Piezoelectric laminate, method for manufacturing piezoelectric laminate, and piezoelectric element
A two-stage formation process for KNN films with high (001) orientation and low stress addresses high film stress and dielectric issues, resulting in a spontaneously polarized laminate suitable for sensitive piezoelectric sensors without additional treatment.
Patent Information
- Application Number
- JP2023052799
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing piezoelectric KNN films face challenges with high film stress, which leads to structural deformation and reduced manufacturing yield, and are either spontaneously polarized or have high dielectric constants, necessitating additional polarization treatment.
A method involving the formation of a KNN film in two stages, where the first layer is formed at a temperature ensuring a high (001) orientation rate and low film stress, followed by a second layer to achieve spontaneous polarization, resulting in a film with a dielectric constant of 490 or less and film stress of 150 MPa or less.
The solution provides a piezoelectric laminate with a spontaneously polarized film that does not require additional polarization treatment, has low dielectric constant, and low film stress, enhancing the reliability and sensitivity of piezoelectric elements for sensor applications.
Smart Images

Figure 2024141259000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, and a piezoelectric element. [Background technology]
[0002] Piezoelectric bodies are widely used in functional electronic components such as sensors and actuators. One of the materials used for piezoelectric bodies is a KNN-based ferroelectric material containing potassium, sodium, niobium, and oxygen, and a laminate has been proposed that has a piezoelectric film (KNN film) made using such a piezoelectric body. For example, Patent Document 1 discloses a KNN film, which is a spontaneous polarization film that can obtain sufficient piezoelectric displacement without polarization treatment, that is, a KNN film, which is a hysteresis curve that shows the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under specified conditions to the KNN film, and has a coercive electric field E C + and the coercive field E on the negative field side C - The KNN film has a median coercive electric field between the KNN film and the electrode, the median value being 10.8 kV / cm or more. Patent Document 1 also discloses that the relative dielectric constant of the KNN film can be reduced by generating spontaneous polarization in the KNN film.
[0003] In addition, the piezoelectric film is required to have a small film stress (internal stress). For example, Patent Document 2 discloses a technique in which the lower electrode film, which is the base of the KNN film, is made of platinum (Pt), and the grain size of the crystal grains constituting the lower electrode film is controlled to be uniform to reduce the surface unevenness of the lower electrode film, thereby easing the stress at the interface with the KNN film and reducing the film stress of the KNN film to 1.6 GPa or less. Patent Document 2 also discloses a technique in which the film stress of the KNN film is controlled (reduced) to 1.6 GPa or less by performing a heat treatment after the formation of the KNN film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-207429 A [Patent Document 2] JP 2011-029591 A Summary of the Invention [Problem to be solved by the invention]
[0005] The KNN film obtained by the technique of the above-mentioned Patent Document 1 is a spontaneous polarization film that can obtain sufficient piezoelectric displacement without polarization treatment and has a low relative dielectric constant, but has a large film stress. On the other hand, the KNN film obtained by the technique of the above-mentioned Patent Document 2 is a film with low film stress, but is not a spontaneous polarization film.
[0006] An object of the present disclosure is to provide a piezoelectric laminate having a piezoelectric film that is a spontaneous polarization film, has a relative dielectric constant of 490 or less, and has a film stress of 150 MPa or less, and contains potassium, sodium, niobium, and oxygen. [Means for solving the problem]
[0007] According to one aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive field E on the negative field side C - The median value of the coercive field between The piezoelectric film has a relative dielectric constant of 490 or less, The piezoelectric laminate and the piezoelectric element are provided, wherein the piezoelectric film has a film stress of 150 MPa or less.
[0008] According to another aspect of the present disclosure, forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; The method for manufacturing a piezoelectric laminate provides a process for forming the piezoelectric film, in which a first piezoelectric film, which is a part of the piezoelectric film, is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneous polarization film. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a piezoelectric laminate having a piezoelectric film that is a spontaneous polarization film, has a relative dielectric constant of 490 or less, and a film stress of 150 MPa or less, and contains potassium, sodium, niobium, and oxygen. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing an example of a cross-sectional structure of a piezoelectric laminate according to an embodiment of the present disclosure. [Diagram 2] 1A and 1B are diagrams illustrating an example of a structure of a simplified piezoelectric element according to an embodiment of the present disclosure. [Diagram 3] FIG. 1 is a diagram showing an example of a schematic configuration of a piezoelectric element according to an embodiment of the present disclosure. [Figure 4] 1 is a diagram illustrating an example of a schematic configuration of a piezoelectric device module according to an embodiment of the present disclosure. [Diagram 5] 1 shows the polarization value-electric field hysteresis curve (PE hysteresis curve) of Sample 3. [Figure 6] PE hysteresis curve of Sample 9. [Figure 7] FIG. 1A is a diagram showing an example of a schematic configuration of a simple unimorph cantilever fabricated using each sample, and FIG. 1B is a diagram illustrating a method for measuring the amount of piezoelectric displacement. [Figure 8] 13(a) to 13(e) are graphs showing the results of evaluation of the necessity of polarization treatment using simplified piezoelectric elements produced from Sample 3. FIG. [Figure 9] 13(a) to 13(e) are graphs showing the results of evaluation of the necessity of polarization treatment using simplified piezoelectric elements produced from sample 9. [Figure 10] 4(a) and 4(b) are graphs showing the evaluation results regarding the temperature resistance of spontaneous polarization using a simplified piezoelectric element made from Sample 1. [Figure 11] 13(a) and 13(b) are graphs showing the evaluation results regarding the temperature resistance of spontaneous polarization using a simplified piezoelectric element made from Sample 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <Knowledge gained by the inventors> In the above-mentioned Patent Document 1, when a KNN film is formed on a substrate such as a silicon (Si) substrate by sputtering, the KNN film is formed at a low temperature to realize a spontaneously polarized KNN film (hereinafter also referred to as a "spontaneously polarized KNN film"). The spontaneously polarized KNN film has the advantage that it does not require a polarization process required for the piezoelectric operation of the KNN film as a piezoelectric film. A laminate having a spontaneously polarized KNN film is particularly advantageous when applied to sensor applications. However, the spontaneously polarized KNN film realized in Patent Document 1 has a large film stress. Note that when the temperature during sputtering film formation is low, the film stress generated in the KNN film tends to be a compressive stress, and when the temperature during sputtering film formation is high, the film stress generated in the KNN film tends to be a tensile stress. When the film stress of the KNN film is large, for example, when the film stress of the KNN film is more than 150 MPa, large structural deformation occurs when a piezoelectric element such as a membrane structure or a cantilever structure is manufactured. As a result, the manufactured piezoelectric element does not function properly. In addition, the manufacturing yield of piezoelectric elements and piezoelectric device modules decreases. For this reason, it is required to suppress the film stress of the KNN film to a low level, for example, to suppress the film stress of the KNN film to 150 MPa or less.
[0012] The inventors of the present invention have conducted extensive research to develop a KNN film that has three characteristics that have not been realized so far: a spontaneous polarization film, a low dielectric constant, and a low film stress. As a result, the following five findings were obtained. (First finding) The film stress of the KNN film obtained by sputtering depends greatly on the conditions at the initial stage of the KNN film formation. (Second finding) First, a KNN film is deposited as the first layer (initial layer) under temperature conditions that result in small film stress (at the beginning of film deposition), and then a KNN film is deposited as the second layer on the first layer under temperature conditions that result in the KNN film becoming a spontaneous polarization film. This significantly reduces the film stress of the entire KNN film (the laminate of the first and second layers) even when the KNN film (second layer) is deposited at a low temperature that would normally result in large film stress. (Third finding) In order to obtain a KNN film with a low relative dielectric constant with good reproducibility, it is necessary to increase the (001) orientation rate of the KNN film. To obtain a KNN film with a high (001) orientation rate, it is usually necessary to set the deposition temperature of the KNN film within a certain range. By depositing a KNN film as the first layer under temperature conditions that increase the (001) orientation rate in the early stages of deposition, and then depositing a KNN film as the second layer on the first layer under temperature conditions that make the KNN film a spontaneous polarization film, a KNN film with a high (001) orientation rate can be obtained even if the KNN film (second layer) is deposited at a low temperature that would normally decrease the (001) orientation rate. The (001) orientation rate of the KNN film is the orientation rate of the crystals that make up the KNN film in the (001) plane direction, and will be described in detail later. (Fourth finding) For example, in order to reproducibly obtain a KNN film having a relative dielectric constant of 490 or less, the (001) orientation rate of the KNN film must be 90% or more. By depositing a KNN film as the first layer under conditions that give a (001) orientation rate of 95% or more in the early stages of deposition, a KNN film with a (001) orientation rate of 90% or more can be obtained even when a KNN film as the second layer is subsequently deposited at a low temperature. (Fifth finding) In the early stages of film formation, a KNN film is formed as the first layer under conditions that reduce the film stress and increase the (001) orientation rate. Then, a KNN film is formed as the second layer on the first layer under temperature conditions that make the KNN film a spontaneous polarization film. This makes it possible to realize a KNN film that is a spontaneous polarization film, has a low dielectric constant, and small film stress, i.e., has all three of the above characteristics.
[0013] Based on the above five findings, the inventors have found that a KNN film that is a spontaneous polarization film, has a film stress of 150 MPa or less, and a dielectric constant of 490 or less, can be obtained by depositing a KNN film as a first layer under temperature conditions at the beginning of the film deposition such that the film stress is 100 MPa or less and the (001) orientation rate is 95% or more, and then depositing a KNN film as a second layer under temperature conditions such that the KNN film becomes a spontaneous polarization film.
[0014] The present disclosure has been made based on the above-mentioned problems and findings obtained by the present inventors.
[0015] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described with reference to the drawings.
[0016] (1) Structure of the piezoelectric laminate As shown in FIG. 1, a laminate (laminate substrate) 10 having a piezoelectric film according to this embodiment (hereinafter also referred to as piezoelectric laminate 10) comprises a substrate 1, a lower electrode film 2 deposited on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 deposited on the lower electrode film 2, and an upper electrode film 4 deposited on the piezoelectric film 3.
[0017] As the substrate 1, a single crystal silicon (Si) substrate 1a on which a surface oxide film (SiO2 film) 1b such as a thermal oxide film or a CVD (Chemical Vapor Deposition) oxide film is formed, that is, a Si substrate having a surface oxide film, can be suitably used. As the substrate 1, a Si substrate 1a having an insulating film formed of an insulating material other than SiO2 instead of the surface oxide film 1b can also be used. As the substrate 1, a Si substrate 1a on which the Si(100) face or Si(111) face or the like is exposed on the surface, that is, a Si substrate having no surface oxide film 1b or insulating film can also be used. As the substrate 1, a SOI (Silicon On Insulator) substrate or a quartz glass (SiO2) substrate can also be used. The thickness of the single crystal Si substrate 1a can be, for example, 300 μm or more and 1000 μm or less, and the thickness of the surface oxide film 1b can be, for example, 1 nm or more and 4000 nm or less.
[0018] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film formed using Pt is also referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including the case where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the Pt film is oriented in the (111) plane direction. The Pt film being oriented in the (111) plane direction means that no peaks other than those due to the (111) plane are observed in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measured on the surface of the piezoelectric film 3. Thus, it is preferable that the main surface of the lower electrode film 2 (the surface serving as the base of the piezoelectric film 3) is composed of a Pt (111) plane. The lower electrode film 2 can be formed by a method such as a sputtering method or a vapor deposition method. The material of the lower electrode film 2 may be, other than Pt, various metals such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys mainly composed of these metals, or metal oxides such as strontium ruthenate (SrRuO3, abbreviated as SRO) or lanthanum nickelate (LaNiO3, abbreviated as LNO). When the lower electrode film 2 is formed using a metal oxide, it is preferable that the crystals constituting the lower electrode film 2 are preferentially oriented in the (001) plane direction with respect to the surface of the substrate 1. The lower electrode film 2 may be a single layer film formed using the above-mentioned various metals, alloys mainly composed of the above-mentioned various metals, or metal oxides. The lower electrode film 2 may be a laminate of a Pt film and a film mainly composed of SRO provided on the Pt film, or a laminate of a Pt film and a film mainly composed of LNO provided on the Pt film. The thickness of the lower electrode film 2 (if the lower electrode film 2 is a laminate, the total thickness of each layer) can be, for example, 100 nm or more and 400 nm or less.
[0019] An adhesive layer 6 may be provided between the substrate 1 and the lower electrode film 2 to enhance their adhesion. The adhesive layer 6 may be, for example, a layer containing zinc (Zn) and oxygen (O) as main components (hereinafter also referred to as a "ZnO layer"). The ZnO layer may be formed using, for example, zinc oxide. The composition ratio of Zn and O constituting the ZnO layer preferably satisfies the relationship Zn:O=1:1, but is not limited thereto and may vary to some extent. The ZnO layer is a polycrystalline layer. The ZnO layer is preferably such that its (0001) plane is parallel to the main surface of the substrate 1 (including the case where the (0001) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the ZnO layer is preferably oriented in the (0001) plane direction. The ZnO layer being oriented in the (0001) plane direction means that the intensity of the peak due to the (0002) plane is high in the X-ray diffraction pattern obtained by XRD measured on the surface of the piezoelectric film 3. Thus, the main surface of the ZnO layer (the surface serving as the base of the lower electrode film 2) is preferably composed of a ZnO (0001) surface. The ZnO layer can be formed by a method such as sputtering or vapor deposition. The thickness of the ZnO layer can be, for example, 1 nm to 200 nm, preferably 10 nm to 50 nm. As the adhesion layer 6, for example, a layer mainly composed of titanium (Ti), tantalum (Ta), titanium oxide (TiO2), nickel (Ni), ruthenium oxide (RuO2), iridium oxide (IrO2), or the like may be provided. Such an adhesion layer 6 can also be formed by a method such as sputtering or vapor deposition, and the thickness of the adhesion layer 6 can be, for example, 1 nm to 200 nm, preferably 10 nm to 50 nm. In this specification, the adhesion layer 6 provided between the substrate 1 and the lower electrode film 2 is sometimes referred to as the lower adhesion layer 6.
[0020] The piezoelectric film 3 is a film formed of, for example, an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O). In other words, the piezoelectric film 3 is a film whose main component is an alkali niobium oxide containing K, Na, Nb, and O. The piezoelectric film 3 is a film having a composition formula (K 1-x Na x)It can be formed using an alkali niobium oxide represented by NbO3, that is, potassium sodium niobate (KNN). The coefficient x [=Na / (K + Na)] in the above composition formula can be in the range of 0 < x < 1, preferably 0.4 ≤ x ≤ 0.8. The piezoelectric film 3 is a polycrystalline film of KNN (hereinafter also referred to as the KNN film 3). Also, the crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Further, it is preferable that more than half of the crystals constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is regarded as a tetragonal system. The KNN film 3 can be formed by a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm or more and 5 μm or less, preferably 1 μm or more and 3 μm or less.
[0021] The crystals constituting the KNN film 3 are preferentially oriented in the (001) plane orientation with respect to the main surface of the substrate 1 (when the substrate 1 is, for example, an Si substrate 1a having a surface oxide film 1b or an insulating film, etc., it is the Si substrate 1a). That is, the main surface of the KNN film 3 (the surface that becomes the base of the upper electrode film 4) is mainly composed of the KNN (001) plane. For example, by directly forming the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of the Pt (111) plane, a KNN film 3 whose main surface is mainly composed of the KNN (001) plane can be obtained. In this specification, that the crystals constituting the KNN film 3 are oriented in the (001) plane orientation means that the (001) plane of the crystals constituting the KNN film 3 is parallel or substantially parallel to the main surface of the substrate 1. Also, that the crystals constituting the KNN film 3 are preferentially oriented in the (001) plane orientation means that there are many crystals whose (001) plane is parallel or substantially parallel to the main surface of the substrate 1.
[0022] The alkali niobium oxide constituting the KNN film 3 may be selected from the group consisting of lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), tantalum (Ta), molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), At least one element (dopant) selected from the group consisting of samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), Ni, aluminum (Al), Si, germanium (Ge), tin (Sn), and gallium (Ga) may further be contained. The concentration of these elements in the alkali niobium oxide can be, for example, 5 at% or less (when a plurality of the above elements are contained, the total concentration is 5 at% or less).
[0023] As will be described in detail later, in this embodiment, first, a first KNN film 3a (first piezoelectric film, hereinafter also referred to as "KNN film 3a"), which is a part of the KNN film 3, is deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second KNN film 3b (second piezoelectric film, hereinafter also referred to as "KNN film 3b"), which is the other part of the KNN film 3, is deposited on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. As a result, the KNN film 3 in this embodiment (i.e., a laminate of the KNN film 3a and the KNN film 3b) has all of the characteristics 1 to 3 described later. In addition, the KNN film 3 in this embodiment may further have the characteristic 4 described later.
[0024] Hereinafter, features 1 to 4 that the KNN film 3 of this embodiment can have will be described.
[0025] (Feature 1) The KNN film 3 has a coercive electric field E on the positive electric field side in a hysteresis curve (PE hysteresis curve) that shows the correlation between the polarization amount (P) of the KNN film 3 and the applied electric field (E) obtained by applying an electric field to the KNN film 3 under predetermined conditions. C + and the coercive field E on the negative field side C - The median value of the coercive electric field between the
[0026] The PE hysteresis curve in this embodiment is prepared by, for example, forming an upper electrode film 4 on a KNN film 3 having a thickness of 2 μm, grounding the lower electrode film 2, applying a triangular or sinusoidal (sine wave) electric field of −150 kV / cm to +150 kV / cm (i.e., a triangular or sine wave voltage of −30 V to +30 V) at a frequency of 1 kHz to the KNN film 3 through the upper electrode film 4, measuring the amount of polarization of the KNN film 3, and plotting the obtained amount of polarization. The “coercive field” is a value obtained by measuring the amount of polarization of the KNN film 3 when the amount of polarization is 0 μC / cm. 2 The two electric field values at which the coercive field E C + " means the polarization is 0μC / cm 2 The electric field value on the positive electric field side when C - " means the polarization is 0μC / cm 2 The "median value of the coercive electric field" is the electric field value on the negative electric field side when C + -E C - ) / 2.
[0027] As described above, the KNN film 3 in this embodiment has a feature that the median value of the coercive electric field is a positive value in the PE hysteresis curve. The KNN film 3 having this feature is a spontaneous polarization film (spontaneous polarization KNN film) in which the polarization direction is aligned in a certain direction (e.g., upward).
[0028] The term "spontaneous polarization film" as used herein refers to a KNN film 3 whose polarization direction is spontaneously aligned in a fixed direction (without ever applying an electric field (voltage) via the lower electrode film 2 and the upper electrode film 4 after film formation). In addition, "upward" in this specification refers to the direction from the lower electrode film 2 side toward the upper electrode film 4 side. In addition, "the polarization direction is aligned in a fixed direction" means that the majority (more than half) of the crystals constituting the KNN film 3 are polarized in a fixed direction. For example, "the polarization direction is aligned upward" means that the polarization direction of the majority of the crystals constituting the KNN film 3 is upward.
[0029] In addition, in the case of KNN membranes, which are not spontaneously polarized membranes, the PE hysteresis curve is generally a graph symmetrical about the origin, and the coercive field E C + Absolute value of and coercive field E C - The absolute values of are almost equal. When a piezoelectric element 20, such as a sensor device, is manufactured using a piezoelectric laminate having such a KNN film, a polarization process must be performed during the manufacturing process. The "polarization process" refers to a process in which a large electric field is applied to the KNN film 3 (while heating, if necessary) to align the polarization direction of the KNN film 3 in a certain direction (the direction of the applied electric field).
[0030] Since the KNN film 3 is a spontaneous polarization film, no polarization process is required when the piezoelectric element 20 described below is produced using the piezoelectric laminate 10 having the KNN film 3 of this embodiment.
[0031] The median value of the coercive electric field is preferably 10 kV / cm or more. This allows more of the crystals constituting the KNN film 3 to be polarized in a certain direction (e.g., upward). As a result, the direction of the spontaneous polarization generated in the KNN film 3 (i.e., the polarization direction of the KNN film 3) can be stabilized, and the KNN film 3 that does not require polarization treatment can be reliably obtained.
[0032] The median value of the coercive electric field is preferably 100 kV / cm or less, more preferably 70 kV / cm or less, which can prevent the piezoelectric characteristics (for example, the piezoelectric constant) of the KNN film 3 from deteriorating.
[0033] The polarization characteristics of the KNN film 3 are maintained (not lost) even when the KNN film 3 is exposed to high temperatures, for example, when the KNN film 3 is subjected to a thermal history of 400° C. or more. For example, even when the KNN film 3 is exposed to high temperatures after the formation of the KNN film 3, during the film formation process of the upper electrode film 4, the annealing process, the formation process of the insulating film 8 and the metal wirings 9a and 9b described below (for example, the film formation process of the insulating film 8 by the plasma CVD method or the ALD method, and patterning processing), mounting processing (for example, wire bonding processing, die bonding processing, solder reflow processing), etc., the spontaneous polarization generated in the KNN film 3 is maintained. The inventors have confirmed that the polarization characteristics of the KNN film 3 are maintained without degradation even when the KNN film 3 is subjected to a thermal history of 500° C. The inventors have also confirmed that when the KNN film 3 is subjected to a thermal history of about 600° C., the polarization characteristics of the KNN film 3 deteriorate somewhat, but the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to suitably apply the piezoelectric element 20 (piezoelectric device module 30) described below obtained by processing the piezoelectric laminate 10 having the KNN film 3 to sensor applications. In addition, deterioration in the performance of a sensor fabricated using the piezoelectric element 20 can be avoided.
[0034] (Feature 2) The KNN film 3 further has a characteristic that "the relative dielectric constant is 490 or less."
[0035] Since the dielectric constant of the KNN film 3 is 490 or less, a highly sensitive sensor can be obtained when a piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 is used for a sensor. Note that the lower the dielectric constant of the KNN film 3, the higher the sensitivity of the sensor produced by processing the piezoelectric laminate 10.
[0036] In order to reproducibly (reliably) exhibit this characteristic, the (001) orientation rate of the KNN film 3 must be 90% or more. The (001) orientation rate of the KNN film 3 is the orientation rate of the crystals constituting the KNN film 3 in the (001) plane orientation. "The (001) orientation rate of the KNN film 3 is 90% or more" means that, for example, 90% or more of the crystals constituting the KNN film 3 are oriented in the (001) plane orientation with respect to the main surface of the substrate 1. In this specification, the "orientation rate" is a value calculated by the following formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.
[0037] Orientation rate (%) = {(001) peak intensity / ((001) peak intensity + (110) peak intensity)} × 100 (1)
[0038] The "(001) peak intensity" in the above formula (1) is the intensity of a diffraction peak due to a crystal oriented in the (001) plane direction (i.e., a crystal whose (001) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a 2θ range of 20° to 23°. When multiple peaks appear within a 2θ range of 20° to 23°, it is the intensity of the highest peak. In addition, the "(110) peak intensity" in the above formula (1) is the intensity of a diffraction peak due to a crystal oriented in the (110) plane direction (i.e., a crystal whose (110) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a 2θ range of 30° to 33°. When multiple peaks appear within the 2θ range of 30° to 33°, the intensity is that of the highest peak.
[0039] (Feature 3) The KNN film 3 further has a feature that the film stress is 150 MPa or less.
[0040] By making the film stress of the KNN film 3 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, as described below. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to operate normally.
[0041] (Feature 4) The KNN film 3 may further have the characteristic that "when a negative AC voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film 2 and the upper electrode film 4 (i.e., to the KNN film 3), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of the initial value exceeds 10 million."
[0042] For example, in the case of a piezoelectric laminate 10 having a KNN film 3 with a thickness of 2 μm, when the lower electrode film 2 is grounded and a unipolar triangular or sine wave (sine wave) AC voltage with an amplitude of 0 V to -60 V is continuously applied to the upper electrode film 4 (via the KNN film 3) at a frequency of 300 Hz so that the direction of the electric field applied to the KNN film 3 is not reversed (so that the direction of the electric field is in one direction), the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 falls to 80% or less of its initial value exceeds 10 million.
[0043] In this specification, the term "unipolar electric field" refers to an electric field that is unidirectional even if the magnitude of the voltage applied to the KNN film 3 via the upper electrode film 4 periodically varies within a range of, for example, 0 V to -60 V. In addition, in this specification, "the number of voltage application cycles until the piezoelectric displacement of the KNN film 3 decreases to 80% or less of the initial value when a negative voltage is continuously applied to the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3" is also referred to as "the number of application cycles."
[0044] When an AC voltage is applied to the KNN film 3 via the upper electrode film 4, the KNN film 3 deforms. The higher the applied voltage, the greater the deformation of the KNN film 3. The KNN film 3 in this embodiment can have the characteristic that the amount of piezoelectric displacement is unlikely to decrease even when the KNN film 3 is repeatedly and significantly deformed by continuously applying a large AC voltage, i.e., has excellent AC stress resistance.
[0045] In the piezoelectric laminate 10 obtained by the above-mentioned new method, a KNN film 3a having a high (001) orientation rate and a small film stress, for example, a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less, is interposed between the lower electrode film 2 and the KNN film 3b. As a result, the KNN film 3 in this embodiment (a laminate of the KNN film 3a and the KNN film 3b) can have a superior AC stress resistance compared to a case where the KNN film 3a is not interposed. This is considered to be because the interposition of the KNN film 3a can significantly improve the adhesion between the lower electrode film 2 and the KNN film 3. In this way, the interposition of the KNN film 3a can make the above-mentioned number of application cycles exceed 10 million, that is, the AC stress resistance of the KNN film 3 can be improved, which is a new finding first found as a result of the inventors' intensive research.
[0046] Since the KNN film 3 has excellent AC stress resistance, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10, which will be described later.
[0047] The present inventors have confirmed that in a piezoelectric laminate 10 having a KNN film 3a having a (001) orientation rate of 95% or more and a film stress of 100 MPa or less interposed between a lower electrode film 2 and a KNN film 3b, when a negative voltage is continuously applied to the KNN film 3 via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film 3, the piezoelectric displacement of the KNN film 3 can be maintained at 80% or more of its initial value even after the number of application cycles exceeds 10 million, and even reaches 50 million or more.
[0048] In contrast, when the KNN film 3a is not interposed, that is, when the KNN film 3 is not composed of a laminate of the KNN film 3a and the KNN film 3b, if a large AC voltage is continuously applied to the KNN film 3 via the upper electrode film 4 and the KNN film 3 is continuously and significantly deformed, the KNN film 3 gradually peels off from the lower electrode film 2. As a result, the piezoelectric displacement of the KNN film 3 is easily reduced.
[0049] The inventors have confirmed that in a piezoelectric laminate in which the KNN film 3a is not interposed between the lower electrode film 2 and the KNN film 3b, when a negative voltage is continuously applied to the KNN film via the upper electrode film 4 so as to generate a unipolar AC electric field of 300 kV / cm in the KNN film, the piezoelectric displacement of the KNN film falls to less than 80% of its initial value before the number of application cycles reaches 10 million.
[0050] As described above, the KNN film 3 in this embodiment can have all of the above-mentioned features 1 to 3, and preferably all of the above-mentioned features 1 to 4. When the KNN film 3 has all of the above-mentioned features 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) described below obtained by processing the piezoelectric laminate 10 having the KNN film 3 can be suitably applied to sensor applications. Furthermore, when the KNN film 3 has all of the above-mentioned features 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) described below can be more suitably applied to sensor applications.
[0051] In this embodiment, when the KNN film 3 is formed, the KNN film 3a is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. Therefore, the KNN film 3 in this embodiment has a laminated structure of the KNN film 3a as the first layer (initial layer) formed at the first temperature and the KNN film 3b as the second layer formed at the second temperature.
[0052] The KNN film 3a formed at the first temperature does not have spontaneous polarization. That is, the KNN film 3a is not a spontaneous polarization film. Therefore, when the ratio of the thickness of the KNN film 3a to the total thickness of the KNN film 3 (the total thickness of the KNN film 3a and the KNN film 3b) becomes large, the above-mentioned feature 1 tends to be difficult to be realized. That is, the KNN film 3 tends to be difficult to generate spontaneous polarization. Therefore, it is preferable that the thickness of the KNN film 3a is suppressed to the minimum necessary to relax the film stress of the KNN film 3 and to make the film stress of the entire KNN film 3 150 MPa or less. The thickness of the KNN film 3a is not strictly limited, but is preferably, for example, 20% or less of the total thickness of the KNN film 3. This ensures that the KNN film 3 having the above-mentioned feature 1, that is, the KNN film 3 that is a spontaneous polarization film, can be obtained.
[0053] The upper electrode film 4 is mainly composed of various metals such as Pt, Au, Al, Cu, etc., or alloys thereof. The upper electrode film 4 can be formed by a method such as a sputtering method, a vapor deposition method, a plating method, a metal paste method, etc. The upper electrode film 4 does not have a large effect on the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4 are not particularly limited. In addition, an adhesion layer 7 mainly composed of, for example, RuO2, IrO2, Ti, Ta, TiO2, Ni, etc. may be provided between the KNN film 3 and the upper electrode film 4 in order to improve the adhesion between them. The thickness of the upper electrode film 4 can be, for example, 50 nm to 5000 nm, preferably 50 nm to 300 nm, and when the adhesion layer 7 is provided, the thickness of the adhesion layer 7 can be, for example, 1 nm to 200 nm, preferably 5 nm to 50 nm. In this specification, the adhesion layer 7 provided between the KNN film 3 and the upper electrode film 4 is sometimes referred to as the upper adhesion layer 7.
[0054] (2) Methods for manufacturing piezoelectric laminates, piezoelectric elements, and piezoelectric device modules A method for manufacturing the above-mentioned piezoelectric laminate 10, the piezoelectric element, and the piezoelectric device module will now be described.
[0055] (Deposition of lower adhesive layer and lower electrode film) First, a substrate 1 is prepared, and a lower adhesive layer 6 (e.g., a ZnO layer) and a lower electrode film 2 (e.g., a Pt film) are formed in this order by, for example, a sputtering method on one of the main surfaces of the substrate 1. Note that a substrate 1 on which the lower adhesive layer 6 and the lower electrode film 2 have been formed in advance on one of the main surfaces may be prepared.
[0056] The following conditions are exemplified as conditions for depositing the ZnO layer as the lower adhesion layer 6. The deposition time of the lower adhesion layer 6 is appropriately adjusted depending on the target thickness of the lower adhesion layer 6. Target: ZnO sintered body Temperature (substrate temperature): 200° C. or higher and 700° C. or lower, preferably 300° C. or higher and 700° C. or lower, more preferably 500° C. or higher and 700° C. or lower Discharge power density: 2W / cm 2 More than 6W / cm 2 Less than 3W / cm, preferably 3W / cm 2 More than 5W / cm 2 below Atmosphere: an atmosphere of a mixed gas of argon (Ar) gas and oxygen (O2) gas (hereinafter also referred to as "Ar / O2 mixed gas atmosphere") Ratio of partial pressure of Ar gas to O2 gas (Ar gas partial pressure / O2 gas partial pressure): 5 / 1 to 30 / 1, preferably 7 / 1 to 20 / 1, more preferably 10 / 1 to 15 / 1 Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 10 nm or more and 50 nm or less
[0057] In this specification, when a numerical range is expressed, such as "5 / 1 to 30 / 1," it means that the lower limit and the upper limit are included in the range. The same applies to other numerical ranges.
[0058] The conditions for forming the Ti layer or the like as the lower adhesion layer 6 are exemplified as follows. Target: Ti plate, etc. Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less The other conditions can be the same as those used when providing the ZnO layer.
[0059] The following conditions are exemplified as conditions for depositing a Pt film as the lower electrode film 2. The deposition time of the lower electrode film 2 is appropriately adjusted according to the target thickness of the lower electrode film 2. Target: Pt plate Temperature (substrate temperature): 200°C or higher and 600°C or lower, preferably 300°C or higher and 500°C or lower Discharge power density: 1W / cm 2 More than 5W / cm 2 Less than 2 W / cm, preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 100nm to 400nm
[0060] (KNN membrane production) After the lower adhesive layer 6 and the lower electrode film 2 are formed, the KNN film 3 is formed on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. The composition of the KNN film 3 can be adjusted by controlling the composition of the target used during sputtering. The target can be prepared by mixing K2CO3 powder, Na2CO3 powder, Nb2O5 powder, etc. and firing the mixture. The composition of the target can be controlled by adjusting the mixing ratio of K2CO3 powder, Na2CO3 powder, Nb2O5 powder, etc. When forming the KNN film 3 containing the above elements such as Cu and Mn, a target in which Cu powder (or CuO powder), Mn powder (or MnO powder), etc. are mixed in a predetermined ratio in addition to the above powders may be used.
[0061] The KNN film 3 is formed in two stages by changing the temperature conditions. Specifically, first (at the beginning of the film formation), the KNN film 3a is formed at a first temperature, and then the KNN film 3b is formed at a second temperature.
[0062] The first temperature is a temperature at which the (001) orientation rate of the KNN film 3a is 95% or more and the film stress is 100 MPa or less. For example, the first temperature is a temperature at which the (001) orientation rate of the KNN film 3a is 95% or more when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature. Also, the first temperature is a temperature at which the film stress of the KNN film 3a is 100 MPa or less when the KNN film 3a is formed to a thickness of 2 μm (±10%) at the first temperature.
[0063] The second temperature is a temperature at which the KNN film 3b becomes a spontaneous polarization film, i.e., a temperature at which the median value of the coercive electric field of the PE hysteresis curve becomes a positive value. The second temperature is a temperature at which the KNN film 3b becomes a spontaneous polarization film when the KNN film 3b is deposited at the second temperature to a thickness of 2 μm (±10%).
[0064] Although the first temperature and the second temperature depend somewhat on the sputtering deposition apparatus and deposition conditions, in the sputtering deposition of the KNN film 3 in this embodiment, the second temperature is usually lower than the first temperature (first temperature>second temperature). For example, the first temperature can be in the range of 550°C to 600°C, and the second temperature can be in the range of 400°C to 500°C.
[0065] As conditions other than the temperature when forming the KNN film 3 (KNN film 3a, KNN film 3b), the following conditions are exemplified for both the film formation at the first temperature and the film formation at the second temperature. Discharge power density: 2.7W / cm 2 More than 4.1W / cm 2 Less than or equal to 2.8 W / cm 2 More than 3.8W / cm 2 below Atmosphere: an atmosphere containing at least Ar gas, preferably an Ar / O2 mixed gas atmosphere Ambient pressure: 0.03 Pa or more and 0.5 Pa or less, preferably 0.04 Pa or more and 0.4 Pa or less Ratio of partial pressure of O2 gas to Ar gas (O2 gas partial pressure / Ar gas partial pressure): 0 to 1 / 20, preferably 0 to 1 / 30 Film-forming speed: 0.5 μm / hr or more and 4 μm / hr or less, preferably 0.5 μm / hr or more and 2 μm / hr or less Total thickness of KNN film: 0.5 μm or more and 5 μm or less, preferably 1 μm or more and 3 μm or less
[0066] In addition, "O2 gas partial pressure / Ar gas partial pressure is 0 (zero)" means a state in which the O2 gas partial pressure is 0, that is, the atmosphere is only Ar gas. In addition, "total thickness of KNN film" is the total thickness of the KNN film 3a formed at the first temperature and the KNN film 3b formed at the second temperature. In addition, the deposition time of the KNN film 3a and the KNN film 3b is appropriately adjusted according to the target thickness of the KNN film 3a, 3b. As described above, it is preferable that the thickness of the KNN film 3a is the minimum thickness necessary to reduce the film stress in the KNN film 3b by deposition at the second temperature and to make the film stress of the entire KNN film 3 150 MPa or less. For this reason, it is preferable to adjust the deposition time of the KNN film 3a (deposition time at the first temperature) so that the thickness of the KNN film 3a is 20% or less of the total thickness of the KNN film 3, for example.
[0067] As described above, first, the KNN film 3a is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film. Even if the second temperature is a low temperature at which the (001) orientation rate decreases or a large film stress occurs in the KNN film 3b, the (001) orientation rate of the entire KNN film 3 after the KNN film 3b is formed can be 90% or more, and the film stress of the entire KNN film 3 can be greatly relaxed. As a result, while the KNN film 3 becomes a spontaneous polarization film, the relative dielectric constant of the entire KNN film 3 can be reproducibly set to 490 or less, and the film stress of the entire KNN film 3 can be set to 150 MPa or less. That is, by forming the KNN film 3 (the KNN film 3a and the KNN film 3b) in two stages by changing the temperature under the above-mentioned conditions, the KNN film 3 having all of the above-mentioned characteristics 1 to 3 can be obtained. In addition, by forming the KNN film 3 in two stages by changing the temperature under the above-mentioned conditions, i.e., by providing a KNN film 3a having a high (001) orientation rate and small film stress, a KNN film 3 having all of the above-mentioned characteristics 1 to 4 can be obtained.
[0068] (Deposition of upper adhesive layer and upper electrode film) After the deposition of the KNN film 3 is completed, an upper adhesion layer 7 (eg, a RuO2 layer) and an upper electrode film 4 (eg, a Pt film) are deposited in this order on the KNN film 3 by, for example, a sputtering method.
[0069] The following conditions are exemplified as conditions for depositing a RuO2 layer or the like as the upper adhesion layer 7. The deposition time of the upper adhesion layer 7 is appropriately adjusted according to the target thickness of the upper adhesion layer 7. Target: Ru plate, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 0.3W / cm 2 More than 2W / cm 2 Less than or equal to 0.5 W / cm 2 More than 1W / cm 2 below Atmosphere: Ar / O2 mixed gas atmosphere Ratio of partial pressure of Ar gas to O2 gas (Ar gas partial pressure / O2 gas partial pressure): 3 / 5 to 1 / 1, preferably 3 / 4 to 1 / 1 Ambient pressure: 0.1 Pa or more and 1.0 Pa or less, preferably 0.2 Pa or more and 0.7 Pa or less Thickness: 1 nm or more and 200 nm or less, preferably 5 nm or more and 50 nm or less
[0070] The following conditions are exemplified as conditions for depositing a Pt film or the like as the upper electrode film 4. The deposition time of the upper electrode film 4 is appropriately adjusted according to the target thickness of the upper electrode film 4. Target: Pt plate, etc. Temperature (substrate temperature): Room temperature (25℃) or higher and 500℃ or lower Discharge power density: 1W / cm 2 More than 5W / cm 2 Less than 2 W / cm, preferably 2 W / cm 2 More than 4W / cm 2 below Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Thickness: 50 nm or more and 5000 nm or less, preferably 50 nm or more and 300 nm or less
[0071] As described above, the lower adhesive layer 6, the lower electrode film 2, the KNN film 3 (KNN films 3a, 3b), the upper adhesive layer 7, and the upper electrode film 4 are sequentially formed to obtain the piezoelectric stack 10 as shown in FIG.
[0072] (Preparation of piezoelectric elements) After producing the piezoelectric laminate 10 as shown in FIG. 1, the piezoelectric laminate 10 is processed to form an element having a KNN film 3 (also referred to as a piezoelectric element 20).
[0073] Specifically, first, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are individually patterned by dry etching using, for example, Ar gas or a reactive gas. In the patterning, the upper electrode film 4 (including the upper adhesive layer 7) and the KNN film 3 are each formed into a predetermined shape, and a part of the lower electrode film 2 is exposed. In the patterning, a photoresist can be used as an etching mask. FIG. 2 shows the piezoelectric stack 10 after the patterning is completed, i.e., a piezoelectric element 20. The piezoelectric element 20 shown in FIG. 2 is also called a simplified piezoelectric element.
[0074] 2, the lower electrode film 2 and the lower adhesive layer 6 are patterned by dry etching using, for example, Ar gas or a reactive gas, to form the lower electrode film 2 and the lower adhesive layer 6 into a predetermined shape. In this patterning, a photoresist can be used as an etching mask.
[0075] After the patterning of the lower electrode film 2 and the lower adhesive layer 6 is completed, the insulating film 8 and the metal wirings 9a, 9b are provided. Specifically, first, a layer made of an insulating material is provided from the upper electrode film 4 to the substrate 1 so as to cover the side surface of the KNN film 3, and the layer made of the insulating material is patterned by dry etching using a reactive gas such as Ar gas or CF4 gas, or wet etching, to provide the insulating film 8. The insulating film 8 can be formed using oxides such as silicon oxide (SiO2), aluminum oxide (Al2O3), and tantalum oxide (Ta2O5). The insulating film 8 may be a single layer film or a laminated body having multiple layers stacked. The insulating film 8 can be provided by a method such as a CVD method or a sputtering method.
[0076] After providing the insulating film 8, a layer (metal wiring layer) made of a material containing metal is provided. Then, the metal wiring layer is patterned by dry etching using Ar gas or reactive gas or wet etching to form metal wirings 9a and 9b. The metal wiring 9a is formed (patterned) so as to be connected (contacted) to the lower electrode film 2 and not connected (not contacted) to the upper electrode film 4, and the metal wiring 9b is formed so as to be connected to the upper electrode film 4 and not connected to the lower electrode film 2. The metal wirings 9a and 9b can be formed using various metals such as Au, Al, Ti, and Cr, or alloys mainly composed of these various metals. The metal wirings 9a and 9b may be a single layer film or a laminated body in which multiple layers are laminated. The metal wirings 9a and 9b (metal wiring layer) can be provided by a method such as a sputtering method, a vapor deposition method, a plating method, or a metal paste method.
[0077] Further, a part of the substrate 1 is removed from the back surface side of the substrate 1 (one of the two main surfaces of the substrate 1 opposite to the surface on which the lower electrode film 2 and the like are formed) by Deep-RIE or wet etching, thereby obtaining a piezoelectric element 20 having a membrane structure, a cantilever structure, or the like, for example, a membrane-type MEMS piezoelectric element 20 as shown in FIG.
[0078] The etching conditions for pattern processing when forming the insulating film 8 and the metal wiring 9a, 9b, and the etching conditions for the substrate 1 when processing the piezoelectric laminate 10 into the piezoelectric element 20 can be general etching conditions used in the semiconductor device manufacturing process as long as the conditions do not deteriorate the insulating properties of the KNN film 3.
[0079] (Fabrication of piezoelectric device module) By connecting the voltage detection means 11a to the obtained piezoelectric element 20, a device module 30 having a KNN film 3 (hereinafter also referred to as piezoelectric device module 30) is obtained. FIG. 4 shows a schematic configuration diagram of the piezoelectric device module 30 according to this embodiment. The piezoelectric device module 30 at least includes the piezoelectric element 20 and a voltage detection means 11a connected to the piezoelectric element 20. The voltage detection means 11a is a means for detecting a voltage generated between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). As the voltage detection means 11a, various known means can be used.
[0080] By connecting the voltage detection means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as a sensor. When the KNN film 3 deforms in response to a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4 due to the deformation. By detecting this voltage by the voltage detection means 11a, the magnitude of the physical quantity applied to the KNN film 3 can be measured. In this case, examples of applications of the piezoelectric device module 30 include an angular velocity sensor, an ultrasonic sensor, a pressure sensor, and an acceleration sensor.
[0081] (3) Effects According to this aspect, one or more of the following effects can be obtained.
[0082] (a) The KNN film 3 has all three characteristics: the median value of the coercive electric field is a positive value in the PE hysteresis curve (characteristic 1 above), the dielectric constant is 490 or less (characteristic 2 above), and the film stress is 150 MPa or less (characteristic 3 above). That is, the KNN film 3 is a spontaneous polarization film, but has a small film stress and a low dielectric constant.
[0083] Because the KNN film 3 is a spontaneous polarization film, there is no need to perform a polarization process on the KNN film 3 when processing the piezoelectric stack 10 to fabricate the piezoelectric element 20 (piezoelectric device module 30). Since the polarization process is not required, the manufacturing process of the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 can be simplified.
[0084] Since the relative dielectric constant of the KNN film 3 is 490 or less, when the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 is used as a sensor, a highly sensitive sensor can be obtained.
[0085] Since the film stress of the KNN film 3 is 150 MPa or less, it is possible to suppress large structural deformation when processing the piezoelectric stack 10 to fabricate the piezoelectric element 20 (piezoelectric device module 30) having a membrane structure, a cantilever structure, or the like. This allows the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to operate normally. For example, it becomes possible for the piezoelectric element 20 (piezoelectric device module 30) to reliably function as a sensor.
[0086] In this way, when the KNN film 3 has all of the above-mentioned characteristics 1 to 3, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be suitably used for sensors.
[0087] (b) Since the KNN film 3a having a high (001) orientation rate and small film stress is interposed between the lower electrode film 2 and the KNN film 3b, the KNN film 3 can have the above-mentioned feature (feature 4) of having the above-mentioned number of application cycles exceeding 10 million, in addition to the above-mentioned features 1 to 3. That is, the KNN film 3 can be a film that has small film stress, a low dielectric constant, and excellent AC stress resistance, even though it is a spontaneous polarization film.
[0088] Since the KNN film 3 has excellent AC stress resistance, that is, the piezoelectric displacement amount is unlikely to decrease even if the KNN film 3 is repeatedly and significantly deformed, it is possible to improve the reliability of the piezoelectric element 20 (piezoelectric device module 30).
[0089] In this way, when the KNN film 3 has all of the above-mentioned characteristics 1 to 4, the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric laminate 10 can be more suitably used for sensors.
[0090] (c) The polarization characteristics of the KNN film 3 in this embodiment are maintained even when the KNN film 3 is exposed to high temperatures. For example, even if the KNN film 3 is exposed to high temperatures after deposition of the KNN film 3 during deposition of the upper electrode film 4, annealing, formation of the insulating film 8 and metal wirings 9a and 9b, mounting, etc., the spontaneous polarization generated in the KNN film 3 is maintained. This makes it possible to more suitably apply the piezoelectric element 20 (piezoelectric device module 30) obtained by processing the piezoelectric stack 10 to sensor applications. In addition, deterioration in the performance of a sensor fabricated using the piezoelectric element 20 (piezoelectric device module 30) can be avoided.
[0091] (d) By setting the median value of the coercive electric field to 10 kV / cm or more, it is possible to stabilize the direction of spontaneous polarization generated in the KNN film 3, and to reliably obtain a KNN film 3 that does not require polarization treatment. Furthermore, by setting the median value of the coercive electric field to 10 kV / cm or more, it is possible to maintain the initial polarization direction (spontaneously polarized direction) even if a reverse electric field (an electric field in a direction that reverses the polarization direction aligned in a certain direction) is mistakenly applied to the KNN film 3 during the fabrication of the piezoelectric stack 10, the piezoelectric element 20, and the piezoelectric device module 30, or during the use of the piezoelectric element 20 (piezoelectric device module 30).
[0092] (e) When forming the KNN film 3, first, the KNN film 3a is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then the KNN film 3b is formed on the KNN film 3a at a second temperature at which the KNN film 3b becomes a spontaneous polarization film, thereby making it possible to obtain a KNN film 3 having all of the above-mentioned characteristics 1 to 3, and preferably all of the above-mentioned characteristics 1 to 4.
[0093] <Other aspects> An embodiment of the present disclosure has been specifically described above. However, the present disclosure is not limited to the above embodiment, and various modifications are possible without departing from the spirit of the present disclosure. In addition, these embodiments can be combined in any manner.
[0094] In the above embodiment, the piezoelectric device module 30 is caused to function as a sensor, but the present invention is not limited thereto. That is, the piezoelectric device module 30 may be caused to function as an actuator. In this case, the piezoelectric device module 30 includes at least a piezoelectric element 20 obtained by forming the above-mentioned piezoelectric laminate 10 into a predetermined shape, and a voltage application means 11b (see FIG. 4) connected to the piezoelectric element 20. The voltage application means 11b is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4 (between the electrodes). As the voltage application means 11b, various known means can be used. By connecting the voltage application means 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can be caused to function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 by the voltage application means 11b, the KNN film 3 can be deformed. This deformation operation can operate various members connected to the piezoelectric device module 30. In this case, examples of applications of the piezoelectric device module 30 include heads for inkjet printers, MEMS mirrors for optical scanners, and vibrators for ultrasonic generators.
[0095] Furthermore, for example, when the above-mentioned piezoelectric laminate 10 is molded into the piezoelectric element 20, the substrate 1 from the piezoelectric laminate 10 may be replaced with another substrate, so long as the piezoelectric device module 30 produced using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired application such as a sensor. EXAMPLES
[0096] Hereinafter, experimental results that support the effects of the above-described embodiment will be described.
[0097] [Experiment 1] An experiment was carried out to confirm the applicable temperatures for the first temperature and the second temperature when depositing a KNN film.
[0098] (Preparation of samples A to G) As a substrate, a Si substrate with a surface of (100) plane orientation, a thickness of 610 μm, a diameter of 6 inches (also referred to as "φ6 inches"), and a thermally oxidized film (thickness of 200 nm) formed on the surface was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (thickness of 25 nm) as a lower adhesive layer, a Pt film (preferentially oriented in the (111) plane orientation with respect to the surface of the substrate, thickness of 200 nm) as a lower electrode film, a KNN film (thickness of 2 μm) as a piezoelectric film, a RuO2 layer (thickness of 10 nm) as an upper adhesive layer, and a Pt film (thickness of 100 nm) as an upper electrode film were formed in this order, to produce Samples A to G, which are piezoelectric laminates. In Samples A to G, the lower adhesive layer, the lower electrode film, the KNN film, the upper adhesive layer, and the upper electrode film were all formed by RF magnetron sputtering.
[0099] The conditions for depositing the ZnO layer as the lower adhesive layer were as follows. Target: ZnO sintered body Substrate temperature: 500℃ Discharge power density: 4W / cm 2 Atmosphere: Ar / O2 mixed gas atmosphere Ambient pressure: 0.3Pa Ar gas partial pressure / O2 gas partial pressure: 10 / 1 Film deposition time: 3 minutes (thickness 25 nm)
[0100] The conditions for depositing the Pt film as the lower electrode film were as follows. Target: Pt plate Substrate temperature: 500℃ Discharge power density: 2W / cm 2 Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Film deposition time: 14 minutes (thickness 200 nm)
[0101] The conditions for forming the KNN membrane were as follows: Target: KNN sintered body Discharge power density: 3W / cm 2 Atmosphere: Ar / O2 mixed gas atmosphere Ambient pressure: 0.1Pa O2 gas partial pressure / Ar gas partial pressure: 1 / 20 Film forming temperature: A specified temperature within the range of 300°C to 650°C Film deposition time: 60 minutes (thickness 2000 nm (2 μm))
[0102] The conditions for depositing the RuO2 layer as the upper adhesion layer were as follows: Target: Ru plate Substrate temperature: Room temperature (25℃) Discharge power density: 0.5W / cm 2 Atmosphere: Ar / O2 mixed gas atmosphere Ambient pressure: 0.3Pa Ar gas partial pressure / O2 gas partial pressure: 1 / 1 Film deposition time: 6 minutes (thickness 10 nm)
[0103] The conditions for depositing the Pt film as the upper electrode film were as follows. Target: Pt plate Substrate temperature: Room temperature (25℃) Discharge power density: 2W / cm 2 Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Film deposition time: 7 minutes (thickness 100 nm)
[0104] Each of the samples A to G was produced under the same conditions as described above, except for the deposition temperature of the KNN film. The deposition temperatures of the KNN films of the samples A to G are as shown in Table 1 below.
[0105] <Evaluation> For each of the samples A to G, the (001) orientation rate of the KNN film, the film stress of the KNN film, and the median value of the coercive electric field were evaluated.
[0106] (Evaluation of (001) orientation rate) The (001) orientation rate of the KNN film was evaluated by calculating using the above formula (1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film. The XRD measurement was performed after the KNN film was formed and before the upper adhesive layer and the upper electrode film were formed. The calculation results of the (001) orientation rate are shown in Table 1 below. In Table 1, the "orientation rate" refers to the (001) orientation rate of the KNN film.
[0107] (Evaluation of membrane stress) The stress of the thin film on the substrate can be calculated by measuring the amount of warpage of the substrate caused by the thin film, specifically, the radius of curvature of the warpage of the substrate, as shown in the following formula (2). Therefore, in this evaluation, first, the radius of curvature R of the warpage of the substrate (Si substrate) of each sample was measured after the lower adhesive layer, the lower electrode film, and the KNN film were formed, and before the upper adhesive layer and the upper electrode film were formed. Then, the film stress of the KNN film of each sample was calculated using the following formula (2). In this evaluation, the radius of curvature R of the Si substrate was calculated from the warpage shape of the Si substrate after the lower adhesive layer, the lower electrode film, and the KNN film were formed, measured by a laser displacement meter.
[0108] TIFF2024141259000002.tif17170
[0109] In the above formula (2), σ is the stress of the thin film (KNN film), E s / (1-νs ) is the biaxial elastic modulus of the substrate (Pa), h is the thickness of the substrate (m), R is the radius of curvature of the warp of the substrate (m), and t is the thickness of the KNN film (m). In samples A to G, the value of the biaxial elastic modulus was set to 30.3 because a Si substrate was used as the substrate. In addition, the film stress (σ) of the KNN film was calculated assuming that the Si substrate was sufficiently flat. In addition, in samples A to G, a lower adhesive layer (ZnO layer) and a lower electrode film (Pt film) were formed, but the thickness of the lower adhesive layer (25 nm) and the thickness of the lower electrode film (200 nm) were sufficiently smaller than the thickness of the KNN film (2 μm). For this reason, the influence of the lower adhesive layer and the lower electrode film was ignored to calculate the film stress of the KNN film.
[0110] The calculation results of the membrane stress of the KNN membrane of samples A to G are shown in the following Table 1. In Table 1, "compressive" means that the membrane stress is compressive stress, and "tensile" means that the membrane stress is tensile stress.
[0111] (Evaluation of the median coercive field) The evaluation of the median value of the coercive field was performed as follows. First, the piezoelectric laminates of samples A to G were prepared, and then the upper electrode film (including the upper adhesive layer) and the KNN film were individually patterned by dry etching using Ar gas. In the patterning, a photoresist was used as an etching mask, and the upper electrode film was shaped to a size of φ0.5 mm, and a part of the lower electrode film was exposed, to prepare a simplified piezoelectric element as shown in FIG. 2. Using each simplified piezoelectric element prepared from samples A to G, a PE hysteresis curve was prepared. Specifically, with the lower electrode film grounded, a triangular or sine wave electric field of -150 kV / cm to +150 kV / cm was applied to the KNN film through the upper electrode film at a frequency of 1 kHz, the polarization amount of the KNN film was measured, and the obtained polarization amount and the applied electric field were plotted to prepare a PE hysteresis curve. A device (DBLI) manufactured by Agxact was used to prepare the PE hysteresis curve. The coercive field E C + and coercive field E C - Obtain the value of the coercive field EC + and coercive field E C - From the value of the coercive field, the median value (=(E C + -E C - ) / 2) was calculated. The calculation results of the median values of the coercive electric fields of samples A to G are shown in the following Table 1. Note that the "median value" in Table 1 means the median value of the coercive electric field.
[0112] [Table 1]
[0113] In sample A, the crystal structure of the KNN film was not a perovskite structure. Therefore, in the X-ray diffraction pattern obtained by performing XRD measurement, no peak was observed at least within the range of 2θ of 20° to 23°, and as a result, the (001) orientation rate could not be calculated. In addition, since the crystal structure of the KNN film was not a perovskite structure, the KNN film had low pressure resistance, and when preparing a PE hysteresis curve, it was not possible to apply a triangular or sine wave electric field of -150 kV / cm to +150 kV / cm at a frequency of 1 kHz to the KNN film through the upper electrode film. Therefore, it was not possible to prepare a PE hysteresis curve, and as a result, it was not possible to measure the median value of the coercive electric field. From these, it can be confirmed that the film formation temperature of sample A is not applicable to either the first temperature or the second temperature.
[0114] In samples B to D, the film stress exceeds 100 MPa. This confirms that the film formation temperatures of samples B to D are not applicable to the first temperature. On the other hand, in samples B to D, the median coercive electric field is 10 kV / cm or more. This confirms that the film formation temperatures of samples B to D, that is, the temperature range of 400°C to 500°C, are the temperatures at which the KNN film becomes a spontaneous polarization film and are applicable to the second temperature.
[0115] In samples E and F, the (001) orientation rate is 95% or more, and the film stress is 100 MPa or less. This confirms that the deposition temperatures of samples E and F, i.e., the temperature range of 550°C or more and 600°C or less, are applicable to the first temperature. On the other hand, in samples E and F, the median coercive electric field is 0 kV / cm. In other words, the KNN films of samples E and F are not spontaneous polarization films. This confirms that the deposition temperatures of samples E and F are not applicable to the second temperature.
[0116] In sample G, the (001) orientation rate is less than 95%, and the film stress is more than 100 MPa. In addition, in sample G, the median value of the coercive electric field is 0 kV / cm. From these, it can be confirmed that the film formation temperature of sample G cannot be applied to either the first temperature or the second temperature.
[0117] [Experiment 2] An experiment was conducted to confirm the effect of depositing the KNN film in two stages at different temperatures.
[0118] (Preparation of samples 1 to 16) As a substrate, a Si substrate with a surface orientation of (100), a thickness of 610 μm, a diameter of 6 inches, and a thermally oxidized film (thickness of 200 nm) formed on the surface was prepared. Then, on the thermally oxidized film of this Si substrate, a ZnO layer (thickness of 25 nm) as a lower adhesive layer, a Pt film (preferentially oriented in the (111) orientation with respect to the surface of the substrate, thickness of 200 nm) as a lower electrode film, a KNN film (thickness of 2 μm) as a piezoelectric film, a RuO2 layer (thickness of 10 nm) as an upper adhesive layer, and a Pt film (thickness of 100 nm) as an upper electrode film were formed in this order to produce Samples 1 to 16, which are piezoelectric laminates. The lower adhesive layer, the lower electrode film, the KNN film, the upper adhesive layer, and the upper electrode film were all formed by RF magnetron sputtering.
[0119] In the samples 1 to 14, the KNN film was formed in two stages by changing the temperature conditions. Specifically, the first KNN film was formed at the first temperature, and then the second KNN film was formed on the first KNN film at the second temperature different from the first temperature. The first and second temperatures for forming the KNN films of the samples 1 to 14 were as shown in the following Table 2, respectively, and the film formation time at the first temperature was 6 minutes (thickness 200 nm), and the film formation time at the second temperature was 54 minutes (thickness 1800 nm). In the samples 15 and 16, the KNN film was formed at a predetermined temperature without changing the temperature conditions. The temperature for forming the KNN films of the samples 15 and 16 was as shown in the "second temperature" column in the following Table 2, and the film formation time was 60 minutes (thickness 2000 nm). The conditions other than the deposition temperature and deposition time when depositing the KNN film, and the deposition conditions for each film (each layer) other than the KNN film, were the same as those in the above-mentioned Experiment 1. Moreover, each of Samples 1 to 16 was produced under the same conditions as described above except for the deposition temperature (first temperature, second temperature) of the KNN film.
[0120] <Evaluation> For each of samples 1 to 16, the median coercive electric field, the relative dielectric constant of the KNN film, the film stress of the KNN film, and the AC stress resistance were evaluated. In addition, using the simplified piezoelectric elements made from samples 3 and 9, an evaluation was performed regarding the necessity of polarization treatment. In addition, using the simplified piezoelectric elements made from samples 1, 2, and 8, an evaluation was performed regarding the temperature resistance of the spontaneous polarization generated in the KNN film. Furthermore, using the simplified piezoelectric elements made from samples 3 and 9, an evaluation was performed regarding the heat resistance performance of the piezoelectric elements.
[0121] (Evaluation of the median coercive field) Using Samples 1 to 16, simplified piezoelectric elements as shown in FIG. 2 were fabricated in the same manner as described in the evaluation of the median value of the coercive electric field in Experiment 1 above. Then, using each simplified piezoelectric element fabricated from Samples 1 to 16, a PE hysteresis curve was fabricated. The PE hysteresis curve was fabricated under the same conditions, by the same method, and by the same device as described in the evaluation of the median value of the coercive electric field in Experiment 1 above. The PE hysteresis curves of Samples 3 and 9 are shown in FIG. 5 and FIG. 6, respectively. Also, the coercive electric field E C + and coercive field E C - The values were obtained and the median value of the coercive electric field was calculated. The calculation results of the median value of the coercive electric field of Samples 1 to 16 are shown in Table 2 below. Note that the "median value" in Table 2 means the median value of the coercive electric field.
[0122] (Evaluation of relative dielectric constant) Using Samples 1 to 16, simplified piezoelectric elements as shown in FIG. 2 were fabricated in the same manner as described in the evaluation of the median coercive electric field in Experiment 1 above. Then, using each simplified piezoelectric element fabricated from Samples 1 to 16, the lower electrode film and the upper electrode film were connected to an LCR meter, and the capacitance was measured under conditions of ±1 V and 1 kHz. The measured capacitance, the area of the upper electrode film (0.625 mm 2 The relative dielectric constant of the KNN film of each sample was calculated using the values of the thickness (2 μm) of the KNN film, and the relative dielectric constant of the KNN film of each sample. The relative dielectric constants of Samples 1 to 16 are shown in Table 2 below.
[0123] (Evaluation of membrane stress) The film stress of the KNN film was evaluated for each of Samples 1 to 16 by the same method as that described in the evaluation of the film stress in Experiment 1 above. A lower adhesive layer and a lower electrode film were also formed in Samples 1 to 16, but as in Samples A to G, the thicknesses of the lower adhesive layer and the lower electrode film were sufficiently smaller than the thickness of the KNN film. For this reason, the influence of the lower adhesive layer and the lower electrode film was ignored to calculate the film stress of the KNN film. The calculation results of the film stress of the KNN film for Samples 1 to 16 are shown in Table 2 below. "Compression" and "tension" in Table 2 have the same meanings as "compression" and "tension" in Table 1.
[0124] (Evaluation of AC stress resistance) The AC stress resistance was evaluated by measuring the AC stress life. The evaluation of the AC stress life was performed as follows. First, a small strip of 20 mm long x 2.5 mm wide was cut out from each of the samples 1 to 16. Then, as shown in FIG. 7(a), one end in the longitudinal direction of each small piece obtained from the samples 1 to 16 was fixed by a clamp, and a voltage application means (not shown) was connected between the lower electrode film and the upper electrode film to fabricate a simple unimorph cantilever. Then, using the voltage application means, a negative voltage was continuously applied to the KNN film through the upper electrode film so that a unipolar AC electric field of 300 kV / cm was generated between the lower electrode film and the upper electrode film (i.e., to the KNN film). Specifically, with the lower electrode film being grounded, a unipolar sine wave AC voltage with an amplitude in the range of 0 V to -60 V was continuously applied to the KNN film through the upper electrode film at a frequency of 300 Hz to continuously deform the KNN film (thickness 2 μm) of each small piece. The deformation of the KNN film causes the entire cantilever to bend (vibrate), and the tip of the cantilever to continuously reciprocate up and down. The displacement Δ (piezoelectric displacement) of the tip of the cantilever at this time was measured by irradiating the tip of the cantilever with laser light L from a laser Doppler displacement meter as shown in Figure 7(b). In this evaluation, the measurement of the displacement Δ was performed every time the number of applied cycles reached 1 million. The number of applied cycles at which the displacement Δ became 80% or less of the initial value was taken as the AC stress life. If the displacement Δ was still 80% or more of the initial value after the number of applied cycles reached 50 million, the measurement was stopped and the measurement result of the AC stress life was taken as more than 50 million times (>50 million times). The measurement results are shown in Table 2 below.
[0125] In addition, in Figures 7(a) and 7(b), for ease of understanding, the lower adhesive layer and the upper adhesive layer are omitted, and the stack of the first KNN film and the second KNN film is illustrated as a KNN film.
[0126] [Table 2]
[0127] In Samples 1 to 6, the median value of the coercive electric field is a positive value, the relative dielectric constant is 490 or less, and the film stress is 150 MPa or less. That is, from Samples 1 to 6, it is found that when forming a KNN film, a first KNN film is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film is formed on the first KNN film at a second temperature at which the second KNN film becomes a spontaneous polarization film, thereby obtaining a KNN film having all three characteristics, namely, the median value of the coercive electric field is a positive value (characteristic 1 described above), the relative dielectric constant is 490 or less (characteristic 2 described above), and the film stress is 150 MPa or less (characteristic 3 described above).
[0128] In sample 7, in which the second temperature was set to 300°C, the (001) orientation rate could not be calculated and the median value of the coercive field could not be measured. This is believed to be because the crystal structure of the second KNN film did not become a perovskite structure. In samples 8 to 10, the median value of the coercive field is 0 in all cases. This is believed to be because the second temperature in samples 8 to 10 is greater than 500°C (600°C, 650°C). From this, it can be confirmed that if the second temperature is not a temperature at which the second KNN film becomes a spontaneous polarization film, a KNN film that is a spontaneous polarization film, that is, a KNN film having the above-mentioned characteristic 1, cannot be obtained. In samples 11 and 12, both have a relative dielectric constant greater than 490 and a film stress greater than 150 MPa. This is believed to be because the first temperature in samples 11 and 12 is greater than 600°C (650°C). In addition, in samples 13 and 14, both have a film stress greater than 150 MPa. This is believed to be because the first temperature was less than 550° C. (500° C.) in Samples 13 and 14. It can be seen from Samples 11 to 14 that unless the first temperature is a temperature at which the (001) orientation rate of the first KNN film is 95% or more and the film stress is 100 MPa or less, a KNN film having a relative dielectric constant of 490 or less and a film stress of 150 MPa or less, i.e., a KNN film having the above-mentioned features 2 and 3, cannot be obtained.
[0129] In addition, in Samples 1 to 6 and 8 to 10, the number of application cycles until the displacement Δ became 80% or less of the initial value exceeded 50 million, and the samples had excellent AC stress resistance. This is believed to be due to the presence of a first KNN film with a high (001) orientation rate and low film stress (for example, a first KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) between the lower electrode film and the second KNN film.
[0130] In particular, in Samples 1 to 6, the median value of the coercive electric field is a positive value, the relative dielectric constant is 490 or less, the film stress is 150 MPa or less, and the above-mentioned number of application cycles exceeds 10 million times (50 million times or more). Thus, it can be confirmed that Samples 1 to 6 further have the feature of excellent AC stress resistance (Feature 4 above) in addition to Features 1 to 3 above. From Samples 1 to 6, it can be confirmed that when depositing a KNN film, a first KNN film is first deposited at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second KNN film is deposited on the first KNN film at a second temperature that is a predetermined temperature higher than the first temperature, thereby obtaining a KNN film having all of Features 1 to 4 above.
[0131] In contrast, in sample 7, a large voltage that would generate a unipolar AC electric field of 300 kV / cm could not be applied to the KNN film, and the number of applied cycles could not be measured. This is believed to be because the crystal structure of the second KNN film does not become a perovskite structure, and the KNN film has low voltage resistance. In addition, in samples 11 to 16, the number of applied cycles until the displacement Δ becomes 80% or less of the initial value is 10 million or less, and the AC stress resistance is low. This is believed to be because the first KNN film in samples 11 to 14 is not formed at a temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, i.e., the (001) orientation rate of the first KNN film is low and the film stress is large. In addition, in samples 15 and 16, the KNN film is not constructed of a laminate of a first KNN film and a second KNN film. Specifically, this is thought to be because a KNN film with a high (001) orientation rate and low film stress (for example, a KNN film with a (001) orientation rate of 95% or more and a film stress of 100 MPa or less) is not interposed between the lower electrode film and the KNN film.
[0132] In addition, in the deposition of the KNN film, the deposition time at the first temperature was set to 6 minutes in Samples 1 to 14, but is not limited to this. The inventors have confirmed that the same results as those described above can be obtained if the deposition time at the first temperature is in the range of 1 minute to 12 minutes. In the deposition of the KNN film, it has been confirmed that the deposition time at the first temperature, i.e., the optimal value of the thickness of the KNN film deposited at the first temperature, may have a certain degree of range.
[0133] (Evaluation of membrane stress) In the above-mentioned Experiments 1 and 2, the membrane stress of the KNN film was calculated from the amount of warping of the substrate (Si substrate), i.e., the radius of curvature of the warping of the substrate, but this is not limited to this. The membrane stress of the KNN film can be known by comparing the MEMS simulation with the shape of the actual object even in the state of a piezoelectric element (piezoelectric device module) in which a MEMS structure is fabricated by processing a piezoelectric laminate.
[0134] (Evaluation of the necessity for polarization treatment) Using simplified piezoelectric elements made from the piezoelectric laminates of sample 3, whose median coercive electric field is a positive value, and sample 9, whose median coercive electric field is zero (0), we confirmed whether the KNN films of samples 3 and 9 were spontaneously polarized films, that is, we evaluated whether polarization treatment was necessary.
[0135] In piezoelectric films such as KNN films, the polarization direction is aligned in a certain direction, and when an electric field is applied in that polarization direction, the film undergoes piezoelectric deformation. For this reason, by applying a low voltage (electric field) to a KNN film that has not been subjected to polarization processing and checking whether the KNN film deforms, it is possible to check whether the KNN film is a spontaneous polarization film, i.e., whether polarization processing is necessary.
[0136] The necessity of polarization treatment was confirmed by carrying out the following measurements (a) to (e) in order. The graphs obtained from measurements (a) to (e) are shown in Fig. 8(a) to (e) and Fig. 9(a) to (e). Fig. 8(a) to (e) are graphs for Sample 3, and Fig. 9(a) to (e) are graphs for Sample 9, respectively.
[0137] <Measurement (a)> First, using the simplified piezoelectric elements made from samples 3 and 9, with the lower electrode film grounded, a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film through the upper electrode film at a frequency of 1kHz, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (a)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The graphs obtained in measurement (a) are shown in Figures 8(a) and 9(a), respectively.
[0138] <Measurement (b)> After the measurement (a) was completed, a sine wave voltage of 0V to -30V (sine wave electric field of 0kV / cm to -300kV / cm) was applied to the KNN film through the upper electrode film with a frequency of 1kHz while the lower electrode film was grounded, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (b)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of -30V in measurement (b) corresponds to the implementation of a process for aligning the polarization in the upward direction (hereinafter also referred to as "upward polarization process"). The graphs obtained in measurement (b) are shown in Figures 8(b) and 9(b), respectively.
[0139] <Measurement (c)> After the measurement (b), we again applied a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) to the KNN film through the upper electrode film with a frequency of 1kHz while grounding the lower electrode film, and measured the displacement of the KNN film (surface of the upper electrode film) (measurement (c)). We obtained a graph showing the correlation between the applied voltage and the displacement of the KNN film. The graphs obtained in measurement (c) are shown in Figures 8(c) and 9(c), respectively.
[0140] <Measurement (d)> After the measurement (c) was completed, a sine wave voltage of 0V to +30V (sine wave electric field of 0kV / cm to +300kV / cm) was applied to the KNN film through the upper electrode film at a frequency of 1kHz while the lower electrode film was grounded, and the displacement of the KNN film (surface of the upper electrode film) was measured (measurement (d)), and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. The application of a voltage of +30V in measurement (d) corresponds to the implementation of a process for aligning the polarization in a downward direction (hereinafter also referred to as "downward polarization process"). The graphs obtained in measurement (d) are shown in Figures 8(d) and 9(d), respectively.
[0141] <Measurement (e)> After the measurement (d), we again applied a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) to the KNN film through the upper electrode film with a frequency of 1kHz while grounding the lower electrode film, and measured the displacement of the KNN film (surface of the upper electrode film) (measurement (e)). We obtained a graph showing the correlation between the applied voltage and the displacement of the KNN film. The graphs obtained in measurement (e) are shown in Figures 8(e) and 9(e), respectively.
[0142] In the simplified piezoelectric element of sample 3, a clear piezoelectric displacement can be confirmed in the graph shown in FIG. 8(a). It can also be confirmed that the piezoelectric displacement in the graph shown in FIG. 8(c) is similar to the piezoelectric displacement in the graph shown in FIG. 8(a). From these, it can be seen that the polarization direction of the KNN film of sample 3 is aligned in the upward direction from the initial state before polarization treatment. In other words, it can be seen that the KNN film of sample 3 is a spontaneously polarized film. It can also be seen that the piezoelectric displacement in the graph shown in FIG. 8(e) is similar to the piezoelectric displacement in the graphs shown in FIG. 8(a) and FIG. 8(c). From this, it can be seen that the initial polarization state (polarization in the upward direction) is maintained even after the treatment (measurement (d)) corresponding to the downward polarization treatment, which is the opposite direction to the treatment (measurement (b)) corresponding to the upward polarization treatment. From these, it can be seen that the spontaneous polarization generated in the KNN film of sample 3 is maintained even after a large voltage is applied (regardless of whether it is forward or reverse). That is, it is clear that the polarization process is not necessary for sample 3.
[0143] On the other hand, in the simplified piezoelectric element of sample 9, no clear piezoelectric displacement was observed in the graph shown in FIG. 9(a), but a piezoelectric displacement was observed in the graph shown in FIG. 9(c). This shows that in sample 9, the polarization direction of the KNN film was aligned in the upward direction (forward direction) by performing the upward polarization process (measurement (b)). Also, in FIG. 9(e), a piezoelectric displacement in the opposite direction to the piezoelectric displacement in FIG. 9(c) was observed. This shows that the polarization direction of the KNN film was changed to an aligned downward direction by performing the downward polarization process (measurement (d)), which is the opposite direction to the upward polarization process (measurement (b)). This shows that the KNN film of sample 9 does not have spontaneous polarization, and that this KNN film has the property of aligning its polarization direction in the direction of the applied voltage after a large voltage is applied (regardless of whether it is forward or reverse). Such a property of the KNN film of Sample 9 is a general property of a KNN film (piezoelectric film) that requires polarization treatment. In other words, it is understood that Sample 9 requires polarization treatment.
[0144] (Evaluation of temperature resistance of spontaneous polarization) Using simplified piezoelectric elements fabricated from the piezoelectric laminates of Samples 1 and 2, the temperature resistance of the spontaneous polarization generated in the KNN film was evaluated.
[0145] First, using the simplified piezoelectric element made from sample 1, a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film through the upper electrode film with a frequency of 1kHz while the lower electrode film was grounded, the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 10(a). After that, the simplified piezoelectric element was placed in an air atmosphere at 400°C for 2 hours. After that, again, a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film through the upper electrode film with a frequency of 1kHz while the lower electrode film was grounded, the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 10(b).
[0146] In addition, using the simplified piezoelectric element made from sample 2, a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film through the upper electrode film with a frequency of 1kHz while the lower electrode film was grounded, the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 11(a). After that, the simplified piezoelectric element was placed in an air atmosphere at 500°C for 2 hours. After that, again, a sine wave voltage of -2V to +2V (sine wave electric field of -10kV / cm to +10kV / cm) was applied to the KNN film through the upper electrode film with a frequency of 1kHz while the lower electrode film was grounded, the displacement of the KNN film (surface of the upper electrode film) was measured, and a graph showing the correlation between the applied voltage and the displacement of the KNN film was obtained. This graph is shown in FIG. 11(b).
[0147] 10(a) and 10(b) show that the piezoelectric displacement of the KNN film is almost unchanged before and after exposure to an atmosphere at 400° C. Also, FIG. 11(a) and 11(b) show that the piezoelectric displacement of the KNN film is almost unchanged before and after exposure to an atmosphere at 500° C. These show that the polarization characteristics of the KNN film, which is a spontaneous polarization film formed by the method of the present disclosure, are maintained even when the KNN film is subjected to a thermal history of 400° C. and even a thermal history of 500° C.
[0148] In addition, the KNN film of sample 8 was subjected to a polarization treatment, and the temperature resistance of the polarization generated in the KNN film of sample 8 was also evaluated. Specifically, first, a simple piezoelectric element made from sample 8 was prepared, and a downward polarization treatment (i.e., the above-mentioned measurement (b)) was performed. Then, the displacement amount of the KNN film was observed before and after exposure to an atmosphere at 400°C or 500°C in the same manner as samples 1 and 2. As a result, it was confirmed that the piezoelectric displacement of the KNN film of sample 8 changed before and after exposure to an atmosphere at 400°C or 500°C. Specifically, in sample 8, a clear piezoelectric displacement was confirmed before exposure to an atmosphere at 400°C or 500°C, but a clear piezoelectric displacement was not observed after exposure to an atmosphere at 400°C or 500°C. In other words, it was confirmed that no polarization was generated in the KNN film of sample 8 after exposure to an atmosphere at 400°C or 500°C.
[0149] (Evaluation of heat resistance of piezoelectric elements) Using piezoelectric elements (membrane-type MEMS devices) fabricated from the piezoelectric laminates of Samples 3 and 9, the heat resistance performance of the piezoelectric elements was evaluated.
[0150] First, the piezoelectric element chip was fabricated as follows. The piezoelectric laminates of samples 3 and 9 were prepared, and an insulating film was provided from the upper electrode film to the lower electrode film so as to cover a part of the side of the KNN film of each sample. In this experiment, a laminate of an aluminum oxide (Al2O3) layer having a thickness of 5 nm and a silicon oxide (SiO2) layer having a thickness of 500 nm provided on the Al2O3 layer was provided as the insulating film. Then, the insulating film was patterned by dry etching using CF4 gas. Then, a laminate of a Ti layer having a thickness of 10 nm and an Au layer having a thickness of 300 nm provided on the Ti layer was provided as the metal wiring layer. Then, the metal wiring layer was patterned by wet etching to form metal wiring of a predetermined pattern. Also, a part of the Si substrate was removed from the back side of the Si substrate by Deep-RIE etching to form a membrane structure. Then, the piezoelectric laminates (each sample) were divided into chips to fabricate a plurality of piezoelectric element chips as shown in FIG. 3.
[0151] Then, a polarization process was performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 9, in which spontaneous polarization was not generated, by applying a DC voltage of -30 V to the KNN film via the upper electrode film by probing. Note that no polarization process was performed on the piezoelectric element chip fabricated using the piezoelectric laminate of Sample 3, in which spontaneous polarization was generated.
[0152] Then, the obtained piezoelectric element chips were mounted in a package (by bonding and wire bonding). In order to evaluate the heat resistance of the fabricated piezoelectric element chips, the heat treatment temperature during package mounting (hereinafter also referred to as "PKG temperature") was set to 200°C and 300°C.
[0153] In this piezoelectric element (membrane-type MEMS device), the membrane structure is deformed by the sound pressure of the ultrasonic waves, and a voltage is generated from the KNN film. That is, this piezoelectric element functions as an ultrasonic sensor. Ultrasonic waves were applied to each of the fabricated piezoelectric element chips to evaluate the sensitivity of the piezoelectric element to ultrasonic waves (i.e., sensor sensitivity, hereinafter also referred to as "ultrasonic sensitivity"). The evaluation results are shown in Table 3 below. In the "ultrasonic sensitivity" column in Table 3, "pass" means that the piezoelectric element operated normally after packaging, and "fail" means that the piezoelectric element did not operate normally after packaging.
[0154] [Table 3]
[0155] The piezoelectric element fabricated using the piezoelectric laminate of Sample 3 operated normally regardless of the package temperature.
[0156] On the other hand, the piezoelectric element made using the piezoelectric laminate of sample 9 and subjected to polarization treatment operated normally when the package temperature was 200°C, but did not operate normally when the package temperature was 300°C. This shows that the ultrasonic sensitivity of the piezoelectric element given a thermal history of 300°C after polarization treatment deteriorates. This is presumably because the polarization direction of the KNN film, which was aligned by the polarization treatment, became disturbed by exposure to high temperatures. This shows that the piezoelectric element made using the spontaneously polarized KNN film has higher heat resistance than the piezoelectric element subjected to polarization treatment. It is clear that the piezoelectric element has high heat resistance and is highly reliable.
[0157] <Preferred aspects of the present disclosure> Preferred aspects of the present disclosure will be described below.
[0158] (Appendix 1) According to one aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive field E on the negative field side C - The median value of the coercive field between The piezoelectric film has a relative dielectric constant of 490 or less, The membrane stress of the piezoelectric film is 150 MPa or less. A piezoelectric stack is provided.
[0159] (Appendix 2) The piezoelectric laminate according to claim 1, preferably In the hysteresis curve, the coercive electric field E C + and the coercive field E C - The median value of the coercive electric field between is 10 kV / cm or more.
[0160] (Appendix 3) The piezoelectric laminate according to claim 1 or 2, preferably When a negative voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
[0161] (Appendix 4) The piezoelectric laminate according to any one of Supplementary Notes 1 to 3, preferably The piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % to 2.0 at %.
[0162] (Appendix 5) The piezoelectric laminate according to any one of claims 1 to 4, preferably A layer containing zinc and oxygen is provided between the substrate and the piezoelectric film.
[0163] (Appendix 6) According to another aspect of the present disclosure, forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; In the step of forming the piezoelectric film, first, a first piezoelectric film, which is a part of the piezoelectric film, is formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneous polarization film. A method for manufacturing a piezoelectric stack is provided.
[0164] (Appendix 7) The method according to claim 6, preferably comprising: The thickness of the first piezoelectric film is 20% or less of the total thickness of the piezoelectric film.
[0165] (Appendix 8) The method according to claim 6 or 7, preferably comprising The first temperature is a temperature at which, when the first piezoelectric film is deposited to a thickness of 2 μm at the first temperature, the (001) orientation rate of the first piezoelectric film is 95% or more.
[0166] (Appendix 9) The method according to any one of Supplementary Notes 6 to 8, preferably comprising: The first temperature is a temperature at which the film stress of the first piezoelectric film becomes 100 MPa or less when the first piezoelectric film is formed to a thickness of 2 μm at the first temperature.
[0167] (Appendix 10) The method according to any one of Supplementary Notes 6 to 9, preferably comprising: The method further includes a step of providing a layer containing zinc and oxygen on the substrate before the step of forming the piezoelectric film, In the step of forming the piezoelectric film, the piezoelectric film is formed on the layer containing zinc and oxygen.
[0168] (Appendix 11) According to yet another aspect of the present disclosure, A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and made of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; an upper electrode film formed on the piezoelectric film; In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive field E on the negative field side C - The median value of the coercive field between The piezoelectric film has a relative dielectric constant of 490 or less, The membrane stress of the piezoelectric film is 150 MPa or less. A piezoelectric element or device module is provided.
[0169] (Appendix 12) According to yet another aspect of the present disclosure, A piezoelectric element or a piezoelectric device module utilizing the polarization characteristics of a piezoelectric film, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under specified conditions, the coercive field E C + and the coercive field E on the negative field side C - The piezoelectric film has a positive median coercive field between the The sensor sensitivity does not deteriorate even when subjected to a thermal history of 300°C (sensor sensitivity is maintained). A piezoelectric element or device module is provided.
[0170] (Appendix 13) According to yet another aspect of the present disclosure, A piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive field E on the negative field side C - The median value of the coercive field between The dielectric constant is 490 or less, The membrane stress is 150 MPa or less. A piezoelectric film is provided.
[0171] (Appendix 14) According to yet another aspect of the present disclosure, In the hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under specified conditions, the coercive field E C + and the coercive field E on the negative field side C - The median value of the coercive field between Polarization properties are maintained even when subjected to heat history of 400℃ or more. A piezoelectric film is provided.
[0172] (Appendix 15) The piezoelectric film, the piezoelectric element, or the piezoelectric device module according to any one of claims 11 to 14, preferably When a negative voltage is continuously applied to the upper electrode film (the upper electrode film provided on the piezoelectric film) so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and the upper electrode film (to the piezoelectric film), the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million. [Explanation of symbols]
[0173] 1 Board 2 Lower electrode film 3. Piezoelectric film 4 Upper electrode film 6 Lower adhesive layer 10 Piezoelectric laminate 20 Piezoelectric element 30 Piezoelectric device module
Claims
1. A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; In a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive electric field E on the negative electric field side C - The median value of the coercive field between The piezoelectric film has a relative dielectric constant of 490 or less, A piezoelectric laminate, wherein the piezoelectric film has a film stress of 150 MPa or less.
2. 2. The piezoelectric stack of claim 1, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar AC electric field of 300 kV / cm between the lower electrode film and an upper electrode film provided on the piezoelectric film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
3. 3. The piezoelectric stack according to claim 1, wherein the piezoelectric film contains at least one element selected from copper and manganese as a dopant at a concentration of 0.1 at % or more and 2.0 at % or less.
4. forming a lower electrode film on a substrate; forming a piezoelectric film composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen on the lower electrode film; A method for manufacturing a piezoelectric laminate, in which, in the process of forming the piezoelectric film, a first piezoelectric film, which is a part of the piezoelectric film, is first formed at a first temperature at which the (001) orientation rate is 95% or more and the film stress is 100 MPa or less, and then, a second piezoelectric film, which is the other part of the piezoelectric film, is formed on the first piezoelectric film at a second temperature at which the second piezoelectric film becomes a spontaneous polarization film.
5. A substrate; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film and composed of an alkali niobium oxide containing potassium, sodium, niobium, and oxygen; an upper electrode film formed on the piezoelectric film; In a hysteresis curve showing the correlation between the amount of polarization and the applied electric field obtained by applying an electric field under predetermined conditions to the piezoelectric film, the coercive electric field E C + and the coercive electric field E on the negative electric field side C - The median value of the coercive field between The piezoelectric film has a relative dielectric constant of 490 or less, A piezoelectric element, wherein the piezoelectric film has a film stress of 150 MPa or less.
6. 6. The piezoelectric element of claim 5, wherein when a negative AC voltage is continuously applied to the upper electrode film so as to generate a unipolar electric field of 300 kV / cm between the lower electrode film and the upper electrode film, the number of cycles of application of the voltage until the piezoelectric displacement of the piezoelectric film decreases to 80% or less of its initial value exceeds 10 million.
Citation Information
Patent Citations
Piezoelectric thin-film device, piezoelectric sensor, and vibration power generator
JP2014207429A
Piezoelectric elements, piezoelectric actuators, hard disk drives, inkjet printers, and piezoelectric sensors
JP2015529963A
Piezoelectric thin film-attached laminate board, piezoelectric thin-film device and manufacturing method thereof
JP2017076730A
Piezoelectric laminate, piezoelectric element, and manufacturing method of piezoelectric laminate
JP2021012909A
sputtering target material
JP2022165896A