Particles, and method for producing the particles

Particles containing an oxide of a metal element and a proton-donating functional group address the issues of insufficient antibacterial and antiviral performance, coloration, and stability in coatings by providing high performance and transparency, suitable for transparent films and building materials.

JP2024141110APending Publication Date: 2024-10-10JGC CATALYSTS & CHEMICALS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023052579
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing coatings with antibacterial and antiviral properties face issues such as insufficient performance, coloration, and decreased productivity due to particle size, stability, and compatibility with dispersion media, leading to compromised transparency, strength, and gloss.

Method used

Development of particles containing an oxide of a metal element and a proton-donating functional group, with a proton donating ability of 0.1 to 30 mmol/g, which are produced through a method involving the preparation and deionization of a heteropolyacid salt solution followed by heating, ensuring high antibacterial and antiviral performance without discoloration.

Benefits of technology

The particles achieve high antibacterial and antiviral performance while suppressing coloration and maintaining transparency, strength, and stability, suitable for applications in transparent films and building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141110000001
    Figure 2024141110000001
  • Figure 2024141110000002
    Figure 2024141110000002
Patent Text Reader

Abstract

To provide particles that do not cause coloration when used for a coating film, and have high antibacterial performance or antiviral performance, and a method for producing the particles.SOLUTION: Particles contain oxide of metal element and a proton-donating functional group. Proton-donating performance per unit gram of the particles is 0.1 to 30 mmol / g. The particles have at least one of high antibacterial performance and antiviral performance. According to coating liquid containing the particles, a coating film having suppressed coloration and at least one of high antibacterial performance and antiviral performance is obtained.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to particles containing an oxide of a metal element and a proton-donating functional group, and also to a method for producing the particles. [Background technology]

[0002] Conventionally, in order to prevent reflection on the surface of a substrate such as a sheet or lens made of glass, plastic, etc., an anti-reflection film is formed on the surface. Meanwhile, examples of components that require transparency and anti-reflection performance include display devices having touch panels such as smartphones, ATMs, and ticket vending machines. The surfaces of these devices are problematic in that they are contaminated by fungi such as Escherichia coli and Staphylococcus aureus, and various viruses, and therefore antibacterial and antiviral properties are required from a hygienic standpoint.

[0003] It has been known that antibacterial and antiviral agents are applied to the surface of a coating film to impart antibacterial and antiviral properties. For example, if an organic antibacterial or antiviral agent is used, the coating itself is relatively easy, but there is a risk that the coating film may be damaged by a solvent, and there is a problem with the durability of the antibacterial performance in terms of adhesion to the coating film and scratch resistance. On the other hand, if an inorganic antibacterial or antiviral agent is present in the coating film, the durability of the antibacterial or antiviral performance can be expected, but it is necessary to prepare a coating film containing the agent separately. For example, if an antireflection layer and an antibacterial or antiviral layer are prepared separately, the effect of the layer that is not the outermost surface may be insufficient, or the productivity may decrease, resulting in an increase in production costs. On the other hand, if a low refractive index component, an antibacterial component, and an antiviral component are blended in one coating film, the antireflection performance, antibacterial performance, and antiviral performance may be insufficient, or the transparency and strength of the coating may be insufficient. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-001557 A [Patent Document 2] International Publication No. 2013 / 073555 [Patent Document 3] Patent Publication No. 2021-031450 [Patent Document 4] JP 2007-090336 A [Patent Document 5] Japanese Patent Application Publication No. 7-033616 Summary of the Invention [Problem to be solved by the invention]

[0005] In a coated substrate containing antibacterial particles, if the particle size is as large as a micrometer, the amount of particles must be increased to obtain the desired antibacterial performance, and the dispersion stability of the coating solution containing the particles may decrease. In addition, the hardness, strength, transparency, and gloss of the coated substrate may be impaired (for example, Patent Documents 1 to 3). On the other hand, particles having antibacterial performance smaller than the micrometer order, such as nanometer order, have high dispersibility and a large number per unit amount, so that sufficient antibacterial performance is likely to be exhibited even if the amount of particles in the coated substrate is small. However, if the antibacterial performance is expressed through an oxidative decomposition reaction, the dispersion medium, substrate, etc. may also be decomposed (for example, Patent Document 4). In addition, when Ag, a metal element that exhibits antibacterial properties, is used as a base material, the dispersion medium, substrate, etc. may also be decomposed (for example, Patent Document 4). 2 When it is mixed in the particle as O, Ag 2 There is a risk that O reacts with other compositions to cause coloration, or that particles are non-uniform and may aggregate during dispersion in a solvent (e.g., Patent Document 5). Furthermore, if low-stability particles are present, the dispersion liquid has low concentration stability and cannot be made into a high concentration, which leads to problems such as a large amount of dispersion medium being carried over into the coating liquid, a decrease in productivity in the production of coated substrates due to the use of a low-concentration coating liquid, and a decrease in particle dispersibility in the film.

[0006] Therefore, there is a demand for particles that do not become discolored when used in coatings and have high antibacterial and antiviral properties. [Means for solving the problem]

[0007] In order to solve these problems, the following particles were found.

[0008] The particles contain an oxide of a metal element and a proton-donating functional group, and the proton-donating ability of the particles per unit gram is 0.1 to 30 mmol / g.

[0009] The particles have at least one of high antibacterial and antiviral properties, and a coating solution containing such particles can be obtained that is suppressed in coloration and has at least one of high antibacterial and antiviral properties.

[0010] In order to obtain these particles, the following production method was found.

[0011] First, a first solution containing a heteropolyacid salt containing at least one metal element is prepared. Next, the first solution is deionized to prepare a second solution. Then, the second solution is heated to produce the particles of the present invention.

[0012] The properties of the particles obtained by this production method are similar to those of the particles described above. Effect of the Invention

[0013] According to the particles of the present invention, a coating liquid capable of producing a coating film having at least one of high antibacterial and antiviral properties can be obtained.

[0014] Furthermore, the particles of the present invention can prevent discoloration and coloring of dispersions, coating solutions, and films containing the particles due to heat or light.

[0015] Thus, the particles of the present invention can achieve both high antibacterial and / or antiviral performance and suppression of coloration. Therefore, the particles can be used as highly reliable coating films that can impart antibacterial and antiviral properties to transparent films for televisions and touch panels, as well as building materials and train interior paints in a wide range of fields. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The particles according to the present invention (hereinafter, the particles according to the present invention may be simply referred to as "particles") are particles containing an oxide of a metal element and containing a proton-donating functional group. The proton-donating ability of the particles is 0.1 to 30 mmol / g per unit gram of the particles.

[0017] Such particles have at least one of antibacterial and antiviral properties (hereinafter, the property of "at least one of antibacterial and antiviral properties" according to the present invention may be simply referred to as "antibacterial and antiviral properties"). A substrate with a coating using such particles can obtain antibacterial and antiviral properties.

[0018] When the metal element contained in the particles exists as an oxide, the specific surface area is higher than when the metal exists as a metal, and proton-donating functional groups can be easily introduced.

[0019] The oxide of the metal element contained in the particles is preferably an oxide containing at least one metal element selected from Sb, Mo, Sn, Nb, Zr, and W. The oxide of these metal elements may be composed of one metal element, may be a composite oxide, or may be a mixture. These metal elements contained in the particles exhibit sufficient antibacterial and antiviral properties.

[0020] The oxide is, for example, Sb 2 O 3 , Sb 3 O 5 , Sb 2 O 4 , Sb 2 O 5 , MoO 2 , Mo 2 O 5 , MoO 3 , SnO, SnO 2 , NbO, Nb 2 O 3 , NbO 2 , Nb 2 O 5, WO 2 , WO 3 , H 4 [SiW 12 O 40 ]·nH 2 O(n≒24), H 4 [SiMo 12 O 40 ]·nH 2 Among these, Sb is preferred because it is easy to form nanoparticles and to retain functional groups. 2 O 5 , MoO 3 , SnO 2 , Nb 2 O 5 , WO 3 , Nb 2 O 5 is more preferable.

[0021] The metal element in the particles is preferably contained in an amount of 20 to 100 mass % on an oxide basis. When the content of the metal element is within this range, the particles are porous, proton-donating functional groups can be easily introduced, and sufficient proton-donating ability can be obtained.

[0022] Here, if the content of the metal element in the particles is less than 20 mass%, it may be difficult to introduce a proton-donating functional group, and sufficient proton-donating ability may not be obtained. The content of the metal element in the particles is more preferably 50 to 100 mass%, further preferably 80 to 100 mass%, and particularly preferably 98 to 100 mass%, based on the oxide.

[0023] The particles contain proton-donating functional groups. When the particles contain proton-donating functional groups, they are more likely to exhibit antibacterial and antiviral properties.

[0024] The proton-donating functional groups contained in the particles include -SO 3 OH, -SO 3 H, -PO 3 OH, -OPO(OH) 2 , -COOH, and -OH. 3 OH, -PO3 OH and -OH are more preferred because they easily dissociate protons and have high proton donating properties.

[0025] The proton donating ability of the particles is 0.1 to 30 mmol / g per unit gram of the particles. When the proton donating ability is within this range, the acidity in the system is high, and antibacterial and antiviral properties can be stably expressed. In addition, discoloration or coloring of dispersions, coating solutions, and films containing these particles due to heat or light is suppressed.

[0026] Here, if the proton donating capacity is less than 0.1 mmol / g per unit gram of the particle, the acidity in the system is low, and it may be difficult to obtain antibacterial and antiviral properties. Conversely, if the proton donating capacity is more than 30 mmol / g per unit gram of the particle, the particle may become excessively porous, and it may be difficult to maintain the particle shape. The proton donating capacity per unit gram of the particle is preferably 0.5 to 20 mmol / g, more preferably 0.7 to 18 mmol / g.

[0027] The particles preferably have an alkali metal content of less than 1000 ppm in total on an oxide basis.

[0028] If the content is 1000 ppm or more, the proton donating ability may not be sufficient, the particles may aggregate with each other, the dispersibility of the particles in the coating solution or the film may decrease, the strength and hardness of the film may not be sufficient, and the transparency of the film may become insufficient. The alkali metal content is more preferably less than 500 ppm, even more preferably less than 100 ppm, and most preferably no alkali metal is contained.

[0029] Incidentally, when the particles contain any of alkali metals, alkaline earth metals, ammonia, and amines, the above-mentioned "alkali metal content" is to be read as "the total content of alkali metals, alkaline earth metals, ammonia, and amines." However, for ammonia and amines, NH 3The alkali metals are Li, Na, K, Rb, Cs, and Fr, and the alkaline earth metals are Be, Mg, Ca, Sr, Ba, and Ra.

[0030] The average particle diameter of the particles is not particularly limited because it depends on the application of the coated substrate and the thickness of the coating, but is preferably 1 to 100 nm, for example. This is the average value of the equivalent circle diameters calculated from the areas of 300 randomly selected particles taken at a predetermined magnification using a transmission electron microscope (TEM) and processed to determine the particle areas.

[0031] Here, it is difficult to obtain particles with an average particle size of less than 1 nm. On the other hand, if it exceeds 100 nm, the dispersibility in the coating liquid is low, so that the strength of the coating film may decrease, and the desired antibacterial and antiviral properties may not be obtained. This average particle size is more preferably 5 to 70 nm, and even more preferably 5 to 50 nm.

[0032] The specific surface area of ​​the particles as measured by nitrogen adsorption is 30 to 800 m 2 / g, because when the specific surface area is in this range, the particles have a high surface area and are porous, and can have antibacterial and antiviral properties.

[0033] Here, the specific surface area of ​​the particle is 30 m 2 If the surface area is less than 800 m / g, the surface area is insufficient, and the amount of the metal component element supported may be insufficient. 2 If the specific surface area exceeds 50 to 600 m / g, the particles may become too small, resulting in a decrease in stability and a tendency to aggregate. 2 / g, more preferably 100 to 500m 2 Within this range, it is possible to obtain particles that are highly acidic and more stable.

[0034] The shape of the particles is not particularly limited. For example, the shape may be spherical, ellipsoidal (rugby ball), cocoon-like, confetti-like, chain-like, dice-like, etc. Among them, spherical particles are preferred because they have high dispersibility and can be uniformly dispersed in the coating.

[0035] As described above, the particles of the present invention can achieve both antibacterial and antiviral properties and suppression of coloring of the dispersion, coating, and film containing the particles due to heat and light. Meanwhile, metal elements such as Ag, Cu, Zn, and Bi are known metal elements having antibacterial properties. If these metal elements are contained in the particles, the dispersion, coating, and film containing the particles may be discolored and colored due to heat or light. The particles of the present invention have sufficient antibacterial and antiviral properties even without containing these metal elements. The particles of the present invention have high proton donating properties and strong interactions with these metal elements. Therefore, even if the particles contain metal elements such as Ag, Cu, Zn, and Bi, the dispersion, coating, and film containing the particles of the present invention are suppressed from coloring or discoloring. In this case, the metal elements such as Ag, Cu, Zn, and Bi may be present alone or in multiple species in the particles. The form of these metal elements is preferably ions or complexes. In order to achieve both "improved antibacterial and antiviral properties" and "suppression of coloring and discoloration" by adding metal elements such as Ag, Cu, Zn, and Bi to the particles of the present invention, these metal elements are preferably contained in an amount of 0.1 to 5 mass% on a metal basis. Forms containing such metal elements exhibit higher antibacterial and antiviral properties than those not containing such metal elements.

[0036] Here, if the content of metal elements such as Ag, Cu, Zn, and Bi is less than 0.1% by mass, the synergistic effect of the antibacterial and antiviral properties due to the inclusion of these metal elements may not be obtained. Conversely, if the content exceeds 5% by mass, the antibacterial and antiviral properties will not be improved any further, and in some cases, the components containing these metal elements may become unstable, and may be easily separated from the particles or discolored. The content of these metal elements is more preferably 0.5 to 4% by mass, and even more preferably 2.5 to 3% by mass.

[0037] The particles may be surface-treated with a known organosilicon compound such as a silane coupling agent. Examples of the organosilicon compound include those represented by the following formula (1). Particles surface-treated with such an organosilicon compound are preferred because they have high dispersibility in the particle dispersion medium, the coating solution for forming the coating film, or the matrix of the coating film. In addition, a coated substrate using such surface-treated particles is preferred because it has sufficient hardness and strength due to the suppression of particle aggregation. R n -SiX 4-n ...Equation (1) (In the formula, R represents an unsubstituted or substituted hydrocarbon group having 1 to 10 carbon atoms, and may be the same or different. Examples of the substituent include an alkyl group, a vinyl group, an epoxy group, an acryloyl group, a (meth)acryloyl group, an alkoxy group, a mercapto group, a glycidoxy group, a carboxyl group, an amino group, a phenyl group, and a phenylamino group. X represents an alkoxy group having 1 to 4 carbon atoms, a hydroxyl group, or a hydrogen atom, and n represents an integer of 0 to 4.)

[0038] Specific examples include the organosilicon compounds shown in the following Table 1. Among them, organosilicon compounds containing at least one of an alkyl group, an epoxy group, an acryloyl group, and a (meth)acryloyl group are more preferable because they have a high bond strength with the resin.

[0039] [Table 1]

[0040] The antibacterial test of the particle dispersion is performed according to the shake test method specified by the Antibacterial Product Technology Council. The antibacterial activity value is preferably 2.0 or more. If it is 3.0 or more, it can be judged to have antibacterial properties. The antibacterial activity value is more preferably 4.0 or more.

[0041] The antiviral test of the particle dispersion is carried out in accordance with JIS L1922. The antiviral activity value is preferably 2.0 or more. If it is 3.0 or more, it can be judged to have antiviral properties. The antibacterial activity value is more preferably 4.0 or more.

[0042] The particles may be used as an aqueous dispersion, or may be used after replacing the dispersion medium with an organic dispersion medium, or may be dried and used as a powder.

[0043] [Method of producing particles] The method for producing particles according to the present invention includes the following steps 1, 2, and 3. First, a first solution containing a heteropolyacid salt containing at least one metal element is prepared (step 1). Next, the first solution is deionized to prepare a second solution (step 2). The second solution is heated to obtain particles (step 3).

[0044] In step 1, a first solution containing a heteropolyacid salt containing at least one metal element is prepared. The metal element is preferably at least one selected from Sb, Mo, Sn, Nb, Zr, and W. Examples of heteropolyacid salts containing these metal elements include potassium antimonate, sodium antimonate, ammonium antimonate, sodium phosphotungstate, potassium phosphotungstate, ammonium phosphotungstate, sodium paratungstate, potassium paratungstate, ammonium paratungstate, ammonium silicotungstate, sodium silicotungstate, potassium silicotungstate, sodium tungstate, potassium tungstate, ammonium tungstate, sodium phosphomolybdate, potassium phosphomolybdate, ammonium phosphomolybdate, sodium molybdate, potassium molybdate, ammonium molybdate, sodium silicomolybdate, potassium silicomolybdate, ammonium silicomolybdate, potassium niobate, and potassium stannate. Among these, sodium salts and potassium salts are more preferred from the viewpoints of ease of obtaining nanoparticles and ease of removing impurities.

[0045] In step 2, the first solution prepared in step 1 is deionized. This deionization causes cations, such as counter ions of alkali metal ions, alkaline earth metal ions, ammonium ions, and hydrogen ions, to be eliminated from the heteropolyacid salt. This facilitates the formation of three-dimensional bonds in the subsequent step 3. This deionization can be carried out using a cation exchange resin or the like.

[0046] In step 3, the second solution prepared in step 2 is heated. This heating causes the heteropolyacid to bond three-dimensionally, and the "particles containing an oxide of a metal element" of the present invention are produced. The heating temperature is not particularly limited as long as the desired particles can be produced, but is preferably lower than the boiling point of the solvent. For example, when the solvent is water, it is more preferable to perform the heating at 50°C or higher and lower than 100°C. If the heating temperature is within this range, the heteropolyacid is efficiently bonded three-dimensionally, and the particles are easily formed. In order to promote the formation of these particles, for example, an oxidizing agent that promotes oxidation may be added to the second solution, the solution may be concentrated, or the pH of the solution may be changed to, for example, 5 or higher. These operations may also be performed in combination. In order to further impart another proton-donating functional group, phosphoric acid, sulfuric acid, or acetic acid may be added and further heated and aged, or after drying, the particles may be baked at 200 to 600°C and redispersed in water. The method for redispersing the particles may be a conventionally known dispersion method. For example, a bead mill or ultrasonic dispersion is preferable because it can obtain highly dispersed particles.

[0047] If the above-mentioned metal elements such as Ag, Cu, Zn, and Bi are to be added to the particles, it is preferable to carry out the process after step 3. The components containing metal elements such as Ag, Cu, Zn, and Bi can be added as metal salts such as hydrochlorides, nitrates, sulfates, and acetates, solutions of metal complex ions, and solutions of metal alkoxides to form composite oxide particles. Among them, silver is more preferable for silver, and hydrochlorides, nitrates, sulfates, and acetates are more preferable for copper, zinc, and tin. The amount of the metal elements to be added is preferably such that the metal elements such as Ag, Cu, Zn, and Bi supported in the particles are finally 0.1 to 5 mass% as metal. When adding, a component containing a single metal element such as Ag, Cu, Zn, and Bi may be added, or components containing multiple types of metal species may be added separately or simultaneously. In order to increase the content, the component containing the metal element may be added in multiple batches. The conditions for adding these components containing metal elements are not particularly limited as long as the final content of metal elements such as Ag, Cu, Zn, and Bi is the desired one, but the concentration of the particle dispersion at this time is preferably 1 to 2 mass% as solid content. The pH when adding the components containing metal elements is preferably 2 to 5, more preferably 3 to 4.

[0048] Here, if the pH is less than 2, the metal elements in the particles may dissolve, making the particles unstable and causing aggregation. Conversely, if the pH is more than 5, metal elements such as Ag, Cu, Zn, and Bi may become oxides and discolor. In addition, the temperature when adding the component containing these metal elements is preferably less than the boiling point of the solvent. For example, when the solvent is water, it is preferably less than 100°C, more preferably 30 to 95°C.

[0049] In order to reduce the contents of alkali metals, alkaline earth metals, ammonia, and amines in the particles, it is preferable to wash the particles using an ion exchange resin or an ultrafiltration membrane in at least one of the steps. In particular, washing after the deionization in step 2 is effective. As described above, it is preferable to wash the particles so that the total "alkali metal content" of the particles is less than 1000 ppm.

[0050] [Particle surface treatment] In the present invention, the particles may be surface-treated by adding an organosilicon compound to the dispersion liquid containing the particles. When the particles are surface-treated with an organosilicon compound, it is preferable to perform the surface treatment after step 3. As the organosilicon compound to be used, it is preferable to use an organosilicon compound in which n is 1 to 3 as shown in the above formula (1). Here, when an organosilicon compound in which n is 0 is used, it is preferable to use a partial hydrolyzate of the organosilicon compound. In addition, by introducing a functional group into the particles, the compatibility between the particles and the resin component is improved, which is preferable in terms of obtaining particles with high dispersibility in the coating liquid and film. The organosilicon compound may be used alone or in combination. If a metal element such as Ag, Cu, Zn, or Bi is added to the particles as described above, it is preferable to perform the surface treatment after supporting these metal elements.

[0051] The method of surface treatment of particles is to first prepare a dispersion liquid of particles. As the dispersion medium, it is preferable to use alcohols such as methanol and ethanol. A predetermined amount of an organosilicon compound represented by formula (1) is added to the dispersion liquid, and the organosilicon compound is hydrolyzed. Water can be added to this hydrolysis as necessary. The ratio (Mw / Mo) of the number of moles of water (Mw) to the number of moles of the organosilicon compound (Mo) used is preferably 1 or more.

[0052] Here, if the ratio (Mw / Mo) is less than 1, hydrolysis may be insufficient, and the transparency and haze of the coating may be insufficient. There is no particular upper limit for this ratio, but if this ratio exceeds 500, the hydrolysis reaction may become intense, and the organosilicon compounds may polymerize with each other, making it difficult to efficiently treat the particle surface. This ratio is more preferably 1 to 100.

[0053] In this hydrolysis, an acid or alkali can be used as a hydrolysis catalyst, if necessary. Among them, ammonia is preferred. This is because if ammonia is used, it is easy to remove even if it remains in the dispersion, and the stability of the dispersion is easily maintained. The number of moles of ammonia used (M N ) and the mole number (Mo) of the organosilicon compound (M N / Mo) is preferably in the range of 0.05 to 50.

[0054] Here, the ratio (M N If the ratio (Mo) is less than 0.05, hydrolysis may be insufficient, resulting in insufficient transparency and haze of the coating. If the ratio exceeds 50, the hydrolysis reaction may become so vigorous that the organosilicon compounds may polymerize with each other, making it difficult to efficiently treat the particle surfaces. This ratio is more preferably 0.1 to 10.

[0055] The surface treatment is preferably carried out in a homogeneous system, and in order to promote the reaction between the particles and the organosilicon compound, it is preferable to heat the particles at a temperature below the boiling point of the dispersion medium (for example, room temperature to 120° C.) for 0.5 to 48 hours.

[0056] Examples of the organosilicon compound include those shown in Table 1. The particles may contain one or more of these organosilicon compounds. In the surface treatment, the particles may be treated with one or more of these organosilicon compounds, or may be treated in stages with the same type, a mixture of multiple types, or multiple types separately.

[0057] The amount of this organosilicon compound is 100 parts by mass of the "original particles" before surface treatment. n -SiO (4-n) / 2 ) is preferably 1 to 100 parts by mass.

[0058] Here, if the amount is less than 1 part by mass, it may be difficult to obtain the sufficient effect of the addition. Conversely, if the amount is more than 100 parts by mass, the dispersion stability is improved, but the acidity of the particles may be reduced, and the antibacterial and antiviral properties may be reduced. The amount of the organosilicon compound is more preferably 3 to 50 parts by mass, and further preferably 10 to 30 parts by mass.

[0059] The physical properties and preferred ranges of the finally obtained particles and their dispersion are the same as those of the above-mentioned particles and their dispersion.

[0060] [Coating liquid for film formation] The particles of the present invention can be applied to a coating solution for forming a coating film. This coating solution contains the particles and a matrix forming component. In addition to the above, the coating solution may contain additives such as an organic dispersion medium, a polymerization initiator, a leveling agent, and a surfactant.

[0061] [Coated base material] The particles of the present invention can be used for materials that require antibacterial and antiviral properties. The particles of the present invention not only have high antibacterial and antiviral properties, but also suppress discoloration of the composition and have sufficient hardness and strength. Therefore, for example, they are used in a coating solution that can produce a coating. In addition, this coating solution can be used to produce a substrate with a coating that requires antibacterial and antiviral properties.

[0062] The coated substrate according to the present invention is a substrate having a coating film formed on the substrate, the coating film including the above-mentioned particles and a matrix. The matrix is ​​a solid component other than the particles, and includes resins derived from the coating liquid, and additives such as polymerization initiators and leveling agents. Specifically, the coating liquid is applied to the substrate by a known method, and then dried and irradiated with ultraviolet light to form a coating film on the substrate. In the coating film, the ratio of the solid components of the particles and matrix-forming components in the coating liquid is the same as the ratio of the particle components and matrix in the coating film.

[0063] Between the coating and the substrate, a conventionally known hard coat layer, anti-glare layer, high refractive index layer, conductive layer, etc. may be disposed depending on the application. A plurality of these layers may be combined. For example, when the reflectance is to be further reduced as a substrate with a transparent coating for display applications, a combination of a hard coat layer and a high refractive index layer, or a combination of a hard coat layer and an anti-glare layer may be exemplified.

[0064] The thickness of the coating can be appropriately selected depending on the application. For example, for anti-reflection coating, 80 to 350 nm is preferable. Here, if the thickness is less than 80 nm, the strength and scratch resistance of the coating may be insufficient. In addition, the coating may be too thin and may not provide sufficient anti-reflection performance. Conversely, if the thickness is more than 350 nm, the anti-reflection performance may be reduced. In addition, if the shrinkage is very large, cracks may occur. This thickness is more preferably 85 to 220 nm, and even more preferably 90 to 110 nm.

[0065] The reflectance of the substrate with a transparent coating having antireflection properties is preferably 2.0% or less, and more preferably 1.5% or less.

[0066] The haze of the substrate with the transparent coating is preferably 3.0% or less, and more preferably 0.3% or less.

[0067] The total light transmittance of the transparent coated substrate is preferably 85.0% or more. If the total light transmittance is less than 85.0%, the clarity of the image on the display device of the obtained coating may be insufficient. The total light transmittance is more preferably 90.0% or more.

[0068] The yellowness of the coating (yellow index value: YI value) can be calculated from the value established by the International Commission on Illumination (CIE) in the XYZ color system as CIE1931, and is used as an index for comparing the difference in yellowness of coatings. The yellowness is preferably 1.0 or less, and more preferably less than 0.2. Here, if the YI value is 1.0 or less, it is difficult to clearly visually recognize that the coating film is yellow when confirmed by visual inspection. Furthermore, if the YI value is less than 0.2, the yellow color is not visually recognized, which is more preferable.

[0069] The yellowing degree of the coating (the difference in YI value before and after the light resistance test) is preferably 1.0 or less, more preferably less than 0.2. Here, if the difference in YI value before and after the light resistance test is 1.0 or less, it is difficult to visually recognize a clear yellowing change when visually confirmed. Furthermore, if the difference in YI value is less than 0.2, it is more preferable because the yellowing change is not visually recognized.

[0070] The strength of the coating (scratch resistance) was measured using #0000 steel wool with a load of 1000g / cm 2 The film is evaluated by rubbing against a surface of the film at a temperature of 100° C. It is preferable that no streaky scratches are observed on the film surface after rubbing at least 100 times. More preferably, the scratch resistance is such that no scratches are observed after 500 times, and even more preferably, no scratches are observed after 1000 times.

[0071] The pencil hardness of the coating is preferably H or more. If it is less than H, the hardness is insufficient when used as an anti-reflection film. The pencil hardness is more preferably 2H or more, and further preferably 3H or more.

[0072] The antibacterial activity test of the coating is carried out in accordance with JIS Z 2801. It is preferable that the antibacterial activity value is 2.0 or more. If it is 2.0 or more, it can be judged to have antibacterial activity. The antibacterial activity value is more preferably 4.0 or more.

[0073] The antiviral activity test of the coating is performed in accordance with ISO21702. It is preferable that the antiviral activity value is 2.0 or more. If it is 2.0 or more, it can be judged to have antiviral properties. The antibacterial activity value is more preferably 3.0 or more.

[0074] The substrate may be a known one. For example, a transparent resin substrate such as glass, polycarbonate, acrylic resin, polyethylene terephthalate (PET), triacetyl cellulose (TAC), polyimide, polymethyl methacrylate resin (PMMA), or cycloolefin polymer (COP) is preferred. These substrates have excellent adhesion to the transparent coating formed by the above-mentioned coating liquid, and a substrate with a coating excellent in hardness, strength, etc. can be obtained. For this reason, it is suitable for use with thin substrates. There is no particular restriction on the thickness of the substrate, but it is preferably 10 to 100 μm, and more preferably 20 to 80 μm.

[0075] Hereinafter, an embodiment of the present invention will be described. EXAMPLES

[0076] [Example 1] [Production of diantimony pentoxide particles] In a solution of 1800 g of pure water, 64.1 g of potassium hydroxide (Kanto Chemical Co., Ltd., special grade 1, purity 98%) was dissolved, and antimony trioxide (PATOX-K, orthorhombic, Sb 2 O 3 100 g of the mixture (concentration: 30% by mass) was suspended.

[0077] This suspension was heated to 98°C, and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide (manufactured by Mitsubishi Gas Chemical Co., Inc., concentration 35% by mass) with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate 0.20 mmol / hr.) to dissolve the antimony trioxide.

[0078] After cooling to room temperature, 150 g of undissolved residue was separated from the resulting solution and dissolved in potassium antimonate (Sb 2 O 5 A converted concentration of 4.7% by mass was obtained (Step 1).

[0079] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation) (step 2).

[0080] Next, this deionized solution (Sb 2 O 5 The aqueous dispersion of diantimony pentoxide particles was produced by concentrating the aqueous dispersion of diantimony pentoxide particles at a concentration of 0.05% by mass at a temperature of 60° C. for 10 hours. 2 O 5 The converted concentration was 15% by mass (Step 3).

[0081] Surface treatment of particles with organosilicon compounds The aqueous dispersion of diantimony pentoxide particles produced in step 3 (equivalent to 8 g of solid content), 0.8 g of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 50 g of methanol were mixed and kept in a constant temperature bath at 50°C for 24 hours with stirring.

[0082] The mixture was then concentrated to 50 g using an ultrafiltration membrane.

[0083] Next, 800 g of methanol was continuously added to the mixture while the filtrate was discharged, and the solvent was replaced with methanol. The solid content of the methanol-substituted product was 3.0% by mass, and the water content was 0.3% by mass.

[0084] Next, 50 g of this methanol-substituted product was placed in an eggplant-shaped flask, 150 g of methyl isobutyl ketone (MIBK) was added, and the flask was attached to a rotary evaporator. While reducing the pressure, the solvent was replaced with MIBK in a water bath at 80°C to produce a MIBK dispersion of diantimony pentoxide particles. The solid content at this time was 2.0 mass%, Sb 2 O 5 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0085] The particles and their dispersions were measured by the following methods.

[0086] The characteristics of each production step of the particles, and the properties of the particles and dispersion liquid are shown in Table 2 (the same applies to the following Examples and Comparative Examples).

[0087] (1) Confirmation of oxides of metal elements The particle dispersion was analyzed by X-ray diffraction while in solution to confirm the presence or absence of metal oxide and its morphology. Qualitative analysis of the sample by X-ray diffraction was performed using an X-ray diffraction meter (Smart Lab) manufactured by RIGAKU Corporation. Specifically, the sample was placed in a cell and set in the device, and measurements were performed at a tube voltage of 45.0 kV, a tube current of 200.0 mA, a Cu anticathode, a measurement range of start angle to end angle (2θ) of 5.000° to 70.000°, and a scan speed of 5.000° / min.

[0088] (2) Proton-donating functional group The aqueous dispersion of the particles was collected in a beaker and dried by heating at 200° C. to obtain a powder of the particles. The obtained powder was subjected to FT-IR analysis to examine the presence and type of proton-donating functional groups based on the positions of the absorption peaks.

[0089] (3) Proton donation The aqueous dispersion of the particles was collected in a beaker in an amount equivalent to 1.50 g of particle solid content, and water was added to make it 100 g, and the mixture was transferred to a thermostatic reaction tank maintained at 25 ° C. Next, 20 g of cation exchange resin (Diaion SK-IBH, manufactured by Mitsubishi Chemical Corporation) was added, and the mixture was stirred for 1 hour, after which the ion exchange resin was removed. Next, 50 g of this ion-exchanged solution (particle solid content 0.75 g) was collected in a beaker. This was transferred to a thermostatic reaction tank maintained at 25 ° C., a pH electrode was set, and sodium chloride (special grade, manufactured by Kanto Chemical Co., Ltd.) was added while stirring, and the change in pH was observed. When no change in pH was observed, the addition of sodium chloride was stopped, and the change in pH before and after the addition was measured. From the obtained change in pH, the amount of protons in 50 g of solution was calculated, and the result divided by the solid content in the dispersion was used as the proton-donating ability per unit gram.

[0090] (4) Content of metallic elements, alkali metals, and alkaline earth metals The oxide content of metal elements (Sb, Mo, Sn, Nb, Si, Al, and W) in the particles, the content of metal elements (Ag, Cu, Zn, Bi), and the content of alkali metals and alkaline earth metals as impurity elements were measured by adding 5 g of 61% nitric acid to 0.1 g of a particle dispersion and adding pure water as necessary, and measuring the resulting solution using an ICP inductively coupled plasma optical emission spectrometer (ICP-8500, manufactured by Shimadzu Corporation). Note that if metal elements other than the above-mentioned impurity elements were present, the total amount of metal elements contained in the particles was calculated to be 100 parts by mass on an oxide basis.

[0091] (5) Ammonia and amine content A 20% by mass aqueous solution of NaOH is added to the particle dispersion, and distilled while dissolving the particles. The ammonia that comes out is captured with 0.05 mol / L sulfuric acid and titrated with 0.1N NaOH to determine the amount of sulfuric acid consumed and the total amount of ammonia contained in the liquid.

[0092] (6) Average particle size The particle dispersion was diluted to 0.01% by mass, and then dried on a collodion film of a copper cell for electron microscopes. Next, this was photographed at a specified magnification using a field emission transmission electron microscope (HF5000, manufactured by Hitachi High-Technologies Corporation). The particle area of ​​300 random particles in the obtained photographic projection (TEM photograph) was calculated by image processing, and the circle equivalent diameter was calculated from the area. The average value of the circle equivalent diameters was taken as the average particle diameter of the particles.

[0093] (7) Specific surface area The specific surface area was determined by the BET method using nitrogen adsorption. The measurement sample was prepared by drying the particle dispersion at 105°C and powdering it.

[0094] (8) Particle shape The appearance of 300 randomly selected particles in the TEM photograph taken when determining the average particle size of the above-mentioned particles was observed.

[0095] (9) Antibacterial test of aqueous dispersion of particles The shake test was conducted according to the Antibacterial Products Technology Council's shake test method. The bacteria used was Staphylococcus aureus, and the solids concentration of the aqueous dispersion of the particles was 15 ppm.

[0096] (10) Antiviral test of aqueous dispersion of particles The antiviral test of the aqueous dispersion of the particles was carried out in accordance with JIS L 1922. The virus used was influenza A (H3N2), and the solids concentration of the aqueous dispersion of the particles was 500 ppm.

[0097] (11) Solids concentration of particle dispersion 1 g of the particle dispersion was placed in a porcelain crucible, ignited at 300°C, and weighed to determine the weight loss.

[0098] <Production of Coating Solution for Film Formation> A coating solution for forming a coating was prepared by adding the MIBK dispersion of particles (solid concentration 2.0% by mass) obtained in the above-mentioned "Surface treatment of particles with an organosilicon compound" to an anti-reflective coating material (sometimes called an anti-reflection coating material or an AR coating material) ELCOM-P-5062 (solid concentration 3.0% by mass) manufactured by JGC Catalysts and Chemicals Co., Ltd. in an amount equivalent to 5% by mass of the solid content of the particles.

[0099] <Production of coated substrate> A hard coat paint (ELCOM HP-1004, manufactured by JGC Catalysts and Chemicals Co., Ltd.) was applied to a TAC film (FT-PB80UL-M, manufactured by PANAC Corporation, thickness 80 μm, refractive index 1.51) by the bar coater method (#18), and dried at 80 °C for 120 seconds. Then, 300 mJ / cm 2 The hard coat film was then cured by irradiation with ultraviolet light of 1000 .mu.m to form a hard coat film having a thickness of 8 .mu.m.

[0100] Next, a coating solution for forming a coating film using the particles of the present invention was applied by a bar coater method (#4) and dried at 80° C. for 120 seconds. 2 400mJ / cm under atmospheric pressure 2 The coating was cured by exposure to ultraviolet light of 1000 ohms to produce a coated substrate.

[0101] The coated substrate was measured for the following items, and the results are shown in Table 2 (the same applies to the following Examples and Comparative Examples).

[0102] (12) Film thickness, reflectance The film thickness and reflectance at a wavelength of 550 nm of the coated substrate were measured using an ellipsometer (EMS-1, manufactured by ULVAC Corporation).

[0103] (13) Haze, total light transmittance, and yellow index value The haze, total light transmittance, and yellow index value (YI value) of the coated substrate were measured using a haze meter (manufactured by Suga Test Instruments Co., Ltd.).

[0104] (14) Light resistance test The coated substrate was set in a Sunshine Weather-O-Meter (Model S80DHBBR, manufactured by Suga Test Instruments Co., Ltd.) and the test was carried out according to JIS K 7350-4. The difference in the YI value of the film before and after the test was used as an index of the presence or absence of light resistance.

[0105] (15) Measurement of scratch resistance #0000 steel wool, load 1000g / cm 2 After sliding, the surface of the coated substrate was visually observed and evaluated according to the following criteria. Evaluation criteria; No streaky scratches: ◎ Slight streak marks: Yes Numerous streak-like scratches are observed: △ The entire surface is scraped off.

[0106] (16) Pencil hardness measurement The hardness was measured using a pencil hardness tester according to JIS-K-5400.

[0107] (17) Antibacterial test of coating The antibacterial test of the coating was carried out in accordance with JIS Z 2801, and the antibacterial activity value was calculated by the following formula (2). Q B =U Bt -A Bt (2) (However, Q B is the antibacterial activity value, U Bt is the 1 cm thickness of the untreated test piece after 24 hours. 2 The average logarithm of the number of viable bacteria per unit area, A Bt is the 1 cm 24 hours after antibacterial treatment 2 The mean logarithmic value of the number of viable bacteria per sample is shown.)

[0108] An antibacterial activity value of 2.0 or higher was determined to have antibacterial effect.

[0109] The test bacteria used were Staphylococcus aureus (NBRC 12732) and Escherichia coli (NBRC3972), and the nutrients used were 1 / 500 nutrient bouillon medium (3 g meat extract + 10 g peptone, 5.0 g sodium chloride per 1000 ml of medium).

[0110] For the measurement, 0.4 ml of the bacterial solution was dropped onto the coated substrate and untreated film cut into 5 cm squares, and then covered with a 4 cm square PE film. The test pieces were cultured for 24 hours at 35°C ± 1°C and a relative humidity of 90% or more, and the test bacteria on the test pieces were washed out and collected with 10 ml of SCDLP medium. The viable bacteria count of the washed out liquid was then measured by the pour plate culture method. 2 The number of viable bacteria per unit area was determined.

[0111] (18) Antiviral test of coating The antiviral test of the coating was carried out in accordance with ISO 21702, and the antiviral activity value was calculated by the following formula (3). Q V =U Vt -A Vt (3) (However, Q Vis the antiviral activity value, U Vt is the 1 cm thickness of the untreated test piece after 24 hours. 2 The mean logarithmic value of the viral infectivity per unit area, A Vt is the 1 cm 24 hours after the antiviral treatment 2 The mean logarithmic value of the viral infectivity per sample is shown.)

[0112] An antiviral activity value of 2.0 or higher was determined to have an antiviral effect.

[0113] The measurements were performed on the coated substrate and the unprocessed film cut into 5 cm squares, with a concentration of 1 to 5 × 10 7 0.4 ml of a virus suspension (influenza A virus (H3N2) ATCC VR-1679) adjusted to pfu / ml was dropped onto the specimen and covered with a 4 cm square PE film. The specimen was cultured for 24 hours at 25°C ± 1°C and a relative humidity of 90% or higher, and the test bacteria on the specimen were washed out and collected with 10 ml of SCDLP medium. A 10-fold dilution series of the washed-out liquid was prepared, and the plaque was measured by the plaque measurement method. 2 The viral infectivity per unit time was measured.

[0114] [Example 2] [Production of tungsten oxide particles] Ammonium paratungstate (Kishida Chemical Co., Ltd., WO 3 (Converted concentration: 83 mass%) was suspended in 133 g of the suspension.

[0115] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve ammonium paratungstate.

[0116] Next, after cooling to room temperature, 50 g of undissolved residue was separated from the resulting solution, and ammonium paratungstate solution (WO 3 A converted concentration of 2.7% by mass was obtained.

[0117] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0118] Next, this deionized solution (WO 3 The aqueous dispersion of tungsten oxide particles was produced by heating the aqueous dispersion of tungsten oxide particles (converted concentration: 0.1% by mass) at a temperature of 98°C for 10 hours. The aqueous dispersion was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of tungsten oxide particles. 3 The converted concentration was 15% by mass.

[0119] Surface treatment of particles with organosilicon compounds A dispersion of tungsten oxide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of tungsten oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, and WO 3 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0120] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of tungsten oxide particles was used, and the properties thereof were evaluated.

[0121] [Example 3] [Production of molybdenum oxide particles] Ammonium molybdate tetrahydrate (MoO, manufactured by Fuji Film Wako Co., Ltd.) was added to a solution of 64.1 g of potassium hydroxide in 1,800 g of pure water. 3 (Converted concentration: 82% by mass) 258.6 g was suspended.

[0122] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve ammonium molybdate tetrahydrate.

[0123] Next, after cooling to room temperature, 50 g of undissolved residue was separated from the resulting solution and dissolved in ammonium molybdate (MoO 3 A converted concentration of 5.6% by mass was obtained.

[0124] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0125] Next, this deionized solution (MoO 3 The aqueous dispersion of molybdenum oxide particles (converted concentration: 0.25% by mass) was heated at a temperature of 60° C. for 10 hours. The aqueous dispersion was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of molybdenum oxide particles. 3 The converted concentration was 15% by mass.

[0126] Surface treatment of particles with organosilicon compounds A dispersion of molybdenum oxide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of molybdenum oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, MoO 3 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0127] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of molybdenum oxide particles was used, and the properties thereof were evaluated.

[0128] [Example 4] [Production of tin oxide particles] In a solution of 64.1 g of potassium hydroxide in 1800 g of pure water, potassium stannate (SnO 2 (converted concentration: 51.8 mass%) was suspended.

[0129] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the potassium stannate.

[0130] Next, after cooling to room temperature, 50 g of undissolved residue was separated from the resulting solution to obtain a potassium stannate solution (5.6% in terms of tin oxide).

[0131] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0132] Next, this deionized solution (SnO 2 The aqueous dispersion of tin oxide particles was produced by heating the aqueous dispersion of tin oxide particles at a temperature of 60° C. (converted concentration: 0.2% by mass) for 10 hours. The aqueous dispersion was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of tin oxide particles. 2 The converted concentration was 15% by mass.

[0133] Surface treatment of particles with organosilicon compounds A dispersion of tin oxide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of tin oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, SnO 2 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0134] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of tin oxide particles was used, and the properties thereof were evaluated.

[0135] [Example 5] [Production of niobium pentoxide particles] In a solution of 64.1 g of potassium hydroxide in 1800 g of pure water, potassium niobate (Fujifilm Wako Pure Chemical Industries, Ltd., Nb 2 O 5 (Converted concentration: 72% by mass) was suspended in 300.0 g of the suspension.

[0136] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the potassium niobate.

[0137] Next, after cooling to room temperature, 10 g of undissolved residue was separated from the resulting solution and added to a potassium stannate solution (Nb 2 O 5 A converted concentration of 5.8% by mass was obtained.

[0138] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0139] Next, this deionized solution (Nb 2 O 5 The aqueous dispersion of niobium pentoxide particles was produced by heating the aqueous dispersion at a temperature of 60° C. (converted concentration: 0.2% by mass) for 10 hours. The aqueous dispersion was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of niobium pentoxide particles. 2 O 5 The converted concentration was 15% by mass.

[0140] Surface treatment of particles with organosilicon compounds A dispersion of niobium pentoxide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of niobium pentoxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, Nb 2 O 5 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0141] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of niobium pentoxide particles was used, and the properties thereof were evaluated.

[0142] [Example 6] [Production of tungsten silicide particles] In a solution of 1800 g of pure water and 64.1 g of potassium hydroxide, tungstosilicic acid 24 hydrate (Kishida Chemical Co., Ltd.) was added. 3 (Converted concentration: 85.8 mass%) was suspended in 300.0 g of the suspension.

[0143] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the tungstosilicic acid.

[0144] Next, after cooling to room temperature, 5 g of undissolved residue was separated from the resulting solution, and potassium silicotungstate solution (WO3 A converted concentration of 5.9% by mass was obtained.

[0145] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0146] Next, this deionized solution (concentration of tungstosilicic acid: 0.2% by mass) was heated at 60° C. for 10 hours, after which 100 g of hydrogen peroxide was added and the solution was further heated at 60° C. for 10 hours. Thereafter, the solution was concentrated using an ultrafiltration membrane to produce an aqueous dispersion of tungstosilicic acid particles. 3 The converted concentration was 15% by mass.

[0147] Surface treatment of particles with organosilicon compounds A dispersion of tungsten silicide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of tungsten silicide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, WO 3 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0148] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of the tungsten silicide particles was used, and the properties thereof were evaluated.

[0149] [Example 7] [Production of molybdenum silicic oxide particles] In a solution of 64.1 g of potassium hydroxide in 1,800 g of pure water, silicomolybdic acid n-hydrate (silicomolybdic acid MoO 3 150.0 g of the resulting suspension (converted concentration: 97% by mass) was suspended.

[0150] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the silicomolybdic acid.

[0151] Next, after cooling to room temperature, 10 g of undissolved residue was separated from the resulting solution and dissolved in potassium silicomolybdate (MoO 3 A converted concentration of 5.5% by mass was obtained.

[0152] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0153] Next, this deionized solution (MoO 3 After heating the mixture (converted concentration: 0.2% by mass) at a temperature of 60° C. for 10 hours, 100 g of hydrogen peroxide solution was added and the mixture was further heated at a temperature of 60° C. for 10 hours. The mixture was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of silicomolybdenum oxide particles. 3 The converted concentration was 15% by mass.

[0154] Surface treatment of particles with organosilicon compounds A dispersion of silicomolybdenum oxide particles in MIBK was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of silicomolybdenum oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, MoO 3 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0155] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of the silicomolybdenum oxide particles was used, and the properties thereof were evaluated.

[0156] [Example 8] [Production of phosphorus molybdenum oxide particles] A solution of 64.1 g of potassium hydroxide in 1,800 g of pure water was added to sodium phosphomolybdate 30 hydrate (MoO 3 (Converted concentration: 73 mass%) was suspended in 200.0 g of the suspension.

[0157] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the phosphomolybdic acid.

[0158] After cooling to room temperature, 5 g of undissolved residue was separated from the resulting solution and dissolved in sodium and potassium phosphomolybdate (MoO 3 A converted concentration of 6.0% by mass was obtained.

[0159] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0160] Next, this deionized solution (MoO 3 After heating the mixture (converted concentration: 0.5% by mass) at a temperature of 60° C. for 10 hours, 100 g of hydrogen peroxide solution was added and the mixture was further heated at a temperature of 60° C. for 10 hours. The mixture was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of phosphomolybdenum oxide particles. The MoO 3 The converted concentration was 15% by mass.

[0161] Surface treatment of particles with organosilicon compounds A MIBK dispersion of phosphomolybdenum oxide particles was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of phosphomolybdenum oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, MoO 3 The converted concentration was 1.8 mass%, and the moisture content was 0.2 mass%.

[0162] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of the silicomolybdenum oxide particles was used, and the properties thereof were evaluated.

[0163] [Example 9] [Production of phosphotungsten oxide particles] In a solution of 64.1 g of potassium hydroxide in 1800 g of pure water, tungstophosphoric acid 30 hydrate (WO3 (Converted concentration: 73 mass%), 150.0 g, was suspended.

[0164] This suspension was heated to 98° C., and an aqueous solution prepared by diluting 58.2 g of hydrogen peroxide with 191.6 g of pure water was added thereto over a period of 6 hours (addition rate: 0.20 mmol / hr.) to dissolve the tungstophosphoric acid.

[0165] Next, after cooling to room temperature, 10 g of undissolved residue was separated from the resulting solution, and potassium phosphotungstate solution (WO 3 A converted concentration of 5.6% by mass was obtained.

[0166] This solution was diluted with 10,000 g of pure water and then deionized using a cation exchange resin (PK-216, manufactured by Mitsubishi Chemical Corporation).

[0167] Next, this deionized solution (WO 3 After heating the mixture (converted concentration: 0.2% by mass) at a temperature of 60° C. for 10 hours, 100 g of hydrogen peroxide solution was added and the mixture was further heated at a temperature of 60° C. for 10 hours. The mixture was then concentrated using an ultrafiltration membrane to produce an aqueous dispersion of tungsten phosphonate particles. 3 The converted concentration was 15% by mass.

[0168] Surface treatment of particles with organosilicon compounds A MIBK dispersion of phosphotungsten oxide particles was produced by surface treatment of the particles in the same manner as in Example 1, except that the aqueous dispersion of phosphotungsten oxide particles produced in step 3 was used. The solid content at this time was 2.0 mass%, WO 3 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0169] A coating solution and a coated substrate were produced in the same manner as in Example 1, except that the MIBK dispersion of the phosphotungsten oxide particles was used, and the properties thereof were evaluated.

[0170] [Example 10] [Production of Ag-loaded diantimony pentoxide oxide particles] 100 g of the aqueous dispersion of diantimony pentoxide particles produced in Example 1 was mixed with 1900 g of pure water, followed by mixing with a solution of 1.2 g of silver nitrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Ag equivalent concentration 63% by mass) dissolved in 90 g of pure water.

[0171] The mixture was heated and stirred at 98° C. for 6 hours. After that, it was concentrated using an ultrafiltration membrane until the solid concentration became 15% by mass, and then washed with 400 g of pure water to produce an aqueous dispersion of silver-supported diantimony pentoxide particles. 2 O 5 The equivalent concentration was 15 mass %, and the equivalent Ag concentration was 0.6 mass %.

[0172] Surface treatment of particles with organosilicon compounds Except for using this aqueous dispersion of silver-supported diantimony pentoxide particles, the surface treatment of the particles was carried out in the same manner as in Example 1 to produce an MIBK dispersion of silver-supported diantimony pentoxide particles. 2 O 5 The converted concentration was 1.73 mass%, the Ag converted concentration was 0.07 mass%, and the moisture content was 0.2 mass%.

[0173] A coating solution and a substrate with a coating were prepared in the same manner as in Example 1, except that the MIBK dispersion of silver-supported diantimony pentoxide particles was used, and the properties thereof were evaluated.

[0174] [Example 11] [Preparation of Cu-loaded diantimony pentoxide oxide particles] 100 g of the aqueous dispersion of diantimony pentoxide particles produced in Example 1 was mixed with 1,900 g of pure water, followed by mixing with a solution of 1.5 g of copper nitrate trihydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Cu equivalent concentration 23% by mass) dissolved in 90 g of pure water.

[0175] This mixture was heated and stirred at 98° C. for 6 hours. Thereafter, it was concentrated using an ultrafiltration membrane until the solid concentration became 15% by mass, and then washed with 400 g of pure water to produce an aqueous dispersion of copper-supported diantimony pentoxide particles. 2 O 5 The equivalent concentration was 15 mass %, and the Cu equivalent concentration was 0.3 mass %.

[0176] Surface treatment of particles with organosilicon compounds Except for using this aqueous dispersion of copper-supported diantimony pentoxide particles, the surface treatment of the particles was carried out in the same manner as in Example 1 to produce an MIBK dispersion of copper-supported diantimony pentoxide particles. 2 O 5 The converted concentration was 1.76 mass%, the Cu converted concentration was 0.04 mass%, and the moisture content was 0.2 mass%.

[0177] A coating solution and a substrate with a coating were prepared in the same manner as in Example 1, except that the MIBK dispersion of copper-supported diantimony pentoxide particles was used, and the properties thereof were evaluated.

[0178] [Example 12] [Production of Zn-loaded diantimony pentoxide oxide particles] 100 g of the aqueous dispersion of diantimony pentoxide particles produced in Example 1 was mixed with 1,900 g of pure water, and then mixed with a solution of 2.4 g of zinc nitrate hexahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., Zn equivalent concentration 22% by mass) dissolved in 90 g of pure water.

[0179] This mixture was heated and stirred at 98°C for 6 hours. Thereafter, it was concentrated using an ultrafiltration membrane until the solid concentration became 15% by mass, and then washed with 400 g of pure water to produce an aqueous dispersion of zinc-supported diantimony pentoxide particles. 2 O 5 The equivalent concentration was 15 mass %, and the equivalent Zn concentration was 0.6 mass %.

[0180] Surface treatment of particles with organosilicon compounds Except for using this aqueous dispersion of zinc-supported diantimony pentoxide particles, the particles were surface-treated in the same manner as in Example 1 to produce an MIBK dispersion of zinc-supported diantimony pentoxide particles. 2 O 5 The converted concentration was 1.73 mass%, the Zn converted concentration was 0.07 mass%, and the moisture content was 0.2 mass%.

[0181] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of zinc-supported diantimony pentoxide particles was used, and the properties thereof were evaluated.

[0182] [Example 13] [Production of sulfo-group-added silica particles] Silica sol (JGC Catalysts and Chemicals, Cataloid SI-30 SiO 2 Concentration: 30% by mass; average particle size: 12 nm) was added and mixed in an amount of 333.3 g.

[0183] To this mixture, 200 g of a cation exchange resin (SK-1BH manufactured by Mitsubishi Chemical Corporation) was added and stirred at 80° C. for 24 hours. Then, the mixture was cooled to room temperature, and the ion exchange resin was separated, and SiO 2 An ion-exchanged silica sol having a converted concentration of 5% by mass and an average particle size of 12 nm was obtained. The ion-exchanged silica sol was then dried at 80° C. and sprayed with anhydrous sulfuric acid gas to obtain a dry powder.

[0184] Next, 100 g of this dry powder, 400 g of pure water, and quartz beads (φ0.1 mm, 3 kg) were mixed and dispersed in a bead mill. After that, the quartz beads and the dispersion were separated, and ion exchange was performed at room temperature using a cation exchange resin (SK-1BH, manufactured by Mitsubishi Chemical Corporation) to obtain an aqueous dispersion of silica particles to which sulfo groups were added. The SiO 2 The converted concentration was 15% by mass.

[0185] Surface treatment of particles with organosilicon compounds Except for using this aqueous dispersion of silica particles to which sulfo groups were added, the particles were surface-treated in the same manner as in Example 1 to produce an MIBK dispersion of an aqueous dispersion of silica particles to which sulfo groups were added. 2 The converted concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0186] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of silica particles to which sulfo groups had been added was used, and the properties thereof were evaluated.

[0187] [Example 14] 20 g of the aqueous dispersion of sulfo-group-imparted silica particles produced in Example 13 was added to 80 g of the aqueous dispersion of diantimony pentoxide particles prepared in Example 1, and mixed.

[0188] Surface treatment of particles with organosilicon compounds Except for using this mixed dispersion, the surface treatment of the particles was carried out in the same manner as in Example 1 to produce an MIBK dispersion of an aqueous dispersion of diantimony pentoxide particles and silica particles to which a sulfo group had been added. The solid content at this time was 2.0 mass %, SiO 2 The converted concentration is 0.36 mass%, Sb 2 O 5 The converted concentration was 1.44 mass %, and the moisture content was 0.2 mass %.

[0189] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that this MIBK dispersion was used, and the properties thereof were evaluated.

[0190] [Comparative Example 1] [Production of silica particles] Silica sol (JGC Catalysts and Chemicals, Cataloid SI-30, SiO 2 333.3 g of silica gel (concentration: 30% by mass, average particle size: 12 nm) was added and mixed. Then, 200 g of a cation exchange resin (SK-1BH, manufactured by Mitsubishi Chemical Corporation) was added and stirred at 80° C. for 24 hours. Then, the mixture was cooled to room temperature, and the ion exchange resin was separated to obtain ion-exchanged silica sol (SiO2 The resulting concentration was 5% by mass and the average particle size was 12 nm.

[0191] Surface treatment of particles with organosilicon compounds The surface treatment of the particles was carried out in the same manner as in Example 1, except that 8 g of the solid content of this ion-exchanged silica sol, 0.8 g of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 160 g of methanol were mixed to produce an MIBK dispersion of silica particles. 2 The converted concentration was 14.0% by mass, and the moisture content was 0.2% by mass.

[0192] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of silica particles was used, and the properties thereof were evaluated.

[0193] [Comparative Example 2] [Production of silica particles] The ion-exchanged silica sol (SiO 2 The SiO2 solution (concentration: 5% by mass, average particle size: 12 nm) was placed in an autoclave and aged at 200°C for 24 hours with stirring. 2 The converted concentration was 5% by mass, and the average particle size was 12 nm.

[0194] Surface treatment of particles with organosilicon compounds The silica sol aged product in an amount equivalent to 8 g in terms of solid content, 0.8 g of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 160 g of methanol were mixed together in the same manner as in Example 1 to prepare a dispersion of silica particles in MIBK. The solid content at this time was 16.0% by mass, and SiO 2 The converted concentration was 14.0% by mass, and the moisture content was 0.2% by mass.

[0195] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of silica particles was used, and the properties thereof were evaluated.

[0196] [Comparative Example 3] [Production of silica alumina particles] 800 g of silica alumina sol (JGC Catalysts and Chemicals, Cataloid USBB-120, oxide equivalent concentration 12.5 mass%, alumina fraction 25 mass%, average particle size 25 nm) was added to 1200 g of pure water and mixed. Next, 200 g of cation exchange resin (Mitsubishi Chemical, SK-1BH) was added and stirred until the pH became 4.0. Next, the ion exchange resin was separated to obtain an ion-exchanged silica alumina sol (silica alumina equivalent concentration 5 mass%, average particle size 25 nm).

[0197] Surface treatment of particles with organosilicon compounds A surface treatment of particles was carried out in the same manner as in Example 1, except that 50 g of this ion-exchanged silica-alumina sol, 0.8 g of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 500 g of methanol were mixed to produce an MIBK dispersion of silica-alumina particles. The solid content was 2.0% by mass, the silica-alumina equivalent concentration was 1.8% by mass, and the moisture content was 0.2% by mass.

[0198] A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that the MIBK dispersion of silica-alumina particles was used, and the properties thereof were evaluated.

[0199] [Comparative Example 4] [Production of Ag-loaded silica-alumina particles] 800 g of silica alumina sol (Cataloid USBB-120 manufactured by JGC Catalysts and Chemicals Co., Ltd., oxide equivalent concentration 12.5 mass%, alumina fraction 25 mass%, average particle size 5 nm) was added to 1200 g of pure water and mixed. Next, 200 g of cation exchange resin (SK-1BH manufactured by Mitsubishi Chemical Corporation) was added and stirred until the pH became 4.0. Next, the ion exchange resin was separated to obtain an ion-exchanged silica alumina sol (silica alumina equivalent concentration 5 mass%, average particle size 25 nm).

[0200] Next, 100 g of an aqueous solution of silver nitrate containing 1% by mass of Ag and 28.8% aqueous ammonia were added to 100 g of this ion-exchanged silica-alumina sol, and the pH was adjusted to 10, followed by aging at 98° C. for 6 hours.

[0201] Next, the mixture was concentrated to 50 g using an ultrafiltration membrane, and then the filtrate was drained and washed with 2000 g of pure water while continuously adding the water. 2 An O-supported silica alumina sol was obtained. The solid content concentration at this time was 3.0 mass % (including 1.5 mass % in terms of Ag concentration in the solid content) and the pH was 7.4.

[0202] Next, 100 g of this solution was concentrated to 50 g using an ultrafiltration membrane. The oxide-equivalent concentration of this aqueous dispersion was 1.82 mass %, Ag 2 The O concentration was 0.06 mass % (Ag concentration was 2 mass %).

[0203] Surface treatment of particles with organosilicon compounds This Ag 2 50 g of the O-supported silica alumina sol, 0.8 g of a silane coupling agent (KBM403 manufactured by Shin-Etsu Chemical Co., Ltd.), and 500 g of methanol were mixed and kept in a thermostatic bath at 50° C. for 24 hours while stirring.

[0204] The mixture was then concentrated to 50 g using an ultrafiltration membrane.

[0205] The filtrate was removed while continuously adding 800 g of methanol to the mixture, and the solvent was replaced with methanol. The solid content of the methanol-substituted product was 3.0% by mass, and the water content was 0.3% by mass.

[0206] Next, 50 g of this methanol-substituted product was placed in an eggplant-shaped flask, 150 g of methyl isobutyl ketone (MIBK) was added, and the flask was attached to a rotary evaporator. While reducing the pressure, the solvent was replaced with MIBK in a water bath at 80°C, and Ag 2 A dispersion of O-supported silica-alumina particles in MIBK was prepared. The solid content was 2.0% by mass, the oxide equivalent concentration was 1.82% by mass, and Ag was 1.0% by mass.2 The O concentration was 0.06 mass % (2 mass % in terms of Ag concentration), and the moisture content was 0.2 mass %.

[0207] This Ag 2 A coating solution and a substrate with a coating were produced in the same manner as in Example 1, except that a dispersion of O-supported silica alumina particles in MIBK was used, and the properties thereof were evaluated.

[0208] [Table 2]

Claims

1. Particles containing an oxide of a metal element, the particles include proton-donating functional groups; The particles have a proton donating ability of 0.1 to 30 mmol / g per unit gram of the particles.

2. 2. The particle according to claim 1, wherein the metal element comprises at least one selected from the group consisting of Sb, Mo, Sn, Nb, Zr, and W.

3. 3. The particle according to claim 1, wherein the content of the metal element is 20 to 100 mass % on an oxide basis.

4. The proton donating functional group is -SO 3 OH, -SO 3 H, -PO 3 OH, -OPO(OH) 2 2. The particle according to claim 1, characterized in that the group is at least one selected from the group consisting of --COOH and --OH.

5. 2. The particle of claim 1, having an alkali metal content of less than 1000 ppm on an oxide basis.

6. 2. The particles according to claim 1, characterized in that the average particle size is 1 to 100 nm.

7. 2. The particle of claim 1, wherein the particle comprises an organosilicon compound having a functional group.

8. A step 1 of preparing a first solution containing a heteropolyacid salt containing at least one metal element; Step 2: deionizing the first solution to produce a second solution; A step 3 of heating the second solution; A method for producing particles, comprising:

9. 9. The method for producing particles according to claim 8, wherein the metal element is at least one metal element selected from the group consisting of Sb, Mo, Sn, Nb, Zr, and W.

Citation Information

Patent Citations

  • Composition for use in antistatic film formation

    JP2007106936A

  • Antimicrobial agent

    JP1995033616A

  • Photocatalyst, photocatalyst composition, building material for interior, coating, synthetic resin molding, fiber, method for using photocatalyst and method for decomposing hazardous material

    JP2007090336A

  • Antibacterial zeolite particle and antibacterial resin composition

    JP2008001557A

  • Antibacterial titanium oxide powder and method for producing the same

    JP2021031450A