Resin composition for sealing power module and power module

A resin composition with tailored mechanical properties addresses stress-induced cracking in power modules by ensuring creepage distance and stress alleviation, enhancing reliability and appearance.

JP2024141274APending Publication Date: 2024-10-10SUMITOMO BAKELITE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052824
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional power modules experience cracks due to stress concentration at recesses between terminals, leading to reduced insulation and reliability due to thermal expansion and contraction, as shown by thermal cycle tests.

Method used

A resin composition for power modules with specific mechanical properties, including bending strength, molding shrinkage rate, and linear expansion coefficient, is used to form a sealing material with recesses, ensuring a creepage distance and alleviating stress, thereby preventing cracks.

Benefits of technology

The resin composition provides excellent crack resistance and insulation, resulting in improved product reliability and appearance by suppressing crack generation from recesses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024141274000001_ABST
    Figure 2024141274000001_ABST
Patent Text Reader

Abstract

To provide a sealing resin composition that can suppress the occurrence of cracks arising from recesses, if any, between terminals of a sealing portion of a power module, and a power module using this material.SOLUTION: A sealing resin composition is used for a power module 10 including a power semiconductor element 12, an insulating heat dissipation circuit board 20 having metal layers 16 on both sides of a ceramic substrate 14 provided on one or both sides of the power semiconductor element, a plurality of external connection terminals 22 electrically connected to the element and extending in parallel, a sealing material 24 for sealing these, and a recessed portion 26 provided on an outer peripheral side surface of the sealing material between the external connection terminals in a top view in order to ensure a creepage distance between the external connection terminals. The sealing resin composition has a bending strength of 140 MPa or more at room temperature of 25°C measured under specified conditions, and a molding shrinkage rate after molding of 0.2% or less and a molding shrinkage rate after post-curing of 0.15% or less, both measured under specified conditions.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition for sealing a power module, and a power module. [Background technology]

[0002] Conventionally, in power modules in which power semiconductor elements are sealed with a sealing material, a technology has been adopted to ensure a creepage distance between terminals that protrude beyond the outer periphery of the sealing material by forming recesses on the outer periphery side of the sealing material as a countermeasure against tracking.

[0003] Patent Document 1 discloses a power module including a plurality of terminals protruding from the outer peripheral side surface of a sealing material, and a recess formed in a portion of the outer peripheral side surface of the molded resin between the plurality of terminals, the recess having a depth or height sufficient to ensure a creepage distance between the plurality of terminals, and extending across the opposing portion between the plurality of terminals. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 039466 Summary of the Invention [Problem to be solved by the invention]

[0005] Encapsulating materials for power semiconductor elements are required to ensure high reliability and are required to be stable against expansion and contraction due to heat during use.

[0006] However, in conventional power modules, expansion and contraction due to heat during use can cause cracks to form in the sealing material between the terminals, starting from the recesses on the outer peripheral side of the sealing material, and reaching the terminals, resulting in poor appearance and a failure to ensure insulation, which can reduce product reliability. Such phenomena can be confirmed by a thermal cycle test.

[0007] The reason why cracks occur starting from the recesses in the sealing material between the terminals is believed to be because stress is applied to the bottom of the recesses, causing large distortion. This point will be explained with reference to FIG. As shown in Figures 2(a) and 2(b), packages that do not have recesses on the outer side of the encapsulant between the terminals are manufactured by filling and molding the encapsulant while the terminals are expanded at high temperatures, and then curing it. When there are no recesses on the outer side of the encapsulant as in Figure 2(b), the stress and strain are uniform, and there is no localized increase in stress and strain.

[0008] On the other hand, as shown in Figures 2(c) and (d), a package with a recess on the outer peripheral side of the encapsulant between the terminals is also manufactured by filling and molding the encapsulant while the terminals are expanded at high temperature, and then curing it. As shown in Figure 2(d), the recess in the encapsulant between the terminals has a higher degree of freedom to deform toward the upper part of its opening, and stress is alleviated. However, as shown in Figure 2(d), the bottom of the recess has a lower degree of freedom to deform, and is more susceptible to stress, resulting in greater distortion. Furthermore, it is thought that the deformation of the recess shape due to stress increases the stress load at the bottom. In this way, it is believed that in a package in which a recess is provided on the outer peripheral side surface of the sealing material between terminals, the stress load at the bottom of the recess is high and distortion becomes large, causing cracks to occur from the recess. [Means for solving the problem]

[0009] The present inventors have found that, in an encapsulating resin composition used for forming an encapsulating material for a power module, the above-mentioned problems can be solved by providing a cured product obtained from the encapsulating resin composition with a bending strength at room temperature of 25°C and a molding shrinkage rate within predetermined ranges, and have completed the present invention. That is, the present invention can be shown as follows.

[0010] [1] A power semiconductor element; an insulating heat dissipation circuit board provided on one surface or both surfaces of the power semiconductor element, the insulating heat dissipation circuit board having a ceramic substrate and metal layers on both surfaces of the ceramic substrate; A plurality of external connection terminals electrically connected to the power semiconductor element and extending outward in parallel; a sealing material that seals the power semiconductor element, the metal layer of the insulating heat dissipation circuit board that faces the power semiconductor element, and a part of the plurality of external connection terminals; a recess provided on an outer peripheral side surface of the sealing material between the external connection terminals in a top view in order to ensure a creepage distance between the terminals, The bending strength at room temperature (25°C) measured under the following condition 1 is 140 MPa or more, and A resin composition for sealing a power module, which has a molding shrinkage rate after molding of 0.2% or less and a molding shrinkage rate after post-curing of 0.15% or less, both measured under the following condition 2. (Condition 1) Using a low pressure transfer molding machine, the resin composition for sealing a power module is injected into a mold under the conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 120 seconds to obtain a molded product having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded product is then post-cured at 175°C for 4 hours to prepare a test piece. The bending strength (MPa) of the test piece at room temperature (25°C) is measured in accordance with JIS K 6911. (Condition 2) The resin composition for sealing a power module was molded under conditions of a mold temperature of 175°C, a molding pressure of 9.8 MPa, and a curing time of 120 seconds, and then post-cured at 175°C for 4 days. The mold shrinkage after molding and the mold shrinkage after post-curing of a disk-shaped cured product having a diameter of 100 mm and a thickness of 3 mm were measured, as calculated by the following formula. Formula: Molding shrinkage rate (%) = {(Inner diameter of mold cavity at 25°C - Outer diameter of disc-shaped cured product at 25°C after molding or post-curing) / Inner diameter of mold cavity at 25°C} x 100 [2] The resin composition for sealing a power module according to [1], having a linear expansion coefficient (CTE1) measured under the following condition 3 of 12 ppm / °C or less. (Condition 3) Using a thermomechanical analyzer, the test piece obtained under Condition 1 is measured under conditions of a measurement temperature range of 0° C. to 320° C. and a heating rate of 5° C. / min. From the measurement results, the linear expansion coefficient (CTE1) at 40 to 80° C. is calculated. [3] The resin composition for sealing a power module according to [1] or [2], wherein the flexural modulus measured under the condition 1 is 25,000 MPa or less. [4] The resin composition for sealing a power module according to any one of [1] to [3], wherein the minimum torque value is 1 N m or less when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C. [5] Contains epoxy resin, The resin composition for sealing a power module according to any one of [1] to [4], wherein the epoxy resin contains at least one selected from a biphenyl-type epoxy resin and a tri- or higher functional epoxy resin. [6] The resin composition for sealing a power module according to [5], further comprising a curing agent. [7] further comprising an inorganic filler; The resin composition for sealing a power module according to [6], wherein the content of the inorganic filler is 84 mass% or more relative to 100 mass% of the resin composition for sealing a power module. [8] The resin composition for power module encapsulation according to [7], wherein the content of the resin component contained in the resin composition for power module encapsulation is less than 14 mass% relative to 100 mass% of the resin composition for power module encapsulation. [9] A power semiconductor element; an insulating heat dissipation circuit board provided on one surface or both surfaces of the power semiconductor element, the insulating heat dissipation circuit board having a ceramic substrate and metal layers on both surfaces of the ceramic substrate; A plurality of external connection terminals electrically connected to the power semiconductor element and extending outward in parallel; a sealing material that seals the power semiconductor element, a metal layer of the insulating heat dissipation circuit board that faces the power semiconductor element, and some of the external connection terminals; a recess provided on an outer peripheral side surface of the sealing material between the external connection terminals in a top view in order to ensure a creepage distance between the terminals, A power module, wherein the sealing material has a bending strength of 140 MPa or more at room temperature (25°C) measured in accordance with JIS K 6911.

[10] The power module according to [9], wherein the encapsulant has a coefficient of linear expansion (CTE1) of 12 ppm / °C or less at 40 to 80°C, as measured using a thermomechanical analyzer under conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min.

[11] The power module according to [9] or

[10] , having a flexural modulus at room temperature (25°C) of 25,000 MPa or less, measured in accordance with JIS K 6911.

[12] The power module according to any one of [9] to

[11] , wherein the sealing material between the external connection terminals has residual compressive strain. Effect of the Invention

[0011] According to the present invention, it is possible to provide a resin composition for sealing a power module, which, when used as a sealing material having recesses between terminals in a power module, can provide a sealing material having excellent crack resistance by suppressing the occurrence of cracks arising from the recesses. Furthermore, by using the sealing material, it is possible to provide a power module having excellent product reliability because the appearance is excellent and insulation properties are guaranteed. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1(a) shows a schematic cross-sectional view of the power module of this embodiment, and FIG. 1(b) shows a schematic top view. [Diagram 2] FIG. 2 is a diagram for explaining the reason why cracks occur from recesses in the sealing material between terminals in a conventional power module. [Diagram 3]FIG. 3 is a diagram for explaining that compressive strain remains in the sealing material (recesses) between the external connection terminals in the power module of this embodiment. [Figure 4] FIG. 4(a) is a top view of a power module used in a crack resistance test in an embodiment, and FIG. 4(b) is a cross-sectional view taken along line XX' in FIG. 4(a). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described with reference to the drawings. In all drawings, the same components are denoted by the same reference numerals, and the description will be omitted as appropriate. For example, "1 to 10" means "1 or more" to "10 or less" unless otherwise specified.

[0014] The encapsulating resin composition of the present embodiment is used as a power module encapsulating resin composition. First, the power module will be described.

[0015] <Power module> As shown in FIG. 1(a), a power module 10 includes a power semiconductor element 12, an insulating heat dissipation circuit board 20, an external connection terminal 22, and a sealing material .

[0016] Examples of the power semiconductor element 12 include an IGBT (Insulated Gate Bipolar Transistor), a power transistor, a power MOSFET (Metal Oxide Semiconductor Field Effect Transistor), a GaN-HEMT (High Electron Mobility Transistor), and a SiC MOSFET.

[0017] The sealing material 24 seals the power semiconductor element 12, the metal layer 16 of the insulating heat dissipation circuit board 20 facing the power semiconductor element 12, and parts of the external connection terminals 22. As shown in Fig. 1(b), the sealing material 24 has a rectangular shape when viewed from above.

[0018] 1(b), the power module 10 has a plurality of external connection terminals 22, which extend outward in parallel and protrude from the outer peripheral side surface of the sealing material 24. The external connection terminals 22 are electrically connected to the power semiconductor elements 12 via solder, wires, or the like, and can be electrically connected to an external device via the exposed external connection terminals 22 that are not sealed by the sealing material 24.

[0019] As shown in FIG. 1(b), the outer circumferential side surface of the sealing material 24 between the external connection terminals 22, 22 is provided with a recess (notch, cut) 26 provided to ensure a creepage distance between the external connection terminals 22, 22.

[0020] As shown in FIG. 1(a), the insulating heat dissipation circuit board 20 is provided on both sides of the power semiconductor element 12, but it may be provided on one side of the power semiconductor element 12.

[0021] The insulating heat dissipation circuit board 20 has metal layers 16, 16 laminated on both sides of a ceramic substrate 14. The ceramic substrate 14 may be made of alumina, aluminum nitride, silicon nitride, etc. The metal layer 16 may be a layer made of copper or aluminum.

[0022] A base substrate (heat dissipation substrate) (not shown), or a base substrate (heat dissipation substrate) and a heat dissipation member are laminated in this order on the insulating heat dissipation circuit substrate 20, so that the heat of the power semiconductor elements can be dissipated. Examples of the heat dissipation member include heat dissipation fins. The power module sealing resin composition constituting the sealing material 24 will be described below.

[0023] <Power module encapsulation resin composition> The power module encapsulating resin composition of the present embodiment (hereinafter also referred to as the encapsulating resin composition) has a bending strength (a) at room temperature (25° C.) of 140 MPa or more, measured under the following condition 1: The mold shrinkage rate (b1) after molding is 0.2% or less, and the mold shrinkage rate (b2) after post-curing is 0.15% or less, as measured under the following condition 2. (Condition 1) Using a low pressure transfer molding machine, the resin composition for sealing a power module is injected into a mold under the conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 120 seconds to obtain a molded product having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded product is then post-cured at 175°C for 4 hours to prepare a test piece. The bending strength (MPa) of the test piece at room temperature (25°C) is measured in accordance with JIS K 6911. (Condition 2) The resin composition for sealing a power module was molded under conditions of a mold temperature of 175°C, a molding pressure of 9.8 MPa, and a curing time of 120 seconds, and then post-cured at 175°C for 4 days. The mold shrinkage after molding and the mold shrinkage after post-curing of a disk-shaped cured product having a diameter of 100 mm and a thickness of 3 mm were measured, as calculated by the following formula. Formula: Molding shrinkage rate (%) = {(Inner diameter of mold cavity at 25°C - Outer diameter of disc-shaped cured product at 25°C after molding or post-curing) / Inner diameter of mold cavity at 25°C} x 100

[0024] As shown in FIG. 1, the package of the power module 10 contains a mixture of a ceramic substrate 14 with a low linear expansion coefficient and a metal substrate 16 with a high linear expansion coefficient, which constitute the insulating heat dissipation circuit board 20. This causes a large stress load due to thermal expansion and contraction, which causes cracks in the sealing material, particularly in sealing materials with recesses between terminals. As a result of focusing on and studying the mechanical strength and molding shrinkage of the sealing material, it was found that by setting the bending strength (a) at room temperature of 25°C, the molding shrinkage (b1) after molding, and the molding shrinkage (b2) after post-curing within a predetermined range, the stress caused by the difference in linear expansion coefficient between the ceramic substrate 14 and the metal substrate 16 can be alleviated, and the occurrence of cracks can be suppressed, and the present invention was completed. That is, by setting the characteristics (a), (b1), and (b2) within the above ranges, when the sealing material is used as a sealing material with recesses between the terminals of a power module, the occurrence of cracks caused by the recesses is suppressed, and a power module with excellent appearance and product reliability can be obtained.

[0025] From the viewpoint of the effects of the present invention, the bending strength (a) at room temperature of 25° C. is preferably 145 MPa or more, more preferably 150 MPa or more, and even more preferably 152 MPa or more. The upper limit of the bending strength (a) is not particularly limited, but can be 300 MPa or less. From the viewpoint of the effects of the present invention, the molding shrinkage rate (b1) after molding is preferably 0.18% or less, more preferably 0.15% or less, and further preferably 0.13% or less. The lower limit of the molding shrinkage rate (b1) is not particularly limited, but can be 0.02% or more. From the viewpoint of the effects of the present invention, the mold shrinkage rate (b2) after post-curing is preferably 0.12% or less, more preferably 0.10% or less, and further preferably 0.08% or less. The lower limit of the mold shrinkage rate (b2) is not particularly limited, but can be 0.005% or more. The numerical ranges of the bending strength (a), molding shrinkage rate (b1) and molding shrinkage rate (b2) can be appropriately combined. By setting the characteristics (a), (b1) and (b2) within the preferred ranges as described above, the occurrence of cracks can be further suppressed.

[0026] The power module encapsulating resin composition of the present embodiment can have a coefficient of linear expansion (CTE1)(c) measured under the following condition 3 of 12 ppm / ° C. or less, preferably 10 ppm / ° C. or less, more preferably 8 ppm / ° C. or less, and further preferably 7 ppm / ° C. or less. The lower limit is not particularly limited, but can be 1 ppm / ° C. or more. (Condition 3) Using a thermomechanical analyzer, the test piece obtained under Condition 1 is measured under conditions of a measurement temperature range of 0° C. to 320° C. and a heating rate of 5° C. / min. From the measurement results, the linear expansion coefficient (CTE1) at 40 to 80° C. is calculated.

[0027] By having the linear expansion coefficient (CTE1)(c) within the above range, the stress caused by the difference in the linear expansion coefficient between the ceramic substrate 14 and the metal substrate 16 is further alleviated, and the occurrence of cracks arising from the recesses is further suppressed, making it possible to provide a power module with superior appearance and product reliability.

[0028] The power module encapsulating resin composition of the present embodiment can have a flexural modulus (d) of 25,000 MPa or less, preferably 24,000 MPa or less, and more preferably 23,000 MPa or less, measured under the above-mentioned condition 1. The lower limit is not particularly limited, but can be 10,000 MPa or more.

[0029] By having the flexural modulus (d) within the above range, stress on the package (sealing material) caused by thermal history can be alleviated, and since the crack resistance is superior, the occurrence of cracks arising from the recesses is further suppressed, making it possible to provide a power module with superior appearance and product reliability.

[0030] The power module encapsulating resin composition of this embodiment can have a minimum torque value (e) of 1 N·m or less, preferably 0.8 N·m or less, and more preferably 0.6 N·m or less, when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175° C. The lower limit is not particularly limited, but can be 0.1 N·m or more. When the encapsulating resin composition of the present embodiment has a minimum torque value (e) within the above range, the composition has high fluidity and excellent moldability.

[0031] In the present embodiment, the physical properties of the power module encapsulating resin composition and the cured product can be controlled by appropriately selecting the type and amount of each component contained in the encapsulating resin composition, the preparation method of the encapsulating resin composition, and the like. Each component contained in the power module encapsulating resin composition of the present embodiment will be described.

[0032] [Epoxy resin] The power module encapsulating resin composition of the present embodiment can contain an epoxy resin.

[0033] As the epoxy resin, known epoxy resins can be used within the scope of the effects of the present invention, for example, bisphenol type epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, tetramethylbisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol E type epoxy resin, bisphenol M type epoxy resin, bisphenol P type epoxy resin, and bisphenol Z type epoxy resin; Multifunctional epoxy resins with three or more functionalities, such as trisphenylmethane type epoxy resins and alkyl-modified triphenolmethane type epoxy resins; Novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; Examples of the epoxy resin include biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, aryl alkylene type epoxy resins, naphthalene type epoxy resins, anthracene type epoxy resins, phenoxy type epoxy resins, dicyclopentadiene type epoxy resins, norbornene type epoxy resins, adamantane type epoxy resins, and fluorene type epoxy resins.

[0034] The resin molding material of the present embodiment may contain only one type of epoxy resin, or may contain two or more types of epoxy resins. Furthermore, even if the epoxy resins are the same type, those having different molecular weights may be used in combination.

[0035] The epoxy resin preferably contains at least one selected from biphenyl-type epoxy resins and trifunctional or higher polyfunctional epoxy resins. The moderate rigidity of the structure of these epoxy resins can improve the heat resistance and durability of the resulting molded article. As the polyfunctional epoxy resin having three or more functional groups, a trisphenylmethane type epoxy resin is preferable.

[0036] Specifically, triphenylmethane type epoxy resin is an epoxy resin containing a partial structure in which three of the four hydrogen atoms of methane (CH4) are replaced with a benzene ring. The benzene ring may be unsubstituted or substituted with a substituent. Examples of the substituent include a hydroxyl group and a glycidyloxy group.

[0037] Specifically, the triphenylmethane type epoxy resin contains a structural unit represented by the following general formula (a1): Two or more of these structural units are linked together to form a triphenylmethane skeleton.

[0038] [ka]

[0039] In general formula (a1), R 11each independently, when there are two or more, is a monovalent organic group, a halogen atom, a hydroxyl group, or a cyano group; R 12 each independently, when there are two or more, is a monovalent organic group, a halogen atom, a hydroxyl group, or a cyano group; i is an integer from 0 to 3; j is an integer from 0 to 4.

[0040] R 11 and R 12 Examples of the monovalent organic group include R in the general formula (BP) described below. a and R b Examples of the monovalent organic group include those listed as the monovalent organic group. Each of i and j independently is preferably 0 to 2, and more preferably 0 to 1.

[0041] In one embodiment, both i and j are 0. That is, in one embodiment, all of the benzene rings in general formula (a1) have no substituents other than the explicitly stated glycidyloxy group as monovalent substituents.

[0042] Specifically, the biphenyl type epoxy resin is an epoxy resin containing a structure in which two benzene rings are linked by a single bond. The benzene ring here may or may not have a substituent. Specifically, an epoxy resin containing a biphenyl structure has a partial structure represented by the following general formula (BP).

[0043] [ka]

[0044] In the general formula (BP), R a and R b each independently, when there are more than one, is a monovalent organic group, a hydroxyl group, or a halogen atom; r and s each independently represent 0 to 4; * indicates a bond to another atomic group.

[0045] R a and R b Specific examples of the monovalent organic group include an alkyl group, an alkenyl group, an alkynyl group, an alkylidene group, an aryl group, an aralkyl group, an alkaryl group, a cycloalkyl group, an alkoxy group, a heterocyclic group, and a carboxyl group.

[0046] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Examples of the alkenyl group include an allyl group, a pentenyl group, and a vinyl group.

[0047] The alkynyl group includes, for example, an ethynyl group. Examples of the alkylidene group include a methylidene group and an ethylidene group. Examples of the aryl group include a tolyl group, a xylyl group, a phenyl group, a naphthyl group, and an anthracenyl group.

[0048] Examples of the aralkyl group include a benzyl group and a phenethyl group. Examples of the alkaryl group include a tolyl group and a xylyl group. Examples of the cycloalkyl group include an adamantyl group, a cyclopentyl group, a cyclohexyl group, and a cyclooctyl group.

[0049] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an s-butoxy group, an isobutoxy group, a t-butoxy group, an n-pentyloxy group, a neopentyloxy group, and an n-hexyloxy group. Examples of the heterocyclic group include an epoxy group and an oxetanyl group.

[0050] R a and R b The total number of carbon atoms in each of the monovalent organic groups is, for example, 1 to 30, preferably 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6. Each of r and s is independently preferably 0 to 2, and more preferably 0 to 1. In one embodiment, both of r and s are 0.

[0051] More specifically, the epoxy resin containing a biphenyl structure has a structural unit represented by the following general formula (BP1).

[0052] [ka]

[0053] In general formula (BP1), R a and R b The definition and specific embodiment of are the same as those of general formula (BP), The definitions and preferred ranges of r and s are the same as those of general formula (BP), R c each independently, when there are more than one, is a monovalent organic group, a hydroxyl group, or a halogen atom; t is an integer from 0 to 3.

[0054] R c Specific examples of the monovalent organic group include R a and R b Examples of the above-mentioned specific examples are the same as those given above. t is preferably 0 to 2, and more preferably 0 to 1.

[0055] The amount of the epoxy resin contained in the power module sealing resin composition of this embodiment (100% by mass) can be preferably 1 to 10% by mass, and more preferably 2 to 8% by mass.

[0056] [Hardening agent] The power module encapsulating resin composition of the present embodiment may contain a curing agent.

[0057] The curing agent is not particularly limited as long as it is capable of reacting with the epoxy group of the epoxy resin to form a bond, and examples of the curing agent include amine compounds such as aliphatic polyamines, aromatic polyamines, aromatic diamines, and diamine diamide; acid anhydrides such as alicyclic acid anhydrides and aromatic acid anhydrides; phenol compounds such as novolac-type phenolic resins; and imidazole compounds.

[0058] The curing agent preferably contains a phenol-based curing agent (phenol compound). This is expected to further improve the durability of the finally obtained molded body. The phenol-based curing agent typically has two or more hydroxyl groups per molecule.

[0059] The phenol-based curing agent preferably contains a skeleton selected from the group consisting of a novolac skeleton and a biphenyl skeleton. When the phenol-based curing agent contains any of these skeletons, the durability of the molded article can be particularly improved. Specifically, the "biphenyl skeleton" is a structure in which two benzene rings are linked by a single bond, as in the general formula (BP) in the above description of the epoxy resin.

[0060] Specific examples of phenol-based curing agents having a biphenyl skeleton include those having a structure in which the glycidyl group in the general formula (BP1) in the above description of epoxy resins is replaced with a hydrogen atom.

[0061] Specific examples of phenol-based curing agents having a novolac skeleton include those having a structural unit represented by the following general formula (N).

[0062] [ka]

[0063] In general formula (N), R 4 represents a monovalent substituent, u is an integer from 0 to 3. R 4 Specific examples of the monovalent substituent include R a and R b Examples of the monovalent substituent include those described above. u is preferably 0 to 2, more preferably 0 to 1, and further preferably 0.

[0064] The amount of the curing agent contained in the power module sealing resin composition of this embodiment (100% by mass) can be preferably 1 to 10% by mass, and more preferably 2 to 7% by mass.

[0065] The content of the resin components (epoxy resin + curing agent) contained in the power module encapsulating resin composition of this embodiment is preferably less than 14 mass%, more preferably 12 mass% or less, and even more preferably 10 mass% or less, relative to 100 mass% of the power module encapsulating resin composition. By having the amount of the resin component fall within the above range, the composition has excellent high strength and low shrinkage, and it becomes easier to adjust the properties (a), (b1), and (b2) to the desired ranges.

[0066] [Inorganic filler] The power module encapsulating resin composition of the present embodiment can contain an inorganic filler.

[0067] As the inorganic filler, any of those generally used in semiconductor encapsulation resin compositions can be used. The inorganic filler may be surface-treated.

[0068] Specific examples of inorganic fillers include silica such as fused silica, crystalline silica, and amorphous silicon dioxide; alumina; talc; titanium oxide; silicon nitride; and aluminum nitride. These inorganic fillers may be used alone or in combination of two or more. The inorganic filler preferably contains silica from the viewpoint of excellent versatility. Examples of the shape of the silica include spherical silica and crushed silica.

[0069] Average diameter of inorganic filler (D 50 From the viewpoint of improving moldability and adhesion, the thickness is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 80 μm or less, more preferably 50 μm or less, and even more preferably 40 μm or less.

[0070] Here, the particle size distribution of the inorganic filler can be obtained by measuring the particle size distribution of the particles on a volume basis using a commercially available laser diffraction particle size distribution measuring device (for example, SALD-7000 manufactured by Shimadzu Corporation).

[0071] The content of the inorganic filler in the power module encapsulating resin composition is preferably 84 mass% or more, more preferably 86 mass% or more, and even more preferably 88 mass% or more, relative to 100 mass% of the entire encapsulating resin composition, from the viewpoint of improving the low moisture absorption and low thermal expansion properties of the encapsulating material formed using the encapsulating resin composition and more effectively improving the moisture resistance reliability and reflow resistance of the obtained power module.

[0072] In addition, from the viewpoint of more effectively improving the fluidity and filling property during molding of the encapsulating resin composition, the content of the inorganic filler in the encapsulating resin composition is preferably 97 mass % or less, more preferably 95 mass % or less, and even more preferably 93 mass % or less, relative to 100 mass % of the entire encapsulating resin composition. By setting the amount of the inorganic filler within the above range, the composition has excellent high strength and low shrinkage, and it becomes easier to adjust the properties (a), (b1), and (b2) within the desired ranges.

[0073] [Coupling agent] The power module encapsulating resin composition of the present embodiment may contain a coupling agent. The coupling agent here is contained in the encapsulating resin composition as a single coupling agent. For example, the above-mentioned coupling agent used in the surface treatment of the inorganic filler (combined with the inorganic filler) does not fall under the coupling agent here.

[0074] As the coupling agent, for example, various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, methacrylsilane, titanium-based compounds, aluminum chelates, aluminum / zirconium-based compounds, and other known coupling agents can be used. More specifically, the following can be exemplified.

[0075] ·Silane coupling agents Vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-[bis(β-hydroxyethyl)]aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(amino N-ethyl)-γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, phenylaminopropyltrimethoxysilane, γ-(β-aminoethyl)aminopropyldimethoxymethylsilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilane, vinyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, hydrolyzate of 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and the like.

[0076] Titanate coupling agent Isopropyl triisostearoyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecyl benzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, tetraisopropyl bis(dioctyl phosphite) titanate, and the like. When the encapsulating resin composition contains a coupling agent, it may contain only one type of coupling agent, or may contain two or more types of coupling agents.

[0077] The content of the coupling agent is preferably 0.1% by mass or more, and more preferably 0.15% by mass or more, based on 100% by mass of the entire encapsulating resin composition. By making the content of the coupling agent equal to or more than the above lower limit, the dispersibility of the inorganic filler can be improved.

[0078] On the other hand, the content of the coupling agent is preferably 1 mass % or less, more preferably 0.5 mass % or less, based on the total of the encapsulating resin composition. By making the content of the coupling agent equal to or less than the upper limit, the flowability of the encapsulating resin composition during encapsulation molding can be improved, and the filling property and moldability can be improved, and the strength of the encapsulating material can be increased.

[0079] [Curing catalyst] The power module encapsulating resin composition of the present embodiment may further contain a curing catalyst. The curing catalyst may also be called a curing accelerator, etc. The curing catalyst is not particularly limited as long as it accelerates the curing reaction of the thermosetting resin, and any known curing catalyst may be used.

[0080] Specific examples of the curing catalyst include phosphorus atom-containing compounds such as organic phosphines, tetra-substituted phosphonium compounds, phosphobetaine compounds, adducts of phosphine compounds and quinone compounds, and adducts of phosphonium compounds and silane compounds; imidazoles (imidazole curing accelerators) such as 2-methylimidazole and 2-phenylimidazole; and nitrogen atom-containing compounds such as amidines and tertiary amines, exemplified by 1,8-diazabicyclo[5.4.0]undecene-7 and benzyldimethylamine, and quaternary salts of amidines and amines. Only one type may be used, or two or more types may be used.

[0081] Among these, from the viewpoint of improving the curability and obtaining a sealing material excellent in mechanical strength such as bending strength, it is preferable to contain a phosphorus atom-containing compound, more preferably to contain a compound having latency such as a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound, and particularly preferably a tetra-substituted phosphonium compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound.

[0082] By using the epoxy resin (A) containing a naphthol aralkyl type epoxy resin in combination with a latent curing catalyst, it is possible to obtain an encapsulating material which is excellent in moldability and mechanical strength such as bending strength.

[0083] Examples of the organic phosphines include primary phosphines such as ethylphosphine and phenylphosphine; secondary phosphines such as dimethylphosphine and diphenylphosphine; and tertiary phosphines such as trimethylphosphine, triethylphosphine, tributylphosphine and triphenylphosphine. Examples of the tetra-substituted phosphonium compound include compounds represented by the following general formula (6).

[0084] [ka]

[0085] In general formula (6), P represents a phosphorus atom. R 4 , R 5 , R 6 and R 7 each independently represents an aromatic group or an alkyl group. A represents the anion of an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring.

[0086] AH represents an aromatic organic acid having at least one functional group selected from a hydroxyl group, a carboxyl group, and a thiol group on an aromatic ring. x and y are 1 to 3, z is 0 to 3, and x=y. The compound represented by the general formula (6) can be obtained, for example, as follows.

[0087] First, a tetra-substituted phosphonium halide, an aromatic organic acid, and a base are mixed uniformly in an organic solvent to generate an aromatic organic acid anion in the solution system. Then, water is added to precipitate the compound represented by general formula (6). In the compound represented by general formula (6), R bonded to the phosphorus atom 4 , R 5 , R 6 and R 7is preferably a phenyl group, AH is a compound having a hydroxyl group on an aromatic ring, i.e., a phenol, and A is an anion of the phenol. Examples of the phenol include monocyclic phenols such as phenol, cresol, resorcin, and catechol, condensed polycyclic phenols such as naphthol, dihydroxynaphthalene, and anthraquinol, bisphenols such as bisphenol A, bisphenol F, and bisphenol S, and polycyclic phenols such as phenylphenol and biphenol.

[0088] Examples of the phosphobetaine compound include compounds represented by the following general formula (7).

[0089] [ka]

[0090] In general formula (7), P represents a phosphorus atom. R 8 is an alkyl group having 1 to 3 carbon atoms, R 9 represents a hydroxyl group. f is 0 to 5 and g is 0 to 3. The compound represented by the general formula (7) can be obtained, for example, as follows.

[0091] First, a triaromatic substituted phosphine, which is a tertiary phosphine, is contacted with a diazonium salt to substitute the diazonium group of the diazonium salt for the triaromatic substituted phosphine.

[0092] Examples of the adduct of a phosphine compound and a quinone compound include compounds represented by the following general formula (8).

[0093] [ka]

[0094] In general formula (8), P represents a phosphorus atom. R 10 , R 11 and R 12 represents an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 12 carbon atoms, and may be the same or different.

[0095] R 13 , R 14 and R 15 represents a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms, and may be the same or different; R 14 and R 15 may be bonded to form a cyclic structure.

[0096] The phosphine compound used in the adduct of the phosphine compound and the quinone compound is preferably, for example, triphenylphosphine, tris(alkylphenyl)phosphine, tris(alkoxyphenyl)phosphine, trinaphthylphosphine, tris(benzyl)phosphine, etc., which is unsubstituted or has a substituent such as an alkyl group or an alkoxy group on the aromatic ring, and examples of the substituent such as the alkyl group or alkoxy group include those having a carbon number of 1 to 6. From the viewpoint of availability, triphenylphosphine is preferred.

[0097] As the quinone compound used in the adduct of the phosphine compound and the quinone compound, benzoquinone and anthraquinones can be mentioned, and among them, p-benzoquinone is preferred from the viewpoint of storage stability.

[0098] The method for producing an adduct of a phosphine compound and a quinone compound is to contact and mix the organic tertiary phosphine and the benzoquinone in a solvent in which both can dissolve, to obtain the adduct. The solvent is preferably a ketone such as acetone or methyl ethyl ketone, which has low solubility in the adduct, but is not limited thereto.

[0099] In the compound represented by the general formula (8), R, R, and R bonded to the phosphorus atom are phenyl groups, and R13 , R 14 and R 15 A compound in which is a hydrogen atom, that is, an addition compound of 1,4-benzoquinone and triphenylphosphine, is preferred in terms of decreasing the hot elastic modulus of the cured product of the encapsulating resin composition.

[0100] Examples of the adduct of a phosphonium compound and a silane compound include a compound represented by the following general formula (9).

[0101] [ka]

[0102] In general formula (9), P represents a phosphorus atom, and Si represents a silicon atom. R 16 , R 17 , R 18 and R 19 each represents an organic group having an aromatic ring or a heterocycle, or an aliphatic group, and may be the same or different. R 20 is the group Y 2 and Y 3 It is an organic group that bonds to R 21 is the group Y 4 and Y 5 It is an organic group that bonds to

[0103] Y 2 and Y 3 represents a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure.

[0104] Y 4 and Y 5 represents a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. R 20 , and R 21 may be the same or different, and Y 2 , Y 3 , Y 4 and Y 5 may be the same or different from each other. Z1 is an organic group having an aromatic ring or a heterocyclic ring, or an aliphatic group.

[0105] In the general formula (9), R 16 , R 17 , R 18 and R 19 Examples of the alkyl group include a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, a naphthyl group, a hydroxynaphthyl group, a benzyl group, a methyl group, an ethyl group, an n-butyl group, an n-octyl group, and a cyclohexyl group. Among these, an aromatic group having a substituent such as an alkyl group, an alkoxy group, or a hydroxyl group, such as a phenyl group, a methylphenyl group, a methoxyphenyl group, a hydroxyphenyl group, or a hydroxynaphthyl group, or an unsubstituted aromatic group is more preferable.

[0106] In the general formula (9), R 20 is Y 2 and Y 3 Similarly, R 21 is the group Y 4 and Y 5 It is an organic group that bonds with Y. 2 and Y 3 is a group formed by releasing a proton from a proton-donating group, and a group Y 2 and Y 3 is bonded to a silicon atom to form a chelate structure. 4 and Y 5 is a group formed by releasing a proton from a proton-donating group, and a group Y 4 and Y 5 is bonded to a silicon atom to form a chelate structure. 20 and R 21 may be the same or different, and the group Y2 , Y 3 , Y 4 and Y5 may be the same or different. 2 -R 20 -Y 3 - and Y 4 -R 21 -Y 5 The group represented by - is composed of a group formed by releasing two protons from a proton donor. As the proton donor, an organic acid having at least two carboxyl groups or hydroxyl groups in the molecule is preferable, an aromatic compound having at least two carboxyl groups or hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable, and an aromatic compound having at least two hydroxyl groups on adjacent carbons constituting an aromatic ring is more preferable. Examples of the proton donor include catechol, pyrogallol, 1,2-dihydro- Examples of the hydroxynaphthalene include xynaphthalene, 2,3-dihydroxynaphthalene, 2,2'-biphenol, 1,1'-bi-2-naphthol, salicylic acid, 1-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, chloranilic acid, tannic acid, 2-hydroxybenzyl alcohol, 1,2-cyclohexanediol, 1,2-propanediol, and glycerin. Of these, catechol, 1,2-dihydroxynaphthalene, and 2,3-dihydroxynaphthalene are more preferred.

[0107] Z in general formula (9) 1 represents an organic group or an aliphatic group having an aromatic ring or a heterocyclic ring, and specific examples thereof include aliphatic hydrocarbon groups such as methyl group, ethyl group, propyl group, butyl group, hexyl group, and octyl group; aromatic hydrocarbon groups such as phenyl group, benzyl group, naphthyl group, and biphenyl group; glycidyloxy groups such as glycidyloxypropyl group, mercaptopropyl group, and aminopropyl group; mercapto group; and reactive substituents such as an alkyl group having an amino group and a vinyl group. Among these, the methyl group, the ethyl group, the phenyl group, the naphthyl group, and the biphenyl group are more preferable in terms of thermal stability. A method for producing an adduct of a phosphonium compound and a silane compound is, for example, as follows.

[0108] In a flask containing methanol, a silane compound such as phenyltrimethoxysilane and a proton donor such as 2,3-dihydroxynaphthalene are dissolved, and then a sodium methoxide-methanol solution is added dropwise at room temperature with stirring. A previously prepared solution of a tetra-substituted phosphonium halide such as tetraphenylphosphonium bromide dissolved in methanol is then added dropwise at room temperature with stirring, causing crystals to precipitate. The precipitated crystals are filtered, washed with water, and vacuum dried to obtain an adduct of the phosphonium compound and the silane compound.

[0109] When a curing catalyst is used, the content thereof is preferably 0.01 to 3 mass %, more preferably 0.03 to 2 mass %, relative to 100 mass % of the power module encapsulating resin composition. By setting the content within such a numerical range, a sufficient curing promotion effect can be obtained without excessively impairing other performances.

[0110] [Rubber particles] The encapsulating resin composition of the present embodiment may contain rubber particles. The resin composition containing the rubber particles has high strength and low elastic modulus, and therefore has high toughness. As the rubber particles, core-shell type rubber particles are preferably used because they have an excellent toughening effect.

[0111] The core-shell type rubber particles refer to rubber particles in which a particulate core component, mainly composed of a crosslinked rubbery polymer, is coated in part or in whole with a shell component by graft polymerizing a polymer different from the core component onto the surface of the particulate core component.

[0112] The core component may be, for example, a crosslinked rubber particle. Examples of the crosslinked rubber particle include a diene rubber, an acrylic rubber, and a polysiloxane rubber. More specifically, examples of the crosslinked rubber include butadiene rubber, acrylic rubber, silicone rubber, butyl rubber, nitrile rubber, styrene rubber, synthetic natural rubber, and ethylene propylene rubber.

[0113] Examples of the shell component include diene rubber, acrylic rubber, and polysiloxane rubber. Preferably, the shell component is a polymer obtained by polymerizing one or more monomers selected from the group consisting of acrylic acid esters, methacrylic acid esters, and aromatic vinyl compounds. The shell component is preferably graft-polymerized to the core component and chemically bonded to the polymer that constitutes the core component. When a crosslinked rubber-like polymer composed of a polymer of styrene and butadiene is used as the core component, it is preferable to use a polymer of methyl methacrylate, which is a methacrylic acid ester, and styrene, which is an aromatic vinyl compound, as the shell component.

[0114] Commercially available core-shell rubber particles include, for example, "PARALOID (registered trademark)" EXL-2655 (manufactured by Kureha Chemical Industry Co., Ltd.), which is made of a butadiene-alkyl methacrylate-styrene copolymer; "STAFILOID (registered trademark)" AC-3355, TR-2122 (manufactured by Takeda Pharmaceutical Co., Ltd.), which are made of an acrylic acid ester-methacrylic acid ester copolymer; "PARALOID (registered trademark)" EXL-2611, EXL-3387 (manufactured by Rohm & Haas Co., Ltd.), which are made of a butyl acrylate-methyl methacrylate copolymer; and "KANE ACE (registered trademark)" MX series (manufactured by Kaneka Corporation).

[0115] The content of the rubber particles is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, based on 100% by mass of the entire encapsulating resin composition, since a resin composition capable of forming a cured product having high strength and low elastic modulus can be obtained. The upper limit of the content of the rubber particles is preferably 5% by mass or less, more preferably 3% by mass or less.

[0116] The average particle size of the primary particles of the rubber particles is preferably in the range of 50 to 500 nm, and more preferably in the range of 50 to 300 nm, since a resin composition capable of forming a cured product having high strength and low elastic modulus can be obtained.

[0117] [Other ingredients] The resin composition for sealing a power module of the present embodiment may contain components other than the above-mentioned components, and may contain various additives such as an ion scavenger, a flame retardant, a release agent, a stress reducing agent, a colorant, and an adhesion assistant.

[0118] As the ion capturing agent (also called an ion catcher or an ion trapping agent), for example, hydrotalcite can be used. Bismuth oxide and yttrium oxide are also known as ion capturing agents. When an ion scavenger is used, only one type may be used, or two or more types may be used in combination. When an ion scavenger is used, the amount thereof is, for example, 0.01 to 0.5 mass %, and preferably 0.05 to 0.3 mass %, based on the total amount of the encapsulating resin composition.

[0119] Examples of flame retardants include inorganic flame retardants (for example, hydrated metal compounds such as aluminum hydroxide, available from Sumitomo Chemical Co., Ltd., etc.), halogen-based flame retardants, phosphorus-based flame retardants, and organic metal salt-based flame retardants. When a flame retardant is used, only one type may be used, or two or more types may be used in combination. The amount of the flame retardant is, for example, 0 to 15 mass %, and preferably 0 to 10 mass %, based on the total amount of the encapsulating resin composition.

[0120] Examples of the release agent include natural waxes, synthetic waxes such as montanic acid esters, higher fatty acids or metal salts thereof, paraffin, and polyethylene oxide. When a release agent is used, only one type may be used, or two or more types may be used in combination. When a release agent is used, the amount thereof is, for example, 0.1 to 0.8 mass %, and preferably 0.2 to 0.5 mass %, based on the total mass of the encapsulating resin composition.

[0121] Examples of the low stress agent include silicone oil, silicone rubber, polyisoprene, polybutadienes such as 1,2-polybutadiene and 1,4-polybutadiene, styrene-butadiene rubber, acrylonitrile-butadiene rubber, polychloroprene, thermoplastic elastomers such as poly(oxypropylene), poly(oxytetramethylene) glycol, polyolefin glycol and poly-ε-caprolactone, polysulfide rubber, and fluororubber.

[0122] Among these, silicone rubber, silicone oil, acrylonitrile-butadiene rubber, and the like are particularly preferred from the viewpoint of controlling the flexural modulus and shrinkage rate within a desired range and suppressing the occurrence of warping in the resulting power device. When using a low stress agent, only one type may be used, or two or more types may be used in combination. The amount of the stress reducing agent is, for example, 0.05 to 5 mass %, and preferably 0.1 to 3 mass %, based on the total amount of the encapsulating resin composition.

[0123] <Power module encapsulation resin composition> The power module encapsulating resin composition of the present embodiment is solid at room temperature (25° C.), and its shape can be selected depending on the molding method of the encapsulating resin composition, etc., and examples thereof include a tablet form; a particulate form such as a powder form or a granule form; and a sheet form.

[0124] The encapsulating resin composition can be produced, for example, by mixing the above-mentioned components by known means, melt-kneading them with a kneader such as a roll, a kneader or an extruder, cooling, and then pulverizing them. After pulverization, the mixture may be molded to obtain a particulate or sheet-like encapsulating resin composition. For example, the particulate encapsulating resin composition may be molded into a tablet shape. For example, a sheet-like encapsulating resin composition may be obtained by a vacuum extruder.

[0125] The power module sealing resin composition of this embodiment can be used for transfer molding, injection molding, or compression molding. Furthermore, by using the encapsulating resin composition obtained in this embodiment, a power module having excellent appearance and excellent product reliability can be obtained.

[0126] <Power module> The power module of this embodiment has the above-mentioned configuration shown in Fig. 1. As shown in Fig. 1(a), the insulating heat dissipation circuit board 20 is provided on both sides of the power semiconductor element 12, but may be provided on one side of the power semiconductor element 12.

[0127] The sealing material 24 constituting the power module 10 has a bending strength at room temperature of 25° C. of 140 MPa or more, preferably 145 MPa or more, more preferably 150 MPa or more, and further preferably 152 MPa or more, measured in accordance with JIS K 6911. The upper limit of the bending strength is not particularly limited, but can be 300 MPa or less. When the bending strength is within the above range, the mechanical strength of the sealing material 24 is improved, making it possible to provide a power module with superior appearance and product reliability.

[0128] Furthermore, the sealing material 24 can have a coefficient of linear expansion (CTE1) at 40 to 80° C., measured using a thermomechanical analyzer under conditions of a measurement temperature range of 0° C. to 320° C. and a temperature increase rate of 5° C. / min, of 12 ppm / ° C. or less, preferably 10 ppm / ° C. or less, more preferably 8 ppm / ° C. or less, and further preferably 7 ppm / ° C. or less. The lower limit is not particularly limited, but can be 1 ppm / ° C. or more.

[0129] By having the linear expansion coefficient (CTE1) within the above range, the effect of the difference in the linear expansion coefficient between the ceramic substrate 14 and the metal substrate 16 can be reduced, the occurrence of cracks arising from the recesses is further suppressed, and a power module with superior appearance and product reliability can be provided.

[0130] The sealing material 24 may have a flexural modulus of 25,000 MPa or less, preferably 24,000 MPa or less, and more preferably 23,000 MPa or less at room temperature of 25° C., measured in accordance with JIS K 6911. The lower limit is not particularly limited, but may be 10,000 MPa or more.

[0131] By ensuring that the flexural modulus is within the above range, the stress on the package (sealing material) caused by thermal history can be alleviated, and since the crack resistance is superior, the occurrence of cracks arising from the recesses is further suppressed, making it possible to provide a power module with superior appearance and superior product reliability.

[0132] In the power module of this embodiment, compressive strain remains in the sealing material between the external connection terminals. This point will be described with reference to FIG. As shown in Figures 3(a) and (b), power modules are manufactured by filling and molding an encapsulating resin composition while the terminals are in a state of expansion at high temperatures, followed by curing. When the molding shrinkage rate of the encapsulating resin composition is large as in the past, the shrinkage of the encapsulating material becomes greater than the shrinkage of the terminals after molding (at room temperature), as shown in Figure 3(b). Since the shrinkage of the encapsulating material is greater, it is believed that a stress acts in the tensile direction on the encapsulating material (recesses) between the terminals, and a strain (tensile strain) remains in the tensile direction. On the other hand, in Fig. 3(c) and (d), the power module is also manufactured by filling and molding the encapsulating resin composition in a state in which the terminals are expanded at high temperature, and then curing. Since the molding shrinkage rate of the encapsulating resin composition of this embodiment is small, the shrinkage of the encapsulating material is smaller than the shrinkage of the terminals after molding (at room temperature), as shown in Fig. 3(d). Since the shrinkage of the encapsulating material is smaller, it is considered that a stress acts in the compressive direction on the encapsulating material (recess) between the terminals, and a strain (compressive strain) remains in the compressive direction.

[0133] The power module 10 of this embodiment can be manufactured using the above-mentioned sealing resin composition. Furthermore, a base substrate (not shown) or a base substrate (heat dissipation substrate) and a heat dissipation member (not shown) are laminated in this order on the insulating heat dissipation circuit board 20 of the power module 10, so that the power module 10 can be configured to dissipate heat from the power semiconductor elements. Examples of the heat dissipation member include heat dissipation fins.

[0134] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES

[0135] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0136] [Examples 1-2, Comparative Examples 1-3] A mixture was obtained by mixing the components shown in Table 1 in the amount ratio shown. The mixing was carried out at room temperature using a Henschel mixer.

[0137] The mixture was then roll-kneaded at 70 to 100° C. to obtain a kneaded product. The kneaded product was cooled and then pulverized to obtain an encapsulating resin composition. The components listed in Table 1 are as follows.

[0138] (Inorganic filler) Filler 1: Fused spherical silica (Admatechs, SC-2500-SQ) Filler 2: Fused spherical silica (manufactured by Denka Co., Ltd., FB-950FC)

[0139] (Coloring agent) Colorant 1: Carbon black (manufactured by Tokai Carbon Co., Ltd.)

[0140] (Coupling Agent) Coupling agent 1: N-phenylaminopropyltrimethoxysilane represented by the following formula (S1) (manufactured by Dow Corning Toray Co., Ltd., CF-4083) [ka]

[0141] Coupling agent 2: (Chisso Corporation, S810)

[0142] (Epoxy resin) Epoxy resin 1: Trisphenylmethane type epoxy resin (Mitsubishi Chemical Corporation, E1032H60, solid at room temperature of 25°C) Epoxy resin 2: A mixture of trishydroxyphenylmethane type epoxy resin and 4,4'-biphenol type epoxy resin (manufactured by Mitsubishi Chemical Corporation, jER YL6677, solid at room temperature of 25°C)

[0143] (hardening agent) Hardener 1: Phenol aralkyl type phenolic resin containing biphenylene skeleton (Meiwa Kasei Co., Ltd., MEH-7851SS)

[0144] (curing catalyst) Curing catalyst 1: 4-hydroxy-2-(triphenylphosphonium)phenolate (K.I. Chemicals, TPP-BQ) Curing catalyst 2: 2,3-dihydroxynaphthalene (Air Water Corporation, 2,3-DON)

[0145] (Plasticizer) Epoxidized soybean oil: O-130P, manufactured by ADEKA

[0146] (Flame retardant) Flame retardant 1: Aluminum hydroxide (Sumitomo Chemical Co., Ltd., CL-303, powder)

[0147] (Release agent) Wax 1: Montanic acid wax (Clariant Japan, WE-4) Wax 2: Stearic acid (SR-Sakura, manufactured by Nippon Oil & Fats Co., Ltd.)

[0148] (Ion scavenger) Ion scavenger 1: Hydroxytalcite (Toagosei)

[0149] (Adhesion aid) Adhesion aid 1: Heavy metal deactivator (ADEKA, CDA-1M) Adhesion aid 2: 3-amino-5-mercapto-1,2,4-triazole (Nippon Carbide Corporation)

[0150] (Low stress agent) Silicone oil 1: Silicone oil represented by the following chemical formula (3) (FZ-3730, manufactured by Dow Corning Toray Co., Ltd.) [ka]

[0151] (rubber particles) Core-shell rubber 1: Core-shell rubber (core: butadiene rubber, shell: acrylic rubber) (Dow Chemical Company, EXL-2655) please.

[0152] <Evaluation> The encapsulating resin composition obtained in each example or a sample for evaluation was prepared using the composition by the following method, and various physical properties were evaluated by the following methods.

[0153] (Flexural strength and flexural modulus (room temperature 25℃)) The encapsulating resin compositions of the examples and comparative examples were injected into a mold using a low pressure transfer molding machine (KOTAKISEIKI Co., Ltd. "KTS-30") under conditions of a mold temperature of 175°C, an injection pressure of 9.8MPa, and a curing time of 120 seconds to obtain a molded product having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded product thus obtained was then post-cured at 175°C for 4 hours to prepare a test piece. The flexural strength (MPa) and flexural modulus (MPa) of the test piece at room temperature (25°C) were measured in accordance with JIS K 6911.

[0154] (ASM (Amold Shrinkage)) The encapsulating resin compositions of the Examples and Comparative Examples were transfer molded under the conditions of a mold temperature of 175°C, molding pressure of 9.8 MPa, and curing time of 120 seconds to obtain a disk-shaped cured product having a diameter of 100 mm and a thickness of 3 mm. The mold shrinkage (ASM) of the disk-shaped cured product was calculated using the following formula. More specifically, the dimensions of a disk-shaped mold were measured at four points at room temperature, and the average value was calculated. The encapsulating resin composition was then poured into the mold to mold a disk-shaped cured product, and the diameter (outer dimensions) of the resulting disk-shaped cured product at 25°C was measured at four points corresponding to the points measured on the mold, and the average value was calculated. The obtained values ​​were applied to the following formula to determine the mold shrinkage (ASM) (%). Formula: Molding shrinkage rate (%) = {(inner diameter of mold cavity at 25°C - outer diameter of disk-shaped cured product at 25°C after molding) / inner diameter of mold cavity at 25°C} x 100

[0155] (Molding shrinkage rate (PMC)) The encapsulating resin compositions of the Examples and Comparative Examples were transfer molded under the conditions of a mold temperature of 175°C, molding pressure of 14 MPa, and curing time of 120 seconds to obtain a disk-shaped cured product having a diameter of 100 mm and a thickness of 3 mm. The disk-shaped cured product was cooled to room temperature and then post-cured at 175°C for 4 hours. Furthermore, the diameter (outer dimension) of the resulting disc-shaped cured product at 25° C. was measured at four corresponding points before and after post-cure, and the average value was calculated. The obtained values ​​were applied to the following formula to calculate the mold shrinkage rate (PMC) (%). Formula: Mold shrinkage rate (%) = {(inner diameter of mold cavity at 25°C - outer diameter of disc-shaped cured product at 25°C after post-curing) / inner diameter of mold cavity at 25°C} x 100

[0156] (Coefficient of linear expansion (CTE1)) Using a thermomechanical analyzer (Seiko Denshi Kogyo Co., Ltd., TMA100), the test pieces obtained in the measurement of the "flexural strength and flexural modulus" were measured under the conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min. From the measurement results, the linear expansion coefficient (CTE1) at 40 to 80°C was calculated.

[0157] (Minimum torque value) Using a Labo Plastomill tester (4C150, manufactured by Toyo Seiki Seisakusho), the melt torque value of the encapsulating resin composition was measured over time at a rotation speed of 30 rpm and a measurement temperature of 175° C. to obtain the minimum torque value.

[0158] (Curelast maximum torque and time to reach 80% of maximum torque) Using a curing meter (JSR Curing meter IVPS type, manufactured by Orientec Co., Ltd.), the curing torque of the encapsulating resin composition was measured over time at a mold temperature of 175° C. At this time, the torque at 300 seconds from the start of the measurement was defined as the maximum torque, and the time T80% until the torque reached 80% of the maximum torque was calculated.

[0159] (Gel Time (GT)) Each of the encapsulating resin compositions of the Examples and Comparative Examples was melted on a hot plate heated to 175° C., and the time (unit: seconds) until the composition hardened was measured while kneading with a spatula.

[0160] (Rectangular viscosity) The rectangular flow channel pressure (rectangular pressure) of the encapsulating resin composition of the examples or comparative examples was measured as follows. First, the encapsulating resin composition was injected into a rectangular flow channel having a width of 13 mm, a thickness of 0.5 mm, and a length of 175 mm, using a low-pressure transfer molding machine (NEC, 40t manual press) under conditions of a mold temperature of 175°C and an injection speed of 24.7 mm / sec. At this time, the pressure change over time was measured with a pressure sensor embedded at a position 25 mm from the upstream end of the flow channel, and the minimum pressure (MPa) during the flow of the encapsulating resin composition was measured, and this was taken as the rectangular viscosity (minimum melt viscosity). The rectangular viscosity is a parameter of the melt viscosity, and a smaller value indicates a lower melt viscosity.

[0161] [Glass transition temperature (Tg)] The glass transition temperature Tg (°C) can be measured, for example, by the following method. First, a transfer molding machine is used to inject and mold a semiconductor encapsulation resin composition at a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 3 minutes to obtain a test piece of 15 mm x 4 mm x 4 mm. Next, the obtained test piece is post-cured at 175°C for 4 hours or at 200°C for 4 hours, and then measured using a thermomechanical analyzer (Seiko Denshi Kogyo Co., Ltd., TMA100) under the conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min. From the measurement results, the glass transition temperature Tg (°C) is calculated.

[0162] (Crack resistance) A power semiconductor element was encapsulated by transfer molding using the encapsulating resin compositions of the Examples and Comparative Examples to produce a power module as shown in Fig. 4. Fig. 4(a) shows a top view of the power module, and Fig. 4(b) shows a cross-sectional view of the power module taken along line X-X' in Fig. 4(a). In detail, first, a power semiconductor element (Si / SiC) 12 was mounted on the upper surface of a DBC substrate (insulating heat dissipation circuit substrate 20) (manufactured by Ferrotec Corporation, configuration: Cu (metal layer 16) / ceramic (ceramic substrate 14) / Cu (metal layer 16), size: 28 mm×28 mm, thickness: 920 μm), and an external connection terminal (CuLF) 22 was mounted via solder 21. The DBC substrate (insulating heat dissipation circuit substrate 20) was mounted on the power semiconductor element 12 via a spacer 13. The structure was transfer molded using the sealing resin composition of the examples and comparative examples at a mold temperature of 175° C., injection pressure of 9.3 MPa, and curing time of 90 seconds, and post-cured at 175° C. for 4 hours to obtain a power module. The package size of the obtained power module was 48 mm×90 mm×height 4340 μm. As shown in FIG. 4(a), the size of the recess (notch) 26 provided between the external connection terminals 22 was 2.5 mm×1.0 mm. The obtained power module was subjected to a thermal cycle test of 1000 cycles in a temperature range of −40° C. to 125° C. using a thermal cycle tester. Next, the power module after the thermal cycle test was examined using an electron microscope to check for the presence or absence of cracks arising from the recesses 26, and was evaluated according to the following criteria. (standard) ◯: No cracks were observed. ×: Cracks were observed.

[0163] [Table 1]

[0164] As shown in Table 1, according to the power module sealing resin composition of the embodiment of the present invention, the occurrence of cracks arising from the recesses is suppressed and a sealing material with excellent crack resistance is obtained, and it has become clear that a power module with excellent appearance and excellent product reliability can be provided. [Explanation of symbols]

[0165] 10 Power Module 12 Power semiconductor elements 13 Spacer 14 Ceramic Substrate 16 metal layer 20. Insulating heat dissipation circuit board 21 Solder 22 External connection terminal 24 Encapsulating materials 26 Recess

Claims

1. A power semiconductor element; an insulating heat dissipation circuit board provided on one surface or both surfaces of the power semiconductor element, the insulating heat dissipation circuit board having a ceramic substrate and metal layers on both surfaces of the ceramic substrate; A plurality of external connection terminals electrically connected to the power semiconductor element and extending outward in parallel; a sealing material that seals the power semiconductor element, the metal layer of the insulating heat dissipation circuit board that faces the power semiconductor element, and a part of the plurality of external connection terminals; a recess provided on an outer peripheral side surface of the sealing material between the external connection terminals in a top view in order to ensure a creepage distance between the terminals, The bending strength at room temperature (25°C) measured under the following condition 1 is 140 MPa or more, and A resin composition for sealing a power module, which has a molding shrinkage rate after molding of 0.2% or less and a molding shrinkage rate after post-curing of 0.15% or less, both measured under the following condition 2: (Condition 1) Using a low pressure transfer molding machine, the resin composition for sealing a power module is injected into a mold under the conditions of a mold temperature of 175°C, an injection pressure of 9.8 MPa, and a curing time of 120 seconds to obtain a molded product having a width of 10 mm, a thickness of 4 mm, and a length of 80 mm. The molded product is then post-cured under the conditions of 175°C and 4 hours to prepare a test piece. The bending strength (MPa) of the test piece at room temperature (25°C) is then measured in accordance with JIS K 6911. (Condition 2) The power module encapsulating resin composition was molded under conditions of a mold temperature of 175°C, a molding pressure of 9.8 MPa, and a curing time of 120 seconds, and then post-cured at 175°C for 4 hours. The mold shrinkage rate after molding and the mold shrinkage rate after post-curing were measured for a disk-shaped cured product having a diameter of 100 mm and a thickness of 3 mm, which were calculated according to the following formulas. Formula: Molding shrinkage rate (%) = {(inner diameter dimension of mold cavity at 25°C - outer diameter dimension of disc-shaped cured product at 25°C after molding or post-curing) / inner diameter dimension of mold cavity at 25°C} x 100

2. The resin composition for sealing a power module according to claim 1, having a linear expansion coefficient (CTE1) measured under the following condition 3 of 12 ppm / °C or less. (Condition 3) Using a thermomechanical analyzer, the test piece obtained under Condition 1 is measured under the conditions of a measurement temperature range of 0° C. to 320° C. and a temperature rise rate of 5° C. / min. From the measurement results, the linear expansion coefficient (CTE1) at 40 to 80° C. is calculated.

3. 2. The power module sealing resin composition according to claim 1, wherein the flexural modulus measured under the condition 1 is 25,000 MPa or less.

4. 2. The power module sealing resin composition according to claim 1, wherein the minimum torque value is 1 N·m or less when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C.

5. Contains epoxy resin, 2. The power module sealing resin composition according to claim 1, wherein the epoxy resin comprises at least one selected from a biphenyl type epoxy resin and a trifunctional or higher polyfunctional epoxy resin.

6. The power module sealing resin composition according to claim 5 , further comprising a curing agent.

7. Further, the composition contains an inorganic filler. The power module encapsulating resin composition according to claim 6 , wherein a content of the inorganic filler is 84% ​​by mass or more relative to 100% by mass of the power module encapsulating resin composition.

8. 8. The power module encapsulating resin composition according to claim 7, wherein a content of the resin component contained in the power module encapsulating resin composition is less than 14% by mass with respect to 100% by mass of the power module encapsulating resin composition.

9. A power semiconductor element; an insulating heat dissipation circuit board provided on one surface or both surfaces of the power semiconductor element, the insulating heat dissipation circuit board having a ceramic substrate and metal layers on both surfaces of the ceramic substrate; A plurality of external connection terminals electrically connected to the power semiconductor element and extending outward in parallel; a sealing material that seals the power semiconductor element, a metal layer of the insulating heat dissipation circuit board that faces the power semiconductor element, and some of the external connection terminals; a recess provided on an outer peripheral side surface of the sealing material between the external connection terminals in a top view in order to ensure a creepage distance between the terminals, The power module, wherein the sealing material has a bending strength at room temperature (25°C) of 140 MPa or more as measured in accordance with JIS K 6911.

10. The sealing material has a linear expansion coefficient (CTE1) at 40 to 80 ° C. measured using a thermomechanical analyzer under conditions of a measurement temperature range of 0 ° C. to 320 ° C. and a temperature increase rate of 5 ° C. / min. The power module according to claim 9, wherein the linear expansion coefficient (CTE1) at 40 to 80 ° C. is 12 ppm / ° C. or less.

11. 10. The power module according to claim 9, having a flexural modulus at room temperature (25°C) of 25,000 MPa or less, measured in accordance with JIS K 6911.

12. 10. The power module according to claim 9, wherein compressive strain remains in the sealing material between the external connection terminals.