound having a cyclic ether structure, comprising the steps of: The vinyl polymer (A) is obtained by subjecting a vinyl compound (a) to a living radical polymerization reaction with an initiator which is an organic halide having at least one halogen atom in the presence of a catalyst (C).

2. The method for producing a composition according to claim 1, wherein the amount of the organic compound having a cyclic ether structure added is 0.5 to 5 parts by mass per 100 parts by mass of the vinyl polymer (A).

3. The method for producing a composition according to claim 1 or 2, wherein the catalyst (C) is a compound represented by the following formula 2: R 4 4 N + (X 2 ) - ・・・Formula 2 (In the above formula 2, R 4 represents a linear or branched alkyl group having 1 to 10 carbon atoms, a linear or branched alkoxy group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, or a heteroaryl group having 5 to 10 carbon atoms. The alkyl group, aryl group, and heteroaryl group may each have a substituent, and when they have a substituent, the number of carbon atoms included in the number of carbon atoms of the substituent. 4 may be the same or different. 2 represents a halogen atom.)

4. The method for producing a composition according to claim 1 or 2, wherein the initiator is an organic iodine compound.

5. 3. A method for producing the composition according to claim 1, comprising holding the composition at 50 to 300° C. for 2 hours or more.

6. The method for producing a composition according to claim 1 or 2, wherein the vinyl compound (a) comprises a vinyl compound (a1) having a (meth)acryloyloxy group.

7. The method for producing a composition according to claim 6, wherein the vinyl compound (a1) comprises either or both of a vinyl compound (a11) having no reactive silicon group and represented by the following formula 1, and a vinyl compound (a12) having a reactive silicon group and represented by the following formula 1: -SiR 1 3-a X a ・・・Formula 1 (In the above formula 1, R 1 represents a monovalent organic group having 1 to 20 carbon atoms and not containing a hydrolyzable group, X represents a hydroxyl group, a halogen atom or a hydrolyzable group, and a is an integer of 1 to 3. When a is 1, two R 1 may be the same or different, and when a is 2 or 3, multiple Xs may be the same or different.

8. The method for producing a composition according to claim 7, wherein the vinyl compound (a11) and the vinyl compound (a12) are subjected to a living radical polymerization reaction with the initiator in the presence of the catalyst (C), and then the vinyl compound (a12) is further added and subjected to a living radical polymerization reaction to obtain the vinyl polymer (A).

9. The method for producing a composition according to claim 7, wherein the vinyl polymer (A) has an average of 0.5 to 20.0 reactive silicon groups represented by the formula 1 per molecule.

10. The method for producing a composition according to claim 1 or 2, wherein the vinyl polymer (A) has a number average molecular weight of 1,000 to 300,000.

Citation Information

Patent Citations

  • Manufacturing method of (METH)acrylate polymer having reactive silicon group and manufacturing method of curable composition

    JP2022075627A

  • Curable composition

    WO2005095492A1