Abrasive pad, method for producing abrasive pad, and method for polishing surface of optical material or semiconductor material
By integrating an inert heat storage agent with specific heat storage particles and microspheres into the polishing layer, the polishing pad stabilizes the polishing surface temperature and maintains a consistent polishing rate, addressing the temperature fluctuations and rate variations in existing polishing technologies.
Patent Information
- Application Number
- JP2023052671
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing polishing pads for semiconductor and optical materials fail to effectively suppress the increase in temperature of the polishing surface during polishing, leading to fluctuations in polishing rate due to chemical reactions and mechanical friction, which affects the quality of the polished surface.
Incorporating a heat storage agent that is inert to isocyanate, hydroxyl, and amino groups into the polishing layer, with specific heat storage particles and microspheres, to absorb and maintain the polishing surface temperature, thereby stabilizing the polishing rate.
The polishing pad effectively suppresses the increase in polishing surface temperature and maintains a stable polishing rate by absorbing heat, ensuring precise and consistent polishing results.
Smart Images

Figure 2024141175000004 
Figure 2024141175000005 
Figure 2024141175000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad, a method for manufacturing a polishing pad, and a method for polishing the surface of an optical material or a semiconductor material. The polishing pad of the present invention is used for polishing optical materials, semiconductor wafers, semiconductor devices, hard disk substrates, etc., and is particularly suitable for polishing devices in which an oxide layer, a metal layer, etc. is formed on a semiconductor wafer. [Background technology]
[0002] Polishing of semiconductor devices and the like is generally performed by the so-called chemical mechanical polishing method (CMP). CMP is a technology that obtains a smooth polished surface by utilizing the action of the chemical components contained in the abrasive (hereinafter referred to as slurry) and the mechanical action caused by the relative movement between the object to be polished and the polishing pad.
[0003] In such a polishing operation, the polishing pad is pressed against the workpiece to be polished while the slurry is supplied, and it is known that as polishing proceeds, heat from processing (heat from chemical reaction and frictional heat) accumulates on the polishing surface of the polishing layer, causing the polishing surface temperature to rise. When the polishing surface temperature rises, the slurry is heated, the chemical action becomes stronger, and there is a problem that the polishing rate becomes too high (overpolishing). In addition, when the polishing surface temperature of the polishing layer rises, there is a problem that the physical properties of the polishing pad change, causing a change in the polishing rate.
[0004] In addition, polishing pads used for polishing semiconductor devices and the like have a polishing layer made of synthetic resin such as polyurethane, and voids are formed inside the polishing layer. The voids are open on the surface of the polishing layer, and during polishing, the abrasive grains contained in the slurry are held in the open holes on the surface of the polishing layer, so that the polishing of the object to be polished progresses. As one method for forming voids inside the polishing layer, a method of mixing microspheres in resin is known, and in recent years, studies have been made to make the voids (openings) smaller and more uniform in order to achieve more precise polishing.
[0005] Patent Document 1 discloses that in a polishing pad manufacturing method using a mechanical foaming method, the bubble diameter can be uniformly controlled by mixing a heat storage agent having a melting point of 70 to 110°C and containing a hydroxyl group or a urethane group into the raw material. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-235416 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the method for producing a polishing pad described in Patent Document 1, a non-coated (non-encapsulated) heat storage agent having a hydroxyl group or a urethane group is mixed into the raw material to prevent bubble expansion by mechanical foaming during the production process. Therefore, the heat storage agent in Patent Document 1 reacts with an isocyanate compound or an active hydrogen-containing compound during the production process of the polishing pad, and therefore it cannot be expected to suppress the rise in the polishing surface temperature during polishing. As described above, there is a demand for a polishing pad that can suppress an increase in the temperature of the polishing surface of the polishing layer during polishing.
[0008] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a polishing pad that can suppress an increase in the temperature of the polishing surface of the polishing layer during polishing, a method for manufacturing such a polishing pad, and a method for polishing the surface of an optical material or a semiconductor material using such a polishing pad. Another object of the present invention is to provide a polishing pad or the like that can suppress an increase in the temperature of the polishing surface of the polishing layer during polishing, as well as maintain the polishing rate during polishing (suppress fluctuations in the polishing rate). [Means for solving the problem]
[0009] As a result of intensive research to solve the above problems, the inventors have found that the above problems can be solved by adding a specific heat storage agent to the polishing layer, and have completed the present invention. Specific aspects of the present invention are as follows.
[0010] [1] A polishing pad having a polishing layer, The polishing pad, wherein the polishing layer contains a heat storage agent that is inactive to an isocyanate group, a hydroxyl group, and an amino group. [2] The polishing pad according to [1], wherein the melting point of the heat storage agent is 20 to 37°C. [3] The polishing pad according to [1] or [2], wherein the heat storage agent includes heat storage particles having a core portion containing a heat storage material and a shell portion. [4] The polishing pad according to [3], wherein the heat storage particles have an average particle size (D50) of 2 to 20 μm. [5] The polishing pad according to any one of [1] to [4], wherein the polishing layer further contains microspheres. [6] The polishing pad according to [5], wherein the microspheres have an average particle size (D50) of 10 to 20 μm. [7] The polishing pad according to any one of [1] to [6], wherein the polishing layer further contains a polyurethane resin. [8] The polishing pad according to [7], wherein the polyurethane resin is a cured product of a curable resin composition containing an isocyanate-terminated urethane prepolymer, a curing agent, and the heat storage agent. [9] A method for producing a polishing pad according to any one of [1] to [8], (a) preparing a curable resin composition containing the heat storage agent; (b) injecting the curable resin composition into a mold; and (c) curing the curable resin composition in the mold. A method for producing the polishing pad comprising the steps of:
[10] A method for polishing a surface of an optical or semiconductor material, comprising the steps of: The method includes a step of polishing a surface of an optical material or a semiconductor material using a polishing pad having a polishing layer containing a heat storage agent under a temperature condition equal to or higher than the melting point of the heat storage agent.
[11] The method according to
[10] , wherein the polishing pad is the polishing pad according to any one of [1] to [8].
[0011] (definition) In this specification, when a numerical range is expressed using "X to Y", the range includes the numerical values X and Y at both ends. Effect of the Invention
[0012] The polishing pad of the present invention can suppress the increase in the temperature of the polishing surface of the polishing layer during polishing. In some cases, the polishing pad of the present invention can not only suppress the increase in the temperature of the polishing surface of the polishing layer, but also maintain the polishing rate during polishing (can suppress fluctuations in the polishing rate). [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a heat storage particle. [Diagram 2] FIG. 2 is a schematic diagram showing the cross-sectional state of a polishing layer in a method for polishing the surface of an optical material or a semiconductor material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (action) The present inventors have intensively studied the relationship between the composition of the polishing layer and the increase in the polishing surface temperature of the polishing layer during polishing, and as a result, unexpectedly found that the increase in the polishing surface temperature can be suppressed by adding a heat storage agent that is inactive to isocyanate groups, hydroxyl groups, and amino groups to the polishing layer. Although the details of why such characteristics are obtained are not clear, it is considered that the heat storage agent is inactive to isocyanate groups, hydroxyl groups, and amino groups, and does not react with other components contained in the polishing layer (e.g., isocyanate-terminated urethane prepolymer, curing agent), and therefore can exist in the polishing layer without impairing the structure and mobility of the heat storage agent. Therefore, it is presumed that the heat storage agent in the polishing layer can absorb the polishing heat generated during polishing and convert it into the energy of phase change of the heat storage agent, thereby keeping the polishing surface temperature of the polishing layer constant. For the type of heat storage agent having a shell portion described later, the heat storage material exists inside the particles dispersed in the polymer component in the polishing layer. On the other hand, in the case of a non-coated type heat storage material having no shell portion, it is presumed that the heat storage material forms island components and the polymer component and the like form a sea-island structure in the polishing layer.
[0015] The polishing pad of the present invention, the method for producing the polishing pad, and the method for polishing the surface of an optical material or a semiconductor material will be described below.
[0016] 1. Polishing pad The polishing pad of the present invention is 1. A polishing pad having a polishing layer, The polishing layer contains a heat storage agent that is inactive to an isocyanate group, a hydroxyl group, and an amino group.
[0017] (Heat storage agent that is inactive to isocyanate groups, hydroxyl groups, and amino groups) A heat storage agent (latent heat storage agent) is a substance that absorbs or releases thermal energy when it undergoes a phase change (from solid to liquid, liquid to solid, etc.). While a phase change is occurring, the thermal energy is in a state that is not expressed as temperature (latent heat), and the temperature of the substance remains constant. For example, when a solid heat storage agent changes phase to liquid (melts), it absorbs the energy of the surroundings. By using a heat storage agent, it is possible to suppress changes in the surrounding temperature and maintain a constant temperature.
[0018] The heat storage agent in the present invention is inactive (non-reactive) to isocyanate group, hydroxyl group, and amino group. Therefore, as described above, the heat storage agent does not react with other components (e.g., isocyanate-terminated urethane prepolymer, curing agent) contained in the polishing layer, and therefore it is considered that the structure and mobility of the heat storage agent are not impaired and the heat storage agent can exist in the polishing layer.
[0019] The melting point (also called melting point or phase change temperature) of the heat storage agent is not particularly limited, but is preferably -5 to 42°C, more preferably 10 to 40°C, and most preferably 20 to 37°C. If the melting point of the heat storage agent is equal to or lower than the polishing surface temperature of the polishing layer, the heat storage agent melts and becomes liquid during polishing, and does not flow out of the pores of the polishing layer and have an adverse effect on polishing, which is preferable. The preferable polishing surface temperature varies depending on the polishing process, but is often about room temperature (20°C) to 40°C, so it is most preferable to set the melting point of the heat storage agent to 20 to 37°C.
[0020] The type of the heat storage agent is not particularly limited, but examples thereof include normal paraffin, fatty acid ester, aliphatic ketone, aliphatic alcohol, aliphatic ether, etc. These compounds can be used alone or in combination of two or more kinds. A typical heat storage agent is paraffin such as normal paraffin. Paraffin has the general formula C n H 2n+2 It is a general term for saturated hydrocarbons having the above structure. The phase change temperature can be controlled by changing the carbon number of the above hydrocarbons. The above hydrocarbons may be either straight-chain or branched, but straight-chain hydrocarbons are preferred because they have a large amount of latent heat. In the polishing pad of this embodiment, the heat storage agent may leak from the surface of the polishing pad during polishing, so the heat storage agent preferably contains a component that does not affect the chemical reaction of polishing.
[0021] The content of the heat storage agent in the entire polishing layer or the entire cured product of the curable resin composition described below is not particularly limited, but is preferably 0.1 to 20% by weight, more preferably 1 to 10% by weight, and most preferably 2 to 5% by weight. When the content of the heat storage agent is within the above numerical range, the temperature rise of the polishing layer during polishing can be suppressed. If the content of the heat storage agent is less than 0.1% by weight, a sufficient heat absorbing effect cannot be obtained, and if the content is more than 20% by weight, the components of the heat storage material may adversely affect the polishing performance. The content of the heat storage agent in the entire polishing layer or the entire cured product of the curable resin composition described below can be considered to be equal to the content of the heat storage agent in the entire uncured curable resin composition.
[0022] <Heat storage particles> The heat storage agent is not particularly limited, but may comprise or consist of heat storage particles having a core portion containing a heat storage material and a shell portion. The heat storage particles present in the polishing layer of the polishing pad absorb the processing heat generated on the surface of the polishing pad as polishing proceeds, thereby suppressing an increase in the temperature of the polishing surface. On the other hand, when the heat storage material exposed on the polishing surface reaches a temperature equal to or higher than the melting point, it becomes liquid and is discharged to the outside together with the slurry. In this case, the part of the heat storage particle after the heat storage material is discharged (the shell part) functions as a surface recess that holds the slurry.
[0023] The heat storage particles are capsule-type particles in which a heat storage material or the like is enclosed within a shell. 1 is a cross-sectional view showing an example of a heat storage particle. The heat storage particle 10 has a core portion 12 containing a heat storage substance and a shell portion 14 that covers the core portion 12. The heat storage particle may have an outermost layer on the outside of the shell portion as necessary, as long as the effect of the present invention is not impaired.
[0024] The average particle size (D50) of the heat storage particles is not particularly limited, but is preferably 0.5 to 200 μm, more preferably 1 to 20 μm, and most preferably 2 to 10 μm. If the average particle diameter (D50) of the heat storage particles is equal to or greater than the lower limit of the above range, the heat storage capacity of the heat storage particles is sufficiently large. In addition, the heat storage material in the core is unlikely to bleed out even when the particles are repeatedly heated and cooled. In addition, the mechanical strength of the shell is increased, making the shell less likely to be damaged by compression or the like. When the average particle size (D50) of the heat storage particles is equal to or less than the upper limit of the above numerical range, the heat storage particles function as openings for retaining the polishing slurry after the heat storage material flows out during polishing. The average particle size (D50, median diameter) can be measured using a laser diffraction particle size distribution measuring device (for example, Mastersizer 2000, manufactured by Spectris Co., Ltd.).
[0025] The shape of the heat storage particles may be a perfect sphere, a partially distorted sphere, a potbellied shape, a cylindrical shape, a cone shape, a rectangular parallelepiped shape, or the like. The content of the heat storage material in the heat storage particles is preferably 30 to 99.9 mass%, more preferably 50 to 99 mass%, and even more preferably 70 to 99 mass%, of 100 mass% of the heat storage particles, from the viewpoint of the mechanical strength of the shell portion and the heat storage amount of the core portion. The thickness of the shell portion is preferably 0.1 to 20 μm, and more preferably 0.5 to 10 μm, from the viewpoints of the mechanical strength and thermal conductivity of the shell portion.
[0026] (Core) The core portion contains a heat storage material. The core portion may contain other components as necessary within the range not impairing the effects of the present invention.
[0027] Examples of heat storage materials include (i) materials that undergo a change of state (phase transition) from liquid to solid or vice versa within the temperature range in which the heat storage material is used, (ii) materials that have a high specific heat (the amount of heat required to raise the temperature of a material by a unit amount) within the temperature range in which the heat storage material is used, and (iii) materials that undergo chemical changes involving the intake and exhaust of heat within the temperature range in which the heat storage material is used.
[0028] (i) An abrasive layer containing heat storage particles using a heat storage material becomes a latent heat storage material that utilizes the latent heat (transition heat) associated with a phase transition, and can store the transition heat as thermal energy or extract the thermal energy as transition heat. (ii) The polishing layer containing heat storage particles using a heat storage material becomes a sensible heat storage material that utilizes the specific heat of the material and can store and extract the amount of heat required to change the temperature of the material. The polishing layer containing heat storage particles using the heat storage material (iii) serves as a chemical heat storage material that utilizes the transfer of heat that accompanies chemical changes in the material.
[0029] As the heat storage material, the heat storage material (i) is preferred because it has a higher heat storage density than sensible heat storage materials, the temperature at which heat is supplied and absorbed is constant, and it is easier to control the supply and absorption of heat than chemical heat storage materials, and it is possible to obtain a latent heat storage material that is stable and safe. As the heat storage material, an organic compound is preferred from the viewpoint of easiness in producing heat storage particles by the production method described below, and an organic material that is liquid at the temperature during production is more preferred. As the heat storage material, at least one selected from the group consisting of saturated hydrocarbons (paraffins), fatty acids, fatty acid metal salts, fatty acid esters, aliphatic ethers, aliphatic ketones, and aliphatic alcohols is preferred, since it is possible to obtain a latent heat storage material with a large heat storage capacity and the heat storage particles are easy to produce.
[0030] As the saturated hydrocarbon, a saturated hydrocarbon having a carbon number of 7 to 60 is preferable because the phase transition temperature is useful as the temperature at which the heat storage material is used. As the saturated hydrocarbon, a straight-chain saturated hydrocarbon is preferred because it has a large latent heat. Saturated hydrocarbons are classified into (a) relatively low molecular weight saturated hydrocarbons and (b) relatively high molecular weight petroleum waxes.
[0031] Since the phase transition temperature is useful as the temperature at which the heat storage material is used, the carbon number of the saturated hydrocarbon (a) is preferably 7 to 24, and more preferably 11 to 20. The carbon number of the saturated hydrocarbon (a) may be appropriately selected from the above range depending on the temperature at which the heat storage material is used. The saturated hydrocarbon (a) may be linear or branched, and linear saturated hydrocarbons are preferred because they have a large latent heat. As the saturated hydrocarbon (a), those having a melting point in the temperature range of -20 to 50°C are preferred in order to broaden the usable temperature range of the heat storage material. The melting point is an extrapolated melting initiation temperature (Tim) at the crystalline melting peak when measured by a differential scanning calorimeter (DSC) in accordance with JIS K 7121. As the saturated hydrocarbon (a), n-undecane (-21°C), n-dodecane (-12°C), n-tridecane (-5°C), n-tetradecane (6°C), n-pentadecane (9°C), n-hexadecane (18°C), n-heptadecane (21°C), n-octadecane (28°C), n-nonadecane (32°C), n-icosane (37°C), n-henicosane (41°C), and n-docosane (46°C) are preferred. The temperatures in parentheses are melting points.
[0032] From the viewpoints of latent heat and availability, the petroleum wax (b) is preferably one having a carbon number of 20 or more. Examples of the petroleum wax (b) include paraffin wax and microcrystalline wax. Paraffin wax is a saturated hydrocarbon that is solid at room temperature and is produced by separating and refining the distillate from vacuum distillation using petroleum or natural gas as a raw material. From the viewpoints of latent heat amount and availability, paraffin wax having a carbon number of 20 to 40 is preferred. Commercially available paraffin wax products include HNP-9, HNP-51, FNP-0090, and FT115 manufactured by Nippon Seiro Co., Ltd. Microcrystalline wax is a saturated hydrocarbon that is solid at room temperature and is produced by separating and refining vacuum distillation residue oil or heavy distillate oil using petroleum as a raw material. As the microcrystalline wax, those having 30 to 60 carbon atoms are preferred from the viewpoints of latent heat amount and availability.
[0033] As the fatty acid, a fatty acid having 8 to 30 carbon atoms is preferred because the phase transition temperature is useful as the temperature at which the heat storage material is used. The fatty acid may be any of linear saturated fatty acid, linear unsaturated fatty acid, branched saturated fatty acid and branched unsaturated fatty acid, with linear saturated fatty acid being preferred because of its large latent heat. Examples of straight-chain saturated fatty acids include octanoic acid, nonanoic acid, decanoic acid (capric acid), dodecanoic acid (lauric acid), tetradecanoic acid (myristic acid), hexadecanoic acid (palmitic acid), octadecanoic acid (stearic acid), eicosanoic acid, docosanoic acid, tetracosanoic acid, hexacosanoic acid, octacosanoic acid, and triacontanoic acid. Examples of fatty acid metal salts include lithium 12-hydroxystearate and aluminum 2-ethylhexanoate.
[0034] Examples of fatty acid esters include butyl lactate, ethyl lactate, methyl oleate, diethyl succinate, ethyl decanoate, methyl decanoate, methyl tetradecanoate, methyl hexadecanoate, methyl octadecanoate, methyl eicosanoate, methyl behenate, butyl dodecanoate, n-hexadecyl palmitate, and stearyl stearate. As the aliphatic ether, a fatty acid ether having 14 to 60 carbon atoms is preferred, since the phase transition temperature is useful as the temperature at which the heat storage material is used. Examples of the aliphatic ether include heptyl ether, octyl ether, tetradecyl ether, and hexadecyl ether. From the viewpoints of large latent heat and ease of synthesis, ethers having one oxygen atom and a symmetrical structure are preferred. Examples of the aliphatic ketones include 2-octanone, 3-octanone, 2-nonanone, 3-nonanone, and cycloheptanone. The aliphatic alcohol is preferably an aliphatic alcohol having 8 to 60 carbon atoms, since the phase transition temperature corresponds to the useful temperature at which the heat storage material is used. As the aliphatic alcohol, a primary alcohol is preferred because it has a large latent heat. Examples of the aliphatic alcohol include 2-dodecanol, 1-tetradecanol, 7-tetradecanol, 1-octadecanol, 1-eicosanol, and 1,10-decanediol.
[0035] The heat storage material is preferably made of saturated hydrocarbons; or a combination of at least one selected from the group consisting of fatty acid esters, aliphatic ketones, aliphatic alcohols and aliphatic ethers with a fatty acid or a fatty acid metal salt. The heat storage material may be used alone or in combination of two or more. From the viewpoint of increasing the amount of latent heat at a specific temperature, it is preferable to use one alone or in combination of two types, and from the viewpoint of widening the range of temperatures at which the heat storage material can be used, it is preferable to use two or more types in combination, and it is more preferable to use three or more types in combination.
[0036] Other components that may be contained in the core portion include resins, rubbers, fillers, functional agents, inevitable impurities, and the like. Examples of the filler include metals, metal compounds, carbon materials, glasses, minerals, and the like. Examples of functional agents include antioxidants, antistatic agents, weather resistance agents, UV absorbers, antiblocking agents, crystal nucleating agents, flame retardants, vulcanizing agents, vulcanization assistants, antibacterial and antifungal agents, dispersants, color prevention agents, foaming agents, rust inhibitors, heavy metal deactivators, and melting point adjusters (freezing point depressants). The content of the other components is preferably 10 parts by mass or less, more preferably 3 parts by mass or less, and particularly preferably 0 part by mass, per 100 parts by mass of the heat storage material.
[0037] (Shell part) The shell portion may contain or consist of a polymer, but is not particularly limited thereto. The shell portion may contain other components as necessary, as long as the effects of the present invention are not impaired. From the viewpoint of maintaining the shape from mixing of the raw materials to curing, the shell part preferably has a heat resistance temperature of 100° C. or more, and more preferably has a heat resistance temperature of 150° C. or more. Here, the heat resistance temperature refers to the temperature obtained in a heat resistance test according to the JIS standard (JIS S 2029), and means the temperature obtained by subtracting 10° C. from the temperature at which functional abnormality or significant deformation occurs.
[0038] The polymer forming the shell portion may include or consist of a melamine resin, an acrylic resin, a urethane resin, or a combination of two or more of these.
[0039] Examples of components other than the polymer that may be contained in the shell portion include rubber, fillers, functional agents, and inevitable impurities. The content of the other components is preferably 10 parts by mass or less, more preferably 3 parts by mass or less, and particularly preferably 0 part by mass, based on 100 parts by mass of the polymer.
[0040] (outermost layer) The outermost layer that the heat storage particle may have is a layer that imparts functions such as heat resistance, solvent resistance, and water resistance to the heat storage particle. The material constituting the outermost layer may be a thermoplastic resin, a cured product of a curable resin, an inorganic compound, etc. Some examples include:
[0041] (microsphere) The abrasive layer may further include microspheres. The microspheres may be hollow particles. The microspheres may be a component other than the heat storage agent. The microspheres are not particularly limited, but examples thereof include unexpanded heat-expandable microspheres having an outer shell (polymer shell) made of a thermoplastic resin and a low-boiling point hydrocarbon encapsulated in the outer shell, spheres obtained by heating and expanding the unexpanded heat-expandable microspheres, and combinations thereof.
[0042] The average particle size (D50) of the microspheres is not particularly limited, but is preferably 5 to 40 μm, more preferably 7 to 30 μm, and most preferably 10 to 20 μm. When the average particle size (D50) of the microspheres is within the above numerical range, the object to be polished can be polished more precisely. The average particle size (D50, median diameter) can be measured using a laser diffraction particle size distribution measuring device (e.g., Mastersizer 2000, manufactured by Spectris Co., Ltd.).
[0043] As the polymer forming the polymer shell, a thermoplastic resin such as polyvinyl alcohol, polyvinylpyrrolidone, poly(meth)acrylic acid, polyacrylamide, polyethylene glycol, polyhydroxyether acrylate, maleic acid copolymer, polyethylene oxide, polyurethane, poly(meth)acrylonitrile, polyvinylidene chloride, polyvinyl chloride, and organic silicone resins, as well as copolymers of two or more of the monomers constituting these resins (e.g., acrylonitrile-vinylidene chloride copolymer, acrylonitrile-methyl methacrylate copolymer, vinyl chloride-ethylene copolymer, etc.) can be used. Among these, it is preferable to use an acrylonitrile-methyl methacrylate copolymer in terms of achieving the effects described in this specification. The low-boiling point hydrocarbon encapsulated in the polymer shell may be, for example, isobutane, pentane, isopentane, petroleum ether, or a combination of two or more of these.
[0044] The content of the microspheres in the entire polishing layer or the entire cured product of the curable resin composition described below is not particularly limited, but is preferably 0.1 to 10% by weight, more preferably 1 to 5% by weight, and most preferably 2 to 4% by weight. When the content of the microspheres is within the above numerical range, the density of the polishing layer is made uniform. The content of the microspheres in the entire polishing layer or the entire cured product of the curable resin composition described below can be considered to be equal to the content of the microspheres in the entire uncured curable resin composition.
[0045] (Open hole) In the polishing pad of this embodiment, open pores may be present on the surface of the polishing layer. The pores present on the surface of the polishing layer are not particularly limited, but can be the pores caused by the heat storage agent, the pores caused by the microspheres, the pores formed by chemical foaming and / or mechanical foaming, or a combination of two or more of them.Among these, the combination of the pores caused by the heat storage agent and the pores caused by the microspheres improves the retention ability of polishing slurry. If the temperature conditions in the polishing step are equal to or higher than the melting point of the heat storage agent (heat storage substance), the heat storage agent becomes liquid and flows out during polishing, leaving behind openings formed by the heat storage agent (openings corresponding to the remaining shell parts when the above-mentioned capsule-type heat storage particles are used).The openings formed by the heat storage agent can be regarded as openings caused by the heat storage agent. The chemical foaming may be, for example, a method of generating carbon dioxide from an isocyanate compound by adding water, while the mechanical foaming may be a method of mechanically stirring and mixing an inert gas such as air, nitrogen, oxygen, carbon dioxide, helium, or argon into a foamable curable composition.
[0046] The average pore size on the surface of the polishing layer is not particularly limited, but is preferably 5 to 20 μm, more preferably 8 to 18 μm, and most preferably 10 to 15 μm. When the average pore size is within the above numerical range, the object to be polished can be polished more precisely. The average pore size on the surface of the polishing layer can correspond to the average particle size (D50) of the heat storage agent, or to both the average particle size (D50) of the heat storage agent and the average particle size (D50) of the microspheres.
[0047] The average pore size on the surface of the abrasive layer can be calculated by binarizing an image obtained using a laser microscope with image processing software.
[0048] (polishing layer) The polishing pad of the present invention has a polishing layer. The polishing layer is disposed in a position in direct contact with the material to be polished, and the other parts of the polishing pad may be made of a material for supporting the polishing pad, for example, a material having high elasticity such as rubber. Depending on the rigidity of the polishing pad, the polishing layer can be made into a polishing pad.
[0049] The polishing pad of the present invention has no significant difference in shape from a general polishing pad, except that it can suppress the rise in the temperature of the polishing surface of the polishing layer during polishing, and can be used in the same way as a general polishing pad.For example, the polishing pad can be rotated while the polishing layer is pressed against the material to be polished, or the material to be polished can be rotated while being pressed against the polishing layer to polish it.
[0050] The polishing pad of the present invention can be produced by a commonly known manufacturing method such as molding or slab molding. First, the polishing layer is directly molded as a molded product of polyurethane resin or the like by those manufacturing methods, and then laminated to a support or the like. Alternatively, a block of polyurethane resin or the like is formed by those manufacturing methods, and the block is sliced or the like to form a sheet-like polishing layer, which is then laminated to a support or the like. Alternatively, the polishing layer can be molded directly on the support.
[0051] More specifically, a double-sided tape is attached to the surface of the polishing layer opposite to the polishing surface of the polishing layer, and the polishing pad is cut into a predetermined shape. There is no particular limitation on the double-sided tape, and any double-sided tape known in the art can be selected and used. In addition, the polishing pad may be a single-layer structure consisting of only the polishing layer, or may be a multi-layer structure in which other layers (lower layer, support layer) are attached to the surface of the polishing layer opposite to the polishing surface.
[0052] The polishing layer may further include a polyurethane resin. The polyurethane resin is not particularly limited, but may be a cured product of a curable resin composition containing an isocyanate-terminated urethane prepolymer, a curing agent, and the heat storage agent. The polishing layer can be formed by preparing a curable resin composition containing an isocyanate-terminated urethane prepolymer, a curing agent, and the above-mentioned heat storage agent, and foaming and curing the curable resin composition. The curable resin composition may be, for example, a two-liquid composition prepared by mixing liquid A containing an isocyanate-terminated urethane prepolymer with liquid B containing a curing agent component. Other components may be added to liquid A or liquid B, but if problems arise, the composition may be divided into multiple liquids and mixed to form a composition consisting of three or more liquids.
[0053] (Isocyanate-terminated urethane prepolymer) The isocyanate-terminated urethane prepolymer may be a product obtained by reacting a polyol component with a polyisocyanate component.
[0054] (Polyol component) As the polyol component, a low molecular weight polyol, a high molecular weight polyol, or a combination thereof can be used. In this specification, a low molecular weight polyol is a polyol having a number average molecular weight of 30 to 300, and a high molecular weight polyol is a polyol having a number average molecular weight of more than 300. The number average molecular weights of the high molecular weight polyol and the low molecular weight polyol can be measured as polyethylene glycol / polyethylene oxide (PEG / PEO) molecular weights based on gel permeation chromatography (GPC) under the following conditions. <Measurement conditions> Column: Ohpak SB-802.5HQ (exclusion limit 10000) + SB-803HQ (exclusion limit 100000) Mobile phase: 5mM LiBr / DMF Flow rate: 0.3ml / min (26kg / cm 2 ) Oven: 60℃ Detector: RI 40℃ Sample volume: 20 μl
[0055] Examples of the low molecular weight polyol include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, neopentyl glycol, pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, and combinations of two or more of these.
[0056] Examples of the high molecular weight polyol include Polyether polyols such as polytetramethylene ether glycol (PTMG), polyethylene glycol, and polypropylene glycol; polyester polyols such as the reaction product of ethylene glycol with adipic acid and the reaction product of butylene glycol with adipic acid; Polycarbonate polyols; polycaprolactone polyols; or a combination of two or more thereof.
[0057] (Polyisocyanate component) Examples of the polyisocyanate component include: m-phenylene diisocyanate, p-phenylene diisocyanate, 2,6-tolylene diisocyanate (2,6-TDI), 2,4-tolylene diisocyanate (2,4-TDI), Naphthalene-1,4-diisocyanate, Diphenylmethane-4,4'-diisocyanate (MDI), 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI), 3,3'-dimethoxy-4,4'-biphenyl diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, Xylylene-1,4-diisocyanate, 4,4'-diphenylpropane diisocyanate, Trimethylene diisocyanate, Hexamethylene diisocyanate, Propylene-1,2-diisocyanate, butylene-1,2-diisocyanate, Cyclohexylene-1,2-diisocyanate, Cyclohexylene-1,4-diisocyanate, p-phenylene diisothiocyanate, Xylylene-1,4-diisothiocyanate, ethylidine diisothiocyanate, or a combination of two or more thereof. Among these, from the viewpoint of polishing properties, it is preferable to use tolylene diisocyanates such as 2,6-tolylene diisocyanate (2,6-TDI) and 2,4-tolylene diisocyanate (2,4-TDI).
[0058] The NCO equivalent (g / eq) of the isocyanate-terminated urethane prepolymer is preferably less than 600, more preferably 350 to 550, and most preferably 400 to 500. The NCO equivalent (g / eq) is within the above numerical range, so that the polishing layer can exhibit an appropriate hardness. The NCO equivalent (g / eq) is calculated by "(parts by mass of polyisocyanate compound + parts by mass of polyol compound) / [(number of functional groups per molecule of polyisocyanate compound x parts by mass of polyisocyanate compound / molecular weight of polyisocyanate compound)-(number of functional groups per molecule of polyol compound x parts by mass of polyol compound / molecular weight of polyol compound)]", and is a numerical value indicating the molecular weight of the prepolymer per NCO group.
[0059] (hardening agent) The curing agent contained in the curable resin composition may, for example, be an amine-based curing agent described below. Examples of polyamines constituting the amine-based curing agent include diamines, such as alkylenediamines such as ethylenediamine, propylenediamine, and hexamethylenediamine; diamines having an aliphatic ring such as isophoronediamine and dicyclohexylmethane-4,4'-diamine; diamines having an aromatic ring such as 3,3'-dichloro-4,4'-diaminodiphenylmethane (also known as methylenebis-o-chloroaniline) (hereinafter abbreviated as MOCA); diamines having a hydroxyl group such as 2-hydroxyethylethylenediamine, 2-hydroxyethylpropylenediamine, di-2-hydroxyethylethylenediamine, di-2-hydroxyethylpropylenediamine, 2-hydroxypropylethylenediamine, and di-2-hydroxypropylethylenediamine, particularly hydroxyalkylalkylenediamines; or combinations of two or more of these. Also usable are trifunctional triamine compounds and polyamine compounds having four or more functional groups.
[0060] A particularly preferred amine-based curing agent is the above-mentioned MOCA, the chemical structure of which is as follows:
[0061] [ka]
[0062] The total amount of the curing agent is such that the ratio of the number of moles of active hydrogen groups (such as NH2) in the curing agent to the number of moles of NCO in the isocyanate-terminated urethane prepolymer (number of moles of active hydrogen groups / number of moles of NCO) is preferably 0.70 to 1.10, more preferably 0.80 to 1.00, and most preferably 0.85 to 0.95.
[0063] (Other Ingredients) In addition, catalysts and the like that are generally used in the industry may be added to the curable resin composition. The polyisocyanate component can also be added later to the curable resin composition. The weight ratio of the additional polyisocyanate component to the total weight of the isocyanate-terminated urethane prepolymer and the additional polyisocyanate component is preferably 0.1 to 10.0% by weight, more preferably 0.5 to 8.0% by weight, and particularly preferably 1.0 to 5.0% by weight. As the polyisocyanate component additionally added to the polyurethane resin curable composition, the above-mentioned polyisocyanate components can be used without particular limitation, but 4,4'-methylene-bis(cyclohexyl isocyanate) (hydrogenated MDI) is preferred.
[0064] 2. Manufacturing method of polishing pad The method for producing a polishing pad of the present invention comprises the steps of: A method for producing the polishing pad described in 1 above, (a) preparing a curable resin composition containing the heat storage agent; (b) injecting the curable resin composition into a mold; and (c) curing the curable resin composition in the mold. A method for producing the polishing pad comprising the steps of:
[0065] The characteristics of the heat storage agent, the composition of the curable resin composition, the content, etc. may be the same as those described in 1 above.
[0066] Step (a) may include a step of mixing the heat storage agent, the isocyanate-terminated urethane prepolymer, and the curing agent. The isocyanate-terminated urethane prepolymer and the curing agent may be the same as the isocyanate-terminated urethane prepolymer and the curing agent described in 1 above.
[0067] The temperature of the mold in step (b) is preferably 100° C. or less or 90° C. or less to prevent the curable resin composition from curing before being cast into a mold.
[0068] As in Examples 1 to 3 described later, step (b) can be a primary curing step performed inside a mold, and after the primary curing step, the formed resin foam can be extracted from the mold and the resin foam can be secondary cured. Even in this case, the pores of the resulting polishing pad are formed in step (b) (primary curing), so the characteristics of the pores in the polishing pad are mainly determined by the conditions in step (b).
[0069] The temperature condition of the primary curing step is not particularly limited, but is preferably 75 to 100° C., more preferably 75 to 95° C., and most preferably 75 to 92° C. The time of the primary curing step is not particularly limited, but is preferably 5 minutes to 1 hour, more preferably 5 minutes to 40 minutes, and most preferably 10 minutes to 30 minutes. The temperature conditions for the secondary curing step are not particularly limited, but are preferably 80 to 140° C., more preferably 90 to 130° C., and most preferably 100 to 120° C. The time for the secondary curing step is not particularly limited, but is preferably 1 to 6 hours, more preferably 1 to 5 hours, and most preferably 1 to 4 hours. During secondary curing, since the heat storage particles are present in the cured resin, even if the secondary curing temperature exceeds the heat resistance temperature of the shell part, there is little possibility that the heat storage particles will deform, but it is more preferable to set the secondary curing temperature to the heat resistance temperature of the shell part or lower.
[0070] In step (c), the cured product obtained by curing the curable resin composition in the mold may be used as it is as the polishing layer. In this case, the shape of the mold needs to correspond to the polishing layer, and the method of this embodiment does not include the step of processing the cured product of the curable resin composition to form the polishing layer. By not including such a step of forming the polishing layer, there is no risk of the heat storage agent becoming liquid and leaking during the process, as described later, so this is preferable. On the other hand, step (c) may further include a step of processing the cured product of the curable resin composition obtained by curing in a mold to form an abrasive layer. An example of such a forming step is a molding method (slicing step) in which a block-shaped cured product is sliced (cut) to obtain an abrasive layer. When performing such a step of processing the cured product to form an abrasive layer, it is preferable to perform the step at a temperature below the melting point of the heat storage agent so that the heat storage agent does not become liquid and leak.
[0071] The polishing pad described above in 1 can be obtained by the method for producing a polishing pad of the present invention.
[0072] 3. Method for polishing the surface of an optical material or a semiconductor material The method for polishing a surface of an optical material or a semiconductor material of the present invention comprises the steps of: The method includes a step of polishing the surface of an optical material or a semiconductor material using a polishing pad having a polishing layer containing a heat storage agent under a temperature condition equal to or higher than the melting point of the heat storage agent.
[0073] The characteristics of the heat storage agent, such as its composition, content, melting point, polishing layer, and polishing pad, may be the same as those described in 1 above.
[0074] The temperature conditions in the process of polishing the surface of an optical material or a semiconductor material are equal to or higher than the melting point of the heat storage agent. As a result, during polishing, the heat storage agent becomes liquid and flows out together with the slurry from the openings on the surface of the polishing layer, enabling precise polishing without adversely affecting the polishing. In addition, since the temperature conditions are equal to or higher than the melting point of the heat storage agent, during polishing, the heat storage agent becomes liquid and flows out, leaving openings formed by the heat storage agent (openings corresponding to the remaining shell parts when the above capsule-type heat storage particles are used), enabling more precise polishing. The temperature conditions in the step of polishing the surface of an optical material or a semiconductor material are not particularly limited, but are preferably 0 to 50° C., more preferably 15 to 45° C., and most preferably 25 to 40° C. By keeping the temperature conditions within the above numerical ranges, precise polishing can be achieved without adversely affecting the polishing.
[0075] In the method for polishing the surface of an optical material or semiconductor material of this embodiment, the polishing pad described in 1 above can be used as the polishing pad.
[0076] FIG. 2 shows an example of a schematic diagram illustrating the cross-sectional state of a polishing layer in a method for polishing the surface of an optical material or a semiconductor material. The polishing layer includes microcapsules 21 and microspheres (hollow particles) 30 that contain a heat storage material 22 therein.
[0077] Fig. 2(a) shows the state before the microcapsules 21 are exposed to the polishing surface, Fig. 2(b) shows the state immediately after the microcapsules 21 are exposed to the polishing surface, and Fig. 2(c) shows the state after sufficient time has passed since the microcapsules 21 were exposed to the polishing surface. As the workpiece is polished with the polishing pad, the surface of the polishing layer is worn away, and as polishing progresses, the state of the polishing layer changes in the order of Fig. 2(a), (b), and then Fig. 2(c).
[0078] As shown in Fig. 2(b), as polishing progresses, the heat generated on the polishing surface is absorbed by the heat storage material 22 in the microcapsules 21 (A in Figs. 2(b) and (c)). If the temperature conditions in the polishing process are equal to or higher than the melting point of the heat storage agent (heat storage material), the heat storage agent becomes liquid during polishing and flows out of the openings in the surface of the polishing layer together with the slurry, allowing precise polishing without adversely affecting the polishing. In addition, openings formed by the heat storage agent (openings corresponding to the remaining shell parts when the above-mentioned capsule-shaped heat storage particles are used) remain, allowing more precise polishing (B in Fig. 2(b)). In the method of polishing the surface of an optical material or a semiconductor material of this embodiment, the step of polishing the surface of the optical material or semiconductor material may include or consist of a step of proceeding with polishing to expose the heat storage agent or the heat storage particles on the surface of the polishing layer, a step of melting the heat storage agent or the heat storage substance in the heat storage particles to make it liquid and forming openings caused by the heat storage agent or openings corresponding to the shell portion in the polishing layer, a step of polishing through the openings caused by the heat storage agent or the openings corresponding to the shell portion, or a combination of two or more of these steps.
[0079] The method of polishing the surface of an optical or semiconductor material can further include, but is not limited to, applying a slurry to the surface of the polishing pad, the surface of the optical or semiconductor material, or both.
[0080] (slurry) The liquid component contained in the slurry is not particularly limited, but may be water (pure water), acid, alkali, organic solvent, or a combination thereof, and may be selected depending on the material of the workpiece to be polished, the desired polishing conditions, etc. The slurry is preferably mainly composed of water (pure water), and preferably contains 80% by weight or more of water based on the entire slurry. The abrasive component contained in the slurry is not particularly limited, but may be silica, zirconium silicate, cerium oxide, aluminum oxide, manganese oxide, or a combination thereof. The slurry may contain other components, such as organic matter soluble in the liquid component and a pH adjuster. EXAMPLES
[0081] The present invention will be experimentally described by the following examples, but the following description is not intended to limit the scope of the present invention to the following examples.
[0082] (material) The materials used in Examples 1 to 3 and Comparative Example 1 described below are listed below.
[0083] Isocyanate-terminated urethane prepolymer: Prepolymer (1) A urethane prepolymer having an NCO equivalent of 455, which contains 2,4-tolylene diisocyanate as a polyisocyanate component, polytetramethylene ether glycol having a number average molecular weight of 650 and polytetramethylene ether glycol having a number average molecular weight of 1000 as high molecular weight polyol components, and diethylene glycol as a low molecular weight polyol component.
[0084] Hardener: MOCA ··· 3,3'-dichloro-4,4'-diaminodiphenylmethane (also known as methylenebis-o-chloroaniline) (MOCA) (NH2 equivalent = 133.5)
[0085] Heat storage material: Heat storage agent (1)···PMCD-28 (Miki Riken Kogyo Co., Ltd.) (heat storage particles having a core containing a heat storage material and a shell, heat storage material: paraffin, shell: melamine, melting point of heat storage material: about 28°C, average particle size (D50): 2 to 10 μm, slurry-like, heat storage component: about 30% by weight, ionicity: anionic) Heat storage agent (2) AMC-28SP (Miki Riken Kogyo Co., Ltd.) (heat storage particles having a core containing a heat storage material and a shell, heat storage material: paraffin, shell: acrylic, melting point of heat storage material: about 28°C, average particle size (D50): about 5 μm, powder form, heat storage component: about 65% by weight)
[0086] ·Microspheres: Microsphere (1)... Expancel (registered trademark) 461DU20 (Nippon Fillite Co., Ltd.) (unexpanded type, average particle size (D50) in unexpanded state: 6 to 9 μm, expansion start temperature: 100 to 106°C, maximum expansion temperature: 143 to 151°C, shell composition: acrylonitrile-vinylidene chloride copolymer)
[0087] Example 1 As component A, 100g of prepolymer (1) was prepared, as component B, 26.3g of MOCA, the hardener, as component B, 4.0g of heat storage agent (1) as component C, and 2.7g of microspheres (1) as component D. Note that the amounts are listed in grams to show the ratio of each component, but it is sufficient to prepare the required weight (parts) depending on the size of the molded product. The amounts below will also be listed in grams (parts). Components A, C, and D were mixed, and the resulting mixture of components A, C, and D was degassed under reduced pressure. Also, MOCA, which is component B, was degassed under reduced pressure. The degassed mixture of components A, C, and D and the degassed component B were fed to a mixer to obtain a mixed solution of components A to D. In the obtained mixed solution of components A to D, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) is 0.9. The content of heat storage agent (1) of component C in the entire mixed solution is 3% by weight, and the content of microspheres (1) of component D in the entire mixed solution is 2% by weight. The obtained mixed liquid of components A to D was poured into a mold (circular shape with a diameter of 800 mm, depth of 1.3 mm) heated to 80°C. After pouring, the mixed liquid in the mold was primarily cured at 95°C for 20 minutes to obtain a resin foam. The obtained resin foam was removed from the mold and secondary cured in an oven at 100°C for 4 hours. Double-sided tape was attached to the back surface of the obtained resin foam (circular shape with a diameter of 800 mm, thickness of 1.3 mm) (corresponding to the polishing layer) to obtain a polishing pad.
[0088] Example 2 A resin foam was produced in the same manner as in Example 1, except that 4.0 g of the heat storage agent (2) was used instead of 4.0 g of the heat storage agent (1) as component C, to obtain a polishing pad of Example 2. In the obtained mixed solution of components A to D, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) is 0.9. The content of heat storage agent (2) of component C in the entire mixed solution is 3% by weight, and the content of microspheres (1) of component D in the entire mixed solution is 2% by weight.
[0089] Example 3 A resin foam was prepared in the same manner as in Example 2, except that 3.9 g of the heat storage agent (2) as component C was used instead of 4.0 g of the heat storage agent (2) as component C and 2.7 g of the microspheres (1) as component D, to obtain the polishing pad of Example 3. In the obtained mixed solution of components A, B, and C, the ratio of the number of moles of NH2 of MOCA of component B to the number of moles of NCO of prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) is 0.9. The content of heat storage agent (2) of component C in the entire mixed solution is 3% by weight.
[0090] Comparative Example 1 A resin foam was prepared in the same manner as in Example 1, except that 3.9 g of the microspheres (1) as component D was used instead of 4.0 g of the heat storage agent (1) as component C and 2.7 g of the microspheres (1) as component D, to obtain a polishing pad of Comparative Example 1. In the obtained mixture of components A, B, and D, the ratio of the number of moles of NH2 in MOCA of component B to the number of moles of NCO in prepolymer (1) of component A (number of moles of NH2 / number of moles of NCO) was 0.9. The content of microspheres (1) of component D in the entire mixture was 3% by weight.
[0091] (Evaluation method) The following measurements of (1) the polishing rate variation rate and (2) the polishing surface temperature were carried out for each of the polishing pads of Examples 1 to 3 and Comparative Example 1. The measurement results are shown in Table 1 below.
[0092] (1) Average removal rate and removal rate fluctuation rate for all wafers The polishing pad was used to polish 100 TEOS-coated silicon wafers as the workpieces under the polishing conditions described below in (Polishing Test), and the polishing rate (Å) for each wafer was measured as follows. <Measurement of polishing rate>: The silicon wafer with TEOS before and after the polishing test was measured in the diameter direction on the wafer, and the thickness at those points before and after the polishing test was measured. Based on the measured thickness, the average thickness before the polishing test and the average thickness after the polishing test were calculated, and the average polished thickness was calculated by taking the difference between these average values, and this average value was used as the average polishing rate (Å) for each wafer. In addition, the average polishing rate (Å) (Rave) for all wafers was calculated by averaging the average polishing rate (Å) (100 pieces) for each wafer. Furthermore, the maximum value (Rmax) and the minimum value (Rmin) were selected from the average polishing rate (Å) (100 pieces) for each wafer. The thickness was measured using a four-probe sheet resistance measuring device (manufactured by KLA Tencor, product name "RS-200", measurement: DBS mode). Then, the polishing rate fluctuation rate (%) was calculated based on the following formula (1).
[0093]
number
[0094] (Polishing test) Polishing machine used: F-REX300X (manufactured by Ebara Corporation) Disk: A188 (3M) Retainer ring: Retainer ring GXKD (manufactured by Ebara Corporation) Polishing platen rotation speed: 90 rpm Polishing head rotation speed: 81 rpm Grinding pressure: 3.2psi Polishing slurry: PL-6115 (manufactured by Fujimi Corporation) Polishing slurry flow rate: 200ml / min Polishing time: 60 seconds Workpiece: Silicon wafer with TEOS (Tetra Ethyl Ortho Silicate) (disk shape with a diameter of 300 mm) Pad break: 32N 20min Conditioning: In-situ 18N 16 scans, Ex-situ 32N 4 scans
[0095] (2) Polishing surface temperature When polishing 100 TEOS-attached silicon wafers in the above "(1) Polishing rate", the surface temperature of the polishing layer of the polishing pad was continuously measured by a radiation thermometer (manufactured by Ebara Corporation) attached to the polishing machine. The average value of the obtained surface temperatures of the polishing layer was calculated and used as the polishing surface temperature of the polishing layer.
[0096] [Table 1]
[0097] Examples 1 to 3 relate to polishing pads having a polishing layer containing a heat storage agent that is inactive to isocyanate groups, hydroxyl groups, and amino groups, while Comparative Example 1 relates to a polishing pad having a polishing layer that does not contain a heat storage agent that is inactive to isocyanate groups, hydroxyl groups, and amino groups. The results in Table 1 show that the polishing pads of Examples 1 to 3 had small fluctuations in the polishing rate and low polishing surface temperatures. On the other hand, it was found that the polishing pad of Comparative Example 1 had a large fluctuation rate of the polishing rate and a high polishing surface temperature. The above results are believed to be due to the endothermic effect of the heat storage agent contained in the polishing layer of the polishing pads of Examples 1 to 3, which suppresses the rise in the temperature of the polishing surface, and as a result, the fluctuation range of the polishing rate fluctuation rate was able to be kept small compared to the polishing pad of Comparative Example 1. Furthermore, the average polishing rate for all wafers of the polishing pads of Examples 1 to 3 was not significantly different from the average polishing rate for all wafers of the polishing pad of Comparative Example 1, indicating that the flow of the heat storage agent into the slurry had almost no effect on the polishing rate.
[0098] From the above results, it was found that the polishing pad having a polishing layer containing a heat storage agent inactive to isocyanate groups, hydroxyl groups, and amino groups of the present invention can suppress the increase in the polishing surface temperature of the polishing layer during polishing. In addition, it was found that the polishing pad can not only suppress the increase in the polishing surface temperature of the polishing layer, but also maintain the polishing rate during polishing (suppress the fluctuation of the polishing rate). [Explanation of symbols]
[0099] 10...Heat storage particles 12…Core section 14…Shell part 21...Microcapsules 22...Heat storage substance 30...Microsphere (hollow particle)
Claims
1. 1. A polishing pad having a polishing layer, The polishing pad, wherein the polishing layer contains a heat storage agent that is inactive to an isocyanate group, a hydroxyl group, and an amino group.
2. 2. The polishing pad according to claim 1, wherein the heat storage agent has a melting point of 20 to 37°C.
3. 3. The polishing pad according to claim 1, wherein the heat storage agent comprises heat storage particles having a core portion containing a heat storage substance and a shell portion.
4. 4. The polishing pad according to claim 3, wherein the heat storage particles have an average particle size (D50) of 2 to 20 μm.
5. The polishing pad of claim 1 or 2, wherein the polishing layer further comprises microspheres.
6. 6. The polishing pad according to claim 5, wherein the microspheres have an average particle size (D50) of 10 to 20 μm.
7. The polishing pad according to claim 1 or 2, wherein the polishing layer further comprises a polyurethane resin.
8. 8. The polishing pad according to claim 7, wherein the polyurethane resin is a cured product of a curable resin composition comprising an isocyanate-terminated urethane prepolymer, a curing agent, and the heat storage agent.
9. A method for producing the polishing pad according to claim 1 or 2, comprising the steps of: (a) preparing a curable resin composition containing the heat storage agent; (b) injecting the curable resin composition into a mold; and (c) curing the curable resin composition in the mold. The method for producing the polishing pad includes the steps of:
10. 1. A method for polishing a surface of an optical or semiconductor material, comprising the steps of: The method includes a step of polishing a surface of an optical material or a semiconductor material using a polishing pad having a polishing layer containing a heat storage agent under a temperature condition equal to or higher than the melting point of the heat storage agent.
11. The method of claim 10, wherein the polishing pad is the polishing pad of claim 1 or 2.
Citation Information
Patent Citations
Method for manufacturing polishing pad
JP2011235416A