Ink set and inkjet recording method
The ink set with pH-controlled white and non-white ink compositions addresses the limitations of existing ink sets by enhancing color development and wet rubbing fastness through controlled aggregation, achieving superior storage stability and image quality on fabrics.
Patent Information
- Application Number
- JP2023052905
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ink set described in Patent Document 1 fails to achieve both color development and wet rubbing fastness of printed fabrics, and does not account for the pH differences between white and color inks, leading to issues with ink stability and performance.
The ink set comprises a white inkjet ink composition with a pH of 5 to 7 and a non-white inkjet ink composition with a pH of 8 to 10, which allows for controlled acid-alkali reactions, promoting suitable aggregation and reducing water solubility, thereby enhancing color development and wet rubbing fastness on recording media.
The proposed ink set achieves excellent color development and wet rubbing fastness on fabrics, with improved storage stability due to controlled pH differences and aggregation, resulting in high-quality printed fabrics.
Smart Images

Figure 2024141322000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink set and an inkjet recording method. [Background technology]
[0002] Inkjet recording methods are not only used to record images on recording media such as paper, but are also being applied to textile printing on fabrics, and various ink compositions and recording methods for inkjet textile printing are being investigated. For example, Patent Document 1 describes an ink set used in inkjet recording methods that includes a white ink and a color ink, and the viscosity of the white ink is 1.5 to 4.0 times that of the color ink. It is described that this makes it possible to suppress strike-through and bleeding after the color ink lands. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-62783 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the ink set described in Patent Document 1 cannot achieve both color development and wet friction fastness of the printed matter and storage stability of the ink. Furthermore, Patent Document 1 does not state anything about the white ink and the color inks having different pH values. [Means for solving the problem]
[0005] The present invention provides an ink set comprising a white inkjet ink composition and a non-white inkjet ink composition, wherein the white inkjet ink composition has a pH of 5 or more and 7 or less at 25° C., and the non-white inkjet ink composition has a pH of 8 or more and 10 or less at 25° C. [Brief description of the drawings]
[0006] [Figure 1] 2 is a flowchart showing an example of an inkjet recording method according to the present embodiment. [Diagram 2] 1 shows the compositions of white inkjet ink compositions in Examples and Comparative Examples. [Diagram 3] 1 is Table 2 showing the compositions of white inkjet ink compositions in Examples and Comparative Examples. [Figure 4] 1 is Table 3 showing compositions of non-white inkjet ink compositions in Examples and Comparative Examples. [Diagram 5] Table 4 shows the compositions of non-white inkjet ink compositions in Examples and Comparative Examples. [Figure 6] Table 5 shows the evaluation results of the examples and comparative examples. [Figure 7] Table 6 shows the evaluation results of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.
[0008] The ink set of this embodiment comprises a white inkjet ink composition (hereinafter also referred to as the "white ink composition") and a non-white inkjet ink composition (hereinafter also referred to as the "non-white ink composition"), wherein the white inkjet ink composition has a pH of 5 or more and 7 or less at 25°C, and the non-white inkjet ink composition has a pH of 8 or more and 10 or less at 25°C.
[0009] By using the ink set of this embodiment, it is possible to obtain a printed material having excellent color development and wet rub fastness, and also to obtain a white ink composition and a non-white ink composition having excellent storage stability. Although the reason why this embodiment provides such excellent effects is not clear, the inventors presume it as follows.
[0010] That is, in this embodiment, a white ink composition having a pH of 5 to 7 at 25° C. is discharged by an inkjet method and adhered to a recording medium. At the same time, a non-white ink composition having a pH of 8 to 10 at 25° C. is discharged by an inkjet method and adhered to the recording medium. In this embodiment, since there is an appropriate difference in pH between the white ink composition and the non-white ink composition, when these ink compositions are mixed, the dispersibility of the ink composition is destroyed by an acid-alkali reaction, and it becomes possible to suitably aggregate. Therefore, before the white ink composition and the non-white ink composition penetrate into the recording medium, these ink compositions suitably aggregate and can be retained in the vicinity of the recording medium. Then, due to such aggregation, the non-white ink composition is less susceptible to the influence of the base of the recording medium, and excellent color development can be obtained for the recording medium. In addition, since the ink compositions suitably aggregate and the water solubility of the ink composition is also suppressed, excellent wet friction fastness can also be obtained. Excellent color development and wet friction fastness can be remarkably obtained when a cloth is used as the recording medium. Furthermore, it is presumed that the white ink composition and the non-white ink composition are maintained at a suitable pH, and therefore excellent storage stability can be obtained, although the reason is not limited to this.
[0011] Next, the physical properties and components contained in the white ink composition and non-white ink composition will be described.
[0012] 1. White ink composition The white ink composition of this embodiment has a pH of 5 or more and 7 or less at 25° C. The white ink composition is used to be discharged by an inkjet method and adhered to a recording medium. Since a printed material having better color development and wet friction fastness can be obtained, the recording medium is preferably cloth, and more preferably woven fabric.
[0013] 1.1. Physical properties of white ink composition The physical properties of the white ink composition can be adjusted as desired depending on the type of recording medium and the method of attaching the white ink composition to the recording medium, i.e., the coating method, etc., so long as the white ink composition has a pH of 5 or more and 7 or less at 25° C. The coating method of the white ink composition will be described later.
[0014] pH The pH of the white ink composition is 5 or more and 7 or less at 25°C. When the pH is within the above range, the aggregation of each component, particularly particles, contained in the white ink composition is suppressed, and therefore the white ink composition has excellent storage stability. In addition, the reactivity between the white ink composition and the non-white ink composition is improved, and the white ink and the non-white ink are suitably aggregated, so that a printed material having excellent color development and wet friction fastness as well as excellent image quality and texture can be obtained. In this specification, the pH of the ink composition can be measured, for example, by immersing an electrode part in the ink composition using a tabletop pH meter.
[0015] 1.1.2.Viscosity The viscosity of the white ink composition at 20°C is preferably 1.5 mPa·s to 15 mPa·s, more preferably 1.5 mPa·s to 7 mPa·s. When the viscosity is in the above range, the white ink composition has excellent storage stability, and a printed material having excellent color development and wet friction fastness as well as excellent image quality and texture can be obtained. In this specification, the viscosity is measured, for example, using a viscoelasticity tester MCR-300 (manufactured by Pysica). Specifically, the viscosity can be measured by adjusting the temperature of the measurement object such as the reaction liquid composition to 20°C and reading the shear viscosity (mPa·s) at a shear rate of 200 (1 / s).
[0016] 1.2. White pigment The white ink composition preferably contains a white pigment. The white pigment may be used alone or in combination of two or more kinds. The white pigment may be a resin particle having a hollow structure (hereinafter, also referred to as "hollow resin particle"). In this specification, "hollow resin particle" refers to a resin particle having a void inside the resin particle, and the void is filled with a liquid or gas. As a method for determining whether a particle is hollow, when the particle cross section is observed with a scanning electron microscope, the particle is determined to be hollow if the particle has a structure in which a void is observed inside the particle. Alternatively, as a method for determining whether a particle is hollow, when the particle is observed with a transmission electron microscope, the particle is determined to be hollow if the particle has a structure in which a difference in the contrast of transmitted electrons is observed. In transmission electron microscope observation, when a resin particle has a void inside, the internal void is easily transmitted by an electron beam and is observed with a bright contrast, so that the presence or absence of an internal void can be determined based on the presence or absence of a difference in the contrast of transmitted electrons.
[0017] Examples of the resin of the hollow resin particles include known resins such as urethane resins, acrylic resins, fluorene resins, polyolefin resins, rosin-modified resins, terpene resins, polyester resins, polyamide resins, epoxy resins, vinyl chloride resins, vinyl chloride-vinyl acetate copolymers, and ethylene vinyl acetate resins. These resins can be used alone or in combination of two or more.
[0018] Of these resins, those containing an acrylic resin are preferred as the hollow resin particles, since they provide a white ink composition with superior storage stability, and can produce printed matter having superior color development and wet friction fastness as well as superior image quality and texture.
[0019] Acrylic resin is a general term for polymers obtained by polymerizing at least acrylic monomers such as acrylic acid, methacrylic acid, acrylic acid esters, and methacrylic acid esters as one component. Examples of acrylic resins include resins obtained from acrylic monomers and resins that are copolymers of acrylic monomers and other monomers. Examples of such resins include acrylic-vinyl resins and acrylic-styrene resins that are copolymers of acrylic monomers and vinyl monomers.
[0020] When a resin that is both an acrylic resin and another type of resin is to be classified as either an acrylic resin or another type of resin, the resin is considered to be an acrylic resin if the structure derived from an acrylic monomer accounts for 50% or more by mass of the resin.
[0021] As the acrylic monomer, acrylamide, acrylonitrile, etc. can also be used.
[0022] Examples of acrylic-styrene resins include styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylate copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylate copolymers.
[0023] As the hollow resin particles, commercially available products can be used, for example, ROPAQUE (registered trademark) HT1432 (trade name, product name of The Dow Chemical Company, styrene-acrylic resin).
[0024] In addition, the white pigment may be, for example, a metal oxide, or a metal compound such as barium sulfate or calcium carbonate. Examples of the metal oxide include titanium dioxide, zinc oxide, silica, alumina, and magnesium oxide.
[0025] Among them, a typical example of a white pigment is titanium dioxide. Examples of titanium dioxide include Typepaque (registered trademark) CR-50-2, CR-57, CR-58-2, CR-60-2, CR-60-3, CR-Super-70, CR-90-2, CR-95, CR953, PC-3, PF-690, PF-691, PF-699, PF-711, PF-728, PF-736, PF-737, PF-739, PF-740, PF-742, R-980, and UT-771 (all trade names, manufactured by Ishihara Sangyo Kaisha, Ltd.), and CI Pigment White 6.
[0026] The content of the white pigment is preferably 0.5% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 17% by mass or less, and even more preferably 3% by mass or more and 15% by mass or less, in terms of solid content, relative to the total amount of the white ink composition. By having the content of the white pigment within the above range, it tends to be possible to obtain a printed material having even more excellent storage stability of the white ink composition, and even more excellent color development and wet friction fastness as well as even more excellent image quality and texture.
[0027] The white pigment is preferably capable of being stably dispersed or dissolved in the dispersion medium, and may be dispersed using a dispersant as necessary. Examples of such dispersants include resin dispersants, and are selected from those that can improve the dispersion stability of the pigment in the white ink composition.
[0028] Examples of the resin dispersant include (meth)acrylic resins and salts thereof, such as poly(meth)acrylic acid, (meth)acrylic acid-acrylonitrile copolymer, (meth)acrylic acid-(meth)acrylic acid ester copolymer, vinyl acetate-(meth)acrylic acid ester copolymer, vinyl acetate-(meth)acrylic acid copolymer, and vinylnaphthalene-(meth)acrylic acid copolymer; styrene-(meth)acrylic acid copolymer, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymer, styrene-α-methylstyrene-(meth)acrylic acid copolymer, and styrene-α-methylstyrene-(meth)acrylic acid copolymer. Examples of the water-soluble resins include acrylic acid-(meth)acrylic acid ester copolymers, styrene-maleic acid copolymers, styrene-maleic anhydride copolymers, and other styrene-based resins and their salts; urethane-based resins and their salts, which are polymeric compounds (resins) containing urethane bonds formed by the reaction of an isocyanate group with a hydroxyl group and may be linear and / or branched, and may have or may not have a crosslinked structure; polyvinyl alcohols; vinyl naphthalene-maleic acid copolymers and their salts; vinyl acetate-maleic acid ester copolymers and their salts; and vinyl acetate-crotonic acid copolymers and their salts. Among these, preferred are copolymers of a monomer having a hydrophobic functional group and a monomer having a hydrophilic functional group, and polymers made of a monomer having both a hydrophobic functional group and a hydrophilic functional group. The copolymers may be in the form of any of random copolymers, block copolymers, alternating copolymers, and graft copolymers. The resin dispersants may be used alone or in combination of two or more.
[0029] Examples of commercially available styrene-based resin dispersants include X-200, X-1, X-205, X-220, and X-228 (manufactured by Seiko PMC Co., Ltd.), Nopcosperse (registered trademark) 6100 and 6110 (manufactured by San Nopco Co., Ltd.), Joncryl (registered trademark) 67, 586, 611, 678, 680, 682, and 819 (manufactured by BASF), DISPERBYK (registered trademark)-190 (manufactured by BYK Japan Co., Ltd.), N-EA137, N-EA157, N-EA167, N-EA177, N-EA197D, N-EA207D, and E-EN10 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0030] Commercially available acrylic resin dispersants include, for example, DISPERBYK-187, BYK-190, BYK-191, BYK-194N, and BYK-199 (manufactured by BYK Japan Co., Ltd.), Aron (registered trademark) A-210, A6114, AS-1100, AS-1800, A-30SL, A-7250, and CL-2 (manufactured by Toa Gosei Co., Ltd.).
[0031] Commercially available urethane resin dispersants include, for example, DISPERBYK-182, BYK-183, BYK-184, BYK-185 (manufactured by BYK Japan Co., Ltd.), TEGO (registered trademark) Disperse 710 (manufactured by Evonic Tego Chemi), and Borchi (registered trademark) Gen 1350 (manufactured by OMG Borschers).
[0032] Although commercially available products are listed above, the dispersants may be obtained by synthesis using conventional methods.
[0033] The total content of the resin dispersant in the ink composition is preferably 0.1 parts by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the white pigment.
[0034] 1.3.Resin The white ink composition preferably contains a resin. Examples of the resin include a resin formed from an aqueous dispersion obtained by self-emulsifying the resin in an aqueous solvent. When the white ink composition contains a resin, the white ink composition has better storage stability, and the white ink composition tends to have better color development and wet friction fastness, as well as better image quality and texture. The resin can further improve the adhesion of the image formed by the white ink composition attached to the recording medium. The resin can be used alone or in combination of two or more types.
[0035] The resin preferably contains a resin having an acid value of 50 mgKOH / g or more. By using such a resin, the pH of the white ink composition is more stabilized, and in particular the aggregation of particles is more suppressed, so that the white ink composition tends to have better storage stability. In addition, there is a tendency to obtain a printed material having better image quality and texture as well as better color development and wet friction fastness. In this specification, the term "acid value" means the number of mg of KOH required to neutralize 1 g of resin solids, and can be measured by a method described in JIS K0070, for example, an electrolytic titration method. As the titration reagent, for example, an ethanol solution of sodium hydroxide can be used. In addition, the upper limit of the acid value of the resin is not particularly limited, but is, for example, 300 mgKOH / g or less.
[0036] Since there is a tendency that the white ink composition has even better storage stability, and that printed matter having even better color development and wet rubbing fastness as well as even better image quality and texture can be obtained, it is preferable that the resin have an acid value of 60 mgKOH / g or more and 100 mgKOH / g or less.
[0037] The resin preferably contains a resin having a glass transition temperature of -10°C or lower. The white ink composition is applied as a base against the adhesion of the non-white ink composition. Therefore, the amount of the white ink composition applied to the recording medium is relatively large, and it is easy to affect the texture of the printed textile. By using a resin having a glass transition temperature of -10°C or lower, a softer coating film of the white ink composition can be formed, so that the texture of the printed textile can be improved even if a relatively large amount of the white ink composition is applied. In addition, the white ink composition has a tendency to have a better storage stability, and to obtain a printed textile having a better image quality and texture as well as a better color development and wet friction fastness. In this specification, the glass transition temperature can be measured, for example, by a differential scanning calorimeter. In addition, the lower limit of the glass transition temperature of the resin is not particularly limited, but is, for example, -50°C or higher.
[0038] Since there is a tendency to be able to obtain a printed material having even better storage stability of the white ink composition, even better color development and wet rubbing fastness as well as even better image quality and even better texture, it is preferable for the resin to have a glass transition temperature of -35°C or more and -15°C or less.
[0039] Examples of the resin include urethane-based resins, acrylic-based resins (including styrene-acrylic-based resins), fluorene-based resins, polyolefin-based resins, rosin-modified resins, terpene-based resins, polyester-based resins, polyamide-based resins, epoxy-based resins, vinyl chloride-vinyl acetate copolymers, ethylene-vinyl acetate-based resins, etc. Since there is a tendency that the white ink composition has better storage stability, better color development and wet friction fastness as well as better image quality and better texture, it is possible to obtain printed matter. Among them, it is preferable to use one or more selected from the group consisting of urethane-based resins, acrylic-based resins, polyolefin-based resins, and polyester-based resins, and it is more preferable to use a urethane-based resin. These resins are often handled in the form of an emulsion, but may be supplied in the form of a powder.
[0040] Urethane resin is a general term for resins having urethane bonds. Examples of urethane resins include polyether-type urethane resins containing ether bonds in the main chain in addition to urethane bonds, polyester-type urethane resins containing ester bonds in the main chain, and polycarbonate-type urethane resins containing carbonate bonds in the main chain. In addition, commercially available products may be used as the urethane resin. Examples of such urethane resins include Takelac (registered trademark) W-6110, WS-6021, W-512-A-6 (trade name, manufactured by Mitsui Chemicals, Inc.), WS-5100 (trade name, manufactured by Mitsui Chemicals, Inc.), Elastron (registered trademark) E-37, H-3, Elastron (registered trademark) H-38, BAP, C-52, F-29, W-11P (trade name, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and Superflex (registered trademark) 840, 870, 800, 150, 420, 460. , 460s, 470, 600, 610, 620, 630, 640, 650, 700, E-4000 (trade names, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Parmarin (registered trademark) UA-150, UX-368T, Euprene (registered trademark) UXA-307, and Eukoat (registered trademark) UWS-145 (trade names, manufactured by Sanyo Chemical Industries, Ltd.), Sancure (registered trademark) 2710, Solsverse (registered trademark) 47000 (trade names, manufactured by Lubrizol Japan Co., Ltd.), NeoRez (registered trademark) Trademark) R-9660, R-9637, R-940 (product name, manufactured by Kusumoto Chemicals Co., Ltd.), ADEKA BONTITOR (registered trademark) HUX-380, 290K (product name, manufactured by ADEKA Corporation), ETERNACALL (registered trademark) UW-1501F, UW-1527DF, UW-1614AF, UW-2201AF (product name, manufactured by Ube Industries, Ltd.), HYDRAN (registered trademark) CP-7010, CP-7020, CP-7030, CP-7040, CP-7050, CP-706 0, CP-7610 (trade name, manufactured by Dainippon Ink and Chemicals, Inc.), ACRYT (registered trademark) WBR-022U (trade name), urethane emulsion WBR-2120C, WBR-2122C (trade name, manufactured by Taisei Fine Chemical Co., Ltd.), REZAMIN (registered trademark) D-1060, D-2020, D-4080, D-4200, D-6300, D-6455 (manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd.), and SANCURE (registered trademark) 2710 (manufactured by LUBRIZOL).
[0041] Examples of the acrylic monomer that can be used include acrylamide and acrylonitrile. Examples of the resin emulsion made from an acrylic resin include commercially available products such as FK-854 (manufactured by Chuo Rika Kogyo Co., Ltd.), Mowinyl (registered trademark) 952B and 718A (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), and Nipol (registered trademark) LX852 and LX874 (manufactured by Nippon Zeon Co., Ltd.).
[0042] The acrylic resin may be a styrene-acrylic resin. In addition, in this specification, the term "(meth)acrylic" means at least one of acrylic and methacrylic.
[0043] Styrene-acrylic resins are copolymers obtained from a styrene monomer and a (meth)acrylic monomer, and examples thereof include styrene-acrylic acid copolymers, styrene-methacrylic acid copolymers, styrene-methacrylic acid-acrylate copolymers, styrene-α-methylstyrene-acrylic acid copolymers, and styrene-α-methylstyrene-acrylic acid-acrylate copolymers. As the styrene-acrylic resin, commercially available products may be used, and examples thereof include JONCRYL (registered trademark) 62J, 7100, 390, 711, 511, 7001, 632, 741, 450, 840, 74J, HRC-1645J, 734, 852, 7600, 775, 537J, 1535, PDX-7630A, 352J, 352D, PDX-7145, 538J, 7640, 7641, 631, 790, 780, and 7610 (manufactured by BASF), Mowinyl (registered trademark) 966A and 975N (manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), and Vinybran (registered trademark) 2586 (manufactured by Nissin Chemical Industry Co., Ltd.).
[0044] The polyolefin resin has an olefin such as ethylene, propylene, butylene, etc. in the structural skeleton, and a known one can be appropriately selected and used. As the olefin resin, a commercially available product can be used, for example, Arrowbase (registered trademark) CB-1200, CD-1200 (manufactured by Unitika Co., Ltd.), etc. may be used.
[0045] Although commercially available products are listed above, the resins may be obtained by synthesis using conventional methods.
[0046] The resin content, in terms of solid content, relative to the total amount of the ink composition, is preferably from 0.1% by mass to 20% by mass, more preferably from 1% by mass to 15% by mass, and even more preferably from 2% by mass to 10% by mass.
[0047] 1.4. Water-soluble organic solvents The white ink composition preferably contains a water-soluble organic solvent. The functions of the water-soluble organic solvent include, for example, mitigating the water absorption behavior of the recording medium, improving the wettability of the white ink composition to the recording medium, and increasing the moisture retention of the white ink composition. The water-soluble organic solvent may be used alone or in combination of two or more.
[0048] Examples of the water-soluble organic solvent include water-soluble esters, alkylene glycol ethers, cyclic esters, nitrogen-containing solvents, and alcohols. Examples of the nitrogen-containing solvent include water-soluble cyclic amides and non-cyclic amides. Examples of the non-cyclic amides include water-soluble alkoxyalkylamides.
[0049] Examples of the esters include glycol monoacetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and methoxybutyl acetate; Examples of glycol diesters include glycol diacetate, propylene glycol diacetate, dipropylene glycol diacetate, ethylene glycol acetate propionate, ethylene glycol acetate butyrate, diethylene glycol acetate butyrate, diethylene glycol acetate propionate, diethylene glycol acetate butyrate, propylene glycol acetate propionate, propylene glycol acetate butyrate, dipropylene glycol acetate butyrate, and dipropylene glycol acetate propionate.
[0050] Examples of alkylene glycol ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, tetraethylene glycol monoethyl ether, tetraethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monoethyl ether, and alkylene glycol dialkyl ethers such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol methyl ethyl ether, diethylene glycol methyl butyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol dibutyl ether, triethylene glycol methyl butyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol dibutyl ether, propylene glycol dimethyl ether, propylene glycol diethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol diethyl ether, and tripropylene glycol dimethyl ether.
[0051] Examples of cyclic esters include cyclic esters (lactones) such as β-propiolactone, γ-butyrolactone, δ-valerolactone, ε-caprolactone, β-butyrolactone, β-valerolactone, γ-valerolactone, β-hexanolactone, γ-hexanolactone, δ-hexanolactone, β-heptanolactone, γ-heptanolactone, δ-heptanolactone, ε-heptanolactone, γ-octanolactone, δ-octanolactone, ε-octanolactone, δ-nonalactone, ε-nonalactone, and ε-decanolactone, as well as compounds in which the hydrogen of the methylene group adjacent to the carbonyl group is substituted with an alkyl group having 1 to 4 carbon atoms.
[0052] Examples of alkoxyalkylamides include 3-methoxy-N,N-dimethylpropionamide, 3-methoxy-N,N-diethylpropionamide, 3-methoxy-N,N-methylethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-diethylpropionamide, 3-ethoxy-N,N-methylethylpropionamide, 3-n-butoxy-N,N-dimethylpropionamide, 3-n-butoxy-N,N-diethylpropionamide, 3-n-butoxy-N,N-methylethylpropionamide, 3-n-propoxy -N,N-dimethylpropionamide, 3-n-propoxy-N,N-diethylpropionamide, 3-n-propoxy-N,N-methylethylpropionamide, 3-iso-propoxy-N,N-dimethylpropionamide, 3-iso-propoxy-N,N-diethylpropionamide, 3-iso-propoxy-N,N-methylethylpropionamide, 3-tert-butoxy-N,N-dimethylpropionamide, 3-tert-butoxy-N,N-diethylpropionamide, 3-tert-butoxy-N,N-methylethylpropionamide, and the like.
[0053] Examples of cyclic amides include lactams, and more specifically, pyrrolidones such as 2-pyrrolidone, 1-methyl-2-pyrrolidone, 1-ethyl-2-pyrrolidone, 1-propyl-2-pyrrolidone, and 1-butyl-2-pyrrolidone.
[0054] Examples of alcohols include methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, 2-butanol, tert-butanol, iso-butanol, n-pentanol, 2-pentanol, 3-pentanol, tert-pentanol, ethylene glycol, propylene glycol, 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,2-octanediol, diethylene glycol, dipropylene glycol, triethylene glycol, 1,3-propanediol, Examples of suitable glyceryl ethers include 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-ethyl-2-methyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,3-pentanediol, 3-methyl-1,5-pentanediol, 2-methylpentane-2,4-diol, trimethylolpropane, and glycerin.
[0055] The water-soluble organic solvent preferably contains one or more solvents selected from the group consisting of glycerin, triethylene glycol, triethylene glycol monomethyl ether, and triethylene glycol monobutyl ether, because this allows the white ink composition to have excellent storage stability, and to produce printed matter having better color development and wet rub fastness as well as better image quality and texture.
[0056] The content of the water-soluble organic solvent is preferably 0.1% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 30% by mass or less, and even more preferably 15% by mass or more and 25% by mass or less, in total, relative to the total amount of the white ink composition. By having the content of the water-soluble organic solvent within the above range, the storage stability of the white ink composition tends to be more excellent, and a printed material having more excellent color development and wet friction fastness as well as more excellent image quality and texture can be obtained.
[0057] The water-soluble organic solvent preferably includes a water-soluble organic solvent (a) having an SP value of 9 to 11. The content of the water-soluble organic solvent (a) is preferably 0.1% by mass to 40% by mass in total relative to the total amount of the treatment liquid composition. The content of the water-soluble organic solvent (a) is more preferably 0.5% by mass to 30% by mass in total relative to the total amount of the treatment liquid composition, and more preferably 0.7% by mass to 20% by mass in total. By using such a water-soluble organic solvent (a), the permeability of the white ink composition into the recording medium becomes better, and the white ink composition can form a coating film in a manner that takes root in the recording medium. Therefore, the non-white ink composition can be retained not only in the vicinity of the recording medium but also in the recording medium, and there is a tendency that a printed material having even better color development, even better wet friction fastness, and even better image quality and texture can be obtained. The water-soluble organic solvent (a) can be used alone or in combination of two or more kinds.
[0058] In this specification, the SP value is a solubility parameter based on the Hansen method, and is also referred to as the Hansen SP value. The Hansen method classifies the SP value δ into three terms, and δ 2 = δ d 2 +δ p 2 +δ h 2 The calculation was expressed as δ d , δ p , δ hare the solubility parameters corresponding to the dispersion term, dipole-dipole term, and hydrogen bond term, respectively. The units of the SP value and Hansen SP value are (cal / cm 3 ) 1 / 2 The Hansen SP value may be a value derived using the calculation software Hansen-Solubility HSPiP.
[0059] Examples of the water-soluble organic solvent (a) include diethylene glycol monobutyl ether (SP value: 9.5), propylene glycol monomethyl ether (SP value: 9.99), triethylene glycol monoethyl ether (SP value: 10.0), triethylene glycol monobutyl ether (SP value: 10.5), and 2-methyl-1,3-pentanediol (SP value: 10.3).
[0060] The water-soluble organic solvent (a) is preferably at least one selected from the group consisting of triethylene glycol monomethyl ether and triethylene glycol monobutyl ether, since this allows the white ink composition to have even more excellent storage stability, and allows the production of printed matter having even more excellent color development and wet rubbing fastness as well as even more excellent image quality and texture. 1.5.Surfactants The white ink composition preferably contains a surfactant. The surfactant has a function of lowering the surface tension of the white ink composition and adjusting the wettability with a recording medium. Examples of the surfactant include acetylene glycol surfactants, silicone surfactants, and fluorine surfactants. The surfactants can be used alone or in combination of two or more.
[0061] It is preferable that the surfactant contains an acetylene glycol-based surfactant, since this provides a printed material having superior storage stability of the white ink composition, superior color development and wet rubbing fastness, as well as superior image quality and texture.
[0062] Examples of acetylene glycol surfactants include Surfynol (registered trademark) 104, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 104S, 420, 440, 465, 485, SE, SE-F, 504, 61, DF37, CT111, CT121, CT131, CT136, TG, GA, and DF110D (manufactured by Nissin Chemical Industry Co., Ltd.); Olfine (registered trademark) Examples of suitable terpolymers include (trademark) B, Y, P, A, STG, SPC, E1004, E1010, PD-001, PD-002W, PD-003, PD-004, EXP.4001, EXP.4036, EXP.4051, AF-103, AF-104, AK-02, and SK-14; AE-3 (manufactured by Nissin Chemical Industry Co., Ltd.); and Acetylenol (registered trademark) E00, E00P, E40, and E100 (manufactured by Kawaken Fine Chemical Co., Ltd.).
[0063] Examples of silicone surfactants include polysiloxane compounds such as polyether-modified organosiloxanes. Examples of commercially available polyether-modified organosiloxanes include BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, and BYK-348 (manufactured by BYK Japan Co., Ltd.), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6004, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, and KF-6017 (manufactured by Shin-Etsu Chemical Co., Ltd.).
[0064] Examples of fluorosurfactants include fluorine-modified polymers, and examples of commercially available products include BYK-340 (manufactured by BYK Japan KK).
[0065] The content of the surfactant is preferably from 0.01% by mass to 10% by mass, more preferably from 0.05% by mass to 5.0% by mass, and even more preferably from 0.1% by mass to 1.0% by mass, relative to the total amount of the white ink composition. By having the content of the surfactant within the above range, the storage stability of the white ink composition tends to be even more excellent, and a printed material having even better color development and wet friction fastness as well as even better image quality and texture can be obtained.
[0066] 1.6.pH Adjusters The white ink composition preferably contains a pH adjuster. When a pH adjuster is contained in the white ink composition, the storage stability of the white ink composition tends to be further improved. The pH adjuster can be used alone or in combination of two or more.
[0067] Examples of pH adjusters include suitable combinations of acids, bases, weak acids, and weak bases. Examples of acids and bases used in such combinations include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid; inorganic bases such as lithium hydroxide, sodium hydroxide, potassium hydroxide, potassium dihydrogen phosphate, disodium hydrogen phosphate, potassium carbonate, sodium carbonate, sodium bicarbonate, and ammonia; organic bases such as triethylamine, trimethylamine, diethylethanolamine, triethanolamine, diethanolamine, monoethanolamine, tripropanolamine, triisopropanolamine, diisopropanolamine, and trishydroxymethylaminomethane (THAM); adipic acid, citric acid, succinic acid, lactic acid, N,N-bis(2-hydroxyethyl) 2-aminoethanesulfonic acid (BES), 4-(2-hydroxyethyl)-1-piperazineethanesulfonic acid (HEPES), morpholinoethanesulfonic acid (MES), morpholinopropanesulfonic acid (MOPS), carbamoylmethyliminobisacetic acid (ADA), piperazine-1,4-bis(2-ethanesulfonic acid) (PIPES), N-(2-acetamido)-2-aminoethanesulfonic acid (ACES), cholamine hydrochloride, N-tris(hydroxymethyl)methyl-2-aminoethanesulfonic acid (TES), acetamidoglycine, tricine, glycineamide, Good's buffers such as bicine, phosphate buffer, citrate buffer, and Tris buffer. In addition, since the pH buffering effect can be obtained more stably, tertiary amines such as triethanolamine and triisopropanolamine, and carboxyl group-containing organic acids such as adipic acid, citric acid, succinic acid, and lactic acid may be included as part or all of the pH adjuster. In addition, sodium acetate, ammonium acetate, sodium formate, ammonium formate, sodium carbonate, sodium bicarbonate, potassium bicarbonate, monosodium phosphate, monopotassium phosphate, disodium phosphate, and trisodium phosphate, which have a buffering effect, may be used together with the pH adjuster.
[0068] The pH adjuster is preferably at least one selected from the group consisting of triethanolamine and adipic acid, since this allows the white ink composition to have superior storage stability, and to produce printed matter having superior color development and wet rubbing fastness as well as superior image quality and texture.
[0069] The content of the pH adjuster is preferably 0.05% by mass or more and 5.0% by mass or less, more preferably 0.1% by mass or more and 3.0% by mass or less, in total, relative to the total amount of the white ink composition. By having the content of the pH adjuster within the above range, the storage stability of the white ink composition tends to be even more excellent, and it tends to be possible to obtain a printed material having even better color development and wet rubbing fastness as well as even better image quality and texture.
[0070] 1.7.Water The white ink composition preferably contains water. Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, as well as ultrapure water from which ionic impurities have been removed as much as possible. Water sterilized by ultraviolet irradiation, addition of hydrogen peroxide, or the like is preferred because it can suppress the growth of mold and bacteria when the reaction liquid composition is stored for a long period of time.
[0071] The water content is preferably 40% by mass or more and 85% by mass or less relative to the total amount of the white ink composition. By keeping the water content within this range, an increase in viscosity of the white ink composition can be suppressed.
[0072] 1.8.Other Ingredients The white ink composition may contain various additives such as a dissolution aid, a viscosity modifier, an antioxidant, an ultraviolet absorber, an oxygen absorber, a rust inhibitor, a corrosion inhibitor, and a chelating agent. The additives may be used alone or in combination of two or more.
[0073] The content of the additives is preferably 0.01% by mass or more and 10% by mass or less in total relative to the total amount of the white ink composition. When the content of the additives is within the above range, the white ink composition has excellent storage stability, and it tends to be possible to obtain a printed material having excellent color development and wet friction fastness as well as excellent image quality and texture.
[0074] 1.9. Method for preparing white ink composition The white ink composition can be prepared by mixing the components in any order so that the pH is 5 to 7 at 25°C, and removing impurities and foreign matter by filtration or the like as necessary. The components can be mixed by sequentially adding the components to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer, and stirring and mixing the components. Filtration methods include centrifugal filtration and filter filtration. The pH of the white ink composition can be confirmed, for example, using a benchtop pH meter.
[0075] 2. Non-white ink composition The non-white ink composition of this embodiment has a pH of 8 or more and 10 or less at 25° C. The non-white ink composition is used to be ejected by an inkjet method and adhered to a recording medium. The recording medium is preferably cloth, and more preferably woven fabric, since a printed material having superior color development and wet friction fastness as well as superior image quality and texture can be obtained.
[0076] 2.1. Physical properties of non-white ink composition The physical properties of the non-white ink composition can be adjusted as desired depending on the type of recording medium and the method of attaching the non-white ink composition to the recording medium, i.e., the application method, etc., so long as the non-white ink composition has a pH of 8 or more and 10 or less at 25° C. The application method of the non-white ink composition will be described later.
[0077] 2.1.1.pH The pH of the non-white ink composition is 8 or more and 10 or less at 25° C. When the pH is within the above range, the aggregation of the components, particularly the particles, contained in the non-white ink composition is suppressed, and therefore the non-white ink composition has excellent storage stability. In addition, the reactivity between the white ink composition and the non-white ink composition is good, and the white ink and the non-white ink are suitably aggregated, so that a printed material having excellent color development and wet friction fastness as well as excellent image quality and texture can be obtained.
[0078] 2.1.2.Viscosity The viscosity of the non-white ink composition is preferably from 1.5 mPa·s to 15 mPa·s, and more preferably from 1.5 mPa·s to 7 mPa·s, at 20° C. When the viscosity is within the above range, the non-white ink composition has excellent storage stability, and it is possible to obtain printed matter having excellent color development and wet rubbing fastness as well as excellent image quality and texture.
[0079] 2.2.Pigments The non-white ink composition preferably contains a pigment other than a white pigment. Examples of such pigments include azo pigments such as insoluble azo pigments, condensed azo pigments, azo lakes, and chelate azo pigments, polycyclic pigments such as phthalocyanine pigments, perylene and perinone pigments, anthraquinone pigments, quinacridone pigments, dioxane pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments, dye chelates, dye lakes, nitro pigments, nitroso pigments, aniline black, daylight fluorescent pigments, and carbon black. The pigments can be used alone or in combination of two or more.
[0080] Specific examples of pigments include the following:
[0081] Examples of black pigments include No. 2300, 900, MCF88, No. 20B, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, and No. 2200B manufactured by Mitsubishi Chemical Corporation; Color Black FW1, FW2, FW2V, FW18, FW200, S150, S160, S170, Pretex (registered trademark) 35, U, V, 140U, Special Black 6, 5, 4A, 4, and 250 manufactured by Degussa; and Conda Examples of such polyurethane foams include Kutex SC, Raven 1255, 5750, 5250, 5000, 3500, 1255, and 700 manufactured by Cabot Corporation; Regal 400R, 330R, 660R, Mogul L, Monarch 700, 800, 880, 900, 1000, 1100, 1300, 1400, and Elftex 12 manufactured by Cabot Corporation; and Microjet CW-1, CW-1S, CW-2, CW-3, and M-800 manufactured by Orient Chemical Industry Co., Ltd.
[0082] Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 167, 172, and 180.
[0083] Examples of magenta pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, 245, and CI Pigment Violet. 19, 23, 32, 33, 36, 38, 43, and 50.
[0084] Cyan pigments include, for example, CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, and 66, and CI Vat Blue 4 and 60.
[0085] Examples of pigments other than magenta, cyan, and yellow include CI Pigment Green 7 and 10, CI Pigment Brown 3, 5, 25, and 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43, and 63.
[0086] Examples of pearl pigments include pigments having pearlescent luster or interference luster, such as titanium dioxide-coated mica, fish scale foil, and bismuth oxychloride.
[0087] Examples of metallic pigments include particles of simple metals such as aluminum, silver, gold, platinum, nickel, chromium, tin, zinc, indium, titanium, and copper, or alloys thereof.
[0088] Since there is a tendency for the storage stability of the non-white ink composition to be excellent, and for printed matter having better color development and wet rubbing fastness as well as better image quality and texture to be obtained, the pigment content is preferably 1% by mass or more and 10% by mass or less relative to the total amount of the non-white ink composition.
[0089] It is preferable that the pigment can be stably dispersed or dissolved in the dispersion medium, and if necessary, the pigment may be dispersed using a dispersant, such as the same dispersant as that used for the white pigment in the white ink composition.
[0090] 2.3.Resin The non-white ink preferably contains a resin. Examples of the resin include a resin formed from an aqueous dispersion obtained by self-emulsifying a resin in an aqueous solvent. When the non-white ink composition contains a resin, the non-white ink composition has excellent storage stability, and tends to have better color development and wet friction fastness as well as better image quality and texture, leading to the production of a printed matter. The resin can further improve the adhesion of an image formed by the non-white ink composition applied to a recording medium. The resin can be used alone or in combination of two or more types.
[0091] The resin preferably contains a resin having an acid value of less than 50 mgKOH / g. By using such a resin, the pH of the non-white ink composition is more stabilized, and in particular the aggregation of particles is more suppressed, so that the non-white ink composition tends to have better storage stability. In addition, there is a tendency to obtain a printed material having better color development and wet friction fastness as well as better image quality and texture. The lower limit of the acid value of the resin is not particularly limited, but is, for example, 1 mgKOH / g or more.
[0092] Since there is a tendency that the storage stability of the non-white ink composition can be improved, and printed matter having improved color development and wet rubbing fastness as well as improved image quality and texture can be obtained, it is preferable that the resin have an acid value of 20 mgKOH / g or more and 40 mgKOH / g or less.
[0093] The resin preferably contains a resin having a glass transition temperature of 0° C. or higher. Since a resin having a glass transition temperature of 0° C. or higher has a relatively high hardness, the use of such a resin can make the aggregate of the non-white ink composition and the white ink composition more robust. Therefore, there is a tendency to obtain a printed material having better wet friction robustness. Note that a resin having a glass transition temperature of 0° C. or higher tends to lose texture if applied too much, but it is possible to apply the resin appropriately to the recording medium by ejecting the resin by the inkjet method and attaching it to the recording medium. The upper limit of the glass transition temperature of the resin is not particularly limited, but is, for example, 50° C. or lower.
[0094] Since there is a tendency that a non-white ink composition having even better storage stability, even better color development and wet rubbing fastness as well as even better image quality can be obtained, and printed matter having even better texture can be obtained, it is preferable that the resin have a glass transition temperature of 10° C. or more and 30° C. or less.
[0095] Examples of the resin include the same resin as that contained in the white ink composition. Since there is a tendency that the non-white ink composition has better storage stability, better color development and wet friction fastness as well as better image quality and better texture, it is preferable that the resin is one or more selected from the group consisting of urethane-based resins, acrylic-based resins, polyolefin-based resins, and polyester-based resins, and more preferably a urethane-based resin. These resins are often handled in the form of an emulsion, but may be supplied in the form of a powder.
[0096] The resin content, in terms of solid content, relative to the total amount of the non-white ink composition is preferably from 0.1% to 15% by mass, more preferably from 0.5% to 10% by mass, and even more preferably from 1% to 7% by mass.
[0097] 2.4. Water-soluble organic solvents The non-white ink composition preferably contains a water-soluble organic solvent. The functions of the water-soluble organic solvent include, for example, mitigating the water absorption behavior of the recording medium, improving the wettability of the non-white ink composition to the recording medium, and increasing the moisture retention of the non-white ink composition. As the water-soluble organic solvent, reference may be made to the water-soluble organic solvent contained in the white ink composition described above. The water-soluble organic solvent may be used alone or in combination of two or more kinds.
[0098] Since there is a tendency that a printed material having even better storage stability of the non-white ink composition, even better color development and wet rubbing fastness as well as even better image quality and even better texture can be obtained, it is preferable that the water-soluble organic solvent contains one or more solvents selected from the group consisting of glycerin, triethylene glycol, and triethylene glycol monobutyl ether.
[0099] The content of the water-soluble organic solvent is preferably 0.1% by mass or more and 40% by mass or less, more preferably 10% by mass or more and 30% by mass or less, and even more preferably 15% by mass or more and 25% by mass or less, in total, relative to the total amount of the non-white ink composition. When the content of the water-soluble organic solvent is within the above range, the storage stability of the non-white ink composition is more excellent, and it tends to be possible to obtain a printed material having more excellent color development and wet friction fastness as well as more excellent image quality and texture.
[0100] 2.5.Surfactants The non-white ink composition preferably contains a surfactant. The surfactant has a function of lowering the surface tension of the non-white ink composition and adjusting the wettability with a recording medium. As the surfactant, reference may be made to the surfactants contained in the white ink composition described above. The surfactant may be used alone or in combination of two or more kinds.
[0101] Since there is a tendency that a printed material having even better storage stability of the non-white ink composition, even better color development and wet rubbing fastness as well as even better image quality and even better texture can be obtained, it is preferable that the surfactant contain an acetylene glycol-based surfactant.
[0102] The content of the surfactant is preferably from 0.01% by mass to 10% by mass, more preferably from 0.05% by mass to 5.0% by mass, and even more preferably from 0.1% by mass to 1.0% by mass, relative to the total amount of the non-white ink composition. By having the surfactant content within the above range, the storage stability of the non-white ink composition tends to be even more excellent, and it tends to be possible to obtain a printed material having even better color development and wet rubbing fastness as well as even better image quality and texture.
[0103] 2.6.pH Adjusters The non-white ink composition preferably contains a pH adjuster. When the non-white ink composition contains a pH adjuster, the storage stability of the non-white ink composition tends to be further improved. As the pH adjuster, reference may be made to the pH adjusters contained in the white ink composition described above. The pH adjusters can be used alone or in combination of two or more.
[0104] The pH adjuster is preferably at least one selected from the group consisting of triethanolamine and adipic acid, since this allows the non-white ink composition to have excellent storage stability, and to produce printed matter having superior color development and wet rubbing fastness as well as superior image quality and texture.
[0105] The content of the pH adjuster is preferably 0.05% by mass or more and 5.0% by mass or less, more preferably 0.1% by mass or more and 3.0% by mass or less, in total, relative to the total amount of the non-white ink composition. By having the content of the pH adjuster within the above range, it tends to be possible to obtain a printed material having even more excellent storage stability of the non-white ink composition, and even more excellent color development and wet rubbing fastness as well as even more excellent image quality and texture.
[0106] 2.7.Water The non-white ink composition preferably contains water. As for the water, reference may be made to the water contained in the white ink composition described above.
[0107] The water content is preferably 40% by mass or more and 85% by mass or less relative to the total amount of the non-white ink composition. By keeping the water content within this range, an increase in viscosity of the non-white ink composition can be suppressed.
[0108] 2.8.Other Ingredients The non-white ink composition may contain various additives such as a dissolution aid, a viscosity modifier, an antioxidant, an ultraviolet absorber, an oxygen absorber, a rust inhibitor, a corrosion inhibitor, and a chelating agent. The additives may be used alone or in combination of two or more.
[0109] The content of the additives is preferably 0.01% by mass or more and 10% by mass or less in total relative to the total amount of the non-white ink composition. When the content of the additives is within the above range, the non-white ink composition has excellent storage stability, and it tends to be possible to obtain a printed material having excellent color development and wet rubbing fastness as well as excellent image quality and texture.
[0110] 2.9. Method for preparing non-white ink composition The non-white ink composition can be prepared by mixing the components in any order so that the pH is 8 to 10 at 25° C., and removing impurities and foreign matter by filtration or the like as necessary. The method for mixing the components may refer to the above-mentioned method for preparing a white ink composition. The pH of the non-white ink composition can be confirmed, for example, using a desktop pH meter.
[0111] 3. Inkjet recording method The inkjet recording method of the present embodiment (hereinafter also simply referred to as the "recording method") includes a white inkjet ink composition application step (hereinafter also referred to as the "white ink composition application step") in which the white ink composition provided in the set according to the present embodiment is discharged from a recording head and applied to a recording medium, and a non-white inkjet ink composition application step (hereinafter also referred to as the "non-white ink composition application step") in which a non-white ink composition provided in the set according to the present embodiment is discharged from a recording head and applied to the recording medium to which at least the white ink composition has been applied, and after the white ink composition is applied to the recording medium in the white ink composition application step, the non-white ink composition application step is performed within a time interval of 5 seconds. According to such a recording method, a printed textile having better color development and wet friction fastness as well as better image quality and texture can be obtained. In addition, since both the white ink composition and the non-white ink composition have excellent storage stability, in the recording method, it is easy to appropriately adjust the application amount of the white ink composition and the non-white ink composition to the recording medium. The recording method can be applied to various recording media and good textile printing can be performed. In the recording method, the white ink composition applying step may be performed simultaneously with the non-white ink composition applying step. An example of the inkjet recording method of this embodiment is shown in Fig. 1. This inkjet recording method includes, in this order, the above-mentioned white ink composition applying step, a non-white ink composition applying step, and a heating step, which will be described in detail later. Next, the recording medium and each step will be described.
[0112] 5.1. Recording medium Examples of the recording medium include an absorbent recording medium, a low absorbent recording medium, a non-absorbent recording medium, and cloth. The recording medium is preferably cloth, and more preferably woven fabric, because it can provide a printed material having better color development and wet friction fastness as well as better image quality and texture. In this specification, cloth refers to fibers that have been thinly processed. Fabric refers to fabric woven with fibers.
[0113] A low-absorbency recording medium or a non-absorbency recording medium has a water absorption rate of 10 mL / m2 within 30 msec from the start of contact in the Bristow method. 2 This refers to a recording medium that is as follows. The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also adopted by the Japan Pulp and Paper Technical Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and paperboard - Liquid absorbency test method - Bristow method" of the "JAPAN TAPPI Paper and Pulp Test Method 2000 Edition".
[0114] Non-absorbent recording media or low absorbent recording media can be classified according to the wettability of the recording surface to water. Specifically, the recording media can be characterized by dropping a 0.5 μL water droplet on the recording surface of the recording media and measuring the contact angle drop rate, i.e., the contact angle at 0.5 milliseconds after landing and the contact angle at 5 seconds. More specifically, as the properties of the recording media, the non-absorbency of a non-absorbent recording medium means that the drop rate is less than 1%, and the low absorbency of a low absorbent recording medium means that the drop rate is 1% or more and less than 5%. Absorbency means that the drop rate is 5% or more. The contact angle can be measured, for example, using a portable contact angle meter PCA-1 (trade name, Kyowa Interface Science Co., Ltd.).
[0115] Examples of absorbent recording media include those containing fabric, plain paper such as electrophotographic paper, and inkjet paper, which have high permeability to the white ink composition and non-white ink composition, as well as art paper, coated paper, and cast paper used in general offset printing, which have relatively low permeability to the ink composition.
[0116] An example of a low-absorbency recording medium is coated paper having a coating layer on the surface for receiving oil-based ink. Examples of coated paper include printing paper such as art paper, coated paper, and matte paper.
[0117] Examples of non-absorbent recording media include plastic films that do not have an ink-absorbing layer, substrates such as paper coated with plastic, substrates with a plastic film bonded thereto, etc. Examples of plastics include polyvinyl chloride, polyethylene terephthalate, polycarbonate, polystyrene, polyurethane, polyethylene, and polypropylene.
[0118] In addition to the above-mentioned recording media, metal plates such as iron, silver, copper, and aluminum, and recording media that are non-ink absorbing or have low ink absorbing properties, such as glass, can also be used.
[0119] Examples of fabrics include woven fabric, knitted fabric, cotton, felt, and nonwoven fabric.
[0120] Examples of fibers constituting the fabric include natural fibers such as cotton, hemp, wool, leather, and silk, synthetic fibers such as polypropylene, polyester, acetate, triacetate, polyamide, acrylic, and polyurethane, and biodegradable fibers such as polylactic acid. The fabric may also be a blend of these fibers.
[0121] Examples of the form of the fabric include woven fabric, knitted fabric, nonwoven fabric, cloth, and clothing and other accessories. Examples of the clothing and other accessories include furniture such as sewn T-shirts, handkerchiefs, scarves, towels, carrier bags, cloth bags, curtains, sheets, bed covers, and wallpaper; and fabrics before and after cutting as parts before sewing. Examples of the form of the fabric include long ones wound in a roll, ones cut to a predetermined size, and ones in a product shape. Note that the fabric may be one to which at least the reaction liquid composition has been applied in advance.
[0122] The basis weight of the fabric is preferably, for example, 1.0 oz or more and 10.0 oz or less. If the basis weight of the fabric is in this range, good recording can be performed.
[0123] The fabric may be a fabric that has been colored in advance with a dye. The white ink composition and the non-white ink composition are less likely to leave processing marks, so that even fabrics that have been colored in advance can be used. In other words, even if the fabric is colored, it is possible to perform printing that suppresses the occurrence of processing marks, so that the quality and commercial value of the printed textile product can be improved compared to conventional methods.
[0124] Examples of dyes with which the fabric is pre-colored include water-soluble dyes such as acid dyes and basic dyes; disperse dyes used in combination with a dispersant; reactive dyes; and solvent dyes.
[0125] 3.2. White ink composition application step The inkjet recording method includes a white ink composition applying step of ejecting a white ink composition from a recording head and applying it to a recording medium. The white ink composition applying step is performed simultaneously with the non-white ink composition applying step or before the non-white ink composition applying step. Since there is a tendency to obtain a printed material having better color development and wet friction fastness as well as better image quality and texture, when the white ink composition applying step is performed before the non-white ink composition applying step, it is preferable to set the time interval between the white ink composition applying step and the non-white ink composition applying step to within 5 seconds. Through this process, a recording medium to which the white ink composition is adhered can be obtained. Furthermore, by adhering the white ink composition to this recording medium, a printed material having superior color development and wet friction fastness as well as superior image quality and texture can be obtained.
[0126] Examples of methods for adhering the white ink composition to a recording medium include a dip coating method in which a recording medium is immersed in the white ink composition, a roller coating method in which the white ink composition is applied using a mangle roller and a roll coater, etc., a spray coating method in which the white ink composition is sprayed using a spray device, etc., and an inkjet coating method in which the white ink composition is sprayed by an inkjet method. Of these coating methods, one method may be used alone to adhere the white ink composition to a recording medium, or two or more methods may be combined to adhere the white ink composition to a recording medium. In this embodiment, it is preferable to apply the white ink composition to the recording medium using an inkjet method, since this increases the degree of freedom in designing the amount of the white ink composition applied, reduces the occurrence of problems during application, and enables the white ink composition to be applied more uniformly to the recording medium. In addition, since the white ink composition has excellent storage stability, it is possible to perform stable and continuous application when applying the white ink composition using the inkjet method.
[0127] The amount of the white ink composition attached to the recording medium is preferably 20% by mass or more and 80% by mass or less, and more preferably 30% by mass or more and 75% by mass or less, based on the mass of the area of the recording medium to which the white ink composition is attached. When the amount of attachment is within the above range, the white ink composition is more suitably compatible with the recording medium and is more uniformly attached, so that the recording medium tends to absorb water and swell suitably. This tends to result in a printed material having better color development and wet friction fastness as well as better image quality and texture. In this specification, the amount of the white ink composition attached is expressed as a percentage of the mass of the white ink composition attached to the area of the recording medium to which the white ink composition is attached.
[0128] After this step, if necessary, a drying step of drying the recording medium to which the white ink composition has been applied may be included, but since this tends to result in a printed material having better color development and wet rubbing fastness as well as better image quality and texture, it is preferable not to include a drying step. Note that for the drying method and drying time in the drying step, the heating method and heating time in the non-white ink composition application step described below may be referenced.
[0129] 3.3. Non-white ink composition application step The inkjet recording method includes a non-white ink composition applying step of ejecting a non-white ink composition from a recording head and applying it in an overlapping manner to at least an area of the recording medium to which the white ink composition has been applied. The non-white ink composition applying step is performed simultaneously with the white ink composition applying step or after the white ink composition applying step. Since there is a tendency to obtain a printed material having better color development and wet friction fastness as well as better image quality and texture, when the non-white ink composition applying step is performed before the non-white ink composition applying step, it is preferable to set the time interval between the white ink composition applying step and the non-white ink composition applying step to within 5 seconds. Through this process, a recording medium having at least the white ink composition and the non-white ink composition attached thereto can be obtained. By attaching the non-white ink composition to the recording medium, a printed material having superior color development and wet rub fastness as well as superior image quality and texture can be obtained.
[0130] The recording medium to be applied in this step may be a recording medium to which at least a white ink composition has been applied, and for example, a non-white ink composition may be applied to a cloth to which a white ink composition has already been applied. The application of the non-white ink composition may be performed simultaneously with the application of the white composition, or may be performed after the application of the reaction liquid composition.
[0131] The non-white ink composition application step is a step of ejecting the non-white ink composition from an inkjet head by an inkjet method and applying it to a recording medium to which at least the white ink composition has been applied. By adopting the inkjet method, even dyed parts of fine patterns can be easily and reliably formed. In addition, it can be applied to various recording media, and good printing can be performed. In textile printing by such a recording method, for example, even if a thick fabric such as cloth is used as the recording medium, good printing with small color difference between the front and back can be performed. In addition, by recording on a recording medium using the non-white ink composition, a printed textile having excellent wet friction fastness and color development as well as excellent image quality and texture can be easily obtained. In addition, since the non-white ink composition has excellent storage stability, it is possible to stably perform continuous printing in textile printing by the inkjet method.
[0132] The application method is preferably performed in the same inkjet recording apparatus as the white ink composition application step, in which case the non-white ink composition is adjusted so as to be ejected from a nozzle of the recording head different from the nozzle from which the white ink composition is ejected.
[0133] In the non-white ink composition application process, the maximum amount of the ink applied to the recording medium is 50 mg / cm 2 More than 200mg / cm 2 Preferably, it is 80 mg / cm or less. 2 More than 150mg / cm 2 When the maximum adhesion amount is within the above range, a printed material having superior wet rub fastness and color development as well as superior image quality and texture can be obtained.
[0134] 3.4. Time intervals for each step In the inkjet recording method, it is preferable that after the white ink composition is applied to the recording medium in the white ink composition application step, the non-white ink composition application step is carried out within a time interval of 5 seconds.
[0135] By setting the time interval to 5 seconds or less after the white ink composition is applied to the recording medium, the penetration of the white ink composition into the recording medium can be more suitably suppressed, and the white ink composition can suitably aggregate with the non-white ink composition in the vicinity of the recording medium, which tends to result in a printed material having better wet friction fastness and color development as well as better image quality and texture.
[0136] The lower limit of the time interval is not particularly limited, and is 0 seconds or more since the white ink composition application step and the non-white ink composition application step may be carried out simultaneously.
[0137] 3.5.Drying process It is preferable that the inkjet recording method further includes a drying step of heating and drying the white ink composition and the recording medium to which the non-white ink composition is attached, after the non-white ink composition attachment step. The drying temperature in the drying step is preferably 160° C. or higher. By passing through the drying step, the white ink composition and the non-white ink composition can be more suitably attached to the recording medium, and the pigments can be more suitably aggregated. As a result, there is a tendency to obtain a printed material having better wet friction fastness and color development as well as better image quality and texture. This tendency is further strengthened by setting the drying temperature in the drying step to 160° C. or higher.
[0138] The drying temperature is, for example, preferably 300° C. or less, and more preferably 200° C. or less. As a result, for example, when cloth is used as the recording medium, even if the cloth is pre-colored with a dye, sublimation of the dye due to heat drying can be suppressed, and fading of the fabric color of the cloth can be suppressed.
[0139] Examples of the heating method include hot air drying, heat pressing, normal pressure steam, high pressure steam, and Thermofix, and examples of the heat source for heating include hot air, infrared rays, and microwaves.
[0140] In the case where a cloth is used as the recording medium during heating, the surface temperature of the heated recording medium is preferably 60° C. or more and 180° C. or less. When the surface temperature is within the above range, damage to the inkjet head and the cloth can be reduced, and the ink can easily spread and penetrate uniformly into the cloth. The surface temperature can be measured, for example, using a non-contact thermometer (product name "IT2-80", manufactured by Keyence Corporation).
[0141] The heating time is preferably, for example, from 5 seconds to 10 minutes. By keeping the heating time within the above range, it becomes possible to sufficiently heat the recording medium while reducing damage to the inkjet head and the recording medium.
[0142] 3.6.Other processes The inkjet recording method may further include a washing step of washing the printed matter after the drying step. By including this step in the recording method, components that are not attached to the recording medium can be removed.
[0143] The recording method may include a step of depositing one or more types of ink compositions selected from the group consisting of a white ink composition and a non-white ink composition onto the recording medium, if necessary. In this case, there is no restriction on the order or number of these steps, and they may be carried out appropriately as necessary.
[0144] 3.7. Inkjet recording device The inkjet recording device used in the inkjet recording method is not particularly limited as long as it has at least an ink container that contains an ink composition and a recording head connected thereto, and can eject the ink composition from the recording head to form an image on a recording medium. In addition, the inkjet recording device preferably has a container that contains both a white ink composition and a non-white ink composition as ink compositions, and a recording head connected thereto. In that case, the white ink composition and the non-white ink composition can be ejected from the recording head to adhere to the recording medium.
[0145] The inkjet recording apparatus may be either a serial type or a line type. A recording head is mounted on these types of inkjet recording apparatus. Such an inkjet recording apparatus ejects droplets of the ink composition intermittently and in a predetermined volume from the nozzle holes of the recording head at a predetermined timing while changing the relative positional relationship between the recording medium and the recording head. This allows the white ink composition and the non-white ink composition to adhere to the recording medium, forming a predetermined transfer image.
[0146] In general, in a serial type inkjet recording device, the transport direction of the recording medium and the direction of the reciprocating motion of the recording head intersect, and the relative positional relationship between the recording medium and the recording head is changed by combining the reciprocating motion of the recording head and the transport motion of the recording medium. In this case, generally, a plurality of nozzle holes are arranged in the recording head, and a row of nozzle holes, i.e., a nozzle row, is formed along the transport direction of the recording medium. In addition, a recording head may be formed with a plurality of nozzle rows depending on the type and number of ink compositions.
[0147] Generally, in a line-type inkjet recording device, the recording head does not perform a reciprocating motion, but changes the relative positional relationship between the recording medium and the recording head by conveying the recording medium. Even in this case, generally, the recording head has a plurality of nozzle holes arranged therein, and a nozzle row is formed along a direction intersecting the conveying direction of the recording medium. EXAMPLES
[0148] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following, "parts" refers to parts by mass unless otherwise specified.
[0149] 1. Preparation of White Ink Composition (Examples 1 to 12 and Comparative Examples 1 to 4) Each component was placed in a mixing tank so as to obtain the composition shown in Tables 1 and 2, and then mixed and stirred, and further filtered through a 5 μm PTFE membrane filter, to obtain each white ink composition.
[0150] The numerical values of the blending amounts of each component in Tables 2 and 3 represent mass %. Ion-exchanged water was used as water, and was added so that the mass of each reaction liquid composition was 100 mass %.
[0151] [White pigment] HT1432...ROPAQUE (registered trademark) HT1432 (product name, manufactured by Dow Chemical Japan, styrene-acrylic resin dispersion)
[0152] 〔resin〕 · W-6110... Takelac (registered trademark) W-6110 (product name, manufactured by Mitsui Chemicals, Inc., urethane resin dispersion, oxidation: 50 mg KOH / g or more, Tg: -20°C) · UW-1527DF…ETERNACALL (registered trademark) UW-1527DF (product name, manufactured by Ube Industries, Ltd., urethane resin dispersion, oxidation: less than 50 mg KOH / g, Tg: 0°C or higher)
[0153] [Water-soluble organic solvent] Glycerin (SP value: 17.5) Triethylene glycol (SP value: 12.8) Triethylene glycol monobutyl ether (SP value: 10.5) Triethylene glycol monomethyl ether (SP value: 10.0)
[0154] [Surfactant] E1010: Olfine (registered trademark) E1010 (product name, manufactured by Nissin Chemical Industry Co., Ltd.)
[0155] [pH adjuster] Triethanolamine Adipic Acid
[0156] 2. Preparation of Non-White Ink Compositions (Examples 1 to 12 and Comparative Examples 1 to 4) Each of the components was placed in a mixing tank so as to obtain the composition shown in Tables 3 and 4, and then mixed and stirred, and further filtered through a 5 μm PTFE membrane filter, to obtain each of the non-white ink compositions.
[0157] The numerical values of the blending amounts of each component in Tables 3 and 4 represent mass %. Ion-exchanged water was used as water, and was added so that the mass of each reaction liquid composition was 100 mass %.
[0158] [Non-white pigment] PB15:3…CI Pigment Blue 15:3 (commercially available)
[0159] 〔resin〕 · W-6110... Takelac (registered trademark) W-6110 (product name, manufactured by Mitsui Chemicals, Inc., urethane resin dispersion, oxidation: 50 mg KOH / g or more, Tg: -20°C) · UW-1527DF…ETERNACALL (registered trademark) UW-1527DF (product name, manufactured by Ube Industries, Ltd., urethane resin dispersion, oxidation: less than 50 mg KOH / g, Tg: 0°C or higher) In addition, "Tg" represents the glass transition temperature (°C).
[0160] [Water-soluble organic solvent] Glycerin Triethylene glycol ·Triethylene glycol monobutyl ether
[0161] [Surfactant] E1010: Olfine (registered trademark) E1010 (product name, manufactured by Nissin Chemical Industry Co., Ltd.)
[0162] [pH adjuster] Triethanolamine Adipic Acid
[0163] 3. Physical properties of white ink composition and non-white ink composition 3.1.pH The pH of each of the white ink compositions of Examples 1 to 12 and Comparative Examples 1 to 4 and the non-white ink compositions of Examples 1 to 12 and Comparative Examples 1 to 4 was measured. Specifically, the pH was measured using a tabletop pH meter F-72 model (manufactured by Horiba, Ltd.) by immersing the electrode portion in each ink composition. The results are shown in Tables 5 and 6.
[0164] 3.2. Storage stability The storage stability of each of the white ink compositions of Examples 1 to 12 and Comparative Examples 1 to 4 and the non-white ink compositions of Examples 1 to 12 and Comparative Examples 1 to 4 was evaluated. Specifically, first, the viscosity of each ink composition was measured in an environment of 20°C using a viscoelasticity tester MCR-300 (trade name, manufactured by Pysica), and the values were taken as initial viscosities. Then, each ink composition was placed in a screw tube, and left for 5 days in an environment of 60°C with the lid closed. The viscosity of each ink composition after 5 days was measured in an environment of 20°C using a viscoelasticity tester MCR-300 (trade name, manufactured by Pysica), and the values were taken as viscosities after 5 days. The storage stability was evaluated by calculating the rate of change in the viscosity value after 5 days relative to the initial viscosity value, and the following criteria were used. The results are shown in Tables 5 and 6. A: The viscosity change rate is less than 5%. B: The viscosity change rate is 5% or more and less than 10%. C: The viscosity change rate is 10% or more and less than 20%. D: The viscosity change rate is 20% or more.
[0165] 4. Preparation of printed matter 4.1. Preparation of fabric with white ink composition attached (Examples 1 to 12 and Comparative Examples 1 to 4) The white ink composition was applied to a fabric as a recording medium using each of the white ink compositions of Examples 1 to 12 and Comparative Examples 1 to 4. Specifically, a fabric to which the white ink composition was applied was obtained as follows. Each of the white ink compositions obtained in Examples 1 to 12 and Comparative Examples 1 to 4 was applied to a heavy weight T-shirt (black 00085-CVT, product name, manufactured by PrintStar) as a fabric by an inkjet method using an inkjet printer (SC-F2000, product name, manufactured by Seiko Epson Corporation). The amount of the white ink composition applied was a solid pattern with a duty of 100% under conditions of an ink droplet mass (Iw) of 24 ng / dot and a resolution of 2880×1440 dpi. The time interval between the application of each white ink composition to the fabric and the application of each non-white ink composition was always within 5 seconds.
[0166] 4.2.Textile printing (Examples 1 to 12 and Comparative Examples 1 to 4) The non-white ink composition was applied to each of the fabrics to which the white ink composition obtained in Examples 1 to 12 and Comparative Examples 1 to 4 was applied, and an image was recorded. Specifically, the non-white ink compositions obtained in Examples 1 to 12 and Comparative Examples 1 to 4 were applied to each of the fabrics to which the white ink composition had been applied by an inkjet method using an inkjet printer (SC-F2000, product name, manufactured by Seiko Epson Corporation). The amount of the non-white ink composition applied was a solid pattern with a duty of 100% under conditions of an ink droplet mass (Iw) of 24 ng / dot and a resolution of 2880×1440 dpi.
[0167] After printing the images, the images were dried by heat treatment at 160° C. for 5 minutes in a conveyor oven, ie, by hot air drying, to obtain printed matter in Examples 1 to 12 and Comparative Examples 1 to 4, respectively.
[0168] 5. Evaluation of printed matter 5.1.Color development For each of the printed materials in Examples 1 to 12 and Comparative Examples 1 to 4 obtained by the above-mentioned production of printed materials, the OD (Optical Density) value of the portion of each recorded material where the ink was applied was measured using a colorimeter i1 (product name, manufactured by X-rite Corporation). The obtained values were evaluated for color development according to the following criteria. The results are shown in Tables 5 and 6. A: The OD value is 1.3 or higher. B: The OD value is 1.1 or more and less than 1.3. C:OD value is 0.9 or more and less than 1.1. D: The OD value is less than 0.9.
[0169] 5.2.Image quality evaluation The printed textiles of Examples 1 to 12 and Comparative Examples 1 to 4 obtained by the above-mentioned printing process were visually observed for bleeding and the image quality was evaluated according to the following criteria. The results are shown in Tables 5 and 6. A: There is no bleeding. B: There is some bleeding, but it doesn't bother me. C: Bleed is noticeable but acceptable. D: Bleeding is noticeable.
[0170] 5.3. Wet rubbing fastness The wet rub fastness of each of the printed textiles in Examples 1 to 12 and Comparative Examples 1 to 4 obtained by the above-mentioned printing process was evaluated according to the following criteria in accordance with ISO 105 X12. The test was performed by the crock meter method. The results are shown in Tables 5 and 6. (standard) A: Wet rubbing fastness is 3 or higher. B: Wet friction fastness is grade 2-3 (intermediate grade). C: Wet rubbing fastness is 2. D: Wet rubbing fastness is less than grade 2.
[0171] 5.4. Texture The prints obtained by the above-mentioned production of the prints in Examples 1 to 12 and Comparative Examples 1 to 4 were evaluated for feel according to the following criteria. The results are shown in Tables 5 and 6. A:Soft. B: It doesn't feel soft or hard. C: It feels a little hard. D: It feels noticeably stiffer.
[0172] As shown in Tables 5 and 6, it was found that the ink set of this embodiment can provide a white ink composition and a non-white ink composition having excellent storage stability, and can provide printed matter having excellent color development and wet rub fastness.
[0173] It was found from Examples 2 and 6 to 9 that when the white ink composition contains a water-soluble organic solvent having an SP value of 9 or more and 11 or less, better wet rub fastness can be obtained.
[0174] From Examples 2, 10, and 11, it was found that when the white ink composition contains a resin having an acid value of 50 mgKOH / g or more, better storage stability can be obtained.
[0175] From Examples 2, 11, and 12, it was found that when the non-white ink composition contains a resin having an acid value of less than 50 mgKOH / g, better storage stability can be obtained.
[0176] From Examples 2, 10, and 11, it was found that when the white ink composition contains a resin having a glass transition temperature of -10°C or lower, a more excellent texture can be obtained.
[0177] From Examples 2, 11, and 12, it was found that when the non-white ink composition contains a resin having a glass transition temperature of −10° C. or lower, better wet rub fastness can be obtained.
Claims
1. a white ink-jet ink composition and a non-white ink-jet ink composition, the white inkjet ink composition has a pH of 5 or more and 7 or less at 25° C.; The non-white inkjet ink composition has a pH of 8 or more and 10 or less at 25° C. Ink set.
2. the white inkjet ink composition contains a water-soluble organic solvent having an SP value of 9 or more and 11 or less; The ink set according to claim 1.
3. the white inkjet ink composition contains a resin having an acid value of 50 mgKOH / g or more, the non-white inkjet ink composition comprises a resin having an acid value of less than 50 mg KOH / g; The ink set according to claim 1.
4. the white inkjet ink composition contains a resin having a glass transition temperature of −10° C. or lower; The ink set according to claim 1.
5. The non-white inkjet ink composition contains a resin having a glass transition temperature of 0° C. or higher. The ink set according to claim 1.
6. a white ink-jet ink composition depositing step of ejecting the white ink-jet ink composition provided in the set according to claim 1 from a recording head and depositing the white ink-jet ink composition on a recording medium; a non-white ink-jet ink composition applying step of ejecting the non-white ink-jet ink composition provided in the set according to claim 1 from a recording head and applying the non-white ink-jet ink composition to a recording medium to which at least the white ink-jet ink composition has been applied; Including, the step of applying the non-white inkjet ink composition is performed within a time interval of 5 seconds after the step of applying the white inkjet ink composition to the recording medium; Inkjet recording method.
7. The ink-jet recording method according to claim 6, wherein the recording medium is a fabric.
Citation Information
Patent Citations
Image formation method and ink set
JP2020062783A