Resin composition, film, multilayer film, laminate, and package
A resin composition combining propylene polymer, 1-butene α-olefin copolymer, and high-pressure low-density polyethylene addresses the balance of low-temperature sealing and moldability issues in heat-seal packaging films, ensuring robust and recyclable film performance.
Patent Information
- Application Number
- JP2023052815
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing heat-seal packaging films made of monomaterial olefin compositions, such as PP and PE, face challenges in achieving a balanced performance between low-temperature heat-sealing properties, heat-sealing strength, and moldability, with issues like low heat resistance, insufficient sealing strength, and impact resistance.
A resin composition comprising 5 to 94% propylene polymer, 5 to 75% 1-butene α-olefin copolymer, and 1 to 20% high-pressure low-density polyethylene, with specific melting points and melt flow rates, is used to create a film with a sealant layer that exhibits strain hardening properties, improving moldability and low-temperature sealing properties.
The resin composition achieves excellent low-temperature sealing, easy peelability, and sealing properties, with a balanced performance across various temperature ranges, enhancing the film's functionality and recyclability.
Smart Images

Figure 2024141269000001 
Figure 2024141269000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a film, a multilayer film, a laminate, and a packaging material. [Background technology]
[0002] Heat-seal packaging films are made up of multiple layers of film. In the field of heat-seal packaging films, for example, for packages that require high sealing strength for liquids or retort packaging, there is a tendency for non-oriented films to be used in the multilayer film. In addition, polypropylene (PP) films and polyethylene (PE) films are widely used as heat-seal packaging films, and among these, mono-material films such as PP mono-material packaging and PE mono-material packaging are considered important from the perspective of recycling needs.
[0003] As sealant films for packaging applications, resin compositions in which a propylene-based copolymer is blended with an ethylene-based copolymer, or films using only an ethylene-based copolymer, are widely used. For example, Patent Documents 1 and 2 describe laminates having excellent low-temperature heat sealability, which include a sealant film containing a polypropylene resin, a propylene / α-olefin copolymer, and a 1-butene / α-olefin copolymer.
[0004] In addition, when polypropylene-based films are formed, polypropylene generally has insufficient melting properties (e.g., elongational viscosity and melt tension), and therefore, in many cases, cannot fully ensure molding processability. In order to compensate for the problems with the melting properties of polypropylene, blending with high-pressure low-density polyethylene having long-chain branches has been investigated. High-pressure low-density polyethylene having a long-chain branching structure exhibits strain hardening, in which the elongational viscosity rises sharply during melt elongation and hardens. By exhibiting strain hardening, film thickness unevenness during film forming is stabilized, and uniform bubbles are obtained during foaming, and a molded body with a uniform thickness tends to be obtained during deep drawing. For example, Patent Document 3 describes a sealant having excellent moldability, which has a sealant film containing polypropylene and high-pressure low-density polyethylene. Patent Document 4 describes a sealant having an excellent balance between easy peelability and sealing properties, which has propylene and polyethylene containing branches with 6 or more carbon atoms. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2016 / 027885 [Patent Document 2] Patent Publication No. 2021-070250 [Patent Document 3] JP 2020-090559 A [Patent Document 4] JP 2012-184392 A Summary of the Invention [Problem to be solved by the invention]
[0006] Normally, in mono-material packaging using an olefin material (e.g., PP), the heat resistance of the substrate (e.g., PP) is reduced, so that the sealant layer of the non-stretched film needs to have a sealability (low-temperature sealability) at a temperature at which the substrate does not thermally shrink. However, when the films described in Patent Documents 1 and 2 are used as the non-stretched film, further improvement is required in terms of the balance between the low-temperature heat sealability and the heat seal strength of the resulting laminate.
[0007] Patent Document 3 proposes adding high-pressure low-density polyethylene to polypropylene to improve melting properties and moldability, but this composition tends not to provide sufficient low-temperature sealability and easy peelability. In addition, the introduction of a long-chain branched structure results in a lower material strength than linear low-density polyethylene and a lower compatibility with polypropylene. As a result, when used as a resin composition containing polypropylene, there are problems such as low heat seal strength and insufficient impact resistance. Patent Document 4 proposes improving the balance between easy peelability and sealability by adding polyethylene containing branches with 6 or more carbon atoms to polypropylene, but this structure tends not to provide sufficient low-temperature sealability.
[0008] The present invention has been made in consideration of the above, and has an object to provide a resin composition which can provide a film that has excellent melting characteristics (strain hardening properties) and moldability, and is capable of constituting a laminate having a well-balanced low-temperature sealability, easy peel property, and sealability. [Means for solving the problem]
[0009] The present invention relates to, for example, the following [1] to
[11] . [1] 5 to 94% by mass of a propylene-based polymer (A), 5 to 75 mass% of a 1-butene / α-olefin copolymer (B); High-pressure low-density polyethylene (C) is 1 to 20 mass% (wherein the total of the propylene polymer (A), the copolymer (B) and the polyethylene (C) is 100 mass%); The propylene polymer (A) has a melting point measured by differential scanning calorimetry (DSC) of 120 to 170°C; The copolymer (B) has a melting point of less than 120°C as measured by differential scanning calorimetry (DSC) or no melting point is observed by differential scanning calorimetry (DSC), and contains 51 to 99 mol % of structural units derived from 1-butene and 1 to 49 mol % of structural units derived from an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms (with the proviso that the total of the structural units derived from 1-butene and the structural units derived from the α-olefin is 100 mol %); The polyethylene (C) is a resin composition having a melt flow rate (MFR) measured in accordance with ASTM D1238 at 190° C. under a load of 2.16 kg in the range of 0.1 to 100 g / 10 min.
[0010] [2] A film made of the resin composition according to [1].
[0011] [3] A multilayer film having a sealant layer made of the resin composition according to [1].
[0012] [4] The multilayer film according to [3], wherein the sealant layer has a thickness of 3 to 30 μm.
[0013] [5] A laminate having the film according to [2] or the multilayer film according to [3] or [4], and a stretched film.
[0014] [6] The laminate according to [5], wherein the stretched film is a stretched polypropylene film.
[0015] [7] The laminate according to [5] or [6], wherein the stretched film has a thickness of 10 to 50 μm.
[0016] [8] The laminate according to any one of [5] to [7], wherein the maximum heat seal strength in a temperature range of 70 to 120° C. is in the range of 2 to 10 N / 15 mm.
[0017] [9] The laminate according to any one of [5] to [8], which has a maximum heat seal strength of 10 N / 15 mm or more in a temperature range of 140 to 160° C.
[0018]
[10] Further comprising at least one functional layer selected from a printing layer, a barrier layer, and an embossed layer; The laminate according to any one of [5] to [9], wherein the functional layer is adjacent to or in contact with at least one film selected from the film or multilayer film, and a stretched film via an adhesive layer.
[0019]
[11] A packaging material formed from the laminate according to any one of [5] to
[10] . Effect of the Invention
[0020] The resin composition of the present invention uses a specific propylene polymer, 1-butene-α-olefin copolymer, and high-pressure low-density polyethylene in a specified ratio, and thus has excellent moldability and strain hardening properties, as well as a good balance of low-temperature sealability, easy peelability, and sealability. Furthermore, a laminate using a film made of the resin composition of the present invention also tends to have excellent appearance after peeling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] [Resin composition] The resin composition of the present invention (hereinafter also referred to as "the composition") contains the following (A) to (C) in given proportions. (A) A propylene-based polymer (hereinafter also referred to as "(co)polymer (A)") having a melting point (Tm) of 120 to 170°C as measured by differential scanning calorimetry (DSC). (B) A 1-butene-α-olefin copolymer (hereinafter also referred to as "copolymer (B)") which has a melting point of less than 120°C as measured by DSC or no melting point is observed by DSC, and contains 51 to 99 mol % of structural units derived from 1-butene and 1 to 49 mol % of structural units derived from an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms (however, the total of the structural units derived from 1-butene and the structural units derived from an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms is 100 mol %). (C) High-pressure low-density polyethylene (C) having a melt flow rate (MFR) in the range of 0.1 to 100 g / 10 min, measured at 190°C under a load of 2.16 kg in accordance with ASTM D1238 (hereinafter also referred to as "polyethylene (C)").
[0022] The composition contains a (co)polymer (A), a copolymer (B), and a polyethylene (C). The content of each component is 5 to 94% by mass, preferably 13 to 84% by mass, and more preferably 25 to 70% by mass of the (co)polymer (A), 5 to 75% by mass, preferably 10 to 70% by mass, and more preferably 20 to 65% by mass of the copolymer (B), and 1 to 20% by mass, preferably 3 to 17% by mass, and more preferably 5 to 15% by mass of the copolymer (C) (however, the total content of the (co)polymer (A), the copolymer (B), and the polyethylene (C) is 100% by mass).
[0023] When the content of (co)polymer (A) is within the above range, the resulting composition has excellent rigidity, heat resistance and sealing property. When the content of copolymer (B) is within the above range, the resulting composition has excellent low-temperature sealing property and surface properties. When the content of polyethylene (C) is within the above range, the resulting composition has excellent strain hardening property and improved moldability.
[0024] <Propylene-based polymer (A)> Examples of the propylene polymer (A) include a homopolymer of propylene, a random copolymer of propylene and an α-olefin having 2 or 4 to 20 carbon atoms, and a block copolymer of propylene and an α-olefin having 2 or 4 to 20 carbon atoms, and preferably a homopolymer of propylene or a random copolymer of propylene and an α-olefin having 2 or 4 to 20 carbon atoms. The (co)polymer (A) may be one type of copolymer or two or more types of copolymers.
[0025] In the present composition, it is particularly preferable to use a homopolymer of propylene in order to impart heat resistance and rigidity to the film, while it is particularly preferable to use a random copolymer of propylene and an α-olefin having 2 carbon atoms or 4 to 20 carbon atoms in order to impart flexibility and transparency to the sealant layer.
[0026] Examples of the α-olefin having 2 carbon atoms or 4 to 20 carbon atoms to be copolymerized with propylene include ethylene, 1-butene, 1-pentene, 3-methyl-1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. The α-olefins may be used alone or in combination of two or more.
[0027] When a random copolymer of propylene and an α-olefin having 2 carbon atoms or 4 to 20 carbon atoms is used as the (co)polymer (A), the (co)polymer (A) contains preferably 91 to 99.9 mol %, more preferably 92 to 99.8 mol %, and even more preferably 93 to 99.7 mol % of structural units derived from propylene, and 0.1 to 9 mol %, preferably 0.2 to 8 mol %, and even more preferably 0.3 to 7 mol % of structural units derived from an α-olefin having 2 carbon atoms or 4 to 20 carbon atoms (however, the total of the structural units derived from propylene and the structural units derived from the α-olefin is 100 mol %).
[0028] The (co)polymer (A) has a melting point (Tm) measured by differential scanning calorimetry (DSC) of 120 to 170° C., preferably 125 to 165° C. By using the (co)polymer (A) having a melting point (Tm) within the above range, the formability of the film can be improved, and the film can be provided with heat resistance and transparency. Furthermore, the heat of fusion (ΔH) obtained simultaneously with the melting point by DSC is preferably 50 mJ / mg or more.
[0029] The melting point (Tm) of the (co)polymer (A) is measured by heating about 5 mg of a sample to 200° C. under a nitrogen atmosphere (20 mL / min) using a differential scanning calorimeter (e.g., DSCPyris1 or DSC7 manufactured by PerkinElmer), holding the sample for 10 minutes, then cooling the sample to 30° C. at 10° C. / min, holding the sample for 5 minutes, and then heating the sample to 200° C. at 10° C. / min. The temperature at the apex of the crystal melting peak is taken as the melting point (Tm) of the polymer. When multiple peaks are detected, the peak detected at the highest temperature is used.
[0030] The melt flow rate (MFR) of the (co)polymer (A) measured according to ASTM D1238 at 230°C under a load of 2.16 kg is preferably 0.01 to 40 g / 10 min, more preferably 0.1 to 10 g / 10 min. By using the (co)polymer (A) having an MFR within the above range, the fluidity of the resin composition is improved, and even a relatively large sheet can be easily molded.
[0031] The (co)polymer (A) can be produced by polymerizing monomers in the presence of a known catalyst such as a Ziegler-Natta catalyst, a metallocene catalyst, etc., by a known polymerization method such as a gas phase method, a bulk method, a slurry method, etc. As an example of a method for adjusting the melting point to 120 to 170°C, there can be mentioned a method of controlling the polymerization conditions such as the monomer feed amount to control the comonomer content to less than 20 mol% in the case of polymerization with a Ziegler-Natta catalyst, and to less than 10 mol% in the case of polymerization with a metallocene catalyst, and by this method, a polymer having a target melting point can be obtained.
[0032] <1-butene / α-olefin copolymer (B)> The 1-butene-α-olefin copolymer (B) may be, for example, a copolymer of 1-butene and an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms. The copolymer (B) may be one type of copolymer or two or more types of copolymers. In general, the use of 1-butene·α-olefin copolymers improves the low-temperature sealability and easy peelability of laminates.
[0033] Examples of α-olefins having 2 to 3 carbon atoms or 5 to 20 carbon atoms that are copolymerized with 1-butene include ethylene, propylene, 1-pentene, 3-methyl-1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene, and among these α-olefins, ethylene, propylene, and 1-pentene are preferred, ethylene and propylene are more preferred, and propylene is even more preferred. The α-olefins may be used alone or in combination of two or more.
[0034] The copolymer (B) contains 51 to 99 mol %, preferably 60 to 97 mol %, and more preferably 70 to 95 mol % of structural units derived from 1-butene, and 1 to 49 mol %, preferably 3 to 40 mol %, and more preferably 5 to 30 mol % of structural units derived from an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms (however, the total of the structural units derived from 1-butene and the structural units derived from the α-olefin is 100 mol %). By containing each structural unit in the above range, the copolymer has excellent handleability during molding and is easy to heat seal even at a relatively low temperature.
[0035] The copolymer (B) has a melting point (Tm) measured by DSC of less than 120° C. or no melting point (Tm) is observed by DSC, and preferably has a melting point (Tm) of 50 to 115° C., more preferably 60 to 110° C., and further preferably 65 to 110° C. By using the copolymer (B) having a melting point (Tm) within the above range, the laminate can be easily heat-sealed even at a relatively low temperature, and good surface properties can be obtained.
[0036] The melting point (Tm) of the copolymer (B) is measured by using a differential scanning calorimeter (e.g., DSC manufactured by Seiko Instruments Inc.) by filling an aluminum pan with about 10 mg of a sample, heating it to 200°C at 100°C / min and holding it there for 5 minutes, then cooling it to -100°C at 10°C / min, and then heating it to 200°C at 10°C / min. The temperature at the peak of the crystal melting peak at this time is taken as the melting point (Tm) of the polymer. When multiple peaks are detected, the peak detected on the highest temperature side is used.
[0037] The melt flow rate (MFR) of the copolymer (B) measured according to ASTM D1238 at 230°C and under a load of 2.16 kg is preferably 0.1 to 30 g / 10 min, more preferably 0.5 to 20 g / 10 min, and even more preferably 1.0 to 10 g / 10 min. Furthermore, in the copolymer (B) having an MFR at 230°C within the above range, the melt flow rate (MFR) measured according to ASTM D1238 at 190°C and under a load of 2.16 kg is preferably 0.1 to 30 g / 10 min, more preferably 0.5 to 20 g / 10 min, and even more preferably 1.0 to 10 g / 10 min. By using the copolymer (B) having an MFR within the above range, the fluidity of the resin composition constituting the sealant layer is improved, and even a relatively large sheet can be easily molded.
[0038] The copolymer (B) can be produced by polymerizing monomers in the presence of a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst by a known polymerization method such as a gas phase method, a bulk method, a slurry method, etc. As an example of a method for making the melting point less than 120°C, there is a method of controlling the polymerization conditions such as the monomer feed amount, and controlling the comonomer content to 20 mol% or more and 50 mol% or less when polymerizing with a Ziegler-Natta catalyst, and controlling the comonomer content to 10 mol% or more and 50 mol% or less when polymerizing with a metallocene catalyst, and by this method, a copolymer having a target melting point can be obtained.
[0039] <High-pressure low-density polyethylene (C)> The high-pressure low-density polyethylene (C) may be, for example, an ethylene homopolymer. One or more kinds of the polyethylene (C) may be used. In general, by using high pressure low density polyethylene, the resulting composition has excellent strain hardening properties and improved moldability.
[0040] The polyethylene (C) has a melt flow rate (MFR) of 0.1 to 100 g / 10 min, preferably 0.2 to 50 g / 10 min, more preferably 0.5 to 30 g / 10 min, and further preferably 1.0 to 20 g / 10 min, as measured in accordance with ASTM D1238 at 190° C. and a load of 2.16 kg. By using the copolymer (C) having an MFR within the above range, the fluidity of the resin composition constituting the sealant layer is improved, and even a relatively large sheet can be easily molded.
[0041] The density of the polyethylene (C), measured in accordance with ASTM D1505, is preferably 900 to 940 kg / m 3 , more preferably 900 to 930 kg / m 3 , and more preferably 900 to 925 kg / m 3 , particularly preferably 910 to 925 kg / m 3 By using the polyethylene (C) having a density within the above range, the flowability of the resin composition constituting the sealant layer is improved, and even a relatively large sheet can be easily molded.
[0042] The method for producing the polyethylene (C) is not particularly limited, but examples thereof include a radical polymerization method in which radical polymerization is carried out under conditions of 500 to 2000 atmospheric pressure and 150 to 300° C. In addition, examples of the polymerization initiator include organic peroxides.
[0043] The present composition may contain additives, such as a resin other than the (co)polymer (A), the copolymer (B), and the polyethylene (C), a tackifier, a weather resistance stabilizer, a heat resistance stabilizer, an antistatic agent, a slip agent, an antiblocking agent, a lubricant, a pigment, a dye, a plasticizer, an antiaging agent, a hydrochloric acid absorber, and an antioxidant, as necessary, within the scope of the object of the present invention.
[0044] The (co)polymer (A), copolymer (B), and polyethylene (C) used in the present composition, and the (co)polymer used in the resin composition constituting the substrate layer described below may each contain at least one type of biomass-derived monomer (biomass-derived propylene, biomass-derived ethylene, biomass-derived α-olefin having a carbon number of 4 to 20). The same type of monomer constituting the polymer may be only biomass-derived monomers, may be only fossil fuel-derived monomers, or may contain both biomass-derived monomers and fossil fuel-derived monomers.
[0045] [Film, multi-layer film] The film of the present invention (hereinafter also referred to as "the present film") is characterized by being made of the present composition, and is preferably a multilayer film having a sealant layer made of the present composition. When the present film is a multilayer film, the multilayer film usually has a structure in which a sealant layer and a layer that supports the sealant layer, such as a substrate layer, are laminated.
[0046] <Sealant layer> The sealant layer is a layer that imparts thermal adhesion to a laminate having the present film and a stretched film described later. The sealant layer may be composed of one layer or multiple layers. When multiple sealant layers are used, one type may be used alone, or two or more types may be used.
[0047] The thickness of the sealant layer is preferably 3 to 30 μm, more preferably 5 to 25 μm. When there are a plurality of sealant layers, it is preferable that the thickness of each sealant layer is within the above range.
[0048] ≪Base material layer≫ The resin composition constituting the base layer is preferably polypropylene. Examples of the polypropylene include a homopolymer of propylene and a copolymer having propylene as a main monomer. In the case of the copolymer, it may be a random copolymer or a block copolymer. Examples of other monomers copolymerized with propylene include α-olefins having 2 or 4 to 20 carbon atoms, diene compounds, and the like. The polypropylene contains 85 to 100 mol %, preferably 90 to 99.5 mol %, of structural units derived from propylene, and 0 to 15 mol %, preferably 0.5 to 10 mol %, of structural units derived from other monomers (however, the total of the structural units derived from propylene and the structural units derived from other monomers is 100 mol %).
[0049] Examples of the α-olefin having 2 carbon atoms or 4 to 20 carbon atoms to be copolymerized with propylene include ethylene, 1-butene, 1-pentene, 3-methyl-1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, etc. The α-olefins may be used alone or in combination of two or more.
[0050] The melt flow rate (MFR) of the polypropylene is measured in accordance with ASTM D1238 under conditions of 230°C and a load of 2.16 kg and is preferably 0.01 to 400 g / 10 min, more preferably 0.1 to 100 g / 10 min, and the melting point (Tm) is preferably 115 to 175°C, more preferably 120 to 170°C.
[0051] Specific examples of the polypropylene include propylene homopolymers, propylene-ethylene random copolymers, propylene-1-butene random copolymers, propylene-1-butene-ethylene random copolymers, propylene-1-hexene random copolymers, propylene-3-methyl-1-butene random copolymers, propylene-4-methyl-1-pentene random copolymers, etc. The polypropylenes may be used alone or in combination of two or more.
[0052] The polypropylene can be produced by polymerizing monomers in the presence of a known catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst by a known polymerization method such as a gas phase method, a bulk method, or a slurry method. The polypropylene contained in the resin composition constituting the base layer is preferably the (co)polymer (A) contained in the present composition. When the resin composition constituting the base layer contains the (co)polymer (A), the type of the (co)polymer (A) may be the same as or different from the (co)polymer (A) used in the present composition.
[0053] The base layer may contain additives such as resins other than polypropylene, tackifiers, weather stabilizers, heat stabilizers, antistatic agents, slip agents, antiblocking agents, lubricants, pigments, dyes, plasticizers, antioxidants, hydrochloric acid absorbers, and antioxidants, as long as the object of the present invention is not impaired. The substrate layer may be composed of one layer or multiple layers. When multiple substrate layers are used, one type may be used alone, or two or more types may be used.
[0054] The thickness of the base layer is preferably 10 to 100 μm, more preferably 20 to 75 μm. When there are a plurality of base layers, it is preferable that the thickness of each base layer is within the above range.
[0055] <How to make the film> The present film may be a non-stretched film or a stretched film, and is preferably a non-stretched film. The present film can be produced by extrusion molding using a known extruder. For example, when the present film is a multi-layer film having a sealant layer, it is obtained by laminating the sealant layer and the base layer. Specifically, it can be produced by using two extruders connected to a T-die, supplying the present composition and the resin composition constituting the base layer to each extruder, and co-extrusion molding. The total thickness of the present film is usually 13 to 130 μm, and preferably 25 to 100 μm.
[0056] <Laminate> The laminate of the present invention (hereinafter also referred to as "the laminate") has the present film and a stretched film. The laminate may have a structure such as the present film / stretched film, the present film / stretched film / stretched film, but is not limited thereto. For example, when a plurality of the present films are used, one type may be used alone, or two or more types may be used. In addition, an adhesive layer may be provided between the present film and the stretched film. In the case where the present film contains a base layer in the present laminate, it is preferable that the base layer is adjacent to the stretched film or in contact with the stretched film via an adhesive layer.
[0057] <Stretched film> The film constituting the stretched film may be any conventionally known film depending on the application, specific examples of which include films made of polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate, polyethylene carbonate films, polyamide films such as nylon 6 and nylon 66, ethylene-vinyl alcohol copolymer films, polyvinylidene chloride films, and films made of polyolefins such as polypropylene (PP). The stretched film made of these films may be used alone or in combination of two or more kinds. Furthermore, these films may be films on which inorganic substances such as aluminum, zinc, silica, or oxides thereof are vapor-deposited.
[0058] Among these, preferred is at least one selected from the group consisting of a stretched PET film obtained by stretching a film formed from polyethylene terephthalate (PET), and a stretched PP film obtained by stretching a film formed from polypropylene (PP). The stretching method may be a known method for producing a stretched film. Specific examples include roll stretching, tenter stretching, tubular stretching, etc. The stretching ratio is usually 1.5 to 20 times, and preferably 2 to 15 times.
[0059] The thickness of the stretched film is usually 10 to 50 μm, preferably 15 to 45 μm, and when there are multiple stretched films, it is preferable that the thickness of each stretched film is within the above range. The total thickness of the laminate of the present invention is usually 30 to 150 μm, preferably 40 to 115 μm.
[0060] The laminate has an excellent balance of low-temperature sealability, easy peelability and airtightness. "Excellent low-temperature sealability" means that the maximum heat seal strength of the laminate in the temperature range of 70 to 120°C, i.e., the maximum peel strength of each test piece prepared by changing the temperature of the upper seal bar within the range of 70 to 120°C in the measurement of heat seal strength described later, is preferably 2 to 10 N / 15 mm, more preferably 3 to 10 N / 15 mm or more, and even more preferably 4 to 10 N / 15 mm or more. When the maximum heat seal strength of the laminate in the temperature range of 70 to 100°C is within the above range, heat sealing at low temperatures is possible, and high-speed filling is also possible.
[0061] In the present invention, "excellent easy peelability" means that the heat seal strength is preferably 2 to 10 N / 15 mm, and the range of heat seal temperatures in which the difference between the maximum and minimum values of the heat seal strength is less than 1.5 N / 15 mm is preferably 20° C. or more. From the viewpoint of easy peelability, the heat seal strength is more preferably 2 to 9 N / 15 mm, and even more preferably 2 to 7 N / 15 mm. Furthermore, if the range of heat seal temperatures in which the difference between the maximum and minimum values of the heat seal strength is less than 1.5 N / 15 mm is 30° C. or more, the range of heat seal temperatures in which easy peelability is exhibited is wider, which is more preferable.
[0062] The term "excellent sealability" means that the maximum heat seal strength of the laminate in the temperature range of 140 to 160°C, i.e., the maximum peel strength of each test piece produced by changing the temperature of the upper seal bar within the range of 140 to 160°C in the measurement of heat seal strength described later, is preferably 10N / 15mm or more, more preferably 11N / 15mm or more, even more preferably 12N / 15mm or more, and particularly preferably 13N / 15mm or more. The upper limit of the maximum heat seal strength in the temperature range of 140 to 160°C is usually 100N / 15mm.
[0063] In the above-mentioned measurement of heat seal strength, the heat-sealed portions of the two sealed laminates peel off in the form of edge tearing, cohesive peeling, etc., or the film is cut, torn, etc. In the present invention, when the heat seal strength is maximized in the heat seal strength measurement in the temperature range of 70 to 160°C, it is preferable that the heat-sealed portions of the laminate peel off in the form of edge tearing or cohesive peeling.
[0064] In this specification, the heat seal strength refers to the peel strength (N / mm) measured when two identical laminates are overlapped with the sealant layer surfaces facing each other, the lower seal bar is heated to 70°C, the upper seal bar to 70, 80, 90, 100, 110, 120, 130, 140, 150, or 160°C, and the seal bar is heated at a pressure of 0.2 MPa for one second at a width of 5 mm, and then allowed to cool. Next, 15 mm wide test pieces are cut from each of the heat-sealed test pieces, and the heat-sealed portion of each test piece is peeled off in a direction 180° from the laminate surfaces at a crosshead speed of 300 mm / min.
[0065] The present laminate may be produced by laminating the present film and a stretched film by dry lamination, non-solvent lamination, sand lamination, etc., or may be produced by laminating the present film and a stretched film by melt extrusion lamination. Among these, the method of laminating by dry lamination or melt extrusion lamination is preferable.
[0066] In addition, the laminate may further have at least one functional layer selected from a printed layer, a barrier layer, and an embossed layer to impart a specific function to the film and the stretched film. From the viewpoint of imparting a function to the film and the stretched film, it is preferable that the functional layer is adjacent to the film and the stretched film or is in contact with the film via an adhesive layer.
[0067] The functional material layer may be a resin film on which an inorganic compound or an inorganic oxide is vapor-deposited, a metal foil, a coating film of a resin having a special function, a resin film on which a pattern is printed, or the like. The resin film used here can be the same as the resin film used for the base film, and further, similar plastic compounding agents and additives can be added in any amount depending on the purpose, as long as they do not adversely affect other performance properties.
[0068] The resin film can be produced, for example, by a conventional film-forming method such as extrusion, cast molding, T-die, cutting, or inflation using one or more resins selected from the same group of resins as those for the base film, or by a multilayer co-extrusion film-forming method using two or more resins. Furthermore, from the viewpoint of film strength, dimensional stability, and heat resistance, the film can be stretched uniaxially or biaxially using, for example, a tenter system or a tubular system.
[0069] For example, a laminate further comprising a barrier layer can be produced by a method similar to the method for producing a laminate, which includes a step of forming the barrier layer as a layer in the present film or a stretched film by metal deposition, a coating method or a coextrusion method, and a step of laminating the present film and the stretched film described above.
[0070] <Package> The package formed from the laminate has excellent low-temperature sealing properties and easy peeling properties. Furthermore, the package formed from the laminate can maintain the same heat seal strength as conventional products when molded at conventional heat seal temperatures (e.g., from 100°C to 160°C).
[0071] The method for producing the package includes, for example, placing the sealant layers of the laminate face each other, or placing the sealant layer of the laminate face another film, and then heat-sealing at least a part of the periphery from the outer surface side to form a desired container shape. Also, by heat-sealing the entire periphery, a sealed package can be produced. When the molding process of this package is combined with a filling process of the contents, that is, by heat-sealing the bottom and sides of the package, filling the contents, and then heat-sealing the top, a package containing the contents can be produced. This package can be used in an automatic packaging device for solids such as snacks and bread, powders, or liquid materials.
[0072] In addition, the present laminate or a sheet of the present laminate can be used to fill a container, such as a container previously formed into a cup shape by vacuum forming, compressed air forming, or the like, a container obtained by injection molding, or a container formed from a paper base material, with the contents, and then the present laminate can be used as a lid to cover the container and heat seal the top or sides thereof to obtain a container packed with the contents. This container is suitable for packaging instant noodles, miso paste, jelly, pudding, snacks, etc.
[0073] When the laminate or a package formed from the laminate has a mono-material structure, it can be effectively used as a recycled product. A molded product that is a recycled product of the laminate or a package can reduce the amount of newly polymerized plastic used, and can contribute to reducing the environmental load. EXAMPLES
[0074] Next, the laminate of the present invention will be described in more detail with reference to examples, but the present invention is not limited to these. The materials used in the examples and comparative examples are shown below.
[0075] (A) Propylene-based polymer rPP (A-1): Random polypropylene (MFR (230°C, 2.16 kg load, compliant with ASTM D1238): 7 g / 10 min, melting point: 138°C, propylene content: 95 mol%, ethylene content: 2 mol%, 1-butene content: 3 mol%)
[0076] (B) 1-butene-α-olefin copolymer BPR (B-1): 1-butene-propylene copolymer (MFR (230°C, 2.16 kg load, conforming to ASTM D1238): 9 g / 10 min, MFR (190°C, 2.16 kg load, conforming to ASTM D1238): 4 g / 10 min, melting point: 100°C, 1-butene content: 87 mol%, propylene content: 13 mol%)
[0077] (C) High-pressure low-density polyethylene LDPE (C-1): Dow Mitsui Polychemicals Mirason 16P (MFR (190°C, 2.16 kg load, conforms to ASTM D1238): 3.7 g / 10 min, density (conforms to ASTM D1505): 923 kg / m 3 )
[0078] [Melt point measurement method] (Propylene polymer) Using a differential scanning calorimeter (PerkinElmer DSCPyris1) in a nitrogen atmosphere (20 mL / min), about 5 mg of a sample was heated to 200°C and held for 10 minutes, then cooled to 30°C at 10°C / min and held for 5 minutes, and then heated to 200°C at 10°C / min. The temperature at the apex of the crystal melting peak was determined as the melting point (Tm) of the propylene polymer.
[0079] (1-butene-α-olefin copolymer) Using a differential scanning calorimeter (Seiko Instruments DSC) in a nitrogen atmosphere (20 mL / min), about 10 mg of the sample was packed into a measurement aluminum pan, heated to 200°C at 100°C / min and held for 5 minutes, then cooled to -100°C at 10°C / min and heated to 200°C at 10°C / min. The temperature at the apex of the crystal melting peak at this time was taken as the melting point (Tm) of the 1-butene·α-olefin copolymer or propylene·α-olefin copolymer.
[0080] [Evaluation method for strain hardening] The resin compositions obtained in Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-4 were kneaded using a single-screw extruder (φ40 mm), and the resulting pellets were hot-pressed at a molding temperature of 230° C. to prepare a sheet having a thickness of 1 mm. The uniaxial extensional viscosity was measured under the following conditions using a rheometer (Ares-G2 manufactured by TA Instruments). (Measurement conditions) Deformation mode: Uniaxial extension ·Measurement temperature: 190℃ Strain rate: 10 / sec Environment: Nitrogen atmosphere Using the obtained uniaxial extensional viscosity results, the strain hardening of the resin composition was evaluated according to the following criteria. (Evaluation of the presence or absence of strain hardening) ○ (Strain hardening): When time t (seconds) is plotted on the horizontal axis and extensional viscosity η (Pa sec) on the vertical axis in a double logarithmic graph, the graph obtained does not form an upward convex curve. × (No strain hardening): When time t (seconds) is plotted on the horizontal axis and extensional viscosity η (Pa sec) on the vertical axis on a logarithmic graph, the graph obtained is an upward convex curve.
[0081] [Method of measuring heat seal strength] The sealant layer surfaces of the two laminates were placed together, and the lower seal bar was heated to 70°C, and the upper seal bar was heated to 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, or 160°C, with a pressure of 0.2 MPa for 1 second at a seal bar width of 5 mm, and then allowed to cool. Next, 15 mm wide test pieces were cut from each of the heat-sealed test pieces, and the peel strength was measured for each test piece when the heat-sealed portion was peeled off in a 180° direction with respect to the laminate surface at a crosshead speed of 300 mm / min, and the value was taken as the heat seal strength.
[0082] (Low temperature sealing) The low-temperature sealability of the laminate was evaluated according to the following criteria. ○: The maximum heat seal strength in the temperature range of 70 to 100°C is 8N / 15mm or more. ×: The maximum heat seal strength in the temperature range of 70 to 100°C is less than 8N / 15mm
[0083] (Easy peeling) The easy peel property of the laminate was evaluated according to the following criteria. ◯: The heat seal strength is 2 to 10 N / 15 mm, and there is at least one heat seal temperature range in which the difference between the maximum and minimum heat seal strength values is less than 1.5 N / 15 mm and the range width of the heat seal temperature is 20° C. or more. ×: There is no heat sealing temperature range in which the heat sealing strength is 2 to 10 N / 15 mm and the difference between the maximum and minimum heat sealing strength values is less than 1.5 N / 15 mm and the range width of the heat sealing temperature is 20° C. or more.
[0084] (Sealability) The sealability of the laminate was evaluated according to the following criteria. ○: The easy peel property is rated as ○, and the maximum heat seal strength in the temperature range of 140 to 160 ° C is 10 N / 15 mm or more. ×: The easy peel property is rated as ◯ and the maximum heat seal strength in the temperature range of 140 to 160° C. is less than 10 N / 15 mm, or the easy peel property is rated as ×
[0085] (Peeled appearance (peeled form)) In the measurement of the heat seal strength, the peeling state of the heat sealed portion of the sample peeled off at a heat seal temperature of 140° C. was confirmed, and the occurrence of edge cuts, cohesive peeling, film cuts, and film tearing was evaluated.
[0086] [Example 1-1] 63 parts by mass of rPP (A-1), 30 parts by mass of BPR (B-1), and 7 parts by mass of LDPE (C-1) were blended to prepare a resin composition. The strain hardening property of the obtained resin composition was evaluated according to the above-mentioned measurement method. The results are shown in Table 1.
[0087] [Example 1-2, Comparative Examples 1-1 to 1-2] Resin compositions were prepared in the same manner as in Example 1-1, except that the composition of the resin composition was changed to the composition shown in Table 1. The strain hardening property of each of the obtained resin compositions was evaluated according to the measurement method described above. The results are shown in Table 1.
[0088] [Table 1]
[0089] [Example 2-1] A resin composition for producing a sealant layer was prepared by blending 66.5 parts by mass of rPP (A-1), 28.5 parts by mass of BPR (B-1), and 5 parts by mass of high-pressure low-density polyethylene (C). Furthermore, 1000 ppm of erucic acid amide as a slip agent and 1200 ppm of silica (particle size 3 μm) as an antiblocking agent were added to the resin composition and blended.
[0090] Using two extruders connected to a T-die, the resin composition for producing the sealant layer to which the additives were added and rPP (A-1) for producing the base layer were fed to each extruder, the die and resin temperatures were set to 230°C, and the extrusion amount of each extruder was adjusted to produce an unstretched film in which a 25 μm-thick unstretched base layer and a 10 μm-thick unstretched sealant layer were laminated by co-extrusion molding. Next, a 25 μm-thick stretched PP film (manufactured by Mitsui Chemicals Tohcello Co., Ltd.) was laminated on the base layer surface of the obtained unstretched film via an adhesive layer by dry lamination to produce a laminate. Using this laminate, low-temperature sealability, easy peelability, and sealability were determined according to the above-mentioned method. The results are shown in Table 2.
[0091] [Examples 2-2 to 2-5, Comparative Examples 2-1 to 2-3] A laminate was produced in the same manner as in Example 2-1, except that the composition of the resin composition for producing the sealant layer was changed to the composition shown in Table 1. The low-temperature sealability, easy peel property, and sealability of the obtained laminate were determined by the above-mentioned methods. The results are shown in Table 2.
[0092] [Table 2]
Claims
1. 5 to 94% by mass of a propylene-based polymer (A), 5 to 75% by mass of a 1-butene / α-olefin copolymer (B); High-pressure low-density polyethylene (C) is 1 to 20 mass % (wherein the total of the propylene polymer (A), the copolymer (B) and the polyethylene (C) is 100 mass%); The propylene polymer (A) has a melting point measured by differential scanning calorimetry (DSC) of 120 to 170° C.; The copolymer (B) has a melting point of less than 120° C. as measured by differential scanning calorimetry (DSC) or no melting point is observed by differential scanning calorimetry (DSC), and contains 51 to 99 mol % of structural units derived from 1-butene and 1 to 49 mol % of structural units derived from an α-olefin having 2 to 3 carbon atoms or 5 to 20 carbon atoms (with the proviso that the total of the structural units derived from 1-butene and the structural units derived from the α-olefin is 100 mol %); The polyethylene (C) is a resin composition having a melt flow rate (MFR) measured in accordance with ASTM D1238 at 190° C. under a load of 2.16 kg in the range of 0.1 to 100 g / 10 min.
2. A film comprising the resin composition according to claim 1.
3. A multi-layer film having a sealant layer comprising the resin composition according to claim 1.
4. The multilayer film of claim 3, wherein the sealant layer has a thickness of 3 to 30 μm.
5. A laminate comprising the film according to claim 2 or the multilayer film according to claim 3 or 4, and a stretched film.
6. The laminate of claim 5 , wherein the oriented film is a stretched polypropylene film.
7. The laminate according to claim 5, wherein the stretched film has a thickness of 10 to 50 μm.
8. The laminate according to claim 5, having a maximum heat seal strength in the temperature range of 70 to 120°C in the range of 2 to 10 N / 15 mm.
9. The laminate according to claim 5, having a maximum heat seal strength of 10 N / 15 mm or more in a temperature range of 140 to 160°C.
10. Further comprising at least one functional layer selected from a printing layer, a barrier layer, and an embossed layer; The laminate according to claim 5 , wherein the functional layer is adjacent to or in contact with at least one film selected from the film or multilayer film, and a stretched film via an adhesive layer.
11. A package formed from the laminate according to claim 5.
Citation Information
Patent Citations
Polyolefin resin composition, film, packaging material, multi-chamber container and cover material
JP2012184392A
Polypropylene resin composition, packaging material and package
JP2020090559A
Laminate
JP2021070250A
Laminate film and packaging bag using same
WO2016027885A1